Laminate and packaging bag

A laminate of polyethylene or polypropylene films, treated with stretching and electron beam irradiation, and incorporating white pigments, addresses recyclability and content concealment issues in packaging materials, ensuring strength and heat resistance.

JP2024149524APending Publication Date: 2024-10-18DAI NIPPON PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024121011
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional packaging materials composed of different resin materials face challenges in recyclability due to difficulty in separation, and the use of a background layer to conceal contents leads to reduced lamination strength and hand-tearability.

Method used

A laminate composed of polyethylene or polypropylene films, subjected to stretching and electron beam irradiation, with integrated white pigments in the base and sealant layers, enhancing strength, heat resistance, and recyclability while concealing contents effectively.

Benefits of technology

The laminate achieves sufficient strength, heat resistance, and recyclability, along with effective content concealment without compromising lamination strength or hand-tearability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149524000001_ABST
    Figure 2024149524000001_ABST
Patent Text Reader

Abstract

To provide a laminate capable of preparing a packaging bag or the like having sufficient strength and heat resistance and excellent recyclability and an excellent concealability of contents.SOLUTION: There is provided a laminate comprising a substrate and a sealant layer, wherein the substrate and the sealant layer are constituted of a same material, the substrate is subjected to at least one of stretching treatment and electron beam irradiation treatment, the same material is polyethylene or polypropylene, at least one of the substrate and the sealant layer contains a white pigment and at least one of the substrate and the sealant layer contains polyethylene derived from biomass or polypropylene derived from biomass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate used for producing a packaging material, etc. The present invention also relates to a packaging material composed of the laminate.

[0002] Conventionally, resin films made of resin materials have been used as materials for forming packaging materials. For example, resin films made of polyolefins have appropriate flexibility and transparency as well as excellent heat sealability, and therefore are widely used as packaging materials.

[0003] Generally, resin films made of polyolefins are inferior in strength and heat resistance and therefore cannot be used as a base material for constructing packaging materials, etc., and are used by laminating them with resin films made of polyester, polyamide, etc. For this reason, normal packaging materials are composed of a laminate in which the base material and the sealant layer are made of different types of resin materials (for example, Patent Document 1).

[0004] In recent years, with the growing demand for the creation of a recycling-oriented society, there is a demand for high recyclability in packaging materials, etc. However, conventional packaging materials are composed of different resin materials as described above, and since it is difficult to separate each resin material, they are not currently recycled.

[0005] In addition, various contents are filled into such packaging materials, and the contents, such as detergent, In some cases, the color of the packaging material can be seen through the packaging material, which can cause images formed on the surface of the substrate to become unclear. In order to solve such problems, a background layer is formed between the substrate and the sealant layer using an ink containing a white pigment to conceal the contents. However, when a background layer is formed, new problems arise, such as a decrease in the lamination strength between the substrate and the heat seal and a decrease in the hand tearability of the packaging material. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2009-202519 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors have found that by subjecting a polyethylene film or a polypropylene film to at least one of a stretching treatment and an electron beam irradiation treatment, the strength and heat resistance of the film can be significantly improved, making it possible to use the film as a substrate in a laminate used in the manufacture of packaging materials, etc. Furthermore, the present inventors have found that by forming the sealant layer from a polyolefin, like the substrate, the recyclability of the laminate can be significantly improved. Furthermore, the inventors have discovered that by incorporating a white pigment into at least one of the substrate and the sealant layer, or into an intermediate layer provided between the substrate and the sealant layer, the contents can be effectively concealed without reducing the laminate strength between the layers or the ease of tearing the packaging material by hand.

[0008] The present invention has been made in consideration of the above findings, and the problem to be solved by the present invention is to provide a laminate that enables the production of packaging materials and the like that have sufficient strength and heat resistance, and are also excellent in recyclability and content concealment properties.

[0009] Another problem to be solved by the present invention is to provide a packaging material formed from the laminate. [Means for solving the problem]

[0010] In a first embodiment, the laminate of the present invention is a laminate comprising a substrate and a sealant layer, The substrate and the sealant layer are made of the same material; The substrate has been subjected to at least one of a stretching treatment and an electron beam irradiation treatment, The same material is polyethylene or polypropylene, At least one of the substrate and the sealant layer comprises a white pigment; At least one of the substrate and the sealant layer is characterized in that it contains biomass-derived polyethylene or biomass-derived polypropylene.

[0011] In one embodiment, the substrate comprises a white pigment; The content of the white pigment in the base material is 0.5% by mass or more and 20% by mass or less.

[0012] In one embodiment, the thickness of the substrate is 15 μm or more and 40 μm or less.

[0013] In one embodiment, the sealant layer comprises a white pigment; The content of the white pigment in the sealant layer is 2% by mass or more and 15% by mass or less.

[0014] In one embodiment, the thickness of the sealant layer is 40 μm or more and 180 μm or less.

[0015] In a second embodiment, the laminate of the present invention is a laminate comprising a substrate, an intermediate layer, and a sealant layer, The substrate, the intermediate layer and the sealant layer are made of the same material; The substrate has been subjected to at least one of a stretching treatment and an electron beam irradiation treatment, The same material is polyethylene or polypropylene, The intermediate layer contains a white pigment, At least one of the substrate, intermediate layer and sealant layer is characterized by containing biomass-derived polyethylene or biomass-derived polypropylene.

[0016] In one embodiment, the laminate is used in packaging applications.

[0017] The packaging material of the present invention is characterized in that it is constituted by the above-mentioned laminate.

[0018] In one embodiment, the packaging material comprises a brewing nozzle.

[0019] In one embodiment, the packaging material comprises a spout. Effect of the Invention

[0020] According to the present invention, it is possible to provide a laminate that has sufficient strength and heat resistance, and is capable of producing a packaging material having excellent recyclability and content concealment properties. [Brief description of the drawings]

[0021] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 4] FIG. 1 is a perspective view showing one embodiment of a packaging material produced using a laminate of the present invention. [Diagram 5] FIG. 1 is a front view showing one embodiment of a packaging material produced using a laminate of the present invention. [Figure 6] FIG. 1 is a front view showing one embodiment of a packaging material produced using a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] (Laminate in the first embodiment) In a first embodiment, a laminate 10 of the present invention is characterized by comprising a substrate 11 and a sealant layer 12, as shown in FIG. In the present invention, the substrate and the sealant layer are made of the same material, i.e., polyethylene or polypropylene, which can improve the recyclability of the laminate. In the present invention, at least one of the substrate and the sealant layer contains a white pigment. This can improve the visibility of an image formed on the substrate and can conceal the contents. When the substrate contains a white pigment, it becomes difficult to form an image on the sealant layer side of the substrate, but from the viewpoint of image storage stability, it is preferable to form an image on the sealant layer side of the substrate. From this viewpoint, it is preferable that the sealant layer contains a white pigment. Furthermore, in the present invention, at least one of the substrate and the sealant layer contains, as the polyethylene or polypropylene, a biomass-derived polyethylene or a biomass-derived polypropylene, which can effectively reduce the environmental impact of packaging materials produced using the laminate of the present invention.

[0023] Furthermore, the laminate 10 of the present invention may include an intermediate layer 13 between the substrate 11 and the sealant layer 12, as shown in FIG. Furthermore, the laminate 10 of the present invention may include an adhesive layer 14 between any of the layers, for example, between the substrate 11 and the sealant layer 12 as shown in FIG.

[0024] (base material) The substrate constituting the laminate of the present invention is made of polyethylene or polypropylene, and is characterized by having been subjected to at least one of a stretching treatment and an electron beam irradiation treatment. By carrying out the stretching treatment and electron beam irradiation treatment, the heat resistance and strength of the substrate can be significantly improved, and the physical properties required for the outer layer of a packaging material or the like can be satisfied. When the substrate has been subjected to electron beam irradiation treatment, the substrate is provided so that the surface of the substrate irradiated with electron beams becomes the outermost surface of the laminate.

[0025] As the polyethylene, high density polyethylene, medium density polyethylene, low density polyethylene, linear low density polyethylene and very low density polyethylene can be used. Among these, high density polyethylene and medium density polyethylene are preferred from the viewpoint of the strength and heat resistance of the substrate, and medium density polyethylene is more preferred from the viewpoint of stretchability.

[0026] In the present invention, the high density polyethylene has a density of 0.945 g / cm 3 The polyethylene having a density of 0.925 g / cm3 or more can be used. 3 More than 0.945g / cm 3 Polyethylene having a density of less than 0.900 g / cm3 can be used. 3 More than 0.925g / cm 3 For linear low density polyethylene, a polyethylene having a density of 0.900 g / cm3 or less can be used. 3 More than 0.925g / cm 3 For ultra-low density polyethylene, a polyethylene having a density of 0.900 g / cm3 can be used. 3 Less than 100 mm of polyethylene can be used.

[0027] In addition, as long as the characteristics of the present invention are not impaired, a copolymer of ethylene and another monomer can also be used as the polyethylene. The ethylene copolymer includes a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms, and examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. In addition, as long as the object of the present invention is not impaired, a copolymer with vinyl acetate or an acrylic acid ester may also be used.

[0028] In one embodiment, the substrate contains biomass-derived polyethylene, which is obtained by polymerizing a monomer containing biomass-derived ethylene. Since such biomass-derived polyethylene is a carbon-neutral material, the environmental impact of producing the laminate can be reduced. Since biomass-derived ethylene is used as the raw material monomer, the polyethylene obtained by polymerization is derived from biomass. Note that the raw material monomer for polyethylene does not have to contain 100% by mass of biomass-derived ethylene.

[0029] When the substrate contains biomass-derived polyethylene, the content thereof is preferably from 5% by mass to 100% by mass, and more preferably from 10% by mass to 70% by mass.

[0030] The monomers that are the raw material for the biomass-derived polyethylene may further contain ethylene and / or α-olefins derived from fossil fuels, or may further contain α-olefins derived from biomass.

[0031] The concentration of ethylene derived from biomass in the polyethylene contained in the base material (hereinafter sometimes referred to as "biomass ratio") is preferably 10% or more. "Biomass content" is a value measured by radiocarbon (C14) measurement to determine the amount of carbon derived from biomass. Carbon dioxide in the atmosphere contains a certain percentage of C14 (105.5 pMC), so it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain very little C14. Therefore, the proportion of carbon derived from biomass can be calculated by measuring the proportion of C14 in the total carbon atoms in the polyethylene. C14 The content of carbon derived from biomass, P bio It can be calculated as follows: P bio (%)=P C14 / 105.5×100

[0032] In the present invention, theoretically, if all ethylene derived from biomass is used as a raw material for polyethylene, the concentration of biomass-derived ethylene is 100%, and the biomass content of the biomass-derived polyethylene is 100%. In addition, the concentration of biomass-derived ethylene in fossil fuel-derived polyethylene produced only from fossil fuel-derived raw materials is 0%, and the biomass content of fossil fuel-derived polyethylene is 0%.

[0033] Biomass-derived ethylene can be produced using biomass-derived ethanol as a raw material. In particular, it is preferable to use biomass-derived fermented ethanol obtained from a plant raw material. The plant raw material is not particularly limited, and any conventionally known plant can be used. Examples of the plant raw material include corn, sugarcane, beet, and manioc.

[0034] In the present invention, the fermented ethanol derived from biomass refers to ethanol produced by contacting a culture solution containing a carbon source obtained from a plant raw material with an ethanol-producing microorganism or a product derived from its crushed material, and then purifying the ethanol. Conventionally known methods such as distillation, membrane separation, and extraction can be applied to purify ethanol from the culture solution. For example, a method of adding benzene, cyclohexane, etc., and removing water by azeotropy or membrane separation can be used.

[0035] A catalyst is usually used when obtaining ethylene by the dehydration reaction of ethanol, but the catalyst is not particularly limited and any conventionally known catalyst can be used. From the viewpoint of the process, a fixed bed flow reaction is advantageous because it is easy to separate the catalyst from the product, and for example, γ-alumina is preferable.

[0036] This dehydration reaction is an endothermic reaction, and is usually carried out under heating conditions. As long as the reaction proceeds at a commercially useful reaction rate, the heating temperature is not limited, but is preferably 100° C. or higher, more preferably 250° C. or higher, and even more preferably 300° C. or higher. There is no particular upper limit, but from the viewpoint of energy balance and equipment, it is preferably 500° C. or lower, more preferably 400° C. or lower.

[0037] The reaction pressure is not particularly limited, but is preferably equal to or higher than atmospheric pressure in order to facilitate the subsequent gas-liquid separation. From an industrial perspective, a fixed bed flow reaction is preferred because it is easy to separate the catalyst, but a liquid phase suspension bed, a fluidized bed, etc. may also be used.

[0038] In the dehydration reaction of ethanol, the yield of the reaction depends on the amount of water contained in the ethanol supplied as a raw material. In general, when performing a dehydration reaction, it is preferable to have no water, considering the efficiency of removing water. However, in the case of the dehydration reaction of ethanol using a solid catalyst, it has been found that the amount of other olefins, especially butene, produced tends to increase if water is not present. It is presumed that this is because ethylene dimerization after dehydration cannot be suppressed if a small amount of water is not present. The lower limit of the allowable water content is 0.1% or more, preferably 0.5% or more. There is no particular limit to the upper limit, but from the viewpoint of material balance and heat balance, it is preferably 50% by weight or less, more preferably 30% or less, and even more preferably 20% or less.

[0039] By carrying out the dehydration reaction of ethanol in this manner, a mixture of ethylene, water and a small amount of unreacted ethanol is obtained, but since ethylene is in a gaseous state at room temperature under about 5 MPa or less, water and ethanol can be removed from this mixture by gas-liquid separation to obtain ethylene. This method may be performed by any known method.

[0040] The ethylene obtained by the gas-liquid separation is further distilled. The distillation method, operation temperature, residence time, etc. are not particularly limited, except that the operation pressure at this time is normal pressure or higher.

[0041] When the raw material is biomass-derived ethanol, the obtained ethylene contains trace amounts of carbonyl compounds such as ketones, aldehydes, and esters, which are impurities mixed in during the ethanol fermentation process, as well as carbon dioxide gas, which is a decomposition product thereof, and nitrogen-containing compounds such as amines and amino acids, which are enzyme decomposition products and impurities, as well as ammonia, which is a decomposition product thereof. Depending on the use of ethylene, these trace amounts of impurities may be problematic, so they may be removed by purification. The purification method is not particularly limited, and can be performed by a conventionally known method. An example of a suitable purification operation is an adsorption purification method. The adsorbent used is not particularly limited, and a conventionally known adsorbent can be used. For example, a material with a high surface area is preferable, and the type of adsorbent is selected according to the type and amount of impurities in the ethylene obtained by the dehydration reaction of biomass-derived ethanol.

[0042] In addition, a caustic water treatment may be used in combination as a method for purifying impurities in ethylene. When caustic water treatment is used, it is preferable to carry out the treatment before adsorption purification. In that case, it is necessary to carry out a water removal treatment after the caustic treatment and before the adsorption purification.

[0043] The base material can also contain polyethylene recycled by mechanical recycling. Mechanical recycling generally refers to a method in which recovered polyethylene films are crushed, washed with an alkali to remove dirt and foreign matter from the film surface, and then dried at high temperature and reduced pressure for a certain period of time to diffuse and decontaminate the contaminants remaining inside the film, removing dirt from the polyethylene film and returning it to polyethylene.

[0044] The polypropylene may be a homopolymer, a random copolymer or a block copolymer. A polypropylene homopolymer is a polymer of propylene alone, a polypropylene random copolymer is a random copolymer of propylene and an α-olefin other than propylene (e.g., ethylene, butene-1, 4-methyl-1-pentene, etc.), and a polypropylene block copolymer is a copolymer having a polymer block of propylene and a polymer block of the above-mentioned α-olefin other than propylene. Among these polypropylenes, it is preferable to use a homopolymer or a random copolymer from the viewpoint of improving the transparency of the substrate and improving the visibility of an image formed on the adhesive layer side surface of the substrate. When the rigidity and heat resistance of the packaging material are important, a homopolymer can be used, and when impact resistance and the like are important, a random copolymer can be used.

[0045] Also, in one embodiment, the substrate comprises biomass-derived polypropylene.

[0046] When the base material contains biomass-derived polypropylene, the content thereof is preferably from 5% by mass to 95% by mass, and more preferably from 10% by mass to 70% by mass. Moreover, the biomass content of the biomass-derived polypropylene is preferably 10% or more.

[0047] The substrate can also include recycled polypropylene by mechanical recycling.

[0048] In one embodiment, the substrate contains a white pigment. This can improve the visibility of an image formed on the substrate. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be concealed. In addition, the light-shielding property of the laminate can be improved. Furthermore, the laminate of this configuration does not require a background layer to be formed with an ink containing a white pigment, which is preferable because it does not cause a decrease in the lamination strength between the layers of the laminate or a decrease in the hand tearability of the packaging material.

[0049] Examples of white pigments include titanium white (titanium(IV) oxide), zinc oxide (zinc oxide), lithopone, calcium carbonate, barium sulfate, aluminum hydroxide, etc. Among these, titanium oxide is preferred because it has no specific absorption in the visible region and has a high refractive index. The substrate may contain two or more of these white pigments.

[0050] The content of the white pigment in the substrate is preferably from 2% by mass to 20% by mass, and more preferably from 4% by mass to 15% by mass. By making the content of the white pigment in the substrate 4% by mass or more, when an image is formed on the substrate, the visibility of the image can be further improved. In addition, the light blocking property of the laminate can be further improved. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be more concealed. Furthermore, by keeping the white pigment content in the substrate at 20 mass % or less, a film with a stable thickness can be produced during film formation, processing suitability comparable to that of transparent films can be maintained during printing and lamination, the physical properties of the product after processing can be maintained, and unnecessary increases in film prices can be suppressed.

[0051] The substrate may contain additives within the range that does not impair the characteristics of the present invention. Examples of such additives include crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins.

[0052] In one embodiment, the substrate has a multi-layer structure. In the case of a substrate having a multi-layer structure, the biomass-derived polyethylene or polypropylene and the white pigment may be contained in at least one layer. From the viewpoint of suitability for printing on a substrate, the white pigment is preferably contained in the intermediate layer.

[0053] In one embodiment, the substrate comprises a layer made of high density polyethylene (hereinafter referred to as high density polyethylene layer), a layer made of medium density polyethylene (hereinafter referred to as medium density polyethylene layer), and a layer made of high density polyethylene (hereinafter referred to as high density polyethylene layer). By adopting such a configuration, it is possible to further improve the strength and heat resistance of the substrate, prevent the substrate from curling, and improve the stretchability of the substrate. In this case, the thickness of the high density polyethylene layer is preferably thinner than the thickness of the medium density polyethylene layer. The ratio of the thickness of the high density polyethylene layer to the thickness of the medium density polyethylene layer is preferably 1 / 10 or more and 1 / 1 or less, and more preferably 1 / 5 or more and 1 / 2 or less. By setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the medium-density polyethylene layer to 1 / 10 or more, the strength and heat resistance of the substrate can be further improved. Also, by setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the medium-density polyethylene layer to 1 / 1 or less, the stretchability of the substrate can be further improved.

[0054] In one embodiment, the substrate has a multilayer structure including a layer made of high density polyethylene (hereinafter referred to as high density polyethylene layer), a layer made of medium density polyethylene (hereinafter referred to as medium density polyethylene layer), and a layer made of high density polyethylene (hereinafter referred to as high density polyethylene layer). By adopting such a configuration, it is possible to further improve the strength and heat resistance of the substrate, prevent the substrate from curling, and improve the stretchability of the substrate. In this case, the thickness of the high density polyethylene layer is preferably thinner than the thickness of the medium density polyethylene layer. The ratio of the thickness of the high density polyethylene layer to the thickness of the medium density polyethylene layer is preferably 1 / 10 or more and 1 / 1 or less, and more preferably 1 / 5 or more and 1 / 2 or less. By setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the medium-density polyethylene layer to 1 / 10 or more, the strength and heat resistance of the substrate can be further improved. Also, by setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the medium-density polyethylene layer to 1 / 1 or less, the stretchability of the substrate can be further improved.

[0055] In one embodiment, the substrate comprises a high density polyethylene layer, a medium density polyethylene layer, a low density polyethylene layer, a linear low density polyethylene layer or an ultra low density polyethylene layer (collectively referred to as a low density polyethylene layer in this paragraph for the sake of simplicity), a medium density polyethylene layer and a high density polyethylene layer. By adopting such a configuration, it is possible to improve the stretchability of the substrate, to improve the strength and heat resistance of the substrate, to prevent the substrate from curling, and to improve the production efficiency of the substrate. In this case, the thickness of the high density polyethylene layer is preferably thinner than the thickness of the medium density polyethylene layer. The ratio of the thickness of the high density polyethylene layer to the thickness of the medium density polyethylene layer is preferably 1 / 10 or more and 1 / 1 or less, and more preferably 1 / 5 or more and 1 / 2 or less. By setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the medium-density polyethylene layer to 1 / 10 or more, the strength and heat resistance of the substrate can be improved, and by setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the medium-density polyethylene layer to 1 / 1 or less, the stretchability of the substrate can be improved. In addition, the thickness of the high density polyethylene layer is preferably the same as or greater than the thickness of the low density polyethylene layer. The ratio of the thickness of the high density polyethylene layer to the thickness of the low density polyethylene layer is preferably 1 / 0.25 or more and 1 / 2 or less, and more preferably 1 / 0.5 or more and 1 / 1 or less. By setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the low-density polyethylene layer to 1 / 0.25 or more, the heat resistance of the substrate can be improved. Also, by setting the ratio of the thickness of the high-density polyethylene layer to the thickness of the low-density polyethylene layer to 1 / 1 or less, the adhesion between the medium-density polyethylene layers can be improved. The thickness of each high-density polyethylene layer is preferably 1 μm or more and 20 μm or less, and more preferably 2 μm or more and 10 μm or less. By making the thickness of the high-density polyethylene layer 1 μm or more, the strength and heat resistance of the laminate of the present invention can be further improved. In addition, by making the thickness of the high-density polyethylene layer 20 μm or less, the processability of the laminate of the present invention can be further improved. The thickness of the medium-density polyethylene layer is preferably 1 μm or more and 30 μm or less, and more preferably 5 μm or more and 20 μm or less. By making the thickness of the medium-density polyethylene layer 1 μm or more, the stretchability of the film can be further improved. In addition, by making the thickness of the medium-density polyethylene layer 30 μm or less, the processability of the laminate of the present invention can be further improved. The thickness of the low-density polyethylene layer is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 5 μm or less. By making the thickness of the low-density polyethylene layer 1 μm or more, the adhesion between the high-density polyethylene layer and the medium-density polyethylene layer can be further improved. In addition, by making the thickness of the low-density polyethylene layer 5 μm or less, the processability of the laminate of the present invention can be further improved. In one embodiment, a substrate having such a configuration can be produced by, for example, an inflation method. Specifically, the film can be produced by co-extruding, from the outside, a high-density polyethylene layer, a medium-density polyethylene layer, and a low-density polyethylene layer, a linear low-density polyethylene layer, or an ultra-low-density polyethylene layer into a tubular shape, and then pressing the opposing low-density polyethylene layers, linear low-density polyethylene layers, or ultra-low-density polyethylene layers together using a rubber roll or the like. By using such a method, the number of defective products during manufacturing can be significantly reduced, and ultimately, production efficiency can be improved. In addition, the stretching can also be carried out in the inflation film forming machine, which can further improve the production efficiency.

[0056] In one embodiment, the seven-layer co-extruded film may be configured to include, from the outside, a high-density polyethylene layer, a blend resin layer of high-density polyethylene and medium-density polyethylene, a medium-density polyethylene layer, a low-density polyethylene layer, a linear low-density polyethylene layer or an ultra-low-density polyethylene layer (in this paragraph, for simplicity, these are collectively referred to as low-density polyethylene layers), a medium-density polyethylene layer, a blend resin layer of high-density polyethylene and medium-density polyethylene, and a high-density polyethylene layer. By adopting such a structure, it is possible to improve the adhesion between the high density polyethylene layer and the medium density polyethylene layer, and also to improve the processability of the laminate of the present invention. The thickness of each high-density polyethylene layer is preferably 1 μm or more and 20 μm or less, and more preferably 2 μm or more and 10 μm or less. By making the thickness of the high-density polyethylene layer 1 μm or more, the strength and heat resistance of the laminate of the present invention can be further improved. In addition, by making the thickness of the high-density polyethylene layer 20 μm or less, the processability of the laminate of the present invention can be further improved. The thickness of each blend resin layer of high density polyethylene and medium density polyethylene is preferably 1 μm or more and 20 μm or less, more preferably 2 μm or more and 10 μm or less. This can improve the adhesion between the high density polyethylene layer and the medium density polyethylene layer. In addition, the processability of the laminate of the present invention can be improved. The thickness of the medium-density polyethylene layer is preferably 1 μm or more and 30 μm or less, and more preferably 5 μm or more and 20 μm or less. By making the thickness of the medium-density polyethylene layer 1 μm or more, the stretchability of the film can be further improved. In addition, by making the thickness of the medium-density polyethylene layer 30 μm or less, the processability of the laminate of the present invention can be further improved. The thickness of the low-density polyethylene layer is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 5 μm or less. By making the thickness of the low-density polyethylene layer 1 μm or more, the adhesion between the high-density polyethylene layer and the medium-density polyethylene layer can be further improved, and by making the thickness of the low-density polyethylene layer 5 μm or less, the processability of the laminate of the present invention can be further improved. In one embodiment, the stretched polyethylene film having such a configuration can be produced by the above-mentioned inflation method. By using such a method, the number of defective products during manufacturing can be significantly reduced, and ultimately, production efficiency can be improved. In addition, the stretching can also be carried out in the inflation film forming machine, which can further improve the production efficiency.

[0057] When the substrate is subjected to a stretching treatment, the stretching may be uniaxial or biaxial. The stretching ratio in the machine direction (MD) of the substrate is preferably 2 times or more and 10 times or less, and more preferably 3 times or more and 7 times or less. By making the stretching ratio in the longitudinal direction (MD) of the substrate 2 times or more, the strength and heat resistance of the substrate can be improved. Furthermore, the printability of the substrate can be improved. Furthermore, the transparency of the substrate can be improved. On the other hand, the upper limit of the stretching ratio in the longitudinal direction (MD) of the substrate is not particularly limited, but it is preferably 10 times or less from the viewpoint of the breaking limit of the substrate. The stretch ratio in the transverse direction (TD) of the substrate is preferably 2 times or more and 10 times or less, and more preferably 3 times or more and 7 times or less. By setting the stretch ratio in the transverse direction (TD) of the substrate to 2 times or more, the strength and heat resistance of the substrate can be improved. Furthermore, the printability of the substrate can be improved. Furthermore, the transparency of the substrate can be improved. On the other hand, the upper limit of the stretch ratio in the transverse direction (TD) of the substrate is not particularly limited, but it is preferably 10 times or less from the viewpoint of the breaking limit of the substrate.

[0058] When the substrate is irradiated with an electron beam, the crosslink density of the polyethylene or polypropylene contained in the substrate is increased by the electron beam irradiation, and the heat resistance and strength of the substrate can be significantly improved. This embodiment is particularly suitable for the substrate made of polyethylene.

[0059] The substrate may be one in which the polyethylene on one surface has been irradiated with an electron beam to increase the crosslink density, or the crosslink density of the polyolefin throughout the substrate may be increased. When the substrate has a multi-layer structure, it is sufficient that the crosslink density of at least the polyethylene in the outermost layer is improved by electron beam irradiation. From the viewpoint of strength and heat resistance, it is preferable that the crosslink density of the polyethylene as a whole is improved by electron beam irradiation.

[0060] As an apparatus that can be used for irradiating the substrate with an electron beam, a conventionally known apparatus can be used. For example, a curtain-type electron irradiation apparatus (LB1023, manufactured by I-Electron Beam Inc.), a line-irradiation type low-energy electron beam irradiation apparatus (EB-ENGINE, manufactured by Hamamatsu Photonics K.K.), and a drum roll-type electron beam irradiation apparatus (EZ-CURE, manufactured by I-Electron Beam Inc.) can be suitably used.

[0061] The dose of the electron beam irradiated to the substrate is preferably in the range of 10 kGy to 2000 kGy, more preferably in the range of 20 kGy to 1000 kGy, and even more preferably in the range of 150 kGy to 500 kGy. The accelerating voltage of the electron beam is preferably in the range of 30 kV or more and 300 kV or less, more preferably in the range of 50 kV or more and 300 kV or less, and even more preferably in the range of 50 kV or more and 250 kV or less. Furthermore, the irradiation energy of the electron beam is preferably in the range of 20 keV or more and 750 keV or less, more preferably in the range of 25 keV or more and 500 keV or less, even more preferably in the range of 30 keV or more and 400 keV or less, and particularly preferably in the range of 20 keV or more and 200 keV or less.

[0062] The oxygen concentration in the electron beam irradiation device is preferably 500 ppm or less, more preferably 100 ppm or less. By performing electron beam irradiation under such conditions, it is possible to suppress the generation of ozone and also to suppress the radicals generated by electron beam irradiation from being deactivated by oxygen in the atmosphere. Such conditions can be achieved, for example, by making the inside of the device an inert gas (nitrogen, argon, etc.) atmosphere.

[0063] In one embodiment, the irradiation with the electron beam can be performed simultaneously with cooling using a cooling drum or the like.

[0064] The substrate may be subjected to a surface treatment, which can improve adhesion to adjacent layers. The method of surface treatment is not particularly limited, and examples thereof include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, as well as chemical treatments such as oxidation treatment using chemicals. Furthermore, an anchor coat layer may be formed on the surface of the substrate using a conventionally known anchor coat agent.

[0065] The substrate may have a printed layer on its surface. The image formed on the printed layer is not particularly limited, and may be a character, a pattern, a symbol, or a combination thereof. From the viewpoint of environmental impact, it is preferable that the printing layer is formed on the substrate using ink made from raw materials derived from biomass (resin materials such as polyolefin and polyester). Examples of biomass-derived inks include Finart BM manufactured by DIC Graphics Corporation and XA-55 manufactured by Sakata Inx Corporation. The method for forming the printed layer is not particularly limited, and examples of the method include conventionally known printing methods such as gravure printing, offset printing, flexographic printing, etc. Among these, flexographic printing is preferred from the viewpoint of environmental load.

[0066] The thickness of the substrate is preferably 10 μm or more and 50 μm or less, more preferably 15 μm or more and 30 μm or less. By making the thickness of the substrate 10 μm or more, the strength and heat resistance can be further improved. In addition, by making the thickness of the substrate 50 μm or less, the processability of the laminate including the substrate can be improved. Furthermore, when the substrate contains a white pigment, the visibility of the image formed on the substrate can be improved. Also, the contents filled in the packaging material produced using the laminate of the present invention can be more concealed. Also, the light-shielding property of the laminate can be more improved.

[0067] In one embodiment, the substrate may have a vapor-deposited film on the surface thereof on the dry laminate layer side, thereby improving the gas barrier properties, specifically the oxygen barrier properties and water vapor barrier properties, of the laminate. When the contents to be filled into a packaging material produced using the laminate of the present invention are detergents, shampoos, or the like, the barrier properties are not required, and from the viewpoint of the processability of the laminate, it is preferable that the laminate does not have a vapor-deposited film.

[0068] Examples of the vapor-deposited film include vapor-deposited films composed of metals such as aluminum, and inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, and barium oxide.

[0069] The thickness of the evaporated film is preferably 1 nm or more and 150 nm or less, more preferably 5 nm or more and 60 nm or less, and even more preferably 10 nm or more and 40 nm or less. By making the thickness of the vapor-deposited film 1 nm or more, the oxygen barrier property and water vapor barrier property of the laminate can be further improved. Also, by making the thickness of the vapor-deposited film 150 nm or less, the occurrence of cracks in the vapor-deposited film can be prevented. Also, the recyclability of the laminate can be maintained.

[0070] In one embodiment, the substrate has a barrier coat layer on the surface on the dry laminate layer side, which can improve the oxygen barrier property and water vapor barrier property of the laminate. When the substrate has a vapor-deposited film, the barrier coat layer may be provided on or under the vapor-deposited film.

[0071] In one embodiment, the barrier coat layer contains a gas barrier resin such as an ethylene-vinyl alcohol copolymer (EVOH), polyvinyl alcohol, polyacrylonitrile, polyamide such as nylon 6, nylon 6,6, and polymetaxylylene adipamide (MXD6), polyester, polyurethane, and (meth)acrylic resin. Among these, polyvinyl alcohol is preferred from the viewpoint of oxygen barrier property and water vapor barrier property. Furthermore, when the vapor-deposited film is made of an inorganic oxide, the occurrence of cracks in the vapor-deposited film can be effectively prevented by including polyvinyl alcohol in the barrier coat layer.

[0072] The content of the gas barrier resin in the barrier coat layer is preferably 50% by mass or more and 95% by mass or less, and more preferably 75% by mass or more and 90% by mass or less. By making the content of the gas barrier resin in the barrier coat layer 50% by mass or more, the oxygen barrier property and water vapor barrier property of the substrate can be further improved.

[0073] The barrier coat layer may contain the above-mentioned additives to the extent that the characteristics of the present invention are not impaired.

[0074] The thickness of the barrier coat layer is preferably 0.01 μm or more and 10 μm or less, and more preferably 0.1 μm or more and 5 μm or less. By making the thickness of the barrier coat layer 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the laminate can be further improved, and by making the thickness of the barrier coat layer 10 μm or less, the recyclability of the laminate can be maintained.

[0075] The barrier coat layer can be formed by dissolving or dispersing the above-mentioned material in water or a suitable solvent, applying the solution, and drying the solution. Alternatively, the barrier coat layer can be formed by applying a commercially available barrier coat agent and drying the solution.

[0076] In another embodiment, the barrier coat layer is a gas barrier coating film containing at least one resin composition such as a hydrolysate of a metal alkoxide or a hydrolyzed condensate of a metal alkoxide obtained by polycondensing a mixture of a metal alkoxide and a water-soluble polymer by a sol-gel method in the presence of a sol-gel catalyst, water, an organic solvent, etc. When the substrate has a vapor-deposited film made of an inorganic oxide, the barrier coat layer of this type is provided adjacent to the vapor-deposited film, thereby making it possible to effectively prevent cracks from occurring in the vapor-deposited film.

[0077] In one embodiment, the metal alkoxide is represented by the following general formula: R 1 n M(OR 2 ) m (In the formula, R 1 , R 2 each represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M.

[0078] As the metal atom M, for example, silicon, zirconium, titanium, aluminum, etc. can be used. Also, R 1 and R 2 Examples of the organic group represented by the formula (I) include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, and an i-butyl group.

[0079] Examples of metal alkoxides that satisfy the above general formula include tetramethoxysilane (Si(OCH3)4), tetraethoxysilane (mass %) Si(OC2H5)4), tetrapropoxysilane (Si(OC3H7)4), and tetrabutoxysilane (Si(OC4H9)4).

[0080] It is also preferable to use a silane coupling agent together with the metal alkoxide. As the silane coupling agent, known organic reactive group-containing organoalkoxysilanes can be used, and in particular, organoalkoxysilanes having epoxy groups are preferred. As organoalkoxysilanes having epoxy groups, for example, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane can be mentioned.

[0081] Two or more of the above silane coupling agents may be used, and the silane coupling agent is preferably used in an amount within the range of about 1 to 20 parts by mass per 100 parts by mass of the total amount of the alkoxide.

[0082] As the water-soluble polymer, polyvinyl alcohol and an ethylene-vinyl alcohol copolymer are preferred, and from the viewpoints of oxygen barrier properties, water vapor barrier properties, water resistance and weather resistance, it is preferred to use these in combination.

[0083] The content of the water-soluble polymer in the gas barrier coating film is preferably 5 parts by mass or more and 500 parts by mass or less per 100 parts by mass of the metal alkoxide. By making the content of the water-soluble polymer in the gas barrier coating film 5 parts by mass or more per 100 parts by mass of the metal alkoxide, the oxygen barrier property and water vapor barrier property of the laminate can be further improved. Also, by making the content of the water-soluble polymer in the gas barrier coating film 500 parts by mass or less per 100 parts by mass of the metal alkoxide, the film formability of the gas barrier coating film can be improved.

[0084] The thickness of the gas barrier coating film is preferably from 0.01 μm to 100 μm, and more preferably from 0.1 μm to 50 μm, which can improve the oxygen barrier property and water vapor barrier property while maintaining recyclability. By making the thickness of the gas barrier coating film 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the laminate can be improved. In addition, when the gas barrier coating film is provided adjacent to a vapor deposition film made of an inorganic oxide, the occurrence of cracks in the vapor deposition film can be prevented.

[0085] The gas barrier coating film can be formed by applying a composition containing the above-mentioned materials by a conventionally known means such as roll coating using a gravure roll coater or the like, spray coating, spin coating, dipping, brushing, bar coding, or an applicator, and then polycondensing the composition by a sol-gel method. As the sol-gel catalyst, an acid or an amine compound is preferable. As the amine compound, a tertiary amine that is substantially insoluble in water and soluble in an organic solvent is preferable, and examples thereof include N,N-dimethylbenzylamine, tripropylamine, tributylamine, and tripentylamine. Among these, N,N-dimethylbenzylamine is preferable. The sol-gel catalyst is preferably used in the range of 0.01 to 1.0 part by mass, and more preferably 0.03 to 0.3 part by mass, per 100 parts by mass of the metal alkoxide. By using a sol-gel catalyst in an amount of 0.01 part by mass or more per 100 parts by mass of the metal alkoxide, the catalytic effect can be improved, and by using a sol-gel catalyst in an amount of 1.0 part by mass or less per 100 parts by mass of the metal alkoxide, the thickness of the gas barrier coating film formed can be made uniform.

[0086] The composition may further contain an acid, which is used as a catalyst in the sol-gel process, mainly for the hydrolysis of alkoxides, silane coupling agents, and the like. The acid may be a mineral acid such as sulfuric acid, hydrochloric acid, or nitric acid, or an organic acid such as acetic acid, tartaric acid, etc. The amount of the acid used is preferably 0.001 mol or more and 0.05 mol or less based on the total molar amount of the alkoxide and the alkoxide portion (e.g., silicate portion) of the silane coupling agent. The amount of acid used is 0.001 moles or more relative to the total molar amount of the alkoxide and the alkoxide portion (e.g., silicate portion) of the silane coupling agent, thereby improving the catalytic effect. Also, the amount of acid used is 0.05 moles or less relative to the total molar amount of the alkoxide and the alkoxide portion (e.g., silicate portion) of the silane coupling agent, thereby making the thickness of the gas barrier coating film formed uniform.

[0087] The composition preferably contains water in an amount of 0.1 to 100 moles, more preferably 0.8 to 2 moles, per mole of the total molar amount of the alkoxides. By controlling the water content to 0.1 moles or more per mole of the total molar amount of the alkoxides, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be improved. Also, by controlling the water content to 100 moles or more per mole of the total molar amount of the alkoxides, the hydrolysis reaction can be carried out quickly.

[0088] The composition may also contain an organic solvent, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, or n-butanol.

[0089] Hereinafter, one embodiment of the method for forming a gas barrier coating film will be described. First, a composition is prepared by mixing a metal alkoxide, a water-soluble polymer, a sol-gel catalyst, water, an organic solvent, and optionally a silane coupling agent, etc. In the composition, a polycondensation reaction gradually proceeds. Next, the composition is applied onto a substrate by the above-mentioned conventionally known method and dried. This drying process further advances the polycondensation reaction between the alkoxide and the water-soluble polymer (and the silane coupling agent, if the composition contains a silane coupling agent) to form a composite polymer layer. Finally, the composition is heated at a temperature of 20 to 250° C., preferably 50 to 220° C., for 1 second to 10 minutes to form a gas barrier coating film.

[0090] The barrier coat layer may have a printed layer formed thereon. The method for forming the printed layer is as described above.

[0091] The substrate can be produced by forming a resin composition containing at least polyethylene into a resin film using a T-die method, an inflation method or the like, and then stretching and / or irradiating it with electron beams. By forming the film by the inflation method, the resin film can be stretched at the same time. When the resin film is stretched and irradiated with electron beams at the same time, either one may be carried out first, but from the standpoint of suitability for stretch processing, it is preferable to carry out the stretching first.

[0092] When the substrate is produced by the T-die method, the MFR of the resin composition is preferably 3 g / 10 min or more and 20 g / 10 min or less. By setting the MFR of the resin composition to 3 g / 10 min or more, the processability of the substrate can be improved, and by setting the MFR of the resin composition to 20 g / 10 min or less, the substrate can be prevented from breaking during stretching.

[0093] When the substrate is produced by an inflation method, the MFR of the resin composition is preferably 0.5 g / 10 min or more and 5 g / 10 min or less. By setting the MFR of the resin composition to 0.5 g / 10 min or more, the processability of the substrate can be improved, and by setting the MFR of the resin composition to 5 g / 10 min or less, the film-forming property can be improved.

[0094] The deposition film on the substrate can be formed by a conventional method, for example, physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.

[0095] Also, for example, a composite film consisting of two or more layers of vapor-deposited films of different inorganic oxides can be formed and used by combining both physical vapor deposition and chemical vapor deposition. The degree of vacuum in the vapor deposition chamber is 10 -2 ~10 -8 After oxygen is introduced, the pressure is preferably about 10 -1 ~10 -6 The pressure is preferably about mbar. The amount of oxygen introduced varies depending on the size of the deposition machine. For the oxygen to be introduced, an inert gas such as argon gas, helium gas, or nitrogen gas may be used as a carrier gas to the extent that no problems occur. The film transport speed can be about 10 to 800 m / min.

[0096] The surface of the deposited film is preferably subjected to the above-mentioned surface treatment, which can improve adhesion to adjacent layers.

[0097] (Sealant layer) In one embodiment, the sealant layer is made of the same material as the substrate, i.e., polyethylene or polypropylene, which can improve the recyclability of the laminate.

[0098] From the viewpoint of low-temperature heat sealability and drop resistance, the sealant layer preferably contains polyethylene, and more preferably contains low-density polyethylene, linear low-density polyethylene, and very low-density polyethylene. From the viewpoint of heat resistance, the sealant layer preferably contains polypropylene.

[0099] In order to improve the hand-tearability of a packaging material produced using the laminate of the present invention, the sealant layer preferably contains low-density polyethylene. Furthermore, in order to improve the drop strength of the packaging material produced using the laminate of the present invention, the sealant layer preferably contains linear low density polyethylene. Examples of linear low density polyethylene include C-4LLDPE and C-6LLDPE. From the viewpoint of the balance between tearability and impact strength, C-4LLDPE is preferred, and from the viewpoint of improving drop strength, C-6LLDPE is preferred. Preferably, the sealant layer comprises both C-4 LLDPE and C-6 LLDPE.

[0100] When the sealant layer contains low-density polyethylene and linear low-density polyethylene, the content of the low-density polyethylene is preferably 5% by mass or more and 20% by mass or less, and more preferably 9% by mass or more and 15% by mass or less. By making the content of the low-density polyethylene 5% by mass or more, the hand-tearability of the packaging material produced using the laminate of the present invention can be further improved. By making the content of the low-density polyethylene 20% by mass or less, the drop strength of the packaging material produced using the laminate of the present invention can be maintained. The content of the linear low density polyethylene is preferably 65% ​​by mass or more and 90% by mass or less, and more preferably 70% by mass or more and 80% by mass or less. By making the content of the linear low density polyethylene 65% by mass or more, the drop strength of the packaging material produced using the laminate of the present invention can be further improved. By making the content of the linear low density polyethylene 90% by mass or less, additives such as slip agents and antiblocking agents can be added, and a film of excellent quality with excellent processability can be obtained.

[0101] In one embodiment, the sealant layer comprises polyethylene or polypropylene derived from the biomass.

[0102] When the sealant layer contains biomass-derived polyethylene or polypropylene, the content thereof is preferably from 5% by mass to 100% by mass, and more preferably from 10% by mass to 70% by mass.

[0103] The sealant layer may also include mechanically recycled polyethylene, polypropylene, and the like.

[0104] In one embodiment, the sealant layer comprises the white pigment described above. The content of the white pigment in the sealant layer is preferably from 2% by mass to 15% by mass, and more preferably from 4% by mass to 10% by mass. By making the content of the white pigment in the sealant layer 2% by mass or more, the visibility of the image formed on the substrate can be improved. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be more concealed. In addition, the light-shielding property of the laminate can be more improved. Furthermore, by setting the content of the white pigment in the sealant layer to 15% by mass or less, a film can be obtained that does not impair the mechanical properties of the film and prevents an increase in costs.

[0105] The sealant layer may contain the above-mentioned additives as long as the characteristics of the present invention are not impaired.

[0106] In one embodiment, the sealant layer has a multi-layer structure. In the sealant layer having a multi-layer structure, the biomass-derived polyethylene or polypropylene and the white pigment may be contained in at least one layer. From the viewpoint of adhesion to adjacent layers and heat sealability, it is preferable that the intermediate layer contains a white pigment. For example, it is composed of a lamination layer that is laminated to a substrate, an intermediate layer containing a white pigment, and a heat seal layer.

[0107] In one embodiment, the intermediate sealant layer of the multi-layer sealant layer contains at least one of medium density polyethylene and high density polyethylene, which can further improve the strength of the laminate of the present invention. Specific examples of intermediate layers containing at least one of medium-density polyethylene and high-density polyethylene include a layer containing at least one of low-density polyethylene, linear low-density polyethylene, and very-low-density polyethylene, a layer containing at least one of medium-density polyethylene and high-density polyethylene, and a layer containing at least one of low-density polyethylene, linear low-density polyethylene, and very-low-density polyethylene. By adopting the above-mentioned configuration, the bag-making suitability and strength of the laminate of the present invention can be further improved while maintaining the heat sealability.

[0108] The thickness of the sealant layer is preferably 40 μm or more and 180 μm or less, more preferably 80 μm or more and 150 μm or less. This can further improve the heat sealability of the laminate of the present invention. In addition, when the sealant layer contains a white pigment, the visibility of the image formed on the substrate can be further improved. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be further concealed. In addition, the light-shielding property of the laminate can be further improved.

[0109] (adhesive layer) The adhesive layer may be formed from a conventionally known adhesive, which may be a one-component curing type, a two-component curing type, or a non-curing type. The adhesive may be either a solvent-free adhesive or a solvent-based adhesive, but from the standpoint of environmental impact, a solvent-free adhesive is preferably used. Examples of solvent-free adhesives include polyether adhesives, polyester adhesives, silicone adhesives, epoxy adhesives, and urethane adhesives, and among these, two-component curing urethane adhesives can be preferably used. Examples of the solvent-based adhesive include rubber-based adhesives, vinyl-based adhesives, silicone-based adhesives, epoxy-based adhesives, phenol-based adhesives, and olefin-based adhesives.

[0110] In addition, the adhesive layer is preferably formed of an adhesive using a raw material derived from biomass, which makes it possible to more effectively reduce the environmental impact of the packaging material produced using the laminate of the present invention. Examples of such adhesives include Adlock RU-80 manufactured by Rock Paint, ECOAD manufactured by Toyo Ink Co., Ltd., and HA-233B-EM manufactured by DIC Graphics Corporation.

[0111] Furthermore, when the laminate of the present invention includes an aluminum vapor-deposited film, the adhesive layer provided adjacent to the aluminum vapor-deposited film preferably comprises a cured product of a resin composition containing a polyester polyol and an isocyanate compound. When forming a laminate with a vapor-deposited film into a packaging material, a bending load is applied to the laminate by a molding machine or the like, which may cause cracks in the aluminum vapor-deposited film. By configuring the adhesive layer as described above, it is possible to prevent cracks from occurring in the aluminum vapor-deposited film, and even if cracks do occur, it is possible to suppress a decrease in the oxygen barrier property and water vapor barrier property (flexural load resistance).

[0112] The polyester polyol has two or more hydroxyl groups as functional groups in one molecule. The isocyanate compound has two or more isocyanate groups as functional groups in one molecule. The polyester polyol has, for example, a polyester structure or a polyester polyurethane structure as a main skeleton.

[0113] As a specific example of a resin composition (adhesive) containing a polyester polyol and an isocyanate compound, the PASLIM series sold by DIC Corporation can be used.

[0114] The resin composition may further contain a plate-like inorganic compound, a coupling agent, cyclodextrin and / or a derivative thereof, and the like.

[0115] As the polyester polyol having two or more hydroxyl groups in one molecule as a functional group, for example, the following [First Example] to [Third Example] can be used. [Example 1] Polyester polyol obtained by polycondensation of ortho-oriented polycarboxylic acid or its anhydride with polyhydric alcohol [Example 2] Polyester polyol with glycerol structure [Example 3] Polyester polyol with isocyanuric ring Each polyester polyol will be described below.

[0116] The polyester polyol according to the first example is a polycondensate obtained by polycondensing a polycarboxylic acid component containing at least one or more types of orthophthalic acid and its anhydride, and a polyhydric alcohol component containing at least one type selected from the group consisting of ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol, and cyclohexanedimethanol. In particular, polyester polyols in which the content of orthophthalic acid or its anhydride in the total polyvalent carboxylic acid components is 70 to 100 mass % are preferred.

[0117] The polyester polyol according to the first example essentially contains orthophthalic acid and its anhydride as the polycarboxylic acid component, but may be copolymerized with other polycarboxylic acid components as long as the effect of the present embodiment is not impaired. Specifically, the polybasic acids include aliphatic polybasic carboxylic acids such as succinic acid, adipic acid, azelaic acid, sebacic acid, and dodecane dicarboxylic acid, unsaturated bond-containing polybasic carboxylic acids such as maleic anhydride, maleic acid, and fumaric acid, alicyclic polybasic carboxylic acids such as 1,3-cyclopentane dicarboxylic acid and 1,4-cyclohexane dicarboxylic acid, aromatic polybasic carboxylic acids such as terephthalic acid, isophthalic acid, pyromellitic acid, trimellitic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, naphthalic acid, biphenyl dicarboxylic acid, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, anhydrides of these dicarboxylic acids, and ester-forming derivatives of these dicarboxylic acids, p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, and ester-forming derivatives of these dihydroxycarboxylic acids. Among these, succinic acid, 1,3-cyclopentane dicarboxylic acid, and isophthalic acid are preferred. Two or more of the above other polyvalent carboxylic acids may be used.

[0118] As a polyester polyol according to a second example, a polyester polyol having a glycerol skeleton represented by general formula (1) can be mentioned. [ka] In general formula (1), R1, R2, and R3 each independently represent H (hydrogen atom) or a group represented by the following general formula (2). [ka]

[0119] In formula (2), n represents an integer of 1 to 5, X represents an arylene group selected from the group consisting of 1,2-phenylene groups, 1,2-naphthylene groups, 2,3-naphthylene groups, 2,3-anthraquinonediyl groups, and 2,3-anthracenediyl groups, which may have a substituent, and Y represents an alkylene group having 2 to 6 carbon atoms. However, at least one of R1, R2, and R3 represents a group represented by general formula (2).

[0120] In general formula (1), at least one of R1, R2, and R3 must be a group represented by general formula (2). In particular, it is preferable that all of R1, R2, and R3 are groups represented by general formula (2).

[0121] In addition, the compound may be a mixture of two or more of a compound in which any one of R1, R2, and R3 is a group represented by general formula (2), a compound in which any two of R1, R2, and R3 are groups represented by general formula (2), and a compound in which all of R1, R2, and R3 are groups represented by general formula (2).

[0122] X represents an optionally substituted arylene group selected from the group consisting of a 1,2-phenylene group, a 1,2-naphthylene group, a 2,3-naphthylene group, a 2,3-anthraquinonediyl group, and a 2,3-anthracenediyl group. When X is substituted, it may be substituted with one or more substituents, and the substituent is attached to any carbon atom on X other than the free radical. The substituents include a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimido group, a carboxyl group, a carbamoyl group, a N-ethylcarbamoyl group, a phenyl group, and a naphthyl group.

[0123] In the general formula (2), Y represents an alkylene group having 2 to 6 carbon atoms, such as an ethylene group, a propylene group, a butylene group, a neopentylene group, a 1,5-pentylene group, a 3-methyl-1,5-pentylene group, a 1,6-hexylene group, a methylpentylene group, or a dimethylbutylene group. Among these, Y is preferably a propylene group or an ethylene group, and most preferably an ethylene group.

[0124] The polyester resin compound having a glycerol skeleton represented by general formula (1) can be synthesized by reacting glycerol, an aromatic polycarboxylic acid or its anhydride in which a carboxylic acid is substituted at the ortho position, and a polyhydric alcohol component as essential components.

[0125] Examples of aromatic polycarboxylic acids or anhydrides in which a carboxylic acid is substituted at the ortho position include orthophthalic acid or anhydride, naphthalene 2,3-dicarboxylic acid or anhydride, naphthalene 1,2-dicarboxylic acid or anhydride, anthraquinone 2,3-dicarboxylic acid or anhydride, and 2,3-anthracene carboxylic acid or anhydride. These compounds may have a substituent at any carbon atom of the aromatic ring, such as a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimido group, a carboxyl group, a carbamoyl group, an N-ethylcarbamoyl group, a phenyl group, or a naphthyl group.

[0126] Examples of the polyhydric alcohol component include alkylene diols having 2 to 6 carbon atoms, such as ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, methylpentanediol, and dimethylbutanediol.

[0127] The polyester polyol according to the third example is a polyester polyol having an isocyanuric ring represented by the following general formula (3). [ka] In the general formula (3), R1, R2, and R3 each independently represent "-(CH2)n1-OH (wherein n1 represents an integer of 2 to 4)" or a structure represented by the general formula (4). [ka]

[0128] In the general formula (4), n2 represents an integer of 2 to 4, n3 represents an integer of 1 to 5, X represents an arylene group selected from the group consisting of a 1,2-phenylene group, a 1,2-naphthylene group, a 2,3-naphthylene group, a 2,3-anthraquinonediyl group, and a 2,3-anthracenediyl group, which may have a substituent, and Y represents an alkylene group having 2 to 6 carbon atoms. However, at least one of R1, R2, and R3 is a group represented by the general formula (4).

[0129] In the general formula (3), the alkylene group represented by -(CH2)n1- may be linear or branched. Among them, n1 is preferably 2 or 3, and most preferably 2.

[0130] In the general formula (4), n2 represents an integer of 2 to 4; n3 represents an integer of 1 to 5. X represents an optionally substituted arylene group selected from the group consisting of a 1,2-phenylene group, a 1,2-naphthylene group, a 2,3-naphthylene group, a 2,3-anthraquinonediyl group, and a 2,3-anthracenediyl group.

[0131] When X is substituted, it may be substituted with one or more substituents, and the substituent is attached to any carbon atom on X other than the free radical. The substituents include a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimido group, a carboxyl group, a carbamoyl group, a N-ethylcarbamoyl group, a phenyl group, and a naphthyl group. The substituent for X is preferably a hydroxyl group, a cyano group, a nitro group, an amino group, a phthalimido group, a carbamoyl group, an N-ethylcarbamoyl group, or a phenyl group, and most preferably a hydroxyl group, a phenoxy group, a cyano group, a nitro group, a phthalimido group, or a phenyl group.

[0132] In the general formula (4), Y represents an alkylene group having 2 to 6 carbon atoms, such as an ethylene group, a propylene group, a butylene group, a neopentylene group, a 1,5-pentylene group, a 3-methyl-1,5-pentylene group, a 1,6-hexylene group, a methylpentylene group, or a dimethylbutylene group. Among these, Y is preferably a propylene group or an ethylene group, and most preferably an ethylene group.

[0133] In general formula (3), at least one of R1, R2, and R3 is a group represented by general formula (4). Of these, it is preferable that all of R1, R2, and R3 are groups represented by general formula (4).

[0134] In addition, the compound may be a mixture of two or more of a compound in which any one of R1, R2, and R3 is a group represented by general formula (4), a compound in which any two of R1, R2, and R3 are groups represented by general formula (4), and a compound in which all of R1, R2, and R3 are groups represented by general formula (4).

[0135] The polyester polyol having an isocyanuric ring represented by the general formula (3) can be synthesized by reacting a triol having an isocyanuric ring, an aromatic polycarboxylic acid or its anhydride in which a carboxylic acid is substituted at the ortho position, and a polyhydric alcohol component as essential components.

[0136] Examples of triols having an isocyanuric ring include alkylene oxide adducts of isocyanuric acid such as 1,3,5-tris(2-hydroxyethyl)isocyanuric acid and 1,3,5-tris(2-hydroxypropyl)isocyanuric acid.

[0137] Examples of aromatic polycarboxylic acids or anhydrides in which a carboxylic acid is substituted at the ortho position include orthophthalic acid or anhydride, naphthalene 2,3-dicarboxylic acid or anhydride, naphthalene 1,2-dicarboxylic acid or anhydride, anthraquinone 2,3-dicarboxylic acid or anhydride, and 2,3-anthracene carboxylic acid or anhydride, etc. These compounds may have a substituent on any carbon atom of the aromatic ring.

[0138] Examples of the substituent include a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimido group, a carboxyl group, a carbamoyl group, an N-ethylcarbamoyl group, a phenyl group, and a naphthyl group.

[0139] The polyhydric alcohol component may be an alkylene diol having 2 to 6 carbon atoms, such as ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, methylpentanediol, and dimethylbutanediol. Among these, polyester polyol compounds having an isocyanuric ring, which use 1,3,5-tris(2-hydroxyethyl)isocyanuric acid or 1,3,5-tris(2-hydroxypropyl)isocyanuric acid as a triol compound having an isocyanuric ring, orthophthalic anhydride as an aromatic polycarboxylic acid or its anhydride in which a carboxylic acid is substituted at the ortho position, and ethylene glycol as a polyhydric alcohol, are particularly excellent in oxygen barrier properties and adhesion and are therefore preferred.

[0140] The isocyanuric ring is highly polar and trifunctional, and can increase the polarity of the entire system and increase the crosslink density. From this viewpoint, it is preferable that the adhesive resin contains 5% by mass or more of the isocyanuric ring based on the total solid content of the adhesive resin.

[0141] The isocyanate compound has two or more isocyanate groups in the molecule. The isocyanate compound may be either aromatic or aliphatic, and may be either a low molecular weight compound or a high molecular weight compound. Furthermore, the isocyanate compound may be a blocked isocyanate compound obtained by subjecting a known isocyanate blocking agent to an addition reaction by a known, conventional appropriate method. Among these, from the viewpoints of adhesiveness and retort resistance, polyisocyanate compounds having three or more isocyanate groups are preferred, and from the viewpoints of oxygen barrier property and water vapor barrier property, aromatic compounds are preferred.

[0142] Specific examples of the isocyanate compound include tetramethylene diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, metaxylylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, and trimers of these isocyanate compounds, as well as adducts, biurets, and allophanates obtained by reacting these isocyanate compounds with low-molecular-weight active hydrogen compounds or their alkylene oxide adducts, or high-molecular-weight active hydrogen compounds. Examples of low molecular weight active hydrogen compounds include ethylene glycol, propylene glycol, metaxylylene alcohol, 1,3-bishydroxyethylbenzene, 1,4-bishydroxyethylbenzene, trimethylolpropane, glycerol, pentaerythritol, erythritol, sorbitol, ethylenediamine, monoethanolamine, diethanolamine, triethanolamine, and metaxylylenediamine. Examples of molecular weight active hydrogen compounds include polymeric active hydrogen compounds such as various polyester resins, polyether polyols, and polyamides.

[0143] The resin composition may contain a phosphoric acid-modified compound in addition to the polyester polyol and the isocyanate compound, and is, for example, a compound represented by the following general formula (5) or (6). [ka] In general formula (5), R1, R2, and R3 are groups selected from a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, a (meth)acryloyl group, a phenyl group which may have a substituent, and an alkyl group having 1 to 4 carbon atoms which has a (meth)acryloyloxy group, at least one of which is a hydrogen atom, and n is an integer of 1 to 4. [ka] In the formula, R4 and R5 are groups selected from a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, a (meth)acryloyl group, a phenyl group which may have a substituent, and an alkyl group having 1 to 4 carbon atoms and having a (meth)acryloyloxy group, n is an integer of 1 to 4, x is an integer of 0 to 30, and y is an integer of 0 to 30, except for the case where both x and y are 0.

[0144] More specific examples include phosphoric acid, pyrophosphoric acid, triphosphoric acid, methyl acid phosphate, ethyl acid phosphate, butyl acid phosphate, dibutyl phosphate, 2-ethylhexyl acid phosphate, bis(2-ethylhexyl) phosphate, isododecyl acid phosphate, butoxyethyl acid phosphate, oleyl acid phosphate, tetracosyl acid phosphate, 2-hydroxyethyl methacrylate acid phosphate, and polyoxyethylene alkyl ether phosphate, and one or more of these can be used.

[0145] The content of the phosphoric acid-modified compound in the resin composition is preferably from 0.005% by mass to 10% by mass, and more preferably from 0.01% by mass to 1% by mass. By making the content of the phosphoric acid-modified compound 0.005% by mass or more, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be improved, and by making the content of the phosphoric acid-modified compound 10% by mass or less, the adhesiveness of the adhesive layer can be improved.

[0146] The resin composition containing the polyester polyol and the isocyanate compound may contain a plate-like inorganic compound, which can improve the adhesiveness of the adhesive layer and the bending load resistance of the laminate of the present invention. Examples of the plate-like inorganic compounds include kaolinite-serpentine group clay minerals (such as halloysite, kaolinite, endelite, dickite, nacrite, antigorite, and chrysotile) and pyrophyllite-talc group (such as pyrophyllite, talc, and keroli).

[0147] Examples of the coupling agent include silane-based coupling agents, titanium-based coupling agents, and aluminum-based coupling agents represented by the following general formula (7). These coupling agents may be used alone or in combination of two or more kinds. [ka]

[0148] Examples of silane coupling agents include vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-methacryloxytrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, N-β( aminoethyl) γ-aminopropyl methyl dimethoxysilane, N-β (aminoethyl) γ-aminopropyl trimethoxysilane, N-β (aminoethyl) γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, γ-chloropropyl trimethoxysilane, γ-mercaptopropyl trimethoxysilane, 3-isocyanatopropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane and 3-triethoxysilyl-N-(1,3-dimethyl-butylidene).

[0149] Examples of titanium-based coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, tetraoctyl bis(didodecyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyl trioctyl nor titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl isostearoyl diacryl titanate, diisostearoyl ethylene titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and dicumyl phenyl oxyacetate titanate.

[0150] Specific examples of aluminum-based coupling agents include acetoalkoxyaluminum diisopropylate, diisopropoxyaluminum ethyl acetoacetate, diisopropoxyaluminum monomethacrylate, isopropoxyaluminum alkyl acetoacetate mono(dioctyl phosphate), aluminum 2-ethylhexanoate oxide trimer, aluminum stearate oxide trimer, and alkyl acetoacetate aluminum oxide trimer.

[0151] The resin composition may contain cyclodextrin and / or a derivative thereof, which can improve the adhesiveness of the adhesive layer and can further improve the bending load resistance of the laminate of the present invention. Specifically, for example, cyclodextrin, alkylated cyclodextrin, acetylated cyclodextrin, hydroxyalkylated cyclodextrin, and other cyclodextrins in which the hydrogen atom of the hydroxyl group of the glucose unit of cyclodextrin is substituted with another functional group can be used. Branched cyclic dextrins can also be used. Furthermore, the cyclodextrin skeleton in cyclodextrin and cyclodextrin derivatives may be any of α-cyclodextrin consisting of six glucose units, β-cyclodextrin consisting of seven glucose units, and γ-cyclodextrin consisting of eight glucose units. These compounds may be used alone or in combination of two or more. Hereinafter, these cyclodextrins and / or their derivatives may be collectively referred to as dextrin compounds.

[0152] From the viewpoint of compatibility and dispersibility in the resin composition, it is preferable to use a cyclodextrin derivative as the cyclodextrin compound.

[0153] Examples of alkylated cyclodextrins include methyl-α-cyclodextrin, methyl-β-cyclodextrin, and methyl-γ-cyclodextrin. These compounds may be used alone or in combination of two or more.

[0154] Examples of acetylated cyclodextrin include monoacetyl-α-cyclodextrin, monoacetyl-β-cyclodextrin, and monoacetyl-γ-cyclodextrin. These compounds may be used alone or in combination of two or more.

[0155] Examples of hydroxyalkylated cyclodextrins include hydroxypropyl-α-cyclodextrin, hydroxypropyl-β-cyclodextrin, and hydroxypropyl-γ-cyclodextrin, etc. These compounds may be used alone or in combination of two or more kinds.

[0156] As long as the properties of the present invention are not impaired, the adhesive layer may contain additives such as pigments such as titanium oxide, zinc oxide and carbon black, dyes such as disperse dyes, acid dyes and cationic dyes, antioxidants, lubricants, colorants, stabilizers, wetting agents, thickeners, coagulants, gelling agents, anti-settling agents, softeners, hardeners, plasticizers, leveling agents, ultraviolet absorbers and flame retardants.

[0157] The thickness of the adhesive layer is not particularly limited, and can be, for example, 1 μm or more and 5 μm or less.

[0158] (Middle class) In one embodiment, the laminate of the present invention comprises as an intermediate layer a layer composed of polyethylene or polypropylene.

[0159] In one embodiment, the intermediate layer may contain the white pigment. The content of the white pigment in the polyethylene layer is preferably from 0.5% by mass to 20% by mass, and more preferably from 2% by mass to 10% by mass. By making the content of the white pigment in the intermediate layer 2% by mass or more, when an image is formed on a substrate, the visibility of the image can be further improved. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be more concealed. In addition, the light-shielding property of the laminate can be further improved. Furthermore, by setting the content of the white pigment in the intermediate layer to 15% by mass or less, a film can be obtained that does not impair the mechanical properties of the film and prevents an increase in costs.

[0160] The intermediate layer may be composed of a stretched film, and may be a uniaxially stretched film or a biaxially stretched film, and the preferred stretch ratio is as described above. The intermediate layer may also be an extruded resin layer formed by melt extruding polyethylene or polypropylene.

[0161] The thickness of the intermediate layer made of polyethylene or polypropylene is preferably 10 μm or more and 70 μm or less, and more preferably 15 μm or more and 50 μm or less. When the intermediate layer contains a white pigment, the visibility of an image formed on a substrate can be improved. In addition, the contents filled in a packaging material produced using the laminate of the present invention can be more concealed. In addition, the light-shielding property of the laminate can be more improved.

[0162] In one embodiment, the laminate of the present invention includes, as an intermediate layer, a gas barrier layer made of a gas barrier resin. By providing the laminate of the present invention with such an intermediate layer, the oxygen barrier property and water vapor barrier property can be improved. Examples of gas barrier resins include ethylene-vinyl alcohol copolymers (EVOH), polyvinyl alcohol, polyacrylonitrile, polyamides such as nylon 6, nylon 6,6 and polymetaxylylene adipamide (MXD6), polyesters, polyurethanes, and (meth)acrylic resins.

[0163] In one embodiment, the gas barrier layer may contain the above-mentioned white pigment. The content of the white pigment in the gas barrier layer is preferably from 1% by mass to 10% by mass, and more preferably from 2% by mass to 8% by mass. By making the content of the white pigment in the gas barrier layer 1% by mass or more, when an image is formed on a substrate, the visibility of the image can be improved. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be more concealed. In addition, the light blocking property of the laminate can be more improved. Furthermore, by setting the content of the white pigment in the gas barrier layer to 10% by mass or less, the whiteness of the gas barrier layer can be improved while maintaining the gas barrier properties.

[0164] The thickness of the gas barrier layer is preferably from 0.01 μm to 10 μm, and more preferably from 0.1 μm to 5 μm. By making the thickness of the gas barrier layer 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be further improved, and by making the thickness of the gas barrier layer 10 μm or less, the recyclability of the laminate of the present invention can be maintained. In addition, when the intermediate layer contains a white pigment, the visibility of an image formed on a substrate can be improved. In addition, the contents filled in a packaging material produced using the laminate of the present invention can be more concealed. In addition, the light-shielding property of the laminate can be more improved.

[0165] In one embodiment, the intermediate layer comprises a vapor-deposited film. The form, preferred thickness, and formation method of the vapor-deposited film that can be used are as described above.

[0166] In one embodiment, the intermediate layer comprises a barrier coat layer, the configuration, preferred thickness, forming method, etc. of which are as described above.

[0167] (Laminate in the second embodiment) In a second embodiment, the laminate of the present invention comprises a substrate, an intermediate layer and a sealant layer, which are characterized in that they are made of the same material, namely polyethylene or polypropylene. In the present invention, at least the intermediate layer contains a white pigment. According to such an embodiment, the printability to the substrate and the heat sealability of the sealant layer can be maintained, and the visibility of the image formed on the substrate can be improved. In addition, the contents filled in the packaging material produced using the laminate of the present invention can be concealed. In addition, the light-shielding property of the laminate can be improved. Furthermore, in the present invention, at least one of the substrate, intermediate layer and sealant layer contains biomass-derived polyethylene or biomass-derived polypropylene, which can reduce the environmental impact of packaging materials produced using the laminate of the present invention.

[0168] The laminate of the present invention may further include an adhesive layer between any of the layers.

[0169] The configurations of the substrate, intermediate layer, sealant layer and adhesive layer in the laminate of the second embodiment are similar to those of the laminate of the first embodiment, and therefore detailed description thereof will be omitted here.

[0170] (packaging material) The packaging material of the present invention is characterized in that it is composed of the above-mentioned laminate. The shape of the packaging material is not particularly limited, and may be a bag-shaped stand-up pouch as shown in FIG.

[0171] In one embodiment, the packaging material 20 of the present invention may be a stand-up pouch equipped with a dispensing nozzle portion 21 as shown in FIG. 5 when the contents are liquid, viscous material, or powder such as detergent or shampoo. From the viewpoint of ease of opening, the packaging material 20 may have a curved portion 22 that is curved inward, as shown in FIG. Additionally, cutouts 23 may be provided, such as those formed by a laser beam.

[0172] In one embodiment, the packaging material 30 of the present invention may be a stand-up pouch having a spout 32 interposed by an upper edge seal portion 31, as shown in Figure 6. A lid plug 33 is screwed onto the upper end of the spout 32.

[0173] In addition, the hatched areas represent heat-sealed areas in Figures 4 to 6. In addition, although a stand-up pouch is shown as an example of the packaging material in Figures 4 to 6, the packaging material is not limited to this.

[0174] In one embodiment, the packaging material can be produced by folding the laminate of the present invention in half, overlapping it so that the sealant layer is on the inside, and heat sealing the ends. In another embodiment, the packaging material can also be produced by overlapping two laminates with the sealant layers facing each other and heat sealing the ends.

[0175] In one embodiment, the packaging material can be produced by overlapping two of the above laminates with their sealant layers facing each other and heat-sealing two sides to form a body, and then folding another laminate into a V shape with the sealant layer on the outside, sandwiching it from one end of the body, and heat-sealing it to form a bottom.

[0176] In one embodiment, the packaging material can be produced by stacking two of the above-mentioned laminates with their sealant layers facing each other and heat-sealing one side to form a bottom, and then folding two more laminates into a V shape with the sealant layers facing outwards, sandwiching both ends of the facing laminate, and heat-sealing to form a body.

[0177] The heat sealing method is not particularly limited, and can be performed by a known method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, etc.

[0178] The contents filled in the packaging material are not particularly limited, and may be liquid, powder, or gel. In addition, the contents may be food or non-food. According to the packaging material of the present invention, even if the contents are colored, such as detergent, the image formed on the base material is not affected, and the contents can be suitably filled. EXAMPLES

[0179] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0180] Example 1 Biomass-derived polyethylene (biomass content 16%) was extruded using an inflation extruder to produce a polyethylene film with a thickness of 125 μm. This was then uniaxially stretched in the longitudinal direction to obtain a substrate film with a thickness of 25 μm. An image was formed on one side of the substrate using ink made from biomass-derived materials (biomass content 10%) with a gravure printer.

[0181] The resin composition containing the biomass-derived polyethylene and titanium oxide was extruded using an inflation extruder to produce a 140 μm-thick unstretched film for a sealant layer. The titanium oxide content was adjusted to 5% by mass.

[0182] The image forming surface of the substrate film and the unstretched film for the sealant layer were laminated together using an aromatic polyester polyurethane adhesive (manufactured by Rock Paint Co., Ltd., base material RU-80, curing agent H-5, blend ratio 15:1) that uses biomass-derived sepacic acid as part of the base material, to obtain a laminate of the present invention.

[0183] Example 2 A substrate film having a thickness of 25 μm was prepared in the same manner as in Example 1. An image was formed on one surface of the substrate film by a gravure printer using ink made of a biomass-derived material (biomass content: 10%).

[0184] The resin composition containing the biomass-derived polyethylene and titanium oxide was extruded using an inflation extruder to produce an unstretched film for intermediate layer having a thickness of 40 μm. The titanium oxide content was adjusted to 5% by mass. The image forming surface of the substrate film and the intermediate layer film were laminated together with the aromatic polyester polyurethane adhesive.

[0185] C6LLDPE (density: 0.919g / m 3 , MFR: 2.3 g / 10 min) 60.5 parts by mass, Biomass-derived polyethylene (density: 0.916 g / m 3 , MFR: 1.0 g / 10 min) 18.5 parts by mass, LDPE (density: 0.919g / m 3 , MFR: 2.0 g / 10 min) 20.0 parts by mass; LDPE-based additive (density: 0.921 g / m 3 1.0 part by mass of 1,2-dichlorophenyl ether (MFR: 5.4 g / 10 min) was mixed with 1.0 part by mass of 1,2-dichlorophenyl ether (MFR: 5.4 g / 10 min) to obtain a resin composition, which was then extruded using an inflation extruder to a thickness of 80 μm and a density of 0.918 g / m 3 An unstretched film for the sealant layer with a biomass content of 16% was produced.

[0186] The unstretched film for the sealant layer was laminated on the other surface of the unstretched film for the intermediate layer with the aromatic polyester polyurethane adhesive to obtain a laminate of the present invention.

[0187] Example 3 A substrate film having a thickness of 25 μm was prepared in the same manner as in Example 1. An image was formed on one surface of the substrate film by a gravure printer using ink made of a biomass-derived material (biomass content: 10%).

[0188] The resin composition containing the biomass-derived polyethylene and titanium oxide was extruded using an inflation extruder to produce an unstretched intermediate layer film having a thickness of 40 μm. The titanium oxide content was adjusted to 5 mass %. Both sides of the unstretched intermediate layer film were subjected to a corona treatment.

[0189] The image forming surface of the substrate film and the intermediate layer film were laminated together with the aromatic polyester polyurethane adhesive.

[0190] In the same manner as in Example 2, a 40 μm thick film for a sealant layer was prepared and laminated to the other surface of the unstretched intermediate layer film with the above-mentioned aromatic polyester polyurethane adhesive to obtain a laminate of the present invention.

[0191] Example 4 A substrate film having a thickness of 25 μm was prepared in the same manner as in Example 1. An image was formed on one surface of the substrate film by a gravure printer using ink made of a biomass-derived material (biomass content: 10%).

[0192] The resin composition containing the biomass-derived polyethylene and titanium oxide was extruded using an inflation extruder to produce an unstretched intermediate layer film having a thickness of 40 μm. The titanium oxide content was adjusted to 5 mass %. Both sides of the unstretched intermediate layer film were subjected to a corona treatment.

[0193] The image forming surface of the substrate film and the intermediate layer film were laminated together with the aromatic polyester polyurethane adhesive.

[0194] In the same manner as in Example 2, a 80 μm thick film for a sealant layer was prepared and laminated to the other surface of the unstretched intermediate layer film with the above-mentioned aromatic polyester polyurethane adhesive to obtain a laminate of the present invention.

[0195] Comparative Example 1 A laminate was produced in the same manner as in Example 1, except that titanium oxide was not used in producing the unstretched film for the sealant layer.

[0196] Comparative Example 2 A laminate was produced in the same manner as in Comparative Example 1, except that a 1 μm-thick white ink layer was provided on the image-forming surface of the substrate film in order to conceal the contents.

[0197] Comparative Example 3 A laminate was produced in the same manner as in Example 1, except that the substrate film was changed to an unstretched polyethylene film having a thickness of 25 μm.

[0198] <<Content Concealment Test>> The laminates produced in the above Examples and Comparative Examples were cut to a size of 220 mm length x 130 mm width. Two of the laminates cut as described above were stacked together with the sealant layers facing each other, and a laminate prepared in the above Examples and Comparative Examples was folded into a V shape at one end of the body so that the sealant layer was on the outside and sandwiched between the laminates. Next, the two vertical sides and the side sandwiching the V-shaped laminate were heat-sealed. The heat sealing temperature was 155°C. Moreover, in the laminate of Comparative Example 3, the heat resistance of the base film was insufficient, and heat sealing could not be performed.

[0199] Next, a carbon dioxide laser (Keyence, 3Axis-CO2 laser marker ML-Z9520A, output 70%, printing speed 1000 mm / min) was used to form the cutouts, and a pouring nozzle and curved part as shown in Figure 5 were formed by punching, producing a packaging material in the shape of a stand pouch with an opening. This packaging material was filled with 300 mL of blue liquid detergent, and the remaining side was heat sealed to form a package.

[0200] The packages prepared as described above were visually observed and evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1. (Evaluation Criteria) A: The color of the contents was not confirmed, confirming high content concealment ability. NG: The color of the contents was visible and affected the color of the image formed on the base material.

[0201] <<Laminate strength test>> The package produced as described above was cut in the machine direction of the film to a width of 15 mm to obtain a test piece. The interface between the base layer and the sealant layer or the base layer and the intermediate layer on this test side was peeled off, and the peeling was stopped halfway. Both ends of the test piece that had been peeled off halfway were pulled up and down at a test speed of 300 mm / min, and the stress at that time was measured to evaluate the laminate strength. The evaluation results are summarized in Table 1. (Evaluation Criteria) A: The white ink layer did not undergo cohesive failure and peeled off with a constant strength. NG: Peeling due to cohesive failure of the white ink layer was observed.

[0202] <<Hand tearability test>> The packages obtained in the above content concealment test were opened by hand, and the ease of opening was evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1. (Evaluation Criteria) A: I was able to open it with almost no force. NG: It was necessary to apply a strong force, which caused problems in practical use, such as stretching or tearing.

[0203] <<Drop strength test>> The package obtained in the above content concealment test was dropped 10 times from a height of 100 cm onto a hard floor with the body of the package horizontal to the ground. The test was carried out for 10 bags at a time, and the presence or absence of damage was visually observed, and the strength was evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1. A: No damage was found in any of the 10 bags. NG: Damage was confirmed in one or more of the 10 bags, making the product unusable.

[0204] [Table 1] [Explanation of symbols]

[0205] 10: laminate, 11: substrate, 12: sealant layer, 13: intermediate layer, 14: adhesive layer, 20: packaging material, 21: pouring nozzle portion, 22: curved portion, 23: cut-out portion, 30: packaging material, 31: upper edge seal portion, 32: spout, 33: lid stopper

Claims

1. A laminate comprising a multi-layer substrate and a sealant layer, the substrate and the sealant layer are made of the same material; The substrate has been subjected to at least one of a stretching treatment and an electron beam irradiation treatment, The same material is polyethylene or polypropylene; At least one of the substrate and the sealant layer comprises a white pigment; 13. A laminate, wherein at least one of the substrate and the sealant layer comprises biomass-derived polyethylene or biomass-derived polypropylene.

2. The substrate includes the white pigment, The laminate according to claim 1 , wherein the content of the white pigment in the base material is from 0.5% by mass to 20% by mass.

3. The laminate according to claim 2 , wherein the substrate has a thickness of 15 μm or more and 40 μm or less.

4. The sealant layer includes the white pigment, The laminate according to claim 1 , wherein the content of the white pigment in the sealant layer is from 2% by mass to 15% by mass.

5. The laminate according to claim 4 , wherein the sealant layer has a thickness of 40 μm or more and 180 μm or less.

6. A laminate comprising a multi-layer substrate, an intermediate layer, and a sealant layer, the substrate, the intermediate layer and the sealant layer are made of the same material; The substrate has been subjected to at least one of a stretching treatment and an electron beam irradiation treatment, The same material is polyethylene or polypropylene; The intermediate layer contains a white pigment, A laminate, wherein at least one of the substrate, intermediate layer and sealant layer contains biomass-derived polyethylene or biomass-derived polypropylene.

7. The laminate according to any one of claims 1 to 6, which is used for packaging material applications.

8. A packaging material comprising the laminate according to any one of claims 1 to 7.

9. The packaging material according to claim 8, further comprising a nozzle portion for extraction.

10. The packaging material of claim 8 comprising a spout.

Citation Information

Patent Citations

  • Gas barrier film, packaging material, package

    JP2009202519A