Method for producing nickel powder, method for producing coating material, method for producing member, method for producing resin composition, and method for producing resin formed object
By wet milling nickel powder with a hydrogen-containing solvent, the method simplifies and reduces costs while achieving high antifungal efficacy in nickel powder production, applicable in paints, members, and resin compositions.
Patent Information
- Application Number
- JP2023063420
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing hydrogen-containing nickel powder for antifungal applications involve complex steps and separate pulverization treatments, leading to increased manufacturing costs.
A method involving wet milling of raw nickel powder using a solvent containing hydrogen, with a hydrogen content of 0.05% by mass or more, to produce nickel powder with excellent antifungal properties, optionally incorporating phosphorus and using fatty acids to facilitate pulverization.
The method enables simple and low-cost production of nickel powder with enhanced antifungal activity, suitable for use in paints, members, resin compositions, and resin molded articles.
Smart Images

Figure 2024150154000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing nickel powder, a method for producing a paint, a method for producing a component, a method for producing a resin composition, and a method for producing a resin molded product. [Background technology]
[0002] In recent years, from a hygienic point of view, coatings aimed at suppressing mold are applied in various situations, and it is common to add antifungal agents to coating agents and apply them. There are many types of antifungal agents known, but nickel powder is superior in terms of the durability of antifungal properties (see Patent Document 1 and Patent Document 2).
[0003] In order to impart mildew resistance to nickel powder, it is necessary to incorporate hydrogen into the powder. For example, in the following Patent Document 1, hydrogen is incorporated into the powder by immersion in an acid or oxidizing agent and heat treatment in a hydrogen atmosphere. In addition, in the following Patent Document 2, a method is used in which nickel is alloyed with Mg, which has excellent hydrogen storage properties, and then heat treatment is performed in a hydrogen gas atmosphere.
[0004] The hydrogen-containing raw nickel powder is pulverized to obtain nickel powder having a particle size required for the intended use. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-64401 A [Patent Document 2] Japanese Patent Application Publication No. 10-251702 Summary of the Invention [Problem to be solved by the invention]
[0006] The above-mentioned hydrogen-containing treatment method involves complicated steps and requires a separate pulverization treatment, which tends to increase production costs.
[0007] The present disclosure has been made based on the above-mentioned circumstances, and aims to provide a method for producing nickel powder that has excellent anti-fungal properties and can be produced easily and at low cost, as well as a method for producing a paint using nickel powder produced by the nickel powder production method, a method for producing a component, a method for producing a resin composition, and a method for producing a resin molded product. [Means for solving the problem]
[0008] A method for producing nickel powder according to one embodiment of the present disclosure is a method for producing nickel powder whose main component is nickel or a nickel alloy, and includes a wet-grinding process in which raw nickel powder is wet-grinded using a solvent containing elemental hydrogen, and the content of elemental hydrogen relative to the total mass of the nickel powder after the wet-grinding process is 0.05 mass% or more.
[0009] A paint manufacturing method according to another aspect of the present disclosure includes a paint preparation step of adding nickel powder to a paint material, and nickel powder manufactured by the nickel powder manufacturing method of the present disclosure is used as the nickel powder.
[0010] A method for manufacturing a member according to another aspect of the present disclosure includes a coating step of coating a member to be coated with paint, and uses paint manufactured by the method for manufacturing a paint according to the present disclosure as the paint.
[0011] A method for producing a resin composition according to another embodiment of the present disclosure includes a resin preparation step of adding nickel powder to a resin, and nickel powder produced by the nickel powder production method of the present disclosure is used as the nickel powder.
[0012] A method for producing a resin molded product according to another embodiment of the present disclosure includes a molding step of molding a resin composition, and uses a resin composition produced by the method for producing a resin composition according to the present disclosure as the resin composition. Effect of the Invention
[0013] The method for producing nickel powder of the present disclosure allows for simple and low-cost production, and the resulting nickel powder has excellent antifungal properties. In addition, the method for producing paint, the method for producing member, the method for producing resin composition, and the method for producing resin molded article of the present disclosure allow for simple and low-cost production, and the resulting paint, member, resin composition, and resin molded article have excellent antifungal properties. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a flow diagram showing a method for producing nickel powder according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a flow diagram showing a method for producing a paint and a method for producing a member according to one embodiment of the present disclosure. [Diagram 3] FIG. 3 is a flow diagram showing a method for producing a resin composition and a method for producing a resin molded article according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Description of the embodiments of the present disclosure] (1) A method for producing nickel powder according to one embodiment of the present disclosure is a method for producing nickel powder whose main component is nickel or a nickel alloy, comprising a wet-grinding step of wet-grinding a raw nickel powder using a solvent containing elemental hydrogen, and the content of elemental hydrogen relative to the total mass of the nickel powder after the wet-grinding step is 0.05 mass% or more.
[0016] In the method for producing nickel powder, the raw nickel powder is pulverized to a predetermined particle size, and hydrogen is added to the raw nickel powder from a solvent containing hydrogen element at the same time. Therefore, nickel powder can be produced simply and at low cost. In addition, the nickel powder is mainly composed of nickel or a nickel alloy, and nickel ions are eluted into adsorbed water that may be present in small amounts on the surface of the powder when in use. These nickel ions can come into contact with and kill bacteria and mold that may grow in the adsorbed water. Furthermore, since the content of hydrogen element relative to the total mass of the nickel powder is set to be equal to or higher than the lower limit, the hydrogen element easily forms hydrides that alter the proteins that constitute bacteria and mold, and the produced nickel powder exhibits excellent antifungal properties.
[0017] (2) In the method for producing nickel powder described in (1) above, the raw nickel powder may contain phosphorus. By including phosphorus in the raw nickel powder in this way, the phosphorus penetrates into the grain boundaries of the raw nickel powder, promoting the dissolution of nickel ions. Therefore, the antifungal effect is improved.
[0018] (3) In the method for producing nickel powder described in (2) above, the content of phosphorus element relative to the total mass of the nickel powder after the wet-pulverizing step may be 0.15 mass% or more and 15.70 mass% or less. By setting the content of phosphorus element relative to the total mass of the nickel powder after the wet-pulverizing step within the above range, the elution of nickel ions can be promoted.
[0019] (4) In the method for producing nickel powder according to any one of (1) to (3) above, the solvent may contain a fatty acid having a carboxyl group. By including a fatty acid having a carboxyl group in the solvent in this manner, the raw nickel powder can be rapidly pulverized to a predetermined particle size.
[0020] (5) In the method for producing nickel powder described in (4) above, the fatty acid may include one or more selected from the group consisting of stearic acid, oleic acid, azelaic acid, and suberic acid. By including one or more selected from the group consisting of stearic acid, oleic acid, azelaic acid, and suberic acid in the fatty acid, it is possible to promote pulverization of the raw nickel powder while suppressing an increase in production costs.
[0021] (6) In the method for producing nickel powder according to any one of (1) to (5) above, the particle size of the nickel powder after the wet grinding step may be 0.1 μm to 20 μm in terms of 50% cumulative volume measured by a laser scattering particle size distribution device. By setting the particle size of the nickel powder after the wet grinding step within the above range, it is possible to improve the antifungal effect of the obtained nickel powder while suppressing an increase in production costs.
[0022] (7) The method for producing nickel powder according to any one of (1) to (6) above may be a method for producing nickel powder to be used as an antifungal agent. The nickel powder produced by the method for producing nickel powder according to the present disclosure can be suitably used as an antifungal agent.
[0023] (8) A method for producing a paint according to another embodiment of the present disclosure includes a paint preparation step of adding nickel powder to a paint material, and the nickel powder used is nickel powder produced by the method for producing nickel powder described in any one of (1) to (6) above.
[0024] (9) A method for manufacturing a component according to another embodiment of the present disclosure includes a coating step of applying paint to a component to be coated, and uses paint manufactured by the paint manufacturing method described in (8) above as the paint.
[0025] (10) A method for producing a resin composition according to another embodiment of the present disclosure includes a resin preparation step of adding nickel powder to a resin, and the nickel powder used is nickel powder produced by the method for producing nickel powder described in any one of (1) to (6) above.
[0026] (11) A method for producing a resin molded product according to another embodiment of the present disclosure includes a molding step of molding a resin composition, and uses, as the resin composition, a resin composition produced by the method for producing a resin composition described in (10) above.
[0027] The coating material manufacturing method, component manufacturing method, resin composition manufacturing method, and resin molded product manufacturing method disclosed herein use nickel powder manufactured by the nickel powder manufacturing method described in any one of (1) to (6) above, and therefore enable simple and low-cost manufacturing and have excellent antifungal properties.
[0028] Here, the term "main component" refers to the component with the largest content in terms of mass, for example, a component with a content of 50 mass% or more. The "hydrogen element content" of the nickel powder refers to the amount measured by the inert gas fusion method.
[0029] [Details of the embodiment of the present disclosure] Hereinafter, a method for producing a nickel powder, a method for producing a paint, a method for producing a part, a method for producing a resin composition, and a method for producing a resin molded product according to an embodiment of the present disclosure will be described.
[0030] [Method of producing nickel powder] A method for producing nickel powder according to one embodiment of the present disclosure is a method for producing nickel powder containing nickel or a nickel alloy as a main component. As shown in FIG. 1, the method for producing nickel powder includes a wet-pulverizing step S1.
[0031] The nickel powder manufacturing method is particularly suitable for manufacturing nickel powder for use as an antifungal agent. The nickel powder manufactured by the nickel powder manufacturing method has a high antifungal effect.
[0032] <Wet grinding process> In the wet-pulverization step S1, the raw nickel powder is wet-pulverized using a solvent containing elemental hydrogen. In this nickel powder manufacturing method, the raw nickel powder is wet-pulverized to a desired particle size, and at the same time, elemental hydrogen can be added from the solvent containing elemental hydrogen to the raw nickel powder.
[0033] (Raw Nickel Powder) The raw material nickel powder contains nickel or a nickel alloy as a main component.
[0034] The raw nickel powder may contain a metal other than nickel. Also, the raw nickel powder may be a powder mainly composed of a nickel alloy as described above. Examples of metal elements other than nickel contained in the raw nickel powder include Fe, Co, and Zn.
[0035] The content of nickel element relative to the total mass of the raw nickel powder is determined so that the content of nickel element relative to the total mass of the nickel powder after the wet-pulverizing step S1 will be a desired value (described later).
[0036] The content of metal elements other than nickel in the raw nickel powder is preferably set within a range in which the content of nickel element relative to the total mass of the nickel powder after the wet grinding step S1 is within a preferred range. On the other hand, the raw nickel powder may contain substantially only nickel as a metal element. Note that "containing substantially only nickel as a metal element" means that the metal element is composed only of nickel and metal elements that are inevitably contained.
[0037] The raw nickel powder may contain phosphorus. By including phosphorus in the raw nickel powder, the phosphorus penetrates into the grain boundaries of the raw nickel powder, promoting the dissolution of nickel ions. This improves the mold prevention effect.
[0038] The content of phosphorus element relative to the total mass of the raw nickel powder is determined so that the content of phosphorus element relative to the total mass of the nickel powder after the wet-pulverizing step S1 will be a desired value (described later).
[0039] The raw nickel powder can be produced by, for example, a known melting process. Examples of the melting process include water atomizing, gas atomizing, and rotating electrode methods. When the raw nickel powder contains phosphorus, for example, a method can be used in which a predetermined amount of pure nickel and a Ni-P alloy are mixed and produced by water atomizing.
[0040] (solvent) The solvent is not particularly limited as long as it is a known solvent containing hydrogen element, and examples thereof include water, ethanol, etc. When water or ethanol is used as the solvent, it is considered that the hydrogen element generated by decomposition of the water or ethanol becomes in a state of solid solution in nickel or in a state of being adsorbed on the surface of nickel.
[0041] The solvent may contain a fatty acid having a carboxyl group. The fatty acid having a carboxyl group functions as a dispersant, improving the dispersibility of the raw nickel powder in the solvent and increasing the grindability. Therefore, by including a fatty acid having a carboxyl group in the solvent, the raw nickel powder can be quickly ground to a predetermined particle size.
[0042] The fatty acid may include one or more selected from the group consisting of stearic acid, oleic acid, azelaic acid, and suberic acid. By including one or more selected from the group consisting of stearic acid, oleic acid, azelaic acid, and suberic acid in the fatty acid, it is possible to promote pulverization of the raw nickel powder while suppressing an increase in production costs.
[0043] The upper limit of the content of the fatty acid relative to the total mass of the solvent is preferably 3% by mass, more preferably 2% by mass. If the content of the fatty acid exceeds the upper limit, there is a risk of insoluble residues remaining, which increases the manufacturing cost of the nickel powder manufacturing method. On the other hand, the lower limit of the content of the fatty acid is not particularly limited, and it is sufficient for the fatty acid to exceed 0% by mass in order to obtain the effect of facilitating pulverization by the fatty acid.
[0044] (Wet grinding) From the viewpoint of the particle size required for the nickel powder (described later), wet pulverization is used for pulverization. Wet pulverization can be performed using a bead mill, a disk mill, a jet mill, etc. Among them, from the viewpoint of the particle size required for the nickel powder, a bead mill is preferred.
[0045] (Nickel powder) The lower limit of the content of the hydrogen element relative to the total mass of the nickel powder after the wet grinding step S1 is 0.05 mass%, more preferably 0.07 mass%. On the other hand, the upper limit of the content of the hydrogen element is preferably 1.0 mass%, more preferably 0.8 mass%. If the content of the hydrogen element is less than the lower limit, the effect of preventing oxidation and deterioration of the nickel powder may be insufficient, and the antifungal effect may be reduced. On the other hand, if the content of the hydrogen element exceeds the upper limit, it may take time to grind the nickel powder to incorporate the hydrogen element, which may increase the production cost.
[0046] The lower limit of the content of the nickel element relative to the total mass of the nickel powder after the wet grinding step S1 is preferably 70 mass%, more preferably 80 mass%, and even more preferably 90 mass%, from the viewpoint of obtaining a desired antifungal effect. On the other hand, the upper limit of the content of the nickel element is not particularly limited, but can be, for example, 99 mass%.
[0047] When the raw nickel powder contains phosphorus, the lower limit of the content of the phosphorus element relative to the total mass of the nickel powder after the wet grinding step S1 is preferably 0.15 mass%, more preferably 0.20 mass%, and even more preferably 0.25 mass%. On the other hand, the upper limit of the content of the phosphorus element is preferably 15.70 mass%, more preferably 12.00 mass%, and even more preferably 10.00 mass%. If the content of the phosphorus element is less than the lower limit, the effect of promoting the dissolution of nickel ions by the phosphorus element may not be sufficiently obtained. Conversely, if the content of the phosphorus element exceeds the upper limit, the corrosion resistance of the resulting nickel powder may be too improved, thereby inhibiting the dissolution of nickel ions.
[0048] The lower limit of the particle size of the nickel powder after the wet grinding step S1 is preferably 0.1 μm, more preferably 0.2 μm, based on a 50% cumulative volume measured by a laser scattering particle size distribution device. On the other hand, the upper limit of the particle size of the nickel powder is preferably 20 μm, more preferably 15 μm. If the particle size of the nickel powder is less than the lower limit, it may take a long time to grind, and the production cost may increase. On the other hand, if the particle size of the nickel powder exceeds the upper limit, the specific surface area of the nickel powder may become small, and the antifungal effect may be reduced.
[0049] The lower limit of the specific surface area of the nickel powder after the wet grinding step S1 is 1 m 2 / g is preferred, and 2m 2 / g is more preferable, and 3m 2 On the other hand, the upper limit of the specific surface area is preferably 11 m 2 / g is preferred, and 10m 2 / g is more preferred, and 9m 2 / g is more preferable. If the specific surface area is less than the lower limit, the amount of nickel ions eluted may not be sufficient, and the antifungal effect may be reduced. Conversely, if the specific surface area exceeds the upper limit, the particles may aggregate to inhibit the elution of nickel ions, and the antifungal effect may be reduced. Here, the "specific surface area" refers to the specific surface area measured by a gas adsorption method, and refers to the amount calculated by analyzing the adsorption amount using N2 gas by the BET method. As specific conditions, the pretreatment conditions are vacuum degassing at 200°C for 3 hours, and the adsorption temperature is -196°C.
[0050] Here, as described above, the particle size of the nickel powder and the content of the hydrogen element relative to the total mass of the nickel powder both depend on the grinding time, and the hydrogen element content also depends on the hydrogen element content of the solvent and the form of hydrogen element in the solvent, so that both can be controlled independently.
[0051] <Advantages> In the method for producing nickel powder, the raw nickel powder is pulverized to a predetermined particle size, and hydrogen is added to the raw nickel powder from a solvent containing hydrogen element at the same time. Therefore, nickel powder can be produced simply and at low cost. In addition, the nickel powder is mainly composed of nickel or a nickel alloy, and nickel ions are eluted into adsorbed water that may be present in small amounts on the surface of the powder when in use. These nickel ions can come into contact with and kill bacteria and mold that may grow in the adsorbed water. Furthermore, since the content of hydrogen element relative to the total mass of the nickel powder is set to be equal to or higher than the lower limit, the hydrogen element easily forms hydrides that alter the proteins that constitute bacteria and mold, and the produced nickel powder exhibits excellent antifungal properties.
[0052] [Manufacturing method of paint and component] <Paint manufacturing method> A method for producing a paint according to another embodiment of the present disclosure includes a paint preparation step S2 of adding nickel powder to a paint material, as shown in Fig. 2. In the method for producing a paint, nickel powder produced by the method for producing nickel powder according to the present disclosure is used as the nickel powder.
[0053] The coating material may or may not contain a solvent, and the coating material or coating material may be in the form of a solvent-based, water-based, or powder.
[0054] The coating material usually contains a resin. The resin contained in the coating material is not particularly limited, and examples thereof include epoxy resin, urethane resin, acrylic resin, and silicone resin. That is, the coating material or the coating material may be any one of an epoxy-based coating material, a urethane-based coating material, an acrylic-based coating material, and a silicone-based coating material.
[0055] The content of the nickel powder in the paint is preferably 0.1% by mass or more and 10% by mass or less.
[0056] <Method of manufacturing components> A method for manufacturing a member according to another embodiment of the present disclosure includes a coating step S3 of coating a coating material on a coating target member, as shown in Fig. 2. In the method for manufacturing the member, a coating material manufactured by the coating material manufacturing method of the present disclosure is used as the coating material.
[0057] The above-mentioned coated member is not particularly limited, and may be various members that require antifungal properties. Examples of the coated member include outdoor equipment covers such as outdoor lighting covers and smart meter covers; components or housing equipment used around water such as kitchens, baths, and toilets; home appliances such as refrigerators and air conditioners; ATMs (automated teller machines) installed in convenience stores; POS terminals; portable terminals such as mobile phones, smartphones, and tablets; computing equipment such as personal computers; various packaging materials; wallpapers; various filters; switches; daily necessities and living materials; sanitary materials; clothing; various plastic parts related to vehicles, etc.
[0058] The coating material may be applied to the entire surface of the member to be coated, or may be applied to a part of the surface.
[0059] <Advantages> The paint manufacturing method and part manufacturing method disclosed herein use nickel powder produced by the nickel powder manufacturing method disclosed herein, which allows for simple and low-cost production and has excellent anti-fungal properties.
[0060] [Method for producing resin composition and resin molded product] <Method of producing resin composition> A method for producing a resin composition according to another embodiment of the present disclosure includes a resin preparation step S4 of adding nickel powder to a resin, as shown in Fig. 3. In the method for producing a resin composition, nickel powder produced by the method for producing nickel powder according to the present disclosure is used as the nickel powder.
[0061] The resin may be a thermoplastic resin or a thermosetting resin.
[0062] Examples of the thermoplastic resin include polyolefin resins such as polypropylene, polyethylene, ethylene-vinyl acetate copolymer (EVA), and ethylene-ethyl acrylate copolymers; polyacrylic resins such as polymethyl methacrylate; polystyrene resins such as polystyrene, styrene-acrylonitrile copolymer (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), methyl methacrylate-butadiene-styrene copolymer (MBS resin), and styrene-methyl methacrylate copolymer (MS resin); polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polycyclohexane dimethylene terephthalate, polybutylene adipate, and polyethylene adipate; polyamide resins such as nylon 66, nylon 69, nylon 612, nylon 6, nylon 11, nylon 12, nylon 46, nylon 6-66 copolymer, and nylon 6-12 copolymer; polycarbonate resins such as polycarbonate and polycarbonate-ABS resin alloy; polyacetal resins; and thermoplastic polyurethane resins.
[0063] Examples of the thermosetting resin include unsaturated polyester resins such as crosslinked copolymers of glycols, unsaturated polyesters derived from unsaturated and saturated dibasic acids, and other vinyl monomers; epoxy resins such as polyamines of epoxy resins such as bisphenol-type epoxy resins, novolac-type epoxy resins, and alicyclic epoxy resins, and resins cured with acid anhydrides; thermosetting polyurethane resins such as polyurethane foam; and highly water-absorbent resins such as partial hydrolysates of crosslinked polyacrylamide and crosslinked acrylic acid-acrylamide copolymers.
[0064] The content of the nickel powder in the resin composition is preferably 0.1% by mass or more and 10% by mass or less.
[0065] <Manufacturing method for resin molded products> A method for producing a resin molded product according to another embodiment of the present disclosure includes a molding step S5 of molding a resin composition, as shown in FIG. 3, and uses a resin composition produced by the method for producing a resin composition according to the present disclosure as the resin composition.
[0066] The resin molded product is not particularly limited, and may be, for example, a member exemplified as a member to be coated in the method for producing the member.
[0067] <Advantages> The resin manufacturing method and resin molded product manufacturing method disclosed herein use nickel powder manufactured by the nickel powder manufacturing method disclosed herein, and therefore enable simple and low-cost manufacturing, and have excellent antifungal properties.
[0068] [Other embodiments] The above-mentioned embodiment does not limit the configuration of the present invention. Therefore, the above-mentioned embodiment may omit, replace or add components of each part of the above-mentioned embodiment based on the description in this specification and common technical knowledge, and it should be understood that all of these are within the scope of the present invention.
[0069] The raw nickel powder and thus the nickel powder may contain compounds other than nickel or nickel alloys, hydrogen, and other unavoidably contained impurities. The raw nickel powder and the nickel powder may further contain, for example, nickel oxide. EXAMPLES
[0070] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.
[0071] <Production of nickel powder> [No.1~No.7] A specified amount of pure nickel and Ni-P alloy were mixed, high-frequency melted, and then water atomized to produce raw nickel powder of Ni-1 mass%P (H: 0.0016 mass%) with a particle size (D50) of approximately 10 μm.
[0072] Using this as the raw material, the wet milling process was carried out using a wet bead mill device "Labostar Mini LMZ015" manufactured by Ashizawa Finetech Co., Ltd., and pulverization was carried out under the conditions in Table 1 to obtain nickel powders No. 1 to No. 7.
[0073] In Table 1, "solid content concentration" is the mass ratio of raw nickel powder per unit weight of the slurry when it is fed into the wet bead mill. In addition, when stearic acid was added as a dispersant, the amount of stearic acid added was 2 parts by mass per 100 parts by mass of raw nickel powder.
[0074] [No.8] The raw nickel powder itself produced by the above-mentioned water atomization method was used as nickel powder No. 8.
[0075] [No.9] The raw nickel powder prepared by the water atomization method described above was subjected to a reduction heat treatment in a hydrogen atmosphere to obtain nickel powder No. 9. The reduction heat treatment was carried out at 300°C for 30 minutes in a mixed hydrogen gas atmosphere containing 10% by volume of nitrogen.
[0076] [Table 1]
[0077] In Table 1, "-" indicates that the element does not apply.
[0078] [evaluation] The nickel powders No. 1 to No. 9 were evaluated for particle size, hydrogen element content, phosphorus element content, and mold resistance. The evaluation conditions are as follows. The results are shown in Table 2.
[0079] (Particle size) The particle size (D50) was measured using a laser analysis / scattering type particle size distribution measuring device "MT3300EX" manufactured by Microtrackbell Co., Ltd. No.1 to No.7 are the particle sizes of the nickel powder in the slurry after the wet grinding process. No.8, which was not wet ground, is the particle size of the raw nickel powder. No.9 was not measured.
[0080] (hydrogen element content, phosphorus element content) The hydrogen content was measured by inert gas fusion method using nickel powder obtained by filtering and drying the slurry after the wet grinding process. The phosphorus content was measured by ICP atomic emission spectrometry after dissolving each sample powder in acid.
[0081] (Mold and mildew resistant) Antifungal properties were measured using a modified version of the "Minimum Inhibitory Concentration Measurement Method I (2018 Edition) Liquid Medium Dilution Method" of the Society of Antibacterial Products (SIAA). The test specimen was mixed with subdextrose liquid medium (SDB) so that the maximum concentration of nickel powder was 1000μg / mL, and a two-fold dilution series was prepared in total of 10 steps using SDB to create the test medium. The test bacteria solution was Cladosporium cladosporioides (NBRC6368) with a spore count of 10 7The concentration was adjusted to 100 / mL, inoculated into each test medium, and cultured at 25°C for 48 hours. The presence or absence of growth after culture was observed with the naked eye to determine the MIC. Specifically, the maximum powder concentration of the sample in which no growth was observed was calculated as the "antifungal index [ppm]." In other words, the lower the antifungal index value, the better the antifungal properties.
[0082] [Table 2]
[0083] In Table 2, "-" indicates that the measurement was not performed.
[0084] The results in Table 2 show that the nickel powder produced by the wet grinding process, which is the nickel powder production method of the present disclosure, has excellent antifungal properties. [Industrial Applicability]
[0085] The method for producing nickel powder of the present disclosure allows for simple and low-cost production, and the resulting nickel powder has excellent antifungal properties. In addition, the method for producing paint, the method for producing member, the method for producing resin composition, and the method for producing resin molded article of the present disclosure allow for simple and low-cost production, and the resulting paint, member, resin composition, and resin molded article have excellent antifungal properties.
Claims
1. A method for producing nickel powder containing nickel or a nickel alloy as a main component, comprising the steps of: The method includes a wet-pulverizing step of wet-pulverizing a raw nickel powder using a solvent containing hydrogen element, A method for producing nickel powder, in which the hydrogen element content relative to the total mass of the nickel powder after the wet grinding step is 0.05 mass% or more.
2. The method for producing nickel powder according to claim 1, wherein the raw nickel powder contains phosphorus element.
3. The method for producing nickel powder according to claim 2, wherein the content of phosphorus element relative to the total mass of the nickel powder after the wet grinding step is 0.15 mass% or more and 15.70 mass% or less.
4. The method for producing nickel powder according to any one of claims 1 to 3, wherein the solvent contains a fatty acid having a carboxyl group.
5. The method for producing nickel powder according to claim 4, wherein the fatty acid comprises one or more selected from the group consisting of stearic acid, oleic acid, azelaic acid, and suberic acid.
6. 3. The method for producing nickel powder according to claim 1, wherein the particle size of the nickel powder after the wet grinding step is 0.1 μm or more and 20 μm or less on a 50% volume cumulative basis measured by a laser scattering particle size distribution device.
7. The method for producing nickel powder according to any one of claims 1 to 3, which is a method for producing nickel powder to be used as a fungicide.
8. A paint preparation step of adding nickel powder to a paint material, A method for producing a paint, in which the nickel powder is produced by the method for producing nickel powder according to any one of claims 1 to 3.
9. A coating process is provided for coating a coating material on the coating member. A method for manufacturing a member, comprising the step of: using a paint manufactured by the method for manufacturing a paint according to claim 8 as the paint.
10. A resin preparation step of adding nickel powder to a resin is provided, A method for producing a resin composition, in which nickel powder produced by the method for producing nickel powder according to any one of claims 1 to 3 is used as the nickel powder.
11. A molding step of molding a resin composition is provided, A method for producing a resin molded product, comprising the step of: producing a resin composition according to claim 10 by the method for producing a resin composition;
Citation Information
Patent Citations
Hydrogen storage alloy and its production
JP1998251702A
Ni BASED POWDER HAVING EXCELLENT ANTIBACTERIAL AND MOLD PREVENTION PROPERTIES, PRODUCTION METHOD THEREFOR, AND MATERIAL RESIN AND MEMBER CONTAINING THE SAME Ni BASED POWDER AND HAVING EXCELLENT ANTIBACTERIAL AND ANTIFUNGAL PROPERTIES
JP2003064401A