Anionically modified cellulose nanofiber, and additive and haze improver that contain anionically modified cellulose nanofiber

Anion-modified cellulose nanofibers with high haze are developed by carboxymethylation and oxidation, addressing the need for novel characteristics and enhancing their applicability in matte or cloudy designs.

JP2024148826APending Publication Date: 2024-10-18NIPPON PAPER IND CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023062303
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing cellulose nanofibers lack novel characteristics that could expand their applications beyond their known properties of high thixotropy and water retention.

Method used

Development of anion-modified cellulose nanofibers with high haze, characterized by a total light transmittance of 85.0% or more and a haze of 50.0% or more, achieved through methods such as carboxymethylation and oxidation to introduce anionic groups, followed by defibration to nano-scale fiber diameters.

Benefits of technology

The anion-modified cellulose nanofibers exhibit high haze, making them suitable for applications requiring matte or cloudy designs, such as paints, inks, cosmetics, and films, and can be used as haze improvers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148826000001
    Figure 2024148826000001
Patent Text Reader

Abstract

To provide anionically modified cellulose nanofiber having novel characteristics.SOLUTION: A water dispersion of anionically modified cellulose nanofiber (solids 0.5% (w / v)) is prepared, poured into a silicon frame placed on a polyethylene terephthalate film to be 0.2 g / cm2, and dried at 50°C to produce a film; the total light transmittance and the diffuse transmittance are measured; the haze is calculated as the ratio of the diffuse transmittance to 100% of the total light transmittance; then the total light transmittance is 85.0% or more and the haze is 50.0% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anionically modified cellulose nanofiber. More specifically, the present invention relates to an anionically modified cellulose nanofiber having high haze. The present invention also relates to an additive and a haze enhancer containing an anionically modified cellulose nanofiber having high haze. [Background technology]

[0002] It is known that when anionic groups such as carboxyl groups and carboxymethyl groups are introduced into cellulose molecular chains and mechanically treated (defibrated), the cellulose can be converted into cellulose nanofibers having a nanoscale fiber width with an average fiber width of less than 500 nm (Patent Documents 1 and 2). In particular, cellulose nanofibers with a fiber diameter of around 4 nm correspond to single microfibrils, which are the basic units of cellulose bundles in plant cell walls. Such cellulose nanofibers have high thixotropy and water retention properties and can be used in a variety of fields. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-1728 A [Patent Document 2] International Publication No. 2014 / 088072 Summary of the Invention [Problem to be solved by the invention]

[0004] In order to apply cellulose nanofibers to various applications, it is preferable to develop cellulose nanofibers with novel characteristics. An object of the present invention is to provide anion-modified cellulose nanofibers with novel characteristics. Another object of the present invention is to provide an additive that utilizes the characteristics. [Means for solving the problem]

[0005] As a result of extensive investigations, the present inventors have produced anion-modified cellulose nanofibers having high haze. The present invention includes, but is not limited to, the following. [1] Anion-modified cellulose nanofiber having a total light transmittance of 85.0% or more and a haze of 50.0% or more, measured by the following method: A water dispersion of anion-modified cellulose nanofiber (solid content 0.5% (w / v)) was prepared and placed at 0.2 g / cm in a silicone frame placed on a polyethylene terephthalate film. 2 The mixture is poured into a film so that the thickness becomes 100 μm, and then dried at 50° C. to produce a film, and the total light transmittance and diffuse transmittance are measured. Next, the haze is calculated as a ratio of the diffuse transmittance when the total light transmittance is taken as 100%. [2] The anion-modified cellulose nanofiber according to [1], wherein the anion-modified cellulose nanofiber is a carboxymethylated cellulose nanofiber. [3] The anion-modified cellulose nanofiber according to [1] or [2], having an average fiber diameter of 3 to 500 nm and an aspect ratio of 10 to 1,000. [4] The anion-modified cellulose nanofiber according to [2] or [3], having a degree of carboxymethyl substitution in the range of 0.01 to 0.50 and a degree of crystallinity of cellulose type I of 50% or more. [5] An additive comprising the anion-modified cellulose nanofiber according to any one of [1] to [4]. [6] A haze enhancer comprising the anion-modified cellulose nanofiber according to any one of [1] to [4]. Effect of the Invention

[0006] The anion-modified cellulose nanofiber of the present invention has high haze. A material with high haze can eliminate gloss and impart a matte finish or impart a cloudy appearance, and therefore it is believed that the material can be used as an additive for paints and inks for imparting such design properties, as well as for cosmetics, films, liquid crystals, and the like, particularly as a haze enhancer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention relates to anion-modified cellulose nanofibers (hereinafter, "cellulose nanofibers" will be referred to as "CNF") having a total light transmittance of 85.0% or more and a haze of 50.0% or more, measured by the method described below.

[0008] <Anion-modified CNF> Anion-modified CNF is anion-modified cellulose obtained by introducing anionic groups into the hydroxyl groups of cellulose, which is defibrated to have a fiber diameter of nano-order. The average fiber diameter of the anion-modified CNF used in the present invention is preferably 3 to 500 nm, more preferably 5 to 150 nm, more preferably 10 to 100 nm, more preferably 10 to 50 nm, and more preferably 10 to 20 nm. The fiber diameter of the anion-modified CNF can be determined by measuring the cross-sectional height of the shape image of the fiber observed using an atomic force microscope (AFM). In addition, the average fiber diameter of the anion-modified CNF can be determined by measuring the fiber diameter of 50 randomly selected fibers by the above-mentioned method and calculating the length-weighted average fiber diameter.

[0009] The aspect ratio of the anion-modified CNF is preferably 10 to 1000, and more preferably 10 to 500. The average fiber length of the anion-modified CNF can be determined by measuring the fiber lengths of 200 randomly selected fibers using an atomic force microscope (AFM) and calculating the length-weighted average fiber length, and the aspect ratio of the anion-modified CNF can be determined by the following formula using the above-mentioned average fiber length and average fiber diameter: Aspect ratio = average fiber length (nm) / average fiber diameter (nm).

[0010] <Anion modification> When producing the anion-modified CNF of the present invention, the raw cellulose fiber is first anion-modified to obtain anion-modified cellulose. The types of anion modification include, but are not limited to, oxidation (also called carboxylation) in which a carboxyl group is introduced into the cellulose chain, carboxyalkylation in which a carboxyalkyl group such as a carboxymethyl group (hereinafter, "carboxymethyl" is referred to as "CM") is ether-bonded to the cellulose chain, and phosphate esterification in which a phosphate group is introduced into the cellulose chain. Among them, carboxyalkylation is preferred because it can obtain CNF with high haze even when the degree of defibration is increased, and in particular, CMization is most preferred.

[0011] Anion-modified cellulose may take a form in which an anion group such as a carboxyl group, a CM group, or a phosphate group has a metal ion such as a sodium ion or a potassium ion as a counter ion (this form is called "salt-type anion-modified cellulose"). In this specification, anion-modified cellulose also includes salt-type anion-modified cellulose. Anion-modified CNF also includes salt-type anion-modified CNF. In contrast to salt-type anion-modified cellulose, when the anion group has a proton as a counter ion, it is called "hydrogen-type anion-modified cellulose".

[0012] The anion-modified cellulose used in producing the anion-modified CNF of the present invention maintains at least a part of the fibrous shape of cellulose even when dispersed in water. That is, when an aqueous dispersion of anion-modified cellulose is observed with an electron microscope or the like, a fibrous substance can be observed, and when measured by X-ray diffraction, a peak of cellulose type I crystals can be observed.

[0013] The cellulose as a raw material for obtaining anion-modified cellulose is not particularly limited, and examples thereof include those derived from plants, animals (e.g., ascidians), algae, and microorganisms (e.g., acetic acid bacteria (Acetobacter)). Examples of those derived from plants include wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, and pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), softwood dissolving pulp, hardwood dissolving pulp, recycled pulp, waste paper, etc.). In addition, cellulose powder obtained by pulverizing the above-mentioned cellulose raw material may be used. As the cellulose raw material, any one or a combination of these may be used, but cellulose fibers derived from plants or microorganisms are preferred, cellulose fibers derived from plants are more preferred, and wood-based pulp is even more preferred.

[0014] In order to obtain an anion-modified cellulose having a cellulose type I crystal peak, it is preferable to use cellulose having a high crystallinity of cellulose type I as a raw material. The crystallinity of the cellulose type I of the cellulose raw material is preferably 50% or more, more preferably 60% or more. The method for measuring the crystallinity of cellulose type I will be described later.

[0015] <Anion modification - Carboxyalkylation> An example of anion modification is carboxyalkylation, in which a carboxyalkyl group such as a CM group is ether-bonded to a cellulose chain. In this specification, carboxyalkylated cellulose is called "carboxyalkylated cellulose". Also, CM-modified cellulose is called "CM-modified cellulose". As the carboxyalkylated cellulose, commercially available products may be used, or the cellulose raw material may be produced by carboxyalkylating the above-mentioned cellulose raw material by a known method. The degree of carboxyalkyl substitution per anhydrous glucose unit of cellulose is preferably 0.01 to 0.50. The upper limit is preferably 0.40 or less. If the degree of carboxyalkyl substitution exceeds 0.50, dissolution in water occurs easily, and the fiber form cannot be maintained in water. In order to obtain the effect of carboxyalkylation, it is necessary to have a certain degree of substitution. For example, if the degree of substitution is less than 0.02, depending on the application, the advantage of introducing a carboxyalkyl group may not be obtained. Therefore, the degree of carboxyalkyl substitution is preferably 0.02 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The degree of carboxyalkyl substitution can be adjusted by controlling the amount of the carboxyalkylating agent to be reacted, the amount of the mercerizing agent, the composition ratio of water to the organic solvent, and the like.

[0016] In this specification, anhydroglucose unit means each anhydroglucose (glucose residue) constituting cellulose. In addition, the degree of carboxyalkyl substitution (also called the degree of etherification) indicates the ratio of hydroxyl groups in the glucose residues constituting cellulose that are substituted with carboxyalkyl ethers (the number of carboxyalkyl ethers per glucose residue). The degree of carboxyalkyl substitution is sometimes abbreviated as DS.

[0017] The method for determining the degree of carboxyalkyl substitution is as follows: Weigh out approximately 2.0 g of the sample and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of nitric acid methanol (a solution of 100 mL of concentrated nitric acid added to 1000 mL of methanol) and shake for 3 hours to convert the salt-type carboxyalkylated cellulose to hydrogen-type carboxyalkylated cellulose. Weigh out 1.5 to 2.0 g of hydrogen-type carboxyalkylated cellulose (absolutely dry) and place it in a 300 mL Erlenmeyer flask with a stopper. Moisten with 15 mL of 80% methanol, add 100 mL of 0.1 N-NaOH, and shake at room temperature for 3 hours. Using phenolphthalein as an indicator, back-titrate the excess NaOH with 0.1 N-H2SO4, and calculate the degree of carboxyalkyl substitution (DS) using the following formula. A = [(100 × F'-0.1N-H2SO4 (mL) × F) × 0.1] / (bone-dry mass of hydrogen-type carboxyalkylated cellulose (g)) Degree of carboxyalkyl substitution (DS) = 0.162 x A / (1-0.058 x A) F': Factor of 0.1N-H2SO4 F: Factor of 0.1N NaOH.

[0018] The DS of carboxyalkylated cellulose and the DS of carboxyalkylated CNF obtained by defibrating carboxyalkylated cellulose are usually the same. As an example of a method for producing carboxyalkylated cellulose, an example for producing carboxyalkylated cellulose will be described below.

[0019] First, the cellulose raw material is mixed with a solvent and a mercerizing agent, and the cellulose raw material is mercerized at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Next, the mercerizing agent is added in an amount of 0.05 to 10.0 times the moles per glucose residue, and mercerization is performed at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.

[0020] As the solvent, 3 to 20 times by mass of water or an organic solvent or a mixture thereof can be used. Examples of the organic solvent include, but are not limited to, alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, isobutanol, and tertiary butanol, ketones such as acetone, diethyl ketone, and methyl ethyl ketone, as well as dioxane, diethyl ether, benzene, and dichloromethane. Among these, monohydric alcohols having 1 to 4 carbon atoms are preferred because of their excellent compatibility with water, and monohydric alcohols having 1 to 3 carbon atoms are more preferred. As the mercerizing agent, it is preferred to use 0.5 to 20 times by mole of an alkali metal hydroxide per anhydrous glucose residue of the cellulose raw material, specifically sodium hydroxide or potassium hydroxide. Examples of the mercerizing agent include monochloroacetic acid, sodium monochloroacetate, methyl monochloroacetate, ethyl monochloroacetate, and isopropyl monochloroacetate. Among these, monochloroacetic acid or sodium monochloroacetate is preferred in terms of the ease of availability of the raw material. The amount of the CM agent used is not particularly limited, but is preferably added in the range of 0.5 to 1.5 mol per anhydrous glucose unit of cellulose. The lower limit of the above range is more preferably 0.6 mol or more, and even more preferably 0.7 mol or more, and the upper limit is more preferably 1.3 mol or less, and even more preferably 1.1 mol or less. The CM agent may be added to the reactor as, for example, a 5 to 80 mass % and more preferably a 30 to 60 mass % aqueous solution, but is not limited thereto, or may be added in a powder state without being dissolved in a solvent such as water.

[0021] When monochloroacetic acid or sodium monochloroacetate is used as the CM agent, the molar ratio of the mercerizing agent to the CM agent (mercerizing agent / CM agent) is generally set to 0.90 to 2.45. This is because if it is less than 0.90, the CM reaction may be insufficient, and unreacted monochloroacetic acid or sodium monochloroacetate may remain and be wasted, and if it exceeds 2.45, a side reaction between the excess mercerizing agent and monochloroacetic acid or sodium monochloroacetate may proceed, resulting in the production of an alkali metal glycolate, which may be uneconomical.

[0022] When mercerizing raw cellulose, generally, there are two methods: one in which both mercerization and CM are carried out in a solvent mainly composed of water (aqueous method), and the other in which both mercerization and CM are carried out in a mixed solvent of water and an organic solvent (solvent method). Either method may be used. Alternatively, a solvent mainly composed of water may be used for mercerization, and a mixed solvent of an organic solvent and water may be used for CM. By doing so, it is possible to economically obtain CM-modified cellulose in which CM groups are introduced uniformly, not locally, even when the crystallinity of the cellulose is maintained at 50% or more.

[0023] A solvent that mainly uses water (a solvent that is mainly made of water) refers to a solvent that contains water at a ratio of more than 50% by mass. The amount of water in the solvent that is mainly made of water is preferably 55% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. Particularly preferably, the solvent that is mainly made of water is 100% by mass (i.e., water). The higher the amount of water during mercerization, the more advantageously the CM group is introduced more uniformly into the cellulose. As the solvent other than water in the solvent that is mainly made of water (used in a mixture with water), the organic solvents described above can be used. The amount of the organic solvent in the solvent that is mainly made of water is preferably 45% by mass or less, more preferably 40% by mass or less, more preferably 30% by mass or less, more preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and more preferably 0% by mass.

[0024] It is preferable to add an organic solvent or an aqueous solution of an organic solvent to the reactor simultaneously with the addition of the CM agent, or before or immediately after the addition of the CM agent, or to reduce the amount of organic solvent other than water used in the mercerization treatment by reducing pressure or the like to form a mixed solvent of water and an organic solvent, and to allow the CM reaction to proceed in this mixed solvent of water and an organic solvent. The timing of adding or reducing the organic solvent may be any time between the end of the mercerization reaction and just after the addition of the CM agent, and is not particularly limited, but is preferably within 30 minutes before or after the addition of the CM agent, for example.

[0025] The ratio of the organic solvent in the mixed solvent during CMization is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more, based on the total of water and organic solvent. The higher the ratio of the organic solvent, the more uniform the CM group substitution is, and the more stable the quality of the obtained CM-modified cellulose is. There is no upper limit to the ratio of the organic solvent, and it may be, for example, 99% by mass or less. In consideration of the cost of the organic solvent to be added, it is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less.

[0026] The reaction medium for CM (a mixed solvent of water and an organic solvent, etc., not containing cellulose) preferably has a lower proportion of water (in other words, a higher proportion of organic solvent) than the reaction medium for mercerization. By satisfying this range, the crystallinity of the resulting CM-cellulose is easily maintained. In addition, when the reaction medium for CM has a lower proportion of water (a higher proportion of organic solvent) than the reaction medium for mercerization, there is also an advantage that when transferring from the mercerization reaction to the CM reaction, a mixed solvent for the CM reaction can be formed by the simple means of adding a desired amount of organic solvent to the reaction system after the mercerization reaction is completed.

[0027] <Anion modification-oxidation> An example of anion modification is oxidation (carboxylation) in which a carboxyl group is introduced into a cellulose chain. In this specification, carboxylated cellulose is referred to as "oxidized cellulose." As the oxidized cellulose, commercially available products may be used, or it may be produced by oxidizing the above-mentioned cellulose raw material by a known method. The amount of carboxyl groups is preferably 0.1 to 2.5 mmol / g, more preferably 0.6 mmol / g to 2.5 mmol / g, and even more preferably 1.0 mmol / g to 2.0 mmol / g, based on the bone dry mass of the oxidized cellulose.

[0028] The amount of carboxyl groups in oxidized cellulose can be measured by the following method: 60 ml of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose is prepared, and a 0.1 M aqueous hydrochloric acid solution is added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution is then added dropwise and the electrical conductivity is measured until the pH reaches 11. The electrical conductivity is calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual: Amount of carboxyl groups [mmol / g oxidized cellulose] = a [ml] × 0.05 / mass of oxidized cellulose [g].

[0029] The amount of carboxyl groups in oxidized cellulose is usually the same as the amount of carboxyl groups in oxidized CNF obtained by defibrating oxidized cellulose. One example of the oxidation method is a method in which the cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, and mixtures thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, resulting in the formation of aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO - The concentration of the cellulose raw material during the reaction is not particularly limited, but is preferably 5% by mass or less.

[0030] The term "N-oxyl compound" refers to a compound capable of generating nitroxy radicals. Any compound that can promote the target oxidation reaction can be used as the N-oxyl compound. Examples include 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO). The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the cellulose raw material. For example, 0.01 to 10 mmol is preferable, 0.01 to 1 mmol is more preferable, and 0.05 to 0.5 mmol is even more preferable, per 1 g of bone-dry cellulose raw material. In addition, the amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.

[0031] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose raw material.

[0032] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, peroxide, etc. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The appropriate amount of the oxidizing agent to be used is, for example, preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, further preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose raw material. Also, for example, 1 to 40 mol is preferable per 1 mol of the N-oxyl compound.

[0033] The oxidation process of the cellulose raw material can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose chain, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably about 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions. The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually 0.5 to 6 hours, for example, about 0.5 to 4 hours.

[0034] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.

[0035] Another example of the oxidation method is a method in which the cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 It is preferable that the thickness is 50 to 220 g / m 3 It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and is preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, the cellulose raw material can be prevented from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.

[0036] The amount of carboxyl groups in the oxidized cellulose can be adjusted by controlling the reaction conditions, such as the amount of the oxidizing agent added and the reaction time. <Anion modification - phosphate esterification> An example of anionic modification is phosphorylation, which introduces a phosphate group into a cellulose chain. In this specification, phosphorylated cellulose is referred to as "phosphated cellulose". As the phosphated cellulose, commercially available products may be used, or it may be produced by phosphorylating the above-mentioned cellulose raw material by a known method. The degree of phosphate substitution per glucose unit of the phosphated cellulose is preferably 0.001 or more and less than 0.40. The degree of phosphate substitution in the phosphated cellulose and the degree of phosphate substitution in the phosphated CNF obtained by defibrating the phosphated cellulose are usually the same.

[0037] Examples of the method of phosphate esterification include a method of mixing a powder or an aqueous solution of a compound having a phosphoric acid group with a cellulose raw material, and a method of adding an aqueous solution of a compound having a phosphoric acid group to a slurry of a cellulose raw material. Examples of the compound having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. Phosphate groups can be introduced into the cellulose raw material by using one or more of these in combination. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are preferred from the viewpoints of high efficiency of phosphoric acid group introduction and easy industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is desirable to use the compound having a phosphoric acid group as an aqueous solution, since the reaction can proceed uniformly and the efficiency of phosphoric acid group introduction is high. The pH of the aqueous solution of the compound having a phosphate group is preferably 7 or less since this increases the efficiency of introducing the phosphate group, but is preferably 3 to 7 from the viewpoint of suppressing hydrolysis of the fibers.

[0038] Specific examples of methods for producing cellulose phosphate include the following. A compound having a phosphate group is added to a suspension of a cellulose raw material having a solid content concentration of 0.1 to 10% by mass while stirring to introduce phosphate groups into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of the compound having a phosphate group added is preferably 0.2 to 500 parts by mass, more preferably 1 to 400 parts by mass, in terms of phosphorus element amount.

[0039] After the obtained suspension of cellulose phosphate is dehydrated, from the viewpoint of suppressing hydrolysis of cellulose, it is preferably heat-treated at 100 to 170° C. Furthermore, it is preferable to heat at 130° C. or less, preferably 110° C. or less while water is contained during the heat treatment, and to heat at 100 to 170° C. after the water is removed.

[0040] <Defibrillation> For example, anion-modified CNF can be obtained by defibrating the anion-modified cellulose obtained by the above method to a fiber diameter of the nano-order. The device used for defibration is not particularly limited, and for example, a device capable of applying a strong shear force, such as a high-pressure type, high-speed rotation type, colloid mill type, roll mill type, ultrasonic type, or cavitation type, a disk-type, conical-type, or cylinder-type refiner, a high-pressure homogenizer, a colloid mill, a high-pressure jet disperser, a beater, a PFI mill, a kneader, or a disperser, can be used.

[0041] Defibration is preferably performed in a wet manner (i.e., in the form of a dispersion in which water or the like is used as a dispersion medium). When performing wet defibration, a dispersion of anionically modified cellulose is prepared. The solids concentration in the dispersion of anionically modified cellulose to be used for defibration is preferably 0.1% by mass or more, and more preferably 0.5% by mass or more. The upper limit of the concentration is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 10% by mass or less, and even more preferably 8% by mass or less. The dispersion medium is preferably water.

[0042] As described below, defibration is carried out so that the resulting CNF has a total light transmittance of 85.0% or more and a haze of 50.0% or more. To obtain such anion-modified CNF, it is preferable to adjust the defibration conditions so that the transparency of a 1% (w / v) anion-modified cellulose dispersion does not exceed 50%.

[0043] <Total light transmittance and haze> The anion-modified CNF of the present invention has a total light transmittance of 85.0% or more and a haze of 50.0% or more, as measured by the following method. The measurement method is as follows: A water dispersion of anion-modified cellulose nanofiber (solid content 0.5% (w / v)) was prepared and placed at 0.2 g / cm in a silicone frame placed on a polyethylene terephthalate film. 2 The mixture is poured so that the thickness becomes equal to or less than 100 mm. The mixture is dried at 50°C to prepare a film (test piece), and the total light transmittance and diffuse transmittance are measured. A haze meter such as Haze Meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.) can be used to measure the total light transmittance and diffuse transmittance. The total light transmittance is the transmittance of light rays that pass through the test piece, including both parallel and diffuse components, and the diffuse transmittance is the transmittance of light rays that pass through the test piece, corresponding to the diffuse components excluding the parallel components. Next, the haze is calculated as the percentage of the diffuse transmittance when the total light transmittance is taken as 100%. That is, the haze is calculated by the following formula: Haze = (Diffuse transmittance / Total light transmittance) x 100.

[0044] The total light transmittance of the anion-modified CNF of the present invention measured by the above-mentioned method is 85.0% or more, more preferably 88.0% or more. The haze is 50.0% or more, more preferably 55.0% or more. The anion-modified CNF of the present invention has a high haze, and therefore can be suitably used as an additive to paints, inks, cosmetics, films, liquid crystals, etc., intended to give a matte finish by removing gloss, or to apply a design that imparts cloudiness. In addition, it can be suitably used as a haze enhancer for improving the haze of these materials.

[0045] <Other> The degree of crystallinity of the cellulose in the anion-modified CNF of the present invention is preferably 50% or more, more preferably 60% or more, for crystalline type I. The crystallinity of cellulose can be controlled by the degree of anion modification. There is no particular upper limit to the degree of crystallinity of cellulose type I. In reality, the upper limit is thought to be about 90%.

[0046] The method for measuring the crystallinity of cellulose type I of anion-modified CNF is as follows: The sample is placed in a glass cell and measured using an X-ray diffraction measuring device (product name: LabX XRD-6000, manufactured by Shimadzu Corporation). The degree of crystallinity is calculated using the method of Segal et al., and is calculated from the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous part at 2θ = 18.5° using the diffraction intensity of the X-ray diffraction pattern at 2θ = 10° to 30° as the baseline, according to the following formula.

[0047] Xc = (I002c - Ia) / I002c x 100 Xc = Crystallinity of cellulose type I (%) I002c: 2θ=22.6°, diffraction intensity of 002 plane Ia: 2θ=18.5°, diffraction intensity of the amorphous part.

[0048] The anion-modified CNF of the present invention preferably has a transmittance of light with a wavelength of 660 nm (hereinafter referred to as "transparency") of 50% or less when dispersed in water with a solid content of 1% (w / v). The transparency may be 20% or less, or may be 10% or less. Transparency indicates the degree of defibration, and generally it can be considered that defibration is more advanced when the transparency is high. In the present invention, transparency can be measured by the following method: An aqueous dispersion of anion-modified CNF (solid content concentration: 1% by mass) is prepared, and the transmittance of light with a wavelength of 660 nm is measured using a UV-VIS spectrophotometer UV-1800 (manufactured by Shimadzu Corporation) with a square cell with an optical path length of 10 mm.

[0049] The anion-modified CNF of the present invention may be in the form of a dispersion obtained after production, but may be dried or redispersed in water as necessary. The drying method is not particularly limited, and known methods such as freeze drying, spray drying, tray drying, drum drying, belt drying, thin spreading on a glass plate or the like and drying, fluidized bed drying, microwave drying, and heated fan reduced pressure drying can be used. After drying, the CNF may be pulverized with a cutter mill, hammer mill, pin mill, jet mill, or the like as necessary. The method of redispersing in water is also not particularly limited, and known dispersing devices can be used.

[0050] <Application> Since the anion-modified CNF of the present invention has a high haze, it is considered that it can be used particularly optimally as a material for removing gloss and imparting a matte feel, or as an additive for imparting haze (haze enhancer), although this is not limited thereto. However, it may also be used for other purposes. The field in which the anion-modified CNF is used is not limited, and it is considered that it can be used in various fields in which additives are generally used, such as food, paint, ink, cosmetics, film, liquid crystal, various chemical products, sprays, feed, medicine, papermaking, agricultural chemicals, civil engineering, construction, electronic materials, flame retardants, household goods, adhesives, cleaning agents, fragrances, lubricating compositions, etc.

[0051] For example, an additive containing the anion-modified CNF of the present invention can be added to impart a matte or cloudy design to paints, inks, cosmetics, films, liquid crystals, etc. The amount of anion-modified CNF added to these can be appropriately selected depending on the expected effect, but is preferably 0.1 to 30 mass%, more preferably 0.5 to 20 mass%, and even more preferably 0.5 to 10 mass%. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In addition, parts and % indicate parts by mass and % by mass, unless otherwise specified.

[0053] <Example 1> In a 5L twin-shaft kneader with the rotation speed adjusted to 100 rpm, 1089 parts of isopropanol (IPA) and 242 parts of sodium hydroxide dissolved in 121 parts of water were added, and 200 parts of hardwood pulp (manufactured by Nippon Paper Industries Co., Ltd., LBKP) were added in terms of dry mass when dried at 100 ° C for 60 minutes. The mixture was stirred and mixed at 30 ° C for 60 minutes to prepare mercerized cellulose. 484 parts of sodium monochloroacetate were further added while stirring, and after stirring at 30 ° C for 30 minutes, the mixture was heated to 70 ° C over 30 minutes and subjected to CM reaction at 70 ° C for 60 minutes. The proportion of water in the reaction medium during the mercerization reaction and CM reaction was 10 mass %. After the reaction was completed, the mixture was neutralized, washed with 65% water-containing methanol, deliquored, dried, and pulverized to obtain a sodium salt of CM-modified cellulose with a CM substitution degree of 0.17 and a crystallinity of cellulose I type of 64%.

[0054] The obtained sodium salt of carboxymethyl cellulose was dispersed in water to obtain a 1% (w / v) aqueous dispersion. This was treated three times with a high-pressure homogenizer at 150 MPa to obtain an aqueous dispersion of carboxymethyl cellulose (CNF). The obtained carboxymethyl cellulose (CNF) had an average fiber diameter of 15 nm and an aspect ratio of 41.

[0055] The obtained aqueous dispersion of carboxymethylated CNF was diluted with water to obtain an aqueous dispersion with a solid content of 0.5% (w / v), and then a film was produced by the method described above. The total light transmittance and diffuse transmittance were measured by the method described above, and the haze was calculated. In addition, the transparency of an aqueous dispersion of carboxymethylated CNF with a solid content of 1% (w / v) was measured by the method described above. The results are shown in Table 1.

[0056] <Example 2> In a twin-shaft kneader adjusted to a rotation speed of 100 rpm, 130 parts of water and 20 parts of sodium hydroxide dissolved in 100 parts of water were added, and 100 parts of hardwood pulp (manufactured by Nippon Paper Industries Co., Ltd., LBKP) was added in terms of dry mass when dried at 100 ° C for 60 minutes. The mixture was stirred and mixed at 30 ° C for 90 minutes to prepare mercerized cellulose. Further, 230 parts of IPA and 60 parts of sodium monochloroacetate were added while stirring, and after stirring for 30 minutes, the mixture was heated to 70 ° C and subjected to CM reaction for 90 minutes. The concentration of IPA in the reaction medium during the CM reaction was 50%. After the reaction was completed, the mixture was neutralized, deliquored, dried, and pulverized to obtain a sodium salt of CM-modified cellulose with a CM substitution degree of 0.31 and a crystallinity of cellulose I type of 67%.

[0057] The obtained sodium salt of carboxymethyl cellulose was dispersed in water to obtain a 1% (w / v) aqueous dispersion. This was treated once with a high-pressure homogenizer at 150 MPa to obtain an aqueous dispersion of carboxymethyl cellulose (CNF). The obtained carboxymethyl cellulose (CNF) had an average fiber diameter of 10 nm and an aspect ratio of 50.

[0058] The total light transmittance, diffuse transmittance, haze, and transparency of the obtained carboxymethylated CNF were measured in the same manner as in Example 1. The results are shown in Table 1. <Example 3> 500g (bone dry) of bleached unbeaten kraft pulp (brightness 85%) derived from coniferous trees was added to 500mL of an aqueous solution containing 780mg of TEMPO (Sigma Aldrich) and 75.5g of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system to a concentration of 6.0mmol / g to initiate the oxidation reaction. The pH of the system decreased during the reaction, but 3M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain pulp with carboxyl groups introduced (oxidized cellulose). The amount of carboxyl groups in this oxidized cellulose was 1.42mmol / g, and the crystallinity of cellulose type I was 70%.

[0059] The oxidized pulp was diluted with water to a solids concentration of 3% by mass, and then subjected to two passes in a cavitation jet device at 14 MPa to obtain oxidized CNF. The obtained oxidized CNF had an average fiber diameter of 15 nm and an aspect ratio of 60.

[0060] The total light transmittance, diffuse transmittance, haze, and transparency of the obtained oxidized CNF were measured in the same manner as in Example 1. The results are shown in Table 1. <Comparative Example 1> Except for changing the number of times of treatment with the high-pressure homogenizer to two, an aqueous dispersion of carboxymethylated CNF was obtained in the same manner as in Example 2. The obtained carboxymethylated CNF had an average fiber diameter of 4 nm and an aspect ratio of 55.

[0061] The total light transmittance, diffuse transmittance, haze, and transparency of the obtained carboxymethylated CNF were measured in the same manner as in Example 1. The results are shown in Table 1. <Comparative Example 2> An aqueous dispersion of carboxymethylated CNF was obtained in the same manner as in Example 2, except that the number of times of treatment with the high-pressure homogenizer was changed to 5. The obtained carboxymethylated CNF had an average fiber diameter of 3 nm and an aspect ratio of 40.

[0062] The total light transmittance, diffuse transmittance, haze, and transparency of the obtained carboxymethylated CNF were measured in the same manner as in Example 1. The results are shown in Table 1. <Comparative Example 3> An aqueous dispersion of oxidized CNF was obtained in the same manner as in Example 3, except that the number of treatment passes in the cavitation jet device was changed to 10 passes. The obtained oxidized CNF had an average fiber diameter of 4 nm and an aspect ratio of 150.

[0063] The total light transmittance, diffuse transmittance, haze, and transparency of the obtained oxidized CNF were measured in the same manner as in Example 1. The results are shown in Table 1. <Comparative Example 4> An aqueous dispersion of oxidized CNF was obtained in the same manner as in Example 3, except that the number of treatment passes in the cavitation jet device was changed to 30 passes. The obtained oxidized CNF had an average fiber diameter of 3 nm and an aspect ratio of 180.

[0064] The total light transmittance, diffuse transmittance, haze, and transparency of the obtained oxidized CNF were measured in the same manner as in Example 1. The results are shown in Table 1.

[0065] [Table 1]

[0066] The present invention provides an anion-modified CNF having high haze. Among anion-modified CNF, carboxymethyl CNF in particular tends to show high haze even when the degree of defibration is high (high transparency) compared to oxidized CNF. A high degree of defibration has the advantage of being able to form a more uniform membrane. In other words, carboxymethyl CNF is preferable compared to oxidized CNF in that it is easy to form a uniform membrane while having a high haze.

Claims

1. An anion-modified cellulose nanofiber having a total light transmittance of 85.0% or more and a haze of 50.0% or more, measured by the following method: An aqueous dispersion of anion-modified cellulose nanofibers (solid content 0.5% (w / v)) was prepared and placed in a silicone frame on a polyethylene terephthalate film at a concentration of 0.2 g / cm. 2 The mixture is then dried at 50° C. to prepare a film, and the total light transmittance and diffuse transmittance are measured. Next, the haze is calculated as a ratio of the diffuse transmittance when the total light transmittance is taken as 100%.

2. The anionically modified cellulose nanofiber according to claim 1, wherein the anionically modified cellulose nanofiber is a carboxymethylated cellulose nanofiber.

3. The anion-modified cellulose nanofiber according to claim 2, having an average fiber diameter of 3 to 500 nm and an aspect ratio of 10 to 1000.

4. The anion-modified cellulose nanofiber according to claim 2 or 3, having a degree of carboxymethyl substitution in the range of 0.01 to 0.50 and a crystallinity of cellulose I type of 50% or more.

5. An additive comprising the anionically modified cellulose nanofiber according to any one of claims 1 to 3.

6. A haze enhancer comprising the anion-modified cellulose nanofiber according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Fine cellulose fiber

    JP2008001728A

  • Carboxymethylated cellulose fiber

    WO2014088072A1