Composite material, heat sink member using the same, and method for producing composite material

A composite material with graphite and a copper-titanium metal layer, manufactured via multi-axis sintering, addresses the need for high thermal conductivity and mechanical strength in heat sinks, achieving superior performance for semiconductor devices.

JP2024149121APending Publication Date: 2024-10-18UBE CORPORATION +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023062811
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing composite materials for heat sinks require higher thermal conductivity and mechanical strength to meet the demands of modern semiconductor devices, particularly in terms of workability and handling.

Method used

A composite material comprising graphite and a metal layer containing copper and titanium, with a specific volume ratio and pretreated flaky graphite particles, is manufactured using a multi-axis current sintering method to achieve high thermal conductivity and bending strength.

Benefits of technology

The composite material exhibits thermal conductivity exceeding 600 W/(m·K) and bending strength of 40 MPa or more, surpassing the performance of copper alone, suitable for applications in power semiconductor modules and LEDs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149121000002
    Figure 2024149121000002
  • Figure 2024149121000003
    Figure 2024149121000003
  • Figure 2024149121000004
    Figure 2024149121000004
Patent Text Reader

Abstract

To provide: a composite material having a higher thermal conductivity than copper alone and a bending strength equivalent to or higher than that of a member made of copper alone; a heat sink member using the same; and a method for producing the same.SOLUTION: A composite material comprises graphite and a metal layer. The graphite comprises an aggregate of flake-shaped graphite particles. The metal layer comprises copper and titanium and a titanium content in the metal layer of the composite material is 3.5 atm% or more and 24 atm% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite material, a heat sink member using the same, and a method for producing the composite material. [Background technology]

[0002] Materials for heat dissipation parts of semiconductor devices are required to have high thermal conductivity. As a material with higher and more stable thermal conductivity, a graphite-copper composite material has been proposed that includes a copper layer having an average thickness of 15 μm or less and flake graphite particles laminated via the copper layer, and has a copper volume fraction of 3 to 20% (see, for example, Patent Document 1). In this material, a higher and more stable thermal conductivity is achieved by specifying the upper limits of the average grain size of the copper crystal grains, the mass fraction of Al, and the mass fraction of Si contained in the copper layer, or by setting the gap at the interface between the copper layer and the flake graphite particles to a predetermined value or less. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 7165341 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been an increasing demand for high mechanical strength in addition to high thermal conductivity in the processed bodies such as plate-shaped heat sinks made of composite materials, from the viewpoint of processability and handling. The thermal conductivity of the composite material must be higher than that of copper alone, and the mechanical strength must be equal to or greater than that of a member made of copper alone. Therefore, an object of the present invention is to provide a composite material having a higher thermal conductivity than copper alone and a bending strength equal to or greater than that of a member made of copper alone, a heat sink member using the same, and a method for manufacturing the composite material. [Means for solving the problem]

[0005] As a result of investigations conducted by the present inventors to solve the above problems, they discovered that by mixing graphite, copper and titanium, a composite material can be obtained that has a higher thermal conductivity than copper alone and a bending strength equal to or greater than that of a member made of copper alone.

[0006] That is, the present invention is a composite material comprising graphite and a metal layer, wherein the graphite is composed of an aggregate of flake graphite particles, the metal layer contains copper and titanium, and the titanium content in the metal layer is 3.5 atm% or more and 24 atm% or less.

[0007] The present invention also relates to a heat sink member using the above-mentioned composite material.

[0008] Furthermore, the present invention provides a method for producing the aforementioned composite material, comprising the steps of: pretreating graphite particles to obtain flake graphite particles; mixing the flake graphite particles with copper particles and titanium particles to obtain a raw material for molding; and sintering the molded body obtained by molding the raw material for molding by a multi-axis electric current sintering method. Effect of the Invention

[0009] According to the present invention, it is possible to provide a composite material having a higher thermal conductivity than copper alone and a bending strength equal to or greater than that of a member made of copper alone, a heat sink member using the same, and a method for manufacturing the composite material. [Brief description of the drawings]

[0010] [Figure 1] 1 is an electron microscope photograph of a cross section of a composite material. [Diagram 2] FIG. 2 is a diagram illustrating an example of a method for forming a thin layer of graphite particles. [Diagram 3] FIG. 1 is a diagram illustrating another example of a method for forming a thin layer of graphite particles. [Figure 4] FIG. 2 is a schematic diagram illustrating a multi-axis electric current sintering apparatus. [Diagram 5]FIG. 2 is a schematic diagram illustrating a cooling substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail.

[0012] <Composite materials> As shown in the electron microscope photograph of Fig. 1, the composite material of the present invention includes graphite 11 and a metal layer 12. The graphite 11 is composed of an aggregate of flake graphite particles 11a. The metal layer 12 includes copper 13 and titanium 14. The titanium 14 may form titanium carbide with the graphite 11.

[0013] The graphite 11 is laminated via a metal layer 12 containing copper 13 and titanium 14. Furthermore, the flake graphite particles 11a in the graphite 11 are laminated via a metal layer 12 made of copper 13 or titanium 14. The metal layer 12 present in the gaps between the flake graphite particles 11a contributes to improving strength. Here, "via a metal layer 12" means that the graphite 11 or the flake graphite particles 11a are connected by the adjacent metal layer 12. In the composite material, the graphite 11 and the flake graphite particles 11a are both electrically continuous.

[0014] In the composite material, it is preferable that the metal layer 12 is three-dimensionally continuous. Three-dimensionally continuous means that the metal layer 12 is a continuous phase that exists without interruption in the three-dimensional space in the composite material. The three-dimensionally continuous metal layer 12 can be confirmed by an electron microscope or the like. In the present composite material, the metal layer 12 is three-dimensionally continuous, which is advantageous in that the thermal conductivity in the layering direction is higher than that of a graphite-metal composite material having a so-called layered structure in which the metal layer is not three-dimensionally continuous. From another perspective, the present composite material can be said to have graphite and metal layers intertwined with each other in a random manner.

[0015] The metal layer preferably occupies 3% to 20% by volume of the composite material. Since the content of graphite, which has high thermal conductivity, is as high as 80% to 97% by volume, the composite material of the present invention has very high thermal conductivity. In order to ensure high thermal conductivity and good processability, the volume ratio (graphite:metal layer) is more preferably 82:18 to 95:5. The metal layer acts as a binder in the composite material.

[0016] The titanium content in the metal layer is 3.5 atm% or more and 24 atm% or less. If the titanium content is within the above range, a composite material having both high thermal conductivity and high bending strength can be obtained. The titanium content in the metal layer is more preferably 4 atm% or more, even more preferably 5 atm% or more, even more preferably 6 atm% or more, more preferably 22 atm% or less, even more preferably 21 atm% or less, even more preferably 20 atm% or less, and even more preferably 18 atm% or less. The titanium content in the metal layer can be adjusted by the mixing ratio of raw materials during production.

[0017] Normally, the thermal conductivity of copper alone is known to be about 400 W / (m·K). The composite material of the present invention preferably has a thermal conductivity of 600 W / (m·K) or more. If the thermal conductivity is within the above range, it can be suitably used for power semiconductor modules, LEDs, etc. For use in products that require higher thermal conductivity, the thermal conductivity is more preferably 610 W / (m·K) or more, and even more preferably 640 W / (m·K) or more. The thermal conductivity is measured by cutting a sample with a predetermined dimension of 10 mm outer diameter x 2.5 mm thickness from the center of the sintered body, and measuring it using LFA447 manufactured by NETZSCH in accordance with the laser flash method (JIS H 7801:2005), and the average thermal conductivity of the samples cut from five sintered bodies is calculated.

[0018] The bending strength of a member made of copper alone is generally known to be about 30 to 50 MPa. The bending strength of the composite material of the present invention is preferably 40 MPa or more, and more preferably 45 MPa or more for use in products requiring higher mechanical strength. The bending strength in this specification is a value obtained by measuring five sintered bodies similar to those described above with reference to three-point bending measurement (JIS R 1601:2008) and calculating the average. In this way, the composite material of the present invention has a bending strength equal to or greater than that of a member made of copper alone.

[0019] <Manufacturing method> The composite material of the present invention can be produced by pretreating graphite particles to obtain the desired scaly graphite particles, mixing them with copper particles and titanium particles to obtain a molding raw material, molding this, and sintering it under predetermined conditions. Each step is described below. (Graphite pretreatment) The pretreatment of graphite particles (hereinafter sometimes referred to as "thinning") is carried out by applying shear force to the graphite particles to reduce their thickness. The graphite particles used are not particularly limited, but generally have a long side of about 10 to 2000 μm and a thickness of about 20 to 200 μm. Examples of graphite that can be used include "+3299" (manufactured by Ito Graphite Industries Co., Ltd.).

[0020] In the pretreatment, for example, as shown in FIG. 2, a sieve 21 on which graphite particles 23 are placed and a grindstone 22 capable of moving back and forth in the horizontal direction in contact with the graphite particles 23 can be used. The length of the long side of the resulting scaly graphite particles can be selected according to the mesh size of the sieve 21 used. The mesh size of the sieve 21 can be, for example, about 53 μm. The grindstone 22 is preferably a rough to medium grindstone, and is preferably one using alundum or natural diamond as abrasive grains. The graphite particles 23 are placed on the sieve 21, and the grindstone 22 is moved back and forth in the horizontal direction to apply a shear force, thereby reducing the thickness of the graphite particles 23.

[0021] Sieve 21 removes particles that have internal cavities due to shear force and particles that are brittle and easily crumble. As a result, the thickness of the resulting flake graphite particles is reduced and the density is increased. Furthermore, impurities in the graphite particles are removed, leading to improved purity. By changing the size of the abrasive grains used in the process and the mesh size of the sieve, flake graphite particles of various sizes can be obtained. For example, when sieve 21 with mesh size of 53 μm is used, flake graphite particles with long sides of 60 μm or more can be obtained.

[0022] For the pretreatment of the graphite particles, two grindstones 30a, 30b can be used as shown in FIG. 3. The grindstone 30b is a rotatable rotary grindstone. The grindstones 30a, 30b have metal plates 31a, 31b, respectively, and abrasive grains 33a, 33b made of diamond or the like are provided on the opposing surfaces. The abrasive grains 33a, 33b are fixed by bonding metal members 32a, 32b, such as plating, and the graphite particles 23 to be treated are disposed between the abrasive grains 33a, 33b. When the grindstones 30a, 30b are used to pretreat the graphite particles 13, relatively small and thin flake-like graphite particles can be efficiently obtained.

[0023] The thickness of the flake graphite particles obtained by pretreatment is, for example, 50 μm or less. The thickness shown here is the average thickness of 50 flake graphite particles after pretreatment. The flake graphite particles have a structure in which multiple graphite flakes are stacked on top of each other. The smaller the thickness of the flake graphite particles, the smaller the gaps between the graphite flakes in the graphite particles, resulting in better thermal conductivity and mechanical properties. The thickness of the flake graphite particles can be adjusted by the graphite particles used and the pretreatment conditions, etc. The smaller the thickness of the flake graphite particles, specifically, the thinner it is, 30 μm or less, the higher the thermal conductivity and the better the processability of the resulting composite material.

[0024] (Preparation of copper particles) The copper particles are not particularly specified, and for example, copper particles having a volume-based median diameter of 1.5 μm or less can be used. The median diameter of the copper particles is preferably 1.0 μm or less. When small copper particles having a median diameter of 1.5 μm or less are used, a composite material with stable thermal conductivity and processability can be obtained. The copper particles can be produced by any method. For example, the desired copper particles can be obtained by a chemical reduction method or a physical manufacturing method.

[0025] (Preparation of titanium particles) The titanium particles are not particularly limited, and for example, titanium particles having a median diameter of 25 μm or less can be used. The smaller the median diameter of the particles, the better the dispersion of titanium in the sintered body, and the more uniform the distribution of properties of the sintered body. The median diameter of the titanium particles is more preferably 10 μm or less. As the titanium particles, it is preferable to use titanium metal or titanium hydride particles.

[0026] (mixture) The flake graphite particles obtained by the pretreatment, copper particles, and titanium particles are blended in a predetermined ratio and mixed to obtain a molding raw material. Either dry mixing or wet mixing may be used for the blending. The blending ratio of the raw materials is preferably selected so that the volume ratio (graphite:metal) of graphite to metal (total of copper and titanium) in the composite material is 80:20 to 97:3. From the viewpoint of thermal conductivity and processability, it is more preferable to select the volume ratio (graphite:metal) to be 82:18 to 95:5.

[0027] Regarding titanium, the content in the metal layer is specified to be 3.5 atm% or more and 24 atm% or less. From the viewpoint of thermal conductivity and workability, the content in the metal layer is preferably selected to be 4 atm% or more and 22 atm% or less. The titanium content in the metal layer can be adjusted by weighing the raw materials of graphite, copper, and titanium. It is more preferable to select the titanium content in the metal layer to be 5 atm% or more and 20 atm% or less.

[0028] (Sintering) First, a small amount (about 40 g or less) of the molding raw material is filled into a predetermined mold and compressed at a pressure of 3 MPa to 15 MPa using, for example, a hydraulic hand press. As the mold, for example, a SUS mold with a diameter of 30 mm can be used. By repeating the filling of the molding raw material and compression, a molded body of the desired size is produced. The obtained molded body is sintered by a multi-axis electric current sintering method to obtain a sintered body that is the composite material of the present invention.

[0029] Here, an outline of the multi-axis electric current sintering apparatus will be described with reference to Fig. 4. In the multi-axis electric current sintering apparatus 40 shown in Fig. 4, a carbon mold 44 containing a compact can be fixed in a vacuum container 42 by vertical pressure shafts 45a, 45b and horizontal heating shafts (A) 47a, 47b and heating shafts (B) 49a, 49b. The heating shafts (A) 47a, 47b and heating shafts (B) 49a, 49b are configured so that electricity can be alternately applied. Electricity is applied to the heating shaft (A) in the directions of the arrows x1, x2, and to the heating shaft (B) in the directions of the arrows y1, y2.

[0030] In the multi-axis electric current sintering device 40, the pressure application axes 45a, 45b and the heating axes 47a, 47b, 49a, 49b are separate. Specifically, the pressure application axes 45a, 45b are in the z-axis direction, the heating axes (A) 47a, 47b are in the x-axis direction, and the heating axes (B) 49a, 49b are in the y-axis direction. This makes it possible to control pressure application and heating independently, thereby obtaining a uniform temperature distribution in the radial direction of the sintered portion.

[0031] For sintering, the carbon mold 44 containing the green body is fixed in the vacuum vessel 42, and then the pressure inside the vacuum vessel 42 is reduced to 100 Pa or less, preferably to 50 Pa or less to prevent oxidation and deterioration of parts inside the device. Next, while applying pressure to 10 MPa in the directions of arrows z1 and z2 by the vertical pressure shafts 45a and 45b, electricity is passed through the heating shafts (A) 47a and 47b to heat the material to 650°C to 750°C, preferably 670°C to 730°C.

[0032] During the heating process, the temperature is maintained at 550°C or higher and 650°C or lower for 1 minute or longer and 10 minutes or shorter. For example, when titanium hydride particles are used as the titanium particles, it is preferable to maintain the temperature at 600°C for 3 minutes. By maintaining the temperature at a predetermined level, the evaporation of hydrogen components in the titanium hydride is promoted. As a result, the traces of air bubbles that may remain in the composite material after sintering can be reduced and removed.

[0033] Thereafter, the heating shafts (B) 49a and 49b are switched to heat the material to 930° C. or higher and 980° C. or lower, preferably 940° C. or higher and 970° C. or lower. Furthermore, pressure is applied in the directions of arrows z1 and z2 by the vertical pressure shafts 45a and 45b. The pressure applied at this time is preferably 10 MPa or higher and 100 MPa or lower, more preferably 30 MPa or higher and 50 MPa or lower.

[0034] Multi-axis current sintering allows for uniform temperature distribution, making it possible to manufacture composite materials of stable quality. Furthermore, by using flake graphite particles, copper particles, and titanium particles obtained through pretreatment as raw materials, a composite material was obtained that has a higher thermal conductivity than copper alone and a bending strength equal to or greater than that of a member made of copper alone. By manufacturing in this way, the metal layers exist three-dimensionally in a continuous manner in the composite material.

[0035] The composite material of the present invention can be suitably used as a heat sink (heat sink member). Heat sink members are used in a wide range of fields, including wireless communication, electronic control, and optical communication. Specific applications include power semiconductor modules, optical communication modules, projectors, Peltier coolers, water-cooled coolers, and LED heat dissipation fans.

[0036] 5 shows an example of a cooling substrate using a heat sink. Cooling substrate 55 includes heat sink 50 and cooling layer 54. Heat sink 50 includes electrical insulation layer 52 and wiring layer 51, which are laminated in this order on stress buffer layer 53. Heat generating elements such as semiconductor elements are mounted on mounting surface 51a on the upper surface of wiring layer 51. The composite material of the present invention can be used for at least one of stress buffer layer 53 and wiring layer 51.

[0037] Heat generated in a heat-generating element mounted on mounting surface 51a of heat sink 50 is conducted in sequence to wiring layer 51, electrical insulation layer 52, stress buffer layer 53, and cooling layer 54, and dissipated from cooling layer 54. The composite material of the present invention has a higher thermal conductivity than copper alone, and can efficiently cool heat-generating elements to lower their temperature. Moreover, the composite material of the present invention has bending strength equal to or greater than that of a member made of copper alone, and is highly processable, so that cooling substrates can be obtained using the composite material that has been subjected to various processes. EXAMPLES

[0038] Next, the present invention will be specifically described with reference to examples, but the present invention is not limited to the following examples.

[0039] Example 1 Commercially available graphite particles were pretreated (thinned) by the method described with reference to FIG. 2. The upper and lower grindstones were equipped with diamond as abrasive grains, and 5 g of graphite particles were inserted between them together with 2 mL of water. The rotating grindstones were rotated at 10 Hz, and the graphite particles were pretreated for about 20 seconds. The pressure at that time was 0.5 MPa. The graphite particles after the treatment were classified using a sieve with 500 μm openings, and the graphite particles remaining on the sieve were taken out and dried, and these were used as the raw material flake graphite particles.

[0040] On the other hand, as the copper particles, copper particles having a median diameter of 1.5 μm produced by a chemical reduction method were prepared, and as the titanium particles, titanium hydride particles having a median diameter of 10 μm were prepared. The molding raw material was prepared so that the content of the metal layer in the sintered composite material would be 16 volume % and the content of titanium in the metal layer would be 4 atm %. Specifically, the molding raw material was obtained by mixing 18.321 g of pretreated and dried flake graphite particles, 13.282 g of copper particles, and 0.434 g of titanium hydride particles. These powders were placed in a 250 mL plastic bottle and mixed using a ball mill.

[0041] 3 g of the molding raw material was put into a SUS mold with a diameter of 30 mm and compressed at a pressure of 5 MPa using a hydraulic hand press. The process of putting in the molding raw material and compressing the powder was repeated more than 10 times, and the molded body was removed from the SUS mold.

[0042] The compact thus taken out was placed in a cylindrical carbon mold and sintered by a multi-axis electric current sintering method. A carbon mold 44 was placed in a vacuum vessel 42 of a multi-axis electric current sintering apparatus 40 shown in Fig. 4 and fixed by two diagonally arranged heating shafts (A) 47a, 47b and two pressure shafts 45a, 45b.

[0043] The inside of the vacuum vessel 42 was depressurized to 5 Pa by a rotary pump, and the temperature was raised by increasing the output of the device power supply while pressurizing to 10 MPa in the directions of the arrows z1 and z2 by the vertical pressure shafts 45a and 45b. After heating to 600°C by the heating shafts (A) 47a and 47b, the temperature was maintained for 5 minutes. After that, the temperature was raised to 700°C, and while pressurizing to 50 MPa in the directions of the arrows z1 and z2 by the vertical pressure shafts 45a and 45b, the heating shafts (B) 49a and 49b were used to heat the vessel to 950°C.

[0044] After reaching 950° C., the temperature was maintained for 30 seconds, and the power output was reduced to cool the device. After cooling, the carbon mold 44 was removed from the device, and a cylindrical sintered body was obtained from the mold. The same operation was carried out five times to prepare five sintered bodies, which were used as the composite material of Example 1.

[0045] Example 2 A composite material of Example 2 was produced in the same manner as in Example 1, except that the molding raw materials were changed so that the titanium content in the metal layer of the composite material after sintering was 8 atm %.

[0046] Example 3 A composite material of Example 3 was produced in the same manner as in Example 1, except that the molding raw materials were changed so that the titanium content in the metal layer of the composite material after sintering was 22 atm %.

[0047] Comparative Example 1 A composite material of Comparative Example 1 was produced in the same manner as in Example 1, except that the molding material was changed so that the titanium content in the metal layer of the composite material after sintering was 3 atm %.

[0048] Comparative Example 2 A composite material of Comparative Example 2 was produced in the same manner as in Example 1, except that the molding raw materials were changed so that the titanium content in the metal layer of the composite material after sintering was 25 atm %.

[0049] The samples for measuring the physical properties were prepared as follows. First, a plate was cut out vertically from the center of the cylinder of the composite material of the Example and Comparative Example. This plate was processed to obtain a sample for measuring thermal conductivity with an outer diameter of 10 mm and a thickness of 2.5 mm. The direction for measuring thermal conductivity was perpendicular to the lamination direction of the composite material (perpendicular to the pressure direction). The specimens for measuring bending strength and thermal expansion coefficient were obtained by cutting a plate from the center of the cylinder in the same manner as above, and processing it into a plate with a length of 5 mm, a width of 25 mm, and a thickness of 2 mm. For bending strength measurement, the distance between supports was set to 16 mm, but the measurement methods for each of the other measurements were as follows. Thermal conductivity: Measurement method for thermal diffusivity of metals using the laser flash method: JIS H 7801:2005 Bending strength: Room temperature bending strength test method for fine ceramics: JIS R 1601:2008 Each measurement was carried out on five samples and the average value was calculated. The results are summarized in the table below together with the composition.

[0050] [Table 1]

[0051] As shown in the above table, the composite materials of the examples have a thermal conductivity of 600 W / (m·K) or more and a bending strength of 40 MPa or more. The composite material of the example contains a specified amount of titanium in addition to flake graphite particles and copper, and therefore achieves both a thermal conductivity of 600 W / (m K) or more, higher than that of copper alone, and a bending strength of 40 MPa or more, equal to or greater than that of a member made of copper alone.

[0052] In contrast, a composite material containing a very small amount of titanium cannot obtain bending strength equal to or greater than that of a material made of copper alone (Comparative Example 1), while a composite material containing an excessive amount of titanium cannot obtain sufficient thermal conductivity (Comparative Example 2). In either case, it is not possible to obtain a composite material that has a higher thermal conductivity than copper alone and a bending strength equal to or greater than that of a member made of copper alone. [Explanation of symbols]

[0053] 11...graphite 11a...flake-like graphite particles 12...metal layer 13...copper 14...titanium 21: sieve; 22: grindstone; 23: graphite particles; 30a, 30b: grindstone 31a, 31b... Metal plate 32a, 32b... Metal member for joining 33a, 33b... Abrasive grain 40: Multi-axis electric current sintering device 42: Vacuum container 44: Carbon mold 45a, 45b...pressure shaft 47a, 47b...heating shaft 49a, 49b...heating shaft 50... heat sink plate 51... wiring layer 52... electrical insulation layer 53... stress buffer layer 54... cooling layer 55…Cooling board

Claims

1. A composite material comprising graphite and a metal layer, The graphite is composed of an aggregate of flake graphite particles, the metal layer comprises copper and titanium; The titanium content in the metal layer is 3.5 atm % or more and 24 atm % or less. A composite material comprising:

2. The composite material of claim 1 , wherein the metal layer comprises from 3% to 20% by volume of the composite material.

3. The composite material according to claim 2 , wherein the metal layer is three-dimensionally continuous.

4. A heat sink material using the composite material according to any one of claims 1 to 3.

5. A method for producing the composite material according to claim 1, comprising the steps of: A step of subjecting graphite particles to a pretreatment to obtain flake graphite particles; A step of mixing the flake graphite particles, copper particles, and titanium particles to obtain a forming raw material; a step of sintering the molded body obtained by molding the molding raw material by a multi-axis electric current sintering method; A manufacturing method comprising:

Citation Information

Patent Citations

  • Graphite-copper composite material, heat sink member using the same, and method for producing graphite-copper composite material