Resin composition, resin cured product, and composite molded body
The resin composition with agglomerated inorganic filler and specific epoxy resin addresses voltage and peeling issues in heat dissipation sheets, providing high strength and moisture resistance for reliable power semiconductor modules.
Patent Information
- Application Number
- JP2024125962
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-10-11
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-10-07
Smart Images

Figure 2024149637000001 
Figure 2024149637000002 
Figure 2024149637000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a cured resin, and a composite molded article having a cured part made of the cured resin composition and a metal part. The resin composition, cured resin, and composite molded article of the present invention can be suitably used, for example, as a heat dissipation sheet for a power semiconductor device. [Background technology]
[0002] In recent years, power semiconductor devices used in various fields such as railways, automobiles, and general home appliances are undergoing a transition from conventional Si power semiconductors to power semiconductors using SiC, AlN, GaN, etc. in order to achieve further miniaturization, cost reduction, and efficiency. Power semiconductor devices are generally used as power semiconductor modules in which a plurality of semiconductor devices are arranged on a common heat sink and packaged.
[0003] Various issues have been pointed out for practical application of such power semiconductor devices. One of these issues is the problem of dissipating heat generated by the devices. This problem generally affects the reliability of power semiconductor devices, which are capable of achieving high output and high density by operating at high temperatures. There are concerns that the heat generated by device switching will reduce reliability.
[0004] In recent years, heat generation due to the increasing density of integrated circuits has become a major problem, especially in the electrical and electronics fields. Therefore, how to dissipate heat has become an urgent issue.
[0005] One method to solve this problem is to use highly thermally conductive ceramic substrates such as alumina substrates and aluminum nitride substrates as heat dissipation substrates on which power semiconductor devices are mounted. However, ceramic substrates have drawbacks such as being easily cracked by impact, and being difficult to make thin and compact.
[0006] Therefore, a heat dissipation sheet using a resin such as a highly thermally conductive epoxy resin and a highly thermally conductive inorganic filler has been proposed. For example, Patent Document 1 proposes a heat dissipation resin sheet containing a resin with a Tg of 60° C. or less and a boron nitride filler, in which the content of the boron nitride filler is 30 vol% or more and 60 vol% or less.
[0007] However, when a conventional heat dissipating resin sheet made of an inorganic filler-containing resin composition is applied to a power semiconductor, there are problems as follows.
[0008] (1) Power semiconductors require high voltage and large current flow, making voltage resistance important. However, conventional heat dissipation resin sheets do not have sufficient voltage resistance for use in power semiconductors.
[0009] (2) When a copper foil or other substrate is laminated to form a heat dissipation sheet to improve thermal conductivity, the sheet is prone to peeling at the interface due to thermal expansion and contraction caused by the large amount of heat generated during use. In the case of a ceramic substrate, the substrate is integrated with the copper plate by sintering, so peeling at the interface is unlikely to occur. However, in the case of a heat dissipation resin sheet, the substrate is integrated by heating and pressing the cured film, so peeling at the interface is likely to occur.
[0010] In order to prevent interfacial peeling due to expansion and contraction, it is conceivable to increase the degree of crosslinking of the epoxy resin to increase the strength of the cured product. In order to increase the degree of crosslinking, it is necessary to increase the epoxy equivalent of the epoxy resin. In this case, the addition reaction between the epoxy groups of the epoxy resin and active hydrogen increases the hydroxyl group concentration, and as the concentration increases, the moisture absorption rate tends to increase. The increase in the moisture absorption rate of the epoxy resin reduces the insulating properties of the cured product and also reduces the voltage resistance performance under high temperature and high humidity conditions. For this reason, such a method was considered undesirable.
[0011] One of the processes for assembling a power semiconductor module is the solder reflow process. In the solder reflow process, the temperature of the components is rapidly raised to melt the solder and join the metal components together. In this reflow process, the components used in the module deteriorate, and for example, the interfacial peeling between the hardened material and the metal and the insulation performance deteriorates, which reduces the reliability of the power semiconductor module. In addition, there is also the issue that the components absorb moisture during storage before the reflow process, which significantly accelerates the deterioration of the components in the solder reflow process and further reduces the performance of the resulting power semiconductor module. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2017-36415 A Summary of the Invention [Problem to be solved by the invention]
[0013] An object of the present invention is to provide a resin composition and cured resin that have high strength, excellent moisture absorption reflow resistance, and reduced problems of interfacial peeling associated with thermal expansion and contraction when laminated with a metal plate, as well as a composite molded article using this resin composition. [Means for solving the problem]
[0014] The present inventors have discovered a resin composition containing an aggregated inorganic filler, which has a weight increase rate of 0.80% or less at 85° C. and 85% RH after curing, and a storage modulus of the cured product of the resin composition excluding the inorganic filler at 200° C. of 1.0×10 7 It has been found that a cured resin material made of a resin composition having a resistance of 0.1 Pa or more has high insulating properties after a moisture absorption reflow test in which a reflow test is performed after storage under high temperature and high humidity conditions (hereinafter, this property may be referred to as "moisture absorption reflow resistance") and can solve the problem of interfacial peeling. The present inventors have also found that by using a cured resin having a storage modulus and a weight increase rate within specific ranges, excellent moisture absorption reflow resistance can be achieved and the problem of interfacial peeling can be overcome.
[0015] The present invention relates to the following.
[0016] [1] A resin composition comprising a resin and an aggregated inorganic filler, the weight increase rate of the resin composition after curing at 85°C and 85% RH is 0.80% or less, and the storage modulus of the cured product of the resin composition excluding the inorganic filler at 200°C is 1.0 × 10 7 The resin composition has a viscosity of 100 Pa or more.
[0017] [2] The resin composition contains an epoxy resin having three or more epoxy groups per molecule. The resin composition according to [1],
[0018] [3] The resin composition according to [1] or [2], wherein the resin composition contains an epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more.
[0019] [4] The resin composition according to [3], wherein the epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more further has at least one structure selected from a structure represented by the following structural formula (1) and a structure represented by the following structural formula (2):
[0020] [ka]
[0021] (In formula (1), R 1 and R 2 Each represents an organic group. In formula (2), R 3 represents a divalent cyclic organic group.
[0022] [5] The resin composition according to [3] or [4], wherein the content of the epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more is 1% by weight or more and 50% by weight or less, based on 100% by weight of the solid content of the resin composition excluding inorganic filler.
[0023] [6] The resin composition according to any one of [2] to [5], wherein the content of the epoxy resin having three or more epoxy groups per molecule is 10% by weight or more and 50% by weight or less, based on 100% by weight of the solid content of the resin composition excluding the inorganic filler.
[0024] [7] The resin composition according to any one of [2] to [6], wherein the molecular weight of the epoxy resin having three or more epoxy groups per molecule is 800 or less.
[0025] [8] The resin composition according to any one of [1] to [7], further comprising a compound having a heterocyclic structure containing a nitrogen atom.
[0026] [9] The resin composition according to any one of [1] to [8], wherein the agglomerated inorganic filler is agglomerated particles of boron nitride.
[0027]
[10] The resin composition according to [9], wherein the boron nitride agglomerated particles have a house of cards structure.
[0028]
[11] A composite molded article having a cured part made of a cured product of the resin composition according to any one of [1] to
[10] and a metal part.
[0029]
[12] A semiconductor device having the composite molding described in
[11] .
[0030]
[13] A resin cured product using a resin composition containing a resin and an aggregated inorganic filler, the weight increase rate at 85°C and 85% RH is 0.80% or less, and the storage modulus at 200°C after curing of the resin composition excluding the inorganic filler is 1.0 × 10 7 The hardened resin has a hardness of 1.0 Pa or more. Effect of the Invention
[0031] The resin composition of the present invention has high strength and excellent moisture absorption reflow resistance, and when laminated with a metal plate, there is almost no problem of interfacial peeling due to thermal expansion and contraction.
[0032] The cured resin of the present invention has high strength and excellent resistance to moisture absorption and reflow, and when laminated with a metal plate, there is almost no problem of interfacial peeling due to thermal expansion and contraction.
[0033] The resin composition and cured resin of the present invention, and a composite molded article using this resin composition can be suitably used as a heat dissipation sheet for a power semiconductor device, and a highly reliable power semiconductor module can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments and can be modified in various ways within the scope of the invention.
[0035] [Resin composition] The resin composition of the present invention contains a resin and an aggregated inorganic filler, and the weight increase rate of the resin composition after curing at 85° C. and 85% RH is 0.80% or less, and the storage modulus of the cured product of the resin composition excluding the inorganic filler at 200° C. is 1.0×10 7 Pa or more.
[0036] In the present invention, the term "resin composition" refers to an uncured composition, for example, a composition in a state before curing in a molding and pressing process, etc. More specifically, examples of the resin composition include a slurry-like resin composition to be subjected to a coating process described later, a sheet that has been subjected to a coating process, and a sheet before curing that has been subjected to processes such as coating and drying.
[0037] In the present invention, the term "cured resin" refers to a cured product in which the exothermic peak obtained when the temperature is raised from 40°C to 250°C at a rate of 10°C / min using a differential scanning calorimeter (DSC) is 10 J / g or less.
[0038] In the present invention, the resin composition excluding the inorganic filler refers to components other than the inorganic filler in the resin composition. The inorganic filler will be described later, and includes aggregated inorganic filler and non-aggregated inorganic filler (non-aggregated inorganic filler).
[0039] In the present invention, the "solid content" in the resin composition refers to all components in the resin composition other than the solvent.
[0040] The resin composition of the present invention may contain "other components" other than the resin and the aggregated inorganic filler, as long as the effects of the present invention are not impaired. Examples of other components include non-aggregated inorganic fillers, curing agents, curing catalysts, solvents, surface treatment agents such as silane coupling agents, insulating carbon components such as reducing agents, viscosity adjusters, dispersants, thixotropy imparting agents, flame retardants, colorants, organic fillers, and organic solvents. In particular, the inclusion of a dispersant makes it possible to form a uniform resin cured product, and improves the thermal conductivity and dielectric breakdown properties of the resulting resin cured product. Specific examples of the "other components" that may be contained in the resin composition of the present invention will be described later.
[0041] <Storage modulus> The storage modulus at 200°C after curing of the resin composition of the present invention excluding the inorganic filler is 1.0 x 10 7 The storage modulus is 1×10 Pa or more. 7 If the compressive strength is less than Pa, the strength of the cured resin product (hereinafter simply referred to as "cured resin product") obtained by curing the resin composition of the present invention will be low, and as a result, in a moisture absorption reflow test, voids will be generated inside, resulting in a decrease in insulating performance, and in the case of a composite molded product having a cured product part made of the cured product of the resin composition of the present invention and a metal part, peeling may occur at the interface between the metal part and the cured product part. From the viewpoint of maintaining performance after moisture absorption and reflow testing, this storage modulus is 1.3 × 10 7 Pa or more, and 1.5×10 7More preferably, the pressure is 1.7×10 Pa or more. 7 It is more preferable that the pressure is 1 Pa or more. On the other hand, the storage modulus is 5×10 9 Pa or less, and 1×10 9 Pa or less is more preferable, and 5×10 8 When the storage modulus is equal to or less than the upper limit, excessive internal stress caused by a moisture absorption reflow test can be suppressed, and cracks in the obtained cured resin and interfacial peeling between the metal part and the cured resin part tend to be suppressed. Furthermore, when the storage modulus is within the above range, the cured resin composition can easily penetrate into the unevenness of the metal, which is the adherend described below, and the cured resin that has penetrated into the unevenness exhibits a strong anchor effect, which tends to improve adhesion between the metal and the cured resin.
[0042] The storage modulus after curing can be controlled to fall within the above-mentioned specific range, for example, as described below, by introducing a rigid structure such as an aromatic ring into the components constituting the resin-containing component, or by introducing a polyfunctional component having multiple reactive groups to increase the crosslink density of the cured product.
[0043] The curing conditions of the resin composition of the present invention excluding the inorganic filler when measuring the storage modulus are as shown in the examples described later, that is, the temperature is increased from 25°C to 120°C at a rate of 14°C per minute, held at this temperature for 30 minutes, then increased at a rate of 7°C per minute to 175°C, held at this temperature for 30 minutes, then increased at a rate of 7°C per minute to 200°C, and held at this temperature for 10 minutes.
[0044] The storage modulus may be measured by any conventional method, and specifically, the method described in the Examples section below can be mentioned.
[0045] <Weight increase rate> After curing, the resin composition (containing an inorganic filler) of the present invention has a weight increase rate of 0.8% or less at 85° C. and 85% RH. If the weight increase rate exceeds 0.8%, the problem of the present invention, that is, maintaining high insulation properties and preventing interfacial peeling after a moisture absorption reflow test, cannot be solved. From the viewpoints of maintaining high insulating properties after a moisture absorption reflow test and preventing interfacial peeling, the smaller the weight increase rate, the more preferable, and it is preferably 0.75% or less, and more preferably 0.7% or less. The lower limit of the weight increase rate is not particularly limited, but from the viewpoints of achieving both strength and insulating performance of the resin cured product and film formability, it is, for example, 0.2% or more.
[0046] There are various possible causes for the weight increase of a cured resin, but it is important to control the weight increase due to moisture absorption. The present invention is based on the finding that the problems of the present invention can be solved by providing a resin composition having a weight increase rate at 85° C. and 85% RH after curing within the above-mentioned specific range.
[0047] The resin composition having a weight increase rate within a specific range at 85°C and 85% RH can be obtained by, for example, introducing a highly hydrophobic structure such as an aliphatic skeleton or an aromatic ring into the resin component constituting the resin composition. This can be achieved by controlling the weight gain rate.
[0048] The weight increase rate of the resin composition of the present invention at 85° C. and 85% RH after curing is measured by the method described later in the Examples section.
[0049] <Resin> The resin contained in the resin composition of the present invention is not particularly limited as long as it has a specific storage modulus and weight increase rate after curing. For example, it can be a resin that is cured by heat or light in the presence of a curing agent or a curing catalyst. In particular, a thermosetting resin is preferable from the viewpoint of ease of production.
[0050] Specific examples of the resin include epoxy resin, phenol resin, polycarbonate resin, unsaturated polyester resin, urethane resin, melamine resin, urea resin, maleimide resin, etc. Among these, epoxy resin is preferred from the viewpoints of viscosity, heat resistance, moisture absorption, and handling. Examples of the epoxy resin include epoxy group-containing silicon compounds, aliphatic epoxy resins, bisphenol A or F epoxy resins, novolac epoxy resins, alicyclic epoxy resins, glycidyl ester epoxy resins, multifunctional epoxy resins, and polymeric epoxy resins.
[0051] The resin composition of the present invention preferably contains 5% by weight or more of the resin based on 100% by weight of the solid content of the resin composition excluding the inorganic filler, more preferably 30% by weight or more, and even more preferably 50% by weight or more. The resin composition of the present invention more preferably contains 99% by weight or less based on 100% by weight of the solid content of the resin composition excluding the inorganic filler. When the resin content is equal to or more than the lower limit, the moldability is good, and when the resin content is equal to or less than the upper limit, the content of other components can be secured, and the thermal conductivity tends to be improved.
[0052] (Epoxy resin) Epoxy resin is a general term for compounds that have one or more oxirane rings (epoxy groups) in the molecule. The oxirane rings (epoxy groups) in epoxy resins can be either alicyclic epoxy groups or glycidyl groups.
[0053] The epoxy resin used in the present invention may be an aromatic oxirane ring (epoxy group)-containing compound. Specific examples thereof include bisphenol-type epoxy resins obtained by glycidylating bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethyl bisphenol A, tetramethyl bisphenol F, tetramethyl bisphenol AD, tetramethyl bisphenol S, and tetrafluorobisphenol A, biphenyl-type epoxy resins, dihydroxynaphthalene, 9,9-bis(4-hydroxyphenyl)fluorene, and other divalent phenols, glycidylating trisphenols such as 1,1,1-tris(4-hydroxyphenyl)methane, and other epoxy resins obtained by glycidylating tetrakisphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, and novolac-type epoxy resins obtained by glycidylating novolacs such as phenol novolac, cresol novolac, bisphenol A, novolac, and brominated bisphenol A novolac.
[0054] The resin composition of the present invention preferably contains 20% by weight or more of an epoxy resin, and more preferably 45% by weight or more, based on 100% by weight of the resin contained in the resin composition of the present invention. There is no particular upper limit to the content of the epoxy resin in the resin composition of the present invention, and the epoxy resin may be contained at 100% by weight based on 100% by weight of the total resin components. The epoxy resin may be contained within the above range. By including the above range, it becomes easy to control the high elasticity and weight gain rate of the cured product of the resin composition, and the storage modulus and weight gain rate tend to be more likely to fall within the above-mentioned specific range.
[0055] ((Multifunctional epoxy resin)) The resin composition of the present invention preferably contains an epoxy resin having three or more oxirane rings (epoxy groups) in one molecule (hereinafter, sometimes referred to as a "polyfunctional epoxy resin"). By containing a polyfunctional epoxy resin in the resin composition of the present invention, it becomes possible to introduce highly polar oxirane rings (epoxy groups) at a high density. This increases the effect of physical interactions such as van der Waals forces and hydrogen bonds, and tends to improve the adhesion between the metal and the cured resin in the composite molded product. Furthermore, by including a polyfunctional epoxy resin, the storage modulus of the cured resin tends to be easily adjusted to fall within the specific range described above, and adhesion between metal and the cured resin tends to be improved. Furthermore, by improving the reactivity of the oxirane ring (epoxy group), the amount of hydroxyl groups during the curing reaction can be reduced, and an increase in moisture absorption can be suppressed.
[0056] The polyfunctional epoxy resin may be used alone or in combination of two or more kinds.
[0057] The polyfunctional epoxy resin is an epoxy resin having three or more oxirane rings (epoxy groups) in one molecule, and preferably has four or more oxirane rings (epoxy groups) in one molecule. There is no particular upper limit to the number of oxirane rings (epoxy groups) in one molecule of the polyfunctional epoxy resin, but it is preferably 10 or less, more preferably 8 or less, and particularly preferably 6 or less. By keeping the number of oxirane rings (epoxy groups) in one molecule within this range, the adhesion between the metal and the cured resin is improved, and an increase in moisture absorption tends to be suppressed.
[0058] From the viewpoints of reaction rate and heat resistance, the oxirane ring (epoxy group) is more preferably a glycidyl group.
[0059] The resin composition of the present invention contains a polyfunctional epoxy resin having multiple oxirane rings (epoxy groups), particularly glycidyl groups, in one molecule, which improves the crosslink density of the cured product and tends to result in a stronger cured resin product. As a result, when internal stress occurs in the cured resin product during a moisture absorption reflow test, the cured resin product does not deform or break, but retains its shape, which tends to suppress the generation of voids and other spaces in the cured resin product.
[0060] The molecular weight of the polyfunctional epoxy resin is not particularly limited, but is preferably 1000 or less, more preferably 800 or less, and even more preferably 600 or less. The molecular weight of the polyfunctional epoxy resin is preferably 100 or more, and more preferably 150 or more. When the molecular weight of the polyfunctional epoxy resin is within the above range, the storage modulus at 200°C of the resin cured product after curing of the resin composition can be set to 1.0 x 10 7 It tends to be easier to achieve a value of 0.1 Pa or more.
[0061] Specifically, examples of polyfunctional epoxy resins that can be used include EX321L, DLC301, and DLC402 manufactured by Nagase Chemtex Corporation.
[0062] The content of the polyfunctional epoxy resin in the resin composition of the present invention is not particularly limited, but is preferably 5% by weight or more, and more preferably 10% by weight or more, based on 100% by weight of the solid content of the resin composition excluding the inorganic filler. It is also preferable that it is 50% by weight or less, more preferably 40% by weight or less, and even more preferably 30% by weight or less. It is further preferable that it is 5% by weight or more and 50% by weight or less, further preferably 10% by weight or more and 40% by weight or less, and particularly preferably 10% by weight or more and 30% by weight or less. When the content of the polyfunctional epoxy resin is equal to or more than the lower limit, the above-mentioned advantages due to the inclusion of the polyfunctional epoxy resin can be obtained. On the other hand, by making the content of the polyfunctional epoxy resin equal to or less than the upper limit, it is possible to suppress the moisture absorption of the cured resin material and to improve the strength performance of the cured resin material, thereby making it possible to achieve both of these performances.
[0063] ((Specific epoxy resin)) The resin in the resin composition of the present invention preferably contains an epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more (hereinafter, sometimes referred to as a "specific epoxy resin").
[0064] In the following description, the term "organic group" refers to any group containing carbon atoms. Examples of the organic group include alkyl groups, alkenyl groups, and aryl groups, which may be substituted with halogen atoms, groups containing heteroatoms, or other hydrocarbon groups.
[0065] The specific epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more preferably further has at least one structure selected from a structure represented by the following structural formula (1) (hereinafter, may be referred to as "Structure (1)") and a structure represented by the following structural formula (2) (hereinafter, may be referred to as "Structure (2)").
[0066] [ka]
[0067] (In formula (1), R 1 and R 2 Each represents an organic group. In formula (2), R 3 represents a divalent cyclic organic group.
[0068] Furthermore, the specific epoxy resin may be an epoxy resin having a structure represented by the following structural formula (3) (hereinafter, sometimes referred to as "structure (3)").
[0069] [ka]
[0070] (In formula (3), R 4 , R 5 , R6 , R 7 each independently represents an organic group having a molecular weight of 15 or more.
[0071] In the above formula (1), R 1 and R 2 At least one of them is preferably an organic group having a molecular weight of 16 or more, particularly a molecular weight of 16 to 1000. Examples include alkyl groups such as an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, and a heptyl group, and aryl groups such as a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a fluorenyl group.
[0072] R 1 and R 2 may both be organic groups having a molecular weight of 16 or more, or one may be an organic group having a molecular weight of 16 or more and the other may be an organic group having a molecular weight of 15 or less or a hydrogen atom. 1 and R 2 One of the groups is an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less, and it is particularly preferred that one of the groups is a methyl group and the other a phenyl group, since this makes it easier to control handleability such as the resin viscosity and also from the standpoint of strength of the cured product.
[0073] In formula (2), R 3 is a divalent cyclic organic group, which may be an aromatic ring structure such as a benzene ring structure, a naphthalene ring structure, a fluorene ring structure, etc., or an aliphatic ring structure such as cyclobutane, cyclopentane, cyclohexane, etc. In addition, they may independently have a substituent such as a hydrocarbon group or a halogen atom.
[0074] R 3 The divalent bond of R may be a divalent group on a single carbon atom or on different carbon atoms. Preferred examples include divalent aromatic groups having 6 to 100 carbon atoms and divalent groups derived from cycloalkanes having 2 to 100 carbon atoms, such as cyclopropane and cyclohexane. 3is particularly preferably a 3,3,5-trimethyl-1,1-cyclohexylene group represented by the following structural formula (4) from the viewpoints of controlling handleability such as the viscosity of the resin and strength of the cured product.
[0075] [ka]
[0076] In formula (3), R 4 , R 5 , R 6 , R 7 are each independently an organic group having a molecular weight of 15 or more. Preferably, they are alkyl groups having a molecular weight of 15 to 1000, and particularly preferably R 4 , R 5 , R 6 , R 7 It is preferable that all of the above be methyl groups from the viewpoints of controlling the handleability of the resin, such as viscosity, and strength of the cured product.
[0077] The specific epoxy resin is preferably an epoxy resin containing either one of Structure (1) and Structure (2) and a biphenyl structure, and more preferably an epoxy resin containing either one of Structure (1) and Structure (2) and Structure (3). When the specific epoxy resin contains these structures, it tends to suppress the moisture absorption of the cured product and to simultaneously achieve the strength retention performance of the resin composition.
[0078] Such specific epoxy resins are generally made of bisphenol A or bisphenol F. Compared to epoxy resins having a skeletal structure, they contain many hydrophobic hydrocarbon and aromatic structures. Therefore, by blending specific epoxy resins, the moisture absorption amount of the cured product of the resin composition can be reduced. From the viewpoint of reducing the amount of moisture absorption, the specific epoxy resin preferably contains a large amount of the hydrophobic structures (1), (2), and (3).
[0079] The weight average molecular weight of the specific epoxy resin is preferably 10,000 or more, more preferably 20,000 or more, and even more preferably 25,000 or more, and is preferably 80,000 or less, more preferably 70,000 or less, and even more preferably 60,000 or less.
[0080] The specific epoxy resin is preferably more hydrophobic, and specifically, the epoxy equivalent of the specific epoxy resin is preferably larger, more preferably 3,000 g / equivalent or more, more preferably 4,000 g / equivalent or more, and even more preferably 5,000 g / equivalent or more. The epoxy equivalent of the specific epoxy resin is preferably 20,000 g / equivalent or less, and more preferably 5,000 g / equivalent or more and 20,000 g / equivalent or less.
[0081] The weight average molecular weight of the epoxy resin is a value calculated as polystyrene, measured by gel permeation chromatography. The epoxy equivalent is defined as "the weight of an epoxy resin containing one equivalent of an epoxy group" and can be measured in accordance with JIS K7236.
[0082] Such specific epoxy resins may be used alone or in combination of two or more thereof. The specific epoxy resin may have a plurality of epoxy groups.
[0083] The content of the specific epoxy resin in the resin composition of the present invention is not particularly limited, but is preferably 5% by weight or more, more preferably 10% by weight or more, based on 100% by weight of the solid content of the resin composition excluding the inorganic filler. Also, it is preferably 50% by weight or less, more preferably 40% by weight or less. When the content of the specific epoxy resin is equal to or less than the upper limit, the storage modulus of the cured product tends to be improved or maintained, and the reflow resistance tends to be improved. When the content of the specific epoxy resin is equal to or more than the lower limit, the resin composition is easily applied, and the obtained cured resin tends to have flexibility.
[0084] ((Content ratio of specific epoxy resin to multifunctional epoxy resin)) In particular, it is preferable that the resin composition of the present invention contains both a specific epoxy resin and a polyfunctional epoxy resin as the epoxy resin, in order to achieve both high elasticity and low moisture absorption in the cured product of the resin composition.
[0085] When the resin composition of the present invention contains both the specific epoxy resin and the polyfunctional epoxy resin, the content ratio of the specific epoxy resin to the polyfunctional epoxy resin is not particularly limited, but is preferably specific epoxy resin:polyfunctional epoxy resin=10-90:90-10 (weight ratio), more preferably 20-80:80-20 (weight ratio), and particularly preferably 30-70:70-30 (weight ratio). When the content ratio of the specific epoxy resin to the polyfunctional epoxy resin is within this range, the storage modulus and weight increase rate described above can be easily controlled within appropriate ranges.
[0086] ((Other epoxy resins)) The resin composition of the present invention may contain an epoxy resin other than the specific epoxy resin and the polyfunctional epoxy resin. The epoxy resin other than the specific epoxy resin and the polyfunctional epoxy resin contained in the resin composition of the present invention is not particularly limited, but may be, for example, bisphenol A and various bisphenol-type epoxy resins obtained by glycidylating bisphenols such as bisphenol F-type epoxy resins; various biphenyl-type epoxy resins obtained by glycidylating biphenyls; epoxy resins obtained by glycidylating aromatic compounds having two hydroxyl groups such as dihydroxynaphthalene and 9,9-bis(4-hydroxyphenyl)fluorene; epoxy resins obtained by glycidylating trisphenols such as 1,1,1-tris(4-hydroxyphenyl)methane; epoxy resins obtained by glycidylating tetrakisphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane; novolac-type epoxy resins obtained by glycidylating novolacs such as phenol novolac, cresol novolac, bisphenol A novolac, and brominated bisphenol A novolac; and silicone-containing epoxy resins.
[0087] <Inorganic filler> In the present invention, inorganic fillers include agglomerated inorganic fillers and non-agglomerated inorganic fillers.
[0088] The resin composition of the present invention comprises an aggregated inorganic filler. The resin composition of the present invention may contain a non-agglomerated inorganic filler in addition to the agglomerated inorganic filler. The non-agglomerated inorganic filler also includes a spherical filler, which will be described later.
[0089] By containing the aggregated inorganic filler in the resin composition of the present invention, it is possible to improve the thermal conductivity and insulating properties of the cured resin and control the linear expansion coefficient. In particular, in the pressurizing step described below, the aggregated inorganic fillers are deformed by contacting each other, and by contacting each other on the surface, more thermal conduction paths are formed, so that a cured resin with high thermal conductivity can be obtained. In addition, by deforming the aggregated inorganic filler, the gaps or voids between the fillers can be effectively removed, and the insulating properties are improved.
[0090] The resin composition of the present invention contains a resin and an inorganic filler, and by using the above-mentioned epoxy resin suitable for the present invention in combination with the aggregated inorganic filler, the deformed state of the filler can be maintained even after the aggregated inorganic filler is deformed in the pressurizing step described below. Furthermore, by having the weight increase rate after curing of the resin composition of the present invention be within the above-mentioned specific range, the deformed state of the filler can be maintained even after the moisture absorption reflow step.
[0091] When the resin composition and the cured resin contain only a single filler such as silica or alumina, even after the pressurization process, the contact between the fillers is point contact, and it is not possible to effectively form a heat conduction path. Furthermore, the gaps or voids between the fillers cannot be removed, and the insulation properties may be reduced.
[0092] The aggregate morphology of the aggregated inorganic filler can be confirmed by a scanning electron microscope (SEM).
[0093] (Agglomerated inorganic filler) As the aggregated inorganic filler, an electrically insulating filler can be used, and examples thereof include those composed of at least one type of inorganic particles selected from the group consisting of metal carbides, metal oxides, and metal nitrides.
[0094] Examples of metal carbides include silicon carbide, titanium carbide, tungsten carbide, and the like. Examples of metal oxides include magnesium oxide, aluminum oxide, silicon oxide, calcium oxide, zinc oxide, yttrium oxide, zirconium oxide, cerium oxide, ytterbium oxide, and sialon (ceramics composed of silicon, aluminum, oxygen, and nitrogen). Examples of metal nitrides include boron nitride, aluminum nitride, silicon nitride, etc. .
[0095] In particular, when used in applications requiring insulation, such as power semiconductors, agglomerated inorganic fillers have a volume resistivity of 1×10 13 Ω cm or more, especially 1×10 14 It is preferable that the inorganic particles constituting the aggregated inorganic filler are made of an inorganic compound having excellent insulating properties of Ω·cm or more. In particular, the inorganic particles constituting the aggregated inorganic filler are preferably made of a metal oxide and / or a metal nitride, since the electrical insulating properties of the cured resin are sufficient.
[0096] Specific examples of such metal oxides and metal nitrides include alumina (Al2O3, volume resistivity 1×10 14 Ω cm), aluminum nitride (AlN, volume resistivity 1×10 14 Ω·cm), boron nitride (BN, volume resistivity 1×10 14 Ω·cm), silicon nitride (Si3N4, volume resistivity 1×10 14 Ω cm), silica (SiO2, volume resistivity 1×10 14 Among them, alumina, aluminum nitride, boron nitride, and silica are preferable, and alumina and boron nitride are particularly preferable.
[0097] There are no particular limitations on the method or degree of agglomeration of the agglomerated inorganic filler. The aggregated inorganic filler may be surface-treated with a surface treatment agent. As the surface treatment agent, a known surface treatment agent can be used.
[0098] The aggregated inorganic filler may be used alone or in any combination and ratio of two or more kinds.
[0099] As the agglomerated inorganic filler, it is preferable to use the following agglomerated boron nitride particles, from the viewpoint of effectively exerting the above-mentioned effects of using the agglomerated inorganic filler. The agglomerated boron nitride particles may be used in combination with inorganic fillers of different shapes and types.
[0100] (Boron nitride agglomerated particles) Boron nitride has high thermal conductivity, but because it is scaly, it has excellent thermal conductivity in the planar direction but has high thermal resistance in the direction perpendicular to the plane. Agglomerated particles made by aggregating such scaly particles into a spherical shape are preferable because they are easy to handle.
[0101] In boron nitride agglomerated particles, in which boron nitride particles are layered like cabbage, the radial direction of the agglomerated particle becomes the direction in which the thermal resistance is greatest. As the boron nitride agglomerated particles, those in which the boron nitride particles are aligned in the planar direction so that the radial direction of the agglomerated particles is the direction of good thermal conductivity are preferred.
[0102] The boron nitride agglomerated particles also preferably have a house-of-cards structure. The "house of card structure" is described, for example, in Ceramics 43 No. 2 (published by the Ceramic Society of Japan in 2008), and is a structure in which plate-like particles are not oriented but are laminated in a complex manner. More specifically, boron nitride agglomerated particles having a house of card structure are aggregates of boron nitride primary particles, and have a structure in which the flat surfaces and end surfaces of the primary particles are in contact with each other to form, for example, a T-shaped aggregate.
[0103] As the boron nitride agglomerated particles used in the present invention, the above-mentioned agglomerated particles of boron nitride having a house-of-card structure are particularly preferred. By using the agglomerated particles of boron nitride having a house-of-card structure, the thermal conductivity can be further increased.
[0104] The new Mohs hardness of the boron nitride agglomerated particles is not particularly limited, but is preferably not more than 5. There is no particular lower limit to the new Mohs hardness of the boron nitride agglomerated particles, but it is, for example, 1 or more.
[0105] When the new Mohs hardness is 5 or less, the particles dispersed in the resin composition tend to come into surface contact with each other, forming heat conduction paths between the particles and tending to improve the thermal conductivity of the cured resin.
[0106] The volume average particle diameter of the boron nitride agglomerated particles is not particularly limited, but is preferably 10 μm or more, more preferably 15 μm or more. The volume average particle diameter of the boron nitride agglomerated particles is preferably 100 μm or less, more preferably 90 μm or less. When the volume average particle diameter is equal to or more than the lower limit, the interparticle interface is suppressed in the resin composition and the cured resin, so that the thermal resistance is reduced and high thermal conductivity tends to be obtained. When the volume average particle diameter is equal to or less than the upper limit, the cured resin tends to have a smooth surface.
[0107] The volume average particle size of the boron nitride agglomerated particles means the particle size at which the cumulative volume is 50% when a cumulative curve is drawn with the volume of the powder used for measurement being 100%. Methods for measuring the volume average particle size include a wet measurement method in which a sample in which aggregated particles are dispersed in a pure water medium containing sodium hexametaphosphate as a dispersion stabilizer is measured using a laser diffraction / scattering particle size distribution measuring device, and a dry measurement method in which the measurement is performed using Malvern's "Morphologi." The same applies to the volume average particle size of the spherical inorganic filler described below.
[0108] (Agglomerated inorganic filler content) The content of the aggregated inorganic filler in the resin composition of the present invention is preferably 30% by weight or more, more preferably 40% by weight or more, and even more preferably 45% by weight or more, based on 100% by weight of the solid content of the resin composition. The content of the aggregated inorganic filler in the resin composition of the present invention is preferably 99% by weight or less, more preferably 90% by weight or less, and even more preferably 80% by weight or less, based on 100% by weight of the solid content of the resin composition. When the content of the aggregated inorganic filler is equal to or more than the above lower limit, the effect of improving thermal conductivity and the effect of controlling the linear expansion coefficient due to the inclusion of the aggregated inorganic filler tend to be sufficiently obtained. When the content of the aggregated inorganic filler is equal to or less than the above upper limit, the moldability of the resin composition and the resin cured product and the interfacial adhesion in the composite molded product tend to be improved.
[0109] (Non-agglomerated inorganic filler) The resin composition of the present invention may contain, as the inorganic filler, a non-agglomerated inorganic filler together with an agglomerated inorganic filler.
[0110] The non-agglomerated inorganic filler preferably includes a spherical inorganic filler having a thermal conductivity of 10 W / m·K or more, preferably 15 W / m·K or more, more preferably 20 W / m·K or more, for example, 20 to 30 W / m·K, and a new Mohs hardness of 3.1 or more, for example, 5 to 10. By using such a spherical inorganic filler in combination with the above-mentioned agglomerated inorganic filler, the adhesive strength to metal and heat dissipation properties of the obtained resin cured product can be improved.
[0111] Here, "spherical" refers to anything that is generally recognized as being spherical, and for example, an average circularity of 0.4 or more may be considered spherical, and an average circularity of 0.6 or more may be considered spherical. Usually, the upper limit of the average circularity is 1. The circularity can be measured by subjecting the projected image to image processing, and can be measured, for example, with Sysmex Corporation's FPIA series.
[0112] The spherical inorganic filler is preferably at least one selected from the group consisting of alumina, synthetic magnesite, silica, aluminum nitride, silicon nitride, silicon carbide, zinc oxide, and magnesium oxide. By using these preferable spherical inorganic fillers, the heat dissipation properties of the obtained resin cured product can be further improved.
[0113] The volume average particle diameter of the spherical inorganic filler is preferably in the range of 0.5 μm or more and 40 μm or less. By having a volume average particle diameter of 0.5 μm or more, the resin and the inorganic filler can easily flow during hot molding, and it is considered that the interfacial adhesive strength of the composite molded product of the present invention can be increased. In addition, by having an average particle diameter of 40 μm or less, it becomes easier to maintain the dielectric breakdown characteristics of the resin cured product.
[0114] When an aggregated inorganic filler and a non-aggregated inorganic filler are used in combination as the inorganic filler, the content ratio of the aggregated inorganic filler to the non-aggregated inorganic filler in the resin composition is not particularly limited, but is preferably 90:10 to 10:90 by weight, and more preferably 80:20 to 20:80.
[0115] The total content of the aggregated inorganic filler and the non-aggregated inorganic filler in the resin composition of the present invention is preferably 30% by weight or more, more preferably 40% by weight or more, and even more preferably 50% by weight or more, based on 100% by weight of the solid content of the resin composition. The total content of the aggregated inorganic filler and the non-aggregated inorganic filler in the resin composition of the present invention is preferably 99% by weight or less, more preferably 90% by weight or less, and even more preferably 80% by weight or less, based on 100% by weight of the solid content of the resin composition.
[0116] <Other ingredients> The resin composition of the present invention may contain other components in addition to those described above, as long as the effects of the present invention are not impaired. Examples of other components include a compound having a heterocyclic structure containing a nitrogen atom, a curing agent, a curing catalyst, a surface treatment agent such as a silane coupling agent that improves the interfacial adhesive strength between an inorganic filler and a resin, an insulating carbon component such as a reducing agent, a viscosity adjuster, a dispersant, a thixotropy imparting agent, a flame retardant, a colorant, an organic filler, an organic solvent, a thermoplastic resin, etc. The presence or absence of other components in the resin composition of the present invention and the content ratio thereof are not particularly limited as long as the effects of the present invention are not significantly impaired.
[0117] (Compounds having a heterocyclic structure containing a nitrogen atom) The resin composition of the present invention may contain a compound having a heterocyclic structure containing a nitrogen atom.
[0118] By containing a compound having a heterocyclic structure containing a nitrogen atom (hereinafter, sometimes referred to as "nitrogen-containing heterocyclic compound"), the effect of improving the adhesion between the resin cured product obtained from the resin composition of the present invention and metal tends to be achieved. That is, when the resin composition or the resin cured product is composited with a metal, the nitrogen-containing heterocyclic compound is located at the interface between them, thereby improving the adhesion between the resin composition or the resin cured product and the metal. From this viewpoint, in order to make it easier for the nitrogen-containing heterocyclic compound to remain at the interface between the resin composition or the resin cured product and the metal, it is more preferable that the nitrogen-containing heterocyclic compound has a low molecular weight. The molecular weight of the nitrogen-containing heterocyclic compound is preferably 1,000 or less, more preferably 500 or less. There is no particular lower limit to the molecular weight of the nitrogen-containing heterocyclic compound, but it is preferably 60 or more, more preferably 70 or more.
[0119] Examples of the heterocyclic structure of the nitrogen-containing heterocyclic compound include structures derived from imidazole, triazine, triazole, pyrimidine, pyrazine, pyridine, and azole. The nitrogen-containing heterocyclic compound may have a plurality of heterocyclic structures simultaneously in one molecule. From the viewpoint of improving the insulating properties of the resin composition and adhesion to metals, nitrogen-containing heterocyclic compounds The imidazole-based compounds and triazine-based compounds are preferred.
[0120] Examples of the imidazole-based compound and the triazine-based compound that are preferable as the nitrogen-containing heterocyclic compound include 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino- Examples of the isocyanuric acid adduct include 6-[2'-ethyl-4'methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-vinyl-s-triazine, 2,4-diamino-6-vinyl-s-triazine isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, and 2,4-diamino-6-methacryloyloxyethyl-s-triazine isocyanuric acid adduct.
[0121] Among these, the structure derived from imidazole and the structure derived from triazine are particularly preferred, and the structure derived from triazine is particularly preferred, and the heterocyclic structure of the nitrogen-containing heterocyclic compound is particularly preferably the structure derived from 1,3,5-triazine. The structure may also have a plurality of structural parts exemplified by these. By having the above structure, the resin compatibility of the nitrogen-containing heterocyclic compound tends to be high and the reaction activation temperature tends to be high. Therefore, the curing speed and physical properties after curing can be easily adjusted, which tends to improve the storage stability of the resin composition and further improve the adhesive strength after hot molding.
[0122] The nitrogen-containing heterocyclic compound may contain a curing catalyst, which will be described later, depending on the structure. Therefore, the resin composition of the present invention may contain a nitrogen-containing heterocyclic compound as a curing catalyst.
[0123] The nitrogen-containing heterocyclic compounds may be used alone or in combination of two or more.
[0124] The content of the nitrogen-containing heterocyclic compound is preferably 0.001% by weight or more, more preferably 0.1% by weight or more, and even more preferably 0.5% by weight or more, based on 100% by weight of the solid content of the resin composition excluding inorganic filler. The content of the nitrogen-containing heterocyclic compound is preferably 10% by weight or less, more preferably 7% by weight or less, and even more preferably 5% by weight or less, based on 100% by weight of the solid content of the resin composition excluding inorganic filler. By the content of the nitrogen-containing heterocyclic compound being within the above range, it tends to be easy to control the storage modulus and weight increase rate within the above-mentioned specific range.
[0125] When the curing catalyst described later is contained in the nitrogen-containing heterocyclic compound because of its molecular structure, the total amount including the content of the nitrogen-containing heterocyclic compound is preferably within the above range. When the content of the nitrogen-containing heterocyclic compound is equal to or more than the above lower limit, the above effect of containing the compound can be sufficiently obtained, and when it is equal to or less than the above upper limit, the reaction proceeds effectively, the crosslinking density is improved, the strength is increased, and the storage stability is improved.
[0126] (hardening agent) The resin composition of the present invention may contain a curing agent.
[0127] Although not particularly limited, preferred curing agents are phenol resins, acid anhydrides having an aromatic or alicyclic skeleton, water additives of the acid anhydrides, or modified products of the acid anhydrides. By using these preferred curing agents, a resin cured product having an excellent balance of heat resistance, moisture resistance, and electrical properties can be obtained.
[0128] The curing agent may be used alone or in combination of two or more kinds.
[0129] The phenol resin is not particularly limited. Specific examples of the phenol resin include phenol novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, dicyclopentadiene cresol, polyparavinylphenol, bisphenol A type novolac, xylylene modified novolac, decalin modified novolac, poly(di-o-hydroxyphenyl)methane, poly(di-m-hydroxyphenyl)methane, and poly(di-p-hydroxyphenyl)methane. In order to further improve the flexibility and flame retardancy of the resin composition and to improve the mechanical properties and heat resistance of the cured resin, novolac-type phenolic resins having a rigid main chain skeleton and phenolic resins having a triazine skeleton are preferred. In order to improve the flexibility of the uncured resin composition and the toughness of the cured resin, a phenol resin having an allyl group is preferred.
[0130] Commercially available phenolic resins include MEH-8005, MEH-8000H, and NEH-8015 (all manufactured by Meiwa Chemical Industry Co., Ltd.), YLH903 (manufactured by Mitsubishi Chemical Corporation), LA-7052, LA-7054, LA-7751, LA-1356, and LA-3018-50P (all manufactured by Dainippon Ink Co., Ltd.), as well as PSM6200, PS6313, and PS6492 (manufactured by Gun-ei Chemical Industry Co., Ltd.).
[0131] The acid anhydride having an aromatic skeleton, the water additive of the acid anhydride, or the modified product of the acid anhydride is not particularly limited.Specific examples include SMA resin EF30 and SMA resin EF60 (both manufactured by Sartomer Japan), ODPA-M and PEPA (both manufactured by Manac), Ricadit MTA-10, Ricadit TMTA, Ricadit TMEG-200, Ricadit TMEG-500, Ricadit TMEG-S, Ricadit TH, Ricadit MH-700, Ricadit MT-500, Ricadit DSDA and Ricadit TDA-100 (both manufactured by New Japan Chemical Industry Co., Ltd.), EPICLON B4400, and EPICLON B570 (both manufactured by Dainippon Ink and Chemicals Co., Ltd.).
[0132] The acid anhydride having an alicyclic skeleton, the water addition product of the acid anhydride, or the modified product of the acid anhydride is preferably the acid anhydride having a polyalicyclic skeleton, the water addition product of the acid anhydride, or the modified product of the acid anhydride, or the acid anhydride having an alicyclic skeleton obtained by the addition reaction of a terpene compound and maleic anhydride, the water addition product of the acid anhydride, or the modified product of the acid anhydride.Specific examples include Ricajit HNA and Ricajit HNA-100 (both manufactured by New Japan Chemical Co., Ltd.), and Epicure YH306 and Epicure YH309 (both manufactured by Mitsubishi Chemical Corporation).
[0133] The resin composition of the present invention may or may not contain a curing agent. When the resin composition of the present invention contains a curing agent, the content of the curing agent is not particularly limited.
[0134] When the resin composition of the present invention contains a curing agent, it is preferably contained in an amount of 0.5 to 70% by weight, particularly 0.5 to 55% by weight, based on 100% by weight of the solid content of the resin composition excluding the inorganic filler. When the content of the curing agent is equal to or more than the lower limit, sufficient curing performance can be obtained, and when it is equal to or less than the upper limit, the reaction proceeds effectively, the crosslinking density can be improved, and the strength can be increased. This improves film-forming properties. In addition, when the resin composition contains a curing agent, the curing agent is preferably present in an amount of 0 to 55% by weight relative to the epoxy equivalent in the resin composition. By being in the above range, the reaction proceeds effectively, the crosslinking density can be improved, the strength can be increased, and the film formability tends to be improved.
[0135] (curing catalyst) The resin composition of the present invention may contain a curing catalyst. In order to adjust the curing speed and the physical properties of the cured product, it is preferable to contain a curing catalyst together with the above-mentioned curing agent.
[0136] The curing catalyst is not particularly limited, but is appropriately selected according to the type of resin and curing agent used.Specific examples of the curing catalyst include chain or cyclic tertiary amines, organic phosphorus compounds, quaternary phosphonium salts, diazabicycloalkenes such as organic acid salts, etc.In addition, organic metal compounds, quaternary ammonium salts, metal halides, etc. can also be used. Examples of the organometallic compounds include zinc octoate, tin octoate, and aluminum acetylacetone complex. These may be used alone or in combination of two or more.
[0137] When the resin composition of the present invention contains a curing catalyst, the curing catalyst is preferably contained in an amount of 0.1 to 10% by weight, particularly 0.1 to 5% by weight, based on 100% by weight of the solid content of the resin composition excluding the inorganic filler. When the content of the curing catalyst is equal to or more than the lower limit, the progress of the curing reaction can be sufficiently promoted to achieve good curing. When the content of the curing catalyst is equal to or less than the upper limit, the curing speed is not too fast, and therefore the storage stability of the resin composition of the present invention can be improved.
[0138] (solvent) The resin composition of the present invention may contain an organic solvent, for example, in order to improve the coatability when a sheet-like cured resin product is formed through a coating step.
[0139] Examples of the organic solvent that may be contained in the resin composition of the present invention include methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, butyl acetate, isobutyl acetate, and propylene glycol monomethyl ether. These organic solvents may be used alone or in combination of two or more kinds.
[0140] When the resin composition of the present invention contains an organic solvent, the content thereof is appropriately determined depending on the handleability of the resin composition when producing a cured resin product, the shape before curing, drying conditions, and the like. When the resin composition of the present invention is in the form of a slurry to be subjected to the coating step described below, the organic solvent is preferably used so that the solid content of the resin composition of the present invention becomes 10 to 90% by weight, particularly 40 to 80% by weight. When the resin composition of the present invention is in the form of a sheet that has been subjected to processes such as coating and drying, the solid content of the resin composition of the present invention is preferably 95% by weight or more, and more preferably 98% by weight or more.
[0141] (Dispersant) The resin composition of the present invention may contain a dispersant. When the resin composition of the present invention contains a dispersant, it becomes possible to form a uniform cured resin product, and the thermal conductivity and dielectric breakdown characteristics of the obtained cured resin product may be improved.
[0142] The dispersant preferably has a functional group containing a hydrogen atom capable of bonding with hydrogen. When the dispersant has a functional group containing a hydrogen atom capable of bonding with hydrogen, the thermal conductivity and dielectric breakdown characteristics of the resulting cured resin material can be further improved. Examples of functional groups containing a carboxyl group (pKa=4), a phosphate group (pKa=7), or a phenol group (pKa=10) can be given.
[0143] The pKa of the functional group containing a hydrogen atom having hydrogen bonding ability is preferably in the range of 2 to 10, more preferably in the range of 3 to 9. When the pKa is 2 or more, the acidity of the dispersant is in an appropriate range, and the reaction of the epoxy resin in the resin component may be easily suppressed. Therefore, when the molded product in an uncured state is stored, the storage stability tends to be improved. When the pKa is 10 or less, the function as a dispersant is sufficiently performed, and the thermal conductivity and dielectric breakdown characteristics of the resin cured product tend to be sufficiently improved.
[0144] The functional group containing a hydrogen atom capable of forming a hydrogen bond is preferably a carboxyl group or a phosphate group, which can further improve the thermal conductivity and dielectric breakdown characteristics of the cured resin.
[0145] Specific examples of the dispersant include polyester-based carboxylic acids, polyether-based carboxylic acids, polyacrylic-based carboxylic acids, aliphatic carboxylic acids, polysiloxane-based carboxylic acids, polyester-based phosphoric acids, polyether-based phosphoric acids, polyacrylic-based phosphoric acids, aliphatic phosphoric acids, polysiloxane-based phosphoric acids, polyester-based phenols, polyether-based phenols, polyacrylic-based phenols, and polysiloxane-based phenols. The dispersant may be used alone or in combination of two or more kinds.
[0146] (Organic filler / thermoplastic resin) The resin composition of the present invention may contain an organic filler and / or a thermoplastic resin. When the resin composition of the present invention contains an organic filler or a thermoplastic resin, the resin composition may be given appropriate elongation, the generated stress may be alleviated, and the generation of cracks during a temperature cycle test may be suppressed.
[0147] Any generally known thermoplastic resin can be used as the thermoplastic resin. Examples of the thermoplastic resin include vinyl polymers such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, (meth)acrylic resin, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer, polyesters such as polylactic acid resin, polyethylene terephthalate, and polybutylene terephthalate, polyamides such as nylon and polyamidoamine, polyvinyl acetal resins such as polyvinyl acetoacetal, polyvinyl benzal, and polyvinyl butyral resins, ionomer resins, polyphenylene ether, polyphenylene sulfide, polycarbonate, polyether ether ketone, polyacetal, ABS resin, LCP (liquid crystal polymer), fluororesin, urethane resin, silicone resin, various elastomers, and modified products of these resins.
[0148] The thermoplastic resin may be uniform in the resin phase of the cured resin, or may be phase-separated and have a recognizable shape. In the case of phase separation, the shape of the thermoplastic resin in the cured resin may be particulate or fibrous. In this way, when the shape of the thermoplastic resin is recognizable in the cured resin, the thermoplastic resin may be recognized as an organic filler. However, in the present invention, the organic filler refers to natural products such as wood flour, cellulose which may be modified, starch, various organic pigments, etc., and the thermoplastic resin is not included in the organic filler.
[0149] When the thermoplastic resin or organic filler is insoluble in the resin, the viscosity of the resin composition is prevented from increasing, and when the resin composition is molded into a sheet as described below, the smoothness of the sheet surface can be improved. In this case, by simultaneously mixing the thermoplastic resin and organic filler that are insoluble in the resin with a large amount of inorganic filler, the component phase that is thermoplastic and has good elongation can be efficiently formed. Therefore, the occurrence of cracks in the cured resin can be suppressed without decreasing the elastic modulus of the cured resin. From these viewpoints, preferred thermoplastic resins are polyamide resins such as nylon and cellulose resins, and particularly preferred are polyamide resins such as nylon.
[0150] When the thermoplastic resin that can be observed in the cured resin is in the form of particles, the upper limit of the average particle size is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. By making the average particle size of the particulate thermoplastic resin in the cured resin not more than the above upper limit, it is possible to produce sheet-shaped cured products of various thicknesses without causing a decrease in thermal conductivity. The average particle size of the particulate thermoplastic resin is determined by observing a cross section of the cured resin and averaging the longest diameters of any 20 particles.
[0151] <Cured resin> The cured resin product of the present invention is a cured resin product using a resin composition containing an inorganic aggregate filler, and the cured resin product has a weight increase rate of 0.80% or less at 85° C. and 85% RH, and the storage modulus at 200° C. after curing of the resin composition excluding the inorganic filler is 1.0×10 7 It is more than Pa.
[0152] In the present invention, the term "resin composition" refers to a resin composition containing an aggregated inorganic filler and a resin, which is uncured. Although not particularly limited, it is preferably a mixture of an aggregated inorganic filler and a thermosetting resin component such as an epoxy resin, a curing agent for curing the resin, a curing catalyst serving as a curing assistant, etc., and more preferably contains a compound having a heterocyclic structure containing a nitrogen atom. For example, the above-mentioned resin composition can be mentioned. The resin composition excluding the inorganic filler refers to the components other than the inorganic filler in the resin composition. The resin, the curing agent, the curing catalyst, the compound having a heterocyclic structure containing a nitrogen atom, the inorganic filler, the inorganic aggregate filler, and other components are the same as those in the above-mentioned resin composition, and the preferred ranges thereof are also the same.
[0153] The "cured resin" of the present invention refers to a product obtained by curing a resin composition. The cured resin of the present invention is in a state in which the exothermic peak obtained when the temperature is raised from 40°C to 250°C at a rate of 10°C / min by DSC is 10 J / g or less. The method for obtaining the cured resin product of the present invention is not particularly limited, and may be, for example, a method for obtaining the product by curing the above-mentioned resin composition.
[0154] [Storage modulus] The storage modulus at 200°C after curing of the resin composition excluding the inorganic filler is 1.0 x 10 7 From the viewpoint of maintaining performance after moisture absorption and reflow testing, the storage modulus is 1.3×10 7 Pa or more, and 1.5×10 7 More preferably, the pressure is 1.7×10 Pa or more. 7 On the other hand, the storage modulus is preferably 5×10 9 Pa or less, and 1×10 9 Pa or less is more preferable, and 5×10 8 It is more preferable that the pressure is 0.1 Pa or less. By ensuring that the storage modulus is equal to or less than the above upper limit, excessive internal stress caused by a moisture absorption reflow test can be suppressed, and cracking of the obtained cured resin material and interfacial peeling between metal and the cured resin material tend to be suppressed. When the storage modulus is within the above range, the cured resin can easily penetrate into the unevenness of the metal, which is the adherend described below, and the cured resin that has penetrated into the unevenness exhibits a strong anchor effect, tending to improve adhesion between the metal and the cured resin.
[0155] In this way, in order to control the storage modulus of the resin of the cured resin to a specific range, This can be achieved by introducing a rigid structure such as an aromatic ring into the components constituting the resin composition used to obtain the cured product, or by introducing a polyfunctional component having multiple reactive groups to increase the crosslink density of the cured product. It can also be achieved by obtaining a resin cured product using the above-mentioned resin composition.
[0156] The storage modulus may be measured by any conventionally known method, and specifically, the method described in the Examples section below can be mentioned.
[0157] [Weight increase rate] The cured resin (containing an inorganic filler) of the present invention has a weight gain of 0.8% or less at 85° C. and 85% RH. If the weight gain exceeds 0.8%, the object of the present invention, namely, maintaining high insulation properties and preventing interfacial peeling after a moisture absorption reflow test, cannot be achieved. From the viewpoint of maintaining high insulation properties and preventing interfacial peeling after a moisture absorption reflow test, the smaller this weight increase rate is the more preferable, and it is preferably 0.75% or less, and more preferably 0.7% or less. The lower limit of the weight increase rate is not particularly limited, but from the viewpoint of achieving both strength and insulating performance of the resin cured product and film formability, it is, for example, 0.2% or more. There are various possible causes of the weight increase of the cured resin, but it is important to control the weight increase due to moisture absorption. The present invention has found that the problem of the present invention can be solved by the specific range described above.
[0158] A method for obtaining a cured resin having a weight gain rate within a specific range at 85° C. and 85% RH can be, for example, by controlling the weight gain rate by introducing a highly hydrophobic structure such as an aliphatic skeleton or an aromatic ring into the constituent components. It can also be realized by obtaining a cured resin using the above-mentioned resin composition.
[0159] The weight gain of the cured resin of the present invention at 85° C. and 85% RH is measured by the method described in the Examples section below.
[0160] [Production of resin composition and cured resin] The method for producing the resin composition of the present invention and the cured resin product of the present invention will be described below by taking as an example a method for producing a sheet-shaped cured resin product made of the resin composition of the present invention.
[0161] The sheet-shaped cured resin product can be produced by a commonly used method, for example, by preparing the resin composition of the present invention, forming it into a sheet, and curing it.
[0162] The resin composition of the present invention can be obtained by uniformly mixing the inorganic aggregate filler, the resin, and other components added as necessary by stirring or kneading. For mixing, a general kneading device such as a mixer, a kneader, a single-screw or twin-screw kneader, etc. may be used. During mixing, heating may be performed as necessary.
[0163] The order of mixing the components may be arbitrary as long as there are no particular problems such as the occurrence of reactions or precipitation. For example, the following method may be mentioned. A resin is mixed and dissolved in an organic solvent (e.g., methyl ethyl ketone) to prepare a resin liquid, and a thoroughly mixed inorganic aggregate filler and other components are added to the obtained resin liquid and mixed. After that, an organic solvent is further added for viscosity adjustment and mixed, and then additives such as a curing agent, a curing accelerator, or a dispersing agent are further added and mixed.
[0164] The prepared resin composition can be molded into a sheet by any commonly used method. For example, when the resin composition has plasticity and fluidity, the resin composition can be molded into a desired shape by, for example, curing the resin composition while it is contained in a mold. In this case, injection molding, injection compression molding, extrusion molding, compression molding, and vacuum compression molding can be used.
[0165] The solvent in the resin composition can be removed by a known heating method such as using a hot plate, a hot air oven, an IR heating oven, a vacuum dryer, or a high-frequency heater.
[0166] A sheet-like cured resin product can also be obtained by cutting a cured resin composition into a desired shape.
[0167] The sheet-like cured resin product can also be obtained by forming a slurry-like resin composition into a sheet by a doctor blade method, a solvent casting method, an extrusion film formation method or the like.
[0168] An example of a method for producing a sheet-shaped cured product using this slurry-like resin composition will now be described.
[0169] <Coating process> First, a slurry-like resin composition is applied to the surface of a substrate to form a coating film (a sheet-like resin composition).
[0170] The slurry resin composition is used to form a coating film on a substrate by a dip method, a spin coat method, a spray coat method, a blade method, or any other method. A coating device such as a spin coater, a slit coater, a die coater, or a blade coater can be used to coat the slurry resin composition. Such a coating device can uniformly form a coating film of a predetermined thickness on the substrate.
[0171] As the substrate, a copper plate or copper foil or a PET film, which will be described later, is generally used, but there is no limitation thereto.
[0172] <Drying process> The coating film formed by applying the slurry-like resin composition is dried usually at a temperature of 10 to 150°C, preferably 25 to 120°C, and more preferably 30 to 110°C in order to remove the solvent and low molecular weight components. By setting the drying temperature to the upper limit or lower, curing of the resin in the slurry-like resin composition is suppressed, and the resin in the sheet-like resin composition tends to flow in the subsequent pressurizing step, making it easier to remove voids. By setting the drying temperature to the lower limit or higher, the solvent can be effectively removed, and productivity tends to improve.
[0173] The drying time is not particularly limited, and can be appropriately adjusted depending on the state of the slurry-like resin composition, the drying environment, etc. The drying time is preferably 1 minute or more, more preferably 2 minutes or more, even more preferably 5 minutes or more, even more preferably 10 minutes or more, particularly preferably 20 minutes or more, and most preferably 30 minutes or more. The drying time is preferably 24 hours or less, more preferably 10 hours or less, even more preferably 4 hours or less, and particularly preferably 2 hours or less. By setting the drying time to the above lower limit or more, the solvent can be sufficiently removed, and the residual solvent tends to be prevented from forming voids in the cured resin. By setting the drying time to the above upper limit or less, the productivity tends to be improved, and the production cost tends to be reduced.
[0174] <Pressing process> After the drying step, it is desirable to subject the obtained sheet-like resin composition to a pressurizing step for the purposes of bonding the aggregated inorganic fillers together to form a heat conduction path, eliminating voids and gaps in the sheet, improving adhesion to the substrate, etc.
[0175] The pressurizing step is desirably carried out by applying a load of 2 MPa or more to the sheet-shaped resin composition on the substrate. The load is preferably 5 MPa or more, more preferably 7 MPa or more, and even more preferably 9 MPa or more. The load is preferably 1500 MPa or less, more preferably 1000 MPa or less, and even more preferably 800 MPa or less. By setting the load during pressing to the above upper limit or less, the secondary particles of the aggregated inorganic filler are not destroyed, and a sheet having high thermal conductivity and no voids in the sheet-like cured resin can be obtained. By setting the load to the above lower limit or more, contact between the aggregated inorganic filler particles becomes good, making it easier to form a thermal conduction path, and a cured resin product having high thermal conductivity can be obtained.
[0176] The heating temperature of the sheet-shaped resin composition on the substrate in the pressurizing step is not particularly limited. The heating temperature is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher. The heating temperature is preferably 300° C. or lower, more preferably 250° C. or lower, even more preferably 200° C. or lower, even more preferably 100° C. or lower, and particularly preferably 90° C. or lower. By carrying out the pressurizing step within this temperature range, the melt viscosity of the resin in the sheet-shaped resin composition can be reduced, and voids and gaps in the cured resin can be further reduced. In addition, by heating at or below the upper limit, decomposition of organic components in the sheet-shaped resin composition and the cured resin and voids caused by residual solvent tend to be suppressed.
[0177] The time of the pressurizing step is not particularly limited. The time of the pressurizing step is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 3 minutes or more, and particularly preferably 5 minutes or more. The time of the pressurizing step is preferably 1 hour or less, more preferably 30 minutes or less, and even more preferably 20 minutes or less. By keeping the pressurizing time at or below the upper limit, the production time of the cured resin can be reduced, and the production cost tends to be reduced. By keeping the pressurizing time at or above the lower limit, the gaps and voids in the cured resin can be sufficiently removed, and the heat transfer performance and the voltage resistance characteristics tend to be improved.
[0178] <Curing process> The curing step for completely curing the resin composition of the present invention may be carried out under pressure or without pressure. Also, the pressurizing step and the curing step may be carried out simultaneously.
[0179] The load when the pressing step and the curing step are performed simultaneously is not particularly limited. In this case, it is preferable to apply a load of 5 MPa or more to the sheet-shaped resin composition on the substrate, more preferably 7 Pa or more, even more preferably 9 MPa or more, and particularly preferably 20 MPa or more. In addition, the load is preferably 2000 MPa or less, more preferably 1500 MPa or less. By setting the load when the pressurizing step and the curing step are carried out simultaneously to the above upper limit value or less, the secondary particles of the aggregated inorganic filler are not destroyed, and a sheet-like cured resin product having high thermal conductivity and no voids in the sheet-like cured resin product can be obtained. In addition, by setting the load to the above lower limit value or more, contact between the aggregated inorganic filler particles becomes good, making it easier to form a thermal conduction path, and a cured resin product having high thermal conductivity can be obtained.
[0180] When the pressing step and the curing step are carried out simultaneously, the pressing time is not particularly limited. The pressurization time is preferably 1 hour or less, more preferably 30 minutes or less, still more preferably 1 minute or more, still more preferably 3 minutes or more, and particularly preferably 5 minutes or more. The pressurization time is preferably 1 hour or less, more preferably 30 minutes or less, and still more preferably 20 minutes or less. By setting the pressurizing time to the upper limit or less, the production time for the sheet-shaped cured resin material can be reduced, and the production cost tends to be reduced. By setting the pressurizing time to the lower limit or more, the gaps and voids in the sheet-shaped cured resin material can be sufficiently removed, and the heat transfer performance and the voltage resistance characteristics tend to be improved.
[0181] When the pressing step and the curing step are performed simultaneously, the heating temperature of the sheet-shaped resin composition on the substrate is not particularly limited. The heating temperature is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher. The heating temperature is preferably 300° C. or lower, more preferably 250° C. or lower, even more preferably 200° C. or lower, even more preferably 100° C. or lower, and particularly preferably 90° C. or lower. By setting the heating temperature to the lower limit or higher, the melt viscosity of the resin in the sheet-shaped resin composition can be reduced, and voids and gaps in the cured resin can be eliminated. By setting the heating temperature to the upper limit or lower, decomposition of organic components in the sheet-shaped resin composition and the cured resin sheet and voids caused by residual solvent tend to be suppressed.
[0182] When only the curing step is performed, the heating temperature of the sheet-shaped resin composition on the substrate is not particularly limited. The heating temperature is preferably 10°C or higher, more preferably 50°C or higher, and even more preferably 100°C or higher. The heating temperature is preferably 500°C or lower, more preferably 300°C or lower, even more preferably 200°C or lower, even more preferably 180°C or lower, and particularly preferably 175°C or lower. By setting the heating temperature within this temperature range, the curing reaction of the resin can be effectively promoted. By setting the heating temperature to the upper limit or lower, thermal deterioration of the resin can be prevented. By setting the heating temperature to the lower limit or higher, the curing reaction of the resin can be effectively promoted.
[0183] The thickness of the sheet-like cured resin thus formed is not particularly limited, but is preferably 50 μm or more, more preferably 80 μm or more, and even more preferably 100 μm or more, and is preferably 400 μm or less, and more preferably 300 μm or less. When the thickness of the cured resin is equal to or greater than the lower limit, the voltage resistance is improved and the breakdown voltage tends to be improved. When the thickness of the cured resin is equal to or less than the upper limit, the device can be made smaller and thinner, and the thermal resistance of the cured resin (heat dissipation sheet) obtained tends to be reduced.
[0184] [Composite molded body] The composite molded article of the present invention has a cured part made of the cured product of the resin composition of the present invention and a metal part, which are usually laminated together to form an integrated body.
[0185] The metal part may be provided on only one surface of the cured product part made of the resin cured product of the present invention, or on two or more surfaces. For example, the metal part may be provided on only one surface of the resin cured product, or on both surfaces. The metal part may be patterned.
[0186] The composite molded article of the present invention can be produced by using a metal part as the above-mentioned substrate and forming the cured resin product of the present invention on this substrate according to the above-mentioned method.
[0187] In addition, the composite molded product of the present invention can be produced by peeling a sheet-like resin composition or a cured resin product formed on a substrate separate from a metal portion from the substrate, and then heat-pressing the sheet-like resin composition or the cured resin product onto a metal member that will become the metal portion. It can also be manufactured.
[0188] In this case, a sheet-like resin composition or cured resin of the present invention is formed in the same manner as described above, except that a slurry of the resin composition of the present invention is applied to a substrate such as PET (polyethylene terephthalate) which may be treated with a release agent, and then the substrate is peeled off. The sheet-like resin composition or cured resin is placed on another metal plate or sandwiched between two metal plates and pressurized to be integrated.
[0189] The metal plate may be made of copper, aluminum, nickel-plated metal, or the like, and has a thickness of about 10 μm to 10 cm. The surface of the metal sheet may be physically roughened or chemically treated with a surface treatment agent, etc. From the viewpoint of adhesion between the resin composition and the metal sheet, it is more preferable that the metal sheet is subjected to such treatment.
[0190] [Semiconductor devices] The composite molded article of the present invention can be used as a semiconductor device, and is particularly suitable for use in a power semiconductor device that can achieve high output and high density by operating at high temperatures. EXAMPLES
[0191] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. Various conditions and evaluation result values in the following examples indicate preferred ranges of the present invention, similar to the preferred ranges in the embodiments of the present invention, and the preferred ranges of the present invention can be determined by taking into consideration the preferred ranges in the above-mentioned embodiments and the values in the following examples or the ranges indicated by a combination of values between the examples.
[0192] [raw materials] The raw materials used in the examples and comparative examples are as follows.
[0193] <Resin component> Resin component 1: A resin having the structure (2) (R 3 = Structure (4)) and Structure (3) (R 4 ,R 5 ,R 6 ,R 7 (=methyl group) Weight average molecular weight in polystyrene equivalent: 30,000 Epoxy equivalent: 9,000g / equivalent Resin component 2: A resin having the structure (1) (R 1 = methyl group, R 2 = phenyl group) and structure (3) (R 4 ,R 5 ,R 6 ,R 7 (=methyl group) Weight average molecular weight in polystyrene equivalent: 39,000 Epoxy equivalent: 13,000g / equivalent Resin component 3: Mitsubishi Chemical Corporation Bisphenol F type solid epoxy resin containing a structure with two epoxy groups per molecule Weight average molecular weight in polystyrene equivalent: 60,000 Resin component 4: Bisphenol A type liquid epoxy resin containing a structure with two epoxy groups per molecule (manufactured by Mitsubishi Chemical Corporation) Molecular weight: approx. 370 Resin component 5: Nagase ChemteX Corporation Multifunctional epoxy resin containing a structure having 4 or more glycidyl groups per molecule Molecular weight: approx. 400 Resin component 6: Mitsubishi Chemical Corporation Hydrogenated bisphenol A type liquid epoxy resin containing a structure with two epoxy groups per molecule Molecular weight approx. 410 Resin component 7: p-aminophenol type liquid multifunctional epoxy resin containing a structure having three or more epoxy groups per molecule (manufactured by Mitsubishi Chemical Corporation) Molecular weight: approx. 290
[0194] <Inorganic filler> Inorganic filler 1: Boron nitride agglomerated particles having a house-of-cards structure produced according to the method for producing boron nitride agglomerated particles disclosed in the examples of WO 2015 / 561028. New Mohs hardness: 2 Volume average particle size: 45μm Inorganic filler 2: Admatechs, spherical alumina particles New Mohs hardness: 9 Volume average particle size: 6.5 μm Thermal conductivity: 20~30W / m K
[0195] <Hardening agent> Hardener 1: Meiwa Chemical Industries, Ltd. "MEH-8000H" Phenol Resin Hardener
[0196] <Curing catalyst> Curing catalyst 1: Shikoku Kasei "2E4MZ-A" 2,4-Diamino-6-[2'-ethyl-4'-methylimidazolyl-(17')]-ethyl-s-triazine (Compounds Having a Triazine Ring as a Nitrogen-Containing Heterocyclic Structure) Molecular weight: 247 Curing catalyst 2: Shikoku Kasei "C11Z-CN" 1-Cyanoethyl-2-undecylimidazole Molecular weight: 275
[0197] [Sample preparation, measurement and evaluation] The methods for producing the molded bodies and the measurement conditions and evaluation methods in the examples and comparative examples are as follows.
[0198] <Example 1> A mixture was prepared using a planetary stirring device so that the solid content was 51% by weight of inorganic filler 1, 20% by weight of inorganic filler 2, and 29% by weight of components other than inorganic filler. At this time, the weight ratio of the components other than inorganic filler in the solid content was adjusted to the ratio shown in the column of Example 1 in Table 1. In addition, when preparing the above mixture, equal amounts of methyl ethyl ketone and cyclohexanone were used so that the above mixture was 63% by weight (solid content concentration) of the coating slurry.
[0199] The obtained slurry-like resin composition (slurry for sheet) was applied to a PET substrate by doctor blade method, and after heat drying at 60°C for 120 minutes, it was pressed at 42°C and 147 MPa for 10 minutes to obtain a sheet-like resin composition having a thickness of 150 μm. The total content of methyl ethyl ketone and cyclohexanone in the sheet-like resin composition was 1 wt% or less.
[0200] Next, we used a 500μm thick plate that had been roughened by filing with #120 sandpaper 100 times each. The above sheet-like resin composition was sandwiched between two 2,000 μm copper plates and pressed at 120° C. and 9.8 MPa for 30 minutes, then heated and pressed at 175° C. and 9.8 MPa for 30 minutes.
[0201] The composite molded body containing the copper plate and the cured resin obtained above was etched by a prescribed method to pattern the copper plate with a thickness of 500 μm, leaving two circular patterns with a diameter of 25 mm.
[0202] <Examples 2 to 3, Comparative Examples 1 to 4> A mixture was prepared in accordance with the method of Example 1 so that the solid content contained 51% by weight of inorganic filler 1, 20% by weight of inorganic filler 2, and 29% by weight of components other than the inorganic filler. Except for the weight ratio of the components other than the inorganic filler in the solid content shown in Table 1, a sheet-shaped resin composition and a composite molded product containing a copper plate and a cured resin were obtained in the same manner as in Example 1.
[0203] <Breakdown voltage (BDV) before and after moisture absorption reflow test> <BDV before moisture absorption reflow test> The composite molded bodies prepared in the examples and comparative examples were immersed in Fluorinert FC-40 (manufactured by 3M), and an electrode was placed on the patterned copper of φ25 mm using an ultra-high voltage withstand voltage tester 7470 (manufactured by Keisoku Gijutsu Kenkyusho), a voltage of 0.5 kV was applied, and the voltage was increased by 0.5 kV every 60 seconds until dielectric breakdown was reached. For those with a BDV of 5 kV or more, the BDV was measured after the moisture absorption reflow test, but for those with a BDV of less than 5 kV (ND), the BDV was not measured after the moisture absorption reflow test.
[0204] <BDV after moisture absorption reflow test> The composite molded bodies prepared in the examples and comparative examples were stored in an environment of 85°C and 85% RH for 3 days using a thermohygrostat SH-221 (manufactured by Espec Corp.), and then heated from room temperature to 290°C in 12 minutes in a nitrogen atmosphere within 30 minutes, held at 290°C for 10 minutes, and then cooled to room temperature (moisture absorption reflow test). Thereafter, the dielectric breakdown voltage was measured in the same manner as above, and a BDV of 5 kV or more was marked as "good", and a BDV of less than 5 kV was marked as "bad".
[0205] <Interface peeling after moisture absorption reflow test> The composite molded bodies produced in the examples and comparative examples were subjected to a moisture absorption reflow test in the same manner as above, and then the interface between the copper plate and the sheet-like resin cured product was observed using an ultrasonic imaging device FinSAT (FS300III) (manufactured by Hitachi Power Solutions). Measurements were performed using a probe with a frequency of 50 MHz, a gain of 30 dB, and a pitch of 0.2 mm, with the sample placed in water. Those in which no peeling was observed at the interface were marked with "○", and those in which interfacial peeling was observed were marked with "×".
[0206] <Weight increase rate of cured resin> The sheet-shaped resin cured products prepared in the Examples and Comparative Examples were cut into test pieces measuring 6 cm x 7 cm, dried at 150°C for 1 hour, and their weights a were measured. These sheet-shaped resin cured products were then stored for a certain period of time in an environment of 85°C and 85% RH using a thermohygrostat SH-221 (manufactured by Espec Corporation), and their weights were measured over time until they reached a certain weight (constant weight) b. The weight increase rate was calculated using the following formula. Weight increase rate (%) = (ba) / a × 100
[0207] <Storage modulus of resin composition excluding inorganic filler> In the same manner as in each of the Examples and Comparative Examples, except that no inorganic filler was added, a resin composition was prepared using a planetary stirring apparatus, and after heating and drying, the uncured resin composition was heated and cured using a rheometer "MCR302" manufactured by Anton Paar. The storage modulus at 100 ° C. was measured. For the measurements, aluminum parallel plates were used, and the measurement conditions were a strain of 0.3%, a frequency of 1 Hz, and a gap of 0.5 mm. The temperature profile during heat curing was as follows: starting from 25°C, the temperature was increased at 14°C per minute to 120°C, and after reaching 120°C, it was held for 30 minutes, then the temperature was increased at 7°C per minute to 175°C, and after reaching 175°C, it was held for 30 minutes, and then the temperature was increased at 7°C per minute to 200°C, and after reaching 200°C, it was held for 10 minutes. The storage modulus measured at this 10-minute hold at 200°C was used for evaluation.
[0208] The results of the above measurements and evaluations are shown in Table 1.
[0209] [Table 1]
[0210] It can be seen from Table 1 that the cured resin of the present invention has excellent voltage resistance under high temperature and high humidity conditions, and also does not suffer from the problem of interfacial peeling under high temperature and high humidity conditions when made into a composite molded product with a metal.
[0211] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese Patent Application No. 2018-192691 filed on October 11, 2018, the entirety of which is incorporated by reference.
Claims
1. A resin composition comprising a resin and an aggregated inorganic filler, the weight increase rate of the resin composition after curing at 85° C. and 85% RH is 0.80% or less; The storage modulus of the cured product of the resin composition excluding the inorganic filler at 200° C. is 1.0×10 7 Pa or more, The resin composition comprises an epoxy resin having three or more epoxy groups per molecule; The epoxy resin has a biphenyl structure and a weight average molecular weight of 10,000 or more, The composite molded body produced by the following method has a dielectric breakdown voltage (BDV) of 5 kV or more after a moisture absorption reflow test measured by the following method, The composite molded body is subjected to the following moisture absorption reflow test to check for interfacial peeling, and no interfacial peeling is observed in the resin composition. <Production of Composite Molded Body> The resin composition is applied to a PET substrate, dried by heating, and then pressed at 42° C. and 147 MPa for 10 minutes to obtain a sheet-like resin composition having a thickness of 150 μm. Next, the above sheet-like resin composition is sandwiched between each of the copper plates whose surfaces have been roughened in advance with a #120 file, and pressed at 175° C. and 9.8 MPa for 30 minutes. The resulting composite molded body containing the copper plate and the cured resin is subjected to an etching treatment to pattern the copper plate on one side. <BDV after moisture absorption reflow test> The composite molded body was stored in an environment of 85°C and 85% RH for 3 days, then heated from room temperature to 290°C in 12 minutes in a nitrogen atmosphere, held at 290°C for 10 minutes, and then cooled to room temperature (moisture absorption reflow test). The composite molded body after the moisture absorption reflow test is immersed in insulating oil, electrodes are placed on the patterned copper, and a voltage of 0.5 kV is applied in the thickness direction of the composite molded body. The voltage is increased by 0.5 kV every 60 seconds, and the voltage at which dielectric breakdown occurs (BDV) is measured. <Interface peeling after moisture absorption reflow test> The composite molding is subjected to a moisture absorption reflow test in the same manner as above, and then the presence or absence of interfacial peeling between the copper plate and the sheet-like resin cured product is observed by an ultrasonic imaging device.
2. The resin composition according to claim 1, wherein the epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more further has at least one structure selected from a structure represented by the following structural formula (1) and a structure represented by the following structural formula (2): [Formula 1] (In formula (1), R 1 and R 2 Each of R represents an organic group, and the organic group is an alkyl group, an alkenyl group, or an aryl group, which may be substituted with a halogen atom or a heteroatom. 3 represents a divalent cyclic organic group, and the cyclic organic group is an aromatic ring group or an aliphatic ring group, which may independently have a hydrocarbon group or a halogen atom as a substituent.
3. The resin composition according to claim 2, wherein the epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more further has a structure represented by the following structural formula (3): [Case 2] (In formula (3), R 4 , R 5 , R 6 , R 7 each independently represents an organic group having a molecular weight of 15 or more, and the organic group is an alkyl group, an alkenyl group, or an aryl group, which may be substituted with a halogen atom or a heteroatom.
4. The resin composition according to any one of claims 1 to 3, wherein the epoxy resin having a biphenyl structure and a weight average molecular weight of 10,000 or more has a weight average molecular weight of 80,000 or less.
5. The resin composition according to any one of claims 1 to 4, wherein the content of the epoxy resin having a biphenyl structure and having a weight average molecular weight of 10,000 or more is 1 wt % or more and 50 wt % or less based on 100 wt % of the solid content in the resin composition excluding the inorganic filler.
6. The resin composition according to any one of claims 1 to 5, wherein the content of the epoxy resin having four or more epoxy groups per molecule is 10% by weight or more and 50% by weight or less, based on 100% by weight of a solid content in the resin composition excluding an inorganic filler.
7. The resin composition according to any one of claims 1 to 6, further comprising a compound having a heterocyclic structure containing a nitrogen atom.
8. The resin composition according to any one of claims 1 to 7, wherein the agglomerated inorganic filler is agglomerated boron nitride particles.
9. 9. The resin composition according to claim 8, wherein the boron nitride agglomerated particles have a house of cards structure.
10. A composite molded article having a cured part made of the cured product of the resin composition according to any one of claims 1 to 9 and a metal part.
11. A semiconductor device comprising the composite compact of claim 10.
12. A resin cured product using a resin composition containing a resin and an aggregated inorganic filler, The weight increase rate at 85° C. and 85% RH is 0.80% or less, The storage modulus at 200° C. after curing of the resin composition excluding the inorganic filler is 1.0×10 7 Pa or more, The resin composition comprises an epoxy resin having three or more epoxy groups per molecule; The epoxy resin has a biphenyl structure and a weight average molecular weight of 10,000 or more, The composite molded body produced by the following method has a dielectric breakdown voltage (BDV) of 5 kV or more after a moisture absorption reflow test measured by the following method, The composite molded article is a cured resin, which shows no interfacial peeling when subjected to the following moisture absorption reflow test and then interfacial peeling. <Production of Composite Molded Body> The resin composition is applied to a PET substrate by a doctor blade method, and then heated and dried at 60° C. for 120 minutes. Thereafter, the resin composition is pressed at 42° C. and 147 MPa for 10 minutes to obtain a sheet-like resin composition having a thickness of 150 μm. Next, the above-mentioned sheet-like resin composition is sandwiched between one copper plate each of thickness 500 μm and 2,000 μm, the surfaces of which have been previously roughened 100 times with a #120 file, and pressed at 120° C. and 9.8 MPa for 30 minutes. The temperature is then increased and the plate is pressed at 175° C. and 9.8 MPa for 30 minutes. The resulting composite molded body containing the copper plate and the cured resin is etched to pattern the copper plate having a thickness of 500 μm, so that two circular patterns having a diameter of 25 mm remain. <Production of Composite Molded Body> The resin composition is applied to a PET substrate, dried by heating, and then pressed at 42° C. and 147 MPa for 10 minutes to obtain a sheet-like resin composition having a thickness of 150 μm. Next, the above sheet-like resin composition is sandwiched between each of the copper plates whose surfaces have been roughened in advance with a #120 file, and pressed at 175° C. and 9.8 MPa for 30 minutes. The resulting composite molded body containing the copper plate and the cured resin is subjected to an etching treatment to pattern the copper plate on one side. <BDV after moisture absorption reflow test> The composite molded body was stored in an environment of 85°C and 85% RH for 3 days, then heated from room temperature to 290°C in 12 minutes in a nitrogen atmosphere, held at 290°C for 10 minutes, and then cooled to room temperature (moisture absorption reflow test). The composite molded body after the moisture absorption reflow test is immersed in insulating oil, electrodes are placed on the patterned copper, and a voltage of 0.5 kV is applied in the thickness direction of the composite molded body. The voltage is increased by 0.5 kV every 60 seconds, and the voltage at which dielectric breakdown occurs (BDV) is measured. <Interface peeling after moisture absorption reflow test> The composite molding is subjected to a moisture absorption reflow test in the same manner as above, and then the presence or absence of interfacial delamination between the copper plate and the sheet-like resin cured product is observed by an ultrasonic imaging device.
Citation Information
Patent Citations
Multi-layer insulating sheet, and laminated structure
JP2011070930A
Epoxy resin composition and cured product
JP2011241245A
Boron nitride aggregated particle, composition containing boron nitride aggregated particle, and three-dimensional integrated circuit having layer comprising the composition
JP2015006985A
Adhesive sheet, dicing tape-integrated adhesive sheet, film, manufacturing method of semiconductor device, and semiconductor device
JP2016219619A
Filler composition for space between layers of three-dimensional integrated circuit, coating fluid, and process for producing three-dimensional integrated circuit
WO2012053524A1
Cited By
Resin composition and reactor
JP2026144284A