Extreme ultraviolet pellicle storage and method of preserving extreme ultraviolet pellicle properties thereof
Storing CNT pellicles in non-outgassing materials and inert gas/vacuum conditions maintains their EUV transmittance and mechanical strength, addressing susceptibility to environmental pollutants.
Patent Information
- Application Number
- JP2024060410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-07
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-18
AI Technical Summary
Ultra-thin, ultra-low density carbon nanotube (CNT) pellicles used in EUV lithography are susceptible to damage and property changes during storage, transportation, and handling due to volatile organic compounds and environmental pollutants, affecting EUV transmission and scattering.
Store CNT pellicles in containers made of non-outgassing materials like stainless steel or glass, under vacuum or inert gas conditions, to maintain high EUV transmittance and mechanical integrity.
Preserves the high EUV transmittance and mechanical strength of CNT pellicles, ensuring consistent performance in EUV lithography processes.
Smart Images

Figure 2024149428000002 
Figure 2024149428000003 
Figure 2024149428000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates generally to the storage of ultra-thin films and ultra-thin film devices used in the manufacture of semiconductor microchips, and more particularly to storage container materials for properly storing and transporting ultra-thin, ultra-low density, nanostructured, free-standing pellicle films to avoid or mitigate undesirable effects on the ultra-thin films and / or ultra-thin film devices due to outgassing from the container materials. [Background technology]
[0002] A pellicle is a protective device that covers a photomask and is used in semiconductor microchip manufacturing. A photomask can refer to an opaque plate with holes or transparencies that allow light to filter through in a defined pattern. Such photomasks may be widely used in photolithography and integrated circuit manufacturing. The photomask is used as a master template to create a pattern on a substrate (usually a thin slice of silicon known as a wafer in semiconductor chip manufacturing).
[0003] Particle contamination can often be a significant issue in semiconductor manufacturing, and is even more pronounced in advanced photolithography in many high-resolution processes, where significant particles can alter the printed patterns of logic circuits on chips that do not have built-in redundancy, affecting product yields.
[0004] Photomasks are protected from particles by a pellicle, a thin transparent film stretched over a frame (also called a pellicle border with a central opening) that is fitted over the patterned side of the photomask. The pellicle is close to the mask but far enough away from the mask that small to medium sized particles that land on the pellicle will be too far out of focus to print. However, field reports from the semiconductor industry have shown that falling particles are still observed after periods of exposure using unknown particle sources.
[0005] Recently, the microchip manufacturing industry has realized that pellicles have the potential to protect photomasks from damage caused by sources other than particles and contaminants.
[0006] Extreme ultraviolet (EUV) lithography is an advanced optical lithography technique that uses the EUV wavelength range (more specifically, wavelengths around 13.5 nm). EUV lithography allows semiconductor microchip manufacturers to pattern the most sophisticated features at resolutions of 7 nm or less to place many more transistors without increasing the size of the space required. EUV photomasks work by reflecting light. This reflection of light is achieved by using multiple alternating layers of molybdenum and silicon. When an EUV light source is activated, the EUV light first hits the pellicle film, passes through it, then bounces off from underneath the photomask and hits the pellicle film once more, after which the EUV light continues down the path to print the microchip. Some of the energy is absorbed during this process, which can result in heat being generated, absorbed, and stored. The temperature of the pellicle can heat up to a range of 500°C to over 1000°C.
[0007] While heat resistance is important, the pellicle must also be highly transparent to EUV to ensure that the reflected light and reflected light pattern from the photomask can pass through. This is one of the main reasons why EUV pellicles are generally very thin, with thicknesses of less than 200 nm, preferably less than 100 nm, or even less than 40 nm.
[0008] In 2016, a polysilicon-based EUV pellicle was developed after decades of research and efforts, but the EUV transmittance was only 78% for a simulated relatively low-power 175 watt EUV source. The desire for increased transistor density has led to stringent requirements for higher transmittance, lower transmittance variation, higher temperature tolerance, and stronger mechanical strength, presenting further technical challenges to EUV pellicle developers.
[0009] Attempts have been made to achieve high light transmittance by increasing the carbon nanotube content (e.g., up to 99% by mass) in the carbon nanotube sheet. These attempts have resulted in products that may also meet the mechanical strength and / or durability requirements of pellicle films based on current industry standards. Further improvements include meeting more stringent standards, improving user experience, reducing production costs, and creating economic benefits. Therefore, such carbon nanotube-based thin films need to have a certain thickness to support their structural integrity. As a result, the EUV transmission of such carbon nanotube-based thin films may need to be compromised when dealing with thicker films. Therefore, in an effort to achieve further progress, techniques that go beyond conventional technology and knowledge to address both the EUV light transmission and the thickness of the pellicle film have been explored and created.
[0010] Attempts to produce ultra-thin, ultra-low density carbon nanotube (CNT) pellicle films have reached a milestone with the publication of WO2021 / 090699. In this application, ultra-thin films of size comparable to current industry standards (approximately 3 nm) were achieved. However, such ultra-thin films, as thin as approximately 3 nm, present practical challenges because they are susceptible to damage, modification, or alteration during product packaging, shipping and handling, human and robotic manipulation, and storage after production.
[0011] However, CNTs are also known to be sensitive to volatile organic compounds (VOCs) and can adsorb certain gaseous molecules and environmental pollutants, even in trace amounts, which can eventually alter the CNT surface and, if exposed for a sufficient period of time, can cause changes in the properties of the CNTs, especially in the case of ultra-thin CNT films. Such changes will inevitably affect the optical and EUV transmittance and scattering and should be avoided.
[0012] Therefore, proper storage and shipping environments are important to store ultrathin CNT or nanofiber pellicles and maintain the properties of the pellicle film with little or no change to its high EUV transmission. Summary of the Invention
[0013] According to an embodiment of the present disclosure, a nanostructured film is disclosed after being placed in a storage or shipping container for at least one day. The nanostructured film includes a plurality of nanofibers randomly crossed to form an interconnected network structure in a planar orientation, the interconnected network structure having a thickness ranging from a lower limit of 3 nm to a lower limit of 100 nm or up to an upper limit of 500 nm, an optical transmittance measured at a wavelength of 550 nm of 50% or more to 95% or more, and an EUV transmittance of 75% or more to 94% or more up to 99%, where the nanofiber structure may be in a pristine state (i.e., the nanofiber structure has not undergone any treatment or surface modification after fabrication) or may have undergone an annealing process, such as thermal annealing or laser annealing. The nanostructured film may be further coated with a material selected from a metal, a metal oxide, a derivative thereof, or a combination thereof. The nanofiber may be a carbon nanofiber, a carbon nanotube (CNT), a boron nitride nanotube (BNNT), or a combination thereof. The present disclosure further includes EUV pellicle storage or shipping containers that include non-outgassing or minimally outgassing materials, including but not limited to stainless steel or glass. CNT EUV pellicle films can include any combination of single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes (having three or more walls), as well as other types of carbon-based or non-carbon-based nanofibers. Such nanostructured films exhibit and maintain high EUV transmission and meet other EUV photolithography requirements and standards after being fabricated, coated and / or annealed as required, placed in a storage or shipping container, placed on a shelf, and stored for at least one day, preferably at least one week, and / or at least one month. The disclosed nanostructured films further preserve high EUV transmission substantially equal to that measured upon completion of fabrication.
[0014] According to an aspect of the present disclosure, a storage device is disclosed that includes a material that maintains one or more properties of an extreme ultraviolet (EUV) lithography pellicle, where the one or more properties are selected from EUV transmittance, EUV transmission variation, EUV scattering, EUV pellicle film deflection, EUV pellicle film tensile strength, or a combination thereof.
[0015] According to further aspects of the present disclosure, some materials may outgas and change one or more properties of the EUV lithography pellicle, while other materials may outgas without changing one or more properties of the EUV lithography pellicle. The material of the EUV pellicle storage container must maintain one or more properties of the EUV lithography pellicle even if it outgases. If the material outgases, it should be shielded or treated to maintain one or more properties of the EUV lithography pellicle.
[0016] According to one embodiment of the present disclosure, the material for the EUV pellicle storage container includes stainless steel.
[0017] According to another aspect of the present disclosure, a material for the EUV pellicle storage container includes glass.
[0018] According to a further aspect of the present disclosure, the material for the EUV pellicle storage container includes glass ceramic or quartz.
[0019] According to yet another aspect of the present disclosure, a material for the EUV pellicle storage container includes borosilicate glass.
[0020] According to a further aspect of the present disclosure, the storage device is vacuum sealed.
[0021] According to a further aspect of the present disclosure, the storage device is filled with an inert gas.
[0022] According to a further aspect of the present disclosure, the material is pre-purged with an inert gas. The pre-purged material may release the inert gas under vacuum pressure.
[0023] According to another aspect of the present disclosure, a method of storing an EUV lithography pellicle is disclosed. The method includes preparing an EUV lithography pellicle and placing the EUV lithography pellicle in a container. The container includes at least a material that maintains one or more properties of the EUV lithography pellicle selected from EUV transmittance, EUV transmission variation, EUV scattering, deflection of the EUV lithography pellicle film, tensile strength of the EUV lithography pellicle film, or a combination thereof.
[0024] According to a further aspect of the present disclosure, the material is selected from stainless steel, glass, borosilicate glass, glass ceramic, or quartz.
[0025] According to a further aspect of the present disclosure, the method further includes maintaining a vacuum pressure within the container.
[0026] According to a further aspect of the present disclosure, the method further comprises filling the container with an inert gas.
[0027] According to a further aspect of the present disclosure, the method further includes purging the material contained within the container with an inert gas.
[0028] According to a further aspect of the present disclosure, the material selected for the EUV pellicle storage container does not release (i.e., does not outgas) gaseous molecules, volatile organic chemicals, or vapors from the interior of the material to the surrounding environment.
[0029] The present disclosure will be further described in the following detailed description with reference to a number of drawings, which are mentioned as non-limiting examples of preferred embodiments of the present disclosure, in which like characters represent like elements throughout the several views of the drawings. [Brief description of the drawings]
[0030] [Figure 1]1 illustrates a filtration method for forming a pellicle film, followed by an optional high temperature annealing step, according to an exemplary embodiment. [Diagram 2] 1 illustrates a scanning electron microscope (SEM) image of the nanostructure of a double-walled CNT (DWCNT) based film, according to an exemplary embodiment. [Diagram 3] 1 illustrates Fourier transform infrared (FTIR) spectra of a CNT film before and after annealing, and an annealed CNT film that was stored in a plastic container for 24 hours after annealing, according to an exemplary embodiment. [Figure 4] 1 illustrates FTIR spectra of a CNT film before and after annealing, and an annealed CNT film stored in a glass container for 24 hours, according to an example embodiment. [Diagram 5] 1 illustrates FTIR spectra of an annealed CNT film immediately after annealing, and annealed CNT films stored in a glass container 1 day, 27 days, and 35 days after annealing, according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] Through one or more of its various aspects, the embodiments and / or specific features, subcomponents, or processes of the present disclosure are intended to demonstrate one or more of the advantages specifically discussed above and below.
[0032] A pellicle may refer to a thin transparent film that protects a photomask during semiconductor microchip fabrication. A pellicle contemplates a protective device with 1) a border or frame, and 2) a central hole or opening. Both the border and the opening are covered by a continuous thin film over at least a portion of the border and a portion of the opening, preferably the entire opening, and a portion of the border adjacent to the opening, or over the entire border. The central portion of such a thin film extending the opening is freestanding. A pellicle may function as a dust cover to prevent particles and contaminants from falling onto the photomask during fabrication. However, the pellicle must be sufficiently transparent to allow the transmission of light necessary to perform lithography. Higher light transmission is required for more effective lithography. For most EUV lithography applications, an 80% EUV transmission from the pellicle may be sufficient. For high resolution EUV lithography below 5 nm, for high energy EUV scanners (>250 watts), or for high numerical aperture EUV lithography scanners (0.25), an EUV transmission greater than 92%, an EUV transmission greater than 94%, or even an EUV transmission between 96% and 99% is desirable.
[0033] Moreover, pellicles for EUV lithography require large (e.g., over 110×140 mm) freestanding thin-film materials with extreme and unique properties. In addition to high transparency to EUV radiation, unexpected EUV transmission variations (also called EUV transmission uniformity) or overall EUV transmission degradation of a single pellicle can have adverse effects during the manufacturing process, leading to poor printing results and reduced production yields. EUV pellicle films may also be required to withstand temperatures in excess of 400°C and be mechanically robust to withstand handling, transportation, and pump-down and evacuation operations during the photolithography process. Pellicle films are required to be gas permeable as well as capable of retaining micrometer-sized particles. Given the many high-level properties, effective EUV pellicles have traditionally been difficult to manufacture and required unconventional care after manufacture.
[0034] Carbon nanotubes and carbon nanotube films Carbon nanotubes (CNTs) or carbon nanofibers, as often referred to herein, are long tubes with small diameters, typically measured in nanometers. They have a high aspect ratio of length to diameter, generally in the range of preferably greater than about 100:1, and sometimes greater than about 1000:1. Another preferred aspect ratio can be at least about 10,000:1. CNTs are composed of one or more graphene sheets wrapped concentrically. Each graphene sheet is considered a wall of the CNT. Single-walled CNTs (SWCNTs) are made of one graphene sheet. Double-walled CNTs (DWCNTs) are made of two graphene sheets. Finally, multi-walled CNTs (MWCNTs) have three or more graphene sheets. Other types of CNTs may include, but are not limited to, coaxial nanotubes (either homogeneous or heterogeneous, meaning that the inner wall(s) and outer wall(s) of the coaxial nanotube are the same or different), conical carbon nanotubes, and closed carbon nanotubes. Other carbon allotropes, including metallic or semiconducting carbon nanotubes, may also form sheets with excellent properties as pellicle films. In the case of CNTs, they may exist in one substantially pure type or in combination with other types, often in terms of the number of CNT walls. CNTs may exist individually, separated from one another, or may form bundles. Bundles may include the same or different types of CNTs, such as SWCNTs, including DWCNTs, SWCNTs (three or more walls), including MWCNTs. Within a bundle, the lengths and diameters of the individual CNTs may vary. Each bundle containing two or more CNTs may be aligned parallel over at least a portion of its length. For simplicity and convenience, CNTs in this application may refer to different types of CNTs, for example CNTs with different numbers of walls, and may include CNTs that exist individually or in bundles.
[0035] As used herein, nanofibers may illustratively refer to fibers having a diameter of less than 1 μm. Nanofibers and nanotubes may be used interchangeably and include SWCNTs, DWCNTs, MWCNTs, and other carbon allotropes in which carbon atoms bond together to form cylindrical structures.
[0036] An individual CNT may cross one or more other CNTs. Many CNTs together can form a mesh-like nanostructured film. An exemplary embodiment may include a free-standing nanostructured thin film, with regions of the thin film lacking a supporting material or substrate on either side of the thin film. Although such formation is possible, it is not guaranteed in all trials, especially in the production of ultra-thin films with properties such as high transparency that are suitable for EUV lithography pellicles.
[0037] Furthermore, among several possible methods to produce freestanding films, a filtration-based approach was utilized to produce films from small size to sufficiently large films with uniform film thickness for EUV lithography. Films of uniform thickness correlate with uniform light transmittance. This filtration-based method allows rapid production of films of CNTs as well as other high aspect ratio nanoparticles and nanofibers (e.g., boron nitride nanotubes (BNNTs) or silver nanowires (AgNWs)). Because this approach separates the synthesis of nanotubes or nanoparticles from the film production process, different types of nanofibers made by virtually any method may be used. Different types of nanotubes (SWCNTs, DWCNTs, MWCNTs, or carbon allotropes) can be mixed in any desired ratio. Filtration can be a self-leveling process in the sense that non-uniformities in film thickness during the filtration process are self-corrected by local transmittance variations, and thus can be a highly desirable film formation process and a promising candidate for the production of highly uniform films.
[0038] Annealing treatment Annealing refers to the process of applying heat treatment to a given material to change its physical, and sometimes chemical, properties to make it more ductile and less hard. Annealing begins with a heat source, imparting heating energy to the material to raise its temperature from ambient to a pre-determined elevated temperature, holding the desired temperature for a pre-selected treatment period, and then allowing the material to cool.
[0039] The heating performed for annealing may be electrical heating in which an electric current, voltage, and / or electrical energy is passed through the material by direct contact with the material.
[0040] Alternatively, heating for annealing may be convection heating, in which a heated gas flows across the surface and / or possibly channels within the material, increasing the temperature of the target.
[0041] Another type of heating used for annealing may be radiative heating, where electromagnetic waves are directed toward the target material. Light sources in the visible spectrum, including lasers, can heat the target material by directing radiation at the target or target surface. Photons of light may be reflected, re-emitted, or scattered, and topographical differences, features, and / or irregularities in a given area of the material may result in uneven heating. If the environment in which such processing is performed obstructs the light path to the target, the annealing results may be uneven. This unevenness caused by direct light processing is more pronounced in areas that are repeatedly irradiated and areas that avoid irradiation if the entire material surface is not irradiated simultaneously. Additionally, laser processing may burn, remove, or sublimate surface material. Such "lifted" material produced by laser processing, even in trace amounts, may be in the form of small molecules or elements, which may be reabsorbed or redeposited on the untreated or possibly treated surface, resulting in new irregularities or exacerbating existing inhomogeneities.
[0042] However, aspects of the disclosure are not limited in this respect and different heating operations / methods may be performed or a combination of heating operations may be performed.
[0043] The annealing may be thermal annealing, which may use electromagnetic waves in the non-visible light spectrum, including but not limited to infrared (e.g., near infrared, mid infrared, and / or far infrared). Such electromagnetic wavelengths may have a range selected from between about 10 nm and about 1 mm. A preferred range may also be selected from between about 400 nm and about 700 nm, or between about 700 nm and about 1 mm. Yet another preferred wavelength may be between about 5 μm and about 20 μm. This heating method transfers energy to the target material, which dissipates the thermal energy into other microscopic motions within the material. That is, thermal annealing distributes its energy power to heat the target material, increasing the temperature uniformly. Thermal annealing covers the entire object, regardless of the direction of the incident energy source. Ceramic heating with a ceramic heating tube with enough internal space to accommodate a full-sized pellicle is one of many options for implementing thermal heating based on the non-visible light spectrum. The heating element may be made of silicon carbide and molybdenum disilicide. Without wishing to be bound by scientific theory, it is believed that other heating elements and heating devices are also applicable.
[0044] In a heating tube, one or more heating sources or heating elements are arranged in a circular array in cross section, or in a tubular array, relative to the overall shape of the heating device. Electromagnetic waves from such heating sources distribute radiation uniformly within the tubular chamber. With the appropriate electromagnetic spectrum and emission source, such annealing ensures uniform radiation reaching the CNT pellicle and covers the entire pellicle area at any point during the process, resulting in minimal or lower EUT transmission variation compared to non-full film field annealing.
[0045] The annealing treatment in this exemplary embodiment includes, but is not limited to, the heating methods described above.
[0046] A typical annealing temperature can be any temperature above ambient temperature. The temperature can be 50°C or higher, 100°C or higher, 300°C or higher, 500°C or higher, 600°C or higher, 650°C or higher, 700°C or higher, 800°C or higher, 900°C or higher, or 1,000°C or higher. The temperature can also be 3,000°C or lower, 2,500°C or lower, 2,000°C or lower, 1,800°C or lower, 1,700°C or lower, 1,600°C or lower, 1,500°C or lower, or 1,400°C or lower. The heating temperature can be within the range of any two of the aforementioned temperatures.
[0047] The selection of the annealing temperature may require further consideration of other factors, such as the appropriate temperature range depending on the material properties of the pellicle boundary, such as the thermal expansion properties of the pellicle boundary, which are preferably low thermal expansion properties (e.g., quartz).
[0048] The annealing temperature may be ramped at a fixed or variable rate depending on the heating device / method used and the heating capacity of the heating device. A typical and practical temperature ramp rate may be about 20° C. / min. A preferred heating scheme heats the CNT pellicle quickly to avoid or limit potential CNT oxidation due to chemical contaminants deposited in the annealing chamber or entrained in the flow-through gases. The heating scheme may also balance the physical, and sometimes chemical, properties and thermal expansion of the pellicle boundary to avoid cracking of the pellicle boundary.
[0049] Cooling after annealing may allow the elevated temperature to naturally return to ambient conditions, or the annealing chamber may be cooled using flowing cold gas, ambient temperature gas, or a gas whose temperature drops over a period of time, with an inert gas being preferred here.
[0050] The annealing process may be performed in a vacuum (e.g., vacuum annealing), a partial vacuum, or at atmospheric pressure. Additionally, the annealing process may be performed in the presence of an inert gas or a non-inert gas, such as a hydrocarbon gas.
[0051] Exemplary inert gases include, but are not limited to, argon, helium, neon, krypton, xenon, and radon. Exemplary hydrocarbon gases include, but are not limited to, methane, ethane, propane, butane, pentane, hexane, and heptane.
[0052] Gases can be flowed through the annealing chamber at a constant or variable flow rate. Two or more gas species as a gas mixture can be flowed through the annealing chamber at a constant or variable flow rate. Also, two or more gases can be flowed continuously or intermittently. The gas or gas mixture can be preheated before being injected into the annealing chamber and / or actively heated in the annealing chamber due to convection heating. Gases or gas mixtures can be purposefully selected and injected during annealing. For example, application of hydrocarbon gases has previously been reported to repair structural defects in nanofibers and nanoparticle formation on the surface of pellicle films. Due to the nature of working with ultra-thin, ultra-low density films, a constant gas flow, or gas with minimal fluctuations in flow rate, may be desirable to avoid film rupture and is contemplated herein.
[0053] The vacuum chamber may be part of an EUV scanner, or it may be directly connected to the EUV scanner as a part, accessory, or attachment to an EUV manufacturing assembly line, or it may be standalone to perform such annealing processes near or remote from the scanner.
[0054] The annealing process may begin by mounting the nanofiber structure on a frame and then directly placing it in an annealing chamber or container. The chamber may be heated for approximately 10 -4 The chamber is evacuated to a vacuum or near vacuum level of 1000 torr or less. The chamber is then heated to a predetermined temperature. At this point, the pellicle is placed in the chamber for a selected period of time. The pellicle may be placed in the chamber before heating begins. After the chamber returns to room temperature and atmospheric pressure, with or without a cooling gas such as argon, the process is complete and the pellicle may be stored at ambient conditions, in vacuum, inert gas, or a combination thereof to avoid contamination, exposure to other gases in the atmosphere that may oxidize, or damage.
[0055] The term annealing may include additional aspects and broader interpretations in various technical fields and industries that are applicable to or related to the present disclosure. One or more innovative contributions herein arise in the fields of materials science and semiconductors.
[0056] Film formation and thermal annealing According to exemplary embodiments of the present disclosure, ultra-thin and ultra-low density CNT pellicle films can be fabricated, followed by a thermal annealing process.
[0057] FIG. 1 illustrates a filtration method for forming the pellicle film shown in FIG. 2 followed by an annealing process according to an exemplary embodiment.
[0058] Another embodiment of the present disclosure may further include any pellicle membrane that is manufactured, to be manufactured, processed, or to be processed by any means prior to the annealing process. Additionally, another embodiment of the present disclosure may include any other pellicle film having various CNT surface modifications, including but not limited to coatings or other means of one or more metal elements, metal oxides, CNT surface modifiers, or combinations thereof.
[0059] As illustrated in Figure 1, a free-standing carbon nanotube-based pellicle film may be created by a filtration-based method. In operation 101, a catalyst is removed from carbon nanotubes (CNTs) to be used to form an aqueous suspension. In an example, the CNTs may be chemically purified to reduce the concentration of catalyst particles to less than 1 wt% or preferably less than 0.5 wt% as measured by thermogravimetric analysis prior to dispersion in the suspension. The removal of the catalyst is not limited to any particular process or procedure, and any suitable process may be used to achieve the desired results.
[0060] In operation 102, an aqueous suspension is prepared using the purified CNTs such that the purified CNTs are uniformly dispersed within the aqueous suspension. When preparing one or more CNT suspensions, the carbon nanotube material can be mixed with a selected solvent to uniformly disperse the nanotubes within the final solution as a suspension. Mixing can include mechanical mixing (e.g., using a magnetic stir bar and stir plate), ultrasonic mixing (e.g., using an immersion ultrasonic probe), or other methods. In some examples, the solvent can be a protic or aprotic polar solvent, such as water, isopropyl alcohol (IPA), and aqueous alcohol mixtures, such as 60, 70, 80, 90, 95% IPA, N-methyl-2-pyrrolidone (NMP), dimethyl sulfide (DMS), and combinations thereof. In another example, a surfactant can be included to aid in the uniform dispersion of the carbon nanofibers within the solvent. Examples of surfactants include, but are not limited to, anionic surfactants.
[0061] Carbon nanofiber films are typically formed from one of MWCNTs, DWCNTs, or SWCNTs. Carbon nanofiber films may also include mixtures of different types of CNTs (i.e., SWCNTs, DWCNTs, and / or MWCNTs) with varying ratios between the different types of CNTs. Other types of CNTs can also be used to produce CNT films by filtration or other known and contemplated methods.
[0062] Each of these three different types of common carbon nanotubes (e.g., MWCNT, DWCNT, and SWCNT) has different properties. In one example, single-walled carbon nanotubes can be more favorably dispersed in a solvent (i.e., most of the nanotubes are suspended separately and less likely to adsorb onto other nanotubes) for subsequent formation into a sheet of randomly oriented carbon nanotubes. This ability to uniformly disperse individual nanotubes in a solvent can result in the production of a more planarly uniform nanotube film formed by removing the solvent from the suspended nanofibers. This physical uniformity can also improve the uniformity of other properties across the film (e.g., transparency and scattering to radiation, mechanical strength under pressure changes, and life / durability testing).
[0063] In an example, the aqueous CNT suspension in operation 102 may have SWCNTs with a purity of at least greater than 85%. The remainder may be a mixture of DWCNTs, MWCNTs, and / or catalyst. In another example, a dispersed CNT suspension containing different ratios of different types of CNTs may be prepared, such as about 20% / 75% DWCNT / SWCNT, about 50% / 45% DWCNT / SWCNT, about 70% / 20% DWCNT / SWCNT, with the remainder being MWCNTs. Mixtures of DWCNTs and SWCNTs blended with 10% or more MWCNTs and various DWCNT / SWCNT percentage ratios may be prepared and subjected to the same filtration process to form nanofiber structures. In one example, an anionic surfactant may be utilized as a dispersant in the suspension to enhance uniform dispersion of the different types of CNT mixture.
[0064] In operation 103, the CNT suspension is then further refined to remove any aggregated or stuck CNTs from the initial mixture. In an example, different morphologies of CNTs (undispersed or aggregated vs. well-dispersed) may be separated from the suspension by centrifugation. Centrifugation of the surfactant-suspended carbon nanotubes before proceeding to the next filtration step may help reduce the turbidity of the suspension solution to ensure full dispersion of the carbon nanotubes in the final suspension solution. However, aspects of the present disclosure are not limited in this respect, and other separation methods or processes may be used. According to an exemplary embodiment, operation 103 may be performed optionally or as a necessary step in the formation of a pellicle film.
[0065] In operation 104, any CNT suspension, preferably the CNT supernatant after the separation procedure from operation 103, is then filtered through a filtration membrane to form a continuous sheet of film of intersecting CNTs, which is the CNT web.
[0066] In an example, one approach to making a CNT film is to deposit nanotubes in a random pattern on a filter (often a flat filter membrane) using water or other fluid. The uniformly dispersed CNT-containing mixture is passed or forced through the filter, leaving a nanofiber structure layer on the filter surface. The size and shape of the resulting film is determined by the size and shape of the desired filtering area of the filter, while the thickness and density of the film are determined by the quantity of nanofiber material applied during the process and the permeability of the filtering membrane to each component of the input material, as the non-permeating components are trapped on the filter surface. If the concentration of nanofibers dispersed in the flow-through filtrate is known, the mass of nanofibers deposited on the filter can be determined from the amount of fluid passing through the filter, and the areal density of the film can be determined by dividing the nanofiber mass by the total filtering area. The filter selected is usually not permeable to any CNTs.
[0067] The filtered CNT films can be a combination of SWCNTs, DWCNTs, and / or MWCNTs in different compositions. The carbon nanofibers can be randomly crossed to form an interconnected network structure in a planar orientation to form a thin CNT film.
[0068] In operation 105, the resulting CNT film is separated from the filtration membrane starting from a first end of the CNT film toward a second end that slightly overlaps the first end. Once completely separated from the filtration membrane, the nanofiber film is ready for the next operation 106.
[0069] In operation 106, the peeled CNT film is then harvested using a frame, also called a collector frame or harvester frame, and then transferred and mounted directly onto virtually any solid substrate, such as a pellicle boundary with a defined opening. The CNT film may be attached to the pellicle boundary and covered over the opening to form a pellicle. The transferred film attached to any frame, such as a metal frame, silicon frame, or pellicle boundary, with an opening as small as 5 mm x 5 mm may be useful. There is a high demand for even larger size films, 110 mm x 140 mm or more, that serve as full size pellicle films for actual EUV scanners. Characterization of the CNT film can be performed, such as optical light transmittance and / or transmittance uniformity testing, EUV transmittance and / or transmittance uniformity testing, mechanical strength, deflection testing, transparency testing, deflection under constant pressure or pumping down conditions, life testing, particle testing, etc. Full size pellicles for EUV lithography scanning may require ultra-thin free-standing films (usually larger than 110 mm x 140 mm) based on current industry standards. A full-size pellicle is sometimes called a full-field pellicle.
[0070] The pellicle frame referred to herein can withstand high temperature processing to sustain high temperature annealing. Additionally, the pellicle frame can have a low coefficient of thermal expansion to avoid or induce stretching of the nanofiber film attached thereto. Exemplary frame materials can be selected from silicon dioxide, commonly known as quartz, silicon carbide, and the like.
[0071] In optional operation 107, the CNT film on the frame, pellicle boundary, or intermediate transfer frame is subjected to a thermal annealing treatment. The thermal annealing treatment is performed by placing the CNT film in an enclosed or vacuum chamber at a predetermined elevated temperature for a specific period of time. However, aspects of the present disclosure are not limited in this respect and various thermal annealing treatments may be performed at different temperatures, for different periods (durations), and with different thermal energy sources, e.g., different electromagnetic wavelengths or wavelength ranges.
[0072] In one example, the thermal annealing process may be performed at target temperatures of about 600°C or more, about 700°C or more, about 800°C or more, about 900°C or more, and less than about 3,000°C, less than about 2,500°C, less than about 2,000°C, or less than about 1,500°C. The actual annealing temperature is preferably constant, but may vary within a temperature range of 2-10% above or below the predetermined target temperature measured in the annealing chamber or near the annealing target, i.e., the pellicle film. For a target temperature of 600°C, the actual temperature may be measured between 540°C and 660°C.
[0073] In another example, the thermal annealing process may be carried out at the target temperature or temperature range for 1 second to 60 minutes, with the preferred process time being 10 minutes to 30 minutes.
[0074] In another example, the annealing process may be performed in a chamber where the annealing chamber pressure is atmospheric, vacuum, or somewhere in between. The annealing process chamber generally supports the distribution of thermal energy, preferably uniform distribution throughout the chamber. The thermal energy can be directed to one or more targets, such as one or more CNT films. The thermal energy can also be diffused within the chamber, immersing one or more films, and uniformly processing the entire set of pellicle films with less variability. Annealing variations, such as uneven energy deposited on or received by the film, can cause, for example, film wrinkling, focal film thickening or thinning, premature film breakage, etc. These events or changes can change the light transmission of the film, exacerbating the transmission variation, weakening the mechanical strength of the film, and shortening the film's lifespan.
[0075] In another example, the annealing process may be performed by electromagnetic radiation, where a selected electromagnetic wave(s), either a single wavelength in the range of 1 nm to 1 mm, or a mixture of two or more overlapping and / or non-overlapping wavelengths, is directed to at least a portion of the pellicle film, or preferably the entire pellicle film, for a predetermined duration of 0.1 ms to 1 s.
[0076] EUV transmission and EUV transmission reduction High EUV transmittance is required for extreme ultraviolet (EUV) pellicles. This is especially important for current EUV photolithography and future high power EUV photolithography. Typical EUV transmittance is often measured at a wavelength of about 13.5 nm and is generally 75% or more, 80% or more, 88% or more, 92% or more, or preferably 95% or more, and up to 99%. The EUV pellicle film may be further annealed to increase the EUV transmittance. In one example, the CNT film produced in operations 101 to 107 can be provided with a transmittance of about 93.05% at EUV 13.5 nm wavelength. However, the storage conditions of the nanofiber EUV pellicle film and the CNTE UV pellicle film are not clearly known. The above CNT pellicle film with an EUV transmittance of 93.05% was stored in a stainless steel container (about 100 cubic inches, inner chamber 15 cubic inches) for one month, after which the EUV transmittance was remeasured. Another CNT pellicle film (sibling sample) from the same sample preparation batch was stored in an acrylic container (3.5" x 3.5" x 0.5" (length x width x height), 1 / 16" thick container material) for one month and the EUV transmittance of the film was measured. Both samples and their containers were stored under ambient conditions, i.e., normal atmospheric pressure, same room temperature, and same humidity. Both containers were filled with room air. The results are summarized in Table 1. [Table 1]
[0077] Table 1 shows that the EUV transmittance of the annealed CNT films changes over time based on the storage conditions of the pellicle films. The EUV transmittance of the samples stored in the insulated acrylic plastic container decreased twice as fast as the EUV transmittance of the samples stored in the stainless steel container. Both insulated containers are not vacuum sealed or filled with inert gas, and are exposed to similar amounts of ambient air within the containers.
[0078] Acrylic is a transparent plastic that is commonly used as a storage container material due to its excellent optical clarity and transparency, resistance to temperature changes, and resistance to various chemicals. However, it also has a high outgassing rate. The volatile organic compounds emitted from the acrylic container were doubled when comparing these two storage container materials, despite the container being much smaller than the stainless steel container. Other low outgassing plastics, such as polyvinylidene fluoride (PVDF), polyetheretherketone (PEEK), polytetrafluoroethylene (PTFE or Teflon), polyimide, ethylene chlorotrifluoroethylene (ECTFE), and polycarbonate, may be better choices for EUV pellicle container materials. Long-term storage of pellicles in synthetic plastic containers should be carefully evaluated as they may have more than normal adverse effects on the properties of ultrathin CNT pellicles and pellicle films. Pre-purging the storage or transport container for pellicle films, including the container material itself and / or the storage space inside the container, with a selected inert gas, including but not limited to nitrogen or argon, may be a preventative option. Container materials that have been previously purged with a selected inert gas may release such inert gas when vacuum sealed.
[0079] Additionally, the decrease in EUV transmittance for the stainless steel pellicle storage container shown in Table 1 may be due to the adsorption of small amounts of gaseous substances from the atmosphere during testing. A vacuum-sealed storage environment or a storage environment filled with inert gas could be one of the additional measures to properly maintain the properties of the CNT EUV pellicle film, such as EUV transmittance, EUV transmission variation, deflection, and tensile strength.
[0080] FTIR spectroscopy measurements Fourier transform infrared spectroscopy (FTIR spectroscopy) measures how much light a target sample, such as a liquid, gas, or solid, absorbs at each wavelength in the infrared spectrum. Depending on its chemical properties and composition, the sample material absorbs some of the infrared light, while other infrared light passes through and can be recorded by the detector. A computer analyzes the recorded raw data, called an interferogram, and displays the corresponding light absorption or transmission at each wavelength in a graphical arrangement. For a given sample material, a representative data set and a computer-generated graph curve are included, which are like a fingerprint of the tested material. When the same material is altered, its light absorption characteristics can change due to changes in its structure, chemical composition, chemical residues, and the resulting molecular vibration patterns. These changes create a new data set or a new curve.
[0081] Because most materials contain multiple chemical components, contaminants, or outgassing substances, FTIR spectroscopy will likely represent the absorption characteristics of the material mixture, resulting in a more complex graph or pattern. A particular range of spectroscopic wavelengths may be typical, meaningful, and / or sufficient to indicate variation within a given test material.
[0082] Comparing data collected before and after annealing a sample material can reveal changes accumulated within the same material. Similar comparisons often correlate with different measurements from the same type of sample material that have been processed in the same way or that have undergone similar changes to the sample material.
[0083] In addition to the EUV transmission measurements, differences observed by FTIR could be studied and may represent or correlate to the same modifications within the nanofiber pellicle film.
[0084] In the experiment, the CNT pellicle film was first annealed at 650 °C for 30 min and then stored in an acrylic plastic container (3.5 in. x 3.5 in. x 0.5 in., 1 / 16 in. thick walls) with silicone rubber-based materials such as silicone rubber gaskets and silicone rubber spacer strips (3.0 in. x 0.25 in. x 0.25 in.) for 24 h. FTIR measurements of the CNT pellicle film were performed before annealing (often referred to as the pristine CNT pellicle film), after annealing, and after 24 h of storage in the acrylic plastic container with the silicone rubber materials. Results (at wavenumber 2950 (cm -1 ) and 2880(cm -1 ) are plotted in Figure 3, and 2940 (cm -1 ) and 2900(cm -1 There is a significant change between these measurements for wavenumbers between 2940 (cm). The graph for the untreated CNT pellicle film before annealing (solid curve) shows -1 ) and 2900(cm -1 ) has a deep "V" shape between the annealed CNT pellicle film and the EUV transmittance. After annealing, the line of the graph flattens out (the annealed CNT pellicle film is shown by the dashed curve), but when stored in an acrylic plastic container with silicone rubber, the curvature returns to a very close original curve (the annealed CNT pellicle film was stored in an acrylic plastic container for 24 hours and measured the next day by the dotted curve). These changes indicate an initial loss of certain material on the CNT surface as shown by an increase in the measured infrared transmittance, followed by a recovery of the material loss as shown by a decrease in the infrared transmittance. Typical chemicals represented in the wavenumber ranges shown in the literature can be aliphatic hydrocarbons. These FTIR measured changes also correspond to the changes in EUV transmittance and EUV transmittance measured by direct EUV transmittance measurements previously observed, as shown above, and other data not included in this specification.
[0085] Silicone rubber has been reported to continue to outgas at very low levels. It is also known that outgassing may occur at high temperatures and low pressures. While the amount of outgassing may be negligible for non-EUV lithography applications, the effect on ultra-thin CNT pellicle films can be significant. CNT pellicle films can adsorb trace amounts of outgassed gas and alter their EUV transmittance.
[0086] In summary, acrylic plastic and / or rubber-like materials affect the EUV transmittance of ultra-thin CNT pellicle films. More specifically, the studied materials can decrease the EUV transmittance of thin CNT pellicle films.
[0087] Other common storage container materials include, but are not limited to, polycarbonate plastic, polypropylene plastic, or other synthetic materials that may release or out-gas trace amounts of the original starting components (monomers or polymers), VOCs, and / or catalysts.
[0088] According to another aspect of the present disclosure, exposure of the CNT EUV pellicle film to the above-mentioned materials for storage and transport containers can affect not only the EUV transmittance but also the EUV scattering, the deflection of the EUV pellicle film, the tensile strength of the EUV pellicle film, or a combination thereof. Because the thickness of the CNT EUV pellicle film is typically in the range of a few nanometers to tens of nanometers, the adsorption of aliphatic carbons can ultimately increase the weight of the ultra-lightweight film, causing the film to sag and reduce the tensile strength.
[0089] In another experiment, the CNT pellicle film was first annealed at 650 °C for 30 min and then stored in a glass container at atmospheric pressure, humidity, and room air for 24 h. FTIR measurements of this CNT pellicle film were performed before annealing, after annealing, and after 24 h of storage in the glass container. The results are plotted in Figure 4. Figure 4 shows a different pattern compared to Figure 3. After the annealing treatment, the line in the graph (dashed curve - annealed CNT pellicle film) also flattened out as expected, but did not return to a curvature close to the original graph (solid curve based on measurements before annealing). It retained a similar baseline (dotted curve - measurements after storing the annealed CNT pellicle film in the glass container) to the results measured immediately after annealing. This data in Figure 4 shows that glass has little effect on the EUV transmittance of the ultrathin CNT pellicle film, at least for the duration of the test.
[0090] Additionally, in a study testing the long-term exposure of storage container materials, CNT pellicle films were first annealed at 650°C for 30 minutes and then stored in a glass container at room temperature environmental conditions for up to 35 days. FTIR measurements of this CNT pellicle film were performed before annealing and after 24 hours (1 day), 27 days, and 35 days of storage in the glass container. The results are plotted in Figure 5. After annealing, the line on the graph disappears from the "V" shape (solid line) and becomes flat, similar to the corresponding changes and curves in both Figures 3 and 4. After 24 hours of storage in the glass container, no significant changes were observed in the FTIR measurements (dashed curve). The samples were re-measured after 27 and 35 days. The graph representing measurements taken 27 days after annealing (dotted line) shows a predominant curvature, or deep "V" characteristic, between the data set of the unannealed sample (not shown) and the annealed sample 24 hours after annealing, with a decrease in infrared transmittance in the corresponding wavelength range. The graph representing measurements taken 35 days after annealing (dash-dotted curve) shows a deeper "V" curvature and further loss of infrared transmittance. This again indicates that CNT pellicle films stored in glass containers reacquire aliphatic hydrocarbons on the CNT surface at a much slower rate than those stored in acrylic containers, both of which ultimately impact the EUV transmission of the CNT EUV pellicle.
[0091] Embodiments of the present disclosure further demonstrate the need and / or necessity to store nanofiber EUV pellicles or pellicle films in vacuum conditions, room air or gas purged environments, or in inert gas filled containers with carefully selected storage and shipping container materials.
[0092] Preferred EUV pellicle or pellicle film container materials include, but are not limited to, metal, stainless steel, glass, borosilicate glass, glass ceramic, or quartz. The illustrations of the embodiments described herein are intended to provide a general understanding of the various embodiments. The figures are not intended to serve as a complete description of all elements and features of the products and methods forming the products or methods described herein. Many other embodiments may become apparent to those skilled in the art upon consideration of the present disclosure. Since other embodiments may be utilized and derived from the present disclosure, structural and logical substitutions and changes may be made without departing from the scope of the present disclosure. Furthermore, the illustrations are merely representative and may not be drawn to scale. Certain proportions within the illustrations may be exaggerated, while other proportions may be minimized. Thus, the present disclosure and the figures should be considered illustrative rather than limiting.
[0093] One or more embodiments of the present disclosure may be referred to herein, individually and / or collectively, by the term "invention" merely for convenience and without any intention to spontaneously limit the scope of the present application to any particular invention or inventive concept. In addition, although specific embodiments have been illustrated and described herein, it will be understood that any subsequent arrangements designed to achieve the same or similar purpose may be substituted for the specific embodiment shown. The present disclosure is intended to cover any and all subsequent adaptations or variations of the various embodiments. Combinations of the foregoing embodiments, as well as other embodiments not specifically described herein, will be apparent to one of ordinary skill in the art upon review of this description.
[0094] The Abstract of the Disclosure is submitted with the understanding that it will not be used to interpret or limit the scope or meaning of the claims. In addition, the foregoing Detailed Description may group or describe various features together in a single embodiment for the purpose of streamlining the disclosure. The disclosure should not be interpreted as reflecting an intention that the claimed embodiments require more features than are expressly recited in each claim. Rather, as the following claims reflect, the inventive subject matter may be directed to less than all of the features of any of the disclosed embodiments. Thus, the following claims are incorporated into the Detailed Description, with each claim standing on its own as defining separately claimed subject matter.
[0095] The subject matter discussed above should be considered illustrative and not limiting, and the appended claims are intended to cover all such modifications, extensions, and other embodiments that fall within the true spirit and scope of the present disclosure. Accordingly, to the maximum extent permitted by law, the scope of the present disclosure should be determined by the broadest permissible interpretation of the following claims and their equivalents, and should not be limited or restricted by the foregoing detailed description.
Claims
1. A storage device, comprising: Including materials, the material maintains one or more properties of an extreme ultraviolet (EUV) lithography pellicle; The storage device, wherein the one or more properties are selected from EUV transmittance, EUV transmission variation, EUV scattering, EUV pellicle film deflection, EUV pellicle film tensile strength, or a combination thereof.
2. The storage device of claim 1 , wherein the material outgases to maintain one or more properties of the EUV lithography pellicle.
3. The storage device of claim 1 , wherein the material is stainless steel.
4. The storage device of claim 1 , wherein the material is selected from glass or borosilicate glass.
5. The storage device of claim 1 , wherein the material is selected from glass ceramic or quartz.
6. The storage device of claim 1 , wherein the storage device is vacuum sealed.
7. 10. The storage device of claim 1, wherein the storage device is filled with an inert gas.
8. The storage device of claim 1 , wherein the material is pre-purged with an inert gas.
9. 1. A method for storing an extreme ultraviolet (EUV) lithography pellicle, comprising: Preparing an EUV lithography pellicle; placing the EUV lithography pellicle in a container; Including, The container contains at least a material; The method, wherein the material maintains one or more properties of an EUV lithography pellicle selected from EUV transmittance, EUV transmission variation, EUV scattering, EUV lithography pellicle film deflection, EUV lithography pellicle film tensile strength, or a combination thereof.
10. The method of claim 9 , wherein the material is selected from stainless steel, glass, borosilicate glass, glass ceramic, or quartz.
11. The method of claim 9 further comprising maintaining a vacuum pressure within the vessel.
12. 10. The method of claim 9, further comprising filling the container with an inert gas.
13. The method of claim 9 further comprising purging the material contained within the vessel with an inert gas.