Novel catalyst for olefin polymerization

A catalyst system combining specific metallocene compounds addresses the moldability issues of metallocene polyolefins by producing ethylene polymers with wide molecular weight distribution and long chain branches, enhancing moldability and mechanical properties.

JP2024149437APending Publication Date: 2024-10-18JAPAN POLYETHYLENE CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024060814
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2024-04-04
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Metallocene polyolefins exhibit excellent mechanical properties but have narrow molecular weight distribution, leading to insufficient moldability, melt tension, and melt fluidity, which are crucial for molding processes. Existing methods to broaden molecular weight distribution or introduce long chain branches have not adequately addressed these issues, particularly in high molecular weight components.

Method used

A catalyst system comprising a combination of metallocene compounds represented by specific formulas (A-1) and (A-2), along with a compound that forms a cationic metallocene compound, is used to produce polyolefins with wide molecular weight distribution and long chain branches in the high molecular weight region, enhancing moldability.

Benefits of technology

The catalyst system produces ethylene polymers with improved molecular weight distribution and long chain branches, resulting in enhanced moldability, melt tension, and fluidity, while maintaining mechanical properties such as rigidity and impact strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149437000037
    Figure 2024149437000037
  • Figure 2024149437000038
    Figure 2024149437000038
  • Figure 2024149437000039
    Figure 2024149437000039
Patent Text Reader

Abstract

To provide a catalyst for olefin polymerization, capable of producing an ethylene polymer having a wide molecular weight distribution and long chain branching in a high molecular weight region, to improve moldability of metallocene-based polyethylene.SOLUTION: A catalyst for olefin polymerization comprises a component (A-1): a metallocene compound represented by formula (1), a component (A-2): a metallocene compound represented by formula (2), and a component (B): a compound that reacts with components (A-1) and (A-2) to produce a cationic metallocene compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel olefin polymerization catalyst, a method for producing an olefin polymer using the catalyst, and an olefin polymer produced by the method. More specifically, the present invention relates to an olefin polymerization catalyst containing two specific types of metallocene compounds and a compound that reacts with the metallocene compound to produce a cationic metallocene compound, a method for producing an olefin polymer using the catalyst, and an olefin polymer or ethylene polymer produced by the method. [Background technology]

[0002] Polyolefins produced with metallocene catalysts for olefin polymerization have a high uniformity of polymer molecular structure, such as molecular weight distribution and copolymer composition distribution, and are excellent in various mechanical properties, such as impact strength and long life, and therefore their usage has been increasing in recent years. However, although metallocene-based polyolefins are excellent in various mechanical properties, due to their narrow molecular weight distribution, they do not satisfy sufficient performance in important properties for polyolefin molding processing, such as melt tension and melt fluidity.

[0003] As a method for improving the moldability of metallocene-based polyolefins, a method for broadening the molecular weight distribution by multi-stage polymerization using a metallocene catalyst is known (Patent Document 1). However, the method for broadening the molecular weight distribution by multi-stage polymerization causes other problems, such as construction costs and operation and management costs for linking and using polymerization reaction groups.

[0004] On the other hand, known methods for improving the insufficient moldability of metallocene-based polyolefins include a method for improving the fluidity and melt tension by introducing long chain branches into polyethylene through a polymerization reaction using a specific metallocene complex to increase the melt viscosity (Patent Document 2), and a method for designing a catalyst to prepare a polymer having multiple peaks in the molecular weight distribution (Patent Document 3).

[0005] As another approach to this problem, a binary complex catalyst technology has been studied in which a catalyst composition containing a combination of two types of complexes is used to produce polyethylene with a sufficient number and appropriate length of long-chain branches introduced (Patent Documents 4 to 8). These patent documents attempt to introduce a long-chain branch structure by designing a binary complex catalyst using a metal complex containing a bridged or unbridged cyclopentadienyl (Cp) group. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 3-234717 [Patent Document 2] Japanese Patent Application Publication No. 2-276807 [Patent Document 3] JP 2017-197739 A [Patent Document 4] JP 2012-214780 A [Patent Document 5] JP 2017-145303 A [Patent Document 6] JP 2019-059934 A [Patent Document 7] Special Publication No. 2019-515997 [Patent Document 8] JP 2010-043152 A Summary of the Invention [Problem to be solved by the invention]

[0007] In order to improve the molding processability of polyolefins, attempts have been made to broaden the molecular weight distribution or introduce long chain branches. In particular, when long chain branches are present up to high molecular weight components (approximately Mw = 100,000 to 10 million) among various molecular weight bands contained in polyolefins, the long-term relaxation components in the melt viscoelasticity increase, and the swell ratio, memory effect, melt tension and flowability ratio increase, which is advantageous for molding processability. The above-mentioned methods have been used as catalysts aimed at realizing such polymers, but in the method of Patent Document 2, the long chain branches in the polymer are not as developed as the structure of high-pressure low-density polyethylene (HPLD), which has excellent melt properties, and the molecular weight distribution is also narrow, so that sufficient improvement in molding processability has not been achieved. In addition, because the molecular weight distribution is narrow, mechanical properties such as rigidity and impact strength are also insufficient. Furthermore, Patent Documents 4 to 8 disclose various metallocene complexes, but these also do not sufficiently introduce a long-chain branched structure, and the physical properties of the resulting polyolefin are not satisfactory in view of molding and processing.

[0008] In order to solve the problems of polyethylenes containing long chain branches in the prior art and to improve the moldability of metallocene-based polyethylenes, there has been a demand for an olefin polymerization catalyst capable of producing ethylene polymers having a broad molecular weight distribution and long chain branches in the high molecular weight region. [Means for solving the problem]

[0009] The present inventors have found that by using a combination of a metal complex having high catalytic activity and a metal catalyst having high copolymerization activity, polyolefins having long chain branches introduced into the high molecular weight region can be obtained without inhibiting the catalytic activities of either of them, and have arrived at the present invention.

[0010] That is, the present invention relates to an olefin polymerization catalyst and an olefin polymer, which are specified by the following [1] to

[19] . [1] An olefin polymerization catalyst comprising the following components (A-1), (A-2) and (B): Component (A-1): A metallocene compound represented by the following formula (1): [ka] [In formula (1), M 1 represents a transition metal atom of Ti, Zr, or Hf, X 1 and X 2 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, an amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, Q 1 and Q 2 represents a carbon atom, a silicon atom, or a germanium atom, R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and adjacent substituents bond to each other with Q 1 and Q 2 may be bonded to form a ring, m is 0 or 1. If m is 0, then Q 1 is R 9 directly bonded to a conjugated five-membered ring containing R 5 ~R 14 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing hydrocarbon group having 1 to 18 carbon atoms including 1 to 6 silicon atoms, a halogen-containing hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 40 carbon atoms including an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, a hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms or a hydrocarbon group-substituted amino group having 1 to 40 carbon atoms; R 5 ~R 8 adjacent substituents may be bonded together to form an aliphatic ring including the carbon atom to which they are bonded, R 10 ~R 14 adjacent substituents may be bonded to each other to form a ring, including the carbon atoms to which they are bonded; n is 0 or 1. When n is 0, R10 and R 11 There is no carbon atom to which R is bonded. 12 The carbon atom to which is bonded and the conjugated five-membered ring are directly bonded to form an indenyl ring. Component (A-2): A metallocene compound represented by the following general formula (2): [ka] [In formula (2), M 2 represents a transition metal atom of Ti, Zr, or Hf, X 21 and X 22 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, an amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, R 51 ~R 60 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing hydrocarbon group having 1 to 18 carbon atoms and including 1 to 6 silicon atoms, a halogen-containing hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 40 carbon atoms which contains an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, a hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms or a hydrocarbon group-substituted amino group having 1 to 40 carbon atoms, R 51 ~R 60 Among these, any one or more pairs of adjacent groups on the same cyclopentadienyl ring may be bonded to each other via the bonding carbon atom to form a ring. Component (B): A compound that reacts with the metallocene compounds of components (A-1) and (A-2) to generate a cationic metallocene compound. [2] The olefin polymerization catalyst according to [1] above, wherein n is 0 in the formula (1) of the component (A-1). [3] The olefin polymerization catalyst according to the above [1] or [2], wherein m is 0 in the formula (1) of the component (A-1). [4] In the formula (1) of the component (A-1), R 9 The olefin polymerization catalyst according to any one of the above [1] to [3], wherein is a hydrogen atom. [5] In the formula (1) of the component (A-1), R 9 The olefin polymerization catalyst according to any one of the above [1] to [3], wherein is a hydrocarbon group having 1 to 20 carbon atoms. [6] In the formula (1) of the component (A-1), R 5 ~R 14 The olefin polymerization catalyst according to any one of the above [1] to [5], wherein at least one of the above is represented by the following formula (5): [ka] [In formula (5), A 1 indicates an atom of group 14, 15, or 16 of the periodic table, R 17 ~R 21 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, a hydrocarbon group-substituted amino group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms, and adjacent substituents may be bonded to each other through the atom bonded thereto to form a ring, p 1 is 0 or 1, and A 1 If is an atom of group 15 or 16 of the periodic table, p 1 is 0 and A 1 Substituent R 17 does not exist, q 1 is 0 or 1, and q 1 If is 0, R 20 does not exist, and R 19 The carbon atom to which R is bonded 21 is directly bonded to the carbon atom to which it is attached. [7] In the formula (1) of the component (A-1), R 5 ~R 14 The olefin polymerization catalyst according to any one of the above [1] to [5], wherein at least one of the above is represented by the following formula (6): [ka] [In formula (6), Z 1 represents an oxygen atom or a sulfur atom, R 22 ~R 24 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen atom, a sulfur atom, or a nitrogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms and containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms; R 22 ~R 24 adjacent substituents may be bonded to each other through the carbon atoms to which they are bonded to form a ring. [8] In the formula (1) of the component (A-1), R 12 The olefin polymerization catalyst according to [6] above, characterized in that the catalyst is represented by the formula (5): [9] In the formula (1) of the component (A-1), R 12 The olefin polymerization catalyst according to [7] above, characterized in that it is represented by the formula (6).

[10] In the formula (2) of the component (A-2), R 51 ~R 60 The olefin polymerization catalyst according to any one of the above [1] to [9], wherein at least one of the above is a hydrocarbon group having 1 to 20 carbon atoms.

[11] In the formula (2) of the component (A-2), R 51 ~R 60 The olefin polymerization catalyst according to any one of the above [1] to [9], wherein at least two of the above are hydrocarbon groups having 1 to 20 carbon atoms.

[12] In the formula (2) of the component (A-2), R 51~R 60 The olefin polymerization catalyst according to any one of the above [1] to [9], wherein at least four of the above are hydrocarbon groups having 1 to 20 carbon atoms.

[13] In the formula (2) of the component (A-2), R 51 ~R 55 At least one of and R 56 ~R 60 and at least one of them is a hydrocarbon group having 1 to 20 carbon atoms.

[14] In the formula (2) of the component (A-2), R 51 ~R 55 At least two of these and R 56 ~R 60 and each of the above two is a hydrocarbon group having 1 to 20 carbon atoms.

[15] The olefin polymerization catalyst according to any one of the above [1] to

[14] , further comprising the following component (C): Component (C): Microparticle carrier

[16] The olefin polymerization catalyst according to

[15] above, further comprising the following component (D): Component (D): Organoaluminum compound

[17] A method for producing an olefin polymer, comprising polymerizing or copolymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of the above [1] to

[16] .

[18] The method for producing an olefin polymer according to

[17] above, wherein the olefin is ethylene.

[19] The method for producing an olefin polymer according to

[17] or

[18] above, wherein the obtained polymer satisfies the following conditions (i) and (ii): Condition (i): The molecular weight distribution (Mw / Mn) based on the weight average molecular weight (Mw) and the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is 3.0 or more and 50.0 or less. Condition (ii): The ratio (HLMFR / MFR) of the melt flow rate at a temperature of 190°C and a load of 21.6 kg (HLMFR) to the melt flow rate at a temperature of 190°C and a load of 2.16 kg (MFR) is greater than 20 and less than 500. Effect of the Invention

[0011] According to the present invention, there is provided an olefin polymerization catalyst capable of producing an ethylene polymer which has a broad molecular weight distribution, has long chain branches in the high molecular weight region, and can have improved moldability. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a diagram showing the low molecular weight component amount ratio (WMW≦10,000) corresponding to HLMFR in the examples and comparative examples. [Diagram 2] FIG. 2 is a diagram showing the low molecular weight component amount ratio (WMW≦5000) relative to HLMFR in the examples and comparative examples. [Diagram 3] FIG. 2 is a graph showing integral and differential dissolution curves versus dissolution temperature for Example 1 and Comparative Example 1. [Figure 4] FIG. 1 is a diagram showing the baseline and intervals of a GPC chromatogram. [Diagram 5] FIG. 1 is a table for calculating the whole weight average molecular weight from the elution ratio (weight % (wt%) in the table) at each elution temperature and the weight average molecular weight (Mw in the table), using a commercially available low-density polyethylene as an example. [Figure 6] FIG. 2 is a contour plot showing the elution amounts with respect to the elution temperature and molecular weight measured by the CFC method in Example 1 and Comparative Example 1. [Figure 7] FIG. 1 shows integral and differential dissolution curves versus dissolution temperature in Example 10. [Figure 8] FIG. 1 shows a contour plot of elution amount with respect to elution temperature and molecular weight as measured by the CFC method in Example 10. [Figure 9] 1 is a schematic diagram of W1 to W4, where the horizontal axis represents the logarithm of the molecular weight and the vertical axis represents the elution temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] One embodiment of the present invention is an olefin polymerization catalyst comprising: component (A-1): a metallocene compound represented by the above formula (1); component (A-2): a metallocene compound represented by the above formula (2); and component (B): a compound that reacts with component (A-1) and component (A-2) to produce a cationic metallocene compound.

[0014] The polymerization catalyst, the method for producing the polymerization catalyst, the monomers constituting the polymer, the polymerization method, etc. will be described in detail below. In the following description, "polymerization" refers to a reaction in which a monomer forms a polymer having 20 or more monomers. The term "polymerization" collectively refers to homopolymerization of one type of monomer and copolymerization of multiple types of monomers, and when there is no need to distinguish between the two, they will be collectively referred to simply as "polymerization". In addition, the present invention also relates to a method for producing a polymer, but the structure of the polymer itself cannot generally be determined unambiguously by a chemical formula or the like. Therefore, in this specification, when describing a polymer, the polymer will be described using its production method as necessary.

[0015] Hereinafter, in the case of specific substituents, when a hydrocarbon group is mentioned, it means a linear, branched, or cyclic group. The valency of the hydrocarbon group will be understood in the context, but a monovalent group is represented by adding "-yl" to the end of the word, and a divalent group is represented by adding "-ene" to the end of the word.

[0016] 1. Ingredient (A-1) The component (A-1) in the olefin polymerization catalyst of the present invention is a metallocene compound represented by the following general formula (1). [ka] (The definition of each group in the formula is as described above.) The metallocene compound of the above formula (1) has a structure in which a cyclopentadienyl ring and an indenyl ring (or an azulenyl ring) are crosslinked. The metallocene compound of the above formula (1) can be used as a catalyst component for olefin polymerization to obtain an ethylene polymer containing a vinyl group at the end at a high rate. Since the vinyl group at the end is further involved in the polymerization reaction, the use of a catalyst containing the metallocene compound of the above formula (1) makes it easier to obtain a polymer into which long chain branches are easily introduced.

[0017] In the general formula (1), M represents a transition metal atom of any one of Ti, Zr and Hf, preferably Zr or Hf, and more preferably Zr.

[0018] In general formula (1), X 1 and X 2 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, an amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. X 1 and X 2 Examples of the halogen atom represented by the formula (I) include a chlorine atom, a bromine atom, and an iodine atom. X 1 and X 2 Examples of the hydrocarbon group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a t-butyl group, an n-pentyl group, a neopentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, a phenyl group, and a benzyl group.

[0019] X 1 and X 2Examples of the hydrocarbon group having 1 to 20 carbon atoms and containing an oxygen atom represented by the formula (I) include a methoxymethyl group, an ethoxymethyl group, an n-propoxymethyl group, an i-propoxymethyl group, an n-butoxymethyl group, an i-butoxymethyl group, a t-butoxymethyl group, a methoxyethyl group, an ethoxyethyl group, an acetyl group, a 1-oxopropyl group, a 1-oxo-n-butyl group, a 2-methyl-1-oxopropyl group, a 2,2-dimethyl-1-oxo-propyl group, a phenylacetyl group, a diphenylacetyl group, a benzoyl group, a 2-methoxyphenyl group, a 3-methoxyphenyl group, a 4-methoxyphenyl group, a 2-furyl group, and a 2-tetrahydrofuryl group.

[0020] X 1 and X 2 Examples of the nitrogen atom-containing hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) include a dimethylaminomethyl group, a diethylaminomethyl group, a di-i-propylaminomethyl group, a bis(dimethylamino)methyl group, a bis(di-i-propylamino)methyl group, a (dimethylamino)(phenyl)methyl group, a methylimino group, an ethylimino group, a 1-(methylimino)ethyl group, a 1-(phenylimino)ethyl group, and a 1-[(phenylmethyl)imino]ethyl group. X 1 and X 2 Examples of the hydrocarbon-substituted amino group having 1 to 20 carbon atoms represented by the formula (I) include a dimethylamino group, a diethylamino group, a di-n-propylamino group, a di-i-propylamino group, a di-n-butylamino group, a di-i-butylamino group, a di-t-butylamino group, and a diphenylamino group. X 1 and X 2 Examples of the alkoxy group having 1 to 20 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, a t-butoxy group, and a phenoxy group.

[0021] Preferred X 1 and X 2Examples of the alkyl group include a chlorine atom, a bromine atom, a methyl group, an n-butyl group, an i-butyl group, a methoxy group, an ethoxy group, an i-propoxy group, an n-butoxy group, a phenoxy group, a dimethylamino group, and a di-i-propylamino group. Among these, a chlorine atom, a methyl group, and a dimethylamino group are particularly preferred.

[0022] In general formula (1), Q 1 and Q 2 represents a carbon atom, a silicon atom, or a germanium atom, preferably represents a carbon atom or a silicon atom, and more preferably represents a silicon atom.

[0023] In general formula (1), R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms; R 1 , R 2 , R 3 and R 4 At least two of the Q groups are adjacent to each other and bond to each other. 1 and / or Q 2 may be bonded to form a ring. m is 0 or 1. If m is 0, then Q 1 is R 9 The preferred value of m is 0.

[0024] R 1 , R 2 , R 3 and R 4 Each of the groups independently includes a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a t-butyl group, an n-pentyl group, a neopentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, a phenyl group, and the like. Also, R 1 , R 2 , R 3 and R 4 At least two of them combine to form Q 1 and Q 2Examples of groups that form a ring together with the above include a cyclobutylidene group, a cyclopentylidene group, a cyclohexylidene group, a silacyclobutyl group, a silacyclopentyl group, and a silacyclohexyl group. Preferred R 1 , R 2 , R 3 and R 4 As a concrete example, Q 1 Or / and Q 2 When Q is a carbon atom, examples of the groups include a hydrogen atom, a methyl group, an ethyl group, a phenyl group, an ethylene group, and a cyclobutylidene group. 1 and Q 2 When R is a carbon atom, it is also possible to form a vinylene group, in which case R 2 , R 4 does not exist, and R 1 , R 3 It is also possible for Q to form a benzene ring or a cyclohexene ring together. 1 Or / and Q 2 When is a silicon atom, examples of the group include a methyl group, an ethyl group, a phenyl group, and a silacyclobutyl group.

[0025] R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 and R 14 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing hydrocarbon group having 1 to 18 carbon atoms including 1 to 6 silicon atoms, a halogen-containing hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 40 carbon atoms which contains an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, a hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms, or a hydrocarbon group-substituted amino group having 1 to 40 carbon atoms.

[0026] R 5 ~R 14 In the above, examples of the halogen atom include a chlorine atom, a bromine atom, and an iodine atom. R 5~R 14 In the above formula, examples of the hydrocarbon group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a propenyl group, an n-butyl group, an i-butyl group, a t-butyl group, a butenyl group, an n-pentyl group, a neopentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, a cyclohexenyl group, a phenyl group, a cyclohexylmethyl group, a benzyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 3,5-dimethylphenyl group, a 4-t-butylphenyl group, a 3,5-di-t-butylphenyl group, a biphenyl group, and a naphthyl group. R 5 ~R 14 In the formula, examples of the silicon-containing hydrocarbon group having 1 to 18 carbon atoms and including 1 to 6 silicon atoms include a bis(trimethylsilyl)methyl group and a bis(t-butyldimethylsilyl)methyl group.

[0027] R 5 ~R 14 In the above formula, examples of the halogen-containing hydrocarbon group having 1 to 20 carbon atoms include a bromomethyl group, a chloromethyl group, a 2-chloroethyl group, a 2-bromoethyl group, a 2-bromopropyl group, a 3-bromopropyl group, a 2-bromocyclopentyl group, a 2,3-dibromocyclopentyl group, a 2-bromo-3-iodocyclopentyl group, a 2,3-dibromocyclohexyl group, a 2-chloro-3-iodocyclohexyl group, a 2-chlorophenyl group, a 4-chlorophenyl group, a 2,3,4,5,6-pentafluorophenyl group, and a 4-trifluoromethylphenyl group. R 5 ~R 14In the above formula, examples of the hydrocarbon group containing an oxygen atom and having 1 to 40 carbon atoms include a methoxymethyl group, an ethoxymethyl group, an n-propoxymethyl group, an i-propoxymethyl group, an n-butoxymethyl group, an i-butoxymethyl group, a t-butoxymethyl group, a methoxyethyl group, an ethoxyethyl group, an acetyl group, an acetoxy group, a 1-oxopropyl group, a 1-oxo-n-butyl group, a 2-methyl-1-oxopropyl group, a 2,2-dimethyl-1-oxopropyl group, a phenylacetyl group, a diphenylacetyl group, a benzoyl group, a 2-methoxyphenyl group, a 3-methoxyphenyl group, a 4-methoxyphenyl group, a 2-furyl group, a 2-methylfuryl group, and a 2-tetrahydrofuryl group.

[0028] R 5 ~R 14 In the above formula, examples of the hydrocarbon group containing a sulfur atom and having 1 to 40 carbon atoms include a methylthiomethyl group, an ethylthiomethyl group, an n-propylthiomethyl group, an i-propylthiomethyl group, an n-butylthiomethyl group, an i-butylthiomethyl group, a t-butylthiomethyl group, a methylthioethyl group, an ethylthioethyl group, a thioacetyl group, a 1-thioxopropyl group, a 1-thioxo-n-butyl group, a 2-methyl-1-thioxopropyl group, a 2,2-dimethyl-1-thioxopropyl group, a phenylthioacetyl group, a diphenylthioacetyl group, a thiobenzoyl group, a 2-methylthiophenyl group, a 3-methylthiophenyl group, a 4-methylthiophenyl group, a 2-thienyl group, a 2-methylthienyl group, and a 2-tetrahydrothienyl group. R 5 ~R 14 In the above formula, examples of the nitrogen atom-containing hydrocarbon group having 1 to 40 carbon atoms include a dimethylaminomethyl group, a diethylaminomethyl group, a di-i-propylaminomethyl group, a bis(dimethylamino)methyl group, a bis(di-i-propylamino)methyl group, a (dimethylamino)(phenyl)methyl group, a methylimino group, an ethylimino group, a 1-(methylimino)ethyl group, a 1-(phenylimino)ethyl group, and a 1-[(phenylmethyl)imino]ethyl group.

[0029] R 5 ~R14 In the above formula, examples of the hydrocarbon group containing a phosphorus atom and having 1 to 40 carbon atoms include a dimethylphosphinomethyl group, a diethylphosphinomethyl group, a di-i-propylphosphinomethyl group, a bis(dimethylphosphino)methyl group, a bis(di-i-propylphosphino)methyl group, a (dimethylphosphino)(phenyl)methyl group, a methylphosphanylidene group, an ethylphosphanylidene group, a 1-(methylphosphanylidene)ethyl group, a 1-(phenylphosphanylidene)ethyl group, and a 1-[(phenylmethyl)phosphanylidene]ethyl group. R 5 ~R 14 In the above, examples of the hydrocarbon-substituted silyl group having 1 to 40 carbon atoms include a trimethylsilyl group, a tri-t-butylsilyl group, a di-t-butylmethylsilyl group, a t-butyldimethylsilyl group, a triphenylsilyl group, a diphenylmethylsilyl group, and a phenyldimethylsilyl group. R 5 ~R 14 In the above, examples of the hydrocarbon-substituted amino group having 1 to 40 carbon atoms include a dimethylamino group, a methylethylamino group, a diethylamino group, a (methyl)(n-propyl)amino group, a di-n-propylamino group, a dipropenylamino group, a di-i-propylamino group, a di-n-butylamino group, a di-i-butylamino group, a di-t-butylamino group, a di-n-pentylamino group, a di-n-hexylamino group, a di-n-octylamino group, a di-n-dodecylamino group, a (methyl)(phenyl)amino group, a diphenylamino group, a di(4-methyl-phenyl)amino group, a di(3,5-dimethyl-phenyl)amino group, and a dibenzylamino group.

[0030] Preferred R 5 ~R 14 is preferably a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon-substituted silyl group having 1 to 40 carbon atoms, more preferably a hydrogen atom, a methyl group, a t-butyl group, or a trimethylsilyl group. R 5 ~R 8 At least two of R 6 and R 7Of these, one of them is not a hydrogen atom, and more preferably, R 6 and R 7 are not both hydrogen atoms, but R 5 ~R 8 In another preferred embodiment, at least three are not hydrogen atoms, and more preferably, R 5 ~R 8 are not all hydrogen atoms, and particularly preferably, R 5 ~R 8 are all methyl groups when not a hydrogen atom, and most preferably, R 5 ~R 8 are all methyl groups.

[0031] In a preferred embodiment, the metallocene compound represented by the general formula (1) has a ligand having a structure in which a cyclopentadienyl group is bridged with an indenyl group or an azulenyl group. Thus, in the above formula (1), n ​​is 0 or 1. When n is 0, R 10 and R 11 There is no carbon atom to which R is bonded. 12 The carbon atom to which n is attached and the conjugated 5-membered ring are directly bonded to form an indenyl ring. The preferred value of n is 0.

[0032] The metallocene compound represented by the general formula (1) is a compound having the above-mentioned structure. 1 More preferred structures of the cyclopentadienyl ring to which is coordinated are described below.

[0033] In one preferred embodiment, the group R 9 is a hydrogen atom.

[0034] In another preferred embodiment, the group R 9 R is a hydrocarbon group having 1 to 20 carbon atoms. 9 is more preferably a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a propenyl group, an n-butyl group, an i-butyl group, a t-butyl group, or a phenyl group, further preferably a methyl group or an ethyl group, and particularly preferably a methyl group.

[0035] In another preferred embodiment, R 5 ~R 14 At least one of R is a halogen or the above-mentioned hydrocarbon group having 1 to 20 carbon atoms. For the purpose of adjusting the molecular weight distribution and the structure of long chain branches of the resulting olefin polymer according to the application of the polymer, or for the purpose of improving the activity of the active species derived from component (A-1), 12 In one preferred embodiment, R 5 ~R 14 At least one of the groups represents a substituent having a cyclic structure represented by the following general formula (5), and preferably represents a phenyl group, a furyl group, or a thienyl group having a specific substituent. [ka]

[0036] In general formula (5), A 1 indicates an atom in Group 14, 15, or 16 of the periodic table. R 17 , R 18 , R 19 , R 20 and R 21 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, a hydrocarbon group-substituted amino group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms, and adjacent substituents may be bonded to each other including the atom bonded thereto to form a ring. p 1 is 0 or 1, and A 1 If is an atom of group 15 or 16 of the periodic table, p 1 is 0 and A 1 Substituent R 17 does not exist. 1 When is 0, A 1 is preferably an oxygen atom. 1 When is 1, A1 is preferably a carbon atom. q 1 is 0 or 1, and q 1 If is 0, R 20 does not exist, and R 19 The carbon atom to which R is bonded 21 is directly bonded to the carbon atom to which it is bonded.

[0037] A 1 If is a carbon atom, R 9 ~R 14 , R 17 ~R 21 It is preferable that at least one of R is not a hydrogen atom. 17 ~R 21 is preferably not a halogen atom. R 17 ~R 21 When the group represented by the formula (I) is other than a hydrogen atom, the halogen atom, the hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, the silicon-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, the halogen-containing hydrocarbon group having 1 to 20 carbon atoms, or the hydrocarbon-substituted silyl group having 1 to 20 carbon atoms can be represented by the same formula (I) as described above. 5 ~R 14 Examples of the amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms or an alkoxy group having 1 to 20 carbon atoms include the same groups as those described above for X 1 and X 2 Examples of the groups include the same groups as those described above.

[0038] In another preferred embodiment, R 5 ~R 14 At least one of the groups represents a substituent having a cyclic structure represented by the following general formula (6). [ka]

[0039] In general formula (6), Z 1 represents an oxygen atom or a sulfur atom. R22 ~R 24 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms; R 22 ~R 24 Adjacent substituents may be bonded to each other via the carbon atoms to which they are bonded to form a ring.

[0040] R 22 ~R 24 In the formula, the halogen atom, the hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, the silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, the halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms or the hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms is preferably any of the above-mentioned R 5 ~R 14 Examples of the groups include the same groups as those described above.

[0041] Specific examples of the group represented by general formula (5) or (6) include a phenyl group, a 4-trimethylsilylphenyl group, a 4-(t-butyldimethylsilyl)phenyl group, a 3,5-bistrimethylsilylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-isopropoxyphenyl group, a 4-n-butoxyphenyl group, a 2-furyl group, a 2-(5-methyl)furyl group, a 2-(5-t-butyl)furyl group, a 2-(5-trimethylsilyl)furyl group, a 2-(4,5-dimethyl)furyl group, a 2-benzofuryl group, a 2-thienyl group, a 2-(5-methyl)thienyl group, a 2-(5-t-butyl)thienyl group, a 2-(5-trimethylsilyl)thienyl group, and a 2-(4,5-dimethyl)thienyl group.

[0042] When the group represented by the general formula (5) or (6) is present, the group is R 5 ~R 14 may be in any position, but R 10 ~R12 Preferably, R 12 It is more preferable that the position is:

[0043] Specific examples of the metallocene compound of component (A-1) are shown in the following Tables 1 and 2, but are not limited thereto. In the tables, Cp is cyclopentadienyl, Ind is indenyl, Azu is azulenyl, Ph is phenyl, Me is methyl, Et is ethyl, n-Pr is normal propyl, i-Pr is isopropyl, n-Bu is normal butyl, and t-Bu is tertiary butyl. In addition, compounds in which the zirconium of the compounds shown in Tables 1 and 2 is replaced with titanium or hafnium are also included as preferred compounds.

[0044] [Table 1]

[0045] [Table 2]

[0046] 2. Component (A-2) The component (A-2) in the olefin polymerization catalyst of the present invention is a metallocene compound represented by the following general formula (2). [ka] M 2 represents a transition metal atom of Ti, Zr or Hf, preferably Zr or Hf, and more preferably Zr. The metallocene compound of the formula (2) has a structure in which the aromatic ring as a ligand is not crosslinked, and is highly efficient in producing low molecular weight polyolefins. Therefore, when a catalyst containing the metallocene compound of the formula (2) is used in combination with the compound of the formula (1), an olefin polymer (especially an ethylene polymer) having a wide molecular weight distribution and improved moldability can be obtained with high productivity. Furthermore, the metallocene compound of the formula (2) has a structure in which the aromatic ring as a ligand is not crosslinked, and is highly efficient in producing polyolefins with narrow molecular weight distribution. Therefore, when a catalyst containing the metallocene compound of the formula (2) is used in combination with the compound of the formula (1), it is possible to prevent the molecular weight distribution from spreading toward the low molecular weight side, and thus to obtain an olefin polymer (especially an ethylene polymer) with improved surface stickiness and product strength with high productivity. Furthermore, the metallocene compound of the above formula (2) has a structure in which the aromatic ring as a ligand is not crosslinked, and although it has excellent ethylene polymerization ability, it tends to have poor polymerization ability for olefins having 3 to 30 carbon atoms. Therefore, when a catalyst containing the metallocene compound of the above formula (2) is combined with the compound of the above formula (1) and used for copolymerization of ethylene and α-olefin, for example, a polymer with a low α-olefin content is produced on the low molecular weight side, and thus an olefin-based polymer (particularly an ethylene-based polymer) having improved product strength can be obtained with high productivity in some cases.

[0047] X 21 and X 22 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, an amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. 2 Specific examples of these groups bonded to the group X of general formula (1) are 1 , X 2 It is similar to the one mentioned above.

[0048] R 51 ~R 60 represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing hydrocarbon group having 1 to 18 carbon atoms including 1 to 6 silicon atoms, a halogen-containing hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 40 carbon atoms which contains an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, a hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms or a hydrocarbon group-substituted amino group having 1 to 40 carbon atoms.

[0049] R51 ~R 55 Two adjacent pairs of 56 ~R 60 Among these, two adjacent pairs may be bonded to each other to form a ring, including the carbon atom to which they are bonded. Specific examples and preferred embodiments of these groups which are the substituents of the Cp group include the group R in the general formula (1). 5 ~R 14 It is similar to the one mentioned above.

[0050] The metallocene compound represented by the general formula (2) is a compound having the above structure. 2 More preferred structures of the cyclopentadienyl ring to which is coordinated are described below.

[0051] R 51 ~R 60 In the formula (I), the halogen atom, the hydrocarbon group having 1 to 20 carbon atoms, the silicon-containing hydrocarbon group having 1 to 18 carbon atoms including 1 to 6 silicon atoms, the halogen-containing hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group having 1 to 40 carbon atoms including an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, the hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms or the hydrocarbon group-substituted amino group having 1 to 40 carbon atoms includes the above-mentioned R 5 ~R 14 Examples of the groups include the same groups as those described above.

[0052] In the formula (2), R 51 ~R 60 In another embodiment, at least one of R 51 ~R 60 It is preferable that at least two of R 51 ~R 60 At least four of these are preferably hydrocarbon groups having 1 to 20 carbon atoms. More specifically, in the formula (2), R 51 ~R 55 At least one of and R 56 ~R 60and at least one of R 51 ~R 55 At least two of these and R 56 ~R 60 At least two of the above are preferably each a hydrocarbon group having 1 to 20 carbon atoms.

[0053] In another preferred embodiment, R 51 ~R 60 At least one of the groups represents a substituent having a cyclic structure represented by the following general formula (7). [ka] In general formula (7), A 2 indicates an atom in Group 14, 15, or 16 of the periodic table. R 75 , R 76 , R 77 , R 78 and R 79 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, a hydrocarbon group-substituted amino group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms, and adjacent substituents may be bonded to each other including the atom bonded thereto to form a ring. p 2 is 0 or 1, and A 2 If is an atom of group 15 or 16 of the periodic table, p 2 is 0 and A 2 Substituent R 75 does not exist. 2 When is 0, A 2 is preferably an oxygen atom. 2 When is 1, A 2 is preferably a carbon atom. q 2 is 0 or 1, and q 2If is 0, R 78 does not exist, and R 77 The carbon atom to which R is bonded 79 is directly bonded to the carbon atom to which it is bonded.

[0054] A 2 If is a carbon atom, R 55 ~R 79 It is preferable that at least one of R is not a hydrogen atom. 75 ~R 79 is preferably not a halogen atom. R 75 ~R 79 When the group represented by the formula (I) is other than a hydrogen atom, the halogen atom, the hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, the silicon-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, the halogen-containing hydrocarbon group having 1 to 20 carbon atoms, or the hydrocarbon-substituted silyl group having 1 to 20 carbon atoms can be represented by the same formula (I) as described above. 5 ~R 16 The same groups as those described in the explanation of X can be mentioned, and the hydrocarbon-substituted amino group having 1 to 20 carbon atoms or the alkoxy group having 1 to 20 carbon atoms can be mentioned as described above. 1 and X 2 Examples of the groups include the same groups as those described above.

[0055] In another preferred embodiment, R 51 ~R 60 At least one of the groups represents a substituent having a cyclic structure represented by the following general formula (8). [ka] In general formula (8), Z 2 represents an oxygen atom or a sulfur atom. R 80 ~R 82each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen atom, a sulfur atom, or a nitrogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms and containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms; R 80 ~R 82 Adjacent substituents may be bonded to each other via the carbon atoms to which they are bonded to form a ring.

[0056] R 80 ~R 82 In the formula, the halogen atom, the hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, the silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, the halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms or the hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms is preferably any of the above-mentioned R 5 ~R 16 Examples of the groups include the same groups as those described above.

[0057] Specific examples of the group represented by general formula (7) or (8) include a phenyl group, a 4-trimethylsilylphenyl group, a 4-(t-butyldimethylsilyl)phenyl group, a 3,5-bistrimethylsilylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-isopropoxyphenyl group, a 4-n-butoxyphenyl group, a 2-furyl group, a 2-(5-methyl)furyl group, a 2-(5-t-butyl)furyl group, a 2-(5-trimethylsilyl)furyl group, a 2-(4,5-dimethyl)furyl group, a 2-benzofuryl group, a 2-thienyl group, a 2-(5-methyl)thienyl group, a 2-(5-t-butyl)thienyl group, a 2-(5-trimethylsilyl)thienyl group, and a 2-(4,5-dimethyl)thienyl group.

[0058] When the group represented by the general formula (7) or (8) is present, the group is R 51 ~R 60 It may be in any position.

[0059] Specific examples of the metallocene compound of component (A-2) are shown in the following Tables 3 to 14, but are not limited thereto. In the tables, Cp is cyclopentadienyl, Ind is an indenyl group, Azu is an azulenyl group, Ph is a phenyl group, Me is a methyl group, Et is an ethyl group, n-Pr is a normal propyl group, i-Pr is an isopropyl group, n-Bu is a normal butyl group, t-Bu is a tertiary butyl group, TMS is a trimethylsilyl group, and MeO is a methoxy group. In addition, compounds in which the zirconium of the compounds shown in Tables 3 to 14 is replaced with titanium or hafnium can also be mentioned as preferred compounds.

[0060] [Table 3]

[0061] [Table 4]

[0062] [Table 5]

[0063] [Table 6]

[0064] [Table 7]

[0065] [Table 8]

[0066] [Table 9]

[0067] [Table 10]

[0068] [Table 11]

[0069] [Table 12]

[0070] [Table 13]

[0071] The bridged-substituted CpInd-type metallocene complex catalyst or CpAzu-type metallocene complex catalyst (component (A-1)) having a substituent on the Cp ring produces a large number of macromonomers containing terminal vinyl groups at the polymer end in ethylene polymerization. Component (A-1) itself also copolymerizes with this to produce long-chain branched polymers. On the other hand, the bisCp-type metallocene complex (component (A-2)) has a lower olefin copolymerizability than (A-1), and the molecular weight of the polymer tends not to be large. When ethylene polymerization is performed using these two types of complexes, unlike when each is used alone as a catalyst, it is thought that a long-chain branched polymer and a low molecular weight polymer are simultaneously produced, and a polymer with properties advantageous for moldability is obtained. Furthermore, when ethylene-α-olefin copolymerization is performed using these two types of complexes, unlike when each is used alone as a catalyst, it is thought that a long-chain branched polymer and a low molecular weight and low α-olefin content polymer are simultaneously produced, and a polymer with properties advantageous for product strength is obtained.

[0072] 3.Method of synthesizing metallocene compounds The metallocene compound of the above formula (1) can be synthesized by any method depending on the substituents or the bonding mode. An example of a representative synthesis route is shown below. [ka]

[0073] In the above synthesis route, 3 is anionized with 1 equivalent of n-butyllithium or the like, then reacted with an excess of dimethyldichlorosilane, and the unreacted dimethyldichlorosilane is distilled off to obtain 4. The resulting 4 is reacted with 2, which has been previously treated with 1 and 1 equivalent of an anionizing agent such as n-butyllithium, to obtain 5. 5 is dianionized with 2 equivalents of n-butyllithium or the like, and then reacted with zirconium tetrachloride to obtain metallocene compound 6.

[0074] Metallocene compounds having different substituents from those in the above synthesis examples can be synthesized by using the corresponding substituted raw materials. By using substituted indenes such as phenyl, 4-trimethylsilylphenyl, 4-methylphenyl, 4-i-propylphenyl, 4-t-butylphenyl, and 4-chlorophenyl instead of the 5-methyl-2-furyl group at the 7-position of indene in 1, metallocene compounds having corresponding substituents at the 4-position of the indenyl ring can be synthesized. In addition, by using substituted indenes such as ethyl, i-propyl, t-butyl, and phenyl instead of the methyl group at the 1-position of indene in 1, metallocene compounds having corresponding substituents at the 3-position of the indenyl ring can be synthesized. Alternatively, by using an indene in which the 1-position of indene in 1 is unsubstituted, metallocene compounds having unsubstituted at the 3-position of the indenyl ring can be synthesized. Alternatively, by using a substituted indene having a substituent at at least one of the 4-, 5-, and 6-positions of the indene 1, a metallocene compound having corresponding substituents at the 5-, 6-, and 7-positions of the indenyl ring can be synthesized. Moreover, by using a corresponding substituted cyclopentadiene, such as 2,3,5-trimethylcyclopentadiene or 2-ethyl-4,5-dimethylcyclopentadiene, instead of 3, metallocene compounds having corresponding substituents introduced into the cyclopentadiene can be synthesized.

[0075] Furthermore, by using a corresponding silane compound, such as diethyldichlorosilane, diphenyldichlorosilane, or 1,1-dichlorosilacyclobutane, instead of dimethyldichlorosilane as a crosslinking agent, it is possible to synthesize a metallocene compound having a corresponding crosslinking group. Also, by referring to Z. Naturforsch. 49b, 451-458 (1994), the crosslinking group structure when m is 1 and the crosslinking group structure when R 1 , R 2 , R 3 , and R 4 Q is bonded to 1 and Q 2 It is possible to introduce a bridging group structure that forms a ring together with the metal M. By using titanium tetrachloride or hafnium tetrachloride instead of zirconium tetrachloride for the metal M, metallocene compounds in which the metal M is titanium or hafnium, respectively, can be synthesized.

[0076] The metallocene compound of the above formula (2) can be produced by any method known to those skilled in the art.

[0077] 4. [Component (B)] A compound that reacts with components (A-1) and (A-2) to generate a cationic metallocene compound. The olefin polymerization catalyst of the present invention contains, as component (B), in addition to the above-mentioned components (A-1) and (A-2), a compound that reacts with the metallocene compounds of components (A-1) and (A-2) to form a cationic metallocene compound. The compound that reacts with component (A-1) and component (A-2) to form a cationic metallocene compound is not particularly limited and any known compound can be used. Examples of the compound include organoaluminum oxy compounds, borane compounds, and borate compounds.

[0078] When an organoaluminum oxy compound, a borane compound or a borate compound is used as component (B), the polymerization activity and copolymerizability are increased, leading to an improvement in the productivity of olefin polymers.

[0079] Also, a mixture of the organoaluminum oxy compound and the borane compound or borate compound can be used as component (B). Furthermore, the borane compound or borate compound can be used in combination of two or more kinds. Each of these compounds will now be described in more detail.

[0080] (i) Organoaluminum oxy compounds The organoaluminum oxy compound has an Al-O-Al bond in the molecule, and the number of bonds is usually in the range of 1 to 100, preferably 1 to 50. Such an organoaluminum oxy compound is usually a product obtained by reacting an organoaluminum compound with water.

[0081] Among the organoaluminum oxy compounds, those obtained by reacting alkylaluminum with water are usually called aluminoxanes, and can be suitably used as component (B). Among the aluminoxanes, methylaluminoxane (including those essentially consisting of methylaluminoxane (MAO)) is particularly suitable as the organoaluminum oxy compound. In addition, as the organoaluminum oxy-compound, two or more of each organoaluminum oxy-compound may be used in combination, and a solution in which the organoaluminum oxy-compound is dissolved or dispersed in an inert hydrocarbon solvent described below may be used.

[0082] The reaction of organoaluminum with water is usually carried out in an inert hydrocarbon (solvent). As the inert hydrocarbon, aliphatic hydrocarbons, alicyclic hydrocarbons and aromatic hydrocarbons such as pentane, hexane, heptane, cyclohexane, methylcyclohexane, benzene, toluene and xylene can be used, but it is preferable to use aliphatic hydrocarbons or aromatic hydrocarbons.

[0083] As the organoaluminum compound used in the preparation of the organoaluminum oxy-compound, any compound represented by the following general formula (I) can be used, but it is preferable to use a trialkylaluminum. R 40 t AIX 3 3-t (I) (In formula (I), R 40 represents a hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 12 carbon atoms, such as an alkyl group, an alkenyl group, an aryl group, or an aralkyl group; X 3 represents a hydrogen atom or a halogen atom, and t represents an integer of 1≦t≦3.

[0084] Examples of the alkyl group of the trialkylaluminum include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, hexyl, octyl, decyl, and dodecyl groups, among which methyl is particularly preferred. The above organoaluminum compounds can be used alone or in combination of two or more.

[0085] The reaction ratio of water to the organoaluminum compound (water / Al molar ratio) is preferably 0.25 / 1 to 1.2 / 1, particularly preferably 0.5 / 1 to 1 / 1, and the reaction temperature is usually in the range of -70 to 100°C, preferably -20 to 20°C. The reaction time is usually selected in the range of 5 minutes to 24 hours, preferably 10 minutes to 5 hours. As the water required for the reaction, not only simple water but also water of crystallization contained in copper sulfate hydrate, aluminum sulfate hydrate, etc., and components that can generate water in the reaction system can be used.

[0086] (ii) Borane or borate compounds As the component (B), the borane compounds and borate compounds described in paragraphs 0229 to 0242 of JP-A-2012-214780 can be suitably used. Examples of such compounds include triphenylborane, tri(o-tolyl)borane, tri(p-tolyl)borane, tri(m-tolyl)borane, tri(o-fluorophenyl)borane, tris(p-fluorophenyl)borane, tris(m-fluorophenyl)borane, tris(2,5-difluorophenyl)borane, tris(3,5-difluorophenyl)borane, tris(4-trifluoromethylphenyl)borane, tris(3,5-ditrifluoromethylphenyl)borane, tris(2,6-ditrifluoromethylphenyl)borane, tris(pentafluorophenyl)borane, tris(perfluoronaphthyl)borane, tris(perfluorobiphenyl), tris(perfluoroanthryl)borane, tris(perfluorobinaphthyl)borane, and the like; tributylammonium tetra(pentafluorophenyl)borate, tributylammonium tetra(2,6-ditrifluoromethylphenyl)borate, tributylammonium tetra(3,5 -ditrifluoromethylphenyl)borate, tributylammonium tetra(perfluoronaphthyl)borate, dimethylanilinium tetra(pentafluorophenyl)borate, dimethylanilinium tetra(2,6-ditrifluoromethylphenyl)borate, dimethylanilinium tetra(3,5-ditrifluoromethylphenyl)borate, dimethylanilinium tetra(perfluoronaphthyl)borate, etc., trityl tetra(pentafluorophenyl)borate, trityl tetra(2,6-ditrifluoromethylphenyl)borate, trityl tetra(3,5-ditrifluoromethylphenyl)borate, trityl tetra(perfluoronaphthyl)borate, tropinium tetra(pentafluorophenyl)borate, tropinium tetra(2,6-ditrifluoromethylphenyl)borate, tropinium tetra(3,5-ditrifluoromethylphenyl)borate, tropinium tetra(perfluoronaphthyl)borate, NaB(C 6 F 5 ) 4 , NaB(2,6-(CF 3) 2 -Ph) 4 , NaB(3,5-(CF 3 ) 2 -Ph) 4 , NaB(C 10 F 7 ) 4 , HB(C 6 F 5 ) 4 2-Diethyl ether, HB(2,6-(CF 3 ) 2 -Ph) 4 2-Diethyl ether, HB(3,5-(CF 3 ) 2 -Ph) 4 2Diethyl ether, HB(C 10 H 7 ) 4 2-Diethyl ether, etc.

[0087] (3-2) Layered silicate A layered silicate can be used as component (B). The layered silicate can be used as a component that serves both as component (B) and component (C) described below. By using a layered silicate as component (B), the polymerization activity and copolymerizability are increased, as in the case of using an organoaluminum oxy compound, a borane compound, or a borate compound, and thus the productivity of the olefin polymer is improved. A layered silicate is a silicate compound having a crystal structure in which planes formed by ionic bonds or the like are stacked in parallel with each other with weak bonding forces. Most layered silicates are naturally produced as the main component of clay minerals, but these layered silicates are not limited to natural products and may be artificially synthesized products. These techniques for using layered silicates as catalyst components for olefin polymerization are well known in JP-A-5-301917, JP-A-8-127613, JP-A-2003-82018, JP-A-2017-165916, etc. Furthermore, compounds having similar effects and listed in JP-A-2002-515522, etc., can also be suitably used as component (B) in the present invention.

[0088] Examples of layered silicates include known compounds described in "Clay Mineralogy" by Shiramizu Haruo, Asakura Publishing (1995) and the like. Specific examples include kaolin group such as dickite, nacrite, kaolinite, anoxite, metahalloysite, and halloysite; serpentine group such as chrysotile, lisardite, and antigorite; smectite group such as montmorillonite, sauconite, beidellite, nontronite, saponite, taeniolite, hectorite, stevensite, bentonite, and sauconite; vermiculite group such as vermiculite; mica group such as mica, illite, sericite, and glauconite; attapulgite, sepiolite, palygorskite, bentonite, pyrophyllite, talc, and chlorite.

[0089] More preferred layered silicates include smectites, vermiculites, and micas, such as montmorillonite, sauconite, beidellite, nontronite, saponite, hectorite, stevensite, bentonite, and taeniolite. Particularly preferred layered silicates are smectites.

[0090] Generally, natural layered silicates are often non-ion exchangeable (non-swellable), and in such cases, it is preferable to carry out a treatment to impart ion exchangeability (or swelling ability) to the layered silicate in order to give the layered silicate a desired ion exchangeability (or swelling ability). Among such treatments, the following chemical treatments are particularly preferable. Here, the chemical treatment can be either a surface treatment for removing impurities adhering to the surface or a treatment for affecting the crystal structure and chemical composition of the layered silicate. As the chemical treatment method, a known chemical treatment method can be applied, including the method described in JP-A-2003-82018. Specifically, it can be an acid treatment, an alkali treatment, a metal salt treatment, an organic matter treatment, etc., and more preferably, the chemical treatment is an acid treatment or a metal salt treatment, specifically as follows. The acid used in the acid treatment is preferably selected from hydrochloric acid, sulfuric acid, nitric acid, acetic acid, and oxalic acid, and more preferably selected from hydrochloric acid, sulfuric acid, and nitric acid.

[0091] The metal salt used in the metal salt treatment is an inorganic compound containing a cation containing at least one atom selected from the group consisting of Groups 2 to 14 atoms, preferably a compound containing a cation containing at least one atom selected from the group consisting of Groups 2 to 14 atoms and at least one anion selected from the group consisting of halogen atoms, inorganic acids, and organic acids, and more preferably a compound containing a cation containing at least one atom selected from the group consisting of Groups 2 to 14 atoms and at least one anion selected from the group consisting of Cl, Br, I, F, PO 4 , S.O. 4 , NO 3 , CO 3 , C 2 O 4 , ClO 4 , OOCCH 4 , C.H. 3 COCHCOCH 3 , OCl 2 , O(NO 3 ) 2 , O(ClO 4 ) 2 , O(SO 4 ), O.H., O. 2 Cl 2 , OCl 3 , OOCH, OOCH 2 CH 3 , C 2 H 4 O 4 and C 6 H 5 O 7 and at least one anion selected from the group consisting of:

[0092] The proportions of the metallocene compounds of components (A-1) and (A-2) and the layered silicate as component (B) used are not particularly limited, but are preferably in the following ranges: The total amount of components (A-1) and (A-2) supported is 0.0001 to 5 mmol, preferably 0.0005 to 0.5 mmol, more preferably 0.001 to 0.1 mmol, and particularly preferably 0.003 to 0.03 mmol per gram of layered silicate support.

[0093] 5.[Component (C)] The olefin polymerization catalyst of the present invention preferably uses, as an additional component, a particulate support (component (C)) which is an inorganic support, a particulate polymer support, or a mixture thereof. As the inorganic support, a metal, a metal oxide, a metal chloride, a metal carbonate, a carbonaceous material, or a mixture thereof can be used.

[0094] Suitable metals that can be used in the inorganic support include, for example, iron, aluminum, nickel, and the like.

[0095] Examples of metal oxides include single oxides or composite oxides of elements in Groups 1 to 14 of the Periodic Table, such as SiO 2 , Al 2 O 3 , MgO, CaO, B 2 O 3 , TiO 2 , ZrO 2 , Fe 2 O 3 , Al 2 O 3 MgO, Al 2 O 3 CaO, Al 2 O 3 SiO 2 , Al 2 O 3 MgO CaO, Al 2 O 3 MgO SiO 2 , Al 2 O 3 CuO, Al 2 O 3 Fe 2 O 3 , Al 2 O 3 NiO, SiO 2 Examples of the oxides include various natural or synthetic single oxides or composite oxides such as MgO. Here, the above formula is not a molecular formula but represents only the composition, and the structure and component ratio of the composite oxide used in the present invention are not particularly limited. In addition, the metal oxide used in the present invention may absorb a small amount of moisture and may contain a small amount of impurities. As the metal chloride, for example, chlorides of alkali metals and alkaline earth metals are preferable, specifically, MgCl 2 , CaCl 2 As the metal carbonate, a carbonate of an alkali metal or an alkaline earth metal is preferable, and specific examples thereof include magnesium carbonate, calcium carbonate, barium carbonate, and the like. Examples of the carbonaceous material include carbon black and activated carbon.

[0096] Any of the above inorganic carriers can be suitably used in the present invention, with metal oxides, silica, alumina and the like being particularly preferred.

[0097] These inorganic supports are preferably used after being calcined in air or in an inert gas such as nitrogen or argon at 200°C to 800°C, preferably 400°C to 600°C, to adjust the amount of surface hydroxyl groups to 0.8mmol / g to 1.5mmol / g. The properties of these inorganic supports are not particularly limited, but usually have an average particle size of 5μm to 200μm, preferably 10μm to 150μm, an average pore size of 20Å to 1000Å, preferably 50Å to 500Å, and a specific surface area of ​​150m 2 / g~1000m 2 / g, preferably 200m 2 / g~700m 2 / g, pore volume is 0.3 cm 3 / g~2.5cm 3 / g, preferably 0.5 cm 3 / g~2.0cm 3 / g, apparent specific gravity is 0.20g / cm 3 ~0.50g / cm 3 , preferably 0.25 g / cm 3 ~0.45g / cm 3 It is preferable to use an inorganic carrier having the following formula:

[0098] The above-mentioned inorganic carrier can be used as it is, but as a pretreatment, these carriers can be used after contacting with organoaluminum compounds such as trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, tripropylaluminum, tributylaluminum, trioctylaluminum, tridecylaluminum, diisobutylaluminum hydride, or organoaluminum oxy compounds containing Al-O-Al bonds.

[0099] 6. [Component (D)] In the present invention, an organoaluminum compound can be further used as component (D) as necessary. Specific examples of the organoaluminum compound include AlR j X 3-j (In the formula, R is a hydrocarbon group having 1 to 20 carbon atoms, X is a hydrogen atom, a halogen atom, an alkoxy group, and j is a number of 0 < j ≦ 3), such as trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, etc. of trialkylaluminum or halogen or alkoxy-containing alkylaluminum such as diethylaluminum monochloride and diethylaluminum methoxide. In addition, aluminoxanes such as methylaluminoxane can also be used. Among these, trialkylaluminum is particularly preferred. The usage amount of the organoaluminum compound as component (D) is 0.01 to 10,000 millimoles, preferably 0.1 to 100 millimoles, more preferably 0.2 to 20 millimoles, and still more preferably 0.5 to 10 millimoles per 1 g of component (B).

[0100] 7. Method for Producing Olefin Polymerization Catalyst The olefin polymerization catalyst used in the method for producing the olefin polymer of the present invention is produced by containing the above components (A-1) and (A-2), (B), and optionally component (C) and / or (D). The method of contacting each component when obtaining an olefin polymerization catalyst from the above components (A) to (D) of the present invention is not particularly limited. The order of contacting components (A-1), (A-2), (B), (C), and (D) is not particularly limited. For example, the following methods can be arbitrarily adopted. Components (A-1) and (A-2) are contacted, then component (B) is contacted, and then components (C) and / or (D) are contacted. Either component (A-1) or component (A-2) is contacted with component (B), then the remaining component (A-1) and component (A-2) are contacted, and then components (C) and / or (D) are contacted. Either component (A-1) or component (A-2) is contacted with components (C) and / or (D), then the remaining of components (A-1) and (A-2) are contacted, and then component (B) is contacted. After component (B) is contacted with component (C) and / or (D), component (A-1) or component (A-2) is contacted in any order. Contacting a contact product obtained by contacting components (A-1) and (A-2) with components (C) and / or (D) with a contact product obtained by contacting component (B) with components (C) and / or (D).

[0101] In any contact method, a method is adopted in which the components are contacted with or without stirring in an inert atmosphere such as nitrogen or argon, generally in the presence of a liquid inert hydrocarbon such as an aromatic hydrocarbon (usually having 6 to 12 carbon atoms) such as benzene, toluene, xylene, ethylbenzene, etc., or an aliphatic or alicyclic hydrocarbon (usually having 5 to 12 carbon atoms) such as pentane, heptane, hexane, decane, dodecane, cyclohexane, etc. This contact is desirably carried out at a temperature of generally -100°C to 200°C, preferably -50°C to 100°C, more preferably 0°C to 50°C, for 5 minutes to 50 hours, preferably 30 minutes to 24 hours, more preferably 30 minutes to 12 hours.

[0102] In addition, when component (A-1), component (A-2), component (B), and components (C) and / or (D) are brought into contact with each other, as described above, it is possible to use either an aromatic hydrocarbon solvent in which a certain component is soluble or slightly soluble, or an aliphatic or alicyclic hydrocarbon solvent in which a certain component is insoluble or slightly soluble.

[0103] When the contact reaction between each component is carried out stepwise, the solvent used in the previous step may be used as it is as the solvent for the contact reaction in the subsequent step without removing it. After the contact reaction in the previous step using a soluble solvent, a liquid inert hydrocarbon in which some components are insoluble or poorly soluble (e.g., aliphatic hydrocarbons, alicyclic hydrocarbons, or aromatic hydrocarbons such as pentane, hexane, decane, dodecane, cyclohexane, benzene, toluene, and xylene) is added to recover the desired product as a solid, or after removing a part or all of the soluble solvent by drying, filtration, decantation, or the like to recover the desired product as a solid, the contact reaction in the subsequent step of the desired product may be carried out using any of the above-mentioned inert hydrocarbon solvents. In the present invention, the contact reaction of each component may be carried out multiple times.

[0104] In the present invention, the proportions of the components (A-1), (A-2), (B) and (C) used are not particularly limited, but the following ranges are preferred.

[0105] When an organoaluminum oxy compound is used as component (B), it is desirable that the molar ratio (Al / M) of aluminum atoms in the organoaluminum oxy compound to the total of the transition metals (M) in components (A-1) and (A-2), which are the metallocene compounds of the present invention, is usually within the range of 1 to 100,000, preferably 5 to 2000, more preferably 50 to 1000, and particularly preferably 200 to 900. When a borane compound or a borate compound is used as component (B), the molar ratio (B / M) of boron atoms to the total transition metal (M) in components (A-1) and (A-2), which are the metallocene compounds of the present invention, is generally within the range of 0.01 to 100, preferably 0.1 to 50, and more preferably 0.2 to 10. Furthermore, when a mixture of an organoaluminum oxy compound and a borane compound and / or a borate compound is used as component (B), it is desirable to use, for each compound in the mixture, the same ratio of aluminum atoms and boron atoms as described above relative to the total of the transition metal (M) in components (A-1) and (A-2), which are the metallocene compounds of the present invention. When a layered silicate is used as a carrier for component (B), the proportion of the layered silicate used is not particularly limited, but is preferably in the following range: The amount of component (A-1) and component (A-2) supported is 0.0001 to 5 mmol, preferably 0.001 to 0.5 mmol, and more preferably 0.01 to 0.1 mmol per gram of layered silicate.

[0106] The amount of the fine particle carrier, component (C), used is 0.0001 to 5 mmol, preferably 0.001 to 0.5 mmol, and more preferably 0.01 to 0.1 mmol, in terms of the total amount of transition metal (M) in components (A-1) and (A-2), per gram of component (C).

[0107] The olefin polymerization catalyst can be obtained as a solid catalyst by contacting the components (A-1), (A-2), (B), and (C) and / or (D) with each other by appropriately selecting the contact method described above, and then removing the solvent. The solvent is desirably removed at normal pressure or reduced pressure, at 0 to 200°C, preferably 20 to 150°C, and more preferably 20 to 100°C, for 1 minute to 100 hours, preferably 10 minutes to 50 hours, and more preferably 30 minutes to 20 hours.

[0108] The olefin polymerization catalyst can be prepared by contacting component (A-1) or component (A-2) with component (B) to remove the solvent, forming a solid catalyst component, which is then contacted with component (C) and / or (D) under polymerization conditions, or by contacting component (B) with component (C) and / or (D) to remove the solvent, forming a solid catalyst component, which is then contacted with component (A-1) and component (A-2) under polymerization conditions. In these contact methods, the component ratios, contact conditions, and solvent removal conditions can be the same as those described above. The olefin polymerization catalyst thus obtained may be used after preliminary polymerization of monomers, if necessary.

[0109] 8. Method for producing olefin polymer The above-mentioned olefin polymerization catalyst can be used for olefin polymerization, particularly for the homopolymerization of ethylene or the copolymerization of ethylene with an olefin. Here, the ethylene homopolymer refers to a polymer produced by supplying only ethylene to a reactor as a monomer raw material. The ethylene may be at least one of ethylene derived from petroleum raw materials, ethylene derived from biomass raw materials, and ethylene obtained by chemical recycling.

[0110] The olefins as comonomers include those having 3 to 30 carbon atoms, preferably 3 to 8 carbon atoms, and specific examples thereof include propylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene. Two or more kinds of olefins can be copolymerized with ethylene. The copolymerization may be any of alternating copolymerization, random copolymerization, and block copolymerization. When ethylene is copolymerized with another olefin, the amount of the other olefin can be selected arbitrarily within a range of 90 mol % or less of the total monomers, but is generally selected within a range of 40 mol % or less, preferably 30 mol % or less, and more preferably 10 mol % or less. Of course, it is also possible to use a small amount of a comonomer other than ethylene or olefin. In this case, examples of the comonomer include compounds having a polymerizable double bond, such as styrenes such as styrene, 4-methylstyrene, and 4-dimethylaminostyrene; dienes such as 1,4-butadiene, 1,5-hexadiene, 1,4-hexadiene, and 1,7-octadiene; cyclic compounds such as norbornene and cyclopentene; and oxygen-containing compounds such as hexenol, hexenoic acid, and methyl octenoate.

[0111] In the present invention, the polymerization reaction can be carried out in the presence of the above-mentioned supported catalyst, preferably by slurry polymerization or gas phase polymerization. In the case of slurry polymerization, ethylene or the like is polymerized in the presence or absence of an inert hydrocarbon solvent selected from aliphatic hydrocarbons such as isobutane, hexane, heptane, etc., aromatic hydrocarbons such as benzene, toluene, xylene, etc., and alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, etc., in a state where oxygen, water, etc. are substantially cut off. It goes without saying that liquid monomers such as liquid ethylene and liquid propylene can also be used as the solvent. In the case of gas phase polymerization, ethylene or the like is polymerized in a reactor into which a gas stream of ethylene or a comonomer is introduced, circulated, or circulated. In the present invention, the more preferred polymerization is gas phase polymerization.

[0112] [Polymerization temperature] The polymerization temperature of the olefin according to the present invention is from 0 to 250°C, preferably from 20 to 110°C, more preferably from 60 to 100°C, further preferably from 60 to 90°C, and particularly preferably from 60 to 85°C.

[0113] [Ethylene partial pressure] The ethylene partial pressure in the olefin polymerization according to the present invention is preferably 0.1 MPa or more and less than 3 MPa, more preferably 0.3 MPa to 2.5 MPa, still more preferably 0.3 MPa to 1.4 MPa, and particularly preferably 0.5 MPa to 1.4 MPa. If the ethylene partial pressure is lower than 0.1 MPa, the polymerization activity may be low and Mw may become too small, which is undesirable. If the ethylene partial pressure is 3 MPa or more, the weight average molecular weight (Mw) may become too large, the number of terminal vinyl groups may decrease, or an excessive pressure resistance may be required for the polymerization reactor or post-treatment equipment, resulting in poor economic efficiency, which is undesirable.

[0114] [Polymerization time] The polymerization time of the olefin according to the present invention is preferably 0.3 hours or more and less than 30 hours, more preferably 0.6 hours to 12 hours, and further preferably 1 hour to 7 hours. If the polymerization time is shorter than 0.3 hours, the macromonomer yield per catalyst becomes low, which is uneconomical. If the polymerization time is 30 hours or more, the amount of macromonomer produced per volume of the polymerization reactor decreases, which is also uneconomical.

[0115] The molecular weight of the polymer produced can be adjusted to some extent by changing the polymerization conditions such as the polymerization temperature and the molar ratio of the catalyst, but the molecular weight can be adjusted more effectively by adding hydrogen to the polymerization reaction system.

[0116] In addition, the polymerization system can be carried out without any trouble even if a component for removing water, so-called scavenger, is added. As such scavengers, organic aluminum compounds such as trimethylaluminum, triethylaluminum, triisobutylaluminum, the above-mentioned organic aluminum oxy compounds, modified organic aluminum compounds containing branched alkyl, organic zinc compounds such as diethylzinc, dibutylzinc, organic magnesium compounds such as diethylmagnesium, dibutylmagnesium, ethylbutylmagnesium, Grignard compounds such as ethylmagnesium chloride, butylmagnesium chloride, etc. are used. Among these, triethylaluminum, triisobutylaluminum, and ethylbutylmagnesium are preferred, and triethylaluminum is particularly preferred. It can also be applied without any trouble to a multi-stage polymerization method of two or more stages in which polymerization conditions such as hydrogen concentration, monomer amount, polymerization pressure, and polymerization temperature are different from each other.

[0117] 9. Properties of polyolefin polymers An olefin polymer, particularly an ethylene polymer, produced using the olefin polymerization catalyst of the present invention preferably satisfies the following conditions (i) and (ii). Condition (i): The molecular weight distribution (Mw / Mn) based on the weight average molecular weight (Mw) and the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is 3.0 or more and 50.0 or less. Condition (ii): The ratio (HLMFR / MFR) of the melt flow rate at a temperature of 190°C and a load of 21.6 kg (HLMFR) to the melt flow rate at a temperature of 190°C and a load of 2.16 kg (MFR) is greater than 20 and less than 500.

[0118] [Condition (i) Mw / Mn] The ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the olefin polymer obtained by the present invention, as measured by gel permeation chromatography (GPC), is preferably 3.0 or more, more preferably 3.5 or more, even more preferably 4.0 or more, particularly preferably 5.0 or more, and is preferably 50 or less, more preferably 30 or less, even more preferably 20 or less, particularly preferably 17 or less. When Mw / Mn is in the above range, molding processability such as melt tension and melt fluidity is excellent, and further, the balance of mechanical strengths such as rigidity, impact strength, and long-term durability is excellent, which is preferable.

[0119] The smaller the Mw / Mn (i.e., the more monodisperse the particle), the more preferable it is, but theoretically it will never be below 1.0.

[0120] In the present invention, Mw and Mn of the olefin polymer are those measured by gel permeation chromatography (GPC).

[0121] [GPC method measurement] The retention volume is measured by GPC, and the molecular weight is calculated by using a calibration curve prepared in advance using standard polystyrenes. The standard polystyrenes used are all the following brands manufactured by Tosoh Corporation: F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, and A1000. A calibration curve is created by injecting 0.2 mL of a solution of orthodichlorobenzene (ODCB) (containing 0.5 mg / mL BHT (2,6-di-t-butyl-4-methylphenol)) so that each is 0.5 mg / mL. The calibration curve uses a cubic equation obtained by approximation using the least squares method. A general-purpose calibration curve is used for conversion to molecular weight, referring to "Size Exclusion Chromatography" by Mori Sadao (Kyoritsu Shuppan). The viscosity equation used in this case is [η] = K × M α The following values ​​are used: PS:K=1.38×10 -4 , α=0.7 PE:K = 3.92 x 10 -4 , α=0.733 The GPC measurement conditions are as follows: Apparatus: Waters GPC (ALC / GPC 150C) Detector: Polymer Char IR-4 Column: Showa Denko AT-806MS (3 columns) Mobile phase solvent: o-dichlorobenzene (ODCB) Measurement temperature: 140℃ Flow rate: 1.0ml / min Injection amount: 0.3ml Sample preparation: Prepare a 1 mg / mL solution of the sample using ODCB (containing 0.5 mg / mL BHT) and dissolve the sample at 140° C. for approximately 1 hour. Methods for setting the baseline and intervals of the obtained chromatogram are well known to those skilled in the art.

[0122] [Condition (ii): HLMFR / MFR] The olefin polymer obtained by the present invention preferably has a ratio (HLMFR / MFR) of the melt flow rate (HLMFR) at a temperature of 190°C and a load of 21.6 kg to the melt flow rate (MFR) at a temperature of 190°C and a load of 2.16 kg, which is more than 20 and is not more than 500. The lower limit of HLMFR / MFR is more preferably 40 or more, even more preferably 50 or more, and particularly preferably 60 or more. The upper limit is more preferably 300 or less, even more preferably 200 or less, and particularly preferably 170 or less. Furthermore, it is empirically known that, in olefin polymers produced by the same catalyst, the HLMFR / MFR increases as the MFR decreases, and this tendency is particularly noticeable in the region where the MFR is 1 or less, so that the olefin polymer obtained by the present invention may preferably satisfy the following condition (iia). Condition (IIA): When MFR>1, as described above, it is preferable that HLMFR / MFR is more than 20 and 500 or less. If MFR≦1, HLMFR / MFR>-71×LogMFR+20 is satisfied. More preferably, HLMFR / MFR>-71×LogMFR+25 is satisfied. More preferably, HLMFR / MFR>-71×LogMFR+30 is satisfied. The upper limit of HLMFR / MFR is as described above, and MFR is usually from 0.001 to 1000. When the HLMFR / MFR value is within this range, the fluidity during melting becomes suitable for molding.

[0123] In this specification, MFR is a value measured in accordance with JIS K7210:2014 under conditions of 190°C and a load of 2.16 kg, and HLMFR is a value measured in accordance with the same JIS under conditions of a load of 21.6 kg. [Ratio of low molecular weight components] The proportion of low molecular weight components (W) of the olefin polymer obtained by the present invention, which are measured by gel permeation chromatography (GPC), is 10,000 or less. MW≦1万 ) and the proportion of low molecular weight components with a molecular weight of 5000 or less (W MW≦5000 ) is preferably equal to or less than that of an olefin polymer of the same HLMFR obtained using a catalyst consisting only of the metallocene compound (A-1) of the above formula (1), i.e., a catalyst synthesized in the present invention without using the metallocene compound (A-2) of the above formula (2). This is because the metallocene compound (A-2) of the above formula (2) has a structure in which the aromatic rings as ligands are not crosslinked, and is highly efficient in producing polyolefins with narrow molecular weight distributions. Therefore, when a catalyst containing a metallocene compound is used in combination with the metallocene compound (A-1) of the above formula (1), it is possible to prevent the molecular weight distribution from spreading to the low molecular weight side, and to produce polyolefins with a narrow molecular weight distribution. MW≦1万 Or W MW≦5000 This is because W becomes smaller. MW≦1万 and W MW≦5000 It is more preferable that at least one of the above is less than that of an olefin polymer having the same HLMFR obtained using a catalyst containing only the metallocene compound (A-1), and W MW≦1万 and W MW≦5000 It is more preferable that both of the above are less than those of the olefin polymer having the same HLMFR obtained by using only the metallocene compound (A-1) as a catalyst. MW≦1万 and WMW≦5000 However, when the above conditions are satisfied, the olefin polymer obtained by the present invention not only has excellent molding processability, but also has improved surface stickiness and product strength, which is preferable.

[0124] [Number of long chain branches] The olefin polymer obtained by the present invention has a molecular weight of 1 million (g' 100万 ) is detected, and it is preferable that the value of g' is 0.20 or more and less than 1.0. 100万 is preferably 0.25 or more, more preferably 0.30 or more, even more preferably 0.35 or more, particularly preferably 0.40 or more, and is preferably less than 0.99, more preferably less than 0.98, even more preferably 0.95 or less, particularly preferably 0.90 or less, and most preferably 0.88 or less. 100万 When the amount is within the above range, an ethylene-based polymer having excellent moldability can be obtained. Furthermore, the olefin polymer obtained by the present invention has a branching index g' of 1 to 10 million components (g' 100万~1000万 ) is detected, and the value is preferably 0.15 to 0.82 in terms of excellent moldability. 100万~1000万 The lower limit of g' may be 0.20 or more, 0.25 or more, 0.30 or more, 0.35 or more, or 0.40 or more. 100万~1000万 The upper limit of g' may be 0.80 or less, 0.79 or less, 0.77 or less, 0.75 or less, or 0.70 or less. 100万~1000万 When the amount of the ethylene-based polymer is within the above range, an ethylene-based polymer having further excellent moldability is easily obtained, which is preferable. In addition, the olefin polymer obtained by the present invention may have a minimum value (gL) of 0.15 to 0.82 in the molecular weight range of 100,000 to 10,000,000 in the measurement of the branching index g' described above, from the viewpoint of excellent moldability. The lower limit of gL may be 0.20 or more, 0.25 or more, 0.30 or more, 0.35 or more, or 0.40 or more. The upper limit of gL may be 0.80 or less, or 0.75 or less. When the minimum value of the branching index (gL) is within the above range, an ethylene polymer having excellent moldability is easily obtained, which is preferable.

[0125] (i) Branch structure analysis by GPC-VIS The GPC apparatus used was an Alliance GPCV2000 (Waters) equipped with a differential refractometer (RI), a viscosity detector (Viscometer), and a light scattering detector. The light scattering detector used was a DAWN-HELEOS II (Wyatt Technology) multi-angle laser light scattering detector (MALLS). The detectors were connected in the order of MALLS, RI, and Viscometer. The mobile phase solvent was 1,2,4-trichlorobenzene (with the antioxidant Irganox1076 added at a concentration of 0.5 mg / mL). The flow rate was 1 mL / min. Two Tosoh GMHHR-H(S) HT columns were used in combination. The temperature of the column, sample injection section, and each detector was 140°C. The sample concentration was 1 mg / mL. The injection volume (sample loop volume) was 0.2175 mL. The absolute molecular weight (M), the radius of inertia (Rg) obtained from MALLS, and the intrinsic viscosity ([η]) obtained from Viscometer were calculated using the data processing software ASTRA (version 4.73.04) attached to MALLS, with reference to the following literature.

[0126] References: 1.Developments in polymer characterization,vol.4.Essex:Applied Science;1984.Chapter 1. 2.Polymer, 45, 6495-6505 (2004) 3.Macromolecules,33,2424-2436(2000) 4.Macromolecules,33,6945-6952(2000)

[0127] (ii) Calculation of branching index (g') The branching index (g') is calculated as the ratio (ηbranch / ηlin) of the intrinsic viscosity (ηbranch) obtained by measuring a sample with the above-mentioned Viscometer to the intrinsic viscosity (ηlin) obtained by separately measuring a linear polymer. When long chain branches are introduced into a polymer molecule, the radius of gyration becomes smaller compared to linear polymer molecules of the same molecular weight. Since the intrinsic viscosity decreases as the radius of gyration becomes smaller, the ratio (ηbranch / ηlin) of the intrinsic viscosity of the branched polymer (ηbranch) to the intrinsic viscosity of the linear polymer (ηlin) of the same molecular weight becomes smaller as long chain branches are introduced. Therefore, when the branching index (g'=ηbranch / ηlin) is smaller than 1, it means that branches have been introduced, and as the value becomes smaller, it means that the number of long chain branches introduced increases. Here, linear polyethylene Standard Reference Material 1475a (National Institute of Standards & Technology) is used as the linear polymer to be compared. If there are sufficient macromonomers that will become long chain branches, the probability of introducing long chain branches increases as the molecular weight (degree of polymerization) of the polymer increases. On the other hand, whether the main chain growth reaction proceeds to a high molecular weight region while copolymerizing the macromonomers is largely dependent on the ability of the olefin polymerization catalyst. It is believed that the novel olefin polymerization catalyst of the present invention can achieve this. In other words, since it is possible to introduce long chain branches while the main chain grows up to an extremely high molecular weight region with a weight average molecular weight of 1 million or more, the value of g' in this molecular weight region is smaller than the value of g' in a region with a lower molecular weight. In the present invention, branches are introduced into a polymer with a molecular weight of 1 million, that is, g'100万 If the value is less than 1.0, it is determined that sufficient branching is introduced into the high molecular weight region.

[0128] [FR] The olefin polymer obtained by the present invention has a melt flow rate (MFR 10kg It is preferable that FR, which is the ratio of the melt flow rate (MFR) at a temperature of 190°C and a load of 2.16 kg, is 8 or more and 100 or less. When FR is in this range, the fluidity during melting becomes more suitable for molding. The lower limit of FR is more preferably 8.5 or more, even more preferably 9 or more, and particularly preferably 9.5 or more. The upper limit of FR is more preferably 60 or less, even more preferably 50 or less, and particularly preferably 40 or less. When FR is in the above range, an ethylene-based polymer having further excellent molding processability is easily obtained, which is preferable. The measurement conditions of MFR for determining the value of FR are as described above.

[0129] [Condition (iv-1): Number of LCBs] The olefin polymer obtained by the present invention is particularly preferred from the viewpoint of excellent moldability if the number of long chain branches (LCB) per 1000 carbon atoms is 0.02 to 2. The comonomer content and the number of long chain branches (LCB) per 1000 carbon atoms can be measured by the following procedure. [Sample preparation] 200 mg of sample was mixed with o-dichlorobenzene / deuterated bromide benzene (C 6 D 5 The mixture was placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a 100% alcohol (Br) solution (volume ratio) and hexamethyldisiloxane, a chemical shift standard substance, and the tube was replaced with nitrogen, sealed, and dissolved uniformly in a block heater at 130°C. For the NMR measurement, an AV400 NMR apparatus manufactured by Bruker Japan Ltd. equipped with a 10 mmφ cryoprobe can be used. For the quantification of total comonomer and number of long chain branches (LCB) per 1000 carbon atoms, 13 C-NMR is used.13 The measurement conditions for C-NMR are a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 20 seconds, and an accumulation of 512 or more times. The measurement is performed using the proton broadband decoupling method. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shifts of the C signals are based on this. The signal integral intensity in the range from the high magnetic field valley to the low magnetic field valley is defined as I(LCB), and the number of long chain branches per 1000 carbon atoms is calculated by the following formula. Number of long chain branches (number / 1000 carbon atoms) = I(LCB) × 1000 / I(total) Here, I(LCB) and I(total) are quantities expressed by the following formulas. I(LCB)=I 38.2~38.1 I(total)=I 180.0~135.0 +I 120.0~10.0 In both calculations, I is the integrated intensity, and the subscripts of I indicate the range of chemical shifts. For example, I 180.0~135.0 was detected between 180.0 ppm and 135.0 ppm. 13 C The integrated intensity of the signal is shown.

[0130] [Condition (iv-2): W 2 +W 3 ] The olefin polymer obtained by the present invention may further satisfy the following condition (iv-2) from the viewpoint of improving the balance between the strength and rigidity of the product. Condition (iv-2): The ratio of components with molecular weights equal to or greater than the weight average molecular weight among components eluted at or below a temperature at which the elution amount is 50% by weight, as determined from an integrated elution curve measured by cross fractionation chromatography (CFC), is 2 ), and the proportion of components with molecular weights less than the weight average molecular weight (W 3 ) (W 2 +W 3) is greater than 35% by weight and less than 80% by weight. W obtained from an integrated elution curve measured by cross fractionation chromatography (CFC) 1 , W 2 , W 3 and W 4 The value of W is a method used to indicate the "comonomer composition distribution" which is an index of the distribution of the amount of comonomer and the molecular weight of each polymer contained in the entire copolymer, and is well known in International Publication WO2015 / 152267, etc. 1 ), polymers with a high amount of comonomer and a high molecular weight (W 2 ), polymers with low amounts of comonomers and low molecular weights (W 3 ), polymers with low comonomer content and high molecular weight (W 4 ) in the total copolymer. Conventionally, ethylene-α-olefin copolymers obtained by conventional catalytic polymerization have a so-called normal comonomer composition, i.e., W 1 +W 4 accounts for 65% by weight or more. 2 +W 3 In most cases, the W content is 35% by weight or less. However, the preferred ethylene polymer of the present invention has one characteristic that the copolymer obtained has a so-called reverse comonomer composition, i.e., W 2 +W 3 The content of the polymer is more than 35% by weight and less than 80% by weight.

[0131] (W 2 +W 3 ) in this range is preferable in terms of suppressing a decrease in the proportion of a low-density, high-molecular-weight component contained in the ethylene-based polymer that effectively acts to improve impact strength and environmental stress crack resistance (ESCR), suppressing a decrease in the high-density, low-molecular-weight component that effectively acts to improve rigidity, maintaining a balance between the contents of the high-density, low-molecular-weight component and the low-density, high-molecular-weight component contained in the ethylene-based polymer, thereby improving mechanical strength, and suppressing deterioration in dispersibility of the low-density, high-molecular-weight component and the high-density, low-molecular-weight component, thereby improving transparency. (W 2 +W3 The lower limit of (a) is preferably more than 38% by weight, more preferably more than 40% by weight, even more preferably more than 41% by weight, and particularly preferably more than 42% by weight. (W 2 +W 3 ) is preferably less than 80% by weight, more preferably less than 70% by weight, even more preferably less than 65% by weight, and particularly preferably less than 60% by weight.

[0132] [Condition (iv-3): W 2 -W 4 ] From the viewpoint of improving the balance between the strength and rigidity of the product, the ethylene polymer of the present invention may further satisfy the following condition (iv-3): Condition (iv-3): The ratio of components with molecular weights equal to or greater than the weight-average molecular weight among components eluted at or below a temperature at which the elution amount determined from an integrated elution curve measured by cross fractionation chromatography (CFC) is 50% by weight or less (W 2 ) is calculated by dividing the total weight of the components that dissolve at a temperature exceeding the temperature at which the amount of dissolution is 50% by weight, calculated from the integral dissolution curve measured by CFC, by the weight average molecular weight or more (W 4 ) minus the value (W 2 -W 4 ) is greater than -7% by weight and less than 40% by weight. (W 2 -W 4 When the content of the low-density, high-molecular-weight component (HMCO) in the ethylene polymer is within this range, a decrease in the low-density, high-molecular-weight component, which is particularly effective in improving the impact strength and ESCR, is suppressed, and the balance between the contents of the high-density, low-molecular-weight component and the low-density, high-molecular-weight component is maintained, which is preferable in terms of the improvement of the impact strength and ESCR, and the suppression of deterioration in the dispersibility of the low-density, high-molecular-weight component and the high-density, low-molecular-weight component, which is preferable in terms of transparency. (W 2 -W 4 The lower limit of ) is preferably greater than -3% by weight, more preferably greater than -1% by weight, and even more preferably greater than 0% by weight. (W 2 -W 4) is preferably less than 30% by weight, more preferably less than 20% by weight, even more preferably less than 16% by weight, and particularly preferably less than 14% by weight.

[0133] [CFC measurement] Cross fractionation chromatography (CFC) consists of a temperature rising elution fractionation (TREF) section for crystallographic fractionation and a gel permeation chromatography (GPC) section for molecular weight fractionation. Analysis using this CFC is performed as follows. First, a polymer sample is completely dissolved at 140°C in ODCB containing 0.5 mg / mL BHT, and then this solution is injected into a TREF column (a column filled with inert glass bead carrier) held at 140°C through the sample loop of the device, and gradually cooled to a predetermined first elution temperature to crystallize the polymer sample. After holding at a predetermined temperature for 30 minutes, ODCB is passed through the TREF column, and the eluted components are injected into the GPC section for molecular weight fractionation, and a chromatogram is obtained using an infrared detector (FOXBORO MIRAN·1A·IR detector, measurement wavelength 3.42 μm). During this time, the temperature is raised to the next elution temperature in the TREF section, and after a chromatogram of the first elution temperature is obtained, the eluted components at the second elution temperature are injected into the GPC section. By repeating the same procedure thereafter, chromatograms of the eluted components at each elution temperature can be obtained.

[0134] The CFC measurement conditions are as follows: GPC column: Showa Denko AD-806MS (3 columns connected in series) Solvent:ODCB Sample concentration: 3mg / mL Injection volume: 0.4mL Crystallization rate: 1℃ / min Solvent flow rate: 1mL / min GPC measurement time: 34 minutes Stabilization time after GPC measurement: 5 minutes Elution temperature (℃):0,5,10,15,20,25,30,35,40,45,49,52,55,58,61,64,67,70,73,76,79,82,85,88,91,94,97,100,102,120,140

[0135] (Data Analysis) From the chromatograms of the eluted components at each elution temperature obtained by the measurement, the elution amount (proportional to the area of ​​the chromatogram) normalized so that the sum is 100% is obtained. Furthermore, an integral elution curve for the elution temperature is calculated as shown in Figure 3. This integral elution curve is differentiated with respect to temperature to obtain a differential elution curve. Furthermore, from each chromatogram, the molecular weight distribution is obtained by the following procedure. The conversion from the retention volume to the molecular weight is performed using a calibration curve prepared in advance using standard polystyrene. The standard polystyrenes used are all the following brands manufactured by Tosoh Corporation: F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000. A calibration curve is created by injecting 0.4 mL of a solution of each of the 0.5 mg / mL ODCB (containing 0.5 mg / mL BHT). The calibration curve is a cubic equation obtained by approximating the curve using the least squares method. For conversion to molecular weight, a general calibration curve is used based on "Size Exclusion Chromatography" by Sadao Mori (Kyoritsu Shuppan). The viscosity formula used is [η] = K × M α The following values ​​are used: PS:K=1.38×10 -4 , α=0.7 PE:K = 3.92 x 10 -4 , α=0.733 In the chromatogram at the first elution temperature, the peak due to the BHT added to the solvent may overlap with the low molecular weight side of the eluted components. In such a case, a baseline is drawn as shown in Figure 4 to determine the interval for determining the molecular weight distribution. Furthermore, as shown in the table of FIG. 5, the whole weight average molecular weight is calculated from the elution ratio at each elution temperature (weight % (wt%) in the table) and the weight average molecular weight (Mw in the table).

[0136] In addition, from the molecular weight distribution and elution amount at each elution temperature, a graph (contour diagram) showing the elution amount relative to the elution temperature and molecular weight as contour lines is obtained according to the method described in the literature (S. Nakano, Y. Goto, Development of automatic Cross Fractionation: Combination of Crystallizability Fractionation and Molecular Weight Fractionation, J. Appl. Polym. Sci., vol. 26, pp. 4217-4231 (1981)). Using the above contour diagram, the amounts of the following components are calculated. W 1 : The ratio of components with molecular weights less than the weight average molecular weight among those that dissolve at or below the temperature at which the amount dissolved is 50% by weight, as determined from the integral dissolution curve W 2 : The ratio of components with molecular weights equal to or greater than the weight average molecular weight among those that dissolve at or below the temperature at which the amount dissolved is 50% by weight, as determined from the integral dissolution curve W 3 : The ratio of components with molecular weights less than the weight average molecular weight that dissolve at temperatures higher than the temperature at which the amount dissolved is 50% by weight, as determined from the integral dissolution curve W 4 : The ratio of components with molecular weights equal to or greater than the weight average molecular weight that dissolve at temperatures higher than the temperature at which the amount dissolved is 50% by weight, as determined from the integral dissolution curve In addition, W 1 +W 2 +W 3 +W 4 =100. If the logarithm of molecular weight (logM) is plotted on the horizontal axis and the elution temperature (Temp) on the vertical axis, W 1 ~W 4 is divided into four quadrants as shown in the schematic diagram 9. (W 2 +W 3 ) and (W 2 -W 4 ) satisfies the above conditions, W 2 Since the value of becomes relatively large, the contour plot in Fig. 6 tends to show an elliptical shape.

[0137] The olefin polymer produced by the production method of the present invention can be isolated from the polymerization reactor and used for various applications as a product in the form of granules, pellets, lumps, sheets, strands, melt, slurry, solution, etc. It is also possible to copolymerize the olefin polymer with other monomers including ethylene and olefins in a second or subsequent polymerization reactor of a multistage polymerization apparatus connected to the polymerization reactor for producing an olefin polymer. In this case, it is preferable because various polyolefin resins having useful long chain branching structures can be produced. EXAMPLES

[0138] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The evaluations and resins used in the examples and comparative examples are as follows. The following catalyst synthesis step and polymerization step were all carried out under a purified nitrogen atmosphere, and the solvents used were dehydrated and purified using molecular sieves 4A, 13X, or the like.

[0139] 1. Various evaluation (measurement) methods (1)MFR: The measurements were performed in accordance with JIS K6760 at 190°C and a load of 2.16 kg. MFR 5kg was similarly measured under conditions of 190°C and a load of 5.0 kg. The HLMFR was similarly measured under conditions of 190°C and a load of 21.6 kg.

[0140] (2) Measurement of molecular weight Mw and molecular weight distribution (Mw / Mn): Measurement was performed according to the method described in the above condition (i).

[0141] Example 1 (1) Synthesis of component (A-1) Dimethylsilylene(3-methyl-4-(2-(5-methyl)-furyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride (metallocene compound 11) shown in the following chemical formula was synthesized according to the following method. [ka]

[0142] (1-1) Synthesis of 1-methyl-7-(2-(5-methyl)-furyl)-indene (1-1-a) Synthesis of 2-bromophenyl-2-chloroethyl ketone 2-Bromobenzoic acid (5.30 g, 26.4 mmol) and 25 ml of thionyl chloride were added to a 100 ml flask and refluxed for 2 hours. After the reaction, excess thionyl chloride was distilled off under reduced pressure, and the resulting acid chloride (5.50 g) was used in the next reaction without purification. The acid chloride (5.00g, 22.7mmol) and 50ml of dichloromethane were added to a 100ml flask to form a solution, and then aluminum chloride (3.02g, 22.7mmol) was added and ethylene was blown in at 20°C for 4 hours. The reaction was quenched with 4N hydrochloric acid, and the organic and aqueous phases were separated. The aqueous phase was washed three times with 50ml of methyl-t-butyl ether, and the organic phase was collected and washed three times with 50ml of water, 100ml of saturated sodium bicarbonate water, and then 100ml of saturated saline. After drying with sodium sulfate, the solvent was distilled off under reduced pressure to obtain 4.80g of compound 3 (85% yield). This was used in the next reaction without further purification.

[0143] (1-1-b) Synthesis of 7-bromo-1-indanone Aluminum chloride (7.40g, 55.6mmol) and sodium chloride (2.15g, 37.1mmol) were added to a 100ml flask and heated to 130℃, after which 2-bromophenyl-2-chloroethyl ketone (4.60g, 18.5mmol) was slowly added and the mixture was stirred at 160℃ for 1 hour. After the reaction, it was cooled to 30℃ and quenched with ice water. After adjusting the pH to 5 with concentrated hydrochloric acid, the organic and aqueous phases were separated, the aqueous phase was washed three times with 100ml of dichloromethane, the organic phase was collected, washed with 100ml of water and 100ml of saturated saline, dried with sodium sulfate, and the solvent was distilled off under reduced pressure to obtain a crude product. It was further purified with a silica gel column (petroleum ether / ethyl acetate=30 / 1) to obtain 1.60g of 7-bromo-1-indanone (yield 33%).

[0144] (1-1-c) Synthesis of 7-(2-(5-methyl)-furyl)-1-indanone 2-Methylfuran (0.933g, 11.4mmol) and 10ml of THF were added to a 100ml flask to form a solution, then n-butyllithium / hexane solution (2.5M, 4.70ml, 11.4mmol) was added at -30℃ and stirred at room temperature for 2 hours. Zinc chloride (1.55g, 11.4mmol) and 10ml of THF were added to a separate 100ml flask, followed by the above reaction solution at 0℃ and stirring at room temperature for 1 hour. Furthermore, copper(I) iodide (90mg, 0.473mmol), Pd(dppf)Cl were added to a separate 100ml flask. 2 The above reaction mixture was added to a suspension of 7-bromo-1-indanone (177 mg, 0.236 mmol), 7-bromo-1-indanone (2.00 g, 9.45 mmol) and 10 ml of DMA, and refluxed for 15 hours. The mixture was cooled to room temperature, 50 ml of water was added, and extraction was performed twice with 50 ml of ethyl acetate. The organic phase was collected, washed twice with 50 ml of water and 50 ml of saturated saline, dried over sodium sulfate, and the solvent was distilled off under reduced pressure to obtain a crude product. The product was further purified using a silica gel column (petroleum ether / ethyl acetate = 20 / 1) to obtain 0.70 g of 7-(2-(5-methyl)-furyl)-1-indanone (yield 35%).

[0145] (1-1-d) Synthesis of 1-methyl-7-(2-(5-methyl)-furyl)-indene 7-(2-(5-methyl)-furyl)-1-indanone (1.40 g, 6.59 mmol) and 20 ml of THF were added to a 100 ml flask to form a solution, and then methyllithium / diethyl ether solution (1.6 M, 7.5 ml, 11.9 mmol) was added at -78°C and stirred at room temperature for 10 hours. The reaction was quenched with 20 ml of saturated aqueous ammonium chloride solution, and the volatile components were removed under reduced pressure. The remaining solution was extracted twice with 50 ml of ethyl acetate, and the organic phase was collected and washed with 50 ml of saturated saline, dried over sodium sulfate, and the solvent was removed under reduced pressure to obtain a crude product. The product was used in the next reaction without further purification. The crude product and 30 ml of toluene were added to a 100 ml flask to form a solution, and then p-toluenesulfonic acid (62.0 mg, 0.330 mmol) was added and stirred at 130°C for 2 hours. During stirring, the water generated was removed using a Dean-Stark trap. The mixture was cooled to room temperature, and 30 ml of saturated aqueous sodium bicarbonate was added to separate the organic phase. The aqueous phase was extracted three times with 50 ml of ethyl acetate, and the organic phase was collected, washed with 50 ml of saturated saline, dried with sodium sulfate, and the solvent was distilled off under reduced pressure to obtain a crude product. The product was further purified using a silica gel column (petroleum ether) to obtain 0.850 g of 1-methyl-7-(2-(5-methyl)-furyl)-indene (yield 61%).

[0146] (1-2) Synthesis of (2,3,4,5-tetramethylcyclopentadienyl)dimethylchlorosilane In a 200 ml flask, 2.40 g (19.6 mmol) of tetramethylcyclopentadiene and 40 ml of THF were added to form a solution, which was then cooled to -78°C and 12.0 ml (30.0 mmol) of n-butyllithium / hexane solution (2.5 M) was added, and the mixture was returned to room temperature and stirred for 3 hours. In a separate 200 ml flask, 5.00 g (38.7 mmol) of dimethyldichlorosilane and 20 ml of THF were added, cooled to -78°C, and the reaction solution was added. The mixture was returned to room temperature and stirred for 12 hours. Volatiles were removed by distillation under reduced pressure to obtain 4.00 g of a yellow liquid. The yellow liquid obtained was used in the next reaction without further purification.

[0147] (1-3) Synthesis of (3-methyl-4-(2-(5-methyl)-furyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)dimethylsilane In a 100 ml flask, 2.60 g (12.4 mmol) of 1-methyl-7-(2-(5-methyl)-furyl)-indene and 40 ml of THF were added to form a solution, which was then cooled to -78°C and 5.2 ml (13.0 mmol) of n-butyllithium / hexane solution (2.5 M) was added, and the mixture was returned to room temperature and stirred for 3 hours. In a separate 200 ml flask, 3.40 g (15.8 mmol) of the unpurified yellow liquid obtained in (1-2) and 10 ml of THF were added, cooled to -78°C, and the previous reaction solution was added. The mixture was returned to room temperature and stirred for 12 hours. The reaction product was slowly added to 40 ml of ice water and extracted twice with 200 ml of ethyl acetate. The obtained organic phase was washed with 50 ml of saturated saline and dried over anhydrous sodium sulfate. The sodium sulfate was filtered, the solution was evaporated under reduced pressure, and the residue was purified with a silica gel column (petroleum ether) to obtain 1.40 g (25% yield) of yellow oil of (3-methyl-4-(2-(5-methyl)-furyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)dimethylsilane.

[0148] (1-4) Synthesis of dimethylsilylene(3-methyl-4-(2-(5-methyl)-furyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride In a 200 ml flask, 2.20 g (5.70 mmol) of (3-methyl-4-(2-(5-methyl)-furyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)dimethylsilane and 30 ml of diethyl ether were added and cooled to -78°C. 4.8 ml (11.9 mmol) of n-butyllithium / n-hexane solution (2.5 M) was added dropwise thereto, and the mixture was returned to room temperature and stirred for 3 hours. The solvent of the reaction solution was distilled off under reduced pressure, 60 ml of dichloromethane was added, and the mixture was cooled to -78°C. 1.40 g (6.01 mmol) of zirconium tetrachloride was added thereto, and the mixture was stirred overnight while gradually returning to room temperature. The reaction solution was filtered, and the solvent was distilled off under reduced pressure from the filtrate obtained, to obtain 3.0 g of a yellow powder. This powder was washed with 25 ml of toluene to obtain 0.75 g (yield 26%) of a yellow powder of dimethylsilylene(3-methyl-4-(2-(5-methyl)-furyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride. 1 H-NMR values ​​(CDCl 3 ):δ0.94(s,3H),δ1.19(s,3H),δ1.90(s,3H),δ1.95(s,3H),δ1.98(s,3H),δ2.04(s,3H),δ2.28(s,3H) ,δ2.38(s,3H),δ5.52(s,1H),δ6.07(d,1H),δ6.38(d,1H),δ7.04(dd,1H),δ7.37(d,1H),δ7.45(d,1H).

[0149] (2) Synthesis of component (A-1) (2) Metallocene compound 12 shown in the following chemical formula was synthesized according to the method described in paragraphs 0140 to 0143 of JP2013-227271A. [ka]

[0150] (3) Synthesis of component (A-1) (3) Metallocene compound 13 shown in the following chemical formula was synthesized according to the method described in paragraphs 0135 to 0139 of JP2017-165726A. [ka]

[0151] (4) Synthesis of component (A-2) (1) Metallocene compound 21 shown in the following chemical formula was obtained from Fujifilm Wako Pure Chemical Industries, Ltd. [ka]

[0152] (5) Synthesis of component (A-2) (2) The metallocene compound 22 shown in the chemical formula below was obtained from Alpha Chemistry (USA) through a Japanese distributor. [ka]

[0153] (6) Synthesis of olefin polymerization catalysts In a nitrogen atmosphere, 10.0 g of silica calcined at 480 ° C for 6 hours was placed in a 500 ml two-neck flask, and dried under reduced pressure for 1 hour with a vacuum pump while heating in an oil bath at 150 ° C. In a separately prepared 200 ml two-neck flask, 27.4 mg of the above metallocene compound 11 (equivalent to 50 μmol of metallocene compound) and 20.2 mg of the above metallocene compound 21 (equivalent to 50 μmol of metallocene compound) were placed at room temperature under a nitrogen atmosphere, and dissolved in 27.4 ml of toluene. At room temperature, 26.7 ml of a toluene solution (20%) of methylaluminoxane manufactured by Albemarle was added to the toluene solution of metallocene compound 11 and metallocene compound 21, and stirred for 30 minutes. A 500 ml two-neck flask containing vacuum-dried silica and 65 ml of dehydrated toluene was heated and stirred in an oil bath at 40 ° C., and the entire amount of the toluene solution in which the above metallocene compound and methylaluminoxane (MAO) were mixed was added. After stirring at 40°C for 1 hour, the mixture was washed three times with hexane while still heated at 40°C, and the solvent was then distilled off under reduced pressure to obtain an olefin polymerization catalyst.

[0154] (7) Production of ethylene polymers Into a 2-liter stainless steel autoclave equipped with stirring and temperature control, 800 ml of thoroughly dehydrated and deoxygenated isobutane, 30 ml of 1-hexene, and 34 mg of triethylaluminum were introduced, and the temperature was raised to 85°C with stirring. After introducing a small amount of hydrogen, ethylene was introduced until the partial pressure reached 0.7 MPa. The slurry of the olefin polymerization catalyst obtained in (6) above was injected with nitrogen gas, and polymerization was continued for 60 minutes while maintaining the ethylene partial pressure at 0.7 MPa and the temperature at 85°C. The average molar ratio of hydrogen to ethylene (H2 / C2) during polymerization was 0.17 mol%. As a result, 68 g of ethylene polymer was produced. The MFR of the obtained polymer was 0.51 g / 10 min and the density was 0.922 g / cm. 3 The results are summarized in Tables 14 and 15.

[0155] (Examples 2 to 11) Ethylene polymers were produced in the same manner as in Example 1, except that the metallocene compounds were changed to the kinds and ratios shown in Table 14. The polymerization conditions and results are summarized in Table 15.

[0156] (Comparative Examples 1 to 9) As shown in Table 14, ethylene polymers were produced in the same manner as in Example 1, except that the metallocene compound used was limited to either (A-1) or (A-2) (Comparative Examples 1 to 9).

[0157] [Table 14]

[0158] The copolymers obtained in the above Examples and Comparative Examples were analyzed by GPC measurement and MFR measurement. The results are summarized in Table 15 together with the polymerization conditions.

[0159] [Table 15]

[0160] As shown in Table 15, the polyolefins obtained using a catalyst containing two types of metallocene compounds in combination had a large HLMFR / MFR value and molecular weight distribution, and had flowability suitable for melt molding. On the other hand, the molecular weight distribution of (A-2) alone was not large enough (Comparative Examples 3 to 6), and was insufficient to exhibit properties suitable for melt molding.

[0161] For the polyolefins obtained in each Example and Comparative Example, the HLMFR is plotted on the horizontal axis, and the ratio of low molecular weight components in the polyethylene (W MW≦1万 , W MW≦5000 The results are shown in Figs. 1 and 2, which are plotted on a two-dimensional coordinate space with the vertical axis representing the ratio of low molecular weight components (W MW≦1万 , W MW≦5000 In the figure, the HLMFR-W of the catalysts of Comparative Examples 1 and 2 is connected by a line, but the catalysts (Examples 1-5, 6-9) in which the same metallocene (A-1) is dualized with metallocene (A-2) are plotted below the line, indicating that they have less W than the comparative examples. Examples 10 and 11 also have smaller W than Comparative Examples 7 and 9, which are catalysts containing only the same metallocene (A-1). From this, it is expected that the polyolefin obtained using the catalyst of the Example will not only have excellent molding processability, but also have improved product surface stickiness and product strength.

[0162] [Examples 12 to 14] Except for changing the metallocene compounds to the types and ratios shown in the table, ethylene polymers were produced in the same manner as in Example 1. The polymerization conditions and results are summarized in Tables 14 and 15.

[0163] As shown in Tables 14 and 15, in Examples 12 to 14, using a catalyst using two types of metallocene compounds of the present invention in combination, ethylene polymers having lower HLMFR and higher density than the ethylene polymers produced in Examples 1 to 11 were produced. The HLMFR / MFR values ​​were large, and the polymers had flowability suitable for melt molding. Furthermore, the low molecular weight component amount ratio W was smaller than the HLMFR-W lines of the catalysts of Comparative Examples 1 and 2, and the product surface was excellent in terms of stickiness and product strength. This shows that the catalyst of the present invention exerts its effects over a wide range of HLMFR and density.

[0164] <Cross fractionation chromatography (CFC)> The polyethylenes of Examples 1, 2, and 3 and Comparative Examples 1 and 2 were subjected to cross-fractionation chromatography measurement according to the above-mentioned method to analyze the distribution of the comonomer. As actual examples, the integral elution curves and differential elution curves versus elution temperature for Example 1 and Comparative Example 1 are shown in FIG. 3, and a contour plot of the elution amount with the elution temperature and molecular weight (logM) on the axis is shown in FIG. 6. In addition, the polymer is divided into four regions W according to the relationship between the amount of comonomer and the molecular weight. 1 ~W 4 The amount of polymer contained therein was calculated and the results are shown in Table 16. The values ​​in the table are in weight percent.

[0165] [Table 16]

[0166] The polyolefins obtained using the catalysts of Examples 1 to 9 have a wide molecular weight distribution and (W 2 +W 3 ) and (W 2 -W 4 ) show large values, indicating that the copolymer has an inverse comonomer composition structure, which is expected to improve the balance between product strength and rigidity. In the polyolefin obtained using the catalyst of Example 10, the ratio of the low-density, high-molecular-weight polymer component derived from the metallocene compound 12 is not sufficiently large due to the large difference in activity between the metallocene compound 12 and the metallocene compound 21, so the spread of the molecular weight distribution is small, and (W2 +W 3 ) and (W 2 -W 4 Although the inverse comonomer composition structure was not evident enough to be reflected in the value of ), the CFC contour map (Figure 8) clearly showed the presence of low-density polymer components, demonstrating that the comonomer composition distribution structure of the resulting polyolefin can be controlled by adjusting the complex mixture ratio of the binary complex catalyst.

Claims

1. An olefin polymerization catalyst comprising the following components (A-1), (A-2) and (B): Component (A-1): A metallocene compound represented by the following formula (1): [Formula 1] [In formula (1), M 1 represents a transition metal atom of Ti, Zr, or Hf; X 1 and X 2 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, an amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, Q 1 and Q 2 represents a carbon atom, a silicon atom, or a germanium atom, R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and adjacent substituents bond to each other with Q 1 and Q. 2 may be bonded to form a ring, m is 0 or 1, and when m is 0, Q 1 is R 9 directly bonded to a conjugated five-membered ring containing R 5 ~R 14 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing hydrocarbon group having 1 to 18 carbon atoms and including 1 to 6 silicon atoms, a halogen-containing hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 40 carbon atoms containing an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, a hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms or a hydrocarbon group-substituted amino group having 1 to 40 carbon atoms; R 5 ~R 8 adjacent substituents may be bonded together through the carbon atoms to which they are bonded to form an aliphatic ring, R 10 ~R 14 adjacent substituents may be bonded to each other to form a ring, including the carbon atoms to which they are bonded; n is 0 or 1, and when n is 0, R 10 and R 11 There is no carbon atom to which R is bonded. 12 and the conjugated five-membered ring are directly bonded to form an indenyl ring. Component (A-2): A metallocene compound represented by the following general formula (2): [Case 2] [In formula (2), M 2 represents a transition metal atom of Ti, Zr, or Hf; X 21 and X 22 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom or a nitrogen atom, an amino group substituted with a hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, R 51 ~R 60 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing hydrocarbon group having 1 to 18 carbon atoms and including 1 to 6 silicon atoms, a halogen-containing hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 40 carbon atoms which contains an oxygen atom, a sulfur atom, a nitrogen atom or a phosphorus atom, a hydrocarbon group-substituted silyl group having 1 to 40 carbon atoms or a hydrocarbon group-substituted amino group having 1 to 40 carbon atoms, R 51 ~R 60 Among these, any one or more pairs of adjacent groups on the same cyclopentadienyl ring may be bonded to each other via the bonding carbon atom to form a ring. Component (B): A compound that reacts with the metallocene compounds of components (A-1) and (A-2) to produce a cationic metallocene compound.

2. 2. The olefin polymerization catalyst according to claim 1, wherein n is 0 in the formula (1) of the component (A-1).

3. 2. The olefin polymerization catalyst according to claim 1, wherein m is 0 in the formula (1) of the component (A-1).

4. In the formula (1) of the component (A-1), R 9 2. The olefin polymerization catalyst according to claim 1, wherein is a hydrogen atom.

5. In the formula (1) of the component (A-1), R 9 2. The olefin polymerization catalyst according to claim 1, wherein: is a hydrocarbon group having 1 to 20 carbon atoms.

6. In the formula (1) of the component (A-1), R 5 ~R 14 The olefin polymerization catalyst according to claim 1, characterized in that at least one of the above is represented by the following formula (5): [C3] [In formula (5), A 1 represents an atom of Group 14, 15, or 16 of the Periodic Table, R 17 ~R 21 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms containing an oxygen atom, a sulfur atom or a nitrogen atom, a hydrocarbon group-substituted amino group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms, and adjacent substituents may be bonded to each other through the atoms bonded thereto to form a ring, p 1 is 0 or 1, A 1 When is an atom of group 15 or 16 of the periodic table, p 1 is 0, and A 1 Substituent R 17 does not exist, q 1 is 0 or 1, and q 1 If is 0, R 20 does not exist, and R 19and the carbon atom to which R 21 is directly bonded to the carbon atom to which it is attached.

7. In the formula (1) of the component (A-1), R 5 ~R 14 The olefin polymerization catalyst according to claim 1, characterized in that at least one of the above is represented by the following formula (6): [C4] [In formula (6), Z 1 represents an oxygen atom or a sulfur atom, R 22 ~R 24 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen atom, a sulfur atom, or a nitrogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, a silicon atom-containing hydrocarbon group having 1 to 18 carbon atoms and containing 1 to 6 silicon atoms, a halogen atom-containing hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group-substituted silyl group having 1 to 20 carbon atoms; R 22 ~R 24 adjacent substituents may be bonded to each other through the carbon atoms to which they are bonded to form a ring.

8. In the formula (1) of the component (A-1), R 12 The olefin polymerization catalyst according to claim 6, characterized in that it is represented by the formula (5).

9. In the formula (1) of the component (A-1), R 12 The olefin polymerization catalyst according to claim 7, characterized in that it is represented by the formula (6).

10. In the formula (2) of the component (A-2), R 51 ~R 60 2. The olefin polymerization catalyst according to claim 1, wherein at least one of the above is a hydrocarbon group having 1 to 20 carbon atoms.

11. In the formula (2) of the component (A-2), R 51 ~R 602. The olefin polymerization catalyst according to claim 1, wherein at least two of the above are hydrocarbon groups having 1 to 20 carbon atoms.

12. In the formula (2) of the component (A-2), R 51 ~R 60 2. The olefin polymerization catalyst according to claim 1, wherein at least four of the above are hydrocarbon groups having 1 to 20 carbon atoms.

13. In the formula (2) of the component (A-2), R 51 ~R 55 At least one of and R 56 ~R 60 and at least one of the above is a hydrocarbon group having 1 to 20 carbon atoms.

14. In the formula (2) of the component (A-2), R 51 ~R 55 At least two of the above and R 56 ~R 60 2. The olefin polymerization catalyst according to claim 1, wherein at least two of said first and second radicals are each a hydrocarbon group having 1 to 20 carbon atoms.

15. The olefin polymerization catalyst according to claim 1, further comprising the following component (C): Component (C): Microparticle Carrier

16. The olefin polymerization catalyst according to claim 15, further comprising the following component (D): Component (D): Organoaluminum Compound

17. A method for producing an olefin polymer, comprising polymerizing or copolymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of claims 1 to 16.

18. 18. The method for producing an olefin polymer according to claim 17, wherein the olefin is ethylene.

19. 18. The process for producing an olefin polymer according to claim 17, wherein the polymer obtained satisfies the following conditions (i) and (ii): Condition (i): The molecular weight distribution (Mw / Mn) based on the weight average molecular weight (Mw) and the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is 3.0 or more and 50.0 or less. Condition (ii): The ratio (HLMFR / MFR) of the melt flow rate at a temperature of 190° C. and a load of 21.6 kg (HLMFR) to the melt flow rate at a temperature of 190° C. and a load of 2.16 kg (MFR) is greater than 20 and is 500 or less.

Citation Information

Patent Citations

  • Ethylenic copolymer and production thereof

    JP1990276807A

  • Production of ethylene polymer composition

    JP1991234717A

  • Catalyst for olefin polymerization and method of producing olefin polymer

    JP2010043152A

  • Catalytic ingredient for olefin polymerization, catalyst for olefin polymerization containing the ingredient, production method of olefin-based polymer using the catalyst, and olefin-based polymer produced by the method

    JP2012214780A

  • Catalyst for olefin polymerization and method for producing ethylenic polymer using the same