Paper base material for humidification molding, paper processed article, and paper container

A paper base material with controlled thickness, Cobb water absorption, and fiber width enhances moldability and drop impact resistance, maintaining surface beauty in harsh conditions.

JP2024150170APending Publication Date: 2024-10-23OJI HLDG CORP

Patent Information

Application Number
JP2023063446
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing paper materials struggle to balance moldability and drop impact resistance, especially in humid environments, and maintain surface beauty under harsh conditions such as high temperature and high humidity with vibrations.

Method used

A paper base material with specific thickness, Cobb water absorption, fiber width, and tensile strength characteristics, comprising two or more paper layers, is developed to enhance moldability and drop impact resistance while maintaining surface beauty.

Benefits of technology

The paper base material achieves high moldability and drop impact resistance, and maintains surface beauty even in high-temperature, high-humidity environments with vibrations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150170000001
    Figure 2024150170000001
  • Figure 2024150170000002
    Figure 2024150170000002
Patent Text Reader

Abstract

To provide a paper base material for humidification molding which achieves moldability and drop impact resistance at a high level by humidification molding, and can maintain surface beauty even by becoming wet under a high temperature and high humidity environment and receiving vibration.SOLUTION: A paper base material for humidification molding has two or more paper layers, in which the thickness of the paper base material is 0.8 to 1.5 mm, when one surface of the paper base material is regarded as an A surface and the other surface thereof is regarded as a B surface, a Cobb water absorption degree measured from the A surface of the paper base material is equal to or less than a Cobb water absorption degree measured from the B surface, the Cobb water absorption degree measured from the A surface is 10 to 700 g / m2 60 sec, the Cobb water absorption degree measured from the B surface is 10 to 1000 g / m2 60 sec, and both an average fiber width of a pulp contained in a paper layer constituting the one surface of the paper base material and an average fiber width of a pulp contained in a paper layer constituting the other surface thereof are 28.0 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a paper substrate for moist forming, and a paper product and a paper container using the paper substrate. [Background technology]

[0002] In recent years, efforts to reduce the use of plastic have been accelerating worldwide due to environmental concerns. Traditionally, plastic materials such as synthetic resins have been widely used for containers such as trays and bottles, as well as tableware, stationery, and medical equipment, but the replacement of plastic products with paper products is progressing. Paper containers and the like require ease of folding for molding, i.e., moldability (flexibility), while strength after molding, such as drop impact resistance, is also required. However, there is a trade-off between the two as paper properties; for example, increasing the thickness of the base material improves drop impact resistance, but reduces moldability. Therefore, there is a demand for good paper that can achieve both moldability and drop impact resistance. On the other hand, as a method for forming a thick paper base material, for example, Patent Document 1 discloses a forming method that includes a step of humidifying the liner before applying pressure when bending cardboard, thereby preventing the occurrence of wrinkles and tears during processing. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2004 / 022327 Summary of the Invention [Problem to be solved by the invention]

[0004] However, according to the study by the present inventors, the technology of the above-mentioned documents is not sufficient in terms of both formability and drop impact resistance when more complicated processing is performed by humidification molding, such as for containers such as trays and bottles. Furthermore, containers such as trays and bottles are exposed to environments that make the surface easily moist, such as high temperature and humidity environments, during transportation and storage after molding, and may also be subjected to vibrations during transportation. A paper base material that can maintain the beauty of the surface even when exposed to such harsh environments has not yet been obtained. The present disclosure provides a paper substrate for humid forming that achieves high levels of formability and drop impact resistance through humid forming, and further that can maintain the beauty of its surface even when moistened in a high-temperature, high-humidity environment and subjected to vibration. [Means for solving the problem]

[0005] This disclosure relates to the following: <1> ~ <8> Regarding. <1> A paper substrate for moist forming, comprising: The paper base material has two or more paper layers, The thickness of the paper base material is 0.8 to 1.5 mm; When one surface of the paper base material is designated as side A and the other surface is designated as side B, The Cobb water absorbency measured from the A side of the paper base material is equal to or lower than the Cobb water absorbency measured from the B side, The Cobb water absorbency measured from the A side is 10 to 700 g / m 2 60 seconds, The Cobb water absorbency measured from the B side is 10 to 1000 g / m 2 60 seconds, The average fiber width of the pulp contained in the paper layer constituting one surface of the paper base material and the average fiber width of the pulp contained in the paper layer constituting the other surface of the paper base material are both 28.0 μm or less. A paper substrate for moist forming, comprising: <2> The paper base material is adjusted to a moisture content of 10% by mass, and the average value of the longitudinal tensile strength of the paper base material per basis weight and the transverse tensile strength of the paper base material per basis weight is 12.0 to 43.0 Nm / g. <1> The paper substrate for moist forming according to claim 1. <3> The paper base material is a multi-layer paper having two or more layers of the paper, or a laminated paper having two or more base papers attached thereto, Each of the two or more base papers includes the paper layer. <1> or <2> The paper substrate for moist forming according to claim 1. <4> The pulp contained in the paper layer contains hardwood kraft pulp and recycled paper pulp. <1> ~ <3> The paper substrate for moist forming according to any one of the preceding claims. <5> The difference between the Cobb absorbency measured from side B and the Cobb absorbency measured from side A (side B - side A) is 20 to 900 g / m 2 - 60 seconds, <1> ~ <4> The paper substrate for moist forming according to any one of the preceding claims. <6> <1> ~ <5> A paper product obtained by using the paper base material for moist forming described in any one of the above items. <7> <1> ~ <5> 2. A paper container comprising the paper base material for humid forming according to claim 1. <8> The paper container has a bottle shape, The A side constitutes at least a part of the outer surface of the paper container. <7> A paper container as described in claim 1. Effect of the Invention

[0006] According to the present disclosure, it is possible to provide a humidified forming paper base material that achieves higher levels of formability and drop impact resistance, and further, is capable of maintaining the beauty of its surface even when moistened in a high-temperature, high-humidity environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] In this specification, the description of "X or more and Y or less" or "X to Y" representing a numerical range means a numerical range including the lower and upper limits which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.

[0008] The machine direction is the machine direction (MD) of the paper base material, which is the same as the direction in which the fibers are oriented, and the cross direction is the direction perpendicular to the machine direction (CD).

[0009] The inventors have discovered that by using a paper base material that includes two or more paper layers and controlling the thickness of the paper base material, the Cobb water absorbency of both surfaces of the paper base material, and the average fiber width of the pulp that constitutes both surfaces of the paper base material all within specific ranges, it is possible to obtain a paper base material for humid molding that can achieve a high level of formability through humid molding (hereinafter also simply referred to as "formability during humid molding") and drop impact resistance, and that can maintain the beauty of its surface even when it is moistened in a high-temperature, high-humidity environment and subjected to vibration (hereinafter also simply referred to as "beauty after wetting").

[0010] By setting the thickness of the paper base material within a specific range, the strength of the paper base material is improved, thereby controlling the drop impact resistance and the moldability during humidification. In addition, when one surface of the paper base material is surface A and the other surface is surface B, the Cobb water absorbency measured from surface A is equal to or lower than the Cobb water absorbency measured from surface B. The Cobb water absorbency measured from surface A and the Cobb water absorbency measured from surface B are set within a specific range. The relationship between these Cobb water absorbencies makes it possible to achieve moldability during humidification and beauty after wetting. Furthermore, the average fiber width of each of the pulps constituting both surfaces of the paper base material is set within a specific range. This makes it possible to control the swelling of the fibers during humidification and achieve beauty after wetting and moldability during humidification.

[0011] Therefore, the thickness of the paper base, the Cobb water absorption of both surfaces of the paper base, and the The inventors believe that by controlling the average fiber width of the pulp that constitutes the surface within a specific range, it is possible to obtain a paper base material for humid forming that is excellent in all respects: formability during humid forming, drop impact resistance, and aesthetics after wetting.

[0012] The paper substrate for moist forming according to the present disclosure will be described below. The paper base material has two or more paper layers. Specifically, the paper base material is preferably a multilayer paper having two or more paper layers or a slip sheet in which two or more base papers are pasted together. When the paper base material is a slip sheet, each of the two or more base papers includes a paper layer. Each of the base papers constituting the slip sheet may be a single-layer paper or a multilayer paper. When the paper base material has two or more paper layers, it becomes easier to arbitrarily adjust the raw material composition, basis weight, and papermaking conditions of each layer and each base paper. The number of paper layers in the paper base material is preferably 2 to 9 layers, more preferably 2 to 4 layers, even more preferably 2 or 3 layers, and even more preferably 2 layers.

[0013] When the paper base material is a multi-layer paper having two or more paper layers, the paper base material is a base paper having a multi-layer structure obtained by multi-layer papermaking, which will be described later. The upper limit of the number of base paper layers constituting the multi-layer paper is not particularly limited, but is usually 9 layers or less. The paper base material is preferably a multi-layer paper having two layers.

[0014] When the paper base material is a slip sheet in which two or more base papers are pasted together, the slip sheet further includes an adhesive layer between the two or more base papers. For example, the slip sheet may be made of only base paper A, an adhesive layer, and base paper B, or may be made by laminating another base paper C via an adhesive layer. There is no particular limit to the upper limit of the number of base papers constituting the slip sheet, but it is usually three or less. The paper base material is preferably a slip sheet in which two base papers are pasted together. When the paper base material is an interleaving paper, the base paper contained in the interleaving paper may be a single-layer paper obtained by the single-layer papermaking process described later, or a multi-layer paper obtained by the multi-layer papermaking process described later, within the scope of not impairing the effects of the present disclosure. For two or more base papers, a single-layer paper and a multi-layer paper may be used in combination.

[0015] The thickness of the paper substrate for humid forming is 0.8 to 1.5 mm. If the thickness is 0.8 mm or more, the drop impact resistance is good. On the other hand, if the thickness is 1.5 mm or less, the moldability during humid forming is good. The thickness in the above range is a relatively thick range for a paper substrate for forming, and in the present disclosure, a paper substrate of such thickness achieves high levels of moldability and drop impact resistance, and further has a beautiful surface. The thickness of the paper substrate for humid forming is preferably 0.9 to 1.5 mm, more preferably 1.0 to 1.4 mm. In addition, when the paper base material is a laminate consisting of two or more base papers attached, the thickness of the paper base material refers to the total thickness of the paper base material including the thickness of the adhesive layer between the two or more base papers.

[0016] Furthermore, when one surface of the paper base material is designated as side A and the other surface is designated as side B, it is necessary that the Cobb water absorbency measured from side A of the paper base material is equal to or lower than the Cobb water absorbency measured from side B. It is preferable that the Cobb water absorbency measured from side A of the paper base material is lower than the Cobb water absorbency measured from side B. And, it is preferable that the Cobb water absorbency measured from side A is 10 to 700 g / m 2 60 seconds, and the Cobb water absorbency measured from side B is 10 to 1000 g / m 2 60 seconds. If the Cobb absorbency measured from side A of the paper base material is the same as the Cobb absorbency measured from side B, either side may be regarded as side A.

[0017] Side B can be the surface to which water vapor is applied during humidification and molding of the paper substrate. When the Cobb water absorbency measured from side B is within the above range, the moisture absorbency is good, and it is easy to improve the moldability during humidification and molding. Side A can also be a surface that can form at least a part of the outer surface of a paper product made using a paper substrate. When the Cobb water absorbency measured from side A is within the above range, the water resistance of the outer surface of a paper product made using a paper substrate is improved, and it is easy to improve the beauty after wetting. In addition, when a label or the like is printed on side A and used as the outer surface, it can maintain its beauty even during humidification and can also contribute to improving the design.

[0018] Cobb water absorption measured from side A is 10g / m 2 If the time is 60 seconds or more, the moldability during humid molding is easily improved. The Cobb water absorbency measured from the A side is 700g / m 2 If it is less than 60 seconds, it is easier to improve the beauty after wetting. The Cobb water absorbency measured from the A side is 10 to 500 g / m 2 60 seconds is preferable, and 10 to 200 g / m 2 60 seconds is more preferable, and 12 to 50 g / m 2 60 seconds is even better.

[0019] On the other hand, the Cobb absorbency measured from side B is 10 g / m 2 If the time is 60 seconds or more, the moldability during humidification molding is easily improved. The Cobb water absorbency measured from the B side is 1000g / m 2 When the time is 60 seconds or less, excessive swelling during humidification molding can be suppressed, and moldability during humidification molding can be improved. The Cobb water absorbency measured from the B side is 11 to 1000 g / m 2 60 seconds is preferable, and 90 to 900 g / m 2 60 seconds is more preferable, and 300 to 900 g / m 2 60 seconds is more preferable, and 600 to 800 g / m 2 60 seconds is even more preferable.

[0020] The difference between the Cobb absorbency measured from side B and the Cobb absorbency measured from side A (side B - side A) is 20 to 900 g / m 2 60 seconds is preferable, and 300 to 800 g / m 2 60 seconds is more preferable, and 500 to 750 g / m 2 When the time is within the above range, it is easy to further improve the moldability during humid molding and the aesthetic appearance after humidification.

[0021] Cobb water absorbency can be controlled by the amount of sizing agent added, etc. In order to reduce the Cobb water absorbency, methods such as increasing the amount of sizing agent added can be exemplified. In addition, in order to make the Cobb water absorbency measured from side A of the paper substrate smaller than the Cobb water absorbency measured from side B, methods such as increasing the amount of sizing agent added in the paper layer constituting the side A side compared to the paper layer constituting the side B side, or applying an overprint varnish (OP varnish) to the side A side of the paper substrate can be exemplified.

[0022] The average fiber width of the pulp contained in the paper layer constituting one surface of the paper base material and the average fiber width of the pulp contained in the paper layer constituting the other surface are both 28.0 μm or less. If the average fiber width of the pulp contained in the paper layer constituting at least one surface of the paper base material exceeds the above upper limit, the fibers tend to swell during moistening and molding, and the beauty after moistening and the moldability during moistening and molding are reduced. In particular, the beauty after moistening is likely to decrease on the A-side, and the moldability during moistening and molding is likely to decrease on the B-side. In measuring the average fiber width of the pulp, the paper layer constituting one surface and the paper layer constituting the other surface are separated and measured. The specific method will be described later.

[0023] The average fiber width of the pulp on both the one surface and the other surface is preferably 27.0 μm or less, more preferably 26.0 μm or less, and even more preferably 21.0 μm or less. There is no particular lower limit, but it is preferably 12.0 μm or more, and more preferably 15.0 μm or more. For example, the average fiber width of the pulp on both the one surface and the other surface is preferably 12.0 μm to 27.0 μm, more preferably 12.0 μm to 26.0 μm on both, and even more preferably 15.0 μm to 21.0 μm on both. It is also a preferred embodiment that the average fiber width of the pulp constituting the paper base material is within the above range. The average fiber width of the pulp can be controlled by the mass ratio of softwood kraft pulp among the pulps constituting the paper base material. In order to reduce the average fiber width of the pulp, a method such as reducing the mass ratio of softwood kraft pulp constituting the paper base material can be used.

[0024] The length-weighted average fiber length of the pulp contained in the paper layer constituting one surface of the paper base material and the length-weighted average fiber length of the pulp contained in the paper layer constituting the other surface are both preferably 0.5 to 2.5 mm, more preferably 0.6 to 2.4 mm, and even more preferably 0.6 to 1.2 mm. It is also a preferred embodiment that the length-weighted average fiber length of the pulp constituting the paper base material is within the above range.

[0025] When both the length-weighted average fiber length of the pulp contained in the paper layer constituting one surface of the paper base material and the length-weighted average fiber length of the pulp contained in the paper layer constituting the other surface are below the above-mentioned upper limit, the fibers are less likely to swell during moist forming, which makes it possible to further improve the aesthetics after moistening on the aforementioned side A, and makes it easier to further improve the formability during moist forming on the aforementioned side B. The length-weighted average fiber length of the pulp can be controlled by the mass ratio of softwood kraft pulp among the pulps constituting the paper base material. In order to reduce the length-weighted average fiber length of the pulp, a method such as reducing the mass ratio of softwood kraft pulp constituting the paper base material can be used.

[0026] The tensile strength of the paper base material per basis weight is also referred to as the specific tensile strength. The average value of the longitudinal tensile strength of the paper base material per basis weight and the transverse tensile strength of the paper base material per basis weight (hereinafter simply referred to as the "specific tensile strength when humidified") measured under a humidity controlled environment specified in JIS P 8111:1998 after adjusting the moisture content of the paper base material to 10% by mass is preferably 12.0 to 43.0 Nm / g. The specific tensile strength of the paper base material when humidified is more preferably 14.0 to 38.0 Nm / g, even more preferably 16.0 to 35.0 Nm / g, and even more preferably 20.0 to 30.0 Nm / g. By setting the specific tensile strength when humidified within the above range, the moldability during humidification molding can be further improved.

[0027] The longitudinal tensile strength ratio is preferably 15.0 to 50.0 Nm / g, more preferably 17.0 to 40.0 Nm / g, and even more preferably 27.0 to 35.0 Nm / g. The transverse tensile strength ratio is preferably 9.5 to 32.0 Nm / g, more preferably 13.0 to 27.0 Nm / g, and even more preferably 16.0 to 24.0 Nm / g. It is also preferable that both the longitudinal tensile strength ratio and the transverse tensile strength ratio of the paper base material when moistened satisfy the above range. By setting the longitudinal tensile strength ratio and the transverse tensile strength ratio when moistened within the above range, the moldability during moistening molding can be further improved. The tensile strength index when humidified can be controlled by the amount of paper strength enhancer added, etc. To increase the tensile strength index when humidified, a method such as increasing the amount of paper strength enhancer added can be used.

[0028] The fiber orientation ratio of the paper base material is preferably 1.40 to 2.50. The fiber orientation ratio indicates the tendency of the fibers to align in the flow direction (longitudinal direction) during the process in which the pulp slurry is discharged onto the wire of a papermaking machine, dewatered, and the paper layer is formed. In other words, the fiber orientation ratio indicates the degree of fiber orientation, and is a value of 1 or more. A low fiber orientation ratio indicates that the fibers are randomly oriented, and a high fiber orientation ratio indicates that the fibers are oriented in the longitudinal direction. By having a fiber orientation ratio equal to or greater than the lower limit, the stiffness in the lateral direction of the paper base material can be appropriately controlled, and the paper base material is more likely to curl in the lateral direction during molding, and cracks and deformations can be suppressed, which makes it easier to improve the moldability during humid molding. By having a fiber orientation ratio equal to or less than the upper limit, the stiffness in the longitudinal direction of the paper base material can be appropriately controlled, and wrinkles in the longitudinal direction can be suppressed, which improves the aesthetics after wetting.

[0029] The fiber orientation ratio of the paper base material is more preferably 1.45 to 2.30, and even more preferably 1.50 to 2.10. The fiber orientation ratio can be controlled by adjusting the ratio between the discharge speed of the pulp-containing paper stock and the wire speed of the papermaking machine in the paper layer or base paper making process. This ratio is also called the J / W ratio (jet / wire ratio). Methods for increasing the fiber orientation ratio include increasing the J / W ratio.

[0030] The paper base material has a basis weight of 500 to 1400 g / m 2 It is preferable that the thickness is 600 to 1300 g / m 2 More preferably, the thickness is 700 to 1220 g / m 2 It is more preferable that the basis weight of the paper base material is the total basis weight of the paper base material, including the weight of the adhesive layer between the two or more base papers, when the paper base material is an interleaving paper in which two or more base papers are adhered together. By having the entire basis weight of the paper base material within the above range, it becomes easier to adjust the thickness of the paper base material, and it becomes easier to further improve drop impact resistance and moldability during humid molding.

[0031] The basis weight of the paper layer that constitutes the A side (basis weight of the A side) is 250 to 700 g / m 2 It is preferable that the thickness is 300 to 650 g / m 2 More preferably, it is 350 to 600 g / m 2 By being in the above range, it is easy to satisfy the desired Cobb water absorbency, and the aesthetic appearance after wetting can be further improved.

[0032] The basis weight of the paper layer on the side that constitutes the B side (basis weight of the B side) is 250 to 700 g / m 2 It is preferable that the thickness is 300 to 650 g / m 2 More preferably, it is 350 to 600 g / m 2 When the content is in the above range, the paper base material is easily swollen and the moldability during moist molding can be further improved.

[0033] The ratio of the basis weight of the paper layer constituting the A side to the basis weight of the paper layer constituting the B side (A side / B side) is preferably 0.5 to 2.0, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1. By being in the above range, it is easier to achieve moldability during moist molding, drop impact resistance, and aesthetic appearance after wetting.

[0034] The paper layer is not particularly limited as long as it is a commonly used paper, and is preferably a paper containing plant-derived pulp as a main component, and more preferably a paper containing wood pulp as a main component. The raw material pulp contained in the paper layer is preferably wood pulp, and more preferably kraft pulp. The kraft pulp includes hardwood kraft pulp (LKP) and softwood kraft pulp (NKP) based on the difference in raw material. The kraft pulp includes bleached kraft pulp (BKP), unbleached kraft pulp (UKP) and oxygen bleached kraft pulp (OKP) based on the difference in processing state, and bleached kraft pulp (BKP) is preferred from the viewpoint of printability. Waste paper pulp may also be used.

[0035] Among these, the raw material pulp is preferably at least one selected from the group consisting of hardwood kraft pulp (LKP), softwood kraft pulp (NKP), and recycled paper pulp. It is more preferable to use hardwood kraft pulp (LKP) and recycled paper pulp in combination, or to use softwood kraft pulp (NKP) and hardwood kraft pulp (LKP) in combination. It is even more preferable that the pulp contained in the paper layer contains hardwood kraft pulp (LKP) and recycled paper pulp.

[0036] When hardwood kraft pulp (LKP) and recycled paper pulp are used in combination, the mass ratio (LKP / recycled paper pulp) is not particularly limited as long as it is a ratio used in general paper, but is preferably 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20, even more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. The mass ratio (NKP / LKP) of softwood kraft pulp (NKP) and hardwood kraft pulp (LKP) used in combination is not particularly limited as long as it is a ratio used in general paper, but is preferably 20 / 80 to 80 / 20, more preferably 40 / 60 to 80 / 20, and more preferably 50 / 60 to 80 / 20. / 50~70 / 30 is even more preferable.

[0037] Moreover, as the hardwood kraft pulp (LKP), hardwood bleached kraft pulp (LBKP) is preferable, and as the softwood kraft pulp (NKP), softwood bleached kraft pulp (NBKP) is preferable.

[0038] For hardwood kraft pulp (LKP), wood chips of known hardwoods such as eucalyptus, tanoak, acacia, etc. can be used, while for softwood kraft pulp (NKP), wood chips of known softwoods such as larch, spruce, cedar, slash pine, lodgepole pine, etc. can be used.

[0039] The Canadian Standard Freeness (CSF) of the pulp is not particularly limited, but is preferably 350 to 700 ml, and more preferably 400 to 500 ml. The CSF is the freeness value measured using a Canadian standard freeness tester in accordance with JIS-P8121 after disintegrating a sample using a standard disintegrator in accordance with JIS-P8220.

[0040] When preparing the paper layer or base paper, internal additives may be added, such as sizing agents, fillers, paper strength agents, retention aids, pH adjusters, drainage improvers, water resistance agents, softeners, antistatic agents, defoamers, slime control agents, dyes and pigments, etc.

[0041] From the viewpoint of easily controlling the Cobb water absorbency of the paper base material, it is preferable that the paper base material contains a sizing agent. The sizing agent is not particularly limited and a known one can be used. Examples of the sizing agent include rosin-based sizing agents, alkyl ketene dimers, alkenyl succinic anhydrides, and styrene-containing polymers such as styrene-(meth)acrylate copolymers. The sizing agent is preferably a rosin-based sizing agent. The content of the rosin-based sizing agent may be such that the desired Cobb water absorbency is obtained. For example, the content is preferably 0.05 to 2.00 parts by mass per 100 parts by mass of pulp. The content of the sizing agent in the paper layer can be measured by mass spectrometry using pyrolysis GC / MS.

[0042] From the viewpoint of making it easier to control the tensile strength index of the paper base material when moistened, it is preferable that the paper layer contains a paper strength agent. Paper strength enhancers include dry strength enhancers and wet strength enhancers, and examples of the dry strength enhancers include cationic starch, polyacrylamide, carboxymethyl cellulose, etc., and examples of the wet strength enhancers include polyamide polyamine epichlorohydrin, urea formaldehyde resin, melamine formaldehyde resin, etc. The paper base material preferably contains a dry strength enhancer, and a polyacrylamide-based dry strength enhancer is more preferred.

[0043] The content of the paper strength agent in the paper layer constituting the aforementioned side A is preferably 0.01 to 0.8 mass %. In the paper layer constituting the aforementioned side B, the content is preferably 0.001 to 0.3 mass %. The content of the paper strength agent in the paper layer can be measured by mass spectrometry using pyrolysis GC / MS.

[0044] In preparing the paper layer or base paper, the strength agent is preferably added in an amount of 0.09 to 0.42 parts (solid content equivalent) per 100 parts (solid content equivalent), more preferably 0.11 to 0.37 parts (solid content equivalent), and even more preferably 0.13 to 0.33 parts (solid content equivalent) to 100 parts (solid content equivalent) of the pulp slurry. By being in the above range, the specific tensile strength of the paper base material when moistened can be easily controlled.

[0045] In the papermaking of the paper layer or base paper, a known wet papermaking machine can be appropriately selected and used. Examples of the paper machine include a Fourdrinier paper machine, a gap former type paper machine, a cylinder paper machine, and a short wire paper machine.

[0046] In the papermaking of a paper layer or base paper, for example, a paper stock is cast onto a wire or the like, dehydrated to obtain a wet paper, and multiple wet papers are stacked as necessary, and this single-layer or multi-layer wet paper is pressed and dried. In this case, if multiple wet papers are not stacked, a single-layer base paper is obtained, and if multiple wet papers are stacked, a multi-layer base paper is obtained. When a multi-layer base paper is obtained, starch, polyacrylamide, etc. that strengthens interlayer adhesion may be applied between the layers during the papermaking process, and the layers may be stacked together.

[0047] When starch is applied, the amount of starch (e.g., the amount of starch applied after drying) is 0.1 to 5.0 g / m 2 It is preferable that the thickness is 0.5 to 2.0 g / m 2 It is more preferable that: The paper layer or base paper formed by the papermaking machine is preferably transported on a felt and dried in a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying in the dryer.

[0048] The paper layer or base paper obtained as described above may be surface-treated with a calendar to make the thickness and profile uniform. A known calendaring machine can be appropriately selected and used for the calendaring.

[0049] The Oken smoothness (JIS P 8155:2010) of the paper layer or base paper is not particularly limited, but is preferably 5 seconds or more, more preferably 10 to 1000 seconds. The 75° gloss of the paper layer or base paper is also not particularly limited, but is preferably 5% or more, more preferably 10 to 70%.

[0050] When the paper substrate is a laminate of two or more base papers, it further includes an adhesive layer between the two or more base papers. That is, when the paper substrate is a laminate, the base papers are laminated via an adhesive layer. The adhesive layer may be any layer made of a material having adhesive properties. The adhesive layer is preferably a resin-based adhesive suitable for dry lamination and wet lamination. An adhesive suitable for wet lamination is more preferable.

[0051] The adhesive layer may be formed by laminating the base paper and the base paper using an adhesive. The adhesive is not particularly limited, but water-based, solvent-based, UV-based, and other types can be used, and among them, water-based adhesives are preferred. That is, the adhesive layer is preferably a water-based adhesive layer formed by a water-based adhesive. Among the water-based adhesives, at least one selected from the group consisting of acrylic adhesives, polyurethane adhesives, epoxy adhesives, and isocyanate adhesives is preferred, and acrylic adhesives are more preferred from the viewpoints of easy control of adhesive strength and heat resistance.

[0052] When an adhesive is used, the amount of adhesive layer per unit area (e.g., coating amount after drying) is 1 to 50 g / m 2 and more preferably 3 to 10 g / m 2 It is preferable to coat the base paper so that the solid content is within this range.

[0053] For coating, it is preferable to use a coating liquid containing an adhesive, and it is more preferable to use a mixed coating liquid in which a curing agent is mixed into a coating liquid containing an adhesive. For example, the adhesive layer is preferably a cured product of a water-based adhesive.

[0054] The adhesive layer may be a layer containing a thermoplastic resin. By using a thermoplastic resin, it is possible to easily obtain an interleaving paper as a laminate by coating the base paper with the resin that has been heated and melted, and then laminating another base paper. The thermoplastic resin used in the thermoplastic resin layer is not particularly limited, and may be appropriately selected from known thermoplastic resins.

[0055] The method for producing the interleaf paper is not particularly limited, and any known method can be used. An example of the production method is shown below. First, base paper A including paper layer A capable of forming side A and base paper B including paper layer B capable of forming side B are prepared, and an adhesive that will become the adhesive layer is coated on one side of base paper A, and base paper B is wet laminated to this coated surface to obtain an interleaving paper.

[0056] As described above, the interleaf paper contains two or more base papers (for example, base paper A and base paper B), but it may contain three or more base papers. When the interleaf paper contains three or more base papers, the adhesive layers that bond the base papers together may be different from each other or may be the same.

[0057] The obtained paper base material may be cut to an appropriate size taking into consideration the size and shape of the stored items, and suitability for transportation and display. Cutting is preferably performed by punching in order to efficiently obtain interleaf sheets of the same shape. The punching process is preferably carried out using a high-speed automatic punching machine, a flat-bed punching machine, or a rotary punching machine, and more preferably a high-speed automatic punching machine. The high-speed automatic punching machine and the flat-bed punching machine can easily and efficiently obtain paper base materials in shapes such as a rectangle, a rounded rectangle, an ellipse, etc.

[0058] The use of the paper substrate is not particularly limited as long as it is for humidification molding, and it may be used as a paper processed product by humidification molding and further processing as appropriate. Examples of the paper processed products include paper containers such as paper bottles, paper cups, and paper trays, clothing hanging tools such as paper hangers and paper hanger hooks, and paper tableware such as paper plates, paper spoons, paper forks, paper knives, paper stirrers, and paper straws. The paper substrate is preferably used as a paper container, more preferably as a bottle-shaped paper container, and the above-mentioned side A preferably constitutes at least a part of the outer surface of the paper container.

[0059] Moisture forming includes known methods of humidifying and forming, for example, a paper substrate is moistened and then processed into a desired shape by press forming, folding forming, or the like. The method for humidifying the paper base material is not particularly limited, but includes a method of blowing water vapor onto one surface of the paper base material, etc. From the viewpoint of processability, it is preferable to blow water vapor onto the B side of the paper base material. The moisture content of the paper base material when the water vapor is sprayed is preferably 5 to 30% by mass, more preferably 5 to 25% by mass, and even more preferably 8 to 15% by mass.

[0060] The measurement methods for each physical property are described below. <Thickness of paper base material> The thickness of the paper base material (paper thickness) is measured in accordance with JIS P 8118:2014 after humidity control under the humidity control environment specified in JIS P 8111:1998. A paper thickness meter (company name: Toyo Seiki Seisakusho Co., Ltd., model number: No. 132 digital thickness measuring instrument) can be used as the measuring device. 10 samples are measured, and the arithmetic average value is used.

[0061] <Cobb Water Absorbency> The Cobb water absorbency is measured in accordance with JISP8140:1998 after conditioning in a humidity-controlled environment as specified in JIS P 8111:1998. The temperature of the water (distilled water is used) that is brought into contact is 23°C, and the contact time is 60 seconds. The Cobb water absorbency is measured on one surface and the other surface of the paper base material. The measuring device is a Cobb sizing tester manufactured by Japan TMC Co., Ltd. Ten samples are measured and the arithmetic average value is used.

[0062] <Length-weighted average fiber length and average fiber width of redisintegrated pulp> After soaking the paper substrate in 80°C water for one hour, separate the paper layer that makes up side A from the paper layer that makes up side B. Specifically, carefully separate the paper layers by hand while checking each layer. If the paper layers are difficult to peel off, repeat the process of soaking in 80°C water. If the paper substrate is an interleaf paper and adhesive is attached to the paper layer being measured, use a knife or cutter to remove as much of the adhesive as possible. The separated paper layer is cut into 40 cm squares, soaked in ion-exchanged water adjusted to a concentration of 2%, and left to soak for 24 hours. After soaking for 24 hours, the pulp is disintegrated into fibers by processing using a standard disintegrator (manufactured by Kumagai Riki Kogyo Co., Ltd.) in accordance with JISP8220-2:2012 until no undisintegrated fibers remain. The slurry after disintegration (dispersion of pulp fibers) is adjusted to a solids concentration of 0.1% by mass, and the pulp solids concentration is calculated in accordance with JIS P8225:2003. The slurry after disintegration is adjusted to a solids concentration of 0.004% by mass, and 500 g of slurry is obtained, and the amount taken is recorded. The solids concentration and the amount of slurry taken are used to calculate the dry weight of the sample. The obtained slurry is used to measure the "length-weighted average fiber length" and "fiber width" using a fiber length measuring instrument (Valmet FS-5 with UHD base unit, manufactured by Valmet Co., Ltd.) in accordance with ISO 16065-2:2007. The device can also detect and measure each fiber using an attached camera, which captures images within a measurement cell with a depth of field of 0.5 mm in accordance with the ISO16505-2:2007 standard. The device captures fiber lengths between 0.01 mm and 10.00 mm. Fibers between 0.2 mm and 7.0 mm are selected for the measurement of "fiber length" and "fiber width." The average fiber width is the arithmetic mean value of the fiber widths of all fibers obtained.

[0063] <Specific tensile strength when humid> The tensile strength of the paper substrate is measured using a load cell type tensile tester (company name: A&D Co., Ltd., model number: RTG-1310) with the distance between the two grips set to 100 mm and the pulling speed set to 5 mm / min. The measurement environment is a humidity controlled environment specified in JIS P 8111:1998. The test pieces were cut to a width of 15 mm and a length of 140 mm, and placed in a constant temperature and humidity chamber set to a temperature of 50° C. and a relative humidity of 65% so that the moisture content was adjusted to 10% by mass. The moisture content was calculated using the following formula. Moisture content (mass%) = {(mass of test piece (after hydration) - bone dry mass of test piece) / mass of test piece (after hydration)} x 100 If the moisture content is not 10% by mass, adjust the relative humidity setting of the temperature and humidity chamber, place the specimen in the temperature and humidity chamber again, and repeat the adjustment until the moisture content reaches 10% by mass. The bone dry mass is the mass of the specimen placed in a dryer at 105°C for 1 hour and then cooled to room temperature, and is measured in advance. The specimen adjusted to a moisture content of 10% by mass is stored in an aluminum pouch until immediately before measurement. The specific tensile strength is calculated by dividing the obtained tensile strength by the basis weight measured in accordance with JIS P 8124: 2011. The specific tensile strength in the machine direction and the specific tensile strength in the cross direction are measured at 10 points each, and the arithmetic average value of these is used.

[0064] <Fiber orientation ratio> The fiber orientation ratio of the paper substrate is measured by measuring the ultrasonic propagation velocity in the longitudinal direction (Vmd) and the ultrasonic propagation velocity in the transverse direction (Vcd) of the paper substrate using a SONIC SHEET TESTER (SST) manufactured by Nomura Shoji Co., Ltd. The ratio (Vmd / Vcd) is taken as the fiber orientation ratio. Ten samples are measured, and the arithmetic average value is used. EXAMPLES

[0065] The present invention will be specifically described below using examples, but the scope of the invention is not limited to the description of the examples. In addition, unless otherwise specified, "parts" means "parts by mass."

[0066] (Example 1-1) (Paper base material) A multi-layer paper base material having two paper layers (paper layer A and paper layer B) was manufactured by the following procedure. As the pulp raw material for paper layer A, LBKP (acacia pulp and eucalyptus pulp manufactured by Oji Paper Co., Ltd.) and waste paper pulp (waste magazine paper and waste newspaper paper) were mixed in a mass ratio of 50:50 and beaten using a double disc refiner to obtain a pulp slurry. The beating conditions were adjusted in terms of pulp concentration, processing amount, and beating power so that the freeness of the pulp slurry was 400 to 450 ml. To 100 parts (solids content) of the obtained pulp slurry, 1.20 parts (solids content) of aluminum sulfate (liquid aluminum sulfate manufactured by Asahi Chemical Industry Co., Ltd.) was added, 0.20 parts (solids content) of a polyacrylamide-based dry strength agent (PS373-20 manufactured by Arakawa Chemical Industry Co., Ltd.) was added as an internal paper strength enhancer, and 1.00 parts (solids content) of a rosin-based sizing agent (Size Pine N811M manufactured by Arakawa Chemical Industry Co., Ltd.) was added as an internal sizing agent, to prepare the paper material for paper layer A.

[0067] As the pulp raw material for paper layer B, LBKP (acacia pulp and eucalyptus pulp manufactured by Oji Paper Co., Ltd.) and waste paper pulp (waste magazine paper and waste newspaper paper) were mixed in a mass ratio of 50:50 and beaten using a double disc refiner to obtain a pulp slurry. The beating conditions were adjusted so that the freeness of the pulp slurry was 400 to 450 ml, with the pulp concentration, processing amount, and beating power being adjusted. To 100 parts (solids content) of the obtained pulp slurry, 0.30 parts (solids content) of aluminum sulfate (liquid aluminum sulfate manufactured by Asahi Chemical Industry Co., Ltd.), 0.20 parts (solids content) of a polyacrylamide-based dry strength agent (PS373-20 manufactured by Arakawa Chemical Industry Co., Ltd.), and 0.10 parts (solids content) of a rosin-based sizing agent (Sizepine N811M manufactured by Arakawa Chemical Industry Co., Ltd.) were added, and the paper material for paper layer B was adjusted.

[0068] The paper materials of paper layers A and B are each 560g / m 2 The paper was made using a fourdrinier paper machine, adjusting the J / W ratio so that the fiber orientation ratio was 1.62, and starch was sprayed between the layers A and B at 1.0 g / m 2By applying and combining, the basis weight is 1121g / m 2 Thus, a paper substrate of 100 g was obtained.

[0069] (Example 1-2) The paper materials of paper layers A and B are each 400g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 801 g / m 2 A paper base material was obtained under the same conditions as in Example 1-1, except that the paper base material was changed to the above.

[0070] (Examples 1-3) The paper materials of paper layers A and B are each 320g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 641 g / m 2 A paper base material was obtained under the same conditions as in Example 1-1, except that the paper base material was changed to the above.

[0071] (Examples 1 to 4) A paper base material was obtained under the same conditions as in Example 1-2, except that 1.30 parts (solids equivalent) of aluminum sulfate and 1.10 parts (solids equivalent) of a rosin-based sizing agent were added to 100 parts (solids equivalent) of the pulp slurry of paper layer A.

[0072] (Examples 1 to 5) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.70 parts (solids equivalent) of aluminum sulfate and 0.50 parts (solids equivalent) of a rosin-based sizing agent were added to 100 parts (solids equivalent) of the pulp slurry of paper layer A.

[0073] (Examples 1 to 6) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.50 parts (solids) of aluminum sulfate and 0.25 parts (solids) of a rosin-based sizing agent were added to 100 parts (solids) of the pulp slurry of paper layer A.

[0074] (Examples 1 to 7) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.70 parts (solids equivalent) of aluminum sulfate and 0.50 parts (solids equivalent) of a rosin-based sizing agent were added to 100 parts (solids equivalent) of the pulp slurry of paper layer B.

[0075] (Examples 1 to 8) A paper base material was obtained under the same conditions as in Example 1-2, except that 1.00 part (solid content equivalent) of aluminum sulfate and 0.90 parts (solid content equivalent) of a rosin-based sizing agent were added to 100 parts (solid content equivalent) of the pulp slurry of paper layer B.

[0076] (Examples 1 to 9) A paper base material was obtained under the same conditions as in Example 1-2, except that NBKP (Douglas fir pulp, radiata pine pulp, and cedar pulp manufactured by Oji Paper Co., Ltd.) and LBKP were mixed in a mass ratio of 60:40 as the pulp raw material for paper layer A.

[0077] (Examples 1 to 10) A paper base material was obtained under the same conditions as in Example 1-2, except that NBKP and LBKP were mixed in a mass ratio of 80:20 as the pulp raw material for paper layer A.

[0078] (Examples 1 to 11) A paper base material was obtained under the same conditions as in Example 1-2, except that NBKP and LBKP were mixed in a mass ratio of 60:40 as the pulp raw material for paper layer B.

[0079] (Examples 1 to 12) A paper base material was obtained under the same conditions as in Example 1-2, except that NBKP and LBKP were mixed in a mass ratio of 80:20 as the pulp raw material for paper layer B.

[0080] (Examples 1 to 13) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.05 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer A, and 0.05 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer B.

[0081] (Examples 1 to 14) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.50 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer A, and 0.50 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer B.

[0082] (Examples 1 to 15) A paper base material was obtained under the same conditions as in Example 1-2, except that the J / W ratio was adjusted so that the fiber orientation ratio became 1.42.

[0083] (Examples 1 to 16) A paper base material was obtained under the same conditions as in Example 1-2, except that the J / W ratio was adjusted so that the fiber orientation ratio became 2.48.

[0084] (Comparative Example 1-1) The paper materials of paper layers A and B are each 200g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 401 g / m 2 A paper base material was obtained under the same conditions as in Example 1-1, except that the paper base material was changed to the above.

[0085] (Comparative Example 1-2) The paper materials of paper layers A and B are each 800g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 1601 g / m 2 A paper base material was obtained under the same conditions as in Example 1-1, except that the paper base material was changed to the above.

[0086] (Comparative Example 1-3) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.30 parts (solid content equivalent) of aluminum sulfate and 0.10 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer A, and 0.30 parts (solid content equivalent) of aluminum sulfate and 0.08 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer B.

[0087] (Comparative Examples 1-4) A paper base material was obtained under the same conditions as in Example 1-2, except that 1.40 parts (solid content equivalent) of aluminum sulfate and 1.20 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer A, and 1.30 parts (solid content equivalent) of aluminum sulfate and 1.10 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer B.

[0088] (Comparative Examples 1-5) A paper base material was obtained under the same conditions as in Example 1-2, except that 0.20 parts (solids) of aluminum sulfate and 0.04 parts (solids) of a rosin-based sizing agent were added to 100 parts (solids) of the pulp slurry of paper layer B.

[0089] (Comparative Examples 1-6) A paper base material was obtained under the same conditions as in Example 1-2, except that NBKP and LBKP were mixed in a mass ratio of 85:15 as the pulp raw material for paper layer A.

[0090] (Comparative Examples 1-7) A paper base material was obtained under the same conditions as in Example 1-2, except that NBKP and LBKP were mixed in a mass ratio of 85:15 as the pulp raw material for paper layer B.

[0091] (Example 2-1) (Paper base material) A paper base material was produced by bonding two sheets of base paper (paper layer A and paper layer B) with an adhesive in the following procedure. The pulp raw material for paper layer A was a mixture of LBKP (acacia pulp and eucalyptus pulp manufactured by Oji Paper Co., Ltd.) and waste paper pulp (recycled magazines and newspapers) in a mass ratio of 50:50. The pulp was beaten using a scrapefiner to obtain a pulp slurry. The beating conditions were adjusted for the pulp concentration, processing amount, and beating power so that the freeness of the pulp slurry was 400 to 450 ml. To 100 parts of the obtained pulp slurry (based on solids), 1.20 parts (based on solids) of aluminum sulfate (liquid aluminum sulfate, manufactured by Asahi Chemical Industry Co., Ltd.) were added as an internal paper strength enhancer (PS373-20, manufactured by Arakawa Chemical Industry Co., Ltd.), 0.20 parts (based on solids) of a polyacrylamide-based dry strength enhancer (PS373-20, manufactured by Arakawa Chemical Industry Co., Ltd.) as an internal sizing agent, and 1.00 parts (based on solids) of a rosin-based sizing agent (Sizepine N811M, manufactured by Arakawa Chemical Industry Co., Ltd.) as an internal sizing agent were added to prepare a paper stock. The obtained paper stock was made using a Fourdrinier paper machine, adjusting the J / W ratio so that the fiber orientation ratio was 1.62, and paper was made to a basis weight of 560 g / m. 2 Thus, paper layer A was obtained.

[0092] As the pulp raw material for paper layer B, LBKP (acacia pulp and eucalyptus pulp manufactured by Oji Paper Co., Ltd.) and waste paper pulp (waste magazine paper and waste newspaper paper) were mixed in a mass ratio of 50:50 and beaten using a double disc refiner to obtain a pulp slurry. The beating conditions were adjusted so that the freeness of the pulp slurry was 400 to 450 ml, with the pulp concentration, processing amount, and beating power being adjusted. To 100 parts of the obtained pulp slurry (based on solid content), 0.30 parts (based on solid content) of aluminum sulfate (liquid aluminum sulfate manufactured by Asahi Chemical Industry Co., Ltd.), 0.20 parts (based on solid content) of a polyacrylamide-based dry strength agent (PS373-20 manufactured by Arakawa Chemical Industry Co., Ltd.), and 0.10 parts (based on solid content) of a rosin-based sizing agent (Sizepine N811M manufactured by Arakawa Chemical Industry Co., Ltd.) were added to prepare a paper stock. The obtained paper stock was made using a Fourdrinier paper machine, adjusting the J / W ratio so that the fiber orientation ratio was 1.62, and paper was made to a basis weight of 560 g / m. 2 Thus, paper layer B was obtained.

[0093] One side of the obtained paper layer A was coated with 5 g / m of acrylic emulsion adhesive. 2 The paper is coated and laminated with paper layer B, with a basis weight of 1125 g / m 2 Thus, a paper base material for an interleaf paper was obtained.

[0094] (Example 2-2) Paper layer A and paper layer B each have a basis weight of 400 g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 805 g / m 2A paper base material was obtained under the same conditions as in Example 2-1, except that the paper base material was changed to the above.

[0095] (Example 2-3) Paper layer A and paper layer B each have a basis weight of 320 g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 645 g / m 2 A paper base material was obtained under the same conditions as in Example 2-1, except that the paper base material was changed to the above.

[0096] (Examples 2-4) A paper base material was obtained under the same conditions as in Example 2-2, except that 1.30 parts (solids equivalent) of aluminum sulfate and 1.10 parts (solids equivalent) of a rosin-based sizing agent were added to 100 parts (solids equivalent) of the pulp slurry of paper layer A.

[0097] (Examples 2-5) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.70 parts (solids equivalent) of aluminum sulfate and 0.50 parts (solids equivalent) of a rosin-based sizing agent were added to 100 parts (solids equivalent) of the pulp slurry of paper layer A.

[0098] (Examples 2-6) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.50 parts (solids equivalent) of aluminum sulfate and 0.25 parts (solids equivalent) of a rosin-based sizing agent were added to 100 parts (solids equivalent) of the pulp slurry of paper layer A.

[0099] (Examples 2-7) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.70 parts (solids) of aluminum sulfate and 0.50 parts (solids) of a rosin-based sizing agent were added to 100 parts (solids) of the pulp slurry of paper layer B.

[0100] (Examples 2-8) A paper base material was obtained under the same conditions as in Example 2-2, except that 1.00 part (solid content equivalent) of aluminum sulfate and 0.90 parts (solid content equivalent) of a rosin-based sizing agent were added to 100 parts (solid content equivalent) of the pulp slurry of paper layer B.

[0101] (Examples 2-9) A paper base material was obtained under the same conditions as in Example 2-2, except that NBKP (Douglas fir pulp, radiata pine pulp, and cedar pulp manufactured by Oji Paper Co., Ltd.) and LBKP were mixed in a mass ratio of 60:40 as the pulp raw material for paper layer A.

[0102] (Examples 2-10) A paper base material was obtained under the same conditions as in Example 2-2, except that NBKP and LBKP were mixed in a mass ratio of 80:20 as the pulp raw material for paper layer A.

[0103] (Example 2-11) A paper base material was obtained under the same conditions as in Example 2-2, except that NBKP and LBKP were mixed in a mass ratio of 60:40 as the pulp raw material for paper layer B.

[0104] (Example 2-12) A paper base material was obtained under the same conditions as in Example 2-2, except that NBKP and LBKP were mixed in a mass ratio of 80:20 as the pulp raw material for paper layer B.

[0105] (Example 2-13) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.05 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer A, and 0.05 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer B.

[0106] (Examples 2-14) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.50 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer A, and 0.50 parts (solids equivalent) of a polyacrylamide-based dry strength agent was added per 100 parts (solids equivalent) of the pulp slurry of paper layer B.

[0107] (Example 2-15) A paper base material was obtained under the same conditions as in Example 2-2, except that the J / W ratio was adjusted so that the fiber orientation ratio became 1.42.

[0108] (Example 2-16) A paper base material was obtained under the same conditions as in Example 2-2, except that the J / W ratio was adjusted so that the fiber orientation ratio became 2.48.

[0109] (Comparative Example 2-1) Paper layer A and paper layer B each have a basis weight of 200 g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 405 g / m 2 A paper base material was obtained under the same conditions as in Example 2-1, except that the paper base material was changed to the above.

[0110] (Comparative Example 2-2) Paper layer A and paper layer B each have a basis weight of 800 g / m 2 The paper was made using a fourdrinier paper machine so that the paper had a basis weight of 1605 g / m 2 A paper base material was obtained under the same conditions as in Example 2-1, except that the paper base material was changed to the above.

[0111] (Comparative Example 2-3) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.30 parts (solid content equivalent) of aluminum sulfate and 0.10 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer A, and 0.30 parts (solid content equivalent) of aluminum sulfate and 0.08 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer B.

[0112] (Comparative Example 2-4) A paper base material was obtained under the same conditions as in Example 2-2, except that 1.40 parts (solid content equivalent) of aluminum sulfate and 1.20 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer A, and 1.30 parts (solid content equivalent) of aluminum sulfate and 1.10 parts (solid content equivalent) of a rosin-based sizing agent were added per 100 parts (solid content equivalent) of the pulp slurry of paper layer B.

[0113] (Comparative Example 2-5) A paper base material was obtained under the same conditions as in Example 2-2, except that 0.20 parts (solids) of aluminum sulfate and 0.04 parts (solids) of a rosin-based sizing agent were added to 100 parts (solids) of the pulp slurry of paper layer B.

[0114] (Comparative Example 2-6) A paper base material was obtained under the same conditions as in Example 2-2, except that NBKP and LBKP were mixed in a mass ratio of 85:15 as the pulp raw material for paper layer A.

[0115] (Comparative Example 2-7) A paper base material was obtained under the same conditions as in Example 2-2, except that NBKP and LBKP were mixed in a mass ratio of 85:15 as the pulp raw material for paper layer B.

[0116] <Humidity molding> The paper substrates obtained in the examples and comparative examples were punched out to a length of 122 mm and a width of 167 mm to prepare blanks for humid molding. In an environment of 23°C temperature and 50% RH humidity, water vapor was sprayed onto side B of the blank so that the moisture content of the blank was 10% by mass, and an acrylic emulsion adhesive was applied to one of the joints at a 1 cm portion of the edge of the blank. The blank was placed between the male and female dies of a specified mold, and then pressed under a pressure of 0.3 kg / cm. 2 The mixture was pressed under conditions of 1000 ml, 1000 ml for a press time of 5 seconds, and cylindrical paper containers with a diameter of 50 mm were produced.

[0117] <Evaluation of moldability during humid molding> The outer and inner surfaces of the three paper containers obtained were observed and evaluated according to the following criteria. The results are shown in Tables 1 and 2. A: 0 containers with cracks (torn or broken areas), dents, or creases in the paper base material B: 0 containers had cracks (torn or broken parts) or dents in the paper base material, and 1 container had a crease. C: 0 containers had cracks (torn or broken parts) or dents in the paper base material, and 2 containers had folds. D: At least one container has cracks (torn or missing parts) or dents in the paper base, or three containers have folds

[0118] <Evaluation of durability when dropped> The resulting paper container was dropped without acceleration from a height of 80 cm onto a floor with a stainless steel plate placed on it, with one opening horizontally. The appearance of the paper container after the drop was observed and evaluated according to the following criteria. The results are shown in Tables 1 and 2. Note that "deformation" refers to a state in which a dent was found on the side of the cylinder or the paper base material was folded in one or more places. A: No deformation was observed even after dropping it three times. B: Deformation is observed after three drops. C: Deformation is observed after two drops. D: Deformation is observed after one drop.

[0119] <Beauty after wetting> The obtained paper container was left to stand for 1 hour in a high temperature and high humidity environment at a temperature of 80°C and a relative humidity of 65%. After the vibration test, the appearance of the paper container was observed and the feel was confirmed, and the container was evaluated according to the following criteria. The results are shown in Tables 1 and 2. The vibration test was conducted in accordance with JIS Z0232:2020 under conditions of random vibration and vertical orientation for 90 minutes. A: There are absolutely no wrinkles on the surface of side A of the paper container, and it feels firm to the touch. B: There are no wrinkles on the surface of side A of the paper container, but it feels soft to the touch. C: Wrinkles appear on the surface of side A of the paper container, but it does not tear when touched. D: Wrinkles have appeared on the surface of side A of the paper container, and some parts are torn when touched.

[0120] [Table 1]

[0121] [Table 2]

Claims

1. A paper substrate for moist forming, comprising: The paper base material has two or more paper layers, The thickness of the paper base material is 0.8 to 1.5 mm; When one surface of the paper base material is designated as side A and the other surface is designated as side B, The Cobb water absorbency measured from the A side of the paper base material is equal to or lower than the Cobb water absorbency measured from the B side, The Cobb water absorbency measured from the A side is 10 to 700 g / m 2 - 60 seconds, The Cobb water absorbency measured from the B side is 10 to 1000 g / m 2 - 60 seconds, Both of the average fiber width of the pulp contained in the paper layer constituting one surface of the paper base material and the average fiber width of the pulp contained in the paper layer constituting the other surface of the paper base material are 28.0 μm or less. A paper substrate for moist forming, comprising:

2. The paper base material for moist forming according to claim 1, wherein the average value of the longitudinal tensile strength of the paper base material per basis weight and the transverse tensile strength of the paper base material per basis weight, measured after adjusting the moisture content of the paper base material to 10% by mass, is 12.0 to 43.0 Nm / g.

3. The paper base material is a multi-layer paper having two or more layers of the paper, or a laminated paper having two or more base papers attached thereto, The paper substrate for moist forming according to claim 1 , wherein each of the two or more base papers comprises the paper layer.

4. The paper base material for moist forming according to claim 1 , wherein the pulp contained in the paper layer contains hardwood kraft pulp and recycled paper pulp.

5. The difference between the Cobb absorbency measured from the B side and the Cobb absorbency measured from the A side (B side - A side) is 20 to 900 g / m 2 The paper substrate for moist forming according to claim 1, wherein the heat retention time is 60 seconds.

6. A paper product obtained by using the paper base material for moist forming according to any one of claims 1 to 5.

7. A paper container comprising the paper base material for moist forming according to any one of claims 1 to 5.

8. The paper container has a bottle shape, The paper container according to claim 7 , wherein the side A constitutes at least a portion of an outer surface of the paper container.

Citation Information

Patent Citations

  • Method and device for producing a rigid paperboard container and container

    JP1984500701A

  • Liquid bottle

    JP1993294347A

  • A novel water-based adhesive for industrial applications

    JP2009507968A

  • Reserver for biological sample

    JP2010124806A

  • Base paper for paper charm

    JP2013064204A

Cited By

  • Thermoformable paperboard-based laminate and a method for manufacturing said laminate

    SE2430607A1

  • Thermoformable paperboard-based laminate and a method for manufacturing said laminate

    WO2026115408A1