film
A film with a balanced resin composition of cellulose ester, aliphatic polyester, and acrylic polymer addresses the challenge of achieving both transparency and gas permeability, enhancing its suitability for diverse applications.
Patent Information
- Application Number
- JP2023062239
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Films laminated on the surface of articles often require both gas permeability and transparency, which existing technologies struggle to balance effectively.
A film composed of a resin composition containing cellulose ester, aliphatic polyester, and acrylic polymer, with specific ratios and properties to achieve optimal transparency and gas permeability, including a glass transition temperature range and permeability values.
The film achieves excellent transparency and gas permeability, suitable for various applications including laminated uses.
Smart Images

Figure 2024148793000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a film. [Background technology]
[0002] Films that are laminated on the surfaces of various articles are known. For example, protective films for polarizing plates, retardation films, viewing angle expansion films, etc., used in liquid crystal display devices It is used as an optical film such as an anti-reflection film for films and plasma displays. USP 5,333,636 describes cellulose ester films which can be used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-54100 A Summary of the Invention [Problem to be solved by the invention]
[0004] The film laminated on the surface of the article may be required to have gas permeability. There are cases where transparency is required to allow the surface of the article underneath the film to be seen. The object of the present invention is to provide a film that is excellent in transparency and gas permeability. . [Means for solving the problem]
[0005] The present invention has the following aspects. [1] A cellulose ester compound (A), an aliphatic polyester (B), and an acrylic polymer The film is made of a resin composition containing the cellulose ester compound (C), A) 100 parts by mass of the acrylic polymer (C) is 20 parts by mass or more and 400 parts by mass or less. Containing 0.1% distortion, 10Hz frequency, and 3℃ heating rate according to JIS K7244-4 The glass transition temperature (Tg) of the film measured at 1000 rpm is 60°C or higher and 115°C or lower. film. [2] The content of the cellulose ester compound (A) relative to the total mass of the resin composition. The film according to [1], wherein the amount is 10% by mass or more and 60% by mass or less. [3] The content of the aliphatic polyester (B) relative to the total mass of the resin composition is 1. The film according to [1] or [2], wherein the content is 0% by mass or more and 50% by mass or less. [4] The content of the acrylic polymer (C) relative to the total mass of the resin composition is 10% by mass. The film according to any one of [1] to [3], wherein the content is from 0.05% by mass to 70% by mass. [5] The aliphatic polyester (B) comprises a constitutional unit derived from an aliphatic polycarboxylic acid and an aliphatic Any of [1] to [4], which is a polymer having a structural unit derived from an aromatic polyhydric alcohol. The film described. [6] The film according to any one of [1] to [5], having a total light transmittance of 90% or more. . [7] Oxygen permeability is 1000-10000cc / (m 2 ·24h·atm), The film according to any one of items 1] to [6]. [8] Nitrogen permeability is 100-5000cc / (m 2 ·24h·atm),[1] The film according to any one of claims 1 to 7. Effect of the Invention
[0006] According to the present invention, a film having excellent transparency and excellent gas permeability can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] In this specification, the term "structural unit" of a polymer refers to a unit (atom) formed from one monomer molecule. It means a group. In this specification, the symbol "~" indicating a range of values indicates that the values before and after the symbol are the lower limit and the It means inclusive as an upper limit.
[0008] ≪Resin composition (X)≫ The resin composition (X) of the present embodiment comprises a cellulose ester compound (A), an aliphatic polyester compound (B), and a cellulose ester compound (C). The copolymer contains a terephthalate (B) and an acrylic polymer (C).
[0009] <Cellulose ester compound (A)> The cellulose ester compound (A) is, for example, cellulose propionate (CP ), cellulose butyrate (CB), cellulose acetate propionate (CAP), Cellulose acetate butyrate (CAB), Cellulose acetate isobutyrate (C AIB), cellulose propionate butyrate (CPB), etc. From the viewpoint of film transparency, cellulose acetate propionate is preferred. The ester compound (A) may be used alone or in combination of two or more kinds. The resin composition (X) is a cellulose ester compound which is a substance derived from a renewable organic resource. By including this, the environmental impact can be reduced.
[0010] The glass transition temperature (Tg) of the cellulose ester compound (A) depends on the function of the resulting film. From the viewpoint of mechanical properties, the temperature is preferably 120°C or higher, and more preferably 130°C or higher. From this viewpoint, the temperature is preferably 180° C. or lower, and more preferably 170° C. or lower. The glass transition temperature (Tg) of the cellulose ester compound (A) is determined according to JIS K7244- 4:1999, using a viscoelastic spectrometer at a heating rate of 3°C / min. It is calculated from the peak top temperature of the loss tangent (tan δ) when the temperature is raised by can be done.
[0011] <Aliphatic polyester (B)> The aliphatic polyester (B) is a polyester having a constitutional unit derived from an aliphatic hydroxycarboxylic acid. The polymer (b-1) has a constitutional unit derived from an aliphatic polyvalent carboxylic acid and a constitutional unit derived from an aliphatic polyhydric alcohol. and polymers (b-2) having the following structural units.
[0012] The polymer (b-1) contains, with respect to all structural units, a structure derived from an aliphatic hydroxycarboxylic acid. The proportion of the structural unit is preferably 80% by mass or more, and more preferably 90% by mass or more. It may be 100% by mass, which is preferable. Specific examples of the polymer (b-1) include polyglycolic acid, polylactic acid, poly(3-hydroxyl) acid, and the like. Poly(4-hydroxybutyric acid), Poly(4-hydroxyvaleric acid), Poly(3-hydroxyhexanoic acid) Examples of the polycaprolactone include acrylic acid and polycaprolactone.
[0013] The polymer (b-2) contains, relative to all structural units, structural units derived from aliphatic polyvalent carboxylic acids. and the total proportion of structural units derived from aliphatic polyhydric alcohols is preferably 80 mass % or more. It is preferably 90% by mass or more, and may be 100% by mass. Specific examples of the polymer (b-2) include polyethylene adipate and polypropylene adipate. Polybutylene adipate, Polyhexene adipate, Polybutylene succinate ( Examples include polybutylene succinate adipate (PBSA), etc.
[0014] Of the above, the aliphatic polyester (B) is more suitable than polybutylene in terms of film flexibility. The succinate resin is preferably polybutylene succinate (PBS) or poly More preferably, it is butylene succinate adipate (PBSA), and among them, Butylene succinate (PBS) is more preferred. Aliphatic polyesters (B) are made from renewable organic resources. preferable.
[0015] <Acrylic polymer (C)> The acrylic polymer (C) includes the following polymer (Ca) and the following polymer (Cb). Acrylic polymer (c-1), polymer (Cd) alone consisting of acrylic polymer (c-2), etc. Some examples include:
[0016] =Acrylic polymer (c-1)= The acrylic polymer (c-1) is a polymer (Ca) obtained by polymerizing the monomer components described below. It is preferable that the polymer (Cb) is a polymer obtained by polymerizing the monomer components of the polymer (Cb) in the presence of stomach. The acrylic polymer (c-1) is a polymer having a core layer and at least one shell layer covering the core layer. The acrylic polymer (c-1) may be a multilayer structure polymer. In the case of the above, the innermost layer is composed of a polymer (Ca) and the outermost layer is composed of a polymer (Cb). It is preferable that
[0017] The acrylic polymer (c-1) may further contain a polymer (Cc). The acrylic polymer (c-1) is a polymer (Ca), a polymer (Cb), and a polymer (Cc). In the case where the acrylic polymer (c-1) contains the polymer (Cc) in the presence of the polymer (Ca), A polymer obtained by polymerizing the monomer component of (Cb) and then polymerizing the monomer component of polymer (Cb). It is preferable that there is. Acrylic polymers (c-1) including polymer (Ca), polymer (Cb), and polymer (Cc) When the polymer has a multi-layer structure, the innermost layer is made of polymer (Ca) and the outermost layer is made of polymer (Cb ), and between the outermost layer and the innermost layer there is a layer composed of a polymer (Cc). preferable.
[0018] [Polymer (Ca)] The polymer (Ca) has an alkyl group having 1 to 8 carbon atoms and one double bond in each molecule. A structural unit derived from (meth)acrylic acid ester (MA1) and a double bond in one molecule. It contains a constituent unit derived from a monomer (MA2) having at least one of the above units.
[0019] In the (meth)acrylic acid ester (MA1), the alkyl group having 1 to 8 carbon atoms is It may be either linear or branched. A specific example of the (meth)acrylic acid ester (MA1) is methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate These may be used alone or in combination of two or more. Among them, those having a low Tg in the homopolymer are preferred, and acrylic acid alkyl esters are preferred. is more preferred, with butyl acrylate being particularly preferred.
[0020] The content of (meth)acrylic acid ester (MA1) is the monomer constituting the polymer (Ca). The total amount of the above is preferably 40% by mass or more, and more preferably 50% by mass or more, based on 100% by mass of the total amount of the above. It is preferably 70% by mass or more, more preferably 90% by mass or more, and particularly preferably 99. It is preferably 9% by mass or less, and more preferably 99.7% by mass or less.
[0021] The monomer (MA2) is copolymerizable with the (meth)acrylic acid ester (MA1). It is a monomer that has two or more double bonds in one molecule. Specific examples of the monomer (MA2) include ethylene glycol di(meth)acrylate, 1 ,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate alkylene glycols such as acrylate, propylene glycol di(meth)acrylate, etc. vinyl di(meth)acrylate; polyvinylbenzene such as divinylbenzene and trivinylbenzene Cyanurate monomers such as triallyl cyanurate and triallyl isocyanurate Allyl esters and methallyl esters of α,β-unsaturated carboxylic acids or dicarboxylic acids These may be used alone or in combination of two or more. They may also be used in combination. Of the above, alkylene glycol di(meth)acrylate, acrylic acid, methacrylate Preferred are allyl esters of allylic acid, maleic acid or fumaric acid, among which allyl methacrylate is preferred. Acrylates are more preferred.
[0022] The content of the monomer (MA2) is, from the viewpoint of flexibility, The total amount of the above is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, based on 100% by mass of the total amount of the above. From the viewpoint of film formability, the content is preferably 60% by mass or less, and more preferably 50% by mass or less. is more preferable, 30 mass % or less is further preferable, and 10 mass % or less is particularly preferable.
[0023] The glass transition temperature (Tg) of the polymer (Ca) is important in terms of flexibility and gas permeability of the film. Therefore, 25° C. or less is preferable, 10° C. or less is more preferable, and 0° C. or less is even more preferable. A temperature lower than 0° C. is particularly preferable. From the viewpoint of film formability, Tg is preferably −100° C. or higher. Preferably, the temperature is −80° C. or higher. The glass transition temperature (Tg) of the polymer (Ca) is HandBook (J. Brandrup, Interscience, 1989)〕 Using the values listed in the table, the monomers that make up the polymer (Ca) are calculated using the FOX formula. In addition, the viscoelasticity spectrum can be calculated using a method conforming to JIS K7244-4:1999. The loss tangent (tan δ) when the temperature was increased at a heating rate of 3°C / min using a trometer It can be determined from the peak top temperature. The glass transition temperatures of the polymers (Cb), (Cc), and (Cd) described below are also similar. do.
[0024] [Polymer (Cb)] The polymer (Cb) has an alkyl group having 1 to 4 carbon atoms and one double bond in each molecule. A polymer containing a structural unit derived from a (meth)acrylic acid ester (MB1) (provided that the polymer The polymer (Cb) is a polymer having a constitutional unit derived from the monomer (MA2). Does not include.
[0025] In the (meth)acrylic acid ester (MB1), the alkyl group having 1 to 4 carbon atoms is It may be either linear or branched. A specific example of the (meth)acrylic acid ester (MB1) is methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate These may be used alone or in combination of two or more. Among these, those having a low Tg in the homopolymer are preferred, and alkyl acrylates are preferred. Esters are more preferred, with butyl acrylate being especially preferred.
[0026] The content of (meth)acrylic acid ester (MB1) is the monomer constituting polymer (Cb). The total amount of the above is preferably 50% by mass or more, and more preferably 80% by mass or more, based on 100% by mass of the total amount of the above. It may be 100% by mass.
[0027] The glass transition temperature (Tg) of the polymer (Cb) may be different from that of the polymer (Ca); The Tg of the polymer (Cb) is preferably higher than the Tg of the polymer (Ca). From the viewpoint of mechanical properties, 60°C or higher is preferable, 70°C or higher is more preferable, and 80°C or higher is even more preferable. From the viewpoint of the gas permeability of the film, the temperature is preferably 150° C. or less, and more preferably 130° C. The following is more preferred:
[0028] [Polymer (Cc)] The polymer (Cc) has an alkyl group having 1 to 8 carbon atoms and one double bond in each molecule. The structural unit derived from (meth)acrylic acid ester (MC1) and the double bond are two in one molecule. It is preferable that the monomer (MC1) contains a structural unit derived from a monomer (MC2) having at least one of the above units. A preferred embodiment of the (meth)acrylic acid ester (MC1) is the same as that of the polymer (Ca). The preferred embodiment of the monomer (MC2) is the same as that of the polymer (Ca). This is similar to (MA2) mentioned above. The composition (type and ratio) of the monomers constituting the polymer (Cc) and the It is preferable that the compositions (types and ratios) of the monomers constituting the polymerization copolymer (polymerization copolymer) are not the same. The monomer composition of the polymer (Cc) is different from that of the polymer (Ca). This makes it easier to improve the flexibility of the material.
[0029] The content of the (meth)acrylic acid ester (MC1) is the same as that of the monomer constituting the polymer (Cc). The amount is preferably 40% by mass or more, more preferably 50% by mass or more, based on 100% by mass of the total amount of the monomers. It is preferably 70% by mass or more, more preferably 70% by mass or more, and particularly preferably 90% by mass or more. It is preferably 9.9% by mass or less, and more preferably 99.7% by mass or less.
[0030] The content of the monomer (MC2) is set to 100% by weight based on the content of the monomer constituting the polymer (Cc) from the viewpoint of flexibility. The total amount of the above is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, based on 100% by mass of the total amount of the above. From the viewpoint of film formability, the content is preferably 60% by mass or less, and more preferably 50% by mass or less. is more preferable, 30 mass % or less is further preferable, and 10 mass % or less is particularly preferable.
[0031] The glass transition temperature (Tg) of the polymer (Cc) is determined from the viewpoint of the flexibility of the film. It is preferable that the Tg is higher than that of a). Specifically, from the viewpoint of flexibility, it is preferable that the Tg is 0° C. or higher. More preferably, the temperature is higher than 0° C., and even more preferably higher than 10° C. In addition, in terms of gas permeability and moldability, Therefore, the temperature is preferably 100° C. or lower, and more preferably 80° C. or lower. For example, if the glass transition temperature (Tg) of polymer (Cc) is higher than the glass transition temperature (Tg) of polymer (Ca), The absolute value of the difference is preferably 10 to 80°C, and more preferably 20 to 70°C. It is more preferable that the absolute value of the difference between the two is equal to or greater than the lower limit of the above range. When the content is equal to or less than the upper limit, the gas permeability and flexibility of the film can be improved. The moldability is also improved.
[0032] The content of the polymer (Ca) relative to the total mass of the acrylic polymer (c-1) is From the viewpoints of transparency and moldability, the content is preferably 5% by mass or more, and more preferably 10% by mass or more. More preferably, the content is 20% by mass or more. Also, the content is preferably 60% by mass or less, and more preferably 55% by mass or less. is more preferred. The content of the polymer (Cb) relative to the total mass of the acrylic polymer (c-1) is 40% by mass. The content is 45% by mass or more, and preferably 45% by mass or more. In addition, it is excellent in transparency and moldability. % or less, more preferably 80% by mass or less, even more preferably 70% by mass or less. preferable. In addition, when the acrylic polymer (c-1) contains the polymer (Cc), the acrylic polymer (c- The content of the polymer (Cc) relative to the total mass of 1) is 1 mass% or more from the viewpoint of flexibility. It is preferably 35% by mass or less. The content of the polymer (Ca), the content of the polymer (Cb), and the content of the polymer ( The total content of Cc) does not exceed 100% by mass. It may be 100% by mass.
[0033] =Acrylic polymer (c-2)= [Polymer (Cd)] The polymer (Cd) has an alkyl group having 1 to 18 carbon atoms and one double bond in each molecule. It is a polymer containing structural units derived from a (meth)acrylic acid ester (MD1).
[0034] In the (meth)acrylic acid ester (MD1), the alkyl group having 1 to 18 carbon atoms is The alkyl group may be either linear or branched. A specific example of the (meth)acrylic acid ester (MD1) is methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl ( (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, desic (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate acrylate, stearyl (meth)acrylate, icosyl (meth)acrylate, heminecosyl (Meth)acrylate, behenyl (meth)acrylate and other linear alkyl (meth)acrylates acrylate; isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec -Butyl (meth)acrylate, t-Butyl (meth)acrylate, Isopentyl (meth)acrylate ) acrylate, neopentyl (meth) acrylate, 2-ethylhexyl (meth) acrylate acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, iso Decyl (meth)acrylate, Isostearyl (meth)acrylate, Isoicosyl (meth)acrylate Branched alkyl (meth)acrylates such as cyclohexyl (meth)acrylate; acrylate, t-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, adamantyl (Meth)acrylate and other alicyclic (meth)acrylates. Among these, T in homopolymers may be used. Those having a low g are preferred, and alkyl acrylates are more preferred, and methyl methacrylates are more preferred. Rate is particularly preferred.
[0035] The content of (meth)acrylic acid ester (MD1) is the monomer that constitutes the polymer (Cd). The total amount of the above is preferably 50% by mass or more, and more preferably 80% by mass or more, based on 100% by mass of the total amount of the above. It may be 100% by mass.
[0036] The glass transition temperature (Tg) of the polymer (Cd) is set to 60°C or higher from the viewpoint of the mechanical properties of the film. Preferably, the temperature is 70°C or higher, more preferably 80°C or higher. From the viewpoint of gas permeability of the rubber, the temperature is preferably 150° C. or lower, and more preferably 130° C. or lower.
[0037] Preferred embodiments of the acrylic polymer (C) include the following embodiments 1, 2 and 3. [Aspect 1] The acrylic polymer (C) contains a polymer (Ca) and a polymer (Cb), Relative to the total mass of the polymer (C), The content of the polymer (Ca) is 5 to 60% by mass, preferably 10 to 60% by mass, more preferably Preferably, it is 20 to 55 mass %. The content of the polymer (Cb) is 40 to 95% by mass, preferably 40 to 90% by mass, more preferably A preferred embodiment is 45 to 80% by mass. [Aspect 2] The acrylic polymer (C) is a polymer (Ca), a polymer (Cb), and a polymer ( Cc), based on the total mass of the acrylic polymer (C), The content of the polymer (Ca) is 5 to 59% by mass, preferably 10 to 55% by mass, and more preferably Preferably, it is 20 to 55 mass %. The content of the polymer (Cb) is 40 to 94% by mass, preferably 40 to 90% by mass, more preferably Preferably, it is 45 to 80 mass %. The content of the polymer (Cc) is 1 to 35% by mass, preferably 3 to 30% by mass, and more preferably Or, in an embodiment, the content is 5 to 25 mass %. [Aspect 3] The acrylic polymer (C) contains a polymer (Cd), and the total amount of the acrylic polymer (C) is With respect to mass, The content of the polymer (Cd) is 50 to 100% by mass, preferably 60 to 99.5% by mass. More preferably, the content is 70 to 99% by mass.
[0038] [Method for producing acrylic polymer (C)] The acrylic polymer (C) can be produced, for example, by a sequential multi-stage emulsion polymerization method, an emulsion suspension polymerization method, or the like. Methods such as suspension polymerization method are included. The acrylic polymer (c-1) can be produced by a sequential multi-stage emulsion polymerization method, for example. The emulsion prepared by mixing the monomer components, water and surfactant to obtain the polymer (Ca) is reacted. After feeding the polymer to the reactor and polymerizing, the monomer components that are the raw materials for the polymer (Cc) are reacted as necessary. After the polymerization is carried out in the reactor, the monomer components that are the raw materials for the polymer (Cb) are fed to the reactor. A method of polymerizing the compound by polymerization is mentioned. The acrylic polymer (c-1) can be produced by emulsion suspension polymerization, for example. In the presence of polymer (Ca), monomer components which are raw materials for polymer (Cc) are successively added as necessary. After multi-stage emulsion polymerization, the suspension polymerization system is used during polymerization of the monomer components that are the raw materials for polymer (Cb). An example of such a method is an emulsion suspension polymerization method in which the copolymer is converted into the copolymer. The acrylic polymer (c-1) obtained by the above-mentioned sequential multistage emulsion polymerization method or emulsion suspension polymerization method is used. The film obtained by this method has the characteristic of having a small number of fish eyes (foreign matter) in the film. It is preferable in this respect. The acrylic polymer (c-2) can be produced, for example, by reacting the polymer (Cd) A known method for this purpose is suspension polymerization.
[0039] The average particle size of the acrylic polymer (C) is determined from the viewpoints of the mechanical properties and transparency of the resulting film. , 0.03 μm or more is preferable, 0.07 μm or more is more preferable, and 0.09 μm or more is It is particularly preferable that the thickness is 0.3 μm or less, more preferably 0.15 μm or less, and 0. .13 μm or less is particularly preferred. The average particle size is a cumulonimbus measured by a dynamic light scattering method using a light scattering photometer. These are measurements taken using optical fiber analysis.
[0040] The mass average molecular weight (Mw) of the acetone soluble portion of the acrylic polymer (C) is preferably 20,000 or more. It is preferable that the molecular weight is 150,000 or less, and more preferable that the molecular weight is 100,000 or less. If Mw is 20,000 or more, the mechanical strength of the obtained film is improved, and cracks during molding are prevented. In addition, when Mw is 150,000 or less, the obtained film has high flexibility and is easy to be molded. Excellent gas permeability and moldability.
[0041] The mass average molecular weight (Mw) is determined based on the acetone soluble content in the acrylic polymer (C). The measured values were determined by gel permeation chromatography (GPC) using the following method. (1) 1 g of acrylic polymer is dissolved in 50 g of acetone and refluxed at 70°C for 6 hours to obtain acetone. Extract ton soluble matter. (2) The obtained extract was incubated at 4°C using a CRG SERIES (Hitachi, Ltd.). The mixture is centrifuged at 14,000 rpm for 30 minutes. (3) Remove the acetone insoluble matter by decantation, and simmer in a vacuum dryer at 50°C for 24 hours. The acetone solubles were then dried for 1 hour and the resulting solution was subjected to GPC measurement under the following conditions. The mass average molecular weight is determined from a calibration curve using styrene. Equipment: Tosoh Corporation "HLC8220" Column: Tosoh "TSKgel SuperMultiporeHZ-H" (Inner diameter 4.6 mm x length 15 cm x 2 pieces, exclusion limit 4 x 10 7 (Estimated) Eluent: Tetrahydrofuran Eluent flow rate: 0.35mL / min Measurement temperature: 40℃ Sample injection volume: 10 μL (sample concentration 0.1%)
[0042] <Optional ingredients> The resin composition (X) may contain various additives as required. Examples of such additives include antioxidants, heat stabilizers, light stabilizers, plasticizers, lubricants, antistatic agents, flame retardants, Fillers, matting agents, processing aids, impact resistance aids, antibacterial agents, antifungal agents, foaming agents, release agents, colorants , ultraviolet absorbers, and thermoplastic polymers. The resin composition (X) is also recyclable. Polysaccharides such as starch may be blended as a material derived from organic resources.
[0043] As the antioxidant, phenol-based, sulfur-based, phosphorus-based, etc. antioxidants can be used. Heat stabilizers include hindered phenol-based, sulfur-based, and hydrazine-based heat stabilizers. The plasticizers that can be used include phthalate esters, phosphate esters, and fats. Acid ester type, aliphatic dibasic acid ester type, oxybenzoic acid ester type, epoxy type, poly As lubricants, fatty acid esters, fatty Use lubricants such as acid-based, metal soap-based, fatty acid amide-based, higher alcohol-based, and paraffin-based. It is possible.
[0044] The antistatic agent may be a cationic, anionic, nonionic, or amphoteric antistatic agent. Flame retardants can be used. Bromine-based, phosphorus-based, chlorine-based, nitrogen-based, aluminum-based, etc. Uses flame retardants such as nium, antimony, magnesium, boron, and zirconium. Fillers include calcium carbonate, barium sulfate, talc, rosewood, and kaolin. etc. can be used.
[0045] As the ultraviolet absorbing agent, a benzotriazole type, a triazine type, or the like is used. As the light stabilizer, a hindered amine-based light stabilizer or the like can be used. The blocking agent is a compound capable of blocking the carboxyl end group of the polymer. There are no particular limitations on the type of compound, and examples include epoxy compounds, oxazoline compounds, oxazine compounds, and carbamide compounds. These compounds are used as blocking agents for the carboxyl ends of polymers, such as carboxyimide compounds. The compatibilizer may be a polymer type compatibilizer, a low molecular weight organic compound, or an inorganic Compounds, organic-inorganic composites, etc. can be used. These compounding agents may be used alone. Two or more of them may be used in combination.
[0046] <Content> The content of the cellulose ester compound (A) relative to the total mass of the resin composition (X) is 1 It is preferably 0% by mass or more, more preferably 20% by mass or more, and particularly preferably 30% by mass or more. In addition, the content is preferably 80% by mass or less, more preferably 70% by mass or less, and more preferably 60% by mass or less. When the content of the cellulose ester compound (A) is within the above range, The resulting film tends to have good gas permeability and transparency.
[0047] The content of the aliphatic polyester (B) is 3 mass% or less based on the total mass of the resin composition (X). The content is preferably 5% by mass or more, more preferably 5% by mass or more, and particularly preferably 10% by mass or more. It is preferably 0% by mass or less, more preferably 40% by mass or less, and particularly preferably 35% by mass or less. When the content of the aliphatic polyester (B) is within the above range, good gas permeability and It is easy to obtain good flexibility.
[0048] The content of the acrylic polymer (C) is 5% by mass or more based on the total mass of the resin composition (X). It is preferably 10% by mass or more, more preferably 15% by mass or more. % by mass or less is preferable, 60% by mass or less is more preferable, and 50% by mass or less is particularly preferable. When the content of the acrylic polymer (C) is within the above range, when the film is formed, Good mechanical properties are easily obtained. In addition, good gas permeability and transparency are easily obtained.
[0049] The ratio of the cellulose ester compound (A) and the aliphatic polyester compound (B) to the total mass of the resin composition (X) is The total content of the ster (B) is preferably 30% by mass or more, more preferably 40% by mass or more. It is preferably 95% by mass or less, and more preferably 90% by mass or less. It is more preferable that the content is 85 mass % or less, and particularly preferable that the content is 85 mass % or less.
[0050] The ratio of the cellulose ester compound (A) and the aliphatic polyester compound (B) to the total mass of the resin composition (X) is The total content of the styrene (B) and the acrylic polymer (C) is preferably 80% by mass or more, and more preferably 90% by mass or more. It is more preferable that the content is at least 10% by mass. It may be 100% by mass.
[0051] In the resin composition (X), the content of the cellulose ester compound (A) is 100 parts by mass. In this case, the content of the aliphatic polyester (B) is preferably 20 parts by mass or more, and more preferably 30 parts by mass or more. More preferably, the amount is 40 parts by mass or more, and even more preferably, 100 parts by mass or less. The amount of the aliphatic polyether ether is preferably 80 parts by mass or less, more preferably 70 parts by mass or less. When the content of the polyester (B) is equal to or more than the above lower limit, the transparency is good, and when it is equal to or less than the upper limit, When present, the formability of the film is improved.
[0052] In the resin composition (X), the content of the cellulose ester compound (A) is 100 parts by mass. In this case, the content of the acrylic polymer (C) is preferably 20 parts by mass or more, and more preferably 30 parts by mass or more. More preferably, the amount is 40 parts by mass or more, and particularly preferably 40 parts by mass or more. Also, the amount is preferably 400 parts by mass or less. The amount of the acrylic polymer is more preferably 300 parts by mass or less, and particularly preferably 200 parts by mass or less. When the content of the polymer (C) is equal to or more than the above lower limit, good transparency is easily obtained. In this case, good mechanical properties are likely to be obtained.
[0053] <Film manufacturing method> The film of the present embodiment is a polymer film made of a cellulose ester compound (A), an aliphatic polyester (B (C) and an acrylic polymer (C) are molded into a film (film formation) An example of a method for producing a film is shown below. For example, the resin composition (X) is melt extruded by a melt casting method, a T-die method, an inflation method, or the like. The film can be formed by known methods such as the casting method, the calendering method, etc. The T-die method is preferred because of its good operability. The stretching method is uniaxial stretching (machine direction or transverse direction (direction perpendicular to the machine direction)), biaxial stretching (sequential stretching) A stretching step such as secondary biaxial stretching or simultaneous biaxial stretching may be provided. In addition, various structures can be formed on the film surface by known methods such as thermal transfer and etching. This is also fine.
[0054] <Film> The film of this embodiment is made of a resin composition (X). When the resin composition (X) is molded into a film, the components may be denatured. Except for the component modification, the composition of the resin composition (X) is the same as the composition of the film.
[0055] The glass transition temperature of the film of the present embodiment is preferably 40° C. or higher, more preferably 50° C. or higher. It is preferable that the temperature is 60° C. or higher, and more preferable that the temperature is 115° C. or lower, and more preferable that the temperature is 110° C. or lower. When the glass transition temperature is within the above range, the gas permeability is good. The glass transition temperature is measured in accordance with JIS K7244-4 at a strain of 0.1% and a frequency of 1 The loss tangent (t anδ) is the temperature at which the main dispersion peak occurs. When two or more glass transition temperatures are observed It is preferable that the glass transition temperature at which the peak intensity is greatest is within the above range.
[0056] The thickness of the film of this embodiment is preferably 10 μm or more, and more preferably 30 μm or more. The thickness is preferably 50 μm or more, and more preferably 500 μm or less, and more preferably 300 μm or less. It is more preferable that the thickness is 200 μm or less, and further more preferable that the thickness is 200 μm or less. Suitable rigidity can be obtained, and the exterior design can be more satisfactorily imparted.
[0057] The total light transmittance of the film of this embodiment is preferably 80% or more, more preferably 83% or more. It is preferable that the content is 100% or less, and more preferably 99% or less. It is preferable that the content is 98% or less, and more preferable that the content is 98% or less. When the total light transmittance is within the above range, the transparency is good. The total light transmittance was measured according to a method conforming to JIS K7361-1:1997. value.
[0058] The total haze of the film of this embodiment is preferably 90% or less, more preferably 70% or less. When the total haze is within the above range, the transparency is good. The total haze is a value measured by a method conforming to JIS K7136:2000. .
[0059] The oxygen permeability of the film of this embodiment is 1000cc / (m 2 ·24h·atm) or more Preferably, 1500cc / (m 2 ·24h·atm) or more is preferable, 2000cc / (m 2 ·24h·atm) or more is more preferable. Also, 10000cc / (m 2 2 4h·atm) or less is preferable, and 8000cc / (m 2 ·24h·atm) or less is preferable I wish. The nitrogen permeability of the film of this embodiment is 100 cc / (m 2 ·24h · atm) or more Above 200cc / (m 2 24h atm) or higher is preferable. 00cc / (m 2 ·24h·atm) or less is preferable, and 3000cc / (m 2 ·24h· atm or less is more preferable. When the oxygen permeability and nitrogen permeability are equal to or higher than the lower limit, the gas permeability of the film is considered to be good. become. The oxygen permeability and nitrogen permeability are based on JIS K7126-2:2006. Using a gas permeation tester (GC method), the temperature was 25°C and the permeation area was 25cm 2 , gas flow rate 20cm 3 / min, and gas types O2 and N2.
[0060] According to this embodiment, the gas permeability of the film can be improved. The reason is clear. Although it is not certain, the following reasons are possible: In the film of this embodiment, the aliphatic polyester (B) and the acrylic polymer (C) By adding a cellulose ester compound (A), aliphatic polyester (B ) crystallization can be suppressed and the glass transition temperature (Tg) can be lowered, so gas It is believed that the transmission is improved.
[0061] The film of the present embodiment has good transparency. The reason for this is not clear. For example, the following reasons may be considered: Cellulose esterification for aliphatic polyester (B) and acrylic polymer (C) By adding the compound (A), the crystallization of the aliphatic polyester (B) can be suppressed. It is believed that the transparency is improved because the total light transmittance can be increased.
[0062] <Application> The film of the present embodiment has good gas permeability and transparency, and can be applied to the surfaces of various articles. It is suitable as a film to be used in a laminated state. For example, interior and exterior materials for buildings, separation membranes for specific gases, protection for cell culture kits, medical use It can be used as a package for equipment, etc. EXAMPLES
[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, the unit of content is "parts" unless otherwise specified. The units represent "parts by mass."
[0064] [Evaluation method / measurement method] <Total light transmittance, total haze> Total light transmittance is based on JIS K7361-1:1997, and total haze is based on JIS K7136 :2000, using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd.), light source D65, The total light transmittance of the film was measured at a temperature of 25°C.
[0065] <Glass transition temperature> The obtained film was measured using a viscoelastic spectrometer DVA-200 (IT Dynamic strain measurement was performed using a 0.1% strain gauge, a frequency of 10 Hz, and a heating rate of 3°C / min. Temperature dispersion measurement of viscoelasticity (dynamic viscoelasticity measurement according to JIS K7244-4 method) was performed, and the loss tangent The temperature at which the main dispersion peak of (tan δ) occurs was determined as the glass transition temperature. When two or more peaks were observed, the glass transition temperature with the largest peak intensity was shown in Table 1. .
[0066] <Oxygen permeability, nitrogen permeability> The obtained film was subjected to a gas permeability test using a gas permeability tester (GC method) at a temperature of 25°C and Total 25cm 2 , gas flow rate 20cm 3 / min, gas types O2 and N2 under JIS The oxygen permeability and nitrogen permeability were measured with reference to K7126-2.
[0067] <Raw materials> In the following production examples, the abbreviations represent the following raw materials. MMA: Methyl methacrylate n-BA: n-butyl acrylate AMA: Allyl methacrylate 1,3-BD: 1,3-butylene glycol dimethacrylate MA: Methyl acrylate RS610NA: Sodium mono-n-dodecyloxytetraoxyethylene phosphate (phosphate Osphanol RS-610NA: manufactured by Toho Chemical Industry Co., Ltd. CHP: Cumene hydroperoxide t-BH: t-butyl hydroperoxide n-OM: n-octyl mercaptan
[0068] The abbreviations in Table 1 represent the following raw materials. Cellulose ester (A1): Cellulose acetate propionate (CAP), glass Transition temperature: 158℃ Aliphatic polyester (B1): Polybutylene succinate (PBS) Acrylic polymer (C1): Acrylic rubber synthesized in Production Example 1 below Acrylic polymer (C2): Acrylic polymer synthesized in Production Example 2 below
[0069] (Production Example 1: Production of Acrylic Polymer (C1)) A container equipped with a stirrer and a cooler was charged with 8.5 parts of ion-exchanged water (hereinafter, all parts by weight). Then, 0.3 parts of MMA and 4 parts of n-BA were added as (meth)acrylic acid ester (MA1-1). 0.5 parts, 0.2 parts of 1,3-BD and 0.05 parts of AMA as monomer (MA2-1), and A monomer component (Ca1-1) consisting of 0.025 parts of CHP was added as an initiator to the mixture, and the mixture was stirred. Next, 1.1 parts of RS610NA as an emulsifier was added to the above container while stirring. Stirring was continued for 20 minutes to prepare an emulsion containing the monomer component (Ca1-1). Next, 186.5 parts of ion-exchanged water was added to a reaction vessel equipped with a cooler and the temperature was raised to 70°C. Heat it, add 5 parts of ion-exchanged water and SFS (sodium formaldehyde sulfoxylate) 0.20 parts, ferrous sulfate 0.0001 parts, EDTA (disodium ethylenediaminetetraacetate The mixture was then added in one portion without stirring under nitrogen. Then, the emulsion containing the monomer component (Ca1-1) was dropped into the reaction vessel over a period of 8 minutes. The reaction was continued for 15 minutes to obtain a polymer consisting of the monomer component (Ca1-1). Next, MMA1. 5 parts and n-BA22.5 parts, 1,3-BD1.0 part as monomer (MA2-2) and A A monomer component (Ca1-) consisting of 0.25 parts of MA and 0.016 parts of CHP as an initiator After adding 2) over 90 minutes, the reaction was continued for 60 minutes to obtain a polymer (Ca1). The Tg of the polymer (Ca1) was -47°C. Next, 6.0 parts of MMA and nB A4.0 parts, AMA0.075 parts as monomer (MC2-1), and CH A monomer component (Cc1-1) consisting of 0.013 parts of P was added dropwise to the reaction vessel over a period of 45 minutes. The reaction was continued for 60 minutes to form an intermediate polymer. The Tg of the polymer (Cc1) composed of 1) was 20°C. Next, 55.2 parts of MMA and n- BA 4.8 parts, n-OM 0.22 parts as chain transfer agent, and t-BH 0.01 parts as initiator. 0.75 parts of monomer component (Cb1-1) was added dropwise to the reaction vessel over a period of 140 minutes. The reaction was continued for 60 minutes to obtain a latex of acrylic polymer (C1). The Tg of the polymer (Cb1) composed of the monomer component (Cb1-1) was 84°C. The obtained latex of the acrylic polymer (C1) was filtered through a SUS mesh (average mesh size) After filtering using a vibrating filter equipped with a 62 μm aperture, the mixture was diluted with 3 parts calcium acetate. The resulting product was salted out in an aqueous solution containing 1,000 ppm of acrylic acid, washed with water, recovered, and then dried to obtain a powdery acrylic polymer (C1). The average particle size of the acrylic polymer (C1) is 0.12 μm, Mw is 59,000, and the temperature is 200° C. The melt viscosity at 1000 Pa·s was 16,000 Pa·s.
[0070] (Production Example 2: Production of Acrylic Polymer (C2)) An acrylic polymer (C) consisting of 87 parts of methyl methacrylate and 13 parts of methyl acrylate 2) was produced by known suspension polymerization. The Mw of the acrylic polymer (C2) was 100,000. The melt viscosity at 200°C was 5,890 Pa·s.
[0071] <Examples 1 to 4, Reference Example 1, Comparative Examples 1 to 4> The cellulose ester compound (A), the lipid, and the like were mixed together to obtain the composition shown in Table 1 (unit: mass %). The aliphatic polyester (B) and the acrylic polymer (C) were dry blended. The mixture was kneaded at 220°C using a 25 mm co-rotating twin screw extruder, and the resin composition (X) was extruded through a T-die. The mixture was then extruded, and then quenched with a casting roll at about 80°C to produce a film having a thickness of 100 μm. We created a room. The evaluation results of various properties of the obtained film are shown in Table 1.
[0072] [Table 1]
[0073] As shown in the results in Table 1, the films of Examples 1 to 4 have a total light transmittance of 90% or more. The film had a low glass transition temperature of 115°C or less. Therefore, it has high oxygen permeability and nitrogen permeability, and has excellent gas permeability.
Claims
1. A cellulose ester compound (A), an aliphatic polyester (B), and an acrylic polymer ( C), and the film is made of a resin composition containing the cellulose ester compound (A) 1 00 parts by mass, and the acrylic polymer (C) is 20 parts by mass or more and 400 parts by mass or less. According to JIS K7244-4, strain is 0.1%, frequency is 10 Hz, and heating rate is 3°C / min. The glass transition temperature (Tg) of the film measured by the method is 60° C. or more and 115° C. or less. Hmm.
2. The content of the cellulose ester compound (A) relative to the total mass of the resin composition is 1 The film according to claim 1 , wherein the content is 0% by weight or more and 60% by weight or less.
3. The content of the aliphatic polyester (B) relative to the total mass of the resin composition is 10 mass %.
2. The film according to claim 1, wherein the content of the polyimide is from 0.1 to 50% by weight.
4. The content of the acrylic polymer (C) is 10% by mass or more based on the total mass of the resin composition. The film according to claim 1 , wherein the moisture content is at least 70% by weight.
5. The aliphatic polyester (B) comprises a structural unit derived from an aliphatic polycarboxylic acid and an aliphatic polycarboxylic acid. The film according to claim 1 , which is a polymer having structural units derived from an alcohol.
6. The film according to claim 1 , having a total light transmittance of 90% or more.
7. Oxygen permeability is 1000 to 10000cc / (m 2 24h atm) according to claim 1 The film according to claim 1.
8. Nitrogen permeability is 100 to 5000 cc / (m 224h atm) according to claim 1. Film featured.
Citation Information
Patent Citations
Cellulose ester film, hard coat film and antireflection film
JP2005054100A