Laminated sheet for paper container, and paper container

The laminated sheet for paper containers addresses bubbling and pinhole issues by using a thermoplastic resin layer with a lower melting point to vent water vapor, enhancing sealing and reducing manufacturing complexity and costs.

JP2024149795AActive Publication Date: 2024-10-18TOPPAN HOLDINGS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024135609
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-18
Estimated Expiration
2039-11-18

AI Technical Summary

Technical Problem

Existing laminated sheets for paper containers face issues with bubbling and pinhole formation during heating due to water vapor expansion, leading to sealing defects and increased manufacturing complexity and costs.

Method used

A laminated sheet structure with a thermoplastic resin layer having a lower melting point than the adhesive resin layer, allowing water vapor to escape through the thermoplastic resin layer during heating, thereby reducing bubbling and pinhole formation.

Benefits of technology

The solution effectively suppresses bubbling and pinholes, maintains sealing performance, and simplifies the manufacturing process while reducing costs by using a single extrusion lamination method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149795000001_ABST
    Figure 2024149795000001_ABST
Patent Text Reader

Abstract

To suppress bubbling and pinholes caused by hot air upon container molding in a simple production process.SOLUTION: Disclosed is a laminated sheet 10 for a paper container in which one face side of a paper layer 2 is laminated with an adhesive resin layer 3, a barrier film layer 4 and a sealant layer 5 in this order, and the other face side of the paper layer 2 is laminated with a thermoplastic resin layer 1. A thermoplastic resin making up the thermoplastic resin layer 1 has a melting point lower than resin making up the adhesive resin layer 3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technology relating to a laminate sheet for paper containers and a paper container using the laminate sheet for paper containers. [Background technology]

[0002] Conventionally, containers such as glass bottles, cans, and plastic bottles have often been used to hold liquids such as beverages and alcohol, and powdery substances. However, in recent years, due to growing awareness of protecting the global environment, paper containers, which are highly recyclable and have a low environmental impact, have come to be widely used as containers for holding beverages, alcohol, and other contents.

[0003] Generally, paper containers for liquids use packaging materials made of laminated sheets of multiple materials in order to ensure the preservation of the contents, the strength of the container, gas barrier properties, etc. A known packaging material (laminate sheet) used for such paper containers for liquids has a layer structure in which a thermoplastic resin layer / paper layer / adhesive resin layer / barrier layer / sealant layer are laminated in this order from the outer surface side of the container. When such a laminated sheet is molded into the desired container shape, a heating step is performed in which hot air is applied to heat the sealant layer to melt it. When hot air is applied to the sealant layer in this heating step, the moisture contained in the paper layer is rapidly heated by the heat and turns into water vapor. The expansion pressure of this water vapor may cause a foaming phenomenon (bubbling) that causes separation between the paper layer and the adhesive resin layer.

[0004] When bubbling occurs, there is a possibility that poor sealing and poor appearance may occur. Furthermore, if heating is continued or if heating is performed at a higher temperature, there is a risk of pinholes (holes) appearing in the adhesive resin layer / barrier layer / sealant layer that have been peeled off by bubbling. The occurrence of pinholes can cause leakage of the contents and a decrease in the barrier function. Since pinholes in particular are defects that can lead to complaints, the sealant heating conditions during the manufacture of paper containers must be carefully adjusted. In light of the above, laminated sheets for paper containers are required to be less susceptible to bubbling and pinholes.

[0005] As techniques for suppressing bubbling and pinholes, methods such as those described in Patent Documents 1 and 2 have been proposed. Patent Document 1 describes a paper container formed by molding a laminated material mainly composed of a paper base material in which at least a paper layer and a barrier film layer are laminated via a melt-extruded resin layer, and the adhesive-coated surface of the paper layer and paper base material has a sizing degree of 400 seconds or more according to the measurement method of JIS P8122, and an adhesive layer made of a two-component curing adhesive having a urethane bond is applied to the adhesive-coated surface at a rate of 0.5 g / m 2 More than 4g / m 2 A paper container is proposed, which is characterized by being formed by coating with the following coating amount, and forming a laminate material in which a paper layer and a barrier film layer are laminated so that the adhesive layer is interposed between the paper layer and the melt-extruded resin layer. In the case of the method described in Patent Document 1, it is disclosed that the provision of the adhesive layer improves heat resistance and provides strength sufficient to withstand the pressure of water vapor expansion. As a result, the method in Patent Document 1 makes it possible to suppress bubbling, which ultimately leads to suppression of pinholes.

[0006] In Patent Document 2, at least an outer resin layer is laminated on one side of a main thick paper layer, and an inner sealant resin layer is laminated on the other side of the thick paper layer via an adhesive layer such as a plastic resin layer or a barrier layer, and the outer resin layer is laminated on the thick paper layer. A paper container sheet material for packaging liquids has been proposed, which is characterized by having perforations consisting of minute pores that are permeable to water vapor reaching the surface of the container. According to the method described in Patent Document 2, the perforations in the outer resin layer serve as escape routes for water vapor evaporated by heating with hot air (heating step), and the expansion pressure caused by water vapor can be reduced, making it possible to suppress bubbling, which ultimately leads to the suppression of pinholes. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 4577001 [Patent Document 2] JP 2000-203565 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the method described in Patent Document 1 requires the provision of an adhesive layer between the paper layer and the melt-extruded resin layer, which increases the material cost and the number of steps, thereby increasing the manufacturing cost. In addition, the method described in Patent Document 2 requires a step of providing holes, which increases the number of steps, and therefore there is a need to further simplify the steps. In addition, in the method described in Patent Document 2, there is a risk that surrounding moisture and odors may enter the paper layer through the pores when the paper container is in use.

[0009] The present invention has been made with attention to the above-mentioned points, and aims to provide a laminated sheet for paper containers that can suppress bubbling and pinholes caused by hot air (heating) during container molding while minimizing an increase in the number of manufacturing steps. [Means for solving the problem]

[0010] In order to solve the problems, one aspect of the present invention is a laminate sheet for paper containers, in which an adhesive resin layer, a barrier film layer and a sealant layer are laminated in that order on one side of a paper layer, and a thermoplastic resin layer is laminated on the other side of the paper layer, and the thermoplastic resin constituting the thermoplastic resin layer has a melting point lower than that of the resin constituting the adhesive resin layer. Another aspect of the present invention is a paper container obtained by forming the laminate sheet for paper containers, which is one aspect of the present invention, into a container shape. Another aspect of the present invention is a method for manufacturing a paper container, which includes a heating step of applying heat to the sealant layer of the laminate sheet for paper containers when forming a paper container from the laminate sheet for paper containers, in which an adhesive resin layer, a barrier film layer, and a sealant layer are laminated in this order on one side of a paper layer and a thermoplastic resin layer is laminated on the other side of the paper layer, wherein in the heating step, at least a portion of the thermoplastic resin layer is melted by heating the sealant layer, and at least a portion of the water vapor generated from the paper layer by the heating is discharged through the molten thermoplastic resin layer. Effect of the Invention

[0011] According to an aspect of the present invention, it is possible to suppress bubbling and pinholes caused by hot air during container molding. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an example of the configuration of a laminate sheet for paper containers according to an embodiment based on the present invention. [Diagram 2] 1A to 1C are diagrams illustrating an example of a manufacturing process according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a conceptual diagram illustrating a production example of a laminate sheet for paper containers according to an embodiment based on the present invention. [Figure 4] 1A to 1C are diagrams illustrating an example of a manufacturing process for a paper container according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a diagram illustrating heating for evaluation in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In addition, each figure is a schematic diagram, and the size and shape of each part are appropriately exaggerated for easy understanding. In addition, the following description is an example of the present invention, and the present invention is not limited thereto.

[0014] (Laminated sheet for paper containers) As shown in FIG. 1, the laminate sheet for paper containers of this embodiment is a laminate sheet in which an adhesive resin layer, a barrier film layer and a sealant layer are laminated in that order on one side of a paper layer, and a thermoplastic resin layer is laminated on the other side of the paper layer.

[0015] Next, each layer constituting the laminated sheet for paper containers will be described individually. (paper layer) The paper layer 2 is a layer that mainly provides formability and rigidity to the container. The paper layer 2 may be, for example, a surface-treated coated paper or an untreated uncoated paper. The paper layer 2 may be made of a known paper material used for paper containers. The paper basis weight of the paper layer 2 is, for example, 200 g / m 2 More than 500g / m 2 The following are preferred, but may be selected appropriately according to the container size. Here, in order to improve adhesion between the surface of the paper layer 2 and the thermoplastic resin layer 1 and the adhesive resin layer 3, it is preferable that a surface treatment such as a corona treatment is appropriately performed.

[0016] (adhesive resin layer) The adhesive resin layer 3 is provided to adhere the barrier film layer 4 to one surface of the paper layer 2. The adhesive resin layer 3 is laminated to adhere the paper layer 2 and the barrier film layer 4 by, for example, extrusion lamination. There are no particular limitations on the adhesive resin layer 3, so long as it has the adhesiveness to bond the paper layer 2 and the barrier film layer 4. The adhesive resin layer 3 may be a single-layer structure made of a single resin, or may be a multi-layer structure formed by co-extrusion molding or the like.

[0017] Examples of resins constituting the adhesive resin layer 3 include low-density polyethylene, medium-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-α-olefin copolymer resins, copolymers of ethylene with unsaturated carboxylic acids or their ester compounds such as ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl acrylate copolymers, and ethylene-methacrylic acid copolymers, ionomer resins, and the like.

[0018] The thickness of the adhesive resin layer 3 is preferably 20 μm or more and 50 μm or less. If the thickness of the adhesive resin layer 3 is thinner than 20 μm, there is a high possibility of delamination occurring due to a decrease in adhesion between the paper layer 2 and the barrier film layer 4. Also, if the thickness of the adhesive resin layer 3 is thicker than 50 μm, problems are likely to occur in the molding process, such as the inability to properly draw creases when molding into the shape of a container. A known method such as a dry lamination method or an extrusion lamination method can be used to laminate the adhesive resin layer 3. Since the dry lamination method requires time for drying steps and aging after lamination, the extrusion lamination method, which does not require these steps, is preferred for laminating the adhesive resin layer 3 because it allows the most efficient production.

[0019] (Barrier film layer) The barrier film layer 4 is provided to impart gas barrier properties to the container. For the barrier film layer 4, for example, a film obtained by depositing an inorganic material such as silica, alumina, or aluminum on a substrate film such as a biaxially oriented polyester film, a nylon film, a polycarbonate film, a polyvinyl alcohol film, or an ethylene-vinyl alcohol copolymer resin can be used. The thickness of this substrate film is suitably about 5 to 30 μm. The thickness of the deposited film itself may be sufficient to achieve the required gas barrier properties, and for example, when silica is deposited, the thickness is preferably about 30 to 200 nm. The barrier film layer 4 may also be prepared by bonding an aluminum foil and the above-mentioned base film by a dry lamination method.

[0020] The barrier film layer 4 is preferably any film selected from the following (1) to (3). (1) PET film with a metal vapor deposition layer (2) PET film with a vapor-deposited layer of inorganic oxide (3) Aluminum foil and PET film laminate Here, the above-mentioned "provided" includes not only the case where the film is provided on one side of the PET film, but also the case where the film is provided on both sides.

[0021] (Sealant layer) Resins generally used as sealant layers can be used for the sealant layer 5. Examples of resins constituting the sealant layer 5 include polyethylene-based resins such as low-density polyethylene, medium-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymer resins, and ethylene-vinyl acetate copolymers, and polypropylene. The sealant layer 5 can be used as a single layer of these resins, or as a multilayer in which a plurality of resins are combined. The thickness of the sealant layer 5 is not particularly limited as long as it has sufficient sealing properties when the container is molded. The thickness of the sealant layer 5 is, for example, 30 μm or more and 100 μm or less. The method for laminating the sealant layer 5 and the barrier film layer 4 is not particularly limited, but is generally a dry lamination method using a two-component curing adhesive having a urethane bond after film formation, or an extrusion lamination method.

[0022] (thermoplastic resin layer) The thermoplastic resin layer 1 is required to have heat sealability since the thermoplastic resin layers are heat-sealed together when the laminated sheet is molded into various container shapes such as rectangular or round shapes. In this embodiment, a resin material having a lower melting point than the resin constituting the adhesive resin layer 3 is used as the thermoplastic resin constituting the thermoplastic resin layer 1. When the adhesive resin layer 3 is composed of two or more layers, the melting point of the thermoplastic resin constituting the thermoplastic resin layer 1 is set to be lower than the melting point of the layer in contact with the paper layer 2 among the multiple layers constituting the adhesive resin layer 3.

[0023] The thermoplastic resin constituting the thermoplastic resin layer is preferably a low-melting thermoplastic resin having a melting point of 107° C. or less, and more preferably has a melting point of 84° C. or more and 100° C. or less. Examples of thermoplastic resins that can be set to such a melting point and have heat sealability include low-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymer resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl acrylate copolymers, ethylene-methyl methacrylate copolymers, ionomer resins, and other ethylene-unsaturated carboxylic acids or esters thereof. and copolymers with tert-butyl compounds.

[0024] The thickness of the thermoplastic resin layer 1 can be a known thickness used for the thermoplastic resin layer of a paper container. The thickness of the thermoplastic resin layer 1 may be the minimum thickness required for heat-sealing the thermoplastic resin layers together during container molding and for enduring impact such as dropping after the container is molded. The thickness of the thermoplastic resin layer 1 is, for example, 10 μm or more and 30 μm or less. The extrusion coating method, in which the thermoplastic resin layer 1 is laminated on the paper layer in a molten state, can be used for laminating the thermoplastic resin layer 1. If the dry lamination method is used, the adhesive layer blocks the escape route of the water vapor generated in the paper layer 2 during hot air heating, increasing the internal pressure in the paper layer 2 and making it more likely to cause bubbling. The surface of the thermoplastic resin layer 1 may be subjected to a surface treatment such as a corona treatment, if necessary, and then printing may be carried out.

[0025] (Paper container) The paper container is formed using the laminate sheet for paper containers described in the above embodiment. The manufacturing process 20 for manufacturing a paper container having a desired container shape from the laminated sheet for paper containers includes a forming process 20A and a heating process 20B, as shown in FIG. In the forming step 20A, the laminated sheet for paper containers is three-dimensionally formed into a container shape. The shape at the time of forming includes an intermediate shape before becoming a final paper container.

[0026] The heating step 20B is a step of applying heat to the sealant layer 5 side of the laminate sheet for paper containers, which will be the inside of the container, to temporarily melt the sealant layer 5. In this heating step 20B, for example, hot air is applied from the sealant layer 5 side to heat it, melt the sealant layer 5, and seal it. Here, as described later, the heating step 20B is performed while forming the paper container. The heating process in the heating step 20B is carried out, for example, by blowing hot air at a temperature of 340° C. for one second. The paper container is then formed into a final intended container shape, which may be, for example, a Gagel-top type container, a brick type container, a cylindrical container, or the like, but is not limited thereto.

[0027] (Example of manufacturing process) An example of a method for manufacturing a laminate sheet for paper containers and a paper container of this embodiment will be described. <Manufacturing example of laminated sheet for paper containers> First, as shown in FIG. 3(a), a laminate sheet (4, 5) is produced by laminating a resin constituting the barrier film layer 4 and a resin constituting the sealant layer 5 by extrusion molding. Next, as shown in FIG. 3(b), the laminated sheets (4, 5) produced above and the paper layer 2 are extrusion molded via the adhesive resin layer 3 to produce laminated sheets (2-5). Next, as shown in FIG. 3(c), the laminate sheets (2 to 5) produced above and a thermoplastic resin layer 1 are laminated by extrusion molding to sequentially form a laminate sheet for paper containers, and the laminate sheet for paper containers is rolled.

[0028] <Example of paper container manufacturing> As shown in FIG. 4(a), the manufactured laminated sheet for paper containers is cut into sheets to obtain blanks as shown in FIG. 4(b) (punching process). Next, as shown in FIG. 4(c), a scoring process is carried out to add creases to the blank material to make it easier to assemble. Next, as shown in FIG. 4(d), it is molded into a cylindrical shape (molding step 20A). Next, as shown in FIG. 4(e), the surface (inner surface) of the bottom sealant layer side of the cylindrical molded product is heated with hot air to seal and close the bottom of the container.

[0029] (Heating process 20B). Next, as shown in FIG. 4(f), the contents are filled from the top side (filling process). Next, as shown in FIG. 4(g), the surface (inner surface) of the top sealant layer is heated with hot air to seal and close the bottom of the container (heating step 20B).

[0030] (Actions and others) When the sealant layer 5 is heated to a temperature high enough to melt it in the heating step 20B, the paper layer 2 above the heating position also reaches 100°C or higher, and the moisture contained in the paper layer 2 turns into steam. When the moisture turns into steam, the pressure increases. In this embodiment, a thermoplastic resin having a lower melting point than the resin provided in the adhesive resin layer 3 is used for the thermoplastic resin layer. Therefore, when the sealant layer 5 is heated in the heating step 20B, at least a part of the thermoplastic resin layer 1 is temporarily put into a molten state by the heating, and at least a part of the water vapor with a relatively high pressure passes through the thermoplastic resin layer 1 and is released to the outside, thereby suppressing the expansion pressure due to the water vapor. This has the effect of suppressing bubbling between the paper layer and the adhesive resin layer 3 caused by evaporation of moisture in the paper, and also suppressing pinholes.

[0031] The above heating causes the thermoplastic resin layer 1 to enter a molten state, temporarily forming fine passages through which water vapor passes in the thermoplastic resin layer 1, but most of the fine passages become blocked when the layer is cooled after heating is completed. This prevents moisture, odors, and other fumes from penetrating into the paper layer when the paper container is in use. During heating, the thermoplastic resin layer 1 reaches a temperature higher than 107° C., although this depends on the heating conditions in the heating step 20B.

[0032] As described above, in the laminate sheet 10 for paper containers of this embodiment, the thermoplastic resin layer 1 and the adhesive resin layer 3 can be laminated directly onto the paper layer 2 by extrusion coating or extrusion lamination without the use of an adhesive. Furthermore, if a tandem extruder is used, the thermoplastic resin layer 1 and the adhesive resin layer 3 can be laminated on the same line, thereby improving manufacturing efficiency. This method can carry out the conventional manufacturing process for laminate sheets for paper containers, and therefore does not require any special process for suppressing bubbling and pinholes, and can provide effects at low cost. Furthermore, by using the laminated sheet 10 for paper containers of this embodiment, it is possible to easily and reliably ensure the sealing performance of the paper container. EXAMPLES

[0033] [Example 1] An LDPE film (thickness: 55 μm) with one side subjected to a corona treatment was prepared as the sealant layer 5. In addition, a PET film (thickness: 12 μm) with one side subjected to silica deposition and the other side subjected to a corona treatment was prepared as the barrier film layer 4. The silica-deposited surface of the barrier film layer 4 and the corona-treated surface of the LDPE film were laminated by dry lamination using a urethane adhesive to prepare a laminate sheet of a barrier film layer / sealant layer. The PET surface exposed on the barrier film layer side of the laminate sheet of the barrier film layer / sealant layer was also subjected to corona treatment.

[0034] Paper layer 2: basis weight 380g / m 2 An uncoated paper was prepared and subjected to corona treatment on both sides of the paper. Then, EVA (Evaflex EV450, manufactured by Mitsui DuPont Polychemicals, melting point 84°C) was extrusion coated on one side of the paper layer 2 to a thickness of 18 μm from the first T-die of the tandem extruder to form a thermoplastic resin layer 1. Next, sandwich lamination was performed between the side of the paper layer 2 opposite to the side on which the thermoplastic resin layer was formed and the PET film side of the above-mentioned barrier film layer / sealant layer laminate film using EMAA (AN4228C, melting point 104°C, manufactured by DuPont-Mitsui Polychemicals Co., Ltd.) from a second T-die to form an adhesive resin layer 3 with a thickness of 30 μm.

[0035] The laminated sheet for paper containers obtained as described above had a composition of EVA (EV450, melting point 84°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / EMAA (AN4228C, melting point 104°C, thickness 30 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm) (see Figure 1).

[0036] [Example 2] The procedure was the same as in Example 1, except that the resin of the adhesive resin layer 3 in Example 1 was changed to a two-layer structure of LDPE (L6810 manufactured by Asahi Kasei Corporation, melting point 107°C) and EMAA (AN4228C manufactured by Mitsui DuPont Polychemicals Co., Ltd., melting point 104°C). The resulting laminated sheet had a composition of EVA (EV450, melting point 84°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L6810, melting point 107°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0037] [Example 3] The procedure was the same as in Example 1, except that the resin of the thermoplastic resin layer 1 in Example 1 was changed to EMAA (AN4228C, melting point 104°C, manufactured by DuPont-Mitsui Polychemicals Co., Ltd.) and the resin of the adhesive resin layer 3 was changed to a two-layer structure of LDPE (L6810, manufactured by Asahi Kasei Corporation, melting point 107°C) and EMAA (AN4228C, melting point 104°C, manufactured by DuPont-Mitsui Polychemicals Co., Ltd.). The resulting laminated sheet had a composition of EMAA (AN4228C, melting point 104°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L6810, melting point 107°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0038] [Example 4] The procedure was the same as in Example 1, except that the resin of the adhesive resin layer 3 in Example 1 was changed to a two-layer structure of LDPE (LW18A manufactured by Tosoh Corporation, melting point 130°C) and EMAA (AN4228C manufactured by Mitsui DuPont Polychemicals, melting point 104°C). The resulting laminated sheet had a composition of EVA (EV450, melting point 84°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LW18A, melting point 130°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0039] [Example 5] The procedure was the same as in Example 1, except that the resin of the thermoplastic resin layer 1 in Example 1 was changed to EMAA (AN4228C, melting point 104°C, manufactured by DuPont-Mitsui Polychemicals Co., Ltd.) and the resin of the adhesive resin layer 3 was changed to a two-layer structure of LDPE (LW18A, manufactured by Tosoh Corporation, melting point 130°C) and EMAA (AN4228C, melting point 104°C, manufactured by DuPont-Mitsui Polychemicals Co., Ltd.). The resulting laminated sheet had a composition of EMAA (AN4228C, melting point 104°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LW18A, melting point 130°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0040] [Comparative Example 1] The resin of the thermoplastic resin layer 1 in Example 1 was LDPE (L6810, manufactured by Asahi Kasei Corporation, melting point 1 The procedure was the same as in Example 1, except that the temperature was changed to 0.07°C. The resulting laminated sheet had a composition of LDPE (L6810, melting point 107°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / EMAA (AN4228C, melting point 104°C, thickness 30 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0041] [Comparative Example 2] The procedure was the same as in Example 1, except that the resin of the thermoplastic resin layer 1 in Example 1 was changed to LDPE (L2340 manufactured by Asahi Kasei Corporation, melting point 112° C.). The resulting laminated sheet had a composition of LDPE (L2340, melting point 112°C, 18 μm) / paper (basis weight 380 g / m 2 ) / EMAA (AN4228C, melting point 104°C, thickness 30 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0042] [Comparative Example 3] The procedure was the same as in Example 1, except that the resin of the thermoplastic resin layer 1 in Example 1 was changed to PP (FL02T manufactured by Japan Polypropylene Corporation, melting point 160° C.). The resulting laminated sheet had a composition of PP (FL02T, melting point 160°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / EMAA (AN4228C, melting point 104°C, thickness 30 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0043] [Comparative Example 4] The procedure was the same as in Example 2, except that the resin of the thermoplastic resin layer 1 in Example 2 was changed to LDPE (L6810 manufactured by Asahi Kasei Corporation, melting point 107° C.). The resulting laminated sheet had a composition of LDPE (L6810, melting point 107°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L6810, melting point 107°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0044] [Comparative Example 5] The procedure was the same as in Example 2, except that the resin of the thermoplastic resin layer 1 in Example 2 was changed to LDPE (L2340 manufactured by Asahi Kasei Corporation, melting point 112° C.). The resulting laminated sheet had a composition of LDPE (L2340, melting point 112°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L6810, melting point 107°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0045] [Comparative Example 6] The procedure was the same as in Example 2, except that the resin of the thermoplastic resin layer 1 in Example 2 was changed to PP (FL02T manufactured by Japan Polypropylene Corporation, melting point 160° C.). The resulting laminated sheet had a composition of PP (FL02T, melting point 160°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L6810, melting point 107°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0046] [Comparative Example 7] The procedure was the same as in Example 4, except that the resin of the thermoplastic resin layer 1 in Example 4 was changed to LDPE (L6810 manufactured by Asahi Kasei Corporation, melting point 107° C.). The resulting laminated sheet had a composition of LDPE (L6810, melting point 107°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LW18A, melting point 130°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0047] [Comparative Example 8] The procedure was the same as in Example 4, except that the resin of the thermoplastic resin layer 1 in Example 4 was changed to LDPE (L2340 manufactured by Asahi Kasei Corporation, melting point 112° C.). The resulting laminated sheet had a composition of LDPE (L2340, melting point 112°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LW18A, melting point 130°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0048] [Comparative Example 9] The procedure was the same as in Example 4, except that the resin of the thermoplastic resin layer 1 in Example 4 was changed to PP (FL02T manufactured by Japan Polypropylene Corporation, melting point 160° C.). The resulting laminated sheet had a composition of PP (FL02T, melting point 160°C, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LW18A, melting point 130°C, thickness 20 μm) / EMAA (AN4228C, melting point 104°C, thickness 10 μm) / silica-deposited PET film (thickness 12 μm) / LDPE (thickness 55 μm).

[0049] (evaluation) The pinhole resistance of the prepared Examples 1 to 5 and Comparative Examples 1 to 9 was evaluated, and the results are shown in Table 1. [Evaluation method] As shown in Figure 5(a), hot air at 340°C was sprayed from a heat gun 40 (Earthman HG-1450B, manufactured by Takagi Corporation) onto the sealant layer 5 side of the laminated sheet 10 at a distance of 2 cm from the sealant layer 5. The time it took for pinholes to appear under these conditions (Figure 5(c)) was then measured. Figure 5(b) shows the state in which bubbling occurred. If the time until pinholes appeared was 4 seconds or longer, it was judged as "○", and if it was shorter than 4 seconds, it was judged as "×".

[0050] [Table 1]

[0051] As shown in Table 1, it was confirmed that by using a resin having a lower melting point than the adhesive resin layer 3 for the thermoplastic resin layer 1, the time it takes for pinholes to appear was delayed, making it clear that pinhole resistance was improved. [Explanation of symbols]

[0052] 1 Thermoplastic resin layer 2 paper layers 3 Adhesive resin layer 4 Barrier film layer 5 Sealant Layer 10. Laminated sheet for paper containers

Claims

1. A laminated sheet for paper containers, comprising an adhesive resin layer, a barrier film layer and a sealant layer laminated in this order on one surface side of a paper layer, and a thermoplastic resin layer laminated on the other surface side of the paper layer, All of the thermoplastic resins constituting the thermoplastic resin layer have a melting point lower than that of the resin in the adhesive resin layer that is in contact with the paper layer, the adhesive resin layer is formed only from an ethylene-methacrylic acid copolymer and / or a low-density polyethylene; The adhesive resin constituting the adhesive resin layer has a melting point of 104° C. or higher and 130° C. or lower, A laminate sheet for paper containers, characterized in that the barrier film layer is any film selected from the following (1) to (3). (1) PET film with a metal deposition layer (2) PET film with a vapor-deposited layer of inorganic oxide (3) Aluminum foil and PET film laminate

2. A paper container obtained by forming the laminated sheet for paper containers according to claim 1 into a container shape.

3. 3. The paper container according to claim 2, wherein the shape of the paper container is any one of a Gagel-top shape, a cup shape, and a cylindrical shape.

Citation Information

Patent Citations

  • Laminate material for cup-formed container

    JP2003221024A

  • Method for manufacturing paper container for liquid and paper container for liquid

    WO2018034350A1

  • Paper-made container sheet material for packaging liquid

    JP2000203565A

  • Method for manufacturing paper containers and the laminated materials constituting those containers.