Resin composition

The resin composition addresses warpage and adhesion issues in printed wiring boards by using a balanced mix of epoxy resins and imide skeleton-containing polymers, achieving low dielectric loss and enhanced adhesion, thereby improving board performance.

JP2024149389APending Publication Date: 2024-10-18AJINOMOTO CO INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024022946
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-02-19
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing resin compositions for printed wiring boards fail to adequately suppress warpage, ensure high adhesion strength to conductor layers, and maintain low dielectric loss tangent, which affects transmission efficiency and reliability.

Method used

A resin composition comprising specific ratios of epoxy resin, epoxy resin curing agent, imide skeleton-containing polymer resins with and without a polybutadiene structure, along with optional components like inorganic fillers and curing agents, to achieve a cured product with improved adhesion and reduced dielectric loss.

Benefits of technology

The composition effectively suppresses warpage, enhances adhesion to conductor layers, and reduces dielectric loss tangent, resulting in improved performance and reliability of printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149389000001
    Figure 2024149389000001
  • Figure 2024149389000002
    Figure 2024149389000002
  • Figure 2024149389000003
    Figure 2024149389000003
Patent Text Reader

Abstract

To provide a resin composition capable of giving a cured product which can suppress warpage, is excellent in adhesion strength to a conductor layer, and has a low dielectric loss tangent.SOLUTION: The resin composition contains (A) an epoxy resin, (B) an epoxy resin curing agent, (C) an imide skeleton-containing polymer resin having a polybutadiene structure, and (D) an imide skeleton-containing polymer resin having no polybutadiene structure. The mass ratio of the component (C) to the component (D) (the content of the component (C) / the content of the component (D)) is 0.2 or more and 4 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing an epoxy resin, and further to a resin sheet, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]

[0002] A known manufacturing technique for printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked. In the build-up method, the insulating layers are generally formed by curing a resin composition containing an epoxy resin.

[0003] In order to reduce transmission loss, the insulating layer of a printed wiring board is required to have a low dielectric tangent. In addition, the insulating layer of a printed wiring board is required to suppress warping and to have high adhesion to a conductor layer. Resin compositions containing polymer resins having an imide skeleton have been known (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7194313 [Patent Document 2] Patent No. 7196275 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a resin composition and the like which is capable of giving a cured product which is suppressed in warping, has excellent adhesive strength with a conductor layer, and has a low dielectric tangent.

[0006] Means for Solving the Problems of the Invention The present inventors conducted intensive research and found that by using a resin composition comprising (A) an epoxy resin, (B) an epoxy resin curing agent, (C) an imide skeleton-containing polymer resin having a polybutadiene structure, and (D) an imide skeleton-containing polymer resin not having a polybutadiene structure, wherein the mass ratio of component (C) to component (D) (content of component (C) / content of component (D)) is 0.2 or more and 4 or less, a cured product can be obtained which is suppressed in warping, has excellent adhesive strength with a conductor layer, and has a low dielectric tangent, and thus completed the present invention. [Means for solving the problem]

[0007] That is, the present invention includes the following. [1] A resin composition comprising: (A) an epoxy resin; (B) an epoxy resin curing agent; (C) an imide skeleton-containing polymer resin having a polybutadiene structure; and (D) an imide skeleton-containing polymer resin not having a polybutadiene structure, A resin composition, in which the mass ratio of the component (C) to the component (D) (the content of the component (C) / the content of the component (D)) is 0.2 or more and 4 or less. [2] The resin composition according to the above [1], wherein the content of the butadiene structure in the component (C) is 60 mass% or more, when the component (C) is 100 mass%. [3] The resin composition according to the above [1] or [2], wherein the number average molecular weight (Mn) of component (C) is 5,000 or more. [4] The resin composition according to any one of the above [1] to [3], wherein the component (C) further has a urethane structure. [5] The resin composition according to any one of the above [1] to [4], wherein the mass ratio of the component (C) to the component (A) (the content of the component (C) / the content of the component (A)) is 0.1 or more and 0.5 or less. [6] The resin composition according to any one of the above [1] to [5], wherein the weight average molecular weight (Mw) of the component (D) is 5,000 or more. [7] The resin composition according to any one of the above [1] to [6], wherein the component (D) has a phenolic hydroxyl group. [8] The resin composition according to any one of the above [1] to [7], wherein the component (D) has a carbon skeleton derived from a dimer acid. [9] The resin composition according to the above [8], wherein the content of the carbon skeleton derived from dimer acid in the component (D) is 20% by mass or more, relative to 100% by mass of the component (D).

[10] The resin composition according to any one of the above [1] to [9], wherein a mass ratio of the component (D) to the component (A) (content of the component (D) / content of the component (A)) is 0.1 or more and 0.5 or less.

[11] The resin composition according to any one of the above [1] to

[10] , wherein the content of the component (A) is 1 mass % or more and 20 mass % or less, when the total amount of non-volatile components in the resin composition is 100 mass %.

[12] The resin composition according to any one of the above [1] to

[11] , wherein the component (B) contains a carbodiimide-based curing agent.

[13] The resin composition according to any one of the above [1] to

[12] , wherein the component (B) contains an active ester-based curing agent.

[14] The resin composition according to any one of the above [1] to

[13] , wherein the component (B) contains an active ester-based curing agent, a phenol-based curing agent, and a carbodiimide-based curing agent.

[15] The resin composition according to any one of the above [1] to

[14] , further comprising (E) an inorganic filler.

[16] The resin composition according to

[15] above, wherein the content of the component (E) is 40 mass% or more, based on 100 mass% of the non-volatile components in the resin composition.

[17] The resin composition according to any one of [1] to

[16] above, wherein, when tensile strength measurements are performed in accordance with JIS K7127, the strength at break of the cured product of the resin composition is 60 MPa or more, the elongation at break of the cured product of the resin composition is 0.5% or more, and the modulus of elasticity of the cured product of the resin composition is 20 GPa or less.

[18] The resin composition according to any one of the above [1] to

[17] , wherein a dielectric loss tangent (Df) of a cured product of the resin composition is 0.0045 or less when measured at 10 GHz and 25°C.

[19] A cured product of the resin composition according to any one of [1] to

[18] above.

[20] A resin sheet comprising: a support; and a resin composition layer formed on the support, the resin composition being any one of the resin compositions described in [1] to

[18] above.

[21] A printed wiring board comprising an insulating layer made of a cured product of the resin composition according to any one of [1] to

[18] above.

[22] A semiconductor device comprising the printed wiring board described in

[21] above. Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin composition which is capable of giving a cured product which is suppressed in warping, has excellent adhesive strength with a conductor layer, and has a low dielectric tangent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified as desired without departing from the scope of the claims and their equivalents.

[0010] <Resin composition> The resin composition of the present invention is a resin composition containing (A) an epoxy resin, (B) an epoxy resin curing agent, (C) an imide skeleton-containing polymer resin having a polybutadiene structure, and (D) an imide skeleton-containing polymer resin not having a polybutadiene structure, wherein the mass ratio of component (C) to component (D) (content of component (C) / content of component (D)) is 0.2 to 4. With such a resin composition, it is possible to obtain a cured product that is suppressed in warping, has excellent adhesive strength with a conductor layer, and has a low dielectric tangent.

[0011] The resin composition of the present invention may further contain optional components in addition to (A) the epoxy resin, (B) the epoxy resin curing agent, (C) the imide skeleton-containing polymer resin having a polybutadiene structure, and (D) the imide skeleton-containing polymer resin not having a polybutadiene structure, such as (E) an inorganic filler, (F) a curing accelerator, (G) other additives, (H) an organic solvent, etc.

[0012] Each component contained in the resin composition will be described in detail below.

[0013] <(A) Epoxy resin> The resin composition of the present invention contains an epoxy resin (A). The epoxy resin (A) may be a curable resin having an epoxy group. The epoxy resin (A) can react with an epoxy resin curing agent (B) to form a bond.

[0014] Examples of the (A) epoxy resin include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, and the like. Examples of the epoxy resin include aryl epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, isocyanurate type epoxy resin, phenolphthalimidine type epoxy resin, glycyrol type epoxy resin, alkyleneoxy skeleton-containing epoxy resin, fluorene structure-containing epoxy resin, etc. (A) Epoxy resin may be used alone or in combination of two or more.

[0015] The epoxy resin (A) preferably contains an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the epoxy resin (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0016] The (A) epoxy resin includes an epoxy resin that is liquid at a temperature of 20° C. (hereinafter sometimes referred to as a "liquid epoxy resin") and an epoxy resin that is solid at a temperature of 20° C. (hereinafter sometimes referred to as a "solid epoxy resin"). The resin composition of the present invention may contain only a liquid epoxy resin, only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin, as component (A).

[0017] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0018] Examples of liquid epoxy resins include glycirol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane dimethanol type epoxy resins, cyclic aliphatic glycidyl ethers, epoxy resins having a butadiene structure, dicyclopentadiene type epoxy resins, epoxy resins containing an alkyleneoxy skeleton, and epoxy resins containing a fluorene structure.

[0019] Specific examples of liquid epoxy resins include "EX-992L" manufactured by Nagase ChemteX Corporation; "YX7400" manufactured by Mitsubishi Chemical Corporation; "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" manufactured by Mitsubishi Chemical Corporation. " (bisphenol F type epoxy resin); "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", "604" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L", "EP-3980S" (glycidylamine type epoxy resin) manufactured by ADEKA Corporation; "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA Corporation; "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation; "EX-991L" (alkyleneoxy skeleton-containing epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin with ester skeleton) manufactured by Daicel Corporation; Examples of such epoxy resins include "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (epoxy resins having a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resins) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EG-280" (fluorene structure-containing epoxy resin) manufactured by Osaka Gas Chemicals Co., Ltd.; and "EX-201" (cyclic aliphatic glycidyl ether) manufactured by Nagase ChemteX Corporation. These may be used alone or in combination of two or more types.

[0020] As the solid epoxy resin, a solid epoxy resin having two or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0021] Examples of solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, and fluorene structure-containing epoxy resins.

[0022] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" and "N-695" (cresol novolac type epoxy resins) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; "EXA-7311", "EXA-7311-G3", and "EXA- 7311-G4, EXA-7311-G4S, HP-6000, HP-6000L (naphthylene ether type epoxy resin); Nippon Kayaku's EPPN-502H (trisphenol type epoxy resin); Nippon Kayaku's NC7000L (naphthol novolac type epoxy resin); Nippon Kayaku's NC3000H, NC3000, NC3000L, NC3000FH, NC3100 (biphenyl type epoxy resin); Nippon Steel Chemical & Material's ESN475V, ESN4100V (naphthyl type epoxy resin). phthalene type epoxy resins); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX7700" manufactured by Mitsubishi Chemical Co., Ltd. (phenol aralkyl type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene structure-containing epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.

[0023] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (A) epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably 10:1 to 1:50, more preferably 5:1 to 1:20, even more preferably 2:1 to 1:10, and particularly preferably 1:1 to 1:3.

[0024] The epoxy equivalent of the (A) epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 2,000 g / eq., even more preferably 70 g / eq. to 1,000 g / eq., and even more preferably 80 g / eq. to 500 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0025] The weight average molecular weight (Mw) of the epoxy resin (A) is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0026] The content of the (A) epoxy resin in the resin composition is not particularly limited when the resin component in the resin composition is taken as 100% by mass, but is preferably 5% by mass or more, more preferably 15% by mass or more, even more preferably 25% by mass or more, and particularly preferably 40% by mass or more, and the upper limit is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, and particularly preferably 50% by mass or less. The resin component refers to non-volatile components excluding the (E) inorganic filler described later.

[0027] The content of the (A) epoxy resin in the resin composition, assuming the non-volatile components in the resin composition to be 100 mass%, is not particularly limited, but is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and particularly preferably 8 mass% or more, and the upper limit is preferably 30 mass% or less, more preferably 20 mass% or less, even more preferably 15 mass% or less, and particularly preferably 10 mass% or less.

[0028] <(B) Epoxy resin hardener> The resin composition of the present invention contains an epoxy resin curing agent (B). The epoxy resin curing agent (B) can have a function of reacting with the epoxy resin (A) to cure it. The epoxy resin curing agent (B) may be used alone or in any combination of two or more kinds.

[0029] The (B) epoxy resin curing agent is not particularly limited, and examples thereof include active ester curing agents, phenolic curing agents, carbodiimide curing agents, acid anhydride curing agents, amine curing agents, benzoxazine curing agents, cyanate ester curing agents, and thiol curing agents. In one embodiment, the (B) epoxy resin curing agent preferably contains one or more curing agents selected from active ester curing agents, phenolic curing agents, and carbodiimide curing agents. In one embodiment, the (B) epoxy resin curing agent more preferably contains a carbodiimide curing agent. When a carbodiimide group reacts with an epoxy group, a hydroxyl group is not formed, so that the dielectric tangent of the cured product of the resin composition can be further reduced by containing a carbodiimide curing agent. In addition, the adhesive strength with the conductor layer can be further improved. Furthermore, the carbodiimide curing agent is excellent in that warpage does not increase even if the amount added is increased. In one embodiment, the (B) epoxy resin curing agent more preferably contains an active ester curing agent from the viewpoint of suppressing the dielectric tangent further. In one embodiment, the epoxy resin curing agent (B) more preferably contains a phenol-based curing agent from the viewpoint of further improving the curing property. In one embodiment, the epoxy resin curing agent (B) more preferably contains two or more curing agents selected from an active ester-based curing agent, a phenol-based curing agent, and a carbodiimide-based curing agent from the viewpoint of significantly obtaining the effects of the present invention, and it is particularly preferable that the epoxy resin curing agent (B) contains all of an active ester-based curing agent, a phenol-based curing agent, and a carbodiimide-based curing agent.

[0030] As the active ester curing agent, generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester compound is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester compound obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester compound obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0031] Specifically, the active ester curing agent is preferably a dicyclopentadiene type active ester compound, a naphthalene type active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, or an active ester compound containing a benzoylated product of phenol novolac, and more preferably at least one selected from a dicyclopentadiene type active ester compound and a naphthalene type active ester compound. As the dicyclopentadiene type active ester compound, an active ester compound containing a dicyclopentadiene type diphenol structure is preferable.

[0032] Commercially available active ester curing agents include active ester compounds containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000L-65TM", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); and active ester compounds containing a naphthalene structure, such as "HP-B-8151-62T", "EXB-8100L-65T", "EXB-9416-70BK", and "HPC-8150-62T". and "EXB-8" (manufactured by DIC Corporation); as an active ester compound containing phosphorus, "EXB9401" (manufactured by DIC Corporation); as an active ester compound which is an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation); as active ester compounds which are benzoylated products of phenol novolac, "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation); as an active ester compound containing a styryl group and a naphthalene structure, "PC1300-02-65MA" (manufactured by Air Water Corporation), etc. These may be used alone or in combination of two or more kinds.

[0033] As the phenol-based curing agent, a curing agent having one or more, preferably two or more, hydroxyl groups (phenolic hydroxyl groups) bonded to an aromatic ring such as a benzene ring or a naphthalene ring in one molecule can be used. From the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure is preferred. Also, from the viewpoint of adhesion to an adherend, a nitrogen-containing phenol-based curing agent is preferred, and a triazine skeleton-containing phenol-based curing agent is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenol novolac resin is preferred.

[0034] Specific examples of phenol-based curing agents include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel Chemical & Material Co., Ltd.; and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD-2090", "TD-2090-60M", and "KA-1160" manufactured by DIC Corporation. These may be used alone or in combination of two or more types.

[0035] Examples of the carbodiimide-based curing agent include curing agents having one or more, preferably two or more, carbodiimide structures in one molecule, such as aliphatic biscarbodiimides, such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides, such as phenylene-bis(xylylcarbodiimide); and aliphatic polycarbodiimides, such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide). and aromatic polycarbodiimides such as poly(phenylenecarbodiimide), poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide]. These may be used alone or in combination of two or more.

[0036] Commercially available carbodiimide curing agents include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Co., Ltd.; "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by LANXESS AG. These may be used alone or in combination of two or more kinds.

[0037] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule, and a curing agent having two or more acid anhydride groups in one molecule is preferable. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and the like. Anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resins in which styrene and maleic acid are copolymerized. These may be used alone or in combination of two or more.

[0038] Commercially available acid anhydride curing agents include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Resonaq; and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Cray Valley. These may be used alone or in combination of two or more types.

[0039] The amine-based curing agent may be a curing agent having one or more, preferably two or more, amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc., and among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or secondary amine, and more preferably a primary amine.

[0040] Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxyphenyl)propane. propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. The amine-based curing agent may be a commercially available product, for example, "SEIKACURE-S" manufactured by Seika Corporation; "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; "Epicure W" manufactured by Mitsubishi Chemical Corporation; and "DTDA" manufactured by Sumitomo Seika Chemicals Co., Ltd. These may be used alone or in combination of two or more types.

[0041] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation, "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd. These may be used alone or in combination of two or more types.

[0042] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which a part or all of bisphenol A dicyanate is triazine-converted to a trimer), manufactured by Arxada. These may be used alone or in combination of two or more.

[0043] Examples of thiol-based curing agents include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), tris(3-mercaptopropyl)isocyanurate, etc. These may be used alone or in combination of two or more.

[0044] The reactive group equivalent of the epoxy resin curing agent (B) is preferably 50 g / eq. to 3,000 g / eq., more preferably 100 g / eq. to 1,000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent is the mass of the epoxy resin curing agent (B) per equivalent of reactive group.

[0045] When a carbodiimide-based curing agent is included as the epoxy resin curing agent (B), the content of the carbodiimide-based curing agent in the resin composition is preferably 0.5% by mass or more or 1% by mass or more, more preferably 2.5% by mass or more, and even more preferably 5% by mass or more, when the resin component in the resin composition is taken as 100% by mass, from the viewpoint of suppressing the dielectric tangent lower and further improving the adhesive strength with the conductor layer. The upper limit is preferably 60% by mass or less or 50% by mass or less, more preferably 40% by mass or less or 30% by mass or less, even more preferably 20% by mass or less, particularly preferably 15% by mass or less, 10% by mass or less, or 6% by mass or less.

[0046] When a carbodiimide-based curing agent is included as the epoxy resin curing agent (B), the content of the carbodiimide-based curing agent in the resin composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoint of suppressing the dielectric tangent lower and further improving the adhesive strength with the conductor layer, when the non-volatile components in the resin composition are taken as 100% by mass. The upper limit is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, particularly preferably 8% by mass or less, 5% by mass or less, or 2% by mass or less.

[0047] In addition, the content of the carbodiimide-based curing agent in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of suppressing the dielectric tangent lower and further improving the adhesive strength with the conductor layer, when the epoxy resin curing agent (B) in the resin composition is taken as 100% by mass. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less or 40% by mass or less, even more preferably 30% by mass or less or 25% by mass or less, and particularly preferably 20% by mass or less.

[0048] When an active ester curing agent is included as the epoxy resin curing agent (B), the content of the active ester curing agent in the resin composition is, from the viewpoint of suppressing the dielectric tangent to a lower value, preferably 0.5% by mass or more or 1% by mass or more, more preferably 2.5% by mass or more, even more preferably 5% by mass or more, and particularly preferably 10% by mass or more, when the resin component in the resin composition is taken as 100% by mass. The upper limit is preferably 60% by mass or less, more preferably 40% by mass or less, even more preferably 20% by mass or less, and particularly preferably 15% by mass or less.

[0049] When an active ester curing agent is included as the epoxy resin curing agent (B), the content of the active ester curing agent in the resin composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and particularly preferably 2% by mass or more, from the viewpoint of suppressing the dielectric tangent lower, when the non-volatile components in the resin composition are taken as 100% by mass. The upper limit is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less, 5% by mass or less, or 3% by mass or less.

[0050] In addition, the content of the active ester curing agent in the resin composition is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 45% by mass or more, from the viewpoint of suppressing the dielectric tangent lower, when the epoxy resin curing agent (B) in the resin composition is taken as 100% by mass. The upper limit is preferably 80% by mass or less, more preferably 70% by mass or less or 60% by mass or less, and even more preferably 50% by mass or less.

[0051] (B) When a phenol-based curing agent is included as the epoxy resin curing agent, the content of the phenol-based curing agent in the resin composition, when the resin component in the resin composition is taken as 100 mass%, is preferably 2.5 mass% or more, more preferably 5 mass% or more, and even more preferably 10 mass% or more from the viewpoint of further improving the curability, and is preferably 25 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less, from the viewpoint of keeping the dielectric tangent low.

[0052] When a phenol-based curing agent is included as the (B) epoxy resin curing agent, the content of the phenol-based curing agent in the resin composition, assuming that the non-volatile components in the resin composition are 100 mass%, is preferably 0.5 mass% or more, and more preferably 1 mass% or more, from the viewpoint of further improving the curability, and is preferably 5 mass% or less, and more preferably 3 mass% or less, from the viewpoint of keeping the dielectric tangent low.

[0053] When a phenol-based curing agent is included as the (B) epoxy resin curing agent, the content of the phenol-based curing agent in the resin composition, assuming the (B) epoxy resin curing agent in the resin composition to be 100 mass%, from the viewpoint of further improving curability, is preferably 10 mass% or more, more preferably 20 mass% or more, even more preferably 30 mass% or more, and particularly preferably 35 mass% or more, and from the viewpoint of further maintaining a low dielectric tangent, is preferably 80 mass% or less, more preferably 70 mass% or less or 60 mass% or less, even more preferably 50 mass% or less, and particularly preferably 45 mass% or less.

[0054] When an active ester-based curing agent, a phenol-based curing agent, and a carbodiimide-based curing agent are all contained as the (B) epoxy resin curing agent, the total content of the active ester-based curing agent, the phenol-based curing agent, and the carbodiimide-based curing agent in the resin composition is, from the viewpoint of significantly obtaining the effects of the present invention, preferably 25% by mass or more, more preferably 50% by mass or more or 80% by mass or more, even more preferably 90% by mass or more or 95% by mass or more, and particularly preferably 99% by mass or more, when the content of the (B) epoxy resin curing agent in the resin composition is 100% by mass.

[0055] The content of the (B) epoxy resin curing agent in the resin composition, when the resin component in the resin composition is taken as 100 mass%, is not particularly limited, but is preferably 0.5 mass% or more or 1 mass% or more, more preferably 2.5 mass% or more, even more preferably 5 mass% or more or 10 mass% or more, still more preferably 15 mass% or more or 20 mass% or more, particularly preferably 25 mass% or more or 30 mass% or more, and the upper limit is preferably 60 mass% or less, more preferably 50 mass% or less, even more preferably 40 mass% or less, and particularly preferably 35 mass% or less.

[0056] The content of the (B) epoxy resin curing agent in the resin composition is not particularly limited, but is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 1 mass% or more, still more preferably 3 mass% or more, and particularly preferably 5 mass% or more, and the upper limit is preferably 30 mass% or less, more preferably 20 mass% or less, even more preferably 10 mass% or less, and particularly preferably 7 mass% or less, assuming that the non-volatile components in the resin composition are 100 mass%.

[0057] The mass ratio of the epoxy resin (B) curing agent to the epoxy resin (A) in the resin composition (content of component (B) / content of component (A)) is not particularly limited, but is preferably 0.2 or more, more preferably 0.4 or more, and particularly preferably 0.5 or more. The upper limit of the mass ratio is not particularly limited, but is preferably 2 or less, more preferably 1 or less, and particularly preferably 0.8 or less.

[0058] When the number of epoxy groups in the (A) epoxy resin is taken as 1, the range of the number of reactive groups in the (B) epoxy resin curing agent is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.3 or more, particularly preferably 0.4 or more, and preferably 5 or less, more preferably 2 or less, and even more preferably 1 or less. The "number of epoxy groups in the (A) epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the (A) epoxy resin present in the resin composition by the epoxy equivalent. The "number of reactive groups in the (B) epoxy resin curing agent" refers to the total value obtained by dividing the mass of the non-volatile components of the (B) epoxy resin curing agent present in the resin composition by the reactive group equivalent.

[0059] <(C) Imide skeleton-containing polymer resin having a polybutadiene structure> The resin composition of the present invention contains (C) an imide skeleton-containing polymer resin having a polybutadiene structure. (C) The imide skeleton-containing polymer resin having a polybutadiene structure has one or more polybutadiene structures and one or more imide skeletons in one molecule. By containing (C) the imide skeleton-containing polymer resin having a polybutadiene structure, the resin composition can suppress warping of the cured product while increasing the adhesive strength with the conductor layer. In one embodiment, (C) the imide skeleton-containing polymer resin having a polybutadiene structure preferably further has a urethane structure (-NH-CO-O-) in addition to the polybutadiene structure and the imide skeleton. (C) The imide skeleton-containing polymer resin having a polybutadiene structure may be used alone or in combination of two or more. The (C) component is a component different from the (A) component and the (B) component.

[0060] The number average molecular weight (Mn) of the imide skeleton-containing polymer resin having a polybutadiene structure (C) is preferably 1,000 or more, more preferably 5,000 or more, even more preferably 8,000 or more, and particularly preferably 10,000 or more, and the upper limit is preferably 1,000,000 or less, more preferably 500,000 or less, even more preferably 100,000 or less, even more preferably 50,000 or less, and particularly preferably 20,000 or less. The number average molecular weight (Mn) of the resin can be measured in terms of polystyrene by gel permeation chromatography (GPC).

[0061] The weight average molecular weight (Mw) of the imide skeleton-containing polymer resin having a polybutadiene structure (C) is preferably 2,000 or more, more preferably 5,000 or more or 6,000 or more, even more preferably 10,000 or more, and particularly preferably 15,000 or more, and the upper limit is preferably 1,000,000 or less, more preferably 500,000 or less, even more preferably 100,000 or less, even more preferably 70,000 or less, and particularly preferably 30,000 or less. The number average molecular weight (Mw) of the resin can be measured in terms of polystyrene by gel permeation chromatography (GPC).

[0062] The polybutadiene structure is a structure obtained by polymerizing 1,3-butadiene as a monomer, and includes a hydrogenated polybutadiene structure in which a part or all of a butadiene polymer is hydrogenated, but a non-hydrogenated polybutadiene structure is preferred. A suitable polybutadiene structure is a structure consisting of one or more repeating units selected from the 1,2-addition unit represented by the following formula (1-1), the trans-1,4-addition unit represented by the following formula (1-2), and the cis-1,4-addition unit represented by the following formula (1-3).

[0063] [ka]

[0064] In one embodiment, the content of 1,2-addition units in the polybutadiene structure is preferably 30 mol% or more, more preferably 50 mol% or more, even more preferably 70 mol% or more, still more preferably 80 mol% or more, and particularly preferably 90 mol% or more, when the total of repeating units selected from 1,2-addition units, trans-1,4-addition units, and cis-1,4-addition units is 100 mol%.

[0065] The average degree of polymerization of 1,3-butadiene in the polybutadiene structure is preferably 10 or more, more preferably 20 or more, even more preferably 30 or more, and particularly preferably 40 or more, and the upper limit is preferably 300 or less, more preferably 200 or less, even more preferably 150 or less, and particularly preferably 100 or less. The average degree of polymerization of the polybutadiene structure referred to here is the average degree of polymerization per independent polybutadiene structure present in the component (C) molecule.

[0066] The content of the butadiene structure in the imide skeleton-containing polymer resin having a polybutadiene structure (C) is preferably 30% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more, when the component (C) is taken as 100% by mass.

[0067] In one embodiment, the (C) imide skeleton-containing polymer resin having a polybutadiene structure preferably contains a polyimide resin having a polybutadiene structure. The polyimide resin referred to here means a chain polyimide resin having two or more imide skeletons in one molecule. The imide skeletons preferably exist in an inverted alternating manner in the main chain of the polyimide resin to form a repeating unit.

[0068] In one embodiment, the imide skeleton-containing polymer resin (C) having a polybutadiene structure is represented by the formula (2):

[0069] [ka]

[0070] [In the formula, X represents a divalent organic group having a polybutadiene structure and containing 10 or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming an imide), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms; Y represents a tetravalent organic group having five or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming an imide), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. It is more preferable that the resin contains an imide skeleton-containing polymer resin having a repeating unit represented by the following formula:

[0071] X represents a divalent organic group having a polybutadiene structure and containing 10 or more (preferably 10 to 3000, more preferably 10 to 1000) skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. X may be a divalent organic group having no aromatic ring, or may be a divalent organic group having an aromatic ring.

[0072] In one embodiment, the divalent organic group in X is preferably represented by the formula (X):

[0073] [ka]

[0074] [In the formula, X a and X c represents a divalent organic group consisting of five or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming an imide), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms; X b represents a divalent hydrocarbon group having a polybutadiene structure; n is 1, 2 or 3; * indicates binding site.] It is a divalent organic group represented by the formula:

[0075] X a and X c represents a divalent organic group consisting of 5 or more (preferably 5 to 200, more preferably 5 to 100, and even more preferably 5 to 50) skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. X a and X c may be a divalent organic group not having an aromatic ring, or may be a divalent organic group having an aromatic ring, but is preferably a divalent organic group having an aromatic ring.

[0076] X a and X c In one embodiment, the divalent organic group in the formula (X1) to (X5) is preferably represented by the formula (X1) to (X5):

[0077] [ka]

[0078] [In the formula, R A and R B each independently represents a substituent; a and b each independently represent 0, 1, 2, or 3; Ring X 31 , Ring X 41 , Ring X 42 , Ring X 51 , Ring X 52 and ring X 53 each independently represents an aromatic ring which may have a substituent, or a non-aromatic ring which may have a substituent; X 2a , X 3a , X 3b , X 4a , X 4b , X 4c , X 5a , X 5b , X 5c and X 5d are each independently a single bond, -C(Rx )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; R x each independently represents a hydrogen atom or an alkyl group which may be substituted with a halogen atom, or two R x are linked together to form a non-aromatic ring which may have a substituent; * indicates binding site.] is a group selected from

[0079] R A and R B each independently represents a substituent, and in one embodiment is preferably an alkyl group.

[0080] R A and R B The "substituent" in is not particularly limited, but examples include monovalent substituents such as halogen atoms, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R, -COR, -OR, -SR, -SOR, -SOR, -NHR, -N(R)2, -COOR, -OCOR, -CONH2, -CONHR, -CON(R)2, and -NHCOR (wherein each R is independently a monovalent hydrocarbon group).

[0081] A monovalent hydrocarbon group is a monovalent hydrocarbon group having one or more (preferably 1 to 50, more preferably 1 to 20) carbon atoms as skeletal atoms and hydrogen atoms as non-skeletal atoms. The monovalent hydrocarbon group may be a monovalent saturated hydrocarbon group or a monovalent unsaturated hydrocarbon group. The monovalent hydrocarbon group may or may not have an aromatic structure. Examples of the monovalent hydrocarbon group include an alkyl group, an alkenyl group, an aryl group, an aralkyl group, and an alkylaryl group.

[0082] The alkyl group means a linear, branched and / or cyclic monovalent aliphatic saturated hydrocarbon group. Unless otherwise specified, the alkyl group is preferably an alkyl group having 1 to 14 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a sec-pentyl group, a neopentyl group, a tert-pentyl group, a hexyl group, an isohexyl group, a heptyl group, an isoheptyl group, an octyl group, an isooctyl group, a tert-octyl group, a cyclopentyl group, a cyclohexyl group, and a cyclohexylmethyl group.

[0083] The alkenyl group refers to a linear, branched, and / or cyclic monovalent aliphatic unsaturated hydrocarbon group having at least one non-aromatic carbon-carbon double bond. Unless otherwise specified, the alkenyl group is preferably an alkenyl group having 2 to 14 carbon atoms, more preferably an alkenyl group having 2 to 10 carbon atoms, further preferably an alkenyl group having 2 to 6 carbon atoms, and particularly preferably an alkenyl group having 2 or 3 carbon atoms. Examples of alkenyl groups include vinyl groups, propenyl groups (allyl groups, 1-propenyl groups, isopropenyl groups), butenyl groups (1-butenyl groups, crotyl groups, methallyl groups, isocrotyl groups, etc.), pentenyl groups (1-pentenyl groups, etc.), hexenyl groups (1-hexenyl groups, etc.), heptenyl groups (1-heptenyl groups, etc.), octenyl groups (1-octenyl groups, etc.), cyclopentenyl groups (2-cyclopentenyl groups, etc.), and cyclohexenyl groups (3-cyclohexenyl groups).

[0084] The aryl group means a monovalent aromatic hydrocarbon group obtained by removing one hydrogen atom from an aromatic carbon ring. Unless otherwise specified, the aryl group is preferably an aryl group having 6 to 14 carbon atoms, more preferably an aryl group having 6 to 10 carbon atoms. Examples of the aryl group include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.

[0085] The aralkyl group means an alkyl group substituted with one or more (preferably one) aryl groups. Unless otherwise specified, the aralkyl group is preferably an aralkyl group having 7 to 15 carbon atoms, more preferably an aralkyl group having 7 to 11 carbon atoms. Examples of the aralkyl group include a benzyl group, a phenethyl group, a hydrocinnamyl group, an α-methylbenzyl group, an α-cumyl group, a 1-naphthylmethyl group, and a 2-naphthylmethyl group.

[0086] The alkylaryl group means an aryl group substituted with one or more (preferably one) alkyl groups. Unless otherwise specified, the alkylaryl group is preferably an alkylaryl group having 7 to 15 carbon atoms, more preferably an alkylaryl group having 7 to 11 carbon atoms. Examples of the alkylaryl group include a 4-methylphenyl group, a 3-methylphenyl group, a 2-methylphenyl group, a 4-ethylphenyl group, a 3-ethylphenyl group, a 2-ethylphenyl group, a 4-isopropylphenyl group, a 3-isopropylphenyl group, and a 2-isopropylphenyl group.

[0087] a and b each independently represent 0, 1, 2, or 3; in one embodiment, a is preferably 0, 1, or 2; more preferably 0 or 1; and even more preferably 0.

[0088] Ring X 31 , Ring X 41 , Ring X 42 , Ring X 51 , Ring X 52 and ring X 53 each independently represents an aromatic ring which may have a substituent, or a non-aromatic ring which may have a substituent; in one embodiment, it is preferably an aromatic ring which may have a substituent, more preferably a benzene ring which may have a substituent, and even more preferably a benzene ring which may be substituted with an alkyl group.

[0089] The aromatic ring means a ring that follows the Huckel rule, in which the number of electrons contained in the π electron system on the ring is 4p+2 (p is a natural number). The aromatic ring may be an aromatic carbocycle having only carbon atoms as ring-constituting atoms, or an aromatic heterocycle having heteroatoms such as oxygen atoms, nitrogen atoms, and sulfur atoms in addition to carbon atoms as ring-constituting atoms. In one embodiment, the aromatic ring is preferably an aromatic carbocycle. In one embodiment, the aromatic ring is preferably a 5- to 14-membered aromatic ring, more preferably a 6- to 14-membered aromatic ring, and even more preferably a 6- to 10-membered aromatic ring. Suitable specific examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, and a phenanthrene ring, and more preferably a benzene ring or a naphthalene ring, and particularly preferably a benzene ring.

[0090] The non-aromatic ring means a ring other than an aromatic ring having aromaticity in the entire ring. The non-aromatic ring may be a non-aromatic carbocycle having only carbon atoms as ring-constituting atoms, or a non-aromatic heterocycle having heteroatoms such as oxygen atoms, nitrogen atoms, and sulfur atoms as ring-constituting atoms in addition to carbon atoms. In one embodiment, the non-aromatic ring is preferably a non-aromatic carbocycle. The non-aromatic ring may be a saturated ring or an unsaturated ring. The non-aromatic ring is preferably a 3- to 21-membered non-aromatic ring, more preferably a 4- to 17-membered non-aromatic ring, and even more preferably a 5- to 14-membered non-aromatic ring. Specific preferred examples of the non-aromatic ring include monocyclic non-aromatic saturated carbon rings such as a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, and a cyclooctane ring; monocyclic non-aromatic unsaturated carbon rings such as a cyclobutene ring, a cyclopentene ring, a cyclohexene ring, a cycloheptene ring, a cyclooctene ring, a cyclopentadiene ring, and a cyclohexadiene ring; bicyclo[2.2.1]heptane ring (norbornane ring), bicyclo[4.4.0]decane ring (decalin ring), bicyclo[5.3.0]decane ring, bicyclo[4.3.0]nonane ring (hydrindane ring), bicyclo[3.2.1]octane ring, bicyclo[5.4.0]undecane ring, bicyclo[3.3.0]octane ring, bicyclo[3.3.1]nonane ring, tricyclo[5.2.1.0 2,6 ] Decane ring (tetrahydrodicyclopentadiene ring), tricyclo[3.3.1.1 3,7]Decane ring (adamantane ring), tricyclo[6.2.1.0 2,7 ] undecane ring and other bicyclic or higher non-aromatic saturated carbocyclic rings; bicyclo[2.2.1] hept-2-ene ring (norbornene ring), bicyclo[2.2.2] oct-2-ene ring, bicyclo[4.4.0] dec-2-ene ring and other bicyclic or higher non-aromatic unsaturated carbocyclic rings. The non-aromatic ring may be a non-aromatic ring partially condensed with an aromatic ring. Examples of the non-aromatic ring partially condensed with an aromatic ring include an indane ring, an indene ring, a tetralin ring, a 1,2-dihydronaphthalene ring, a 1,4-dihydronaphthalene ring, a fluorene ring, a 9,10-dihydroanthracene ring, and a 9,10-dihydrophenanthrene ring.

[0091] Ring X 31 , Ring X 41 , Ring X 42 , Ring X 51 , Ring X 52 and ring X 53 The "substituents" in the "optionally substituted aromatic ring" and the "optionally substituted non-aromatic ring" are R A and R B The substituents are the same as those in the above.

[0092] X 2a , X 3a , X 3b , X 4a , X 4b , X 4c , X 5a , X 5b , X 5c and X 5d are each independently a single bond, -C(R x )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; in one embodiment, preferably a single bond, -C(R x )2-, or -O-.

[0093] R x each independently represents a hydrogen atom or an alkyl group which may be substituted with a halogen atom, or two R xare bonded together to form a non-aromatic ring which may have a substituent; in one embodiment, they are preferably a hydrogen atom or an alkyl group which may be substituted with a halogen atom, more preferably a hydrogen atom or a methyl group which may be substituted with a halogen atom, even more preferably a hydrogen atom, a methyl group, or a trifluoromethyl group, and particularly preferably a hydrogen atom or a methyl group.

[0094] R x The "substituent" in the "non-aromatic ring which may be substituted" formed by R A and R B The substituents are the same as those in the above.

[0095] X b represents a divalent hydrocarbon group having a polybutadiene structure. A divalent hydrocarbon group having a polybutadiene structure is a divalent hydrocarbon group having only carbon atoms as skeletal atoms and hydrogen atoms as non-skeletal atoms, and has a polybutadiene structure. A divalent hydrocarbon group having a polybutadiene structure may or may not have an aromatic structure.

[0096] X b The content of the polybutadiene structure in the "divalent hydrocarbon group having a polybutadiene structure" is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, still more preferably 90% by mass or more, and particularly preferably 95% by mass or more, when the entire divalent hydrocarbon group is taken as 100% by mass.

[0097] n is 1, 2 or 3, and in one embodiment is preferably 1 or 2, and more preferably 1.

[0098] Y represents a tetravalent organic group consisting of 5 or more (preferably 5 to 200, more preferably 5 to 100, and further preferably 5 to 50) skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. Y may be a tetravalent organic group having no aromatic ring, or may be a tetravalent organic group having an aromatic ring.

[0099] In one embodiment, the tetravalent organic group for Y is preferably represented by the formulae (Y1) to (Y5):

[0100] [ka]

[0101] [In the formula, Ring Y 11 , ring Y 21 , ring Y 22 , ring Y 31 , ring Y 32 , ring Y 33 , ring Y 41 , ring Y 42 , ring Y 43 , ring Y 44 , ring Y 51 , ring Y 52 , ring Y 53 , ring Y 54 and ring Y 55 each independently represents an aromatic ring which may have a substituent, or a non-aromatic ring which may have a substituent; Y 2a , Y 3a , Y 3b , Y 4a , Y 4b , Y 4c , Y 5a , Y 5b , Y 5c and Y 5d are each independently a single bond, -C(R y )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; R yeach independently represents a hydrogen atom or an alkyl group which may be substituted with a halogen atom, or two R y are linked together to form a non-aromatic ring which may have a substituent; * indicates binding site.] The two bonding sites on the same ring represented by * are bonding sites to two adjacent carbon atoms on the ring.

[0102] Ring Y 11 , ring Y 21 , ring Y 22 , ring Y 31 , ring Y 32 , ring Y 33 , ring Y 41 , ring Y 42 , ring Y 43 , ring Y 44 , ring Y 51 , ring Y 52 , ring Y 53 , ring Y 54 and ring Y 55 each independently represents an aromatic ring which may have a substituent, or a non-aromatic ring which may have a substituent; in one embodiment, it is preferably an aromatic ring which may have a substituent, more preferably a benzene ring which may have a substituent, and even more preferably a benzene ring which may be substituted with an alkyl group.

[0103] Ring Y 11 , ring Y 21 , ring Y 22 , ring Y 31 , ring Y 32 , ring Y 33 , ring Y 41 , ring Y 42 , ring Y 43 , ring Y 44 , ring Y 51 , ring Y 52 , ring Y 53 , ring Y 54 and ring Y 55 The "substituents" in the "optionally substituted aromatic ring" and the "optionally substituted non-aromatic ring" are R A and R BThe substituents are the same as those in the above.

[0104] Y 2a , Y 3a , Y 3b , Y 4a , Y 4b , Y 4c , Y 5a , Y 5b , Y 5c and Y 5d are each independently a single bond, -C(R y )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; in one embodiment, preferably a single bond, -C(R y )2-, or -O-.

[0105] R y each independently represents a hydrogen atom or an alkyl group which may be substituted with a halogen atom, or two R y are bonded together to form a non-aromatic ring which may have a substituent; in one embodiment, they are preferably a hydrogen atom or an alkyl group which may be substituted with a halogen atom, more preferably a hydrogen atom or a methyl group which may be substituted with a halogen atom, even more preferably a hydrogen atom, a methyl group, or a trifluoromethyl group, and particularly preferably a hydrogen atom or a methyl group.

[0106] R y The "substituent" in the "non-aromatic ring which may be substituted" formed by R A and R B The substituents are the same as those in the above.

[0107] The (C) imide skeleton-containing polymer resin having a polybutadiene structure may be a commercially available product, or may be synthesized by using a known method described in JP-A-2006-37083, WO-A-2008 / 153208, or a method equivalent thereto.

[0108] The content of the (C) imide skeleton-containing polymer resin having a polybutadiene structure in the resin composition, based on 100 mass% of the resin component in the resin composition, is preferably 0.05 mass% or more, more preferably 0.5 mass% or more or 1 mass% or more, even more preferably 2.5 mass% or more, and particularly preferably 5 mass% or more, and the upper limit is preferably 40 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less.

[0109] The content of the (C) imide skeleton-containing polymer resin having a polybutadiene structure in the resin composition is, when the non-volatile components in the resin composition are taken as 100 mass%, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.5 mass% or more, and particularly preferably 1 mass% or more, and the upper limit is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 7 mass% or less, and particularly preferably 4 mass% or less.

[0110] The mass ratio of the (C) imide skeleton-containing polymer resin having a polybutadiene structure to the (A) epoxy resin in the resin composition (the (C) component content / the (A) component content) is not particularly limited, but is preferably 0.05 or more, more preferably 0.08 or more, and particularly preferably 0.1 or more. The upper limit of the mass ratio is not particularly limited, but is preferably 1.5 or less, more preferably 1 or less, and particularly preferably 0.5 or less.

[0111] <(D) Imide skeleton-containing polymer resin not having a polybutadiene structure> The resin composition of the present invention contains (D) an imide skeleton-containing polymer resin that does not have a polybutadiene structure. (D) The imide skeleton-containing polymer resin that does not have a polybutadiene structure has one or more imide skeletons in one molecule, but does not have a polybutadiene structure. By including the component (D) in the resin composition, the dielectric tangent of the cured product can be reduced. (D) The imide skeleton-containing polymer resin that does not have a polybutadiene structure may be used alone or in combination of two or more. Note that the component (D) is a component different from the components (A) and (B).

[0112] The weight average molecular weight (Mw) of the (D) imide skeleton-containing polymer resin not having a polybutadiene structure is preferably 1,000 or more, more preferably 5,000 or more, even more preferably 8,000 or more, and particularly preferably 10,000 or more, and the upper limit is preferably 1,000,000 or less, more preferably 500,000 or less, even more preferably 200,000 or less, even more preferably 100,000 or less, and particularly preferably 70,000 or less. The weight average molecular weight (Mw) of the resin can be measured in terms of polystyrene by gel permeation chromatography (GPC).

[0113] In one embodiment, the imide skeleton-containing polymer resin not having a polybutadiene structure (D) preferably has a phenolic hydroxyl group. In this embodiment, the phenolic hydroxyl value is not particularly limited, but is preferably 1 mgKOH / g or more, more preferably 4 mgKOH / g or more, and the upper limit is preferably 50 mgKOH / g or less, more preferably 20 mgKOH / g or less. The phenolic hydroxyl equivalent is preferably 3,000 g / eq. or more.

[0114] In one embodiment, the (D) imide skeleton-containing polymer resin not having a polybutadiene structure preferably has a phenolic hydroxyl group or an amino group. The phenolic hydroxyl group equivalent is preferably greater than 3,000 g / eq. The amino group equivalent is preferably greater than 3,000 g / eq.

[0115] In one embodiment, the (D) imide skeleton-containing polymer resin having no polybutadiene structure preferably contains a polyimide resin having no polybutadiene structure. The polyimide resin here means a chain-like polyimide resin having two or more imide structures in one molecule. The imide structures preferably exist in an inverted alternating manner in the main chain of the polyimide resin to form a repeating unit. In one embodiment, the polyimide resin having no polybutadiene structure preferably has a phenolic hydroxyl group at the end of the polyimide main chain. In one embodiment, the polyimide resin having no polybutadiene structure preferably has an amino group at the end of the polyimide main chain.

[0116] The (D) imide skeleton-containing polymer resin having no polybutadiene structure preferably has a carbon skeleton derived from a dimer acid, and particularly preferably has a carbon skeleton derived from a dimer acid but does not have a maleimide group (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl group). The content of the dimer acid-derived carbon skeleton in the (D) imide skeleton-containing polymer resin having no polybutadiene structure is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, when the (D) component is taken as 100% by mass.

[0117] The carbon skeleton derived from dimer acid means a carbon skeleton obtained by removing two terminal carboxyl groups (-COOH) of dimer acid, or a carbon skeleton obtained by replacing two terminal carboxyl groups (-COOH) with methylene groups (-CH2-). Dimer acid is a known compound obtained by dimerizing unsaturated fatty acids (preferably those having 11 to 22 carbon atoms, more preferably those having 14 to 20 carbon atoms, and particularly preferably those having 18 carbon atoms), and its industrial production process is almost standardized in the industry. Dimer acid is easily obtained, and is mainly composed of dimer acid having 36 carbon atoms obtained by dimerizing unsaturated fatty acids having 18 carbon atoms, such as oleic acid and linoleic acid, which are particularly inexpensive and easily available. In addition, dimer acid may contain any amount of monomer acid, trimer acid, other polymerized fatty acid, etc., depending on the production method, degree of purification, etc. In addition, although double bonds remain after the polymerization reaction of unsaturated fatty acids, in this specification, hydrogenated products in which the degree of unsaturation is reduced by further hydrogenation reaction are also included in dimer acid.

[0118] In one embodiment, the imide skeleton-containing polymer resin (D) having no polybutadiene structure is represented by the formula (3-1):

[0119] [ka]

[0120] [In the formula, X 1 represents a divalent hydrocarbon group derived from a dimer acid; Y 1 represents a tetravalent organic group consisting of five or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. It is more preferable that the polyimide resin contains a repeating unit represented by the following formula (1):

[0121] The polyimide resin having a repeating unit represented by formula (3-1) and no polybutadiene structure further contains a repeating unit represented by formula (3-2):

[0122] [ka]

[0123] [In the formula, X 2 represents a divalent organic group having five or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming an imide), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms, and having an aromatic ring; Y 2 represents a tetravalent organic group consisting of five or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. The repeating unit represented by formula (3-1) and the repeating unit represented by formula (3-2) may be randomly copolymerized or block copolymerized.

[0124] X 1 represents a divalent hydrocarbon group derived from a dimer acid. The divalent hydrocarbon group derived from a dimer acid means a divalent hydrocarbon group obtained by removing the two terminal carboxy groups (-COOH) of a dimer acid, or a divalent hydrocarbon group obtained by replacing the two terminal carboxy groups (-COOH) with a methylene group (-CH-).

[0125] Y 1 represents a tetravalent organic group consisting of 5 or more (preferably 5 to 200, more preferably 5 to 100, and even more preferably 5 to 50) skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. Y 1 may be a tetravalent organic group that does not have an aromatic ring, or may be a tetravalent organic group that has an aromatic ring.

[0126] Y 1 In one embodiment, the tetravalent organic group in the formula (Y1) is preferably a group selected from the above formulas (Y1) to (Y5).

[0127] X 2 represents a divalent organic group having an aromatic ring and consisting of five or more skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms.

[0128] X 2 In one embodiment, the divalent organic group in the formula (X1) is preferably a group selected from the above formulas (X1) to (X5).

[0129] Y 2 represents a tetravalent organic group consisting of 5 or more (preferably 5 to 200, more preferably 5 to 100, and even more preferably 5 to 50) skeletal atoms selected from carbon atoms, nitrogen atoms (not forming imides), oxygen atoms, and sulfur atoms, and non-skeletal atoms selected from hydrogen atoms and halogen atoms. Y 2 may be a tetravalent organic group that does not have an aromatic ring, or may be a tetravalent organic group that has an aromatic ring.

[0130] Y 2 In one embodiment, the tetravalent organic group in the formula (Y1) is preferably a group selected from the above formulas (Y1) to (Y5).

[0131] There are no particular limitations on the method for producing the component (D). The component (D) can be obtained, for example, by reacting a tetracarboxylic dianhydride with a diamine. Specifically, the component (D) can be obtained, for example, by (i) charging a diamine, an acid anhydride and an organic solvent into a reaction vessel and reacting them; (ii) heating at a temperature higher than that of step (i); The composition can be produced by a production method including the steps of:

[0132] In step (i), a diamine and an acid anhydride are reacted to produce a polyimide precursor. In step (i), a monoamine may be added. In step (i), for example, a separable flask may be used as a reaction vessel. Step (i) may be performed at room temperature or may be heated. An oil bath may be used for heating. When heating, the heating temperature is preferably 25 to 140°C, more preferably 50 to 120°C. The reaction time is preferably 1 to 20 hours.

[0133] In step (ii), polyimide is produced by imidization reaction of the polyimide precursor produced in step (i). The reaction temperature in step (ii) is preferably 150 to 250°C, and the heating time is preferably 5 to 15 hours. In step (ii), it is preferable to carry out the reaction while removing the generated water. Methods for removing the generated water include a method using a Dean-Stark trap and a method of adding a solvent that forms an azeotrope with water. Examples of the solvent that forms an azeotrope with water include toluene and benzene, and toluene is preferable.

[0134] The content of the (D) imide skeleton-containing polymer resin not having a polybutadiene structure in the resin composition, when the resin component in the resin composition is taken as 100 mass%, is not particularly limited, but is preferably 0.5 mass% or more or 1 mass% or more, more preferably 2.5 mass% or more, and even more preferably 5 mass% or more, and the upper limit is preferably 50 mass% or less or 40 mass% or less, more preferably 35 mass% or less or 30 mass% or less, and even more preferably 25 mass% or less or 20 mass% or less.

[0135] The content of the (D) imide skeleton-containing polymer resin not having a polybutadiene structure in the resin composition is not particularly limited, but is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more, and the upper limit is preferably 10 mass% or less, more preferably 7 mass% or less, and even more preferably 4 mass% or less, based on 100 mass% of the non-volatile components in the resin composition.

[0136] The mass ratio of the (D) imide skeleton-containing polymer resin not having a polybutadiene structure to the (A) epoxy resin in the resin composition (the (D) component content / (A) component content) is not particularly limited, but is preferably 0.05 or more, more preferably 0.08 or more, and particularly preferably 0.1 or more. The upper limit thereof is not particularly limited, but is preferably 2 or less, more preferably 1 or less, and particularly preferably 0.5 or less.

[0137] In the resin composition of the present invention, the mass ratio of the imide skeleton-containing polymer resin (C) having a polybutadiene structure to the imide skeleton-containing polymer resin (D) not having a polybutadiene structure (the content of component (C) / the content of component (D)) is 0.2 or more, preferably 0.25 or more, more preferably 0.28 or more, even more preferably 0.3 or more, and particularly preferably 0.32 or more, and the upper limit is 4 or less, preferably 3.7 or less, more preferably 3.4 or less, even more preferably 3.2 or less, and particularly preferably 3 or less.

[0138] The total content of the (A) epoxy resin, (B) epoxy resin curing agent, (C) imide skeleton-containing polymer resin having a polybutadiene structure, and (D) imide skeleton-containing polymer resin not having a polybutadiene structure, when the resin components in the resin composition are taken as 100 mass%, is not particularly limited, but is preferably 5 mass% or more, more preferably 25 mass% or more, even more preferably 50 mass% or more, still more preferably 65 mass% or more, still more preferably 80 mass% or more or 85 mass% or more, and particularly preferably 90 mass% or more, 95 mass% or more, or 99 mass% or more.

[0139] The total content of the (A) epoxy resin, (B) epoxy resin curing agent, (C) imide skeleton-containing polymer resin having a polybutadiene structure, and (D) imide skeleton-containing polymer resin not having a polybutadiene structure is not particularly limited when the non-volatile components in the resin composition are taken as 100 mass%, but is preferably 1 mass% or more, more preferably 5 mass% or more, even more preferably 10 mass% or more, still more preferably 13 mass% or more, still more preferably 17 mass% or more, and particularly preferably 19 mass% or more.

[0140] <(E) Inorganic filler> The resin composition of the present invention may contain an inorganic filler (E) as an optional component. The inorganic filler (E) may be contained in the resin composition in the form of particles.

[0141] (E) Inorganic filler materials may be inorganic compounds. (E) Inorganic filler materials may be, for example, silica, alumina, aluminosilicate, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica, alumina, or aluminosilicate is preferred, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as silica. The (E) inorganic filler may be used alone or in any combination of two or more kinds.

[0142] Examples of commercially available (E) inorganic fillers include "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellspheres" and "MGH-005" manufactured by Taiheiyo Cement Corporation; and "Sfereek" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.

[0143] The average particle size of the (E) inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less, even more preferably 1 μm or less, and particularly preferably 0.8 μm or less. The lower limit of the average particle size of the (E) inorganic filler is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more.

[0144] (E) The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the volume-based particle size distribution of the inorganic filler is measured using a flow cell method, and the average particle size is calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0145] The specific surface area of ​​the (E) inorganic filler is not particularly limited, but is preferably 0.1 m2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of ​​the (E) inorganic filler is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 50m 2 / g or less, more preferably 30m 2 / g or less, particularly preferably 10m 2 The specific surface area of ​​the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0146] (E) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. Furthermore, the surface treatment agent may be used alone or in any combination of two or more types.

[0147] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0148] From the viewpoint of improving the dispersibility of the (E) inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably with 0.2% to 3% by mass of the surface treatment agent, and even more preferably with 0.3% to 2% by mass of the surface treatment agent.

[0149] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0150] (E) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0151] The content of the (E) inorganic filler in the resin composition is, for example, 0% by mass or more, 10% by mass or more, preferably 20% by mass or more, 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, particularly preferably 70% by mass or more, and particularly preferably 75% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass. The upper limit of the content of the (E) inorganic filler is not particularly limited, but is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 83% by mass or less.

[0152] <(F) Curing accelerator> The resin composition of the present invention may further contain, as an optional component, a curing accelerator (F), which functions as a curing catalyst that accelerates the curing of the epoxy resin (A).

[0153] Examples of the (F) curing accelerator include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators. The (F) curing accelerator preferably includes an imidazole-based curing accelerator. The (F) curing accelerator may be used alone or in combination of two or more.

[0154] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitate, tetrabutylphosphonium hydrogenhexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butylmethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate ... aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of the aromatic phosphines include aromatic phosphines such as tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether. These may be used alone or in combination of two or more.

[0155] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. Examples of the aromatic dimethylureas include aromatic dimethylureas such as ethyl urea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bis dimethylurea]. These may be used alone or in combination of two or more.

[0156] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. These may be used alone or in combination of two or more.

[0157] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine. 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl- Examples of the imidazole compound include 4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.

[0158] Commercially available imidazole curing accelerators include, for example, "1B2PZ", "2E4MZ", "2MZA-PW", "2MZ-OK", "2MA-OK", "2MA-OK-PW", "2P4MZ", "2PHZ", "2PHZ-PW", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd.; and "P200-H50" manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more.

[0159] Examples of the metal-based curing accelerator include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt (II) acetylacetonate and cobalt (III) acetylacetonate, organocopper complexes such as copper (II) acetylacetonate, organozinc complexes such as zinc (II) acetylacetonate, organoiron complexes such as iron (III) acetylacetonate, organonickel complexes such as nickel (II) acetylacetonate, and organomanganese complexes such as manganese (II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate. These may be used alone or in combination of two or more.

[0160] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, etc. These may be used alone or in combination of two or more.

[0161] As the amine-based curing accelerator, a commercially available product may be used, for example, "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0162] The content of the (F) curing accelerator in the resin composition is not particularly limited, but when the resin component in the resin composition is taken as 100 mass%, it may be, for example, 0 mass% or more, 0.005 mass% or more, 0.05 mass% or more, 0.25 mass% or more, 0.5 mass% or more, etc. The upper limit of the content of the (F) curing accelerator is not particularly limited, but when the resin component in the resin composition is taken as 100 mass%, it is preferably 5 mass% or less, more preferably 2 mass% or less, even more preferably 1 mass% or less, and particularly preferably 0.7 mass% or less.

[0163] The content of the (F) curing accelerator in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be, for example, 0 mass% or more, 0.001 mass% or more, 0.01 mass% or more, 0.05 mass% or more, etc. The upper limit of the content of the (F) curing accelerator is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it is preferably 5 mass% or less, more preferably 2 mass% or less, even more preferably 1 mass% or less, and particularly preferably 0.5 mass% or less.

[0164] <(G) Other Additives> The resin composition of the present invention may further contain (G) other additives as optional components. (G) other additives include, for example, radical polymerization initiators such as peroxide radical polymerization initiators and azo radical polymerization initiators; thermoplastic resins such as phenoxy resins; organometallic compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, and diazo yellow; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone leveling agents and acrylic polymer leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone defoamers, acrylic defoamers, fluorine defoamers, and vinyl resin defoamers; ultraviolet absorbers such as benzotriazole ultraviolet absorbers; adhesion improvers such as urea silane; and triazoles. Adhesion imparting agents such as tetrazole adhesion imparting agents and triazine adhesion imparting agents; antioxidants such as hindered phenol antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine surfactants and silicone surfactants; flame retardants such as phosphorus flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen flame retardants (e.g., melamine sulfate), and halogen flame retardants; dispersants such as phosphate ester dispersants, polyoxyalkylene dispersants, acetylene dispersants, silicone dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate stabilizers, titanate stabilizers, aluminate stabilizers, zirconate stabilizers, isocyanate stabilizers, and carboxylic acid stabilizers. (G) Other additives may be used alone or in combination of two or more. The components (A) to (F) may have functions such as a radical polymerization initiator, a thermoplastic resin, a colorant, a polymerization inhibitor, a leveling agent, an antifoaming agent, an ultraviolet absorber, an adhesion improver, an adhesion imparting agent, an antioxidant, a fluorescent whitening agent, a surfactant, a flame retardant, a dispersant, a stabilizer, etc. In such a case, the component is regarded as each of the components (A) to (F) rather than the component (G). For example, an example of the component (B) that can function as a stabilizer is a carboxylic acid anhydride stabilizer.

[0165] <(H) Organic Solvent> The resin composition of the present invention may further contain (H) an organic solvent as an optional volatile component. Examples of (H) organic solvents include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methoxypropionic acid. Examples of the organic solvent include ether ester solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent (H) may be used alone or in combination of two or more.

[0166] The content of the (H) organic solvent in the varnish-like resin composition before drying is not particularly limited, but is, for example, 40% by mass or less, preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, when the total components of the resin composition are 100% by mass. The content of the (H) organic solvent in the resin composition after drying to form a resin composition layer in a resin sheet is not particularly limited, but is, when the total components of the resin composition are 100% by mass, preferably 5% by mass or less, more preferably 4% by mass or less, even more preferably 3% by mass or less, and especially preferably 2% by mass or less. The content of the (H) organic solvent may be 0% by mass.

[0167] <Method of producing resin composition> The resin composition of the present invention can be produced, for example, by adding (A) epoxy resin, (B) epoxy resin curing agent, (C) imide skeleton-containing polymer resin having a polybutadiene structure, (D) imide skeleton-containing polymer resin not having a polybutadiene structure, (E) inorganic filler if necessary, (F) curing accelerator if necessary, (G) other additives if necessary, and (H) organic solvent if necessary in any order and / or all at once and mixing them in any preparation vessel. In addition, the temperature can be appropriately set during the process of adding and mixing each component, and heating and / or cooling may be performed temporarily or throughout. In addition, during or after the process of adding and mixing, the resin composition may be stirred or shaken using a stirring device or shaking device such as a mixer to disperse uniformly. In addition, degassing may be performed under low pressure conditions such as under vacuum at the same time as stirring or shaking.

[0168] <Characteristics of resin composition> The resin composition of the present invention contains (A) an epoxy resin, (B) an epoxy resin curing agent, (C) an imide skeleton-containing polymer resin having a polybutadiene structure, and (D) an imide skeleton-containing polymer resin not having a polybutadiene structure, and the mass ratio of component (C) to component (D) (content of component (C) / content of component (D)) is from 0.2 to 4. With such a resin composition, it is possible to obtain a cured product that is suppressed in warping, has excellent adhesive strength with a conductor layer, and has a low dielectric tangent.

[0169] According to the resin composition of the present invention, it is possible to suppress warpage when a cured layer (insulating layer) of the resin composition is formed on a substrate such as a silicon wafer. For example, when a laminate is produced and the amount of warpage is measured as in Test Example 4 described later, the amount of warpage can be preferably less than 2200 μm or less than 2000 μm, more preferably 1700 μm or less.

[0170] According to the resin composition of the present invention, it is possible to obtain a cured product (insulating layer) having excellent adhesive strength with a conductor layer. For example, when a conductor layer is formed as in Test Example 3 described later, the adhesive strength of the cured product of the resin composition with the conductor layer is preferably 400 kgf / cm 2 More preferably, 500kgf / cm 2 More preferably, 550 kgf / cm 2 More preferably, 600kgf / cm 2 More preferably, 650 kgf / cm 2 More preferably, 700 kgf / cm 2 It could be more than that.

[0171] The cured product of the resin composition of the present invention has a low dielectric loss tangent. For example, the dielectric loss tangent (Df) of the cured product of the resin composition measured at 10 GHz and 25° C. as in Test Example 2 described later may be preferably 0.0100 or less, more preferably 0.0070 or less, even more preferably 0.0055 or less or 0.0050 or less, even more preferably 0.0045 or less, and particularly preferably 0.0040 or less. In addition, for example, the dielectric loss tangent (Df) of the cured product of the resin composition measured at 10 GHz and 100° C. as in Test Example 2 described later may be preferably 0.0100 or less, more preferably 0.0070 or less, even more preferably 0.0060 or less, even more preferably 0.0055 or less, and particularly preferably 0.0050 or less.

[0172] In one embodiment, the cured product of the resin composition of the present invention may have excellent mechanical strength. For example, the strength at break of the cured product of the resin composition when the tensile strength is measured according to JIS K7127 as in Test Example 1 described later may be preferably 50 MPa or more, more preferably 60 MPa or more, even more preferably 65 MPa or more, even more preferably 70 MPa or more, and particularly preferably 75 MPa or more. For example, the elongation at break of the cured product of the resin composition when the tensile strength is measured according to JIS K7127 as in Test Example 1 described later may be preferably 0.5% or more, more preferably 0.8% or more, and particularly preferably 1.0% or more. For example, the modulus of elasticity of the cured product of the resin composition when the tensile strength is measured according to JIS K7127 as in Test Example 1 described later may be preferably 30 GPa or less, more preferably 25 GPa or less, even more preferably 20 GPa or less, even more preferably 17 GPa or less, and particularly preferably 15 GPa or less.

[0173] <Applications of resin composition> The resin composition of the present invention can be suitably used as a resin composition for insulating purposes, particularly as a resin composition for forming an insulating layer. Specifically, it can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer for forming a conductor layer) for forming a conductor layer (including a rewiring layer) formed on an insulating layer. In addition, in a printed wiring board described later, it can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for forming an insulating layer of a printed wiring board). The resin composition of the present invention can also be used in a wide range of applications requiring a resin composition, such as a resin sheet, a sheet-like laminate material such as a prepreg, a solder resist, an underfill material, a die bonding material, a semiconductor encapsulant, a hole filling resin, and a component embedding resin.

[0174] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can be suitably used as a resin composition for a rewiring formation layer (resin composition for forming a rewiring formation layer) as an insulating layer for forming a rewiring layer, and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A step of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0175] Furthermore, the resin composition of the present invention provides an insulating layer with good component embedding properties, and therefore can be suitably used when the printed wiring board is a circuit board with built-in components.

[0176] <Sheet-type laminated material> The resin composition of the present invention can be used by coating in the form of a varnish, but from an industrial perspective, it is generally preferred to use the resin composition in the form of a sheet-like laminate material containing the resin composition.

[0177] As the sheet-like laminate material, the following resin sheets and prepregs are preferred.

[0178] In one embodiment, the resin sheet includes a support and a resin composition layer provided on the support, and the resin composition layer is formed from the resin composition of the present invention.

[0179] The thickness of the resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but may be, for example, 5 μm or more, 10 μm or more, etc.

[0180] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0181] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate (PC), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0182] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0183] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0184] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Commercially available release agents include "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation. In addition, the support with a release layer may be a commercially available product, for example, "Lumirror T60" and "Lumirror R80" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Ltd., and "Unipeel" manufactured by Unitika Ltd., which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0185] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0186] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0187] The resin sheet can be produced, for example, by preparing a liquid (varnish-like) resin composition as is or by dissolving the resin composition in an organic solvent to prepare a liquid (varnish-like) resin composition, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.

[0188] The organic solvent may be the same as the organic solvent described as a component of the resin composition. The organic solvent may be used alone or in combination of two or more kinds.

[0189] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin composition, for example, when a resin composition containing 30 mass % to 60 mass % of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0190] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0191] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with the resin composition of the present invention.

[0192] The sheet-like fiber substrate used for the prepreg is not particularly limited, and can be a substrate commonly used for prepreg, such as glass cloth, aramid nonwoven fabric, or liquid crystal polymer nonwoven fabric. From the viewpoint of thinning the printed wiring board, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited, and can be, for example, 10 μm or more.

[0193] The thickness of the prepreg may be in the same range as that of the resin composition layer in the above-mentioned resin sheet.

[0194] The sheet-like laminate material of the present invention can be suitably used for forming an insulating layer of a printed wiring board (for an insulating layer of a printed wiring board), and can be more suitably used for forming an interlayer insulating layer of a printed wiring board (for an interlayer insulating layer of a printed wiring board).

[0195] <Printed wiring board> The printed wiring board of the present invention includes an insulating layer made of a cured product obtained by curing the resin composition of the present invention.

[0196] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate such that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of curing (e.g., heat curing) the resin composition layer to form an insulating layer.

[0197] The "inner layer substrate" used in step (I) is a member that becomes the substrate of the printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0198] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.

[0199] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.

[0200] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0201] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0202] The support may be removed between step (I) and step (II) or after step (II).

[0203] In step (II), the resin composition layer is cured (for example, thermally cured) to form an insulating layer made of a cured product of the resin composition. The curing conditions for the resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a printed wiring board may be used.

[0204] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but in one embodiment, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0205] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. to 120° C., preferably 60° C. to 115° C., more preferably 70° C. to 110° C. for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.

[0206] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (II) to (V) may be repeated to form a multilayer wiring board, as necessary.

[0207] In another embodiment, the printed wiring board of the present invention can be manufactured using the above-mentioned prepreg. The manufacturing method is basically the same as when a resin sheet is used.

[0208] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.

[0209] Step (IV) is a step of roughening the insulating layer. Usually, smears are also removed in this step (IV). The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by carrying out a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.

[0210] The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, etc., and is preferably an alkaline solution, and more preferably a sodium hydroxide solution or a potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes, for example. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.

[0211] The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.

[0212] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product such as "Reduction Solution Securigant P" manufactured by Atotech Japan can be mentioned.

[0213] The treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.

[0214] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is not particularly limited, but is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The root mean square roughness (Rq) of the insulating layer surface after the roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.

[0215] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0216] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0217] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0218] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0219] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0220] In another embodiment, the conductor layer may be formed using a metal foil. When the conductor layer is formed using a metal foil, it is preferable to carry out step (V) between steps (I) and (II). For example, after step (I), the support is removed, and a metal foil is laminated on the exposed surface of the resin composition layer. The lamination of the resin composition layer and the metal foil may be carried out by a vacuum lamination method. The lamination conditions may be the same as those described for step (I). Next, step (II) is carried out to form an insulating layer. Thereafter, a conductor layer having a desired wiring pattern can be formed by a conventionally known technique such as a subtractive method or a modified semi-additive method, using the metal foil on the insulating layer.

[0221] The metal foil can be produced by a known method such as an electrolytic method, a rolling method, etc. Commercially available metal foils include, for example, HLP foil and JXUT-III foil manufactured by JX Metals Corporation, and 3EC-III foil and TP-III foil manufactured by Mitsui Mining & Smelting Co., Ltd.

[0222] <Semiconductor device> The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.

[0223] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES

[0224] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature condition is room temperature (25°C). Unless otherwise specified, the pressure condition is atmospheric pressure (1 atm).

[0225] <Synthesis Example 1: Synthesis of Polymer Resin 1> In a reaction vessel, 50 g of bifunctional hydroxyl-terminated polybutadiene (number average molecular weight: 3,000, hydroxyl equivalent weight = 1,800 g / eq., solid content 100 mass%: "G-3000" manufactured by Nippon Soda Co., Ltd.), 23.5 g of aromatic hydrocarbon mixed solvent ("IPZOL 150" manufactured by Idemitsu Petrochemical Co., Ltd.), and 0.005 g of dibutyltin laurate were mixed and dissolved uniformly. When the mixture became uniform, the temperature was raised to 50°C, and 4.8 g of toluene-2,4-diisocyanate (isocyanate equivalent weight: 87.08 g / eq.) was added while stirring, and the reaction was carried out for about 3 hours. Next, the reaction mixture was cooled to room temperature, and 8.96 g of benzophenonetetracarboxylic dianhydride (acid anhydride equivalent: 161.1 g / eq.), 0.07 g of triethylenediamine, and 40.4 g of ethyl diglycol acetate (manufactured by Daicel Corporation) were added thereto, and the mixture was heated to 130° C. with stirring and reacted for about 4 hours. -1 The disappearance of the NCO peak was confirmed. The disappearance of the NCO peak was regarded as the end point of the reaction, and the reaction mixture was cooled to room temperature and filtered through a 100 mesh filter cloth to obtain a polymer resin 1 (non-volatile components 50% by mass) having an imide structure, a urethane structure, and a polybutadiene structure. The number average molecular weight (Mn) of the obtained polymer resin 1 was 13,700.

[0226] <Synthesis Example 2: Synthesis of Polymer Resin 2> In a 1L separable flask equipped with an oil bath and a stirring rod, 200 g of cyclohexanone was added while introducing nitrogen gas, and 149.4 g of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) as a diamine and 4.7 g of m-aminophenol as a monoamine compound were added while stirring, followed by 67.3 g of 1,2,4,5-cyclohexanetetracarboxylic dianhydride as a tetracarboxylic acid, and stirred at room temperature for 30 minutes. The mixture was heated to 100°C and stirred for 3 hours, after which the oil bath was removed and the temperature was returned to room temperature to obtain a varnish-like polyimide precursor. The mixture was then heated at 170°C for 10 hours while removing the distilled water from the system using a Dean-Stark trap, and imidized to obtain a polymer resin 2 (50% by mass of non-volatile components) having a carbon skeleton derived from dimer acid. The weight average molecular weight (Mw) of the obtained polymer resin 2 was 20,000.

[0227] <Synthesis Example 3: Synthesis of Polymer Resin 3> In a 1L separable flask equipped with an oil bath and a stirring rod, 200 g of cyclohexanone was added while introducing nitrogen gas, and 156.3 g of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) as a diamine and 2.0 g of m-aminophenol as a monoamine compound were added while stirring, followed by adding 67.3 g of 1,2,4,5-cyclohexanetetracarboxylic dianhydride as a tetracarboxylic acid and stirring at room temperature for 30 minutes. The mixture was heated to 100°C and stirred for 3 hours, after which the oil bath was removed and the mixture was returned to room temperature to obtain a varnish-like polyimide precursor. The mixture was then heated at 170°C for 10 hours while removing the distilled water from the system using a Dean-Stark trap, and imidized to obtain a polymer resin 3 (50% by mass of non-volatile components) having a carbon skeleton derived from dimer acid. The weight average molecular weight (Mw) of the obtained polymer resin 3 was 50,000.

[0228] <Synthesis Example 4: Synthesis of Polymer Resin 4> A monomer composition was obtained by mixing 46.5g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 12.6g of 4,4'-[1,4-phenylenebis[(1-methylethylidene)-4,1-phenyleneoxy]]bisbenzenamine (BPPAN), 42.6g of dimer diamine (PRIAMINE 1075 manufactured by Croda Japan), and 40g of toluene in 400g of N,N-dimethylacetamide (DMAc), and the mixture was stirred and reacted at room temperature and atmospheric pressure for 3 hours. As a result, a solution of polyamic acid was obtained.

[0229] Next, the polyamic acid solution was heated and maintained at about 160°C while condensed water was azeotropically removed with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was leaking out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. It was then cooled. This resulted in obtaining polymer resin 4 (non-volatile components 20% by mass). The weight average molecular weight (Mw) of the obtained polymer resin 4 was 17,000.

[0230] <Synthesis Example 5: Synthesis of Polymer Resin 5> A monomer composition was obtained by mixing 46.5g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 5.2g of 4,4'-[1,4-phenylenebis[(1-methylethylidene)-4,1-phenyleneoxy]]bisbenzenamine (BPPAN), 53.2g of dimer diamine (PRIAMINE 1075 manufactured by Croda Japan), and 40g of toluene in 400g of N,N-dimethylacetamide (DMAc), and the mixture was stirred and reacted at room temperature and atmospheric pressure for 3 hours. As a result, a polyamic acid solution was obtained.

[0231] Next, the polyamic acid solution was heated and maintained at about 160°C, while the condensed water was azeotropically removed with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was leaking out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. It was then cooled. This resulted in the production of polymer resin 5 (20% by mass of non-volatile components). The weight average molecular weight (Mw) of the obtained polymer resin 5 was 19,000.

[0232] <Example 1> A resin solution was obtained by dissolving 6 parts of naphthylene ether type epoxy resin (DIC Corporation "HP-6000L", epoxy equivalent 213g / eq.), 6 parts of bisphenol type epoxy resin (Nippon Steel Chemical & Material Corporation "ZX-1059", 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent 165g / eq.), and 5 parts of biphenyl type epoxy resin (Nippon Kayaku Co., Ltd. "NC3100", epoxy equivalent 258g / eq.) in 20 parts of MEK with stirring under heating. This resin solution was cooled to room temperature. Thereafter, to the resin solution, 7.7 parts of an active ester curing agent (DIC Corporation "HPC8000-65T", active ester equivalent 223 g / eq., toluene solution with solid content of 65%), 8 parts of a 50% mass% toluene solution of a phenol novolac resin (DIC Corporation "TD-2090", phenol equivalent 105 g / eq.), 4 parts of the polymer resin 1 (non-volatile component 50% by mass) obtained in Synthesis Example 1, 12 parts of the polymer resin 2 (non-volatile component 50% by mass) obtained in Synthesis Example 2, 4 parts of a carbodiimide-based curing agent (Nisshinbo Chemical Inc. "V-03", active group equivalent approximately 216 g / eq., toluene solution with solid content of 50% by mass), and spherical silica (Admatechs Corporation "SO-C4", average particle size 1 μm, specific surface area 4.5 m) surface-treated with an amine-based alkoxysilane compound (Shin-Etsu Chemical Co., Ltd. "KBM573") were added. 2140 parts of 1-benzyl-2-phenylimidazole (1B2PZ) (MEK solution with a solid content of 10% by mass), 2 parts of a curing accelerator (1-benzyl-2-phenylimidazole (1B2PZ)), and 5 parts of MEK were mixed and uniformly dispersed in a high-speed rotating mixer to obtain a mixture. The mixture was then filtered through a cartridge filter (ROKITECHNO's SHP020) to produce a varnish-like resin composition.

[0233] <Example 2> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 1 (50% by mass of non-volatile components) was changed from 4 parts to 6 parts, and the amount of polymer resin 2 (50% by mass of non-volatile components) was changed from 12 parts to 10 parts.

[0234] <Example 3> A resin composition was obtained in the same manner as in Example 2, except that a carbodiimide-based curing agent ("V-03" manufactured by Nisshinbo Chemical Inc.) was not used.

[0235] <Example 4> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 1 (50% by mass of non-volatile components) was changed from 4 parts to 10 parts, and the amount of polymer resin 2 (50% by mass of non-volatile components) was changed from 12 parts to 6 parts.

[0236] <Example 5> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 1 (50% by mass of non-volatile components) was changed from 4 parts to 12 parts, and the amount of polymer resin 2 (50% by mass of non-volatile components) was changed from 12 parts to 4 parts.

[0237] <Example 6> A resin composition was obtained in the same manner as in Example 2, except that 10 parts of polymer resin 3 (50% by mass of non-volatile component) obtained in Synthesis Example 3 was used instead of 10 parts of polymer resin 2 (50% by mass of non-volatile component).

[0238] <Example 7> A resin composition was obtained in the same manner as in Example 4, except that 15 parts of Polymer Resin 4 (20% by mass of non-volatile component) obtained in Synthesis Example 4 was used instead of 6 parts of Polymer Resin 2 (50% by mass of non-volatile component).

[0239] <Example 8> A resin composition was obtained in the same manner as in Example 4, except that 15 parts of Polymer Resin 5 (20% by mass of non-volatile component) obtained in Synthesis Example 5 was used instead of 6 parts of Polymer Resin 2 (50% by mass of non-volatile component).

[0240] <Comparative Example 1> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 1 (non-volatile component 50% by mass) was changed from 4 parts to 16 parts, and polymer resin 2 was not used.

[0241] <Comparative Example 2> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 1 (50% by mass of non-volatile components) was changed from 4 parts to 14 parts, and the amount of polymer resin 2 (50% by mass of non-volatile components) was changed from 12 parts to 2 parts.

[0242] <Comparative Example 3> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 2 (non-volatile component 50% by mass) was changed from 12 parts to 16 parts, and polymer resin 1 was not used.

[0243] <Comparative Example 4> A resin composition was obtained in the same manner as in Example 1, except that the amount of polymer resin 1 (50% by mass of non-volatile components) was changed from 4 parts to 2 parts, and the amount of polymer resin 2 (50% by mass of non-volatile components) was changed from 12 parts to 14 parts.

[0244] <Comparative Example 5> A resin composition was obtained in the same manner as in Example 1, except that 26.7 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a methyl ethyl ketone / cyclohexanone solution with a solid content of 30% by mass) was used instead of 4 parts of polymer resin 1 (non-volatile component 50% by mass) and 12 parts of polymer resin 2 (non-volatile component 50% by mass).

[0245] <Test Example 1: Measurement of breaking strength, breaking elongation, and elastic modulus by tensile test> The resin compositions obtained in the examples and comparative examples were applied by a die coater onto a polyethylene terephthalate film ("Lumirror R80" manufactured by Toray Industries, Inc., thickness 38 μm, softening point 130° C.) that had been release-treated with an alkyd resin-based release agent ("AL-5" manufactured by Lintec Corporation) so that the thickness of the resin composition layer after drying would be 50 μm, and the film was dried at 100° C. for 3 minutes to obtain a resin sheet A including a resin composition layer.

[0246] The obtained resin sheet A was subjected to tensile strength measurement using a tensile tester "RTC-1250A" manufactured by Orientec Co., Ltd., and the strength at break (MPa), elongation at break (%), and modulus of elasticity (GPa) at 23°C were measured. The measurement was performed in accordance with JIS K7127. The measurement was performed five times, and the average value of the top three points was calculated.

[0247] <Test Example 2: Measurement and evaluation of dielectric properties (dielectric tangent)> The polyethylene terephthalate film was peeled off from the resin sheet A obtained in the same manner as in Test Example 1, and the resin composition layer was thermally cured by heating at 200° C. for 90 minutes. This cured product was cut into a size of 62 mm×75 mm to obtain a cured product for evaluation.

[0248] The dielectric tangents (25°C and 100°C) of the obtained cured products for evaluation were measured at a measurement frequency of 10 GHz by the split cylinder resonance method using an EM Lab "CR-710", and the dielectric tangents were evaluated according to the following criteria.

[0249] Evaluation criteria for dielectric loss tangent: "○": Dielectric tangent (25℃) is 0.0045 or less, and dielectric tangent (100℃) is 0.0055 or less "△": Either the dielectric tangent (25℃) is 0.0045 or less, or the dielectric tangent (100℃) is 0.0055 or less "X": Dielectric tangent (25°C) is greater than 0.0045 and dielectric tangent (100°C) is greater than 0.0055

[0250] <Test Example 3: Measurement and Evaluation of Adhesion Strength> (1) Surface preparation for copper-clad laminate A glass cloth-based epoxy resin double-sided copper-clad laminate with copper foil on the surface (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic "R-1766") was prepared. Both sides were roughened by etching using a microetching agent (Mec "CZ8101") so that the copper etching amount was 2 μm. The copper-clad laminate obtained in this way is called a "roughened copper-clad laminate".

[0251] (2) Lamination onto roughened copper-clad laminate and curing Resin sheet A obtained in the same manner as in Test Example 1 was laminated on one side of the roughened copper-clad laminate using a batch-type vacuum pressure laminator (a two-stage build-up laminator "CVP700" manufactured by Nikko Materials Co., Ltd.) so that the resin composition layer and the roughened copper-clad laminate were bonded. Lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100°C and a pressure of 0.74 MPa for 30 seconds. After lamination, the polyethylene terephthalate film of resin sheet A was peeled off. The resin composition was cured under curing conditions of 100°C for 30 minutes, followed by 190°C for 90 minutes, to obtain a laminate having a layer structure of "roughened copper-clad laminate / cured layer of resin composition".

[0252] (3) Preparation of test specimens The obtained laminate was cut into 1 cm squares and placed on a ceramic backing plate with epoxy adhesive (11.4 cm square, P / N 901450) with the cured layer facing upwards. Furthermore, a stud pin (tack-shaped jig, adhesive surface diameter 2.7 mm, P / N 901106) was fixed on the cured layer with epoxy adhesive and heated at 150°C for 1 hour to bond the stud pin to the cured layer.

[0253] (4) Stud pull test Using a stud pull tester ("ROMULUS" manufactured by Quad Group Inc.), the stud pin was pulled in a direction perpendicular to the main surface of the hardened layer at a speed of 2 kgf / sec. The load value (kgf / cm) at which the hardened layer peeled off was measured. 2) was measured as the adhesion strength, and the adhesion strength was evaluated according to the following criteria.

[0254] Adhesion strength evaluation criteria: "◎": Adhesion strength is 700kgf / cm 2 End "○": Adhesion strength is 550kgf / cm 2 More than 700kgf / cm 2 less than "X": Adhesion strength is 550kgf / cm 2 less than

[0255] <Test Example 4: Measurement and Evaluation of Warpage> Resin sheet A obtained in the same manner as in Test Example 1 was laminated on one entire surface of a 12-inch silicon wafer (thickness 775 μm) using a batch-type vacuum pressure laminator (two-stage build-up laminator "CVP700" manufactured by Nikko Materials Co., Ltd.). This lamination was performed so that the resin composition layer and the silicon wafer were bonded. The polyethylene terephthalate film of the resin sheet A was peeled off to expose the resin composition layer. Resin sheet A was further laminated on the surface of this exposed resin composition layer in the same manner, and the polyethylene terephthalate film was peeled off. Furthermore, the resin sheet A was laminated and the polyethylene terephthalate film was peeled off, and three resin composition layers (total thickness 150 μm) were formed on one surface of the 12-inch silicon wafer. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing for 30 seconds at 100 ° C. and a pressure of 0.74 MPa.

[0256] The sample was heated in an oven at 100°C for 30 minutes, and then further heated at 200°C for 90 minutes to cure the resin composition layer, thereby obtaining a sample laminate having a layer structure of "silicon wafer / cured layer". The obtained sample laminate was placed on the top surface of a horizontal table. The end of the sample laminate was pressed against the top surface of the table. The distance between the end of the silicon wafer on the opposite side to the pressed end and the top surface of the table was measured as the amount of warping, and the amount of warping was evaluated according to the following criteria. The smaller the amount of warping, the more effectively the warping was suppressed.

[0257] Warpage evaluation criteria: "◎": Warpage is between 0μm and 1700μm "○": Warpage is greater than 1700 μm and less than 2200 μm "X": Warpage is 2200μm or more

[0258] The amounts of non-volatile components used in the resin compositions of the Examples and Comparative Examples, as well as the measurement results and evaluation results of the Test Examples, are shown in Table 1 below.

[0259] [Table 1]

[0260] From the above results, it can be seen that by using a resin composition comprising (A) an epoxy resin, (B) an epoxy resin curing agent, (C) an imide skeleton-containing polymer resin having a polybutadiene structure, and (D) an imide skeleton-containing polymer resin not having a polybutadiene structure, wherein the mass ratio of component (C) to component (D) (content of component (C) / content of component (D)) is 0.2 or more and 4 or less, warping is suppressed, and a cured product having excellent adhesive strength with a conductor layer and a low dielectric tangent can be obtained.

Claims

1. A resin composition comprising: (A) an epoxy resin; (B) an epoxy resin curing agent; (C) an imide skeleton-containing polymer resin having a polybutadiene structure; and (D) an imide skeleton-containing polymer resin not having a polybutadiene structure, A resin composition, in which the mass ratio of the (C) component to the (D) component (content of the (C) component / content of the (D) component) is 0.2 or more and 4 or less.

2. The resin composition according to claim 1, wherein the content of the butadiene structure in the component (C) is 60% by mass or more, where the component (C) is taken as 100% by mass.

3. The resin composition according to claim 1, wherein the number average molecular weight (Mn) of component (C) is 5,000 or more.

4. The resin composition according to claim 1 , wherein the component (C) further has a urethane structure.

5. The resin composition according to claim 1, wherein a mass ratio of the component (C) to the component (A) (content of the component (C) / content of the component (A)) is 0.1 or more and 0.5 or less.

6. The resin composition according to claim 1, wherein the weight average molecular weight (Mw) of the component (D) is 5,000 or more.

7. The resin composition according to claim 1 , wherein the component (D) has a phenolic hydroxyl group.

8. The resin composition according to claim 1 , wherein the component (D) has a carbon skeleton derived from a dimer acid.

9. The resin composition according to claim 8 , wherein the content of the carbon skeleton derived from the dimer acid in the component (D) is 20% by mass or more, relative to 100% by mass of the component (D).

10. The resin composition according to claim 1, wherein a mass ratio of the component (D) to the component (A) (content of the component (D) / content of the component (A)) is 0.1 or more and 0.5 or less.

11. The resin composition according to claim 1 , wherein the content of the component (A) is 1% by mass or more and 20% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.

12. The resin composition according to claim 1 , wherein the component (B) comprises a carbodiimide-based curing agent.

13. The resin composition according to claim 1 , wherein the component (B) comprises an active ester-based curing agent.

14. The resin composition according to claim 1 , wherein the component (B) comprises an active ester-based curing agent, a phenol-based curing agent, and a carbodiimide-based curing agent.

15. The resin composition according to claim 1 , further comprising (E) an inorganic filler.

16. The resin composition according to claim 15, wherein the content of the component (E) is 40% by mass or more, based on 100% by mass of non-volatile components in the resin composition.

17. 2. The resin composition according to claim 1, wherein, when tensile strength measurements are performed in accordance with JIS K7127, the strength at break of the cured product of the resin composition is 60 MPa or more, the elongation at break of the cured product of the resin composition is 0.5% or more, and the modulus of elasticity of the cured product of the resin composition is 20 GPa or less.

18. The resin composition according to claim 1, wherein the dielectric loss tangent (Df) of a cured product of the resin composition is 0.0045 or less when measured at 10 GHz and 25°C.

19. A cured product of the resin composition according to any one of claims 1 to 18.

20. A resin sheet comprising a support and a resin composition layer formed from the resin composition according to any one of claims 1 to 18 provided on the support.

21. A printed wiring board comprising an insulating layer made of a cured product of the resin composition according to any one of claims 1 to 18.

22. A semiconductor device comprising the printed wiring board according to claim 21.

Citation Information

Patent Citations

  • Functionalized polyimide resin and epoxy resin composition including the same

    JP2015117278A

  • Resin composition

    JP2019038969A

  • Resin composition