Optical film and polarizing plate
A polycarbonate resin-based optical film with specific properties addresses conveyance defects and enhances flexibility and shape processing, ensuring reduced bright spots and improved crack resistance for thin devices.
Patent Information
- Application Number
- JP2024125949
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thin films for devices like liquid crystal screens suffer from process defects during conveyance, bright spots when pressed, and insufficient flexibility, shape processing properties, and crack resistance.
An optical film containing a polycarbonate resin with specific properties, including in-plane retardation, puncture modulus, and breaking strength, is developed to suppress process defects and enhance flexibility and crack resistance.
The optical film achieves reduced process defects, suppresses bright spots, and exhibits excellent flexibility and shape processing properties, suitable for thin and bendable/foldable devices.
Smart Images

Figure 2024149635000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film and a polarizing plate. [Background technology]
[0002] In recent years, there has been an increasing demand for devices with liquid crystal screens, such as televisions and smartphones, to be made thinner. In order to achieve this, various thin films have been proposed. However, thin films may suffer from process defects such as creases, wrinkles, and dents during film transport. Furthermore, bright spots may occur when the film is pressed, and the film may have insufficient flexibility, irregular shape processing, or crack resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3325560 Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned conventional problems, and its object is to provide an optical film that suppresses the occurrence of process defects during transportation, suppresses the occurrence of bright spots when the film is pressed, and further has excellent flexibility, shape-processability, and crack resistance. [Means for solving the problem]
[0005] The optical film according to the embodiment of the present invention contains a polycarbonate resin, has an in-plane retardation Re(550) of 10 nm or less, Re(450) / Re(550) of 0.98 to 1.03, and a puncture modulus of 50 gf / mm or more. In one embodiment, the optical film has a puncture strength per unit thickness of 10 gf / μm or more. In one embodiment, the optical film has a breaking strength of 800 MPa or more and a breaking elongation of 3% or more. In one embodiment, the optical film has a thickness of 25 μm or less. In one embodiment, the optical film has an absolute value of a rate of change in in-plane retardation Re(550) after 500 hours under conditions of a temperature of 65° C. and a humidity of 90%, of 1% or less. In another embodiment of the present invention, a polarizing plate is provided. The polarizing plate includes a polarizer and the above-mentioned optical film attached to at least one surface of the polarizer via an adhesive layer. Effect of the Invention
[0006] According to an embodiment of the present invention, by containing a specific polycarbonate-based resin and setting the puncture modulus within a specific range, the occurrence of process defects during transportation can be suppressed, and an optical film with excellent flexibility can be realized. Furthermore, by setting the puncture strength, breaking strength, and breaking elongation per unit film thickness within specific ranges, the occurrence of bright spots when the film is pressed can be suppressed, and an optical film with excellent profile processability and crack resistance can be realized. [Brief description of the drawings]
[0007] [Figure 1] 4 is a schematic plan view illustrating an example of an irregular shape or irregularly processed portion in a polarizing plate according to an embodiment of the present invention. FIG. [Diagram 2] 10A to 10C are schematic plan views illustrating modified examples of irregular shapes or irregularly processed portions in a polarizing plate according to an embodiment of the present invention. [Diagram 3] 13A to 13C are schematic plan views illustrating further modified examples of the irregular shape or irregularly processed portion in the polarizing plate according to the embodiment of the present invention. [Figure 4] 13A to 13C are schematic plan views illustrating further modified examples of the irregular shape or irregularly processed portion in the polarizing plate according to the embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film).
[0010] A. Optical Film The optical film according to the embodiment of the present invention contains a polycarbonate resin.The optical film according to the embodiment of the present invention is typically a polycarbonate resin film.
[0011] The in-plane retardation Re(550) of the optical film is 10 nm or less, preferably 8 nm or less, and more preferably 5 nm or less. The lower limit of the in-plane retardation can be, for example, 0 nm.
[0012] The optical film exhibits flat wavelength dispersion characteristics in which the retardation value hardly changes depending on the wavelength of the measuring light. The Re(450) / Re(550) of the optical film is 0.98 to 1.03, preferably 0.99 to 1.03, and more preferably 1.00 to 1.03. By using a polycarbonate-based resin having such a Re(450) / Re(550), excellent antireflection characteristics can be realized.
[0013] The puncture elastic modulus of the optical film is 50 gf / mm or more, preferably 100 gf / mm or more, and more preferably 150 gf / mm or more. The puncture elastic modulus is obtained by dividing the force (gf) just before the film breaks (or tears) when a needle (puncture tool) is pierced perpendicularly to the main surface of the film by the strain (mm) at that time. When the optical film has the above puncture elastic modulus, the occurrence of process defects during transportation is suppressed, and an optical film with excellent flexibility can be obtained.
[0014] The puncture strength per unit thickness of the optical film is preferably 10 gf / μm or more, more preferably 15 gf / μm or more, and even more preferably 20 gf / μm or more. The puncture strength per unit thickness refers to the strength when the film breaks when a needle is vertically lowered onto the film, divided by the thickness. When the film has the puncture strength per unit thickness as described above, the occurrence of bright spots when the film is pressed is suppressed, and an optical film with excellent shape processing properties can be obtained.
[0015] The optical film has a breaking strength of preferably 800 MPa or more and a breaking elongation of preferably 3% or more. The optical film has a breaking strength of more preferably 1500 MPa or more, and further preferably 2500 MPa or more. The upper limit of the breaking strength of the optical film is, for example, 70000 MPa. The breaking elongation of the optical film is more preferably 4% or more, and further preferably 6% or more. The upper limit of the breaking elongation of the optical film can be, for example, 300%. The breaking strength refers to the stress when the film breaks in a tensile test. The breaking elongation refers to the strain (elongation rate) when the film breaks. When the breaking strength and breaking elongation of the optical film are in the above ranges, an optical film having excellent crack resistance can be obtained.
[0016] The thickness of the optical film is preferably 25 μm or less, more preferably 20 μm or less. The lower limit of the thickness of the optical film may be, for example, 0.5 μm. When the thickness of the optical film is in this range, the optical film can be suitably applied to a thin device.
[0017] In the above optical film, the absolute value of the rate of change of the in-plane retardation Re(550) after 500 hours under conditions of a temperature of 65° C. and a humidity of 90% is preferably 1% or less, more preferably 0.5% or less, and further preferably 0.1% or less. The lower limit of the absolute value of the rate of change may be, for example, 0.01%. The rate of change of the retardation is |(Re 500 -Re 0 ) / Re 0 Re is expressed as |×100(%). 0 is the in-plane retardation (nm) of the optical film before the test started, and Re 500 is the in-plane retardation (nm) of the optical film after the test. When the absolute value of the rate of change of the in-plane retardation Re(550) of the optical film is in such a range, when the optical film is applied to an image display device, the hue change due to the retardation at each location on the image display device is small, and the occurrence of color unevenness on the display can be suppressed.
[0018] The moisture permeability of the optical film is preferably 300 g / m 2 - 24h or less, preferably 200g / m 2 24h or less, more preferably 160g / m 2 The lower limit of the moisture permeability is, for example, 1 g / m 2 If the moisture permeability of the optical film is within this range, the change in retardation in a humid environment can be suppressed.
[0019] The absolute value of the photoelastic coefficient of the optical film is preferably 2×10 -11 m 2 / N or less, more preferably 2.0×10 -13 m 2 / N~1.5×10 -11 m 2 / N, and more preferably 1.0×10 -12 m 2 / N~1.2×10 -11 m 2 When the absolute value of the photoelastic coefficient of the optical film is within this range, the retardation is unlikely to change when shrinkage stress occurs during heating. As a result, when the optical film is applied to an image display device, the image display device can be effectively prevented from having uneven heat distribution.
[0020] According to the embodiment of the present invention, as described above, an optical film can be obtained that satisfies the desired in-plane retardation, wavelength dispersion characteristics, and thickness, and further suppresses the occurrence of process defects during transportation, suppresses the occurrence of bright spots when the film is pressed, and has excellent flexibility, profile processability, and crack resistance. Such an optical film can be suitably used, for example, in a thin, bendable and / or foldable EL display device.
[0021] B. Constituent materials As described above, the optical film is typically a resin film containing a polycarbonate resin.
[0022] The polycarbonate resin according to the present invention contains at least a structural unit derived from a dihydroxy compound having a bond structure represented by the following structural formula (1), and has at least one bond structure -CH 2 It is produced by reacting a dihydroxy compound containing at least a dihydroxy compound having --O-- with a carbonic acid diester in the presence of a polymerization catalyst. [ka]
[0023] Here, the dihydroxy compound having the bond structure represented by structural formula (1) is a compound having two alcoholic hydroxyl groups and a linking group -CH 2Any compound having any structure can be used as long as it contains a structure having -O- and can react with a carbonate diester in the presence of a polymerization catalyst to produce a polycarbonate, and multiple compounds may be used in combination. In addition, a dihydroxy compound not having a bond structure represented by structural formula (1) may be used in combination as a dihydroxy compound used in the polycarbonate resin of the present invention. Hereinafter, a dihydroxy compound having a bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (A), and a dihydroxy compound not having a bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (B).
[0024] (Dihydroxy compound (A)) The linking group -CH in the dihydroxy compound (A) 2 "-O-" means a structure in which the linking group is bonded to an atom other than a hydrogen atom to form a molecule. In this linking group, the atom to which at least an oxygen atom can be bonded or the atom to which both a carbon atom and an oxygen atom can be bonded is most preferably a carbon atom. 2 The number of "-O-" is preferably 1 or more, and more preferably 2 to 4.
[0025] More specifically, examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, and 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene. phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl Compounds having an aromatic group in the side chain and an ether group bonded to the aromatic group in the main chain, such as bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, Pan, 2,2-bis[3,5-dimethyl-4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxy 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[3- Bis(hydroxyalkoxyaryl)alkanes, such as cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane, 4,4'-bis(2-hydroxyethoxy)diphenyl ether, 4,dihydroxyalkoxy diaryl ethers, such as 4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxy aryl sulfides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxy aryl sulfoxides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfoxide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfoxide; 4,4'-bis(2-hydroxyethoxyphenyl) sulfone and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfone. Examples of the cyclic ether structure include bishydroxyalkoxyarylsulfones, 1,4-bishydroxyethoxybenzene, 1,3-bishydroxyethoxybenzene, 1,2-bishydroxyethoxybenzene, 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane, anhydrous sugar alcohols represented by the dihydroxy compound represented by the following formula (4), and spiroglycol represented by the following general formula (6). These may be used alone or in combination of two or more.
[0026] [ka]
[0027] These dihydroxy compounds (A) may be used alone or in combination of two or more. In the present invention, the dihydroxy compound represented by the formula (4) includes isosorbide, isomannide, and isoidet, which are stereoisomeric, and these may be used alone or in combination of two or more.
[0028] Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as resources, is the most preferable from the viewpoints of availability and ease of production, optical properties, and moldability. In the present invention, isosorbide is preferably used as the dihydroxy compound (A).
[0029] (Dihydroxy Compound (B)) In the present invention, a dihydroxy compound (B) other than the dihydroxy compound (A) may be used as the dihydroxy compound. As the dihydroxy compound (B), for example, an alicyclic dihydroxy compound, an aliphatic dihydroxy compound, an oxyalkylene glycol, an aromatic dihydroxy compound, or a diol having a cyclic ether structure may be used as a dihydroxy compound serving as a structural unit of polycarbonate together with the dihydroxy compound (A), for example, a dihydroxy compound represented by formula (4).
[0030] The alicyclic dihydroxy compound usable in the present invention is not particularly limited, but preferably, a compound having a 5-membered ring structure or a 6-membered ring structure is used. The 6-membered ring structure may be fixed to a chair or boat shape by a covalent bond. The alicyclic dihydroxy compound has a 5-membered ring or a 6-membered ring structure, so that the heat resistance of the resulting polycarbonate can be increased. The number of carbon atoms contained in the alicyclic dihydroxy compound is usually 70 or less, preferably 50 or less, more preferably 30 or less. The larger this value, the higher the heat resistance, but the more difficult the synthesis, the more difficult the purification, and the higher the cost. The smaller the number of carbon atoms, the easier it is to purify and the easier it is to obtain.
[0031] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure that can be used in the present invention include alicyclic dihydroxy compounds represented by the following general formula (II) or (III). HOCH 2 -R 1-CH 2 OH (II) H.O.R. 2 -OH (III) (In formulas (II) and (III), R 1 , R 2 Each of the groups represents a cycloalkylene group having 4 to 20 carbon atoms. Cyclohexanedimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is a compound represented by the following general formula (II): 1 is represented by the following general formula (IIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.
[0032] [ka]
[0033] The alicyclic dihydroxy compound represented by the above general formula (II), tricyclodecane dimethanol and pentacyclopentadecanedimethanol, are represented by the following general formula (II): 1 is represented by the following general formula (IIb) (wherein n is 0 or 1):
[0034] [ka]
[0035] The alicyclic dihydroxy compound represented by the above general formula (II), decalin dimethanol or tricyclotetradecane dimethanol, is a compound represented by the general formula (II), 1 These include various isomers represented by the following general formula (IIc) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalin dimethanol, 1,5-decalin dimethanol, and 2,3-decalin dimethanol.
[0036] [ka]
[0037] Norbornane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 1 The isomers include various isomers represented by the following general formula (IId): Specific examples of such isomers include 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, etc.
[0038] [ka]
[0039] Adamantane dimethanol, which is an alicyclic dihydroxy compound represented by the general formula (II), is 1 is represented by the following general formula (IIe): Specific examples of such isomers include 1,3-adamantanedimethanol.
[0040] [ka]
[0041] In addition, cyclohexanediol, which is an alicyclic dihydroxy compound represented by the above general formula (III), is a compound represented by the following general formula (III): 2 is represented by the following general formula (IIIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.
[0042] [ka]
[0043] The alicyclic dihydroxy compound represented by the above general formula (III), tricyclodecanediol and pentacyclopentadecanediol, are represented by the following general formula (III): 2 is represented by the following general formula (IIIb) (wherein n is 0 or 1):
[0044] [ka]
[0045] The alicyclic dihydroxy compound represented by the above general formula (III), decalindiol or tricyclotetradecanediol, is preferably a compound represented by the general formula (III), 2 is represented by the following general formula (IIIc) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalindiol, 1,5-decalindiol, and 2,3-decalindiol.
[0046] [ka]
[0047] The norbornanediol, which is an alicyclic dihydroxy compound represented by the above general formula (III), is a compound represented by the following general formula (III): 2 The isomers include various isomers represented by the following general formula (IIId): Specific examples of such isomers include 2,3-norbornanediol and 2,5-norbornanediol.
[0048] [ka]
[0049] The adamantanediol which is an alicyclic dihydroxy compound represented by the above general formula (III) is a compound represented by the following general formula (III): 2 The isomers include various isomers represented by the following general formula (IIIe): Specific examples of such isomers include 1,3-adamantanediol.
[0050] [ka]
[0051] Among the specific examples of the alicyclic dihydroxy compounds described above, cyclohexane dimethanols, tricyclodecane dimethanols, adamantane diols, and pentacyclopentadecanedimethanols are particularly preferred, and from the viewpoints of availability and ease of handling, 1,4-cyclohexane dimethanol, 1,3-cyclohexane dimethanol, 1,2-cyclohexane dimethanol, and tricyclodecane dimethanol are preferred. In the present invention, tricyclodecane dimethanol is preferably used as the dihydroxy compound (B).
[0052] Examples of the aliphatic dihydroxy compounds that can be used in the present invention include ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-heptanediol, and 1,6-hexanediol. Examples of the oxyalkylene glycols that can be used in the present invention include diethylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol.
[0053] Examples of aromatic dihydroxy compounds that can be used in the present invention include 2,2-bis(4-hydroxyphenyl)propane [=bisphenol A], 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(4-hydroxyphenyl)pentane, 2,4'-dihydroxy-diphenylmethane, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-5-nitrophenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 3,3-bis(4-hydroxyphenyl)ethane, 4,4'-bis(4-hydroxyphenyl)ethane, 5,5'-bis(4-hydroxyphenyl)ethane, 6,5'-bis(4-hydroxyphenyl)ethane, 7,5'-bis(4-hydroxyphenyl)ethane, 8,5'-bis(4-hydroxyphenyl)ethane, 9,5'-bis(4-hydroxyphenyl)ethane, 10,5'-bis(4-hydroxyphenyl)ethane, 11,5'-bis(4-hydroxyphenyl)ethane, 12,5'-bis(4-hydroxyphenyl)ethane, 13,5'-bis(4-hydroxyphenyl)ethane, 14,5'-bis(4-hydroxyphenyl)ethane, 15,5'-bis(4-hydroxyphenyl)ethane, 16,5'-bis(4-hydroxyphenyl)ethane, 17,5'-bis(4-hydroxyphenyl)ethane, 18,5'-bis(4-hydroxyphenyl)ethane, 19,5'-bis(4-hydroxyphenyl)ethane, 20,5'-bis(4-hydroxyphenyl)ethane, 21,5'-bis(4-hydroxyphenyl)ethane, 22,5'-bis(4-hydroxyphenyl)ethane, 23, hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl)sulfide, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether, 4,4'-dihydroxy-2,5-diethoxydiphenyl ether, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy-2-methyl)phenyl]fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-2-methylphenyl)fluorene.
[0054] Examples of the diols having a cyclic ether structure that can be used in the present invention include spiroglycols and dioxane glycols.The above-mentioned exemplary compounds are examples of the alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure that can be used in the present invention, and are not limited thereto.One or more of these compounds can be used together with the dihydroxy compound represented by formula (4).
[0055] By using these dihydroxy compounds (B), it is possible to obtain effects such as improvement in flexibility, improvement in heat resistance, and improvement in moldability according to the application. The ratio of the dihydroxy compound (A), for example, the dihydroxy compound represented by formula (4), to the total dihydroxy compounds constituting the polycarbonate resin according to the present invention is not particularly limited, but is preferably 10 mol% or more, more preferably 40 mol% or more, even more preferably 60 mol% or more, preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 70 mol% or less. If the content ratio of the structural unit derived from other dihydroxy compounds is too high, the performance such as optical properties may be deteriorated.
[0056] When an alicyclic dihydroxy compound is used among the other dihydroxy compounds, the proportion of the dihydroxy compound (A), for example the total proportion of the dihydroxy compound represented by formula (4) and the alicyclic dihydroxy compound, relative to all dihydroxy compounds constituting the polycarbonate is not particularly limited, but is preferably 80 mol % or more, more preferably 90 mol % or more, and even more preferably 95 mol % or more.
[0057] In addition, the content ratio of the dihydroxy compound (A), for example, the dihydroxy compound represented by formula (4) derived structural unit and the alicyclic dihydroxy compound derived structural unit in the polycarbonate resin according to the present invention can be selected at any ratio, but the structural unit derived from the dihydroxy compound represented by formula (4): the structural unit derived from the alicyclic dihydroxy compound = 1:99 to 99:1 (mol%) is preferable, and the structural unit derived from the dihydroxy compound represented by formula (4): the structural unit derived from the alicyclic dihydroxy compound = 10:90 to 90:10 (mol%) is particularly preferable. If the structural unit derived from the dihydroxy compound represented by formula (4) is more and the structural unit derived from the alicyclic dihydroxy compound is less than the above range, the coloring is likely to occur, and conversely, if the structural unit derived from the dihydroxy compound represented by formula (4) is less and the structural unit derived from the alicyclic dihydroxy compound is more, the molecular weight tends to be difficult to increase.
[0058] Furthermore, when an aliphatic dihydroxy compound, an oxyalkylene glycol, an aromatic dihydroxy compound, or a diol having a cyclic ether structure is used, the total ratio of the dihydroxy compound (A), for example, the dihydroxy compound represented by formula (4), and each of these dihydroxy compounds to the total dihydroxy compounds constituting the polycarbonate is not particularly limited and can be selected at any ratio. In addition, the content ratio of the dihydroxy compound (A), for example, the constituent unit derived from the dihydroxy compound represented by formula (4), and each of these dihydroxy compounds is not particularly limited and can be selected at any ratio.
[0059] Details of polycarbonate-based resins are described, for example, in JP 2012-31370 A (Patent No. 5448264), the disclosure of which is incorporated herein by reference.
[0060] C. Manufacturing method of optical film The optical film can be obtained by, for example, forming a film from a resin such as the polycarbonate resin described in section B. Any appropriate molding method can be adopted as a method for forming the film. Specific examples include compression molding, transfer molding, injection molding, extrusion molding, blow molding, powder molding, FRP molding, cast coating (for example, casting), calendar molding, and heat pressing. Among them, extrusion molding or cast coating is preferred, which can improve the smoothness of the obtained film and obtain good optical uniformity. Since the cast coating method may cause problems due to residual solvent, extrusion molding is particularly preferred, and melt extrusion molding using a T-die is particularly preferred from the viewpoint of film productivity. The molding conditions can be appropriately set according to the composition and type of the resin used, the properties desired as an optical film, and the like.
[0061] D. Polarizing plate The optical film described in the above items A to C may be provided as a laminate with other optical films and / or optical members. In one embodiment, the optical film may be provided as a laminate with a polarizer (typically, a polarizing plate). Thus, the present invention encompasses a polarizing plate having the optical film.
[0062] The polarizing plate typically includes a polarizer and the optical film bonded to at least one surface of the polarizer via an adhesive layer. The polarizer may have a protective layer on at least one surface of the polarizer. Furthermore, the polarizing plate may have a pressure-sensitive adhesive layer and a separator on the surface opposite to the viewing side.
[0063] In one embodiment, the polarizing plate has a modified part. By including the optical film in the polarizing plate, a polarizing plate having good modified processability can be obtained. In this specification, the "modified part" refers to a part that is processed into a special shape different from a general shape (for example, a rectangle, a chamfered corner). As shown in FIG. 1 and FIG. 2, typical examples of the modified part include a through hole and a cut part that becomes a recess when viewed in a plane. Typical examples of the recess include a shape that resembles a boat shape, a V-shaped notch, and a U-shaped notch. Furthermore, the polarizing plate may be modified as a whole. As such an example, as shown in FIG. 3 and FIG. 4, a shape corresponding to the meter panel of an automobile can be mentioned. The shape includes a part in which the outer edge is formed in an arc shape along the rotation direction of the meter needle and the outer edge forms a V-shaped (including a rounded shape) that is convex inward in the plane direction. The modified part is provided at any appropriate position depending on the purpose.
[0064] As the polarizer, any appropriate polarizer can be adopted. For example, the resin film forming the polarizer may be a single-layer resin film or a laminate of two or more layers.
[0065] Specific examples of polarizers made of a single-layer resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films that have been dyed with iodine or a dichroic substance such as a dichroic dye and stretched, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. A polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it is preferably used because of its excellent optical properties.
[0066] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment, or may be carried out while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based film in water and washing it with water before dyeing, it is possible to wash off dirt and antiblocking agents on the surface of the PVA-based film, and also to swell the PVA-based film and prevent uneven dyeing.
[0067] Specific examples of polarizers obtained using laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. Details of the manufacturing method of such polarizers are described in, for example, JP 2012-73580 A (Patent No. 5414738 A). The description of this patent document is incorporated herein by reference. The entire description of this publication is incorporated herein by reference.
[0068] In one embodiment, the thickness of the polarizer is preferably 1 μm to 25 μm, more preferably 3 μm to 10 μm, and further preferably 3 μm to 8 μm. When the thickness of the polarizer is within this range, curling during heating can be well suppressed, and good appearance durability during heating can be obtained.
[0069] The protective layer is formed of any suitable protective film that can be used as a film for protecting a polarizer. Specific examples of materials that are the main components of the protective film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. In addition, thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxy resins, and silicones can also be used. In addition, glassy polymers such as siloxane polymers can also be used. Polymer films described in JP-A-2001-343529 (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.
[0070] The thickness of the protective layer is preferably 10 μm to 100 μm. The protective layer may be laminated on the polarizer via an adhesive layer (specifically, an adhesive layer, a pressure-sensitive adhesive layer), or may be laminated in close contact with the polarizer (without an adhesive layer). If necessary, a surface treatment layer such as a hard coat layer, an antiglare layer, and an antireflection layer may be formed on the protective layer disposed on the outermost surface of the retardation layer-attached polarizing plate.
[0071] Any suitable adhesive may be used as the adhesive forming the adhesive layer. Examples of the base resin of the adhesive include acrylic resin, styrene resin, silicone resin, urethane resin, and rubber resin. Such base resins are described in, for example, JP 2015-120337 A (Patent No. 6457789) or JP 2011-201983 A. The descriptions in these publications are incorporated herein by reference. Examples of crosslinking agents that may be included in the adhesive include isocyanate compounds, epoxy compounds, and aziridine compounds. The adhesive may include, for example, a silane coupling agent. The formulation of the adhesive may be appropriately set according to the purpose and desired properties.
[0072] The storage modulus of the adhesive layer is preferably 1.0×10 4 Pa~1.0×10 7 Pa, more preferably 2.0×10 4 Pa~5.0×10 6 The storage modulus is Pa. If the pressure-sensitive adhesive layer has a storage modulus in this range, blocking during roll formation can be suppressed. The storage modulus can be determined, for example, by dynamic viscoelasticity measurement at a temperature of 23° C. and an angular velocity of 0.1 rad / s.
[0073] The thickness of the adhesive layer is preferably 1 μm to 60 μm, and more preferably 3 μm to 30 μm. If the thickness is too thin, the adhesiveness becomes insufficient and air bubbles may get into the adhesive interface. If the thickness is too thick, problems such as the adhesive protruding out are likely to occur.
[0074] In practice, a separator is temporarily attached to the surface of the adhesive layer in a peelable manner until the optical film is actually used. By providing the separator, the adhesive layer is protected and the surface protection film can be wound up in a roll. Examples of the separator include plastic (e.g., polyethylene terephthalate (PET), polyethylene, polypropylene) films, nonwoven fabrics, and papers, the surfaces of which are coated with a release agent such as a silicone-based release agent, a fluorine-based release agent, or a long-chain alkyl acrylate-based release agent. The thickness of the separator can be any appropriate thickness depending on the purpose. The thickness of the separator is, for example, 10 μm to 100 μm. EXAMPLES
[0075] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows. (1) In-plane retardation and wavelength dispersion characteristics The optical films obtained in the examples and comparative examples were cut into a length of 4 cm and a width of 4 cm to be used as measurement samples. The in-plane retardation Re(550) of the measurement samples was measured using an Axoscan manufactured by Axometrics. Furthermore, Re(450) was also measured, and Re(450) / Re(550) was calculated. (2) Thickness The thickness of 10 μm or less was measured using an interference film thickness meter (manufactured by Otsuka Electronics, product name "MCPD-3000"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C"). (3) Moisture permeability The optical films obtained in the examples and comparative examples were subjected to a moisture permeability test (cup method) according to JIS Z0208 in an atmosphere at a temperature of 40°C and a humidity of 92% RH, with an area of 1 m 2 The amount of water vapor (g) passing through the sample in 24 hours was measured. (4) Phase difference change The optical films obtained in the examples and comparative examples were cut into 5 cm x 5 cm pieces, adhesive was applied to one side of the pieces with a hand roller, and the adhesive side was applied to one side of an alkaline glass to obtain a test piece. The test piece was stored in an oven at a temperature of 65°C and a humidity of 90% for 500 hours (humidification test), and the phase difference change (%) before and after the test was calculated. (5) Puncture elastic modulus The piercing elastic modulus was determined by dividing the force (gf) just before the optical films obtained in the Examples and Comparative Examples break (or tear) when a needle (piercing tool) was pierced perpendicularly to the main surface of the optical film by the strain (mm) at that time. The needle used had a tip diameter of 1 mmφ and 0.5R. The needle piercing speed was 0.33 cm / sec. The measurement was performed in an environment at a temperature of 23°C. (6)Puncture strength A tester equipped with a needle with a tip diameter of 1 mmφ and 0.5R was used. The optical films obtained in the examples and comparative examples were sandwiched between two jigs with a circular hole in the center, and the optical films were fixed to the tester. The needle was vertically lowered onto the optical film so as to pass through the hole in the jig, and the strength of the optical film was measured when it broke. The test conditions were an environment with a temperature of 23±3°C and a piercing speed of 0.33 cm / sec. A piercing test was performed on 12 test pieces, and the average value was divided by the thickness of the optical film to determine the piercing strength per unit thickness of the optical film. (7) Breaking strength and breaking elongation The optical films obtained in the examples and comparative examples were cut to a width of 1 cm and a length of 13 cm, and then a tensile test was performed using an Autograph ASG-50D (manufactured by Shimadzu Corporation) as a tensile tester at a tensile speed of 200 mm / min, a chuck distance of 50 mm, and room temperature (23°C). The stress at which the optical film broke was determined as the breaking strength, and the strain (elongation) at which the optical film broke was determined as the breaking strength. (8) Adhesiveness The optical film and the polarizer obtained in the examples and comparative examples were laminated together to obtain a laminate. The obtained laminate was cut into a size of 200 mm parallel to the stretching direction of the polarizer and 15 mm in the perpendicular direction, and the laminate was laminated to a glass plate. Then, a cut was made between the optical film and the polarizer with a cutter knife, and the optical film and the polarizer were peeled off in a 90-degree direction at a peeling speed of 1000 mm / min using a Tensilon universal testing machine RTC (manufactured by A&D Co., Ltd.), and the peel strength (N / 15 mm) was measured. A peel strength of 1 N / 15 mm or more was considered good, and a peel strength of less than 1 N / 15 mm was considered bad. (9) Runnability (evaluation of process defects during transportation) When the optical films obtained in the examples and comparative examples were transported by guide rolls at a speed of 5 m / min to 40 m / min, if they did not suffer from defects such as bends, scratches, or dents (if they could be transported without problems), they were rated as good, and if they suffered from bends, scratches, dents, etc., they were rated as bad. (10) Flexibility (MIT test) The MIT test was carried out in accordance with JIS P 8115. Specifically, the optical films obtained in the examples and comparative examples were cut into a length of 15 cm and a width of 1.5 cm to be used as measurement samples. The measurement samples were attached to an MIT folding fatigue tester BE-202 type (manufactured by Tester Sangyo Co., Ltd.) (load 1.0 kgf, clamp R: 0.38 mm), and repeatedly folded at a test speed of 90 cpm and a folding angle of 90°, and the number of foldings at which the measurement sample broke was used as the test value. Those with an empirical value of 500 times or more were rated as good, and those with an empirical value of less than 500 times were rated as bad. (11) Evaluation of bright spots during indentation A sample similar to the sample evaluated in the piercing strength test was attached to a polarizer, and the film side was pressed with a force of 10 gf / μm using a piercing tester. Then, a polarizing plate was prepared so that it formed an axis of 90° with the polarizing plate, and in a crossed Nicol state, transmitted light was transmitted from the opposite side of the film that had been pierced and the sample was rated as good if no bright spots were observed, and as bad if bright spots were observed. (12) Special Shape Formability Test The optical films obtained in the examples and comparative examples were 2The film was irradiated with a laser with an energy of 3 kW, and cut in the machine direction and perpendicular to the machine direction to obtain a measurement sample of 200 mm x 200 mm. The cut portion was observed using a laser microscope, and if there were no cracks, it was rated as good, and if there were cracks and / or it was not possible to cut, it was rated as bad. (13) Crack resistance The optical films obtained in the examples and comparative examples were subjected to a heat shock test from -40°C to 80°C for 300 cycles, and if no cracks of 300 μm or more were generated, they were rated as good, and if cracks of 300 μm or more were generated, they were rated as bad.
[0076] [Example 1] 1. Preparation of Optical Film 81.98 parts by mass of isosorbide (hereinafter sometimes abbreviated as "ISB"), 47.19 parts by mass of tricyclodecane dimethanol (hereinafter sometimes abbreviated as "TCDDM"), 175.1 parts by mass of diphenyl carbonate (hereinafter sometimes abbreviated as "DPC"), and 0.979 parts by mass of cesium carbonate 0.2% by mass aqueous solution as a catalyst were charged into a reaction vessel, and in a nitrogen atmosphere, as the first step of the reaction, the heating tank temperature was heated to 150°C and the raw materials were dissolved while stirring as necessary (about 15 minutes). Next, the pressure was changed from normal pressure to 13.3 kPa, and the heating tank temperature was increased to 190°C over one hour, while the generated phenol was extracted from the reaction vessel. After the entire reaction vessel was kept at 190°C for 15 minutes, in the second step, the pressure in the reaction vessel was set to 6.67 kPa, the heating tank temperature was raised to 230°C in 15 minutes, and the generated phenol was extracted outside the reaction vessel. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure in the reaction vessel was allowed to reach 0.200 kPa or less in order to remove the generated phenol. After reaching a predetermined stirring torque, the reaction was terminated, and the reaction product was extruded into water to obtain polycarbonate resin pellets. The obtained polycarbonate resin was vacuum-dried at 80°C for 5 hours, and then an optical film composed of polycarbonate resin was produced using a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 300 mm, setting temperature: 250°C), a chill roll (setting temperature: 120 to 130°C), and a winder. The wavelength dispersion value of the obtained optical film was 1.02, the in-plane retardation Re(550) was 2 nm, the thickness was 13 μm, and the moisture permeability was 156 g / m 2 The optical film had a puncture modulus of 153 gf / mm, a puncture strength of 25 gf / μm, a breaking strength of 2614 MPa, and a breaking elongation of 6.3%. The optical film thus obtained was subjected to the evaluations (8) to (13) above. The results are shown in Table 1.
[0077] [Example 2] An optical film was obtained in the same manner as in Example 1, except that the thickness of the optical film made of polycarbonate resin was 20 μm. The wavelength dispersion value of the obtained optical film was 1.02, the in-plane retardation Re(550) was 3 nm, and the moisture permeability was 113 g / m 2 24h, and the phase difference change was 0.07%. Furthermore, the optical film had a puncture elastic modulus of 200gf / mm, a puncture strength of 26gf / μm, a breaking strength of 2614MPa, and a breaking elongation of 6.3%. The obtained optical film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0078] [Example 3] An optical film was obtained in the same manner as in Example 1, except that the thickness of the optical film made of polycarbonate resin was 25 μm. The wavelength dispersion value of the obtained optical film was 1.02, the in-plane retardation Re(550) was 2 nm, and the moisture permeability was 102 g / m 2 24h, and the phase difference change was 0.07%. Furthermore, the optical film had a puncture elastic modulus of 264gf / mm, a puncture strength of 23.6gf / μm, a breaking strength of 2614MPa, and a breaking elongation of 6.3%. The obtained optical film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0079] [Comparative Example 1] A commercially available cycloolefin resin film (manufactured by Zeon Corporation, product name "ZEONOR") was used as the resin film. The wavelength dispersion value of the optical film was 1.01, the in-plane retardation Re(550) was 2 nm, the thickness was 25 μm, and the moisture permeability was 10 g / m 2 The optical film had a puncture modulus of 304 gf / mm, a puncture strength of 17 gf / μm, a breaking strength of 2150 MPa, and a breaking elongation of 0.7%. The optical film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0080] [Comparative Example 2] A triacetyl cellulose (TAC) film (Konica Minolta, product name "KC2UA") was used. The wavelength dispersion value of the optical film was 1.09, the in-plane retardation Re(550) was 3 nm, the thickness was 25 μm, and the moisture permeability was 320 g / m 2 The optical film had a puncture modulus of 480 gf / mm, a puncture strength of 22 gf / μm, a breaking strength of 4200 MPa, and a breaking elongation of 8%. The optical film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0081] [Comparative Example 3] An optical film was obtained in the same manner as in Example 1, except that the thickness of the optical film was 5 μm. The wavelength dispersion value of the obtained optical film was 1.02, the in-plane retardation Re(550) was 0.8 nm, and the moisture permeability was 172 g / m 2 The optical film had a puncture modulus of 65 gf / mm, a puncture strength of 20 gf / μm, a breaking strength of 1200 MPa, and a breaking elongation of 5.5%. The optical film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0082] [Table 1]
[0083] As is clear from Table 1, the optical films of the examples of the present invention are excellent in all respects: adhesion, running property, bending property, suppression of bright spots during pressing, shape forming property, and crack resistance. This is presumably achieved by using an optical film containing a specific polycarbonate resin, and by setting the puncture modulus, puncture strength per unit film thickness, breaking strength, and breaking elongation of the optical film all within specific ranges. [Industrial Applicability]
[0084] The optical film and polarizing plate according to the embodiment of the present invention are suitably used in image display devices.
Claims
1. An optical film comprising a polycarbonate resin, having an in-plane retardation Re(550) of 10 nm or less, Re(450) / Re(550) of 0.98 to 1.03, and a puncture modulus of elasticity of 100 gf / mm or more.
2. A polarizing plate comprising: a polarizer; and the optical film according to claim 1 attached to at least one surface of the polarizer via an adhesive layer.
Citation Information