Electrochemical reaction cell stack and flow path forming member for electrochemical reaction cell stack

The angled layered structure in the flow path forming member of electrochemical reaction cell stacks addresses gas leakage issues, improving power generation efficiency and reliability by ensuring stress relaxation and minimizing gas escape.

JP2024150025AActive Publication Date: 2024-10-23MORIMURA SOFC TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023063231
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Conventional flow path forming members in electrochemical reaction cell stacks, such as those used in solid oxide fuel cells (SOFCs) and solid oxide electrolytic cells (SOECs), suffer from gas leakage through gaps between layered particles, leading to decreased power generation efficiency.

Method used

The electrochemical reaction cell stack incorporates a flow path forming member with a layered structure composed of particles angled differently at the ends and center, ensuring stress relaxation properties while minimizing gas leakage by aligning some particles at an angle difference of at least 1.4 degrees and a width ratio of three times the height, preventing gas from escaping into external spaces.

Benefits of technology

This configuration effectively suppresses gas leakage while maintaining stress relaxation properties, enhancing power generation efficiency and reliability by reducing voltage drops due to thermal cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150025000001_ABST
    Figure 2024150025000001_ABST
Patent Text Reader

Abstract

To ensure the stress relaxation properties of a flow passage forming member, and suppress gas leakage from the flow passage forming member compared to a configuration in which the layered particles are uniformly oriented along the second direction.SOLUTION: An electrochemical reaction cell stack includes a plurality of single cells, and a communication passage is formed that communicates with a gas chamber that faces one of an air electrode and a fuel electrode. The electrochemical reaction cell stack includes a first member, a second member arranged to face the first member, a gas flow passage arranged between the first member and the second member, and including the gas chamber and the communication passage, and a flow passage forming member separating the gas passage from a space other than the gas passage. The flow passage forming member has a layered structure made of a plurality of layered particles. There is a first layered particle located at an end of the flow passage forming member, the first angle of the first layered particle is different from a second angle of a centrally located second layered particle.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in this specification relates to a flow path forming member for an electrochemical reaction cell stack. [Background technology]

[0002] As one type of fuel cell that generates electricity by utilizing an electrochemical reaction between hydrogen and oxygen, a solid oxide fuel cell (hereinafter referred to as "SOFC") having an electrolyte layer containing a solid oxide is known. SOFCs are generally used in the form of a fuel cell stack in which a plurality of structural units (electrochemical reaction units) are arranged in a predetermined direction. Each electrochemical reaction unit includes a single cell having an electrolyte layer containing a solid oxide, an air electrode and an anode facing each other with the electrolyte layer therebetween, and an air electrode frame and an anode frame that respectively surround the periphery of an air flow path facing the air electrode and the periphery of a fuel flow path facing the anode. The air electrode frame is formed of, for example, mica (see Patent Document 1). Mica has a layered structure consisting of a plurality of layered particles stacked in the above-mentioned predetermined direction. For this reason, the air electrode frame can relieve stress generated in the fuel cell stack. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-170630 A Summary of the Invention [Problem to be solved by the invention]

[0004] The air electrode frame is preferably arranged to separate the air electrode from a space other than the air electrode (e.g., an external space) to suppress gas leakage from the air flow path facing the air electrode. However, mica conventionally used in the air electrode frame has a layered structure in which a plurality of layered particles are arranged parallel to each other along a surface direction perpendicular to the above-mentioned predetermined direction. For this reason, there is a risk that gas in the air flow path will leak into the external space through the gaps between the layered particles. If gas leaks from the air flow path, problems such as a decrease in the power generation efficiency of the fuel cell will occur.

[0005] Such an issue is also common to electrolysis cell stacks having multiple electrolysis cell units, which are constituent units of solid oxide electrolysis cells (hereinafter referred to as "SOEC") that generate hydrogen using the electrolysis reaction of water. Moreover, such an issue is not limited to SOFCs and SOECs, but is also common to other types of electrochemical reaction cell stacks. Moreover, such an issue is not limited to air electrode frames, but is also common to other flow path forming members. The flow path forming member is a member that is disposed between two members that constitute the electrochemical reaction cell stack, separates a predetermined gas flow path formed in the electrochemical reaction cell stack from the other space, and has a layered structure made of multiple layered particles. [Means for solving the problem]

[0006] (1) The electrochemical reaction cell stack disclosed in this specification includes a plurality of unit cells each including an electrolyte layer and an air electrode and an anode facing each other with the electrolyte layer sandwiched therebetween. The electrochemical reaction cell stack has a communication passage formed therein that communicates with a gas chamber facing one of the air electrode and the anode. The electrochemical reaction cell stack includes a first member, a second member disposed to face the first member, and a flow passage forming member disposed between the first member and the second member, and separating a gas flow passage including the gas chamber and the communication passage from a space other than the gas flow passage. The flow passage forming member has a layered structure made of a plurality of layered particles stacked in a first direction in which the first member and the second member face each other. In at least one specific cross section of the flow path forming member along the first direction, there is a first layered particle located at an end of the flow path forming member in a second direction perpendicular to the first direction, the first layered particle having a first angle with respect to the second direction that is different from a second angle made with respect to the second direction by a second layered particle located at the center of the flow path forming member in the second direction.

[0007] In this electrochemical reaction cell stack, the presence of the second layered particles ensures the stress relaxation of the flow path forming member. In addition, the presence of the first layered particles prevents the gas in the gas chamber from passing between the granular elements constituting the flow path forming member and leaking into the external space. Therefore, according to this electrochemical reaction cell stack, while ensuring the stress relaxation of the flow path forming member, gas leakage from the flow path forming member can be suppressed compared to a configuration in which the layered particles are uniformly aligned along the second direction.

[0008] (2) In the electrochemical reaction cell stack, the absolute value of the difference between the first angle and the second angle may be 1.4 degrees or more. According to this electrochemical reaction cell stack, gas leakage from the flow path forming member can be effectively suppressed compared to, for example, a configuration in which the absolute value of the difference between the first angle and the second angle is less than 1.4 degrees.

[0009] (3) In the electrochemical reaction cell stack, the absolute value of the first angle may be less than 90 degrees. According to this electrochemical reaction cell stack, it is possible to suppress a decrease in the stress relaxation property of the flow path forming member caused by the presence of the first layered particles, compared to a configuration in which the absolute value of the first angle is 90 degrees, for example.

[0010] (4) In the electrochemical reaction cell stack, the width of the flow path forming member in the second direction may be three times or more the width in the first direction in the specific cross section. According to this electrochemical reaction cell stack, compared to a configuration in which the width of the flow path forming member in the second direction is less than three times the width in the first direction, for example, the path in the flow path forming member between the gas chamber and the external space is longer, and therefore it is possible to effectively suppress gas leakage from the flow path forming member while ensuring the stress relaxation property of the flow path forming member.

[0011] (5) A flow path forming member disclosed in the present specification is a flow path forming member for an electrochemical reaction cell stack, and has a layered structure consisting of a plurality of layered particles stacked in a first direction, and in at least one specific cross section along the first direction, there is a first layered particle located at an end of the flow path forming member in a second direction perpendicular to the first direction, and the first layered particle has a first angle with respect to the second direction that is different from a second angle with respect to the second direction made by a second layered particle located at the center of the flow path forming member in the second direction. This flow path forming member can ensure the stress relaxation property of the flow path forming member, while suppressing gas leakage from the flow path forming member compared to a configuration in which the layered particles are uniformly aligned along the second direction. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a perspective view showing an external configuration of a fuel cell stack according to an embodiment; [Diagram 2] FIG. 2 is a cross-sectional view of the fuel cell stack according to the embodiment taken along line II-II in FIG. [Diagram 3] FIG. 3 is a cross-sectional view of the fuel cell stack according to the embodiment taken along line III-III in FIG. [Figure 4] FIG. 4 is a cross-sectional view of the fuel cell stack according to the embodiment taken along line IV-IV in FIG. [Diagram 5] FIG. 2 is a cross-sectional view showing two adjacent electrochemical reaction units in the fuel cell stack according to the embodiment, taken along the same line as in FIG. 1 . [Figure 6] FIG. 3 is a cross-sectional view showing two adjacent electrochemical reaction units in the fuel cell stack according to the embodiment, taken along the same line as in FIG. 1 . [Figure 7] FIG. 6 is an enlarged schematic diagram showing a first portion X1 of the cathode frame 130 in FIG. 5. [Figure 8] FIG. 8 is a schematic diagram showing a layered structure in a divided region E1 of the cathode frame 130 in FIG. [Figure 9] Schematic diagram showing the manufacturing method of each part X1 to X4 of the cathode frame 130 [Figure 10] FIG. 1 is an explanatory diagram showing gas flows in an air electrode frame 130 of the embodiment and an air electrode frame 130X of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Specific examples of the technology disclosed in this specification will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0014] <Embodiment> The embodiment will be described with reference to Figures 1 to 10. A fuel cell stack 10 (an example of an electrochemical reaction cell stack) of the present embodiment is used in a solid oxide fuel cell having an electrolyte layer 112 containing a solid oxide.

[0015] (Overall configuration of fuel cell stack 10) 1 to 4, the fuel cell stack 10 includes a power generation block 100, an end separator 230, a first plate 232, a second plate 260, a first terminal plate 240, a second terminal plate 250, an insulating section 220, a first end plate 210, a second end plate 270, and four gas passage members 280. The first end plate 210, the insulating section 220, the end separator 230, the first terminal plate 240, the power generation block 100, the second terminal plate 250, the second plate 260, and the second end plate 270 have rectangular outer shapes of approximately the same size, and are arranged overlapping in this order in a predetermined arrangement direction (the up-down direction in FIG. 2).

[0016] As shown in Figures 1 and 4, the fuel cell stack 10 has bolt holes BH near each of the four corners, penetrating from the first end plate 210 to the second end plate 270. A bolt B is inserted into each bolt hole BH. A nut N is screwed onto both ends of each bolt B. These bolts B and nuts N fasten the members from the first end plate 210 to the second end plate 270 together. As shown in Figures 2 to 4, the first plate 232 is supported by the end separator 230, and the four gas passage members 280 are connected to the second end plate 270.

[0017] As shown in Figures 2 to 4, the power generation block 100 is composed of multiple (seven in this embodiment) electrochemical reaction units 100U (hereinafter sometimes abbreviated as "reaction units 100U") arranged in a predetermined arrangement direction (up and down direction in Figure 2).

[0018] (Overall configuration of 100U electrochemical reaction units) 5 and 6, the electrochemical reaction unit 100U includes a single cell 110, a single cell separator 120 (an example of a first member), an air electrode frame 130, an anode frame 140, an anode current collecting member 144, two interconnectors 190, and two IC separators 180 (an example of a second member). One IC separator 180, the air electrode frame 130, the single cell separator 120, the anode frame 140, and the other IC separator 180 are stacked in this order. The single cell 110 is supported by the single cell separator 120, the two interconnectors 190 are supported by the two IC separators 180, and the anode current collecting member 144 is disposed between the single cell 110 and the interconnectors 190.

[0019] 5 and 6, the IC separator 180 and the interconnector 190 are shared by two adjacent reaction units 100U. However, as shown in FIG. 2, the reaction unit 100U located at one end (the lower end in FIG. 2) of the multiple reaction units 100U does not have the IC separator 180 and the interconnector 190 adjacent to the fuel electrode frame 140, and the second terminal plate 250 overlaps the fuel electrode frame 140.

[0020] (single cell 110) The unit cell 110 includes an electrolyte layer 112, an air electrode 114, and an anode 116. As shown in Figures 5 and 6, the air electrode 114, the electrolyte layer 112, and the anode 116 are arranged in this order, with a reaction prevention layer 118 interposed between the electrolyte layer 112 and the air electrode 114. The unit cell 110 of this embodiment is an anode-supported unit cell in which the other layers (electrolyte layer 112, air electrode 114, and reaction prevention layer 118) constituting the unit cell 110 are supported by the anode 116.

[0021] The electrolyte layer 112 is a rectangular flat member, and has one surface (upper surface in Figs. 5 and 6) on which the air electrode 114 is disposed, and the other surface (lower surface in Figs. 5 and 6) on which the fuel electrode 116 is disposed and parallel to the first surface. The electrolyte layer 112 is a layer containing a solid oxide (e.g., YSZ (yttria-stabilized zirconia)). The air electrode 114 is a layer having a rectangular shape smaller than that of the electrolyte layer 112, and contains, for example, a perovskite-type oxide (e.g., LSCF (lanthanum strontium cobalt iron oxide)). The fuel electrode 116 is a layer having a rectangular shape of approximately the same size as the electrolyte layer 112, and contains, for example, Ni (nickel), a cermet made of Ni and ceramic particles, a Ni-based alloy, or the like. The reaction prevention layer 118 is a layer having a rectangular shape of approximately the same size as the air electrode 114, and contains, for example, GDC (gadolinium-doped ceria). The reaction prevention layer 118 has the function of suppressing the reaction of an element (e.g., Sr) diffused from the air electrode 114 with an element (e.g., Zr) contained in the electrolyte layer 112 to produce a highly resistive substance (e.g., SrZrO3).

[0022] (Separator for single cell 120) As shown in Figures 5 and 6, the single cell separator 120 is a rectangular frame-like member having a substantially rectangular through-hole 121 near the center, and is made of, for example, metal. The plate thickness of the single cell separator 120 is relatively thin, for example, 0.05 mm or more and 0.2 mm or less. The peripheral portion of the through-hole 121 in the single cell separator 120 is joined to the peripheral portion of one surface of the electrolyte layer 112 (the surface on which the air electrode 114 is disposed: the upper surface in Figures 5 and 6) by a joint 124. The joint 124 is made of, for example, a brazing material (Ag brazing).

[0023] (Air electrode frame 130) 5 and 6, the air electrode frame 130 is a rectangular frame-like member having a substantially rectangular through-hole 131 near the center, and is made of, for example, mica. The thickness of the air electrode frame 130 is preferably 0.5 mm or more and 5 mm or less.

[0024] (fuel electrode frame 140) As shown in FIG. 6, the fuel electrode frame 140 is a rectangular frame-like member having a substantially rectangular through-hole 141 near the center, and is made of, for example, metal.

[0025] (IC separator 180) As shown in FIGS. 5 and 6, IC separator 180 is a rectangular frame-like member having a through hole 181 near the center, and is made of, for example, metal.

[0026] (Interconnector 190 and anode current collecting member 144) 5 and 6, the interconnector 190 includes a rectangular flat plate portion 191, a plurality of plate-shaped air electrode current collectors 192 protruding from one surface of the flat plate portion 191 toward the air electrode 114, and a coating layer 193. The flat plate portion 191 and the air electrode current collector 192 are conductive and made of a metal (e.g., ferritic stainless steel). The coating layer 193 is conductive and is disposed so as to cover the surface of the air electrode current collector 192 and the surface of the flat plate portion 191 on which the air electrode current collector 192 is disposed. The flat plate portion 191 is joined to the periphery of the through hole 181 in the IC separator 180 by, for example, welding.

[0027] The anode current collecting member 144 is a member that connects the interconnector 190 and the anode 116, and is formed of a conductive material such as nickel, a nickel alloy, or stainless steel. As shown in Figures 5 and 6, the anode current collecting member 144 includes an interconnector facing portion 146, an electrode facing portion 145 parallel to the interconnector facing portion 146, and a connecting portion 147 that connects the electrode facing portion 145 and the interconnector facing portion 146, and has a U-shape overall. The electrode facing portion 145 is in contact with the anode 116, and the interconnector facing portion 146 is in contact with a flat portion 191 of the interconnector 190.

[0028] As described above, the interconnector 190 is shared by two adjacent reaction units 100U. More specifically, as shown in Figs. 5 and 6, the air electrode current collector 192 is joined to the air electrode 114 of the unit cell 110 provided in one of the two adjacent reaction units 100U via a conductive bonding material 196 made of, for example, a spinel-type oxide, and is thus electrically connected to the air electrode 114. The flat plate portion 191 is electrically connected to the fuel electrode 116 of the unit cell 110 provided in the other of the two adjacent reaction units 100U via the fuel electrode current collector 144. This ensures electrical continuity between the two adjacent reaction units 100U.

[0029] However, as described above, the reaction unit 100U located at one end (the lower end in FIG. 2) of the multiple reaction units 100U does not have an interconnector 190 on the fuel electrode 116 side. The fuel electrode 116 included in this reaction unit 100U is connected to the second terminal plate 250 via the fuel electrode current collecting member 144.

[0030] A spacer 149 made of, for example, mica is disposed between the electrode facing portion 145 and the interconnector facing portion 146. Therefore, the anode current collecting member 144 follows the deformation of the reaction unit 100U caused by temperature cycles and reactant gas pressure fluctuations, and the electrical connection between the anode 116 and the interconnector 190 (or the second terminal plate 250) via the anode current collecting member 144 is well maintained.

[0031] (Air chamber 313 and fuel chamber 323) 5 and 6, the space partitioned by the single cell separator 120, the single cell 110, the air electrode frame 130, the IC separator 180, and the interconnector 190 faces the air electrode 114 and serves as an air chamber 313 (an example of a gas chamber) through which the oxidant gas OG flows. The air electrode frame 130 partitions the air chamber 313 from the outside space all around, and seals the gap between the single cell separator 120 and the IC separator 180, thereby preventing gas from leaking from the air chamber 313 to the outside space.

[0032] The space partitioned by the single cell separator 120, the single cell 110, the fuel electrode frame 140, the IC separator 180, and the interconnector 190 faces the fuel electrode 116 and serves as a fuel chamber 323 through which the fuel gas FG flows. The fuel electrode frame 140 partitions the entire periphery of the fuel chamber 323 from the external space, and seals the gap between the single cell separator 120 and the IC separator 180, thereby preventing gas from leaking from the fuel chamber 323 to the external space.

[0033] The single cell separator 120 separates the air chamber 313 and the fuel chamber 323, and suppresses gas leakage (cross leakage) from the air electrode 114 side to the fuel electrode 116 side or from the fuel electrode 116 side to the air electrode 114 side around the single cell 110. In addition, the IC separator 180 and the interconnector 190 suppress gas leakage between adjacent reaction units 100U.

[0034] (First end plate 210) The first end plate 210 is a member formed by pressing (bending) a single plate-shaped member, and is formed of a conductive material such as stainless steel. As shown in Figs. 1 to 4, the first end plate 210 includes a rectangular frame-shaped flat portion 211 having a through hole 212 near the center, and an outer convex portion 213 and an inner convex portion 214 that protrude from the flat portion 211 in the opposite direction to the insulating portion 220 (upward in Fig. 2). The flat portion 211 has holes that form the bolt holes BH described above. The outer convex portion 213 protrudes from the outer periphery of the flat portion 211. The outer convex portion 213 is formed around the entire circumference of the outer periphery of the flat portion 211. The inner convex portion 214 protrudes from the inner periphery of the flat portion 211. The inner convex portion 214 is formed around the entire circumference of the inner periphery of the flat portion 211.

[0035] (insulating part 220) Insulating section 220 is a rectangular frame-shaped member having a through hole near the center, and is formed of, for example, an insulating material. Insulating section 220 is sandwiched between first end plate 210 and end separator 230 as shown in Fig. 2, so that insulation between first end plate 210 and end separator 230 is ensured.

[0036] (Terminal separator 230) As shown in FIGS. 2 to 4, end separator 230 is a rectangular frame-like member having a through hole 231 near the center, and is made of, for example, metal.

[0037] (First Plate 232) The first plate 232 is a rectangular flat member and is made of a conductive material such as stainless steel. As shown in Figures 2 to 4, the first plate 232 is joined to the periphery of the through hole 231 in the end separator 230 by, for example, welding. The end separator 230 and the first plate 232 separate the power generation block 100 from the external space of the fuel cell stack 10.

[0038] The first plate 232 is connected to an interconnector 190 provided in the reaction unit 100U arranged at the other end (the upper end in Figure 2) of the multiple reaction units 100U that make up the power generation block 100 via a connecting member having the same structure as the anode current collecting member 144, thereby electrically connecting this reaction unit 100U and the first plate 232.

[0039] (First terminal plate 240) The first terminal plate 240 is a rectangular frame-shaped member having a through hole 241 near the center, and is made of a conductive material such as ferritic stainless steel that forms an alumina oxide film on its surface. The first terminal plate 240 is electrically connected to the reaction unit 100U arranged at the other end (upper end in FIG. 2) of the multiple reaction units 100U constituting the power generation block 100 via the first plate 232 and the end separator 230. One end (right end in FIG. 2) of the first terminal plate 240 protrudes laterally from the power generation block 100, and this protruding portion functions as a positive output terminal of the fuel cell stack 10.

[0040] (2nd terminal plate 250) The second terminal plate 250 is a rectangular plate-like member, and is made of a conductive material such as ferritic stainless steel that forms an alumina oxide film on its surface. As described above, the second terminal plate 250 is connected to the fuel electrode 116 provided in the reaction unit 100U arranged at one end (the lower end in FIG. 2) of the multiple reaction units 100U via the fuel electrode current collecting member 144, thereby electrically connecting the reaction unit 100U to the second terminal plate 250. One end (the right end in FIG. 2) of the second terminal plate 250 protrudes laterally from the power generation block 100, and this protruding portion functions as a negative output terminal of the fuel cell stack 10.

[0041] (Second plate 260) The second plate 260 is a rectangular flat member and is made of, for example, an insulating material. The peripheral portion of the second plate 260 is sandwiched between the second terminal plate 250 and the second end plate 270, thereby ensuring insulation between the second terminal plate 250 and the second end plate 270.

[0042] (Second end plate 270) The second end plate 270 is a member formed by pressing (bending) a single plate-shaped member, and is formed of a conductive material such as stainless steel. The second end plate 270 includes a rectangular frame-shaped flat portion 271 having a through hole 272 near the center, and an outer convex portion 273 and an inner convex portion 274 that protrude from the flat portion 271 in the opposite direction to the second terminal plate 250 (downward in FIG. 2). The flat portion 271 has holes that form the bolt holes BH described above. The outer convex portion 273 protrudes from the outer periphery of the flat portion 271. The outer convex portion 273 is formed around the entire circumference of the outer periphery of the flat portion 271. The inner convex portion 274 protrudes from the inner periphery of the flat portion 271. The inner convex portion 274 is formed around the entire circumference of the inner periphery of the flat portion 271.

[0043] (Manifolds 311, 312, 321, 322) 1, 2, and 3, the fuel cell stack 10 has four holes that penetrate from the power generation block 100 to the second end plate 270. The four holes are an oxidant gas supply manifold 311 (an example of a communication passage), an oxidant gas discharge manifold 312 (an example of a communication passage), a fuel gas supply manifold 321, and a fuel gas discharge manifold 322, respectively.

[0044] 2, the oxidant gas supply manifold 311 is a gas flow path that supplies the oxidant gas OG introduced from outside the fuel cell stack 10 to the air chamber 313 of each reaction unit 100U. The oxidant gas discharge manifold 312 is a gas flow path that discharges the oxidant off-gas OOG discharged from the air chamber 313 of each reaction unit 100U to the outside of the fuel cell stack 10. For example, air is used as the oxidant gas OG. The oxidant gas supply manifold 311 and the oxidant gas discharge manifold 312 are arranged on opposite sides of each other with the air chamber 313 in between.

[0045] As shown in Fig. 3, the fuel gas supply manifold 321 is a gas flow path that supplies the fuel gas FG introduced from outside the fuel cell stack 10 to the fuel chamber 323 of each reaction unit 100U. The fuel gas discharge manifold 322 is a gas flow path that discharges the fuel off-gas FOG discharged from the fuel chamber 323 of each reaction unit 100U to the outside of the fuel cell stack 10. For example, hydrogen-rich gas obtained by reforming city gas is used as the fuel gas FG. The fuel gas supply manifold 321 and the fuel gas discharge manifold 322 are arranged on opposite sides of the fuel chamber 323.

[0046] As shown in FIG. 5, the air electrode frame 130 has an oxidant gas supply communication passage 132 that connects the oxidant gas supply manifold 311 and the air chamber 313, and an oxidant gas discharge communication passage 133 that connects the air chamber 313 and the oxidant gas discharge manifold 312.

[0047] In addition, as shown in FIG. 6, each fuel electrode frame 140 has a fuel gas supply communication passage 142 that connects the fuel gas supply manifold 321 and the fuel chamber 323, and a fuel gas discharge communication passage 143 that connects the fuel chamber 323 and the fuel gas discharge manifold 322.

[0048] (Gas passage member 280) As shown in Figs. 2 and 3, each of the four gas passage members 280 includes a main body portion 281 and a flange portion 282. The main body portion 281 is tubular with both ends open. The flange portion 282 is provided so as to protrude outward from one end (the lower end in Fig. 2) of the main body portion 281. The flange portion 282 has a plurality of bolt holes 284. A bolt (not shown) for connecting the fuel cell stack 10 to an external device is inserted into each bolt hole 284. One end (the upper end in Figs. 2 and 3) of the main body portion 281 included in each of the four gas passage members 280 is joined to the second end plate 270 by, for example, welding, and the internal space of the main body portion 281 is connected to the manifolds 311, 312, 321, and 322, respectively. A gas pipe for supplying or discharging gas is connected to each of the main body portions 281.

[0049] (Operation of fuel cell stack 10) 2 and 5, the oxidizing gas OG is supplied to the oxidizing gas supply manifold 311 via the gas passage member 280, and is then supplied to the air chamber 313 via the oxidizing gas supply communicating passage 132. The oxidizing gas OG flows inside the air chamber 313 from the oxidizing gas supply communicating passage 132 toward the oxidizing gas discharge communicating passage 133.

[0050] Also, as shown in Figures 3 and 6, fuel gas FG is supplied from the gas piping through the gas passage member 280 to the fuel gas supply manifold 321, and is supplied to the fuel chamber 323 through the fuel gas supply communicating passage 142 from the holes that constitute the fuel gas supply manifold 321 of each fuel electrode frame 140.

[0051] When the oxidant gas OG is supplied to the air chamber 313 of each reaction unit 100U and the fuel gas FG is supplied to the fuel chamber 323, power is generated in the single cell 110 by an electrochemical reaction between the oxidant gas OG and the fuel gas FG. This power generation reaction is an exothermic reaction. As described above, the interconnector 190 is shared by two adjacent reaction units 100U, and the interconnector 190 ensures electrical continuity between the two adjacent reaction units 100U. That is, the multiple reaction units 100U included in the fuel cell stack 10 are electrically connected in series. In addition, the second terminal plate 250 is electrically connected to the reaction unit 100U located at one end (the lower end of FIG. 2) of the multiple reaction units 100U, and the first terminal plate 240 is electrically connected to the reaction unit 100U located at the other end (the upper end of FIG. 2). As a result, electrical energy generated in each reaction unit 100U is taken out from the terminal plates 240 and 250 that function as the output terminals of the fuel cell stack 10. Since SOFCs generate electricity at relatively high temperatures (e.g., 700°C to 1000°C), after startup, the fuel cell stack 10 may be heated by a heater (not shown) until the heat generated by power generation can maintain the high temperature.

[0052] 2 and 5, the oxidant off-gas OOG discharged from the air chamber 313 of each reaction unit 100U to the oxidant gas discharge manifold 312 via the oxidant gas discharge communication passage 133 is discharged to the outside of the fuel cell stack 10 through the internal space of the main body 281. Also, as shown in Figures 3 and 6, the fuel off-gas FOG discharged from the fuel chamber 323 of each reaction unit 100U to the fuel gas discharge manifold 322 via the fuel gas discharge communication passage 143 is discharged to the outside of the fuel cell stack 10 through the internal space of the main body 281.

[0053] (Detailed configuration of the air electrode frame 130) As described above, the air electrode frame 130 (an example of a flow path forming member) is disposed between the single cell separator 120 and the IC separator 180. Hereinafter, the space including the air chamber 313, the oxidant gas supply manifold 311, and the oxidant gas discharge manifold 312 will be referred to as the "oxidant gas flow path." The air electrode frame 130 separates the oxidant gas flow path from the fuel chamber 323 (an example of a space other than the gas flow path) and the external space of the fuel cell stack 10 (an example of a space other than the gas flow path).

[0054] Specifically, as shown in Fig. 5, in the air electrode frame 130, a first portion X1 between the through hole constituting the oxidant gas supply manifold 311 and the outer peripheral surface of the air electrode frame 130 separates the oxidant gas flow path from the external space of the fuel cell stack 10. In the air electrode frame 130, a second portion X2 between the through hole constituting the oxidant gas discharge manifold 312 and the outer peripheral surface of the air electrode frame 130 separates the oxidant gas flow path from the external space of the fuel cell stack 10. In addition, as shown in Fig. 6, in the air electrode frame 130, a third portion X3 between the through hole constituting the fuel gas supply manifold 321 and the through hole 131 separates the oxidant gas flow path from the fuel gas supply manifold 321 (fuel chamber 323). In the air electrode frame 130, a fourth portion X4 between the through holes 131 constituting the fuel gas discharge manifold 322 separates the oxidant gas flow path and the fuel gas discharge manifold 322 (fuel chamber 323).

[0055] The air electrode frame 130 (each of the portions X1 to X4) has a layered structure made of a plurality of layered particles 400 stacked in the above-mentioned predetermined arrangement direction (the vertical direction in FIG. 2, an example of the first direction) in which the single cell separator 120 and the IC separator 180 face each other. Specifically, the air electrode frame 130 is made of mica, as described above.

[0056] Here, in at least one specific cross section (e.g., XZ cross section) along the arrangement direction of the air electrode frame 130, first layered particles 400R, 400L and second layered particle 400C are present. The first layered particle 400R is a layered particle 400 located at the right end of each of the portions X1 to X4 of the air electrode frame 130 in a planar direction (the left-right direction in FIG. 2, an example of a second direction) perpendicular to the arrangement direction. The first layered particle 400L is a layered particle 400 located at the left end of each of the portions X1 to X4 of the air electrode frame 130 in the planar direction. The second layered particle 400C is a layered particle 400 located at the center of each of the portions X1 to X4 in the planar direction (a portion through which the center line C passes).

[0057] The relative angle of the first layered particles 400R and 400L with respect to a predetermined reference vector V along the surface direction is defined as a first angle θ1, and the relative angle of the second layered particle 400C with respect to the reference vector V is defined as a second angle θ2. There is a difference between the first angle θ1 of the first layered particle 400R and the second angle θ2 of the second layered particle 400C. There is also a difference between the first angle θ1 of the first layered particle 400L and the second angle θ2 of the second layered particle 400C.

[0058] Hereinafter, a specific description will be given by taking the first portion X1 of the air electrode frame 130 as an example. As shown in FIG. 7, the first portion X1 of the air electrode frame 130 is divided into 10 regions at equal intervals in the arrangement direction (Z-axis direction). Each divided region is called a divided region E (E1 to E10). In at least one divided region E, there is a difference between the first angle θ1 of at least one of the first layered particles 400R, 400L and the second angle θ2 of the second layered particle 400C. In each of the portions X1 to X4 of the air electrode frame 130, the region (the number of divided regions E) where there is an angle difference between the first angle θ1 and the second angle θ2 is preferably 30% or more, more preferably 50% or more, of the total region (10 divided regions E).

[0059] FIG. 8 shows the reference vector V and the measurement regions TR, TL, and TC. The reference vector V is parallel to the surface direction (X-axis direction) and faces the negative X-axis direction. The first angle θ1 and the second angle θ2 are both positive angles when the layered particle 400 is inclined upward (positive Z-axis direction) with respect to the reference vector V, and are both negative angles when the layered particle 400 is inclined downward (negative Z-axis direction) with respect to the reference vector V. The measurement regions TR, TL, and TC are regions for identifying the first angle θ1 and the second angle θ2. The measurement regions TR, TL, and TC are all the same size, have a predetermined width W (e.g., 300 μm) in the surface direction, and have the same height H as the divided region E.

[0060] As shown in FIG. 8, in order to determine the first angle θ1 of the first layered particle 400R, the right side of the measurement area TR located on the right side coincides with the right end of the air electrode frame 130. A plurality of first layered particles 400R are present in this measurement area TR. For each first layered particle 400R, the relative angle with respect to the reference vector V with the right end as the base point is determined as the respective first angle θ1. Note that the first angle θ1 of the first layered particle 400R shown in FIG. 8 is a positive angle. The average value of the first angles θ1 of all the first layered particles 400R present in the measurement area TR is set as the first angle θ1 of the first layered particle 400R in the divided area E1.

[0061] In order to determine the first angle θ1 of the first layered particle 400L, the left side of the measurement area TL located on the left side coincides with the left end of the air electrode frame 130. A plurality of first layered particles 400L are present in this measurement area TL. For each first layered particle 400L, the relative angle with respect to the reference vector V with the right end as the base point is determined as the respective first angle θ1. Note that the first angle θ1 of the first layered particle 400L shown in FIG. 8 is a negative angle. The average value of the first angles θ1 of all the first layered particles 400L present in the measurement area TL is set as the first angle θ1 of the first layered particles 400L in the divided area E1.

[0062] In order to determine the second angle θ2 of the second layered particle 400C, the measurement area TC includes the center (center line C) of the first portion X1. A plurality of second layered particles 400C are present in this measurement area TC. For each second layered particle 400C, a relative angle with respect to the reference vector V with the right end as the base point is determined as the second angle θ2. Note that the second angle θ2 of the second layered particle 400C shown in FIG. 8 is a positive angle. The average value of the second angles θ2 of all the second layered particles 400C present in the measurement area TC is set as the second angle θ2 of the second layered particles 400C in the divided area E1.

[0063] Next, the absolute value of the difference between the first angle θ1 of the first layered particle 400R and the second angle θ2 of the second layered particle 400C is preferably 1.4 degrees or more. Also, the absolute value of the difference between the first angle θ1 of the first layered particle 400L and the second angle θ2 of the second layered particle 400C is preferably 1.4 degrees or more.

[0064] The absolute value of the first angle θ1 of the first layered particle 400R is preferably less than 90 degrees. Also, the absolute value of the first angle θ1 of the first layered particle 400L is preferably less than 90 degrees.

[0065] In a particular cross section, the width D in the planar direction of each of the portions X1 to X4 of the cathode frame 130 is preferably three times or more the height H in the vertical direction (see FIG. 7).

[0066] (Manufacturing method of the air electrode frame 130) As described above, in each of the portions X1 to X4 of the cathode frame 130, the second layered particle 400C located in the center is approximately parallel to the surface direction, and the first layered particles 400R, 400C located at the ends are both inclined with respect to the surface direction in the same divided region E. An example of a method for producing each of the portions X1 to X4 having such a layered structure is as follows.

[0067] As shown in FIG. 9, the mica material 130A is pressed using a mold 500 to produce the individual parts X1 to X4 of the air electrode frame 130. The mica material 130A has a layered structure in which almost all layered particles are aligned along the surface direction (the X-axis direction in FIG. 9). The mold 500 includes a first mold 510 and a second mold 520. The first mold 510 has a base portion 512 and a peripheral wall portion 514. The peripheral wall portion 514 is a cylindrical portion that surrounds the periphery of the mica material 130A. The base portion 512 is a flat plate-like portion that seals one end side of the peripheral wall portion 514 (the Z-axis positive direction side in FIG. 9). A groove 513 is formed in the peripheral edge portion of the surface of the base portion 512 that faces the inside of the peripheral wall portion 514. The groove 513 has a tapered surface 515 that is inclined so that the depth increases toward the peripheral wall portion 514. The second die 520 is a flat plate-like member that can enter the inside of the peripheral wall portion 514 of the first die 510 .

[0068] For example, the mica material 130A is placed on the second die 520, and the mica material 130A is pressed between the first die 510 and the second die 520. This forms the mica material 130B. The mica material 130B has a shape in which the ends of the mica material 130A have protrusions 132B that are inclined along the shape of the grooves 513 of the base portion 512. Next, the tips of the protrusions 132B of the mica material 130B are partially cut away to form the mica material 130C. This mica material 130C has the layered structure of the portions X1 to X4 of the air electrode frame 130.

[0069] (Action and effect) As described above, the fuel cell stack 10 of this embodiment includes a plurality of electrochemical reaction units 100U. Each electrochemical reaction unit 100U includes a single cell 110 in which an air electrode 114, an electrolyte layer 112, and a fuel electrode 116 are stacked in this order, an air electrode frame 130 that separates an air chamber 313 that the air electrode 114 faces from an external space, a single cell separator 120 adjacent to the air electrode frame 130, and an IC separator 180 adjacent to the air electrode frame 130. In each electrochemical reaction unit 100U, first layered particles 400R, 400L and a second layered particle 400C are present in at least one specific cross section (e.g., XZ cross section) of the air electrode frame 130 along the arrangement direction. The first angle θ1 of the first layered particles 400R, 400L located at the end of each of the portions X1-X4 in the cathode frame 130 is different from the second angle θ2 of the second layered particle 400C located in the center of each of the portions X1-X4. In other words, in a specific cross section of each of the portions X1-X4, there are first layered particles 400R, 400L located at the end and inclined with respect to the second layered particle 400C located in the center.

[0070] According to the above configuration, the presence of the second layered particles 400C in the air electrode frame 130 ensures the stress relaxation of the air electrode frame 130. Furthermore, the presence of the first layered particles 400R, 400L prevents the gas G (oxidant gas OG, oxidant off-gas OOG) in the air chamber 313 from passing between the layered particles 400 constituting the flow path forming member and leaking into the external space or the fuel chamber 323. Therefore, according to the present embodiment, while ensuring the stress relaxation of the air electrode frame 130, gas leakage from the air electrode frame 130 can be suppressed compared to a configuration in which the layered particles are uniformly aligned along the surface direction.

[0071] Specifically, in the air electrode frame 130X of the comparative example shown in the lower part of FIG. 10, not only the second layered particle 400C located in the center but also the first layered particles 400RX, 400LX located at the end extend along the surface direction. Therefore, the air electrode frame 130X has a relatively large number of paths that extend linearly along the surface direction, which makes it easy for the gas G to leak from the oxidant gas flow path to another space. In contrast, in the air electrode frame 130 of the present embodiment shown in the upper part of FIG. 10, the second layered particle 400C located in the center extends along the surface direction, and the first layered particles 400RX, 400LX located at the end are inclined with respect to the surface direction. Therefore, the air electrode frame 130 has a relatively large number of paths whose ends are partially inclined with respect to the surface direction, which makes it difficult for the gas G to leak from the oxidant gas flow path to another space.

[0072] In this embodiment, the absolute value of the difference between the first angle θ1 of the first layered particle 400R and the second angle θ2 of the second layered particle 400C is preferably 1.4 degrees or more. With this configuration, gas leakage from the cathode frame 130 can be more effectively suppressed than, for example, a configuration in which the absolute value of the difference between the first angle θ1 and the second angle θ2 is less than 1.4 degrees.

[0073] In this embodiment, the absolute value of the first angle θ1 of the first layered particles 400R, 400L is preferably less than 90 degrees. According to such a configuration, the stress relaxation property of the air electrode frame 130 caused by the presence of the first layered particles 400R, 400L can be suppressed compared to a configuration in which the absolute value of the first angle θ1 is 90 degrees. In this embodiment, the air electrode frame 130 is formed of an insulating material (mica). Therefore, according to this embodiment, the creepage distance between the single cell separator 120 and the IC separator 180 passing through the surface of the layered particle 400 is longer than that in a configuration in which the first angle θ1 is 90 degrees, and the insulation property is improved.

[0074] In this embodiment, in a specific cross section, the planar width D of each of the portions X1-X4 of the air electrode frame 130 is preferably three or more times the vertical width (height) H. According to this embodiment, compared to, for example, a configuration in which the planar width D of each of the portions X1-X4 of the air electrode frame 130 is less than three times the vertical width H, the path within the air electrode frame 130 between the air chamber 313 and a space other than the air chamber 313 (the fuel chamber 323 or the external space) is longer, so that gas leakage from the air electrode frame 130 can be effectively suppressed while ensuring the stress relaxation of the air electrode frame 130.

[0075] (Performance Evaluation of the Present Embodiment) Next, performance evaluation of this embodiment will be described. Nine samples of the air electrode frame 130 were produced, and performance evaluation was carried out for the fuel cell stack 10 using each sample. Table 1 below shows the results of the performance evaluation.

[0076] [Table 1]

[0077] As shown in Table 1, each sample (samples S1 to S9) basically has the same configuration as the cathode frame 130 described above and was manufactured by the manufacturing method described above. However, the cathode frames 130 of the nine samples (samples S1 to S9) differ from each other in at least one of the following elements. The first angle θ1 of the first layered particles 400R and 400L located at the ends The second angle θ2 of the second layered particle 400C located in the center The angle difference between the first angle θ1 and the second angle θ2 The ratio of the width D to the height H of the part of the cathode frame 130 that separates the spaces The method for obtaining these values ​​is as follows: A cross section of the cathode frame 130 of each sample is photographed, for example, by a scanning electron microscope (SEM). The above values ​​of each sample can be obtained by performing image analysis on the SEM images obtained by photographing.

[0078] (1) Initial power generation performance For the fuel cell stack 10 using each sample, an oxidant gas OG was supplied to the air electrode 114 at approximately 700° C., a fuel gas FG was supplied to the fuel electrode 116, and a current density of 0.55 A / cm 2 The output voltage of the single cell 110 at this time was measured, and this measured value was taken as the initial voltage (the output voltage before rated power generation operation).

[0079] Regarding the initial power generation performance of the fuel cell stack 10, for each sample, samples whose initial voltage was equal to or greater than a predetermined first judgment threshold were evaluated as "good (△)", and samples whose initial voltage was less than the first judgment threshold were evaluated as "poor (×)". Samples whose initial voltage was equal to or greater than a second judgment threshold higher than the first judgment threshold were evaluated as "best (◯)".

[0080] (2) Reliability (stress relaxation characteristics) Regarding the reliability of the fuel cell stack 10, for each sample, samples whose voltage drop rate after 50 cycles of the thermal cycle test was below a predetermined first level were rated as "best (O)", and samples whose voltage drop rate after 50 cycles of the thermal cycle test exceeded the first level were rated as "good (△)".

[0081] The thermal cycle test was carried out according to the following procedure. First, to examine the initial power generation performance, an oxidant gas OG was supplied to the air electrode 114 and a fuel gas FG was supplied to the fuel electrode 116 at about 700°C. 2 The output voltage of the single cell 110 at this time was measured. The measured value was taken as the initial voltage (the output voltage before the thermal cycle test). Next, an oxidant gas OG was supplied to the air electrode 114, a fuel gas FG was supplied to the fuel electrode 116, and the current density was 0 A / cm 2 In this state, the temperature was lowered to about 70°C. One cycle consisted of raising the temperature from room temperature to about 700°C and then lowering the temperature from 700°C to 70°C, and a total of 50 cycles were repeated. After the 50 cycles were completed, the temperature was raised again to about 700°C, an oxidant gas OG was supplied to the air electrode 114, a fuel gas FG was supplied to the fuel electrode 116, and a current density of 0.55 A / cm was applied.2 The output voltage of the single cell 110 at this time was measured. The measured value was taken as the output voltage after the thermal cycle. The voltage drop rate after 50 thermal cycles was calculated by "(initial voltage - output voltage after the thermal cycle) / initial voltage".

[0082] As shown in Table 1, the initial power generation performance of sample S1, in which the angle difference was 0.0 degrees, was evaluated as "poor (x)". On the other hand, the initial power generation performance of samples S2 to S9, in which the angle difference was 1.0 degrees or more, was evaluated as "good (△)" or "best (◯)". This means that the difference between the first angle θ1 of the first layered particles 400R, 400L located at the ends of the air electrode frame 130 and the second angle θ2 of the second layered particle 400C located at the center is such that gas leakage from the air electrode frame 130 is suppressed and a drop in the initial voltage is suppressed. In addition, although samples S2 to S6 have the same ratio of width D to height H, sample S2 was evaluated as "good (△)" in initial power generation performance, and samples S3 to S6 were evaluated as "best (◯)" in initial power generation performance. This means that if the angle difference is 5.0 degrees or more, gas leakage from the cathode frame 130 is effectively suppressed, and the drop in initial voltage is further suppressed.

[0083] In sample S6, in which the first angle θ1 was 90 degrees, the reliability was evaluated as "good (△)," while in samples S1 to S5 and S7 to S9 (especially sample S5), in which the first angle θ1 was less than 90 degrees, the reliability was evaluated as "best (◯)." This means that the stress relaxation properties of the cathode frame 130 are ensured by having the first angle θ1 be less than 90 degrees.

[0084] Although the angle difference in samples S3 to S9 was 1.5 degrees or more, the initial power generation performance of sample S7 was evaluated as “good (△),” while the initial power generation performance of samples S3 to S6, S8, and S9 was evaluated as “best (◯).” This means that gas leakage from the cathode frame 130 can be effectively suppressed if the ratio of width D to height H is 3 or more.

[0085] <Other embodiments> In the above embodiment, mica is exemplified as the material of the flow path forming member (air electrode frame 130), but other than mica, for example, vermiculite, or other material having a layered structure made of multiple layered particles may be used. Note that the material of the flow path forming member may be a material that does not have insulating properties.

[0086] In the above embodiment, the air electrode frame 130 is exemplified as the flow path forming member, but it may be, for example, the fuel electrode frame 140 separating the fuel chamber 323 from the other space. In short, the flow path forming member may be any member disposed between two members and separating the gas chamber (air chamber 313 or fuel chamber 323) from the other space. Also, for example, in an electrochemical reaction cell stack including a metal-supported single cell, the flow path forming member is a member disposed between a current collector electrically connected to the single cell and the metal support. Also, for example, in an electrochemical reaction cell stack including an electrolyte-supported single cell, the flow path forming member is a member disposed between the electrolyte of the single cell and the current collector.

[0087] In the above embodiment, only one of the first angle θ1 of the first layered particle 400R and the first angle θ1 of the first layered particle 400L may be different from the second angle θ2 of the second layered particle 400C. In the above embodiment, the absolute value of the difference between the first angle θ1 of the first layered particles 400R, 400L and the second angle θ2 of the second layered particle 400C may be less than 1.4 degrees. In the above embodiment, the first angle θ1 of the first layered particles 400R, 400L may be 90 degrees. In the above embodiment, the width D in the surface direction of each of the portions X1 to X4 of the cathode frame 130 may be less than three times the width H in the up-down direction.

[0088] In the above embodiment, the electrochemical reaction cell stack is a cell stack used in a solid oxide fuel cell (SOFC), but the above configuration is also applicable to cell stacks used in other types of fuel cells such as a polymer electrolyte fuel cell (PEFC), a phosphoric acid fuel cell (PAFC), and a molten carbonate fuel cell (MCFC), or an electrolysis cell stack having an electrolysis cell unit, which is a constituent unit of a solid oxide electrolysis cell (SOEC), as a single cell. [Explanation of symbols]

[0089] 10: Fuel cell stack 100: Power generation block 100U: Reaction unit 110: Single cell 112: Electrolyte layer 114: Air electrode 116: Fuel electrode 118: Reaction prevention layer 120: Separator for single cell 121: Through hole 124: Joint 130, 130X: Air electrode frame 130A-130C: Mica material 132: Oxidant gas supply communication channel 132B: Protrusion 133: Oxidant gas exhaust communication channel 140: Fuel electrode frame 142: Fuel gas supply communication channel 143: Fuel gas exhaust communication channel 144: Fuel electrode current collecting member 145: Electrode facing portion 146: Interconnector facing portion 147: Connection portion 149: Spacer 180: IC separator 190: Interconnector 191: Flat plate portion 192: Air electrode current collecting portion 193: Coating layer 196: Conductive bonding material 210: First end plate 220: Insulating portion 230: Terminal separator 232: First plate 240: First terminal plate 250: Second terminal plate 260: Second plate 270: Second end plate 280: Gas passage member 281: Main body portion 282: Flange portion 311: Oxidant gas supply manifold 312: Oxidant gas exhaust manifold 313: Air chamber 321: Fuel gas supply manifold 322: Fuel gas exhaust manifold 323: Fuel chamber 400: Layered particle 400C: Second layered particle 400R, 400L: First layered particle 400RX, 400LX: First layered particle 500: Mold 510: First mold 512: Base portion 513: Groove 514: Peripheral wall portion 515: Tapered surface 520: Second type B: Bolt N: Nut

Claims

1. The battery includes a plurality of unit cells each including an electrolyte layer and an air electrode and a fuel electrode that face each other with the electrolyte layer interposed therebetween; In an electrochemical reaction cell stack having a communication passage formed therein, the communication passage being in communication with a gas chamber facing one of the air electrode and the fuel electrode, A first member; a second member disposed opposite the first member; a flow passage forming member that is disposed between the first member and the second member and separates a gas flow passage including the gas chamber and the communication passage from a space other than the gas flow passage, the flow passage forming member has a layered structure made of a plurality of layered particles stacked in a first direction in which the first member and the second member face each other, an electrochemical reaction cell stack, characterized in that, in at least one specific cross section along the first direction, among the flow path forming member, there is present a first layered particle located at an end of the flow path forming member in a second direction perpendicular to the first direction, the first layered particle having a first angle with respect to the second direction that is different from a second angle formed with respect to the second direction by a second layered particle located at a center of the flow path forming member in the second direction.

2. 2. The electrochemical reaction cell stack according to claim 1, An electrochemical reaction cell stack, wherein an absolute value of a difference between the first angle and the second angle is 1.4 degrees or more.

3. 2. The electrochemical reaction cell stack according to claim 1, An electrochemical reaction cell stack, wherein an absolute value of the first angle is less than 90 degrees.

4. 2. The electrochemical reaction cell stack according to claim 1, An electrochemical reaction cell stack, wherein in the specific cross section, the width of the flow path forming member in the second direction is three times or more the width of the flow path forming member in the first direction.

5. A flow path forming member for an electrochemical reaction cell stack, comprising: A layered structure including a plurality of layered particles stacked in a first direction, A flow path forming member for an electrochemical reaction cell stack, characterized in that, in at least one specific cross section along the first direction, there are first layered particles located at an end of the flow path forming member in a second direction perpendicular to the first direction, the first layered particles having a first angle with respect to the second direction that is different from a second angle made with respect to the second direction by a second layered particle located at a center of the flow path forming member in the second direction.

Citation Information

Patent Citations

  • Fuel cell, and method of manufacturing the same

    JP2013004271A

  • Electrochemical reaction cell stack

    JP2022081266A

  • Electrochemical reaction cell stack

    JP2020170630A