Film for cell pouch with minimized deformation of laminate and manufacturing method thereof
The 1P3C process addresses the issue of deformation in pouch-type battery manufacturing by minimizing winding tension and improving curl properties through a single in-line coating and laminating method, enhancing the tensile strength and moldability of the cell pouch film.
Patent Information
- Application Number
- JP2024061605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional manufacturing processes for pouch-type batteries result in high deformation of the metal layer due to repeated winding and coating steps, leading to increased running losses and process defects, which affect the tensile strength and curl properties of the cell pouch film.
A single in-line process (1P3C) is employed, where coating and laminating steps are performed in a single run, and a resin film with a lower elastic modulus than the metal layer is laminated to minimize winding tension, ensuring the barrier layer is not wound alone, thereby reducing mechanical deformation and improving curl properties.
The improved manufacturing process minimizes mechanical deformation and enhances tensile strength and moldability, resulting in better curl characteristics before and after molding, reducing the likelihood of process inefficiencies and defects.
Smart Images

Figure 2024149468000001_ABST
Abstract
Description
[Technical field]
[0001] The present specification relates to a film for a cell pouch that minimizes deformation of a laminate, and a method for producing the same. [National research and development project that supported this invention] [Project unique number]1415185612 [Subject number] 20022450 [Department name] Ministry of Trade, Industry and Energy [Name of issue management (specialized) organization] Korea Institute for Industrial Technology Evaluation and Management [Research Project Name] Material Parts Package Type (Top Company) [Research title] Development of next-generation secondary battery pouches capable of achieving more than twice the adhesive strength (60℃) [Contribution rate] 1 / 1 [Name of project execution organization] Kurimura Chemical Co., Ltd. [Research period] 2023.01.01~2023.12.31 [Background technology]
[0002] Pouch-type batteries, which are generally used in electric vehicles, have the advantage of being easier to deform and having a higher energy density than cylindrical or prismatic batteries. Such cell pouches are generally manufactured by carrying out the following steps in order: a first step of performing a surface treatment on one side of a metal layer, a second step of performing a surface treatment on the other side of the metal layer, a third step of laminating an outer layer on one side, and a fourth step of laminating a sealant layer on the other side. After each step, coating, drying, winding, and other processes are repeated in sequence. However, in this case, there is an increased probability of running loss and process defects occurring when feeding the raw material, and improvements are required. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Republic of Korea Patent Publication No. 10-2016-0070468 [Patent Document 2] Republic of Korea Patent Publication No. 10-2022-0031820 Summary of the Invention [Problem to be solved by the invention]
[0004] In one aspect, an exemplary embodiment of the present invention provides a film for a cell pouch and a manufacturing method thereof, which can minimize the winding tension applied to the metal layer and the film for the cell pouch by improving the manufacturing process, thereby minimizing mechanical deformation of the metal layer and minimizing deformation of the film laminate for the cell pouch.
[0005] In another aspect of the exemplary embodiment of the present invention, there is provided a film for a cell pouch, which can improve tensile strength and formability by improving a manufacturing process, and can improve curl properties before and after molding, and a manufacturing method thereof. [Means for solving the problem]
[0006] In an exemplary embodiment of the present invention, there is provided a film for a cell pouch, comprising: a sealant layer; an inner adhesive layer laminated on the sealant layer; a barrier layer laminated on the inner adhesive layer; an outer adhesive layer laminated on the barrier layer; and an outer layer formed on the outer adhesive layer, wherein the film for a cell pouch has a curl deviation of 3 mm or less as measured by the following method (the film for a cell pouch according to claim 1). [Evaluation of curl of film for cell pouches before molding] A film sample for cell pouches is prepared in a rectangular shape with dimensions of 15 cm x 1515 cm, and the sample is placed on a flat fixing table and fixed flat with tape. Make a 15cm long X-shaped cut through the center of the fixed specimen, and measure the height of the curl from two points on the MD (machine direction) side and two points on the TD (transverse direction) side, sandwiching the center point. Calculate the deviation from the difference between the MD and TD measurements.
[0007] In an example embodiment, the film for a cell pouch (the film for a cell pouch as recited in claim 1) may be a film for a cell pouch (the film for a cell pouch as recited in claim 2) having a curl deviation of 5 mm or less after molding, as measured by the following method. [Evaluation of curl after molding] (1) MD forming (evaluation of MD forming curl) A molded test piece measuring 26.6 (MD) x 24.0 (TD) cm is prepared. A molding evaluation is performed at 0.3 MPa using a chrome-coated 1-cup molding machine (molding depth is 8 mm for AL40μm application and 12 mm for AL60μm application). The R value (corner curvature radius value) of the molding machine is 4R (4 mm), the forming size during molding is 90 mm wide x 160 mm long, and single forming is performed. (2) Forming in the TD direction (evaluation of TD forming curl) A molded test piece measuring 26.6 (TD) x 24.0 (MD) cm is prepared. A molding evaluation is performed at 0.3 MPa using a chrome-coated 1-cup molding machine (molding depth is 8 mm for AL40μm application and 12 mm for AL60μm application). The R value (corner curvature radius value) of the molding machine is 4R (4 mm), the forming size during molding is 90 mm wide x 160 mm long, and single forming is performed. To evaluate the curl that occurs after molding, double-sided tape is attached to a flat surface, and the molded cell pouch film is fixed on top of it, and the height of the curl that occurs is measured. Measurements are taken at two points, and the highest value is recorded. After measuring each corner of the molded sample, the height of the corner where the curl occurred the highest is taken as the curl value.
[0008] In an example embodiment, the film for a cell pouch (the film for a cell pouch described in claim 1 or 2) may be a film for a cell pouch in which the barrier layer is not wound up alone during the manufacturing process but is wound up together with at least the outer layer (the film for a cell pouch described in claim 3).
[0009] In an example embodiment, the film for a cell pouch (the film for a cell pouch described in any one of claims 1 to 3) may be a film for a cell pouch (the film for a cell pouch described in claim 4) that has been wound up two or less times during the manufacturing process.
[0010] In an example embodiment, the film for a cell pouch (the film for a cell pouch according to any one of claims 1 to 4) may be a film for a cell pouch (the film for a cell pouch according to claim 5) in which the barrier layer is a metal layer, and the metal of the metal layer includes one or more selected from the group consisting of aluminum or an alloy thereof, titanium or an alloy thereof, tungsten or an alloy thereof, molybdenum or an alloy thereof, copper or an alloy thereof, and stainless steel.
[0011] In an example embodiment, the film for a cell pouch (the film for a cell pouch according to any one of claims 1 to 5) may be a film for a cell pouch (the film for a cell pouch according to claim 6) in which the outer layer includes one or more resins selected from the group consisting of nylon resin, polyethylene terephthalate (PET), and polybutylene terephthalate (PBT) resin. In an example embodiment, the film for a cell pouch (the film for a cell pouch described in any one of claims 1 to 6) may be a film for a cell pouch in which a surface treatment layer is formed on the barrier layer (the film for a cell pouch described in claim 7).
[0012] In an example embodiment, the film for a cell pouch (the film for a cell pouch according to any one of claims 1 to 7) may be a film for a cell pouch (the film for a cell pouch according to claim 8) in which the inner adhesive layer and the outer adhesive layer include one or more of an epoxy-based adhesive, a polyurethane-based adhesive, a phenolic resin-based adhesive, a polyolefin-based adhesive, and a polyester-based adhesive. In an example embodiment, the film for a cell pouch (the film for a cell pouch according to any one of claims 1 to 8) may be a film for a cell pouch (the film for a cell pouch according to claim 9) in which the inner adhesive layer is an adhesive coating layer; an extrusion coating layer; or an adhesive coating layer and an extrusion coating layer.
[0013] In an example embodiment, the film for a cell pouch (the film for a cell pouch according to any one of claims 1 to 9) may be a film for a cell pouch (the film for a cell pouch according to claim 10) in which the sealant layer is a sealant film or an extruded resin layer.
[0014] In addition, in an exemplary embodiment of the present specification, there is provided a cell pouch (cell pouch described in claim 11) including the film for a cell pouch (film for a cell pouch described in any one of claims 1 to 10) or a secondary battery (secondary battery described in claim 12) exteriorly packaged with the film for a cell pouch (film for a cell pouch described in any one of claims 1 to 10), particularly a medium- to large-sized secondary battery.
[0015] In addition, an exemplary embodiment of the present specification provides a method for manufacturing the film for a cell pouch (the film for a cell pouch according to any one of claims 1 to 10), the method comprising: a double-sided surface treatment step of performing a surface treatment on both sides of a metal raw material included in a barrier layer; an outer adhesive layer coating step of applying an adhesive to one side of the metal raw material subjected to the surface treatment to form an outer adhesive layer; and an outer layer lamination step of laminating an outer layer raw material on the outer adhesive layer; the film for a cell pouch is wound up two or less times during the manufacturing process, and the barrier layer in the film for a cell pouch is not wound up alone during the manufacturing process but is wound up together with the outer layer, or is wound up together with the outer layer and the sealant layer (the method for manufacturing the film for a cell pouch according to claim 13).
[0016] In an example embodiment, in the method (the method for manufacturing a film for a cell pouch as described in claim 13), the double-sided surface treatment step may be a method for manufacturing a film for a cell pouch as described in claim 14, in which after surface treatment on one side of the metal raw material, surface treatment on the other side of the metal raw material is immediately performed without performing a drying step.
[0017] In an example embodiment, the method (the method for manufacturing a film for a cell pouch as described in claim 13 or 14) may be a method for manufacturing a film for a cell pouch as described in claim 15, which further includes a physical property stabilization drying step of drying the metal raw material having surface treatments on both sides in a floating manner to stabilize physical properties between the both side surface treatment step and the outer adhesive layer coating step.
[0018] In an example embodiment, in the method (the method for manufacturing a film for a cell pouch according to any one of claims 13 to 15), the double-sided surface treatment step may include performing a first coating on one side of a metal raw material roll by applying a water-based and solvent-based coating liquid by a combined method of direct coating and RKC (Reverse Kiss Coating), and performing a second coating on the other side of the metal raw material roll by applying a coating liquid by a method of RKC and film up / down coating (the method for manufacturing a film for a cell pouch according to claim 16).
[0019] In an example embodiment, in the method (the method for manufacturing a film for a cell pouch according to any one of claims 13 to 16), the method may be a method for manufacturing a film for a cell pouch (the method for manufacturing a film for a cell pouch according to claim 17), including: a step of performing a first winding after the outer layer lamination step; an inner adhesive layer coating step of applying an adhesive to the other side of the surface-treated metal raw material, on which the outer layer is not laminated, to form an inner adhesive layer after the first winding; a step of laminating a sealant layer raw material under the inner adhesive layer; and a step of performing a second winding after laminating the sealant layer raw material. Effect of the Invention
[0020] The cell pouch film according to the exemplary embodiment of the present invention can minimize the mechanical deformation of the metal layer by reducing the number of windings and minimizing the winding tension through the improvement of the manufacturing process, thereby minimizing the deformation of the laminate of the cell pouch film. In addition, since the metal layer is not wound separately but a resin film with a lower elastic modulus than the metal layer is laminated and wound once, it is easy to adjust the tension at a low tension. Furthermore, the improvement of the manufacturing process can improve the tensile strength and formability, and the curl properties before and after forming can be improved. [Brief description of the drawings]
[0021] [Figure 1] 1 is a schematic cross-sectional view of a film for a cell pouch according to an exemplary embodiment of the present invention; [Diagram 2] 1 is a schematic diagram of a manufacturing apparatus for a film for a cell pouch according to an exemplary embodiment of the present invention; [Diagram 3] 1 is a photograph showing a method for evaluating curl of a film for a cell pouch before molding in an experimental example of the present invention. [Figure 4] 1 is a photograph showing a method for evaluating curl after molding in an experimental example of the present invention. [Figure 5a]1 is a graph showing a schematic diagram of winding tension (unit: N) according to winding length (unit: m) in an embodiment of an experimental example of the present invention. [Figure 5b] 1 is a graph showing a schematic diagram of winding tension (unit: N) according to winding length (unit: m) in comparative examples in experimental examples of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, exemplary embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0023] Definition of Terms In this specification, singular expressions may include plural expressions unless the context clearly indicates otherwise. In this application, the terms "comprise" or "have" are intended to indicate the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and do not exclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0024] In this specification, terms such as first, second, etc., are used to refer to features separated from one another, but not to a particular order, unless otherwise specified.
[0025] In this specification, the term "cell" refers to a battery, and has the broadest meaning including all types of batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.
[0026] In this specification, the term "cell pouch" or "cell pouch film" refers to a cell pouch in which cell components such as a positive electrode, a negative electrode, and a separator are impregnated with an electrolyte and housed, and has the broadest meaning including all laminated films processed into a bag or box shape in consideration of gas barrier properties, bendability, electrolyte resistance, thermal adhesiveness, etc., to house the cell components.
[0027] In this specification, the term "final structure" refers to the final layer structure of the film for the cell pouch. Such a final structure may vary slightly depending on the types of various manufacturing processes.
[0028] For example, the final structure may consist of an outer cover substrate (or outer layer), a first adhesive layer, an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, a second adhesive layer, and an inner cover substrate (or sealant layer). Or, the final structure may consist of an outer cover substrate (or outer layer), a first adhesive layer, an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, an extrusion coating layer, and an inner cover substrate (or sealant layer). Or, the final structure may consist of an outer cover substrate (or outer layer), a first adhesive layer, an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, a second adhesive layer, an extrusion coating layer, and an inner cover substrate (or sealant layer).
[0029] In this specification, the intermediate structure refers to a structure formed during the manufacturing process of the film for the cell pouch, and various intermediate structures of the cell pouch may be produced depending on the manufacturing process.
[0030] For example, a first intermediate structure may be produced that is composed of an outer cover substrate (or outer layer), a first adhesive layer (or outer adhesive layer), an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, and a second adhesive layer (or inner adhesive layer). Alternatively, a second intermediate structure may be produced that is composed of an outer cover substrate (or outer layer), a first adhesive layer (or outer adhesive layer), an outer surface treatment layer, a reference substrate (or barrier layer), and an inner surface treatment layer.
[0031] In this specification, an in-line process refers to a roll-to-roll process in which the web makes one pass between the unwinder and the rewinder (take-up roll).
[0032] In this specification, one rewind does not mean that the take-up roll rotates once (the take-up roll may of course rotate multiple times), but rather that the film is wound onto the take-up roll and completes the first run. Thus, two rewinds mean that the film completes the first run, then starts running again and completes the second run during the manufacturing process.
[0033] In this specification, the raw material may refer to the material of the barrier layer or metal layer provided during the manufacturing process.
[0034] In this specification, the functional base fabric may mean a resin base fabric that forms a sealant layer and / or an outer layer.
[0035] Description of exemplary embodiments Generally, the conventional technology includes a step of i) coating one side of a metal layer with a surface treatment layer, drying the layer, and winding the layer up (first winding step), coating the other side of the metal layer with another surface treatment layer, drying the layer, and winding the layer up again (second winding step); ii) forming an outer adhesive layer on one side of the surface-treated metal layer, laminating an outer layer, drying the layer, and winding the layer up (tertiary winding step); and iii) forming an inner adhesive layer on the other side of the surface-treated metal layer, laminating a sealant layer, and drying the layer. When multiple steps are repeated in this manner, the probability of running loss and process defects may increase. In addition, the film manufactured according to the conventional technology includes at least three winding steps until the sealant layer is laminated, so that the metal (such as aluminum) used in the barrier layer is highly likely to be deformed by the winding tension. Furthermore, since metals have a high elastic modulus, winding itself is difficult when winding with a reduced winding tension (for example, aluminum has a Young's elastic modulus of 69 to 86). In addition, since metals have a low restoring force, once they are deformed, there is a limit to how much they can recover, and therefore, when a process that can deform a metal is repeated multiple times, deformation due to tension occurs, which may result in a deterioration in the physical properties of the final cell pouch film.
[0036] Therefore, in an exemplary embodiment of the present invention, unlike the conventional method of manufacturing a film for a cell pouch by repeatedly performing processes such as coating, drying, and winding for each lamination process of each layer, the film is manufactured using a 1P3C (1 Pass 3 Coating) method in which three or more coating processes can be performed in one run of the original roll in a single in-line process, thereby solving the problems of the conventional technology and minimizing mechanical deformation of the metal layer, thereby minimizing deformation of the final film laminate for a cell pouch.
[0037] In addition, since the resin film, which has a lower elastic modulus than the metal layer, is laminated and wound once, rather than winding up the metal layer separately, it is easy to adjust the tension at a low level. Figures 5a and 5b show that it is easier to adjust the tension when the metal layer and the resin film are laminated and wound up (Figure 5a) than in the comparative example where the metal layer is wound up separately (Figure 5b).
[0038] As a result, the curl characteristics of the cell pouch film before and after molding can be improved. In this regard, high formability of the cell pouch film is a necessary characteristic for medium- and large-sized batteries, but the high formability can cause a serious curl phenomenon in which the end of the cell pouch film curls up after molding. This curl phenomenon can reduce the efficiency of the secondary battery manufacturing process. In particular, the cell manufacturing process is carried out through an automated continuous process, and an air suction machine is frequently used in this process. In this case, the curled part further curls up toward the air suction machine, which further reduces the process efficiency. Therefore, it is not easy to improve the curl characteristics, but in the exemplary embodiment of the present invention, the manufacturing process is improved to minimize the deformation of the laminate and improve the curl characteristics before and after molding.
[0039] Referring to FIG. 1, an exemplary embodiment of the present invention includes a sealant layer 500; an inner adhesive layer 400 laminated on the sealant layer 500; a barrier layer 300 laminated on the inner adhesive layer 400; an outer adhesive layer 200 laminated on the barrier layer 300; and an outer layer 100 formed on the outer adhesive layer 200, and the film for a cell pouch has been wound up two or less times, and the barrier layer 300 has been wound up together with at least the outer layer 100 or together with the outer layer 100 and the sealant layer 500, without being wound up alone. In example embodiments, the cell pouch film has a curl (curl before molding) deviation of 3 mm or less, measured by the following method. [Evaluation of curl of film for cell pouches before molding] A film sample for cell pouches is prepared in a rectangular shape with dimensions of 15 cm x 1515 cm, and the sample is placed on a flat fixing table and fixed flat with tape. Make a 15cm long X-shaped cut through the center of the fixed specimen, and measure the height of the curl from two points on the MD (machine direction) side and two points on the TD (transverse direction) side (see Figure 3). Calculate the deviation from the difference between the MD and TD measurements.
[0040] In non-limiting examples, the curl deviation before forming is 3 mm or less, 2.9 mm or less, 2.8 mm or less, 2.7 mm or less, 2.6 mm or less, 2.5 mm or less, 2.4 mm or less, 2.3 mm or less, 2.2 mm or less, 2.1 mm or less, 2.0 mm or less, 1.9 mm or less, 1.8 mm or less, 1.7 mm or less , 1.6 mm or less, 1.5 mm or less, 1.4 mm or less, 1.3 mm or less, 1.2 mm or less, 1.1 mm or less, 1.0 mm or less, 0.9 mm or less, 0.8 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, 0.3 mm or less, 0.2 mm or less, 0.1 mm or less, or 0 mm.
[0041] In example embodiments, the cell pouch film has a curl deviation of 5 mm or less after molding, as measured by the following method. [Evaluation of curl after molding] (1) MD forming (evaluation of MD forming curl) A molded test piece measuring 26.6 (MD) x 24.0 (TD) cm is prepared. A molding evaluation is performed at 0.3 MPa using a chrome-coated 1-cup molding machine (molding depth is 8 mm for AL40μm application and 12 mm for AL60μm application). The R value (corner curvature radius value) of the molding machine is 4R (4 mm), the forming size during molding is 90 mm wide x 160 mm long, and single forming is performed. (2) Forming in the TD direction (evaluation of TD forming curl) A molded test piece measuring 26.6 (TD) x 24.0 (MD) cm is prepared. A molding evaluation is performed at 0.3 MPa using a chrome-coated 1-cup molding machine (molding depth is 8 mm for AL40μm application and 12 mm for AL60μm application). The R value (corner curvature radius value) of the molding machine is 4R (4 mm), the forming size during molding is 90 mm wide x 160 mm long, and single forming is performed. To evaluate the curl that occurs after molding, double-sided tape is attached to a flat surface, and the molded cell pouch film is fixed on top of it, and the height of the curl that occurs is measured. Measurements are taken at two points, and the highest value is recorded. After measuring each corner of the molded sample, the height of the corner where the curl occurred the highest is taken as the curl value.
[0042] In non-limiting examples, the curl deviation after molding is 5 mm or less, 4.9 mm or less, 4.8 mm or less, 4.7 mm or less, 4.6 mm or less, 4.5 mm or less, 4.4 mm or less, 4.3 mm or less, 4.2 mm or less, 4.1 mm or less, 4.0mm or less, 3.9mm or less, 3.8mm or less, 3.7mm or less, 3.6mm or less, 3.5mm or less, 3.4mm or less, 3.3mm or less, 3.2mm or less, 3.1mm or less, 3.0mm or less, 2.9mm or less, 2.8mm or less, 2.7mm or less , 2.6mm or less, 2.5mm or less, 2.4mm or less, 2.3mm or less, 2.2mm or less, 2.1mm or less, 2.0mm or less, 1.9mm or less, 1.8mm or less, 1.7mm or less, 1.6mm or less, 1.5mm or less, 1.4mm or less, 1.3mm Below, it may be 1.2 mm or less, 1.1 mm or less, 1.0 mm or less, 0.9 mm or less, 0.8 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, 0.3 mm or less, 0.2 mm or less, 0.1 mm or less, or 0 mm.
[0043] In the illustrative embodiment of the present invention, the material and thickness of each layer of the film are not particularly limited as long as they can be manufactured into a film for a cell pouch, and may include, for example, the following configurations. The barrier layer is a layer that has the ability to block water vapor or air from the outside of the battery, and gas and / or moisture generated inside the battery.
[0044] In an example embodiment of the present invention, the barrier layer may include a metal layer or a surface treatment layer uniformly coated on both sides of the metal layer, and the metal layer may be a metal thin film or a metal deposition layer. The metal thin film may be a metal foil. The metal deposition layer may be formed by vacuum-depositing a metal on a separate plastic film, for example, a film of polyethylene terephthalate (PET), polyethylene (PE), or polypropylene (PP). In one embodiment, the metal of the metal layer is not particularly limited as long as it has the above-mentioned barrier properties, and examples thereof include at least one selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W) (single metal or mixture of single metals), or an alloy of two or more selected from the group consisting of aluminum or its alloy, titanium or its alloy, tungsten or its alloy, molybdenum or its alloy, copper or its alloy, and stainless steel. More specifically, it may include aluminum. In one embodiment, the surface treatment layer may be a surface treatment layer made of phosphate, chromium, zirconium, cerium, lanthanum, scandium, yttrium, etc. to provide corrosion resistance of the metal. In one embodiment, the barrier layer may have a thickness of 20 μm to 80 μm. If the thickness of the barrier layer is less than 20 μm, pinholes, microcracks, etc. may occur during a molding process, making it difficult to ensure safety, and if the thickness of the barrier layer is more than 80 μm, the energy density may be reduced during the manufacture of a battery. The outer layer is a layer having heat resistance, abrasion resistance, chemical resistance, etc., for protecting the barrier layer.
[0045] In an example embodiment of the present invention, the outer layer may include one or more resins selected from the group consisting of one or more resins selected from nylon resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc. More specifically, it may include oriented nylon. In one embodiment, the outer layer may have a thickness of 5 μm to 40 μm. The outer layer may be composed of a plurality of layers. The sealant layer is an inner layer that is bonded by heat after the cells are built in to provide sealing properties.
[0046] In an example embodiment of the present invention, the sealant layer may include a thermal adhesive resin, i.e., a sealing resin for thermal adhesion. Specifically, the sealant layer may include at least one selected from the group consisting of polyolefins such as polypropylene (PP) and polyethylene (PE), copolymers, terpolymers or derivatives thereof, and ethylene vinyl acetate (EVA). The copolymer or terpolymer may include an ethylene / propylene copolymer or an ethylene / propylene / butadiene terpolymer. In one embodiment, the sealant layer may have a thickness of 20 μm to 100 μm. The sealant layer may be composed of a plurality of layers. The outer adhesive layer is an adhesive layer for bonding the barrier layer and the outer layer.
[0047] In an example embodiment, the outer adhesive layer may include one or more of an epoxy adhesive, a polyurethane adhesive, a phenolic resin adhesive, a polyolefin adhesive, and a polyester adhesive, and may have a thickness of 0.5 μm to 10 μm.
[0048] In example embodiments, the inner adhesive layer may be an adhesive layer or an extruded resin layer for bonding the barrier layer and the sealant layer, or in another embodiment, the inner adhesive layer may be an extruded resin layer further formed between the inner adhesive layer and the sealant layer.
[0049] The inner adhesive layer may include one or more of an epoxy-based adhesive, a polyurethane-based adhesive, a phenolic resin-based adhesive, a polyolefin-based adhesive, and a polyester-based adhesive. In one embodiment, the inner adhesive layer may have a thickness of 0.5 μm to 10 μm. In one embodiment, the extruded resin layer may improve the bendability, adhesiveness, insulation, etc. of the pouch. In one embodiment, the extruded resin layer may include an olefin-based resin such as a polypropylene-based resin. In one embodiment, the extruded resin layer may have a thickness of about 5 to 80 μm.
[0050] The cell pouch film according to the exemplary embodiment of the present invention not only has excellent gas barrier properties, bendability, electrolyte resistance, and thermal adhesion, but also has improved problems in conventional manufacturing methods, such as deformation of the metal layer and deformation of the laminate due to multiple windings, and can exhibit good curl properties before and after molding.
[0051] Meanwhile, in an example embodiment of the present invention, a cell pouch including the above-mentioned cell pouch film or a secondary battery packaged therewith, particularly a medium- to large-sized secondary battery, may be provided.
[0052] Meanwhile, in an exemplary embodiment of the present invention, a method for manufacturing the above-mentioned film for a cell pouch may include a double-sided surface treatment step of performing a surface treatment on both sides of a metal raw material included in a barrier layer; an outer adhesive layer coating step of applying an adhesive to one side of the metal raw material subjected to the surface treatment to form an outer adhesive layer; and an outer layer lamination step of laminating an outer layer raw material on the outer adhesive layer, wherein the cell pouch film is wound up two or less times during the manufacturing process, and the barrier layer in the cell pouch film is not wound up alone during the manufacturing process but is wound up together with the outer layer, or is wound up together with the outer layer and a sealant layer.
[0053] In one embodiment, the two-sided surface treatment step may be performed by a two-sided double coating means including a first coater and a second coater, in which the other side of the metal web is immediately treated without a drying step after the surface treatment of one side of the metal web.
[0054] In one embodiment, the double-sided surface treatment step may include performing a first coating on one side of the metal web by applying a water-based or solvent-based coating liquid by a combined direct coating and reverse kiss coating (RKC) method, and performing a second coating on the other side of the metal web by applying a coating liquid by a RKC and film up / down coating method.
[0055] Specifically, the first coating is performed by applying water-based and solvent-based coating liquids by a first coater in a combined method of direct coating and reverse kiss coating (RKC), so that the physical properties and changes of the coating liquid can be taken into consideration. The other side of the metal roll may be subjected to a second coating by applying a coating liquid by RKC and film up / down coating. Meanwhile, the position of the substrate contact surface forming the outer layer, the coating roll, and the doctor can be adjusted, so that the coating uniformity and the work speed can be improved. More specifically, a chamber method (sealed piping) is configured to precisely control the coating agent, so that the viscosity of the coating agent can be adjusted and the inflow of foreign matter can be fundamentally blocked.
[0056] In one embodiment, the double-sided surface treatment step may more specifically include a web supplying process for unwinding and supplying a wound metal web; a foreign matter removing process for removing foreign matter present on the surface of the supplied metal web; a tension adjusting process for adjusting the tension of the metal web from which the foreign matter on the surface has been removed; and a double-sided coating process for coating both sides of the metal web while maintaining a constant tension.
[0057] In one embodiment, the foreign matter removal process may include a first foreign matter removal process of removing oil by performing an electric discharge treatment on both sides of the metal web. The foreign matter removal process may further include a pinhole inspection process of checking whether pinholes have occurred on both sides of the metal web from which the oil has been removed. The foreign matter removal process may further include a second foreign matter removal process of removing foreign matter occurring on both sides of the metal web after the pinhole inspection by a roll method.
[0058] In addition, the method according to an embodiment may further include a property stabilization drying step of drying the metal raw material having both surfaces treated in a floating manner between the both surface treatment step and the outer adhesive layer coating step to stabilize the physical properties. According to the floating method, both sides of the metal raw material having the surface treatment can be dried simultaneously, and contact between the roll and the raw material can be minimized, so that the occurrence of poor appearance runnability such as transfer of foreign matter due to the roll and puncture of the raw material can be significantly reduced.
[0059] In one embodiment, the method may further include a physical property stabilization drying step of drying the metal web having surface treatments on both sides in a floating manner to stabilize the physical properties, which may be an air floating method so that the web having surface treatments on both sides can be dried in a non-contact manner while floating. This allows the metal web coated on both sides to be dried while minimizing contact with components such as a feed roll. The method may further include a cooling step of cooling the dried metal web and a surface inspection step of inspecting the surface of the cooled metal web.
[0060] In one embodiment, the outer adhesive layer coating step of coating one side of the surface-treated metal roll with an adhesive to form an outer adhesive layer is a process of coating one side of the metal roll that has been surface-treated by two coatings, and may be performed by a third coater, and is prepared for lamination through processes such as drying. After coating the adhesive, the metal roll on which the adhesive is coated is dried to form an adhesive layer, and the thickness of the dried adhesive layer is measured, and the surface of the adhesive layer is corona-treated to strengthen the adhesive force.
[0061] In one embodiment, the method may further include, after the laminating step, an inner adhesive layer coating step of applying an inner adhesive to the other side of the metal sheet where the outer layer is not laminated to form an inner adhesive layer. In one embodiment, the method may further include a drying step after the coating step. In one embodiment, the method may further include a step of laminating a sealant layer sheet under the inner adhesive layer.
[0062] In one embodiment, the method may include a total of two or less winding steps until the final structure of the cell pouch is manufactured in order to prevent punctures and / or indentations from occurring on the raw material used in each step up to the outer layer lamination step.
[0063] Specifically, it is most preferable to produce the final structure of the cell pouch film by winding up the film in a total of two times or less, and more preferably, by winding up the film in a total of one time.
[0064] In one embodiment, the winding step may be performed after the outer layer lamination step or after the sealant layer lamination step. For example, the winding step may be performed in step (10) in FIG. 2.
[0065] In one embodiment, the lamination step of laminating an outer layer raw material on the outer adhesive layer and the step of laminating a sealant layer raw material under the inner adhesive layer are processes of laminating a functional raw material on one side of a metal raw material coated with an adhesive, and the inner side may be laminated with a sealant layer raw material for mainly stabilizing the heat resistance and cold resistance of the battery, and the outer side may be laminated with an outer layer raw material for heat resistance, pinhole resistance, abrasion resistance, etc. In one embodiment, each lamination step may be a step of laminating a previously prepared outer layer raw material or a sealant raw material.
[0066] In one embodiment, between the third coating step and the laminating step, an adhesive drying step of drying the adhesive-coated metal substrate to form an adhesive layer; an adhesive layer thickness measuring step of measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment step of corona-treating the surface of the adhesive layer to enhance adhesive strength may be further included.
[0067] In one embodiment, the method may further include a surface inspection step of inspecting the surfaces of the sealant layer and the outer layer after the lamination step.
[0068] In one embodiment, in order to minimize the occurrence of foreign matter and scratches during the process of feeding each raw web, both a Tendency structure in which the substrate contact roll and the shaft are separated and movable, and an integrated movable shaft structure may be applied to the guide roll. A general driving method of the guide roll is a mechanism in which the rotation from the motor is transmitted to the guide roll with the shaft integrated therewith to drive it at a 1:1 speed, whereas the Tensile driving method is a mechanism in which the guide roll and the shaft are separated to mutually correct the rotation speed of the fine rolls, and may be appropriately applied in the required section. As an example, a rewinder unit and an unwinder unit (raw web supply unit) may be separately configured so that they can be operated separately when a problem occurs in the operation of the equipment.
[0069] In addition, in one embodiment, a suction roll may be applied in the tension control section to minimize the generation of foreign matter and scratches during the feeding of the raw web, and a contact type clean roll may be applied to remove foreign matter generated during the running of the web and prevent the foreign matter from adhering to the roll and causing poor appearance (punctures, scratches, etc.).
[0070] Meanwhile, in an exemplary embodiment of the present invention, a maturing step may be further included. The maturing step is a necessary step for improving the reliability of adhesive strength, electrolyte resistance, peel strength, etc., during the manufacture of the film for cell pouch, but since it takes a somewhat long time, an optimal maturing step is essential. It is preferable in terms of productivity to manufacture the product through only one maturing step for the final structure of the film for cell pouch. Specifically, the method may include two or less maturing steps. More specifically, the method may include applying an adhesive to one side of the surface-treated metal raw material without a maturing step after the both-side surface treatment step, and the maturing step may be included after the lamination step of the outer layer and / or sealant layer. For example, if a maturing step is included in the both-side surface treatment step before the lamination step, the film in the middle of the manufacturing process may be exposed to air for a certain period of time or more, and the surface treatment agent that is not laminated may be desorbed. For example, if a maturing step is included in the adhesive layer formation step, a blocking phenomenon may occur in which the adhesive layer is partially reacted and then adheres to another layer.
[0071] Meanwhile, in an exemplary embodiment of the present invention, a manufacturing apparatus for a film for a cell pouch may be provided, which includes a double-sided surface treatment means including a first coater 3 and a second coater 4 for performing a surface treatment on both sides of a metal raw material forming a barrier layer, a third coater 7 for applying an adhesive to one side of the metal raw material that has been subjected to the surface treatment, and a laminating unit 9 for laminating a functional raw material on one side of the adhesive layer. Figure 2 is a schematic diagram of a manufacturing apparatus for a film for a cell pouch according to an embodiment of the present disclosure.
[0072] In one embodiment, the double-sided surface treatment means may include a web supply unit 1, a foreign matter removal unit 2, a tension adjustment unit, a first coater 3, and a second coater 4. The web supply unit 1 unwinds and supplies a wound metal web. The foreign matter removal unit 2 removes foreign matter present on the surface of the supplied metal web. The tension adjustment unit adjusts the tension of the metal web from which the foreign matter on the surface has been removed. The first coater 3 and the second coater 4 coat both sides of the metal web while maintaining a constant tension.
[0073] In one embodiment, the foreign matter removing means 2 may include a primary foreign matter removing unit that performs discharge treatment on both sides of the metal web to remove oil. Also, it may further include a pinhole inspection unit that checks for pinholes on both sides of the metal web from which the oil has been removed. If no abnormality is found as a result of the inspection, it may further include a secondary foreign matter removing unit that removes foreign matter generated on both sides of the metal web by a roll method.
[0074] In one embodiment, a property stabilization drying unit 5 may be provided between the double-sided surface treatment means and the third coater 7, which dries the metal web coated on both sides in a floating manner to stabilize the property. In this case, the drying method may be an air floating method so that the coated substrate can be dried in a non-contact manner while floating. This allows the metal web coated on both sides to be dried while minimizing contact with components such as a feed roll. Then, the dried metal web may be cooled by a cooling unit 6, and the surface of the cooled metal web may be inspected by a surface inspection unit.
[0075] In one embodiment, the adhesive drying unit 8 may be further provided between the third coater 7 and the laminating unit 9, for drying the adhesive-coated metal substrate to form an adhesive layer; an adhesive layer measuring unit for measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment unit for corona-treating the surface of the adhesive layer to enhance adhesive strength.
[0076] In one embodiment, the laminating unit 9 may further include a surface inspection unit for inspecting the surfaces of the sealant layer and the outer layer.
[0077] According to one embodiment, the film for cell pouches may be manufactured by the manufacturing apparatus shown in Fig. 2. In one embodiment, a fourth coater (not shown) that applies adhesive to the other side of the metal raw material that has been surface-treated, a drying unit (not shown), a functional raw material (outer layer, sealant layer) lamination unit (not shown), an extrusion unit (including co-extrusion) (not shown), etc. may be added as necessary between the lamination unit 9 and the final rewind unit (End, 2nd Rewind) in Fig. 2. EXAMPLES
[0078] The present disclosure will be described in more detail through the following examples. However, it will be obvious to those skilled in the art that these examples are merely for the purpose of illustrating the disclosure and should not be construed as limiting the scope of the present disclosure.
[0079] [experiment] Working Example The experimental examples were prepared by the following method. One side of the aluminum foil metal roll that forms the barrier layer was coated and surface-treated, and then the other side of the metal roll was coated and surface-treated. The metal roll with both sides coated was dried in a floating method to stabilize the physical properties. The dried metal roll was cooled, and a urethane adhesive was applied to one side of the metal roll that was surface-treated by a third coater to form an outer adhesive layer. Then, a PET / nylon film prepared in advance was laminated on the outer adhesive layer to form an outer layer. A urethane adhesive was also applied to the other side of the metal roll that was surface-treated, and a non-oriented polypropylene film was laminated to form a sealant layer, thereby manufacturing a film for a cell pouch. The specifications of each of Examples 1 and 2 are shown in Table 1 below.
[0080] Comparative Example A comparative cell pouch film was produced as follows. First, one side of an aluminum foil metal roll on which a barrier layer is to be formed is coated and dried, and then a primary winding step is performed in which the roll is wound up. Then, another surface treatment layer is coated on the other side of the metal roll, dried, and then the roll is wound up again for a secondary winding step. A urethane-based adhesive layer is coated on one side of the surface-treated metal layer, dried, and then a previously prepared PET / nylon film is laminated to form an outer layer, and a tertiary winding step is performed in which the outer layer is wound up. An inner adhesive layer is formed on the other side of the surface-treated metal layer, dried, and then a non-oriented polypropylene film is laminated to produce a film for a cell pouch. The specifications of each of Comparative Examples 1 and 2 are shown in Table 1 below. The tensile strength, forming depth, and curl before and after forming of the cell pouch film were evaluated for the examples and comparative examples. The results are shown in Table 1.
[0081] Evaluation of film tensile strength First, the tensile strength of the cell pouch film was evaluated. More specifically, the film was cut with a specimen cutter to prepare specimens with dimensions of 130 mm x 15 mm in the machine direction (MD) and transverse direction (TD). The tensile strength of the prepared specimens was measured using a universal testing machine UTM (manufacturer: INSTRON) in accordance with ASTM D638 at a stretching speed of 50 mm / min and a grip distance of 50 mm.
[0082] Evaluation of film formability A cell pouch film specimen measuring 266mm (TD) x 240mm (MD) in both the machine direction (MD) and transverse direction (TD) was taken. The taken specimen was molded into a rectangle (90mm wide, 160mm long). (Moldability was evaluated in one cup using chrome-coated high-form pouch moldability evaluation equipment, and although R values vary, the standard corner R value is 4.) When the depth was measured after molding, if none of the 10 pieces at that depth had any tears, the deeper depth was applied. If even one piece had a tear, the depth just before that was used as the maximum height and defined as formability.
[0083] Evaluation of curl before forming of film for cell pouch As shown in Figure 3, a film specimen for cell pouches was prepared in a square shape with dimensions of 15cm x 1515cm, and the specimen was placed on a flat fixed table and fixed flat with tape. An X-shaped cut 15cm long was made through the center of the fixed specimen, and the height of the curl was measured from two points on the MD (machine direction) side and two points on the TD (transverse direction) side, sandwiching the center point. The deviation was calculated from the difference between the MD and TD measurements.
[0084] Evaluation of curl after forming of film for cell pouches As shown in Figure 4, the cell pouch film was molded in the MD direction (266 mm (MD) x 240 mm (TD)) and in the TD direction (266 mm (TD) x 240 mm (MD)) to prepare test pieces. The molding evaluation is performed at 0.3 MPa using a chrome-coated one-cup molding machine. The molding depth is 8 mm for AL40μm application and 12 mm for AL60μm application. The R value (corner curvature radius) of the molding machine was 4R (4mm). The forming size during molding was 90mm wide x 160mm long, and single forming was performed. To evaluate curling that occurs after molding, double-sided tape is attached to a flat surface, and the molded pouch is then fixed on top of it to measure the height of curling. Measurements are taken at two points, and the highest value is recorded. After measuring each corner of the molded sample, the height of the corner where curling was greatest was taken as the curl value.
[0085] [Table 1]
[0086] As described above, it is clear that the examples are superior in tensile strength and moldability as well as curl properties before and after molding compared to the comparative examples. [Explanation of symbols]
[0087] 1: Original fabric supply section 2: Foreign matter removal means 3: 1st coater 4: 2nd coater 5: Physical property stabilization drying section 6: Cooling section 7: 3rd coater 8: Adhesive drying section 9: Lamination section 10: Winding section 100: Outer layer 200: Outer adhesive layer 300: Barrier layer 310: Surface treatment layer 320: Metal layer 330: Surface treatment layer 400: Inner adhesive layer 500: Sealant layer
Claims
1. A sealant layer; an inner adhesive layer laminated on the sealant layer; a barrier layer laminated on the inner adhesive layer; an outer adhesive layer laminated onto the barrier layer; and an outer layer formed on the outer adhesive layer; A cell pouch film comprising: A film for a cell pouch, characterized in that the curl deviation of the cell pouch film before molding, measured by the following method, is 3 mm or less. [Evaluation of curl of film for cell pouch before molding] A film sample for a cell pouch is prepared in a rectangular shape with dimensions of 15 cm x 1515 cm, and the sample is placed on a flat fixing table and fixed flat with tape. A 15 cm long X-shaped cut is made through the center of the fixed specimen, and the height of the curl is measured from two points on the MD (machine direction) side and two points on the TD (transverse direction) side, sandwiching the center point. The deviation is calculated from the difference between the MD and TD measurements.
2. 2. The film for a cell pouch according to claim 1, wherein the curl deviation of the film for a cell pouch after molding is 5 mm or less, as measured by the following method. [Evaluation of curl after molding] (1) Molding in the MD direction (evaluation of MD molding curl) A molded test piece measuring 26.6 (MD) x 24.0 (TD) cm is prepared. A molding evaluation is performed at 0.3 MPa using a chrome-coated one-cup molding machine (molding depth is 8 mm for AL 40 μm application and 12 mm for AL 60 μm application). The R value (corner curvature radius) of the molding machine is 4R (4 mm), the forming size during molding is 90 mm wide x 160 mm long, and single forming is performed. (2) Forming in the TD direction (evaluation of TD forming curl) A molded test piece measuring 26.6 (TD) x 24.0 (MD) cm is prepared. A molding evaluation is performed at 0.3 MPa using a chrome-coated one-cup molding machine (molding depth is 8 mm for AL 40 μm application and 12 mm for AL 60 μm application). The R value (corner curvature radius) of the molding machine is 4R (4 mm), the forming size during molding is 90 mm wide x 160 mm long, and single forming is performed. In order to evaluate the curl that occurs after molding, a double-sided tape is attached to a flat surface, and the molded cell pouch film is fixed on it, and the height of the curl that occurs is measured. Two points are measured as measurement positions, and the highest value is recorded. After measuring each corner of the molded sample, the height of the corner where the curl occurs most is taken as the curl value.
3. 3. The film for a cell pouch according to claim 2, wherein the barrier layer is not wound up separately during the manufacturing process but is wound up together with at least the outer layer.
4. The film for a cell pouch according to claim 3, wherein the film for a cell pouch is wound up two or less times during a manufacturing process.
5. 2. The film for cell pouches according to claim 1, wherein the metal of the barrier layer comprises at least one selected from the group consisting of aluminum or an alloy thereof, titanium or an alloy thereof, tungsten or an alloy thereof, molybdenum or an alloy thereof, copper or an alloy thereof, and stainless steel.
6. 2. The film for a cell pouch according to claim 1, wherein the outer layer contains one or more resins selected from the group consisting of nylon resin, polyethylene terephthalate (PET), and polybutylene terephthalate (PBT) resin.
7. 2. The film for a cell pouch according to claim 1, wherein a surface treatment layer is formed on the barrier layer.
8. 2. The film for a cell pouch according to claim 1, wherein the inner adhesive layer and the outer adhesive layer include at least one of an epoxy-based adhesive, a polyurethane-based adhesive, a phenolic resin-based adhesive, a polyolefin-based adhesive, and a polyester-based adhesive.
9. The film for a cell pouch according to claim 1, wherein the inner adhesive layer is an adhesive coating layer; an extrusion coating layer; or an adhesive coating layer and an extrusion coating layer.
10. 2. The film for a cell pouch according to claim 1, wherein the sealant layer is a sealant film or an extruded resin layer.
11. A cell pouch comprising the film for cell pouches according to any one of claims 1 to 10.
12. A secondary battery packaged with the cell pouch according to claim 11.
13. A method for producing the cell pouch film according to any one of claims 1 to 10, comprising: a double-sided surface treatment step of performing a surface treatment on both sides of the metal raw material included in the barrier layer; An outer adhesive layer coating step of applying an adhesive to one side of the surface-treated metal sheet to form an outer adhesive layer; and An outer layer lamination step of laminating an outer layer raw material onto the outer adhesive layer; The cell pouch film is wound up two or less times during the manufacturing process, A method for producing a film for a cell pouch, characterized in that in the film for a cell pouch, the barrier layer is not wound up alone during the production process but is wound up together with the outer layer, or is wound up together with the outer layer and the sealant layer.
14. The double-sided surface treatment step includes: The method for manufacturing a film for a cell pouch according to claim 13, wherein after the surface treatment on one side of the metal raw material, the surface treatment on the other side of the metal raw material is immediately performed without a drying step.
15. 14. The method of claim 13, further comprising a physical property stabilization drying step of drying the metal roll having both surfaces treated thereon in a floating manner to stabilize physical properties between the both surface treating step and the outer adhesive layer coating step.
16. In the double-sided surface treatment step, a first coating is performed on one side of the metal sheet by applying a water-based or solvent-based coating liquid using a direct coating method and a reverse kiss coating method (RKC).
14. The method of claim 13, further comprising: performing a second coating on the other side of the metal roll by applying a coating liquid by RKC and film up / down coating.
17. The method comprises: performing a first winding after the outer layer lamination step; an inner adhesive layer coating step of applying an adhesive to the other side of the surface-treated metal web, on which the outer layer is not laminated, to form an inner adhesive layer after the first winding; laminating a sealant layer sheet under the inner adhesive layer; and The method for producing a film for a cell pouch according to claim 13, further comprising the step of: performing a second winding after laminating the original sheet of the sealant layer.
Citation Information
Patent Citations
Manufacturing method for jacket member for power storage device
JP2015232961A
Cell pouch and method of preparing the same
KR1020180064834A
Biomaterial comprising nanomaterial-coated eggshell membrane
KR1020210102735A
Packaging material for batteries, method for producing same, polybutylene terephthalate film for packaging material for batteries, and battery
WO2018174056A1
Battery packaging material, method for manufacturing same, and battery
WO2019156113A1