Resin-coated metal plate and method for manufacturing the same

The resin-coated metal plate with a specific polyester resin coating addresses adhesion and corrosion issues by optimizing crystallinity and molecular orientation, providing enhanced durability and resistance to heat treatment.

JP2024148859AActive Publication Date: 2024-10-18JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023062361
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Conventional metal plates used for cans face issues with adhesion and corrosion resistance after heat treatment, particularly due to film brittleness and crystallization during ink baking, leading to cracks and scratches, which compromise the integrity of the can body.

Method used

A resin-coated metal plate with a polyester resin coating layer containing 85 mol% or more of ethylene terephthalate, characterized by specific Raman spectroscopic ratios and crystallinity, is applied to the metal surface, ensuring balanced crystal orientation and molecular structure for enhanced adhesion and corrosion resistance.

Benefits of technology

The resin-coated metal plate achieves excellent adhesion and corrosion resistance after heat treatment, suitable for containers, by controlling the crystallinity and molecular orientation of the polyester resin layer, thereby preventing film brittleness and ensuring durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148859000001
    Figure 2024148859000001
Patent Text Reader

Abstract

To provide a resin-coated metal plate which is excellent in adhesion and corrosion resistance after heat treatment.SOLUTION: A resin-coated metal plate has a resin-coated layer containing a polyester resin on at least one surface of a surface and a rear face of the metal plate. The polyester resin contains 85 mol% or more of ethylene terephthalate, and the resin-coated layer has a ratio (W1725(90 degrees) / W1725(0 degree)) of a half-value width (W1725(90 degrees)) of a C=O peak at 1,725±10 cm-1 by Raman spectroscopic analysis using the laser polarization plane in the same direction as a direction parallel to a resin-coated layer thickness direction of the resin-coated layer cross section, to a half-value width (W1725(0 degree)) of a C=O peak at 1,725±5 cm-1 by Raman spectroscopic analysis using a laser polarization plane in the same direction as a direction vertical to the resin-coated layer thickness direction of the resin-coated layer cross section of 0.90 or more and 1.30 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin-coated metal sheet used for can bodies and lids of, for example, 18 L cans and food cans. [Background technology]

[0002] Conventionally, metal sheets such as tin-free steel (TFS) and aluminum, which are materials used for 18L cans and food cans, have been painted to improve corrosion resistance, durability, weather resistance, etc. However, this painting process not only involves a complicated baking process, but also requires a long processing time and has the problem of discharging a large amount of solvent.

[0003] In order to solve these problems, resin-coated metal sheets (film-laminated metal sheets) have been developed in place of painted steel sheets, in which a thermoplastic resin film is laminated onto a heated metal sheet. These sheets are currently used industrially as materials for food cans, beverage cans, and aerosol cans.

[0004] These materials are required to have basic properties such as adhesion and covering properties. Furthermore, in recent years, in order to give containers a design, processes such as printing on the outer surface of the can body may be performed, so laminate materials that can withstand heat treatment after printing are required. In the printing process, the film on the laminated metal plate is subjected to ink baking heat treatment and crystallizes and becomes embrittled. Then, when the film is processed into a container, cracks and scratches occur in the film, which causes problems with corrosion resistance when the contents are pressed. For this reason, properties related to workability after heat treatment, i.e., corrosion resistance, are also required. In conventional metal plates coated with polyester resin, the composition and melting point range of the polyester resin have been controlled to improve heat resistance and post-processing workability. Here, the adhesion is a property that the film does not peel off when processed into a container shape, and the corrosion resistance is a property that suppresses corrosion caused by the contents filled in the container after the metal plate is processed into the container shape.

[0005] For example, in Patent Document 1, a polyester film having a resin composition and melting point within a specific range is applied to a metal container, and when heated for 2 minutes in an atmosphere of 210°C, the dimensional change rate is 2.0% or less. However, when the film is subjected to processing after printing and heating, such as distortion printing, peeling of the film occurs after processing, and adhesion is insufficient.

[0006] Patent Document 2 discloses a polyester film in which at least two or more polyesters with different crystallinity, i.e., at least two or more polyesters including a PBT-based polyester (I) and a PET-based polyester (II), are blended in a specific ratio and the heat shrinkage rate at 130°C for 15 minutes is adjusted to be within a specific range, which can suppress the occurrence of shrinkage wrinkles during drying after the adhesive layer is applied, and also has excellent formability for cans, particularly for drawing and ironing, and is also excellent in thermal lamination with metals, impact resistance, and flavor and aroma retention. However, since 80 to 40% by mass of the PBT-based polyester (I) with a melting point in the range of 200 to 223°C is added, the crystallization of the film progresses due to heat treatment after printing, which may lead to embrittlement of the film, and the corrosion resistance is insufficient.

[0007] Patent Document 3 discloses a laminated metal sheet for a two-piece can, comprising a metal sheet, a first polyester resin layer formed on the surface of the metal sheet that will be the outer surface of the container after the container is molded, and a second polyester resin layer formed on the surface of the metal sheet that will be the inner surface of the container after the container is molded. In this laminated metal sheet, the first polyester resin layer contains 30% to 60% by mass of polyethylene terephthalate or copolymerized polyethylene terephthalate having a copolymerization component content of less than 6 mol%, 40% to 70% by mass of polybutylene terephthalate or copolymerized polybutylene terephthalate having a copolymerization component content of less than 5 mol%, and a polyolefin wax in an external ratio of 0.01% to 3.0%, the second polyester resin layer is copolymerized polyethylene terephthalate having a copolymerization component content of less than 22 mol%, and the residual orientation degree of the first and second polyester resin layers is less than 30%. According to this laminated metal sheet, the polyester resin layer formed on the metal sheet surface that will be the outer surface of the container after the container is formed contains 40% by mass to 70% by mass of polybutylene terephthalate component, so that retort whitening, which is discoloration of the polyester resin film, can be suppressed. On the other hand, depending on the heat treatment (retort treatment), crystallization of the film may progress, which may lead to embrittlement of the film, and there is room for improvement in corrosion resistance after such heat treatment.

[0008] Patent Document 4 discloses a polyester film for metal lamination, which uses a biaxially stretched polyester film made of a copolymer polyester containing a specific amount of a carboxylic acid component with a valence of 3 or more in the acid component of the polyester film, and sets the melting point and intrinsic viscosity of the polyester film within a specific range, thereby providing excellent thermal lamination with a metal plate, excellent high-order processability when forming a can after thermal lamination, suppressing the generation of hair at the cut part of the thermally laminated metal plate, and not reducing the impact resistance of the formed can. However, although the generation of hair is suppressed, the melting point is 210°C to 235°C, so that the heating temperature in the baking heat treatment after printing is restricted to less than the above melting point, resulting in insufficient heat resistance. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2006-289989 A [Patent Document 2] JP 2009-221315 A [Patent Document 3] JP 2014-166856 A [Patent Document 4] JP 2010-168432 A Summary of the Invention [Problem to be solved by the invention]

[0010] As described above, it is essential that the resin-coated metal sheet is capable of meeting many of the characteristics required for food can materials. Furthermore, in container applications, since ink baking treatment is required when printing to impart design, excellent corrosion resistance after such heat treatment is also important, particularly in container applications. In view of the above circumstances, an object of the present invention is to provide a resin-coated metal sheet which not only has the above-mentioned excellent adhesion but also has excellent corrosion resistance after heat treatment. [Means for solving the problem]

[0011] The present inventors have conducted extensive research into means for solving the above problems. As a result, the present inventors have found that in a resin-coated metal plate in which at least one of the front and back surfaces of a metal plate is coated with a film containing a polyester resin, the polyester resin contains 85 mol % or more of ethylene terephthalate, and the cross section of the resin-coated layer of the metal plate has a polarization plane of 1725±5 cm by Raman spectroscopy using a laser polarization plane that is the same as the direction perpendicular to the thickness direction of the resin-coated layer. -1 The half-width of the C=O peak (W 1725(0 degrees)) and 1725±10 cm -1 The half-width of the C=O peak (W 1725 (90 degrees)) (W 1725 (90 degrees) / W 1725 It has been found that, when the temperature (°C) (0°) is in the range of 0.90 or more and 1.30 or less, a resin-coated metal sheet having excellent adhesion and corrosion resistance after heat treatment and particularly suitable for use as a container can be obtained.

[0012] Furthermore, the polyester resin film coated on the metal plate was subjected to the above-mentioned ratio (W 1725 (90 degrees) / W 1725 The inventors have also discovered that by setting the angle (angle (angle) (0 degrees)) to 0.93 or more and 1.20 or less in a region within 3 μm from the interface between the metal plate and the resin coating layer in a cross section perpendicular to the plate surface of the resin-coated metal plate, it is possible to ensure a high level of corrosion resistance after heat treatment.

[0013] The present invention has been made based on the above findings, and the gist of the present invention is as follows. [1] A resin-coated metal plate having a resin coating layer containing a polyester resin on at least one of the front and back surfaces of a metal plate, The polyester resin contains 85 mol % or more of ethylene terephthalate, The resin coating layer is 1725±5 cm by Raman spectroscopy using a laser polarization plane that is the same as the direction perpendicular to the thickness direction of the resin coating layer of the resin coating layer cross section. -1 The half-width of the C=O peak (W 1725 (0 degrees)) and a 1725±10 cm -1 The half-width of the C=O peak (W 1725 (90 degrees)) (W 1725 (90 degrees) / W 1725 (0 degrees) is in the range of 0.90 to 1.30. Resin-coated metal sheet.

[0014] [2] The ratio (W 1725 (90 degrees) / W 1725 The resin-coated metal sheet according to the above [1], wherein the refractive index (0 degrees) is in the range of 0.93 to 1.20 in a region within 3 μm of a cross section perpendicular to the plate surface of the resin-coated metal sheet from the interface between the metal sheet and the resin coating layer.

[0015] [3] 1615±5cm by Raman spectroscopy using a laser polarization plane that is the same as the direction perpendicular to the film thickness direction of the film cross section after heat treatment at 180°C for 10 minutes. -1 C=O peak intensity (I 1615 (0 degrees)) and 1725±5cm -1 C=C peak intensity (I 1725 (0 degrees)) (I 1725 / I 1615 ) is 0.52 or more and 0.63 or less.

[0016] [4] A method for producing a resin-coated metal sheet according to any one of [1] to [3], When coating the metal plate with the polyester resin film, The surface temperature of the metal plate at the start of the coating is in the range of Tm (melting point) to Tm+40° C. of the polyester resin; The surface temperature of the pressure roller pressing the polyester resin film is in the range of Tg (glass transition point) to Tg+80° C. of the polyester resin; and The contact time between the polyester resin film and the pressure roller is in the range of 10 to 30 msec. Next, cooling is started within 2 seconds from the completion of the coating, and the temperature is cooled to a temperature range of Tg (glass transition temperature) -20°C to Tg of the polyester resin. A method for manufacturing a resin-coated metal sheet. Effect of the Invention

[0017] According to the present invention, it is possible to provide a resin-coated metal sheet which has excellent adhesion, which is a basic property required for 18L cans and food can materials, and further has excellent corrosion resistance after heat treatment. BEST MODE FOR CARRYING OUT THEINVENTION

[0018] The resin-coated metal sheet of the present invention will be described in detail below. First, the metal sheet used in the present invention will be described. The metal sheet of the present invention may be an aluminum sheet or a mild steel sheet, which are widely used as materials for cans. In particular, a surface-treated steel sheet (hereinafter referred to as TFS) having a two-layer coating formed thereon, the lower layer being metallic chromium and the upper layer being chromium hydroxide, is optimal. The coating weight of the TFS is not particularly limited, but from the viewpoint of post-processing adhesion and corrosion resistance, the metallic chromium layer should be 70 to 200 mg / m2 in terms of Cr for both layers. 2 , chromium hydroxide layer is 10-30mg / m 2 It is desirable to do so.

[0019] At least one of the front and back surfaces of the metal plate has a coating layer containing a polyester resin. This polyester resin coating layer will be described.

[0020] This polyester resin coating layer is mainly composed of polyethylene terephthalate. The term "mainly composed of polyethylene terephthalate" means that 85 mol% or more of the polyester structural units are ethylene terephthalate. More preferably, 87 mol% or more. If the ethylene terephthalate unit is 80 mol% or more, the layer is suitable for applications requiring heat resistance.

[0021] Terephthalic acid, as an acid component of polyethylene terephthalate, is essential for ensuring properties such as mechanical strength, heat resistance, and corrosion resistance. In addition, copolymerization of terephthalic acid with isophthalic acid improves processability. That is, copolymerization of 2 to 10 mol% of an isophthalic acid component with respect to a terephthalic acid component improves deep drawability, making it suitable for high-process applications.

[0022] Furthermore, other dicarboxylic acid components and glycol components may be copolymerized within a range that does not impair the above characteristics. Examples of dicarboxylic acid components include aromatic dicarboxylic acids such as diphenyl carboxylic acid, 5-sodium sulfoisophthalic acid, and phthalic acid, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid, aliphatic dicarboxylic acids such as cyclohexane dicarboxylic acid, and oxycarboxylic acids such as p-oxybenzoic acid. Examples of other glycol components include aliphatic glycols such as propanediol, butanediol, pentanediol, hexanediol, and neopentyl glycol, aromatic glycols such as cyclohexane dimethanol, aromatic glycols such as bisphenol A and bisphenol S, diethylene glycol, and polyethylene glycol. These dicarboxylic acid components and glycol components may be used in combination of two or more. Also, polyfunctional compounds such as trimellitic acid, trimesic acid, and trimethylolpropane may be copolymerized within the range that does not impair the effects of the present invention.

[0023] The resin material is not limited by its manufacturing method. For example, the resin material can be formed by using a method such as (1) esterifying terephthalic acid, ethylene glycol, and a copolymerization component, and then polycondensing the resulting reaction product to obtain a copolymerized polyester, or (2) transesterifying dimethyl terephthalate, ethylene glycol, and a copolymerization component, and then polycondensing the resulting reaction product to obtain a copolymerized polyester. In the production of the copolymerized polyester, additives such as a fluorescent whitening agent, an antioxidant, a heat stabilizer, an ultraviolet absorber, and an antistatic agent may be added as necessary. To improve the whiteness, the addition of a fluorescent whitening agent is effective.

[0024] Next, the polyester resin coating layer mainly composed of polyethylene terephthalate according to the present invention is preferably a coating layer made of a biaxially oriented film. Here, the reason why a biaxially oriented film is preferably used is because of productivity, uniformity of the film thickness, etc.

[0025] The polyester resin coating layer has a polarization plane of 1725±5 cm measured by Raman spectroscopy using a laser polarization plane that is the same as the direction perpendicular to the thickness direction of the resin coating layer in the cross section of the resin coating layer. -1 The half-width of the C=O peak (W 1725 (0 degrees)) and a 1725±10 cm -1 The half-width of the C=O peak (W 1725 (90 degrees)) (W 1725 (90 degrees) / W 1725 (0 degrees)) (hereinafter, simply the ratio (W 1725 (90 degrees) / W 1725 It is important that the θ is between 0.90 and 1.30 for all layers.

[0026] That is, the ratio of the polyester resin layer (W 1725 (90 degrees) / W 1725 By keeping the temperature (°C) in the range of 0.90 to 1.30, it is possible to ensure the adhesion and corrosion resistance after heat treatment, which are the objects of the present invention. The reasons for this will be described below.

[0027] 1725±5cm as measured by Raman spectroscopy as described above -1 Near C=O peak half-width (W 1725 (0 degrees)) is an index of the crystallinity of polyethylene terephthalate resin, and the ratio (W 1725 (90 degrees) / W 1725 The half-width (W (0°)) of the C=O peak indicates the crystal orientation in the thickness direction of the film. 1725 If the C=O peak half-width (W 1725 When the C=O peak half-width (W 1725(0 degrees) is advantageous, and in order to ensure corrosion resistance, the half-width (W 1725 (0 degrees) is more advantageous. Taking all of the above into account, the ratio (W 1725 (90 degrees) / W 1725 By making the refractive index (0 degrees) fall within the range of 0.90 or more and 1.30 or less, it is possible to achieve a high level of both adhesion and corrosion resistance.

[0028] Here, if the crystallinity of the polyester film before coating the metal plate is less than 28%, the crystal orientation of the polyester film will be small, while if the crystallinity exceeds 38%, the crystal orientation of the polyester film will be large. Therefore, the C=O peak half width ratio (W 1725 (90 degrees) / W 1725 In order to set the refractive index (0 degrees) in the range of 0.90 or more and 1.30 or less, it is preferable that the crystallinity of the film is 28% or more and 38% or less.

[0029] Furthermore, in order to improve the corrosion resistance after heat treatment, the above ratio (W 1725 (90 degrees) / W 1725 It is preferable that the ratio (W (0 degrees)) is 0.93 or more and 1.20 or less in a region within 3 μm from the interface between the metal plate and the resin coating layer in a cross section perpendicular to the plate surface of the resin-coated metal plate (hereinafter, the region 3 μm from the metal plate surface). This is because the presence of spherulites generated by heat treatment near the interface between the metal plate and the film contributes to improving corrosion resistance. 1725 (90 degrees) / W 1725 When the spherulite ratio (0 degrees) is between 0.93 and 1.20 in the area 3 μm deep on the surface of the metal plate, the amount of spherulite generated near the interface between the metal plate and the film is well balanced, and the corrosion resistance after heat treatment is excellent. Spherulites are dense, isotropic crystals that are generated by thermal crystallization from random polymers (polymers in a molten or glassy state).

[0030] The above ratio (W 1725 (90 degrees) / W 1725If the film thickness (0 degrees) is less than 0.93, the crystal orientation of the polyester resin coated on the metal plate will be small, resulting in an excessively high randomness of the resin, and the amount of spherulites generated after heat treatment will be excessive, which may cause deterioration of processability, i.e., the occurrence of cracks and scratches. This raises the concern that when the components of the can contents that have permeated the film reach the metal plate, they may start to corrode from the cracks and scratches.

[0031] On the other hand, the ratio (W 1725 (90 degrees) / W 1725 If the ratio (W (0 degrees)) exceeds 1.20, the amount of crystal orientation of the polyester resin coated on the metal plate becomes relatively large, so the amount of spherulites generated by heat treatment decreases, and corrosion resistance does not improve. More preferably, 1725 (90 degrees) / W 1725 (0 degrees) is in the range of 0.94 to 1.16.

[0032] Furthermore, after heat treatment at 180° C. for 10 minutes, the film cross section was analyzed by Raman spectroscopy using a laser polarization plane perpendicular to the film thickness direction. The polarization plane was 1615±5 cm -1 C=O peak intensity (I 1615 (0 degrees)) and 1725±5cm -1 C=C peak intensity (I 1725 (0 degrees)) (I 1725 / I 1615 It is preferable that the peak intensity ratio (I 1725 / I 1615 If the peak intensity ratio (I 1725 / I 1615 If the ratio exceeds 0.63, the amorphous amount decreases, the flexibility of the film decreases, and cracks may occur, and the adhesion after processing (ability to suppress exposure of the metal plate) may deteriorate.

[0033] Furthermore, the intrinsic viscosity (IV) of the polyester resin coating layer is preferably 0.50 dl / g or more and 0.90 dl / g or less. More preferably, it is 0.52 dl / g or more and 0.80 dl / g or less, and more preferably, it is 0.55 dl / g or more and 0.75 dl / g or less. If the intrinsic viscosity of the resin coating layer is 0.50 dl / g or more, the molecular weight of the resin coating layer is high and sufficient mechanical strength can be ensured. On the other hand, if the intrinsic viscosity of the resin coating layer is 0.90 dl / g or less, excellent film-forming properties can be obtained. The intrinsic viscosity (IV) of the resin coating layer can be adjusted by controlling the polymerization conditions (amount of polymerization catalyst, polymerization temperature, polymerization time, etc.) or by solid-phase polymerization in an inert atmosphere such as nitrogen or under vacuum after melt polymerization.

[0034] In addition, the polyester resin coating layer on one side may have a multi-layer structure with each layer having a function. For example, it may have a two-layer structure of an upper layer and a lower layer, or a structure consisting of at least three layers, the outermost layer (upper layer), the middle layer (main layer), and the bottom layer (lower layer). Preferably, it has up to three layers. An example of a multi-layer structure in which each layer has a function is to contain wax in the outermost surface to reduce the amount of wax in the entire resin coating layer, thereby effectively controlling the processability by wax. In addition, it is also possible to control the color tone of the entire layer while ensuring processability, etc., by adding a large amount of pigment to the middle layer in the multi-layer structure. In such a case, the film thickness of the outermost layer and the bottom layer may be 1.0 μm or more and 5.0 μm or less, preferably 1.5 μm or more and 4.0 μm or less, and more preferably 2.0 μm or more and 3.0 μm or less. The thickness of the intermediate layer is preferably in the range of 6 μm to 30 μm, more preferably 8 μm to 25 μm, and even more preferably 10 μm to 20 μm. In order to achieve both whiteness and workability as a layer, the outermost layer and the lowermost layer preferably contain 0% to 2% titanium oxide, and the intermediate layer preferably contains 10% to 30% titanium oxide.

[0035] In particular, when one side is to be the inner surface after the container forming process, the polyester resin coating layer on this side is preferably made into a multi-layer structure, and the outermost resin layer in contact with the contents may contain 0.10 to 2.0% by mass of a wax compound. The purpose of adding the wax compound is to reduce the surface free energy of the resin layer on the inner surface side of the container, and the wax compound makes it difficult for the contents to adhere to the resin layer, improving the ease of removing the contents. The reason why the amount of the wax compound is limited to 0.10% by mass or more is that if it is less than 0.10% by mass, the above effect is poor and the ease of removing the contents is poor. The reason why the amount of the wax compound is limited to 2.0% by mass or less is that if it exceeds 2.0% by mass, the adhesion between the resin layers is likely to deteriorate, and the film formation of the resin layer itself becomes difficult, resulting in a deterioration in productivity.

[0036] It is also preferable that the other surface of the metal plate has a polyester resin coating layer similar to that of the one surface. In particular, it is preferable that the polyester resin coating layer on the other surface has a multi-layer structure. It is also preferable that the layers of this resin coating layer, except for the outermost layer, contain either or both of titanium dioxide and a disazo-based organic pigment as a coloring pigment.

[0037] The number of polyester resin layers on the other side is not particularly limited, but is preferably 2 or more and 3 or less. This is because, by making it 2 or more layers, it is not necessary to add wax necessary for realizing the content removal property to all layers, and the minimum amount of wax required can be added. On the other hand, by making it 3 or less, the film production cost can be reduced.

[0038] For example, when the other surface is to be the outer surface after molding of the container, the polyester resin coating layer here may be required to be gold or white in order to improve the design after molding or during printing processing. In order to give a brilliant gold color, it is preferable to contain either one or both of titanium dioxide and disazo-based organic pigments as coloring pigments. These pigments are yellow in color but transparent, so that they can efficiently obtain a brilliant gold color by utilizing the luster of the metal plate.

[0039] Generally, the use of oil-soluble dyes is known as a method for achieving highly transparent coloring. However, one of the drawbacks of these methods is migration (dissolution of coloring materials from colored resins). This is a phenomenon (bleeding) in which oil-soluble dyes dissolve in the resin to be colored and float to the resin surface when subjected to a thermal history such as retort sterilization. However, disazo organic pigments generally exist in the resin as particles, so migration can be significantly suppressed.

[0040] As the yellow pigment, it is preferable to use a disazo-based organic pigment, and among them, the use of CI Pigment Yellow 180 is particularly suitable. This is because it is a pigment registered with the FDA (Food and Drug Administration), has excellent safety, and can obtain an excellent color tone. The amount added is preferably 0.1% by mass or more and 20.0% by mass or less with respect to the total amount of the resin layer (B). If it is less than 0.1% by mass, the color development is poor and a preferable color tone cannot be obtained. On the other hand, if it exceeds 20.0% by mass, the transparency of the resin may be poor and the color tone may lack brilliance. The particle diameter of the pigment is preferably less than 1 μm. If it is 1 μm or more, the transparency of the polyester resin may be lost, which is not preferable. In addition, a higher fatty acid metal salt such as magnesium stearate can be used as a dispersant. If a dispersant is used, a more uniform and highly transparent color tone can be obtained.

[0041] In addition to the yellow pigment, the addition of a white pigment can conceal the metallic luster of the base and make the printed surface clear, resulting in a good appearance. The pigment to be added must be able to exhibit excellent design after the container is molded, and from this perspective, titanium dioxide is preferably used. Titanium dioxide has strong coloring power and excellent ductility, so it is suitable because it can ensure good design even after the container is molded. The amount of addition is preferably 10.0% by mass or more and 30.0% by mass or less based on the total amount of the resin layer. If it is less than 10.0% by mass, the color is poor and a preferable color tone cannot be obtained. Conversely, if it exceeds 30.0% by mass, the flexibility of the resin layer is impaired, and it may not be possible to follow the container molding.

[0042] Of course, the polyester resin coating layer on the other side may have a function for each layer of the multi-layer structure, similar to the polyester resin coating layer on one side. That is, it may have a two-layer structure of an upper layer and a lower layer, or a structure consisting of at least three layers, an uppermost layer (upper layer), an intermediate layer (main layer), and a lowermost layer (lower layer). The outermost layer may contain wax to reduce the amount of wax in the entire resin coating layer, thereby effectively controlling the processability. Here, too, the film thickness of the outermost layer and the lowermost layer may be 1.0 μm or more and 5.0 μm or less, preferably 1.5 μm or more and 4.0 μm or less, more preferably 2.0 μm or more and 3.0 μm or less. The film thickness of the intermediate layer may be within a range of 6 μm or more and 30 μm or less, preferably 8 μm or more and 25 μm or less, more preferably 10 μm or more and 20 μm or less. In order to achieve both whiteness and workability as a layer, it is preferable that the outermost layer and the lowermost layer contain 0% to 2% titanium oxide, and the intermediate layer contains 10% to 30% titanium oxide.

[0043] When the above resin-coated metal sheet is used as a container, it may be molded and used so that one of the surfaces is the inner surface of the container and the other surface is the outer surface of the container.

[0044] [Manufacturing method] Next, the manufacturing method of the resin-coated metal sheet of the present invention will be described. First, the manufacturing method of the resin layer (film) of single layer or multi-layer structure to be coated on the metal sheet will be described using a resin film of multi-layer structure as a typical example. The manufacturing method of this resin layer does not need to be particularly limited. An example of the manufacturing method will be shown below. Each polyester resin, which is the material for each layer of the multilayer structure, is dried as necessary, and then fed into a known melt lamination extruder, extruded into a sheet form from a slit-shaped die, and adhered to a casting drum by electrostatic application or other methods, cooled and solidified to obtain an unstretched sheet. This unstretched sheet is stretched in the longitudinal and transverse directions of the film to obtain a biaxially stretched film. The stretching ratio can be set arbitrarily depending on the desired degree of orientation, strength, elastic modulus, etc. of the film. The stretching method is preferably a tenter method in terms of film quality, and is preferably either a sequential biaxial stretching method in which stretching is performed in the longitudinal direction and then in the transverse direction, or a simultaneous biaxial stretching method in which stretching is performed in the longitudinal direction and then in the transverse direction almost simultaneously.

[0045] Next, a method for producing a resin-coated metal sheet by laminating a resin layer (film) onto a metal sheet will be described. In the present invention, for example, a method can be used in which a metal plate is heated to a temperature above the melting point of the film, and a pressure-bonding roll (hereinafter referred to as a laminating roll) is used to contact a resin film with one or both sides of the metal plate to heat-seal the resin film (hereinafter referred to as laminating).

[0046] The lamination conditions are appropriately set so as to obtain the resin coating layer defined in the present invention. First, the surface temperature of the metal sheet at the start of lamination must be equal to or higher than the Tm (melting point) of the resin layer in contact with the metal sheet. Specifically, it must be controlled within the range of Tm to Tm+40°C of the resin layer. By making the surface temperature of the metal sheet equal to or higher than the Tm of the resin layer, the resin layer melts and wets the surface of the metal sheet, thereby ensuring good adhesion to the metal sheet. On the other hand, if the surface temperature of the metal sheet exceeds Tm+40°C, the resin layer will melt excessively, which may cause the resin layer to adhere to the lamination roll, and the crystal structure (ratio (W)) of the surface resin layer may deteriorate. 1725 (90 degrees) / W 1725It becomes difficult to control the temperature (Tm) within the range specified in the present invention. The temperature is preferably from Tm to Tm+25°C, and more preferably from Tm to Tm+15°C.

[0047] Furthermore, the crystal structure of the resin layer (ratio (W 1725 (90 degrees) / W 1725 In order to control the temperature (Tg (0 degrees))) to an appropriate state, the surface temperature of the laminating roll must also be adjusted. Specifically, the surface temperature of the laminating roll that comes into contact with the resin layer must be controlled within the range of Tg to Tg+80°C of the resin layer, based on the glass transition point (Tg) of the resin layer. In other words, by setting the surface temperature of the laminating roll at or above the Tg of the resin layer, the resin layer melts and wets the surface of the metal sheet, thereby ensuring good adhesion to the metal sheet. On the other hand, if the surface temperature of the laminating roll exceeds Tg+80°C, the resin layer will melt excessively, raising concerns that the resin layer may adhere to the laminating roll, and the crystal structure (ratio (W)) of the surface resin layer may deteriorate. 1725 (90 degrees) / W 1725 (0 degrees)) within the range specified by the present invention.

[0048] Furthermore, adjustment of the contact time between the laminating roll and the resin layer is also an important factor. The contact time needs to be controlled within the range of 10 to 30 msec. By adjusting the surface temperature of the laminating roll and the contact time within the above range, the crystal structure of the resin defined in the present invention can be realized.

[0049] It is preferable to heat the resin layer before laminating it on the metal plate. By softening the resin layer in advance, the temperature distribution in the cross section of the resin layer during lamination can be made more uniform. This allows the crystal structure in the cross section of the resin layer to change gradually from the interface with the metal plate to the surface layer, resulting in more uniform performance. Specifically, it is preferable to adjust the temperature of the resin layer before lamination to a range of Tg to Tg + 30°C.

[0050] After the lamination is completed, it is necessary to perform cooling (quenching) promptly to fix the crystal structure of the resin layer. The time until the start of this cooling must be limited to within 2 seconds immediately after the lamination is completed, and is preferably within 1 second. This cooling allows the surface temperature of the resin layer to be cooled to a temperature range of the glass transition point (Tg) of the resin layer -20°C to the glass transition point (Tg) or lower. Specifically, the resin-coated metal sheet immediately after lamination is subjected to water cooling, and the water temperature is controlled to a temperature range of the glass transition point (Tg) of the resin layer -20°C to the glass transition point (Tg) or lower, until the surface temperature of the resin layer reaches the temperature range. Here, water cooling refers to cooling by bringing water into contact with the resin-coated metal sheet, and examples of this include mist type, spray type, and immersion in a water tank. EXAMPLES

[0051] Examples of the present invention will now be described. (Metal Sheet Manufacturing Method) The steel sheets with a thickness of 0.22 mm and a width of 977 mm were cold-rolled, annealed, and temper-rolled. They were then degreased, pickled, and chrome-plated to produce chrome-plated steel sheets (TFS). The chrome plating was performed using CrO3, F - , SO4 2- Electrolytic plating is performed in a plating bath containing CrO3, F after intermediate rinsing. - During the chemical conversion treatment, the electrolysis conditions (current density, amount of electricity, etc.) were adjusted to achieve a chromium metal deposition amount and a chromium hydroxide deposition amount of 120 mg / m2, calculated as Cr. 2 and 15 mg / m 2 It was decided.

[0052] (Method of manufacturing resin-coated film) The polyester resins having the resin compositions shown in Table 1 were dried and melted in the usual manner, co-extruded from a T-die, and then cooled and solidified on a cooling drum to obtain an unstretched film. The unstretched film obtained was biaxially stretched and heat-set to obtain a biaxially stretched polyester film.

[0053] (Method of manufacturing resin-coated metal sheet) A polyester film was laminated onto the chromium-plated steel sheet using a thermocompression laminating device under the conditions shown in Table 1. That is, the polyester films shown in Table 1 were laminated onto the front and back surfaces of the chromium-plated steel sheet.

[0054] When the polyester film was coated (laminated) on the metal plate, the surface temperature of the metal plate was controlled to Tm to Tm+40°C of the polyester resin constituting the polyester film. The surface temperature of the pressure roll (laminating roll) was set to Tg to Tg+80°C of the polyester resin. The contact time between the film on the metal plate and the roll was set to 10 to 30 msec. The laminating roll was an internal water-cooled type, and the temperature during film bonding was controlled by circulating cooling water inside the roll. The temperature of the film for the resin layer before lamination was set to Tg+30°C to Tg+100°C of the polyester film, and the temperature distribution in the cross section of the resin layer was made uniform. After that, water cooling at 70°C was performed in a metal band cooling device after 1 sec to produce a resin-coated metal plate. For comparison, production was also performed under conditions that deviated from any of the above production conditions.

[0055] (Evaluation of resin-coated metal sheets) The resin-coated metal sheets and the resin layers on the metal sheets obtained above were measured and evaluated for the following properties. The measurement and evaluation methods are shown below.

[0056] (1) Thermal analysis of film The film was subjected to thermal analysis before being coated on the metal plate to determine the glass transition point (Tg) and melting point (Tm) of the film. Measurement equipment: DSC Q100 manufactured by TA Instruments, Inc. Measurement temperature range: -50℃~290℃ Heating rate: 10℃ / min Atmosphere: Nitrogen atmosphere, flow rate 50m / min

[0057] (2) Evaluation of the film cross-sectional direction by Raman spectroscopy A cross-sectional sample of a resin-coated metal sheet was analyzed by Raman spectroscopy using a laser polarization plane that is the same as the direction perpendicular to the cross-sectional direction of the film. -1 The half-width of the C=O peak (W 1725 (0 degrees)) and 1725±10cm by Raman spectroscopy using a laser polarization plane that is the same as the direction parallel to the film thickness direction of the film cross section. -1 The half-width of the C=O peak (W 1725 The measurement pitch was 0.5 μm. The ratio of the half-width of the Raman peak from the half-width in the 0-degree direction to the half-width in the 90-degree direction (W 1725 (90 degrees) / W 1725 (0 degrees) was calculated.

[0058] (Measurement conditions) Measurement equipment: Raman spectrometer LabRAM HR manufactured by Horiba Ltd. Excitation light source: Semiconductor laser (λ=532nm) Microscope magnification: x100 Aperture: 25μmφ Measurement pitch: 0.5 μm Measurement direction: The laser polarization plane is perpendicular (0 degrees) and horizontal (90 degrees) to the film thickness direction of the film cross section of the resin-coated metal sheet.

[0059] (3) Evaluation of the alignment state after heat treatment using Raman spectroscopy The laminated metal sheet was heat-treated at 180°C for 10 minutes in a hot air drying oven, and the Raman spectroscopic analysis was performed in the cross-sectional direction of the film in the same manner as in (2) above. -1 C=C peak intensity (I 1615 (0 degrees)) and 1725±5cm -1 C=O peak intensity (I 1725 (0 degrees)) ratio (I 1715 (0 degrees) / I 1615 (0 degrees) was calculated.

[0060] (5) Adhesion A test piece measuring 120 mm in the longitudinal direction and 30 mm in the transverse direction was cut out from the resin-coated metal sheet. A portion of the film was peeled off from the long edge of the cut test piece on the inner surface of the can (one side), and the peeled portion of the film was opened in the opposite direction (angle: 180°) to the chrome-plated steel sheet from which the film was peeled off using a tensile tester, and a peel test was performed at a tensile speed of 30 mm / min to evaluate the adhesion per 15 mm width. If this adhesion is 5 N / 15 mm or more, the adhesion between the film and the metal sheet is maintained even if strong processing such as drawing is performed. On the other hand, if the adhesion is less than 5 N / 15 mm, the film may peel off under even stronger processing conditions such as drawing and ironing.

[0061] (Score) ◎: 8N / 15mm or more ○: 5N / 15mm or more and less than 8N / 15mm △: 2N / 15mm or more, less than 5N / 15mm ×: Less than 2N / 15mm

[0062] (6) Corrosion resistance after heat treatment The resin-coated metal plate was heat-treated at 180°C for 10 minutes, then cut to a size of 70 mm x 70 mm and placed in a special cell so that the resin-coated surface was in contact with saline solution (5% by mass). The contact area between the resin-coated metal plate and the saline solution was 19.6 cm 2 The immersion test was carried out at 38°C for three months. The appearance of the samples after immersion was evaluated by examining the area of ​​the peeled film and the area of ​​the corroded area on the sample plate surface, and the total area of ​​the peeled film and corroded area on the sample was used for evaluation. If this area was less than 10%, the can exhibited excellent corrosion resistance when used as a general food can for salmon, seasonings, etc. On the other hand, if the area was 10% or more, there was a risk that the can body would corrode even when used as a general food can for salmon, seasonings, etc.

[0063] (About the ratings) ◎◎: Area of ​​film peeling and corroded area: 0% to less than 2% ◎: Film peeling area and corroded area: 2% to less than 5% ○: Film peeling area and corroded area: 5% to less than 10% △: Film peeling area and corroded area: 10% to less than 30% ×: Film peeling and corroded area: 30% or more

[0064] As shown in Table 1, the resin-coated metal sheet according to the present invention has excellent adhesion and also has excellent corrosion resistance after heat treatment. Therefore, the resin-coated metal sheet according to the present invention is particularly suitable for containers. In contrast, the comparative examples outside the scope of the present invention are inferior in adhesion and corrosion resistance after heat treatment.

[0065] [Table 1] [Industrial Applicability]

[0066] INDUSTRIAL APPLICABILITY The resin-coated metal sheet for containers of the present invention can be suitably used for container and packaging applications required for materials for 18 L cans and materials for food cans.

Claims

1. A resin-coated metal plate having a resin coating layer containing a polyester resin on at least one of the front and back surfaces of a metal plate, The polyester resin contains 85 mol % or more of ethylene terephthalate, The resin coating layer is A Raman spectroscopic analysis using a laser polarization plane that is the same as the direction perpendicular to the thickness direction of the resin coating layer in the cross section of the resin coating layer, 1725±5 cm -1 The half-width (W 1725 (0 degrees)) and a Raman spectroscopic analysis using a laser polarization plane that is the same as the direction parallel to the thickness direction of the resin coating layer of the cross section of the resin coating layer, of 1725 ± 10 cm -1 The half-width (W 1725 (90 degrees)) (W 1725 (90 degrees) / W 1725 (0 degrees) is in the range of 0.90 to 1.30, Resin-coated metal sheet.

2. The ratio (W 1725 (90 degrees) / W 1725 2. The resin-coated metal sheet according to claim 1, wherein the angle (0 degrees) is in the range of 0.93 to 1.20 in a region within 3 μm of a cross section perpendicular to the plate surface of the resin-coated metal sheet from the interface between the metal sheet and the resin coating layer.

3. A Raman spectroscopic analysis using a laser polarization plane that is the same as the direction perpendicular to the thickness direction of the resin coating layer of the cross section of the resin coating layer after heat treatment at 180° C. for 10 minutes has a wavelength of 1615±5 cm -1 C═O peak intensity (I 1615 (0 degrees)) and 1725±5 cm -1 C═C peak intensity (I 1725 (0 degrees)) (I 1725 / I 1615 3. The resin-coated metal sheet according to claim 1, wherein the ratio of the surface roughness to the surface roughness is 0.52 or more and 0.63 or less.

4. A method for producing a resin-coated metal sheet according to claim 1 or 2, When coating the metal plate with the polyester resin film, The surface temperature of the metal plate at the start of the coating is in the range of Tm (melting point) to Tm+40° C. of the polyester resin; The surface temperature of the pressure roller pressing the polyester resin film is in the range of Tg (glass transition point) of the polyester resin to Tg + 80 ° C.; The contact time between the polyester resin film and the pressure roller is in the range of 10 to 30 msec. Next, cooling is started within 2 seconds from the completion of the coating, and the temperature is cooled to a temperature range of Tg (glass transition temperature) of the polyester resin -20°C to Tg. A method for manufacturing a resin-coated metal sheet.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing metallic sheet covered with thermoplastic resin

    WO1997043118A1

  • Resin-coated metal plate for containers

    WO2022202931A1

  • Polyester film for metal plate lamination, film laminated metal plate and metal container

    JP2006289989A

  • Film for metal sheet lamination, film-laminated metal sheet and metal container

    JP2009221315A

  • Polyester film for metal plate lamination