Bisphenol type epoxy resin composition and cured product
By adding a bisphenol derivative to bisphenol-type epoxy resin, the composition achieves enhanced storage stability at high temperatures, preventing polymerization and ring opening, thus maintaining resin quality.
Patent Information
- Application Number
- JP2023062844
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Bisphenol-type epoxy resins suffer from polymerization and ring opening at high temperatures, leading to increased epoxy equivalent and coloring, which deteriorates their quality.
Incorporating a predetermined amount of a bisphenol derivative represented by general formula (A) into the epoxy resin composition, acting as a thermal stabilizer to suppress these reactions.
The composition exhibits improved storage stability under high temperature conditions, minimizing increases in epoxy equivalent and color tone changes.
Smart Images

Figure 2024149143000001 
Figure 2024149143000002 
Figure 2024149143000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a bisphenol-type epoxy resin composition and a cured product of the bisphenol-type epoxy resin composition. [Background technology]
[0002] Bisphenol-type epoxy resins are important materials that are used in a variety of applications, such as adhesives, insulating materials, paints, casting materials, and composite materials, due to their excellent adhesive properties, electrical properties, and heat resistance.
[0003] However, when such bisphenol-type epoxy resins are stored at high temperatures for a long period of time, problems such as polymerization and ring-opening of epoxy groups tend to occur, which may result in an increase in epoxy equivalent weight or coloration, resulting in a deterioration in quality.
[0004] Known methods for improving the storage stability of bisphenol-type epoxy resins include adding a cyclic borate ester compound such as 2,2'-oxybis(5,5'-dimethyl-1,3,2-dioxaborinane) (see Patent Document 1), or a storage stabilizer such as a borate ester, phosphoric acid, an alkyl phosphate ester, or p-toluenesulfonic acid (see Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-204670 A [Patent Document 2] JP 2018-039889 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, although the above-mentioned additives can improve storage stability at room temperature (about 40° C. or less), they cannot improve storage stability at high temperatures. Therefore, there is room for improvement in the technology for storing bisphenol-type epoxy resins under high-temperature conditions without deteriorating their quality.
[0007] An object of the present invention is to provide a bisphenol-type epoxy resin composition having improved storage stability under high-temperature conditions. [Means for solving the problem]
[0008] As a result of investigations aimed at solving the above problems, the present inventors have found that the storage stability of a bisphenol-based epoxy resin under high temperature conditions can be improved by adding a predetermined amount of a bisphenol derivative to the bisphenol-based epoxy resin.
[0009] [1] Contains a bisphenol-type epoxy resin and a compound represented by general formula (A), A bisphenol-type epoxy resin composition, wherein the content of the compound represented by the general formula (A) is 0.001 mass% or more based on the total amount of the bisphenol-type epoxy resin and the compound represented by the general formula (A). [ka] (In general formula (A), R 1 represents an alkylene group having from 1 to 15 carbon atoms which may be substituted, a cycloalkanediyl group having from 3 to 15 carbon atoms which may be substituted, -SO2-, or a 9H-9,9-fluorenediyl group; R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. [2] The bisphenol-type epoxy resin composition according to [1], wherein the content of the compound represented by the general formula (A) is 1.000 mass% or less based on the total amount of the bisphenol-type epoxy resin and the compound represented by the general formula (A). [3] The bisphenol-type epoxy resin composition according to [1] or [2], wherein the bisphenol-type epoxy resin is a bisphenol A-type epoxy resin. [4] The bisphenol-type epoxy resin composition according to any one of [1] to [3], wherein the compound represented by the general formula (A) is a compound represented by the formula (A1). [ka] [5] The bisphenol-type epoxy resin composition according to any one of [1] to [4], further comprising a curing agent. [6] The bisphenol-type epoxy resin composition according to [5], wherein the content of the curing agent is 0.1 parts by mass or more and 1,000 parts by mass or less per 100 parts by mass of the bisphenol-type epoxy resin. [7] The bisphenol-type epoxy resin composition according to [5] or [6], wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, mercaptan compounds, cationic polymerization initiators, and organic phosphines. [8] A method for producing the bisphenol-type epoxy resin composition according to any one of [5] to [7], A method for producing a bisphenol-type epoxy resin composition, comprising a mixing step of mixing the bisphenol-type epoxy resin composition according to any one of [1] to [4] with the curing agent. [9] The method for producing a bisphenol-type epoxy resin composition according to [8], wherein the amount of the curing agent mixed in the mixing step is 0.1 parts by mass or more and 1,000 parts by mass or less with respect to 100 parts by mass of the bisphenol-type epoxy resin.
[10] The method for producing a bisphenol-type epoxy resin composition according to [8] or [9], wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, mercaptan compounds, cationic polymerization initiators, and organic phosphines.
[11] A cured product obtained by curing the bisphenol-type epoxy resin composition according to any one of [5] to [7].
[12] A method for producing a cured product, comprising a curing step of curing the bisphenol-type epoxy resin composition according to any one of [5] to [7].
[13] A compound represented by formula (A1). [ka] Effect of the Invention
[0010] According to the present invention, it is possible to provide a bisphenol-type epoxy resin composition having improved storage stability under high-temperature conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following is a detailed description of the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the scope of the present invention. In addition, in this specification, when a numerical value or physical property value is enclosed before and after "~", the values before and after the "~" are included.
[0012] [1. Bisphenol-type epoxy resin composition] The bisphenol-type epoxy resin composition according to the first embodiment of the present invention contains a bisphenol-type epoxy resin and a predetermined amount of a compound represented by general formula (A) (hereinafter, may be referred to as "compound (A)"). In this embodiment, compound (A) acts as a heat stabilizer and can suppress the polymerization and ring-opening of the epoxy groups of the bisphenol-type epoxy resin under high-temperature conditions, and therefore it is believed that a bisphenol-type epoxy resin composition having improved storage stability under high-temperature conditions can be obtained.
[0013] [1-1. Compound (A)] Compound (A) is a compound represented by the following general formula (A). Compound (A) is preferably a compound represented by the following general formula (A') (hereinafter, sometimes referred to as "compound (A')").
[0014] [ka]
[0015] In the general formulas (A) and (A'), R 1 represents an alkylene group having 1 to 15 carbon atoms which may have a substituent, a cycloalkanediyl group having 3 to 15 carbon atoms which may have a substituent, -SO2-, or a 9H-9,9-fluorenediyl group. 1 is preferably an alkylene group having 1 to 15 carbon atoms which may have a substituent.
[0016] The alkylene group having 1 to 15 carbon atoms, which may have a substituent, preferably has 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, and further preferably 1 to 4 carbon atoms. In this specification, the number of carbon atoms of a group which may have a substituent includes the number of carbon atoms of the substituent.
[0017] Examples of the unsubstituted alkylene group having 1 to 15 carbon atoms include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, and a hexamethylene group, and preferably a methylene group.
[0018] Examples of the substituent that the alkylene group having 1 to 15 carbon atoms may have include alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, n-pentyl, and n-hexyl groups; cycloalkyl groups having 3 to 6 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl groups; and aryl groups having 1 to 10 carbon atoms, such as phenyl, 1-naphthyl, and 2-naphthyl groups. These groups may be further substituted with halogeno groups, such as fluoro, chloro, and bromo groups.
[0019] Of these, the substituent is preferably a group selected from an alkyl group having 1 to 6 carbon atoms and an aryl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably a methyl group.
[0020] The alkylene group having 1 to 15 carbon atoms, which may have a substituent, is preferably a methylene group, a methylmethylene group, a dimethylmethylene group, a bistrifluoromethylmethylene group, an ethylmethylmethylene group, a methylphenylmethylene group, a diphenylmethylene group, or an ethylene group, and more preferably a dimethylmethylene group.
[0021] The number of carbon atoms in the cycloalkanediyl group having 3 to 15 carbon atoms is preferably 3 to 12, more preferably 6 to 12, and even more preferably 6 to 9.
[0022] Examples of the unsubstituted cycloalkanediyl group having 3 to 15 carbon atoms include a cyclopropanediyl group, a cyclobutanediyl group, a cyclopentanediyl group, and a cyclohexanediyl group. Examples of the cycloalkanediyl group include a cyclohexanyl group, a cyclohexanyl group, and a cyclooctanediyl group, and the preferred is a cyclohexanediyl group. The bonding positions of the two benzene rings in the cycloalkanediyl group are not particularly limited. Thus, the cycloalkanediyl group may be a p-membered cycloalkane-q,r-diyl (p is an integer of 3 to 15; q and r are each independently an integer of 1 to p), but it is preferred that q and r are the same integer.
[0023] The substituent that the cycloalkanediyl group having 3 to 15 carbon atoms may have is the same as the substituent that the alkylene group having 1 to 15 carbon atoms may have, and preferred embodiments thereof are also the same.
[0024] The cycloalkanediyl group having 3 to 15 carbon atoms which may have a substituent is preferably a cyclohexane-1,1-diyl group, a 3,3,5-trimethylcyclohexane-1,1-diyl group, or a 3,3,5,5-tetramethylcyclohexane-1,1-diyl group.
[0025] In the general formulas (A) and (A'), R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0026] Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and an isobutyl group.
[0027] In the general formulas (A) and (A'), a plurality of R 2 It is preferable that at least a part of R is a hydrogen atom, and all of R 2 It is more preferable that is a hydrogen atom.
[0028] Among the compounds (A), a particularly preferred one is a compound represented by the following formula (A1) (hereinafter, sometimes referred to as "compound (A1)").
[0029] [ka]
[0030] Compound (A) can be produced by combining known organic synthesis reactions using a bisphenol compound as a raw material, or compound (A) can be produced from a polycarbonate resin and epihalohydrin, as described below.
[0031] In the bisphenol type epoxy resin composition according to the present embodiment, the content of the compound (A) is usually 0.001 mass% or more, preferably 0.002 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.010 mass% or more, based on the total amount of the bisphenol type epoxy resin and the compound (A). The content of the compound (A) is not particularly limited, but is preferably 2.000 mass% or less, more preferably 1.750 mass% or less, even more preferably 1.500 mass% or less, and particularly preferably 1.000 mass% or less, based on the total amount of the bisphenol type epoxy resin and the compound (A). By setting the content of the compound (A) within the above range, the storage stability of the bisphenol type epoxy resin under high temperature conditions is improved, and the increase in the epoxy equivalent due to storage under high temperature conditions and and / or color change can be suppressed.
[0032] [1-2. Bisphenol-type epoxy resin] The bisphenol type epoxy resin is not particularly limited, but is preferably an epoxy resin represented by the following general formula (B) (hereinafter, sometimes referred to as "epoxy resin (B)"). In addition, the epoxy resin (B) is preferably an epoxy resin represented by the following general formula (B').
[0033] [ka]
[0034] R in general formula (B) and (B') 1 and R2 respectively represent R in general formula (A). 1 and R 2 The same applies to the preferred embodiments thereof.
[0035] Examples of the epoxy resin (B) include bisphenol A type epoxy resins, bisphenol C type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, bisphenol Z type epoxy resins, bisphenol S type epoxy resins, bisphenol AD type epoxy resins, bisphenol TMC type epoxy resins, and bisphenol fluorene type epoxy resins.
[0036] Among the above-mentioned bisphenol type epoxy resins, bisphenol A type epoxy resins (represented by general formula (B) or (B') and R 1 is a dimethylmethylene group, R 2 is a hydrogen atom.) is particularly preferred.
[0037] In addition, the combination of bisphenol type epoxy resin and compound (A) is R 1 and R 2 It is also preferable that the epoxy resin (B) and the compound (A) are the same in structure. A bisphenol-type epoxy resin composition containing such a combination of a bisphenol-type epoxy resin and a compound (A) can be easily produced from a polycarbonate resin and an epihalohydrin, as described later.
[0038] As the bisphenol type epoxy resin, in addition to those listed above, known bisphenol type epoxy resins can also be used.
[0039] The bisphenol type epoxy resin may be produced by a known production method or may be a commercially available product. Alternatively, the bisphenol type epoxy resin may be produced from a polycarbonate resin and an epihalohydrin, as described below.
[0040] In the technical field of the present invention, "epoxy resin" includes polymers containing repeating units and epoxy compounds with a monomolecular structure (i.e., non-polymer compounds), both of which are sometimes expressed and sold as "epoxy resins". A mixture of two or more epoxy resins may also be simply called "epoxy resin". In this specification, "epoxy resin" refers to any of polymers containing repeating units, epoxy compounds with a monomolecular structure, and mixtures thereof.
[0041] [1-3. Hardener] The bisphenol type epoxy resin composition according to the present embodiment may not contain a curing agent, but may be a curable composition containing a curing agent. The curing agent is a substance that contributes to the crosslinking reaction and / or chain extension reaction between epoxy groups of the epoxy resin (bisphenol type epoxy resin and, if necessary, other epoxy resins described later). In this embodiment, even a substance that is usually called a "curing accelerator" is considered to be a curing agent as long as it contributes to the crosslinking reaction and / or chain extension reaction between epoxy groups of the epoxy resin.
[0042] The content of the curing agent in the bisphenol-type epoxy resin composition according to this embodiment is preferably 0.1 parts by mass or more, and is also preferably 1,000 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, relative to 100 parts by mass of the bisphenol-type epoxy resin.
[0043] Furthermore, when the bisphenol-type epoxy resin composition according to the present embodiment contains other epoxy compounds described later, the content of the curing agent in the bisphenol-type epoxy resin composition is preferably 0.1 part by mass or more, and preferably 1,000 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, relative to 100 parts by mass of the total epoxy resin components as solid contents. The more preferred amounts of the curing agent are as described below depending on the type of the curing agent.
[0044] In this specification, the term "solid content" refers to the components excluding the solvent, and includes not only solid epoxy compounds but also semi-solid and viscous liquid substances. Moreover, the term "total epoxy resin components" refers to the total of the bisphenol type epoxy resin and other epoxy resins described below.
[0045] In the bisphenol-type epoxy resin composition according to the present embodiment, the curing agent is preferably at least one selected from the group consisting of polyfunctional phenols, polyisocyanate-based compounds, amine-based compounds, acid anhydride-based compounds, imidazole-based compounds, amide-based compounds, mercaptan-based compounds, cationic polymerization initiators, organic phosphines, phosphonium salts, and tetraphenylborate salts, and more preferably at least one selected from the group consisting of polyfunctional phenols, polyisocyanate-based compounds, amine-based compounds, acid anhydride-based compounds, imidazole-based compounds, amide-based compounds, mercaptan-based compounds, cationic polymerization initiators, and organic phosphines. The curing agent may be used alone or in any combination of two or more in any ratio.
[0046] Examples of polyfunctional phenols include bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; benzenediols such as catechol, resorcin, and hydroquinone; and naphthalenediols. The hydrogen atoms bonded to the aromatic rings of these compounds may be substituted with non-interfering substituents, such as halogeno groups, alkyl groups, aryl groups, ether groups, ester groups, sulfur, phosphorus, and organic substituents containing heteroelements such as silicon. In this specification, the term "benzenediols" refers to a compound having one benzene ring and two hydroxyl groups directly bonded to the benzene ring.
[0047] Further, the polyfunctional phenols include phenol, cresol, and alkylphenol. and novolak resins and resol resins which are polycondensates of phenols such as the above-mentioned polyfunctional phenols with aldehydes.
[0048] Examples of polyisocyanate compounds include tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, and lysine triisocyanate.
[0049] Further, examples of the polyisocyanate compounds include polyisocyanate compounds obtained by reacting these polyisocyanate compounds with a compound having at least two active hydrogen atoms, such as an amino group, a hydroxyl group, a carboxyl group, or water; and trimers to pentamers of the above-mentioned polyisocyanate compounds.
[0050] Examples of the amine compounds include aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines, aromatic primary amines, aromatic secondary amines, aromatic tertiary amines, cyclic amines, guanidines, and urea derivatives. More specific examples of the amine compounds include triethylenetetramine, diaminodiphenylmethane, diaminodiphenylether, metaxylenediamine, dicyandiamide, 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.
[0051] Examples of the acid anhydride compound include a condensation product of maleic anhydride and an unsaturated compound, phthalic anhydride, hexahydrophthalic anhydride, and trimellitic anhydride.
[0052] Examples of imidazole compounds include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, and benzimidazole. Although imidazole compounds also function as curing accelerators, they are classified as curing agents in this embodiment.
[0053] Examples of the amide compounds include dicyandiamide and its derivatives, and polyamide resins.
[0054] Examples of the mercaptan compound include polysulfide type mercaptan compounds, thioester type mercaptan compounds, and thioether type mercaptan compounds.
[0055] The cationic polymerization initiator generates cations by heat or irradiation with active energy rays, and examples of the initiator include aromatic onium salts. Specifically, SbF 6- , B.F. 4 -, AsF 6- , P.F. 6- , CF3SO3 2 - and B(C6F5) 4- and an aromatic cation component containing an atom selected from iodine, sulfur, nitrogen, and phosphorus. The aromatic onium salt is preferably one or more salts selected from the group consisting of diaryliodonium salts and triarylsulfonium salts.
[0056] Examples of organic phosphines include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine.
[0057] Examples of phosphonium salts include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate.
[0058] Examples of tetraphenylborate salts include 2-ethyl-4-methylimidazole·tetraphenylborate, and N-methylmorpholine·tetraphenylborate.
[0059] When at least one selected from the group consisting of polyfunctional phenols, amine compounds, and acid anhydride compounds is used as the curing agent, the amount of the curing agent used is preferably such that the equivalent ratio of the functional groups in the curing agent (the total amount of hydroxyl groups of the polyfunctional phenols, amino groups of the amine compounds, and acid anhydride groups of the acid anhydride compounds) to the total epoxy groups in the bisphenol-type epoxy resin composition is 0.8 or more and 1.5 or less.
[0060] When a polyisocyanate compound is used as a curing agent, the amount of the polyisocyanate compound used is preferably such that the equivalent ratio of the number of isocyanate groups in the polyisocyanate compound to the number of hydroxyl groups in the bisphenol-type epoxy resin composition is 0.01 or more and 1.5 or less.
[0061] When an imidazole-based compound is used as a curing agent, the amount of the imidazole-based compound used is preferably 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the total epoxy resin components as solid contents in the bisphenol-type epoxy resin composition.
[0062] When an amide-based compound is used as a curing agent, the amount of the amide-based compound used is preferably 0.1 mass % or more and 20 mass % or less based on the total amount of all epoxy resin components and the amide-based compound as solid contents in the bisphenol-type epoxy resin composition.
[0063] When a cationic polymerization initiator is used as a curing agent, the amount of the cationic polymerization initiator used is preferably 0.01 parts by mass or more and 15 parts by mass or less per 100 parts by mass of the total epoxy resin components as solid contents in the bisphenol-type epoxy resin composition.
[0064] When organic phosphines are used as the curing agent, the amount of the organic phosphines used is preferably 0.1% by mass or more and 20% by mass or less based on the total amount of all epoxy resin components and organic phosphines as solid contents in the bisphenol-type epoxy resin composition.
[0065] [1-4. Other epoxy resins] The bisphenol-type epoxy resin composition according to the present embodiment may contain an epoxy resin other than the bisphenol-type epoxy resin (hereinafter, may be referred to as "other epoxy resin").
[0066] Examples of other epoxy resins include glycidyl ether type epoxy resins such as biphenyl type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, and other polyfunctional phenol type epoxy resins; epoxy resins in which the aromatic rings of the above glycidyl ether type epoxy resins have been hydrogenated; glycidyl ester type epoxy resins; glycidyl amine type epoxy resins; linear aliphatic epoxy resins; alicyclic epoxy resins; and heterocyclic epoxy resins. The other epoxy resins may be used alone or in any combination and ratio of two or more kinds.
[0067] When the bisphenol-type epoxy resin composition according to the present embodiment contains a bisphenol-type epoxy resin and another epoxy resin, the proportion of the other epoxy resin in the total epoxy resin components as solid content in the bisphenol-type epoxy resin composition is preferably 1% by mass or more, more preferably 5% by mass or more, and is preferably 99% by mass or less, more preferably 95% by mass or less. By having the proportion of the other epoxy resin within the above range, the storage stability under high temperature conditions can be sufficiently exhibited, and the physical property improvement effect by blending the other epoxy resin can be sufficiently obtained.
[0068] [1-5. Solvents] The bisphenol-type epoxy resin composition according to the present embodiment may contain a solvent. For example, when the bisphenol-type epoxy resin composition is used for forming a coating film, it is preferable to appropriately adjust the viscosity of the bisphenol-type epoxy resin composition by diluting it with a solvent from the viewpoint of improving the handling property.
[0069] In the present embodiment, the solvent is used to ensure the handleability and / or workability in molding the bisphenol type epoxy resin composition, and the amount of the solvent used is not particularly limited. In this specification, the terms "solvent" and "solvent" are used to distinguish between the two depending on the form of use, but the terms may be used independently of each other and may be the same or different.
[0070] Examples of the solvent include inert organic solvents such as alcohols such as ethanol and isopropanol; ketones such as acetone and methyl ethyl ketone; ethers such as dioxane and ethylene glycol dimethyl ether; glycol ethers such as propylene glycol monomethyl ether; aprotic polar solvents such as dimethyl sulfoxide and dimethylformamide; and aromatic hydrocarbon solvents such as toluene and xylene. The solvent may be used alone or in any combination of two or more in any ratio.
[0071] [1-6. Other ingredients] The bisphenol type epoxy resin composition according to the present embodiment may contain other components in addition to the components listed above. Examples of other components include a curing accelerator (excluding those corresponding to the curing agent), a coupling agent, a flame retardant, an antioxidant, a light stabilizer, a plasticizer, a reactive diluent, a pigment, an inorganic filler, and an organic filler. From the viewpoint of ensuring storage stability under high temperature conditions, it is preferable that the other components are other than the curing accelerator. The above-mentioned other components can be used in appropriate combination depending on the desired physical properties of the bisphenol type epoxy resin composition.
[0072] 2. Method for producing bisphenol-type epoxy resin composition The method for producing the bisphenol-type epoxy resin composition according to the present embodiment is not particularly limited. The bisphenol-type epoxy resin composition according to the present embodiment can be produced, for example, by mixing the respective components. At this time, the order in which the respective components are mixed is not particularly limited.
[0073] Alternatively, the bisphenol-type epoxy resin composition according to the present embodiment can be produced through a composition production process in which a polycarbonate resin, an epihalohydrin, and a metal hydroxide are brought into contact with each other to react with each other. In the composition production process, the decomposition reaction of the polycarbonate resin proceeds, and the formation of the bisphenol-type epoxy resin and the compound (A) also proceeds. As a result, a bisphenol-type epoxy resin composition containing a bisphenol-type epoxy resin and the compound (A) is obtained from the polycarbonate resin and the epihalohydrin. Hereinafter, this production method will be described in more detail.
[0074] [2-1. Polycarbonate resin] The polycarbonate resin is a polymer containing a carbonate bond (-OC(=O)-O-). The polycarbonate resin is not particularly limited as long as it can produce a bisphenol type epoxy resin and compound (A) by decomposition reaction and reaction with epihalohydrin, but is preferably a polycarbonate resin having a repeating unit represented by the following general formula (C). In addition, the repeating unit represented by the following general formula (C) is preferably a repeating unit represented by the following general formula (C').
[0075] [ka]
[0076] R in general formula (C) and (C') 1 and R 2 respectively represent R in general formula (A). 1 and R2 The same applies to the preferred embodiments thereof. Therefore, the repeating unit represented by the general formula (C) is a carbonate unit (R 1 is a dimethylmethylene group, and R 2 is a hydrogen atom.
[0077] In the composition production process, it is believed that an impurity represented by the following general formula (D) is generated from the repeating unit represented by general formula (C) of the polycarbonate resin, and this impurity reacts with epihalohydrin to produce compound (A). When general formula (C) is general formula (C'), it is believed that a compound represented by the following general formula (D') is generated as an impurity represented by general formula (D), resulting in the production of compound (A').
[0078] [ka]
[0079] R in formula (D) and (D') 1 and R 2 respectively represent R in general formula (A). 1 and R 2 The same applies to the preferred embodiments thereof.
[0080] When an epoxy resin is produced from a polycarbonate resin by a conventionally known chemical recycling method, the product does not contain the compound (A), or even if it does, the amount is extremely small (less than 0.001% by mass). The reason for this is presumed to be as follows.
[0081] In the conventional chemical recycling method, polycarbonate is first recycled in the absence of epihalohydrin. A bisphenol compound is generated by decomposing the carbonate resin, and the bisphenol compound is separated and recovered. Then, the bisphenol compound is reacted with epihalohydrin to obtain an epoxy resin. In such a method, the bisphenol compound is generally separated and recovered by a crystallization method. Therefore, when the bisphenol compound is recovered by filtration or the like, the impurity represented by the general formula (D) is removed in a dissolved state in the filtrate. As a result, in the conventionally known chemical recycling method, there is no opportunity for the impurity represented by the general formula (D) to react with epihalohydrin, and it is presumed that a product not containing the compound (A) is obtained.
[0082] On the other hand, in the present production method, the decomposition reaction of the polycarbonate resin and the production of the bisphenol-type epoxy resin are carried out in a single reaction system, and therefore the compound (A) is produced without removing the impurity represented by the general formula (D). Therefore, according to the present production method, a bisphenol-type epoxy resin composition containing a bisphenol-type epoxy resin and a predetermined amount of the compound (A) can be produced.
[0083] The content of compound (A) in the bisphenol type epoxy resin composition can be adjusted to a desired range by adjusting the reaction conditions in the composition production process, particularly the reaction temperature and reaction time.
[0084] From the viewpoint of efficiently obtaining a bisphenol-type epoxy resin and compound (A), the polycarbonate resin preferably contains 70% by mass or more of the repeating unit represented by general formula (C), more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0085] The polycarbonate resin may contain other repeating units other than the repeating unit represented by the general formula (C). Examples of the other repeating units include carbonate units derived from dihydroxy compounds. More specific examples of dihydroxy compounds include biphenols such as biphenol, tetramethylbiphenol, dimethylbiphenol, and tetratert-butylbiphenol; benzenediols such as hydroquinone, methylhydroquinone, dibutylhydroquinone, resorcin, and methylresorcin; dihydroanthrahydroquinone and other dihydroxdiphenylethers such as dihydroxydiphenylether; thiodiphenols such as thiodiphenol; dihydroxynaphthalenes such as dihydroxynaphthalene; and dihydroxystilbenes such as dihydroxystilbene.
[0086] The polycarbonate resin may be used alone or in any combination of two or more kinds in any ratio.
[0087] From the viewpoint of chemical recycling, the polycarbonate resin preferably contains used polycarbonate resin that is treated as waste plastic (hereinafter, sometimes abbreviated as "waste polycarbonate resin"). It is preferable that the waste polycarbonate resin is subjected to treatment such as removal of impurities, washing, crushing, pulverization, etc., prior to being subjected to the composition production process, as necessary. As a method for removing impurities, for example, a method of dissolving waste plastic in epihalohydrin and, if necessary, an organic solvent, and filtering the resultant may be mentioned.
[0088] According to the present production method, it is possible to chemically recycle polycarbonate resin, and further, it is possible to easily obtain a bisphenol-type epoxy resin composition containing a bisphenol-type epoxy resin and a predetermined amount of compound (A). That is, the bisphenol-type epoxy resin composition according to the present embodiment has excellent storage stability under high temperature conditions, and Moreover, since it can be easily produced from waste polycarbonate resin by the above-mentioned chemical recycling method, it is also excellent in terms of environmental friendliness, workability, and economy.
[0089] [2-2. Epihalohydrin] Examples of epihalohydrin include epichlorohydrin, β-methylepichlorohydrin, epibromohydrin, etc. Among these, epihalohydrin is preferably epichlorohydrin from the viewpoints of reactivity, availability, and ability to obtain epoxy resin (B). The epihalohydrin may be used alone or in any combination and ratio of two or more kinds.
[0090] The amount of epihalohydrin used is not particularly limited, but is preferably 1.0 mol or more and 20.0 mol or less, more preferably 3.0 mol or more and 16.0 mol or less, and particularly preferably 6.0 mol or more and 14.0 mol or less per mol of carbonate bond in the polycarbonate resin. If the amount of epihalohydrin used is above the lower limit, it is preferable in that undesirable side reactions such as crosslinking reactions can be suppressed. Also, if the amount of epihalohydrin used is below the upper limit, it is preferable in that industrial production efficiency can be improved.
[0091] [2-3. Metal hydroxide] Examples of metal hydroxides include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide, and alkaline earth metal hydroxides such as magnesium hydroxide, calcium hydroxide, strontium hydroxide, and barium hydroxide. From the viewpoint of availability, the metal hydroxide is preferably an alkali metal hydroxide, and more preferably sodium hydroxide. The metal hydroxides may be used alone or in any combination of two or more in any ratio.
[0092] The supply of the metal hydroxide to the reaction system is carried out by continuously supplying a previously prepared metal hydroxide aqueous solution to the reaction system within the reaction time. The amount of the metal hydroxide used is preferably 2 to 12 moles per mole of carbonate bond in the polycarbonate resin, more preferably 2.4 to 8 moles, and particularly preferably 3 to 6 moles. When the amount of the metal hydroxide used is equal to or more than the lower limit, the reaction rate of the decomposition reaction of the polycarbonate resin and the reaction with epihalohydrin can be sufficiently ensured, which is preferable from the viewpoint of the quality and / or production efficiency of the obtained bisphenol-type epoxy resin. In addition, when the amount of the metal hydroxide used is equal to or less than the upper limit, it is preferable in that excessive reaction and side reactions such as crosslinking reaction can be suppressed.
[0093] From the viewpoint of availability, the metal hydroxide concentration of the aqueous metal hydroxide solution to be supplied to the reaction system is preferably 5% by mass or more and 50% by mass or less.
[0094] [2-4. Reaction conditions] The composition production process is carried out by dehydrating the water generated by glycidylation and the water derived from the aqueous metal hydroxide solution by subjecting the reaction solution to azeotropy while maintaining a predetermined temperature as necessary, cooling the volatilizing steam, and then separating the condensate obtained from the condensate into oil and water, and returning the oil with the water removed to the reaction system. This reduces the amount of water in the reaction system, and promotes the formation of epoxy groups by the metal hydroxide.
[0095] The method for separating epihalohydrin from the azeotropic condensate is not particularly limited, but for example, the azeotropic condensate is subjected to static separation in a static separation device, and only the epihalohydrin in the lower layer is continuously returned to the system, thereby circulating epihalohydrin. is preferably 5 mass % or less based on the total amount of charged epihalohydrin in order to maintain the molar ratio of epihalohydrin in the system.
[0096] The reaction can be carried out under reduced pressure as necessary. The pressure in the reaction system is not particularly limited, but is preferably 380 mmHg or more and 760 mmHg or less. By carrying out the reaction under reduced pressure, the azeotropic reaction between water and epihalohydrin can be promoted.
[0097] The reaction temperature is preferably 30° C. or higher and 100° C. or lower in order to ensure a sufficient reaction rate. In order to allow the reaction to proceed sufficiently, the reaction time is preferably from 10 minutes to 360 minutes, more preferably from 20 minutes to 300 minutes, and even more preferably from 30 minutes to 240 minutes.
[0098] After the reaction is completed, a post-treatment step is carried out as necessary. In the post-treatment, insoluble by-product salts are removed by filtration or by washing with water, and then unreacted epihalohydrin is removed by distillation under reduced pressure to obtain the desired bisphenol-type epoxy resin.
[0099] In addition, for the decomposition reaction of polycarbonate resin, catalysts such as quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts such as ethyltriphenylphosphonium iodide; and phosphines such as triphenylphosphine may be used.
[0100] The reaction in the composition production process may be carried out in a solvent, such as those listed in [1-5. Solvent] above.
[0101] If the amount of saponifiable halogen in the bisphenol epoxy resin obtained by the composition production process is too large, a purified bisphenol epoxy resin with a sufficiently reduced amount of saponifiable halogen can be obtained by reprocessing. That is, the crude bisphenol epoxy resin obtained by the reaction is redissolved in an inert organic solvent such as isopropyl alcohol, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dioxane, methoxypropanol, and dimethyl sulfoxide, and a solid alkali metal hydroxide or an aqueous solution of alkali metal hydroxide is added to perform a ring-closing reaction again, and then excess alkali metal hydroxide and secondary salts are removed by a method such as washing with water, and the organic solvent is distilled under reduced pressure and / or steam distilled to obtain a bisphenol epoxy resin with a reduced amount of hydrolyzable halogen. Here, the reaction temperature of the ring-closing reaction again is preferably 30°C or more and 120°C or less, more preferably 40°C or more and 110°C or less, and even more preferably 50°C or more and 100°C or less. The reaction time of the ring-closing reaction is preferably 0.1 to 8 hours, more preferably 0.3 to 7 hours, and even more preferably 0.5 to 6 hours. If the reaction temperature is too low or the reaction time is too short, the ring-closing reaction may not proceed sufficiently. If the reaction temperature is too high or the reaction time is too long, the reaction proceeds, but there is a risk of problems such as high molecular weight, high epoxy equivalent, and / or high viscosity.
[0102] The bisphenol-type epoxy resin composition obtained by the present production method does not contain a cured product. Therefore, when a composition containing a curing agent is to be obtained, a mixing step of mixing the bisphenol-type epoxy resin composition with the curing agent may be carried out. In addition, regardless of the method for producing the bisphenol-type epoxy resin and the compound (A), when producing a composition containing a curing agent, a bisphenol-type epoxy resin composition containing a bisphenol-type epoxy resin and a predetermined amount of the compound (A) but not a curing agent is mixed with the curing agent. It is preferable to carry out a mixing step in which
[0103] [3. Uses of bisphenol-type epoxy resin composition] The bisphenol-type epoxy resin composition according to this embodiment can be suitably used in the fields of paints, electric and electronic materials, adhesives, fiber reinforced plastics (FRP), and the like.
[0104] [4. Cured product] A cured product can be obtained by carrying out a curing step of curing the bisphenol-type epoxy resin composition according to the present embodiment. The bisphenol-type epoxy resin composition to be cured preferably contains the above-mentioned curing agent. The term "curing" as used herein means intentionally curing the epoxy resin with heat and / or light, and the degree of curing may be controlled depending on the desired physical properties and applications.
[0105] The curing conditions for curing the bisphenol-type epoxy resin composition according to this embodiment vary depending on the components of the bisphenol-type epoxy resin composition, the content of each component, and the shape, but typically include heating conditions of 5 seconds to 180 minutes at 50 to 200° C. This heating is preferably performed in two stages, namely, primary heating at 50 to 160° C. for 5 seconds to 30 minutes, and secondary heating at 90 to 200° C., which is 40 to 120° C. higher than the primary heating temperature, for 1 minute to 150 minutes, in order to reduce curing defects.
[0106] When producing a cured product as a semi-cured product, the curing reaction of the bisphenol-type epoxy resin composition may be allowed to proceed to an extent that allows the shape to be maintained by heating, etc. When the bisphenol-type epoxy resin composition contains a solvent, most of the solvent is removed by techniques such as heating, reducing pressure, and air drying, but 5% by mass or less of the solvent may remain in the semi-cured product. EXAMPLES
[0107] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples. Note that the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples. In the following examples, "room temperature" refers to a temperature range of 15°C or higher and 25°C or lower.
[0108] [analysis] The confirmation of the production of bisphenol-type epoxy resin and the purity and quantification of bisphenol A were carried out by high performance liquid chromatography according to the following procedures and conditions. Equipment: JASCO RHPLC, JASCO 03150-3M Unifinepak C18 3μm 150mm×3.0mmID Method: Gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Acetonitrile Solution B: Distilled water At 0 min of analysis time, the ratio of liquid A: liquid B was 30:70 (volume ratio, the same applies below), and gradually changed to liquid A: liquid B = 100:0 from 0 to 25 min of analysis time. ·Flow rate: 0.40mL / min Detection wavelength: 280nm
[0109] The following compound (A1) was identified according to the following procedures and conditions. Separation equipment: Waters AQUITY UPLC H-CLASS, JASCO Unifinepak C18 3μm 150mm×3.0mmID Method: Gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Distilled water Solution B: Acetonitrile At 0 min of analysis time, the ratio of liquid A: liquid B was 90:10 (volume ratio, the same applies below), and gradually changed to liquid A: liquid B = 100:0 from 0 to 15 min of analysis time. ·Flow rate: 0.50mL / min Detector: Xevo TQD tandem quadrupole mass spectrometer
[0110] [ka]
[0111] [Epoxy equivalent of bisphenol type epoxy resin] The epoxy equivalent of the bisphenol-type epoxy resin obtained in the examples was measured based on JIS K 7236:2009 (revised on January 20, 2009).
[0112] [Color tone of bisphenol type epoxy resin] The color tone of the bisphenol type epoxy resin was evaluated by measuring the Hazen color number (APHA) using "ZE6000" manufactured by Nippon Denshoku Industries Co., Ltd.
[0113] [Storage stability of bisphenol-type epoxy resin] The storage stability of the bisphenol-type epoxy resin was evaluated by heating a 20 mL screw bottle containing the bisphenol-type epoxy resin at 100°C for 14 days in an Espec Corporation thermostatic chamber and measuring the epoxy equivalent of the bisphenol-type epoxy resin.
[0114] (Reference Example 1) Production of bisphenol A using polycarbonate 125 parts by mass of methanol, 300 parts by mass of dimethyl carbonate, and 3 parts by mass of potassium hydroxide were placed in a jacketed separable flask equipped with a Dimroth condenser, a stirring blade, and a thermometer under a nitrogen atmosphere, and then bisphenol A polycarbonate resin (polycarbonate resin "NOVAREX" manufactured by Mitsubishi Chemical Engineering Plastics Corporation) was added. TM 200 parts by mass of "M7027BF" was added at room temperature. Thereafter, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin was observed in the reaction liquid when the temperature reached 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C., to obtain a homogeneous reaction liquid. When the composition of a portion of the resulting reaction solution was confirmed by high performance liquid chromatography, it was found that bisphenol A was produced.
[0115] Dilute sulfuric acid was added to the resulting reaction liquid to adjust the pH of the aqueous phase to 6, and the precipitated potassium sulfate was then filtered off by reduced pressure filtration to obtain an extract. The resulting liquid was transferred to a distillation apparatus equipped with a thermometer, stirring blade, distillation tube, and pressure regulator. The pressure of the distillation apparatus was changed from normal pressure (760 Torr) to 120 Torr, and the amount of distillate was observed. While this was being done, the internal temperature was raised from room temperature to 80° C., and 392 parts by mass of a distillate was distilled out. Thereafter, the pressure was restored with nitrogen, and a bottoms residue was obtained. To the resulting residue, 280 parts by mass of toluene was added to obtain a homogeneous solution at 80° C. The homogeneous solution was then gradually cooled to 5° C. to obtain a slurry liquid. The obtained slurry liquid was filtered using a centrifuge to obtain a crude cake A and a filtrate.
[0116] The entire amount of the obtained crude cake A was supplied to a jacketed separable flask equipped with a Dimroth condenser, a stirring blade, and a thermometer under a nitrogen atmosphere. Then, 280 parts by mass of toluene was supplied into the separable flask to obtain a slurry. The obtained slurry liquid was heated to 80°C to obtain a homogeneous solution. The obtained homogeneous solution was washed three times with 100 parts by mass of desalted water, and then cooled to 5°C to obtain a slurry liquid A. The obtained slurry liquid A was filtered using a centrifuge to obtain a refined cake. The entire amount of the refined cake was dried using an evaporator equipped with an oil bath at an oil bath temperature of 85°C and 15 Torr for 3 hours to obtain 121 parts by mass of a solid. When the obtained solid was confirmed by high performance liquid chromatography, the purity of bisphenol A-1 was 99.9%.
[0117] The entire amount of the filtrate obtained was dried using an evaporator equipped with an oil bath at an oil bath temperature of 85°C and 15 Torr. 50 parts by mass of toluene was added to the obtained solid to obtain slurry liquid B. The obtained slurry liquid B was filtered using a centrifuge to obtain crude cake B. The entire amount of the refined cake was dried using an evaporator equipped with an oil bath at an oil bath temperature of 85°C and 15 Torr for 3 hours to obtain 25 parts by mass of a solid. When the obtained solid was confirmed by high performance liquid chromatography, the purity of bisphenol A-2 was 95%.
[0118] [Production and evaluation of bisphenol-type epoxy resin] Example 1 A separable flask reactor equipped with a thermometer, a dropping funnel, a stirrer, a nitrogen inlet tube, and a cooling tube was filled with bisphenol A polycarbonate (polycarbonate resin "NOVAREX" manufactured by Mitsubishi Chemical Engineering Plastics Corporation). TM 75 parts by mass of "M7027BF") and 327 parts by mass of epichlorohydrin (12.0 moles per mole of carbonate bond in polycarbonate) were charged, and the mixture was heated to 100 ° C. to dissolve the polycarbonate resin. The resulting solution was allowed to cool, and then mixed with 191 parts by mass of propylene glycol monomethyl ether and 52 parts by mass of water, and heated to about 65 ° C. under a nitrogen atmosphere. Thereafter, the resulting polycarbonate resin solution was heated to 90 ° C. while continuously dropping 123 parts by mass of a 48% by mass aqueous sodium hydroxide solution so that the amount of sodium hydroxide per 1.0 mole of carbonate bond in the polycarbonate resin was 5.0 moles, and the reaction was carried out for 120 minutes. Thereafter, 223 parts by mass of water was added to the reaction solution, and the aqueous phase was separated after oil-water separation, and the salt generated by the reaction, residual sodium hydroxide, etc. were removed from the resin solution, and the reaction was stopped.
[0119] The reaction solution obtained was gradually heated while the pressure in the system was reduced, and the pressure was maintained at 150°C and 5mmHg for 30 minutes, and isopropanol and excess epichlorohydrin were completely removed from the system. Thereafter, the pressure in the system was returned to normal while nitrogen was sealed in the system, and 150 parts by mass of methyl isobutyl ketone was added to the system to obtain a methyl isobutyl ketone solution of crude resin. 100 parts by mass of water was added to this solution to separate the aqueous phase, and then the aqueous phase removed with 100 parts by mass of water was repeatedly washed with water several times until it became neutral, and a methyl isobutyl ketone solution of epoxy resin was obtained. The solution was heated while the pressure was reduced, and methyl isobutyl ketone was distilled off from this solution, and the solution was maintained at 150°C and 5mmHg for 30 minutes to completely remove methyl isobutyl ketone, and a liquid bisphenol A type epoxy resin was obtained.
[0120] The epoxy equivalent of the obtained bisphenol A type epoxy resin was 273 g / eq. A part of the obtained bisphenol A type epoxy resin was subjected to high performance liquid chromatography. When the color tone of the obtained bisphenol A type epoxy resin was measured, its APHA was 204.
[0121] The storage stability of the obtained bisphenol A type epoxy resin was confirmed. The epoxy equivalent of the bisphenol A type epoxy resin after the storage stability test was 281 g / eq, which was an increase of 8 g / eq due to the storage stability test. In addition, the color tone of the bisphenol A type epoxy resin after the storage stability test was confirmed. The APHA of the bisphenol A type epoxy resin after the storage stability test was 225, which was an increase of 21 due to the storage stability test.
[0122] Example 2 In Example 1, bisphenol A polycarbonate resin (polycarbonate resin "NOVAREX" manufactured by Mitsubishi Chemical Engineering Plastics Corporation) was used. TMA bisphenol A type epoxy resin was obtained in the same manner as in Example 1, except that bisphenol A polycarbonate resin (MUJI Polycarbonate Pinch) was used instead of bisphenol A polycarbonate resin ("M7027BF")
[0123] The epoxy equivalent of the obtained bisphenol A type epoxy resin was 206 g / eq. A part of the obtained bisphenol A type epoxy resin was confirmed by high performance liquid chromatography to contain 0.005 mass% of compound (A1). Furthermore, the color tone of the obtained bisphenol A type epoxy resin was measured, and its APHA was 211.
[0124] The storage stability of the obtained bisphenol A type epoxy resin was confirmed. The epoxy equivalent of the bisphenol A type epoxy resin after the storage stability test was 281 g / eq, which increased by 5 g / eq due to the storage stability test. The color tone of the bisphenol A type epoxy resin was also confirmed. The APHA of the bisphenol A type epoxy resin after the storage stability test was 237, which increased by 26 due to the storage stability test.
[0125] Example 3 In a 0.5L four-neck flask equipped with a thermometer, a stirrer, and a cooling tube, 5.6 parts by mass of bisphenol A-1 obtained in Reference Example 1, 9.4 parts by mass of bisphenol A-2 obtained in Reference Example 1, 84 parts by mass of epichlorohydrin, 33 parts by mass of isopropanol, and 12 parts by mass of water were charged, and the temperature was raised to 40°C to uniformly dissolve bisphenol A. While dropping 12 parts by mass of a 48.5% by mass aqueous solution of sodium hydroxide into the obtained solution over 90 minutes, the reaction temperature was raised from 40°C to 65°C over 90 minutes, and then the reaction was completed by maintaining at 65°C for 30 minutes. The reaction liquid was transferred to a 1L separatory funnel, 23 parts of water at 65°C was added, and the mixture was allowed to stand at 65°C for 1 hour. After standing, the aqueous phase was extracted from the separated oil phase and aqueous phase, and by-product salt and excess sodium hydroxide were removed. Then, epichlorohydrin was completely removed from the oil phase under reduced pressure at 150°C.
[0126] 33 parts by mass of methyl isobutyl ketone was added to the oil phase after epichlorohydrin removal, and the mixture was heated to 65°C to obtain a homogeneous solution. 0.5 parts by mass of 48.5% by mass aqueous sodium hydroxide solution was added to this solution, and the mixture was reacted for 60 minutes. 19 parts by mass of methyl isobutyl ketone was added to the reaction liquid, and the mixture was washed four times with 100 parts of water, and then the methyl isobutyl ketone was completely removed under reduced pressure at 150°C to obtain a bisphenol A type epoxy resin.
[0127] The epoxy equivalent of the obtained bisphenol A type epoxy resin was 320 g / eq. A part of the obtained bisphenol A type epoxy resin was subjected to high performance liquid chromatography. The APHA of the resulting bisphenol A epoxy resin was 216.
[0128] The storage stability of the obtained bisphenol A type epoxy resin was confirmed. The epoxy equivalent of the bisphenol A type epoxy resin after the storage stability test was 326 g / eq, which was an increase of 6 g / eq due to the storage stability test. In addition, the color tone of the bisphenol A type epoxy resin after the storage stability test was confirmed. The APHA of the bisphenol A type epoxy resin after the storage stability test was 234, which was an increase of 18 due to the storage stability test.
[0129] Example 4 A bisphenol A-type epoxy resin was obtained in the same manner as in Example 3, except that 5.6 parts by mass of bisphenol A-1 obtained in Reference Example 1 and 15 parts by mass of bisphenol A-2 obtained in Reference Example 1 were used instead of 9.4 parts by mass of bisphenol A-2 obtained in Reference Example 1.
[0130] The epoxy equivalent of the obtained bisphenol A type epoxy resin was 335g / eq. A part of the obtained bisphenol A type epoxy resin was confirmed by high performance liquid chromatography to contain 1.5% by mass of compound (A1). Furthermore, the color tone of the obtained bisphenol A type epoxy resin was measured, and its APHA was 219.
[0131] The storage stability of the obtained bisphenol A type epoxy resin was confirmed. The epoxy equivalent of the bisphenol A type epoxy resin after the storage stability test was 351 g / eq, which was an increase of 16 g / eq due to the storage stability test. In addition, the color tone of the bisphenol A type epoxy resin after the storage stability test was confirmed. The APHA of the bisphenol A type epoxy resin after the storage stability test was 272, which was an increase of 53 due to the storage stability test.
[0132] Comparative Example 1 A bisphenol A-type epoxy resin was obtained in the same manner as in Example 3, except that 5.6 parts by mass of bisphenol A-1 obtained in Reference Example 1 and 9.4 parts by mass of bisphenol A-2 obtained in Reference Example 1 were replaced with 15 parts by mass of bisphenol A-1 obtained in Reference Example 1.
[0133] The epoxy equivalent of the obtained bisphenol A type epoxy resin was 190 g / eq. In addition, when a part of the obtained bisphenol A type epoxy resin was confirmed by high performance liquid chromatography, compound (A1) was not detected (detection limit: less than 0.001 mass%). Furthermore, when the color tone of the obtained bisphenol A type epoxy resin was measured, its APHA was 209.
[0134] The storage stability of the obtained bisphenol A type epoxy resin was confirmed. The epoxy equivalent of the bisphenol A type epoxy resin after the storage stability test was 235 g / eq, which was an increase of 45 g / eq due to the storage stability test. In addition, the color tone of the bisphenol A type epoxy resin after the storage stability test was confirmed. The APHA of the bisphenol A type epoxy resin after the storage stability test was 281, which was an increase of 72 due to the storage stability test.
[0135] In Examples 1 to 4 and Comparative Example 1, the bisphenol A type epoxy resin obtained was The amount of compound (A1) contained in the bisphenol A epoxy resin composition, as well as the increase in epoxy equivalent and the increase in APHA due to the storage stability test, are summarized in Table 1. It can be seen from Table 1 that when the amount of compound (A1) contained in the bisphenol A epoxy resin composition is 0.001 mass% or more, the increase in epoxy equivalent in the storage stability test is small, and high storage stability is shown under high temperature conditions. Similarly, the increase in color tone is also small, and high color tone stability is shown under high temperature conditions.
[0136] [Table 1]
Claims
1. Contains a bisphenol-type epoxy resin and a compound represented by general formula (A), A bisphenol-type epoxy resin composition, wherein the content of the compound represented by the general formula (A) is 0.001 mass% or more based on the total amount of the bisphenol-type epoxy resin and the compound represented by the general formula (A). [Formula 1] (In general formula (A), R 1 represents an alkylene group having from 1 to 15 carbon atoms which may have a substituent, a cycloalkanediyl group having from 3 to 15 carbon atoms which may have a substituent, -SO 2 -, or a 9H-9,9-fluorenediyl group; R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
2. 2. The bisphenol-type epoxy resin composition according to claim 1, wherein the content of the compound represented by the general formula (A) is 1.000 mass% or less based on the total amount of the bisphenol-type epoxy resin and the compound represented by the general formula (A).
3. 2. The bisphenol-type epoxy resin composition according to claim 1, wherein the bisphenol-type epoxy resin is a bisphenol A-type epoxy resin.
4. 2. The bisphenol-type epoxy resin composition according to claim 1, wherein the compound represented by general formula (A) is a compound represented by formula (A1). [chemical 2]
5. The bisphenol-type epoxy resin composition according to claim 1 , further comprising a curing agent.
6. 6. The bisphenol-type epoxy resin composition according to claim 5, wherein the content of the curing agent is 0.1 parts by mass or more and 1,000 parts by mass or less per 100 parts by mass of the bisphenol-type epoxy resin.
7. 6. The bisphenol-type epoxy resin composition according to claim 5, wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate-based compounds, amine-based compounds, acid anhydride-based compounds, imidazole-based compounds, amide-based compounds, mercaptan-based compounds, cationic polymerization initiators, and organic phosphines.
8. A method for producing the bisphenol-type epoxy resin composition according to claim 5, comprising the steps of: A method for producing a bisphenol-type epoxy resin composition, comprising a mixing step of mixing the bisphenol-type epoxy resin composition according to claim 1 with the curing agent.
9. 9. The method for producing a bisphenol-type epoxy resin composition according to claim 8, wherein the amount of the curing agent mixed in the mixing step is 0.1 parts by mass or more and 1,000 parts by mass or less with respect to 100 parts by mass of the bisphenol-type epoxy resin.
10. 9. The method for producing a bisphenol-type epoxy resin composition according to claim 8, wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate-based compounds, amine-based compounds, acid anhydride-based compounds, imidazole-based compounds, amide-based compounds, mercaptan-based compounds, cationic polymerization initiators, and organic phosphines.
11. A cured product obtained by curing the bisphenol type epoxy resin composition according to any one of claims 5 to 7.
12. A method for producing a cured product, comprising a curing step of curing the bisphenol-type epoxy resin composition according to any one of claims 5 to 7.
13. A compound represented by formula (A1). [C3]
Citation Information
Patent Citations
Polycarbonate manufacturing method
JP2004537623A
Method for producing epoxy resin, method for producing epoxy resin composition, and method for producing cured product
JP2023101259A
Bisphenol production method, recycled polycarbonate resin production method, carbon dioxide production method, carbonic diester production method, epoxy resin production method, and epoxy resin cured product production method
WO2022092176A1
Polycarbonate resin decomposition method, bisphenol production method, dialkyl carbonate production method, alkyl aryl carbonate production method, diaryl carbonate production method, recycled polycarbonate resin production method, epoxy resin production method, and epoxy resin cured product production method
WO2022113847A1
Method for producing epoxy resin, method for producing epoxy resin composition, method for producing cured product, method for producing fiber-containing epoxy resin composition, method for producing diphenyl carbonate, and method for producing polycarbonate resin
WO2024209710A1