Resin compositions for three-dimensional printers and modeled products thereof

A copolymer of ethylene and α-olefin addresses resin shrinkage and safety issues in 3D printing by providing low melting point and flexibility, enabling safe and versatile 3D printing with reduced temperature requirements.

JP2024149439APending Publication Date: 2024-10-18JAPAN POLYETHYLENE CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024060917
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2024-04-04
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

3D printing using material extrusion methods faces challenges with dimensional changes due to resin shrinkage during cooling, limited resin selection due to amorphous thermoplastic use, and safety concerns from high melting point resins requiring high temperatures.

Method used

A copolymer of ethylene and α-olefin with 3 to 12 carbon atoms is developed, with controlled crystallinity and low melting point, offering flexibility and reduced shrinkage, allowing safe and flexible 3D printing at lower temperatures.

Benefits of technology

The copolymer enables 3D printing with minimal shrinkage, flexibility, and safety, expanding resin selection and reducing the need for high temperatures, enhancing the versatility and safety of 3D printing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149439000002
    Figure 2024149439000002
  • Figure 2024149439000003
    Figure 2024149439000003
  • Figure 2024149439000004
    Figure 2024149439000004
Patent Text Reader

Abstract

To provide resins for three-dimensional printers that have flexibility in the low melting point region.SOLUTION: A resin composition for a three-dimensional printer, comprising a copolymer (P) of ethylene and α-olefin having a carbon number of 3 to 12, and optionally a thermoplastic resin that does not correspond to the copolymer (P), the copolymer (P) comprises 50 mass% or more of the total resin composition, and the copolymer (P) has (A-i) having a melt flow rate (190°C, 21.18 N load) of 0.1 to 200 g / 10 min, and (A-ii) having a density of 0.865 to 0.930 g / cm3.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for 3D printers and a molded article made using the same. [Background technology]

[0002] 3D printing is a technology that manufactures three-dimensional objects based on three-dimensional model data created by a computer. Unlike molding with a metal mold or cutting, 3D printing does not require molds or cutting tools, can respond immediately to frequent design changes, and can create hollow shapes and complex internal shapes. For these reasons, 3D printing technology is rapidly spreading in a wide range of fields.

[0003] In 3D printing, the cross-sectional shape of three-dimensional model data is generally layered to form a shape, and various layering methods are collectively called additive manufacturing. The basic principle of modeling is to harden a resin with fluidity. In particular, a method called material extrusion is easy to use because it does not require any additional equipment. The material extrusion method is a method of creating a three-dimensional shape by melting thermoplastic resin that has been processed into pellets or filaments and layering it while extruding it. Engineering plastics such as ABS resin and polycarbonate can also be used, and it is possible to manufacture objects that are in line with the characteristics of each engineering plastic. Since the operability of modeling with a 3D printer changes depending on the physical properties of the resin, attempts have been made to blend various resins as resins for 3D printers (Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2020-503186 [Patent Document 2] Special Publication No. 2020-500112 [Patent Document 3] Special Publication No. 2021-532005 Summary of the Invention [Problem to be solved by the invention]

[0005] Although 3D printing technology using material extrusion has many advantages, its use can be difficult depending on the physical properties of the resin. For example, unlike modeling in which the material is cut to a fixed dimension, 3D printing using material extrusion involves a cooling process after the molten resin is extruded. If the dimensions change due to shrinkage during cooling, it may not be possible to model the desired shape. For this reason, amorphous thermoplastic resins are mainly used in the molten resin extrusion method, and the resin options are limited. In particular, polyolefins have the advantages of being inexpensive and having excellent mechanical properties, but they have been considered unsuitable for 3D printing because they are crystalline resins and therefore shrink. On the other hand, in order to popularize 3D printing technology, it is also necessary to consider the safety of the method itself. In the process of melting the resin material, 3D printing is equipped with a heating unit for melting the resin, and it is also necessary to heat the area around the outlet from which the molten resin is discharged. In order to melt the resin, it is necessary to heat it to a temperature above the melting point of the resin, and from the viewpoint of safety, it is required to perform 3D printing at the lowest possible temperature. Since the resin described in Patent Document 3 often uses a resin with a relatively high melting point, it is necessary to set the heating unit to a high temperature, and there was a need for improvement from the viewpoint of safety. Furthermore, since the molded product itself has flexibility, the risk of cuts and the like can be reduced when handling the molded product. Thus, there is a demand for resins used in 3D printers that have little shrinkage during the cooling process, a low melting point, and flexibility. The present application aims to provide such a resin for 3D printers. [Means for solving the problem]

[0006] The present inventors have found that by using a copolymer having a uniform molecular structure of ethylene and an α-olefin having 3 to 12 carbon atoms, the above problems can be solved, even though a resin mainly composed of polyolefin is used. In the polymerization of polymers, the structure of the polymer chain may differ depending on the polymerization method. The inventors have found that by appropriately setting the polymerization conditions, including the selection of a catalyst, and controlling the crystallinity of the copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms, even though the main component is a crystalline resin called polyolefin, shrinkage does not occur in the cooling process after extrusion of the molten resin in 3D printing. In addition, compared to the thermoplastic resins used in 3D printing so far, it is possible to mold at low temperatures and it is flexible, so it has advantages from the viewpoint of safety, and this has led to the present invention.

[0007] That is, the present invention relates to the following items. [1] A resin composition for 3D printers, comprising a copolymer (P) of ethylene and an α-olefin having 3 to 12 carbon atoms, and optionally a thermoplastic resin other than the copolymer (P), wherein the amount of the copolymer (P) is 50 mass% or more based on the entire resin composition, and the copolymer (P) has the following characteristics (Ai) to (A-ii). (Ai) Melt flow rate (190°C, 21.18N load) is 0.1 to 300g / 10min. (A-ii) Density is 0.865 to 0.950 g / cm 3 is [2] The resin composition for 3D printers according to [1] above, characterized in that the melting point of the copolymer (P) is 130°C or lower. [3] The resin composition for 3D printers according to [1] or [2], characterized in that the melting point of the copolymer (P) is 30°C or higher. [4] The resin composition for 3D printers according to any one of [1] to [3] above, characterized in that the copolymer (P) has a flexural modulus of 1800 MPa or less. [5] The resin composition for 3D printers according to any one of [1] to [4] above, wherein the copolymer (P) has a crystallinity of 50% or less. [6] A 3D printed product formed by depositing one or more lines using any one of the 3D printer resin compositions [1] to [5] above by fused filament deposition. [7] A method for producing a 3D printed product, comprising the step of depositing any one of the resin compositions for 3D printers according to [1] to [5] in a plurality of layers using a 3D printer to form a 3D printed product. Effect of the Invention

[0008] According to the present invention, a resin composition for 3D printers that can be molded at a low melting point and is flexible, and a molded product using the same are provided by using a copolymer of a specific ethylene and an α-olefin having 3 to 12 carbon atoms as the main component. The resin composition of the present invention is a polyethylene-based soft polymer that is highly flexible compared to ordinary polyethylene and is characterized by a low crystallinity. Compared to thermoplastic resin compositions used in 3D printing so far, it can be molded at a low temperature and has flexibility, so it has an advantage from the viewpoint of safety and can be used in a wide range of applications. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is an image of the molecular structure of a hyperbranched olefin copolymer polymerized by a high-pressure radical polymerization process. [Diagram 2] FIG. 1 is an image of the molecular structure of a linear olefin copolymer containing many short side chains polymerized by a gas phase polymerization process. [Diagram 3] FIG. 1 is an image of the molecular structure of a linear olefin copolymer polymerized using a metal catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention relates to a resin composition for 3D printers, which contains a copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms, and optionally a thermoplastic resin other than said copolymer, and in which the amount of said copolymer is 50% by mass or more based on the total amount of the resin composition, and to a molded article using said resin. The resin composition used in the present invention has the function of imparting good transparency, flexibility, and strength to the molded article.

[0011] The resins constituting the present invention will be described in detail below for each item. In this specification, the numerical range "to" is used to mean that the numerical range includes the numerical range before and after the "to" as the lower and upper limits. In this specification, the copolymer means a binary or higher copolymer containing at least one type of unit (A) and at least one type of unit (B).

[0012] (1) Copolymer of ethylene and α-olefin having 3 to 12 carbon atoms (P) The copolymer (P) used in the present invention is a random copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms, the main component of which is a structural unit derived from ethylene. As the ethylene, ethylene derived from a petroleum raw material or ethylene derived from a non-petroleum raw material such as a plant raw material can be used. Examples of plant-derived ethylene and polyethylene include ethylene and its polymers described in JP-T-2010-511634. Plant-derived ethylene and its polymers have the property of being carbon neutral (does not use fossil raw materials and does not lead to an increase in carbon dioxide in the atmosphere), and it is possible to provide environmentally friendly products. Specific examples of α-olefins used as comonomers include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-heptene, 4-methyl-pentene-1, 4-methyl-hexene-1, 4,4-dimethylpentene-1, and the like. Specific examples of the resin include ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-4-methyl-pentene-1 copolymer, etc. The α-olefin may be one type or a combination of two or more types. When two types of α-olefins are combined to form a terpolymer, examples include ethylene-propylene-hexacenter polymer, ethylene-butene-hexacenter polymer, ethylene-propylene-octene terpolymer, and ethylene-butene-octene terpolymer.

[0013] The content of the α-olefin in the copolymer (P) is preferably 5 to 40% by mass, more preferably 7 to 35% by mass, and particularly preferably 8 to 30% by mass, from the viewpoint of appropriately lowering the crystallinity of the copolymer (P). The content of the α-olefin is preferably 5 to 40% by mass, more preferably 7 to 35% by mass, and particularly preferably 8 to 30% by mass, in accordance with the following conditions: 13 This is a value measured by the C-NMR method. Equipment: JEOL-GSX270 manufactured by JEOL Concentration: 300mg / 2mL Solvent: ortho-dichlorobenzene

[0014] The copolymer (P) used in the present invention can be polymerized by a slurry method in the presence of a catalyst, a gas-phase fluidized bed method (for example, the method described in JP-A-59-23011), a solution method, or a polymerization method under a pressure of 200 kg / cm 2 As described above, means and conditions known to those skilled in the art can be used as a method for obtaining a copolymer with the following properties of the resin, particularly the density, within the specified range, such as high-pressure bulk polymerization or high-pressure ionic polymerization at a polymerization temperature of 100° C. or higher. As a catalyst used in the polymerization reaction of the copolymer (P), the catalysts described in JP 2014-180326 A and the catalysts described in the documents cited therein can be used.

[0015] (2) Resin characteristics (Ai) Melt Flow Rate (MFR) The MFR (190 ° C., 21.18 N load) of the copolymer (P) used in the present invention is 0.1 to 300 g / 10 minutes, preferably 0.3 to 200 g / 10 minutes, more preferably 0.5 to 110 g / 10 minutes, more preferably 1.0 to 80 g / 10 minutes, and even more preferably 1.5 to 50 g / 10 minutes. If the MFR is less than 0.1 g / 10 minutes, the resin has poor fluidity, making it difficult for the resin to come out of the nozzle, resulting in poor moldability. On the other hand, if it exceeds 300 g / 10 minutes, the fluidity is too high during 3D printing, making it difficult to maintain the shape, resulting in poor moldability. The MFR is a value measured in accordance with JIS-K6922-2:2018 Appendix (190°C, 21.18N load).

[0016] (A-ii) Density The density of the copolymer (P) used in the present invention is 0.865 to 0.950 g / cm 3 , preferably 0.870 to 0.940 g / cm 3 , and more preferably 0.880 to 0.933 g / cm 3 and more preferably 0.890 to 0.930 g / cm 3 The density is 0.865g / cm 3 If it is less than 0.950g / cm, the stiffness is insufficient. 3 If it exceeds this value, the flexibility decreases, which is undesirable. The density is a value measured in accordance with JIS-K6922-2:1997 Appendix (for low-density polyethylene) (23°C).

[0017] (A-iii) Mw / Mn The copolymer (P) according to the present invention preferably satisfies the following requirements in addition to the above (Ai) and (A-ii). The molecular weight distribution parameter (Mw / Mn) of the copolymer (P) according to the present invention is preferably 1.0 to 15.0, more preferably 1.5 to 9.0, even more preferably 2.0 to 7.0, and particularly preferably 2.3 to 6.5. If the molecular weight distribution is below 1.0, the fluidity may be poor, and the moldability may be insufficient, and if the molecular weight distribution is above 15.0, the impact resistance and creep resistance may be poor. The weight average molecular weight (Mw) and the number average molecular weight (Mn) are determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) is calculated by further determining the number average molecular weight (Mn) by gel permeation chromatography (GPC) and calculating the ratio of Mw to Mn, Mw / Mn.

[0018] An example of the GPC measurement method according to the present invention is as follows. (Measurement conditions) Machine used: Waters 150C Detector: FOXBORO MIRAN1A IR detector (measurement wavelength: 3.42 μm) Measurement temperature: 140℃ Solvent: orthodichlorobenzene (ODCB) Column: RESONAC AD806M / S (3 columns) Flow rate: 1.0mL / min Injection volume: 0.2mL (Sample preparation) A 1 mg / mL solution of the sample is prepared using ODCB (containing 0.5 mg / mL BHT (2,6-di-t-butyl-4-methylphenol)), and dissolved at 140° C. for about 1 hour. (Calculation of molecular weight (M)) The standard polystyrene method is used, and the conversion from retention volume to molecular weight is performed using a calibration curve of standard polystyrene that has been prepared in advance. The standard polystyrene used is, for example, Tosoh's (F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000) brand, and RESONAC's monodisperse polystyrene (S-7300, S-3900, S-1950, S-1460, S-1010, S-565, S-152, S-66.0, S-28.5, S-5.05, each 0.07 mg / ml solution), etc. A calibration curve is prepared by injecting 0.2 mL of a solution in which each is dissolved in ODCB (containing 0.5 mg / mL BHT) so that the concentration is 0.5 mg / mL. The calibration curve is a cubic equation obtained by approximating the least squares method, or a quartic equation obtained by approximating the logarithm of the elution time and molecular weight. The viscosity equation used to convert to molecular weight (M) is [η] = K × Mα, and the following values ​​are used. Polystyrene (PS): K = 1.38 x 10-4, α = 0.7 Polyethylene (PE): K = 3.92 × 10-4, α = 0.733 Polypropylene (PP): K = 1.03 × 10-4, α = 0.78

[0019] (A-iv) Melting point (Tm, °C): The melting point of the copolymer is indicated by the maximum peak temperature of the endothermic curve measured by a differential scanning calorimeter (DSC). The maximum peak temperature refers to the temperature of the peak with the maximum height from the baseline when multiple peaks are shown in the endothermic curve obtained in the DSC measurement when the heat flow (mW) is plotted on the vertical axis and the temperature (°C) is plotted on the horizontal axis, and refers to the temperature of the peak when there is only one peak. In the present invention, the melting point can be determined, for example, from the absorption curve when using a DSC (DSC7020) manufactured by SII Nano Technology Co., Ltd., packing about 5.0 mg of a sample into an aluminum pan, heating it to 200°C at 10°C / min, holding it isothermally at 200°C for 5 minutes, lowering it to 20°C at 10°C / min, holding it isothermally at 20°C for 5 minutes, and then heating it again to 200°C at 10°C / min. The melting point of the copolymer (P) is preferably 130° C. or lower, since molding at a low temperature is possible, which is sufficient from the viewpoint of safety, and since the low-temperature moldability is superior.

[0020] Low-temperature moldability In the copolymer (P) according to the present invention, in order to improve low-temperature moldability, the melting point is preferably 130° C. or less, more preferably 120° C. or less, and even more preferably 110° C. or less. The melting point is preferably 30° C. or more, more preferably 40° C. or more, and even more preferably 50° C. or more. If the melting point is lower than this range, the heat resistance is insufficient, and if it is higher than this range, the molding temperature becomes too high and molding at a low temperature becomes impossible, which is insufficient from the viewpoint of safety.

[0021] (Av) Crystallinity (%): In the copolymer (P) of the present invention, the crystallinity observed by differential scanning calorimetry (DSC) is not particularly limited, but is preferably 50% or less. More preferably 40% or less, and even more preferably 30% or less. If the crystallinity is greater than 50%, the crystallinity may affect the dimensional stability during molding. In addition, the lower limit of the crystallinity of the copolymer is preferably more than 0%, more preferably more than 5%, and even more preferably 7% or more. If the crystallinity is 0%, the rigidity of the copolymer may not be sufficient. In the present invention, the crystallinity can be determined, for example, by determining the heat of fusion (ΔH) from the area of ​​the melting endothermic peak obtained by DSC measurement using the same procedure as in the measurement of the melting point, and dividing the heat of fusion by the heat of fusion of 293 J / g of perfect crystals of high density polyethylene (HDPE).

[0022] Flexural modulus In the copolymer (P) of the present invention, the flexural modulus measured in accordance with the JIS K6922-2:2018 Appendix is ​​preferably 1800 MPa or less. More preferably, it is 1500 MPa or less, even more preferably, it is 1300 MPa or less, more preferably, it is 1000 MPa or less, more preferably, it is 800 MPa or less, and even more preferably, it is 600 MPa or less. The lower limit of the flexural modulus is not particularly limited, but it is preferably 1 MPa or more. When the flexural modulus is within this range, it is preferable because it has flexibility and can be used for a wide range of applications from the viewpoint of safety.

[0023] ·Moldability In the present invention, the moldability refers to the degree of shrinkage of the resin that causes warping during the cooling process after extruding the molten resin in 3D printing by the material extrusion method. If warping occurs due to shrinkage of the resin, the moldability cannot be formed as designed. The degree of shrinkage can be expressed as the shrinkage rate measured in accordance with JIS K 7152-4:2006. The shrinkage rate measured in accordance with JIS K 7152-4:2006 is preferably 2.2% or less. It is preferably 2.0% or less, more preferably 1.8% or less, more preferably 1.6% or less, and even more preferably 0% or more and 1.4% or less. Since the resin of the present invention is a resin composition for 3D printers containing a copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms as the main component, the shrinkage rate will not be less than 0%. If the shrinkage rate is within this range, the change in dimensions that occurs during cooling is small, so that a molded product as designed can be formed, which is preferable.

[0024] (3) Resin composition for 3D printers One aspect of the present invention is a resin composition for 3D printers containing the copolymer (P). As a resin for 3D printers, one type of the copolymer (P) may be used alone, or two or more types of copolymers (P) may be mixed and used. When the resin composition for 3D printers contains the copolymer (P) of the present invention, a resin having the properties required for 3D printer applications, such as no shrinkage or deformation, is provided. Furthermore, the resin has excellent flexibility, moldability, and low-temperature moldability, and can form molded products having flexibility and low-temperature moldability that could not be achieved with existing thermoplastic resins for 3D printer applications.

[0025] The copolymer (P) can be optionally mixed with a suitable known thermoplastic resin to be used as a resin composition for 3D printers. Crystalline resins may be added as long as low crystallinity suitable for 3D printer applications can be ensured. Examples of resins that can be mixed with the copolymer (P) include polyester, polyamide, polyimide, polyurethane, polyethylene, polyolefin, terephthalic acid derivative resins such as polyethylene terephthalate and polybutylene terephthalate, polystyrene, polyacetal, polyacrylate or ethylene-(meth)acrylate copolymers, modified ethylene-(meth)acrylate copolymers, halogenated polymers such as chlorinated polyethylene and polyvinyl chloride, and ionomers. In addition, ethylene-α-olefin copolymers that do not satisfy at least one of the characteristics (Ai) to (A-ii) can also be mixed and used.

[0026] The blending ratio of the copolymer (P) in the resin composition is 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more when the entire resin composition is taken as 100 parts by mass, and may be 100% by mass, i.e., a resin for 3D printers consisting of the copolymer (P). By using 50% by mass or more of the copolymer (P), a molded product having the flexibility, moldability, and low-temperature moldability inherent to the copolymer can be formed.

[0027] Additives The resin composition for 3D printers according to the present invention may contain additives that are commonly used in resins for 3D printers, such as conventionally known antioxidants, ultraviolet absorbers, lubricants, antistatic agents, colorants, pigments, crosslinking agents, foaming agents, nucleating agents, flame retardants, conductive materials, and fillers, within the scope of the present invention. The use of these additives is appropriately selected according to the purpose of the modeling.

[0028] The resin composition for 3D printers according to the present invention can be obtained by kneading the copolymer (P) and, if necessary, other resins or additives by known means. The kneaded resin can be used in the form of pellets, but may also be processed into filaments.

[0029] ·filament The filament of the resin composition for a 3D printer can be formed by any method known in the art. For example, pellets of the resin composition containing the copolymer (P) are fed to an extruder, extruded through a die in a molten state at a temperature higher than the melting peak temperature of the copolymer, and then cooled to form a filament of a desired diameter. The filament can be obtained as a filament of any diameter depending on the diameter of the extrusion die.

[0030] Filaments useful in the process for 3D printing include filaments comprising the copolymer (P) described herein, wound onto a coil or reel for feeding into the nozzle of a 3D printer. A cartridge containing the wound filament is then attached to the 3D printer for use.

[0031] Process for making filaments The filaments, strands or fibers described herein for use in the fusion manufacturing process can be formed by any method known in the art. For example, pellets containing a copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms are fed into an extruder, where the temperature in the extruder is at least 10° C. above the melting peak temperature of the copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms. The molten polymer composition is extruded through a die and subsequently cooled to form filaments, strands or fibers of the desired diameter. While filaments of any diameter can be prepared, useful diameters are typically in the range of 1.3 to 3.0 mm. Preferably, the filament diameter is in the range of about 1.50 mm to 2.00 mm.

[0032] The filament may further contain optional additives to the copolymer (P) of ethylene and an α-olefin having 3 to 12 carbon atoms, such as a plasticizer, a stabilizer, an antioxidant, an ultraviolet absorber, a hydrolysis stabilizer, an antioxidant, a dye or pigment, a filler, a flame retardant, a lubricant, a processing aid, an anti-blocking agent, a release agent, and / or a mixture thereof, without departing from the spirit of the present invention.

[0033] The resin composition containing the copolymer (P) of the present invention can be used to produce an article by a melt resin extrusion method. This allows an article containing a resin containing the copolymer (P) of the present invention to be molded using a 3D printing technique. A method for producing a molded article by 3D printing includes a step of depositing a 3D printer resin composition containing the copolymer (P) in multiple layers using a 3D printer to form an article.

[0034] In the molten resin extrusion method, which is one of the 3D printing methods, modeling can be performed by fused filament deposition. In this method, a filament containing the copolymer (P) is supplied through a nozzle heated to a sufficient temperature. The heating temperature is sufficient to melt the filament as long as it is a temperature equal to or higher than the melting point of the copolymer (P). By including the copolymer (P), the heating temperature can be kept relatively low. The molten filament is discharged from the nozzle and deposited in a multi-layer shape to form a desired model. The deposition rate can be controlled by changing the filament feed rate, cross-sectional dimensions, and the movement speed of the nozzle and / or the model. Thus, one aspect of the present invention relates to a 3D printed model in which a 3D printer resin composition containing the copolymer (P) is modeled by deposition of one or more lines by fused filament deposition. EXAMPLES

[0035] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The evaluation methods and resins used in the examples and comparative examples are as follows.

[0036] 1. Evaluation method for resin properties (1) Density: As described above, the density of the copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms was measured in accordance with JIS-K6922-2:2018 Appendix (23°C, in the case of low-density polyethylene).

[0037] (2) Mw / Mn: 1) Measurement of weight average molecular weight (Mw) and molecular weight distribution parameter (Mw / Mn) The weight average molecular weight (Mw) was determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) was calculated by determining the number average molecular weight (Mn) by gel permeation chromatography (GPC) and then calculating the ratio of Mw to Mn, Mw / Mn. The measurements were performed according to the following procedures and conditions. 2) Preparation of sample solution 3 mg of sample and 3 mL of o-dichlorobenzene were weighed into a 4 mL vial, and the vial was capped with a screw cap and a Teflon (registered trademark) septum, and then shaken for 2 hours at 150°C using a Senshu Scientific SSC-7300 high-temperature shaker. After shaking, it was visually confirmed that there were no insoluble components. 3) Measurement A Waters Alliance GPCV2000 was connected to one RESONAC high-temperature GPC column, Showdex HT-G, and two HT-806M columns, and measurements were performed using o-dichlorobenzene as the eluent at a temperature of 145°C and a flow rate of 1.0 mL / min. 4) Calibration curve The column was calibrated using monodisperse polystyrene (S-7300, S-3900, S-1950, S-1460, S-1010, S-565, S-152, S-66.0, S-28.5, S-5.05, each 0.07mg / ml solution) manufactured by RESONAC, n-eicosane and n-tetracontane were measured under the same conditions as above, and the elution time and the logarithm of the molecular weight were approximated by a fourth-order equation. The following equation was used to convert the molecular weight of polystyrene (MPS) to the molecular weight of polyethylene (MPE). MPE = 0.468 × MPS

[0038] (3) Melting point and crystallinity: As mentioned above, the measurements were carried out by DSC.

[0039] (4)Melt flow rate (MFR): As described above, the MFR of the copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms was measured in accordance with JIS-K6922-2:2018 (190°C, 21.18 N load).

[0040] (5)Flexural modulus: In accordance with JIS K 6922-1:2018, the specimen was placed in a 4.0 mm thick heat press mold and preheated for 8 minutes in a heat press machine with a surface temperature of 180°C. Residual gas in the molten resin was degassed by repeatedly applying and depressurizing pressure, and then the specimen was pressurized to 4.9 MPa and held for 5 minutes. The specimen was then transferred to a press machine with a surface temperature of 25°C and cooled by holding the specimen at a pressure of 4.9 MPa for 5 minutes to produce a pressed plate of a specimen with a thickness of approximately 4.0 mm. The pressed plate was cut to 4 x 10 x 80 mm to produce a test specimen, which was measured in accordance with the JIS K6922-2:2018 Appendix.

[0041] (6) Shrinkage rate: In accordance with JIS K 7152-4:2006, a 120 x 120 x 2 mm flat plate with a film gate (gate thickness 0.2 mm) on one side was molded using a FANUC ROBOSHOT 2000i-100B injection molding machine at a molding temperature of 190°C and a mold temperature of 40°C, and the machine direction (MD) was measured immediately after molding. The shrinkage rate was calculated by dividing the measured value by the length of the mold.

[0042] [Preparation of test pieces] Standard number: JIS-7152 (ISO294-1) Molding machine: FANUC ROBOSHOT 2000i-100B injection molding machine Molding machine temperature settings: 30, 180, 190, 190, 190℃ from the bottom of the hopper Mold temperature: 40℃ Injection speed: 50mm / sec (speed inside the mold cavity) Holding pressure: 30MPa Pressure retention time: 10 seconds Mold shape: Flat plate (thickness 2mm, width 120mm, length 120mm)

[0043] (7) Formability: Using the method described below, filaments were produced from pellet-shaped resin of the copolymer of the following Examples and Comparative Examples, and then 3D printing objects were produced from the produced filaments.

[0044] <How to make filament> Method for making filaments: Filaments containing copolymers of ethylene and α-olefins with 3-12 carbon atoms were made by feeding copolymer pellets of ethylene and α-olefins with 3-12 carbon atoms into a 65 mm single screw extruder. Depending on the particular copolymer of ethylene and α-olefins with 3-12 carbon atoms used, the barrel temperature was set to the optimum temperature for each resin, ranging from 70 to 240 °C. As the molten resin emerged from the die, it was quenched in a water bath at a quenching temperature of around 20 °C. The quenched filaments were wound on a reel at controlled speeds, and filaments with a diameter of 1.75 mm were made by adjusting the pulling speed of 21 m / min.

[0045] <How to create 3D printing objects> In the examples described herein, the 3D printer used was a Raise3D Pro2 Plus equipped with a standard direct drive extruder and a 0.5 mm nozzle, using a nominal 1.75 mm filament, and the following conditions were used for printing: Model used: Raise3D Pro2 Plus Nozzle temperature: 190℃ Layer pitch: 0.2mm Printing speed: 20mm / s

[0046] The obtained molded product was observed, and the moldability was evaluated according to the following criteria. 〇: There is almost no warping and the shape can be beautifully shaped. ×: The shrinkage is large and the model cannot be formed neatly.

[0047] 2. Examples and Comparative Examples Example 1: Linear low density polyethylene Nippon Polyethylene Kernel KJ640T (MFR: 30g / 10min, density: 0.88 g / cm 3 The evaluation results of the copolymer (Mw / Mn=2.6) are shown in Table 1.

[0048] Example 2: Linear low density polyethylene Nippon Polyethylene Kernel KS240T (MFR: 2.2g / 10min, density: 0.88 g / cm3 The evaluation results of the copolymer (Mw / Mn=2.8) are shown in Table 1.

[0049] Example 3: Linear low density polyethylene Nippon Polyethylene Kernel KF360T (MFR: 3.5g / 10min, density: 0.898g / cm 3 The evaluation results of the copolymer (Mw / Mn=3.1) are shown in Table 1.

[0050] Example 4: Linear low density polyethylene Nippon Polyethylene Kernel KS560T (MFR: 17g / 10min, density: 0.898g / cm 3 The evaluation results of the copolymer (Mw / Mn=2.7) are shown in Table 1.

[0051] Example 5: Linear low density polyethylene Japan Polyethylene Kernel KC581 (MFR: 10g / 10min, density: 0.919 g / cm 3 The evaluation results of the copolymer (Mw / Mn=6.0) are shown in Table 1.

[0052] Example 6: Linear low density polyethylene Japanese Polyethylene Kernel KC577T (MFR: 14g / 10min, density: 0.911g / cm 3 The evaluation results of the copolymer (Mw / Mn=5.8) are shown in Table 1.

[0053] Example 7: Low Density Polyethylene Novatec LJ902 made by Nippon Polyethylene (MFR: 45g / 10min, density: 0.915g / cm 3 The evaluation results of the copolymer (Mw / Mn=5.8) are shown in Table 1.

[0054] Example 8: Low Density Polyethylene Novatec LJ920 made by Nippon Polyethylene (MFR: 58g / 10min, density: 0.923g / cm 3 The evaluation results of the copolymer (Mw / Mn=6.7) are shown in Table 1.

[0055] Example 9: Low Density Polyethylene Novatec UJ890 made by Nippon Polyethylene (MFR: 110g / 10min, density: 0.931g / cm 3 The evaluation results of the copolymer (Mw / Mn=4.3) are shown in Table 1.

[0056] Example 10: Low density polyethylene Novatec UJ960 made by Nippon Polyethylene (MFR: 5.0g / 10min, density: 0.935g / cm 3 The evaluation results of the copolymer (Mw / Mn=4.4) are shown in Table 1.

[0057] Comparative Example 1: High-density polyethylene Novatec HE421 manufactured by Japan Polyethylene Corporation (MFR: 0.14 g / 10 min, density: 0.956 g / cm 3 The evaluation results of the copolymer (Mw / Mn=34) are shown in Table 1.

[0058] [Table 1]

[0059] <Results of consideration of Examples and Comparative Examples> In Examples 1 to 6, 9, and 10, since ethylene and an α-olefin are polymerized, the amorphous portion is increased, and the change in volume between melting and cooling is small, so the shrinkage is small. In Examples 7 to 8, the molecular structure is highly branched and the molecules are highly entangled. As a result, the change in volume between melting and cooling is small, and the shrinkage is small. On the other hand, in Comparative Example 1, the density is high and the structure is linear with few short chain branches, and since rearrangement and crystallization easily occur during cooling, the change in volume between melting and cooling is large, and the shrinkage is large. In addition, the copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms that does not have a linear molecular structure or is copolymerized with an α-olefin has a low melting point, and safety during molding and processing is ensured.

Claims

1. A resin composition for 3D printers, comprising a copolymer (P) of ethylene and an α-olefin having 3 to 12 carbon atoms, and optionally a thermoplastic resin other than the copolymer (P), wherein the amount of the copolymer (P) is 50 mass% or more based on the entire resin composition, and the copolymer (P) has the following characteristics (A-i) to (A-ii): (Ai) Melt flow rate (190°C, 21.18N load) is 0.1 to 300g / 10min. (A-ii) density is 0.865 to 0.950 g / cm 3 is

2. The resin composition for 3D printers according to claim 1, wherein the melting point of the copolymer (P) is 130°C or lower.

3. The resin composition for 3D printers according to claim 1, characterized in that the melting point of the copolymer (P) is 30°C or higher.

4. The resin composition for 3D printers according to claim 1, wherein the copolymer (P) has a flexural modulus of 1800 MPa or less.

5. The resin composition for 3D printers according to claim 1, wherein the degree of crystallinity of the copolymer (P) is 50% or less.

6. A 3D printed product formed by deposition of one or more lines by fused filament deposition using the resin composition for 3D printers according to any one of claims 1 to 5.

7. A method for producing a 3D printed object, comprising the step of depositing the resin composition for a 3D printer according to any one of claims 1 to 5 in a plurality of layers using a 3D printer to form a shaped object.

Citation Information

Patent Citations

  • Ionomer-containing filaments and their use in the manufacture of fused filaments

    JP2020500112A

  • Filament composition for producing fused filaments and method of use thereof

    JP2020503186A

  • Fused filament sculpting manufacturing method and polymer blends used therein

    JP2021532005A