Catalyst particles, film electrode joint body, and fuel battery
Catalyst particles with Pt and Sn oxide on a conductive carrier, enhanced by an ionic liquid, address hydrophilicity and crystallinity issues, improving fuel cell performance and durability.
Patent Information
- Application Number
- JP2023063514
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Pt-SnO2 catalysts used in fuel cells face issues with hydrophilicity leading to flattening and reduced IV characteristics due to lowered crystallinity and increased electronic resistance, affecting durability and performance.
Catalyst particles comprising Pt and Sn oxide on a conductive carrier, with a specific G/D ratio, contacted by an ionic liquid to suppress hydrophilicity and enhance electronic conductivity.
The catalyst particles improve IV characteristics and durability by stabilizing Pt, reducing electronic resistance, and preventing catalyst layer flooding.
Smart Images

Figure 2024150209000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to catalyst particles, a membrane electrode assembly including the catalyst particles, and a fuel cell including the membrane electrode assembly. [Background technology]
[0002] A known solid polymer fuel cell is one that includes an electrolyte layer formed from an ion exchange resin, a fuel-side electrode (anode) to which fuel is supplied, and an oxygen-side electrode (cathode) to which oxygen is supplied.
[0003] In such a fuel cell, fuel is supplied to the anode and air is supplied to the cathode, which generates an electromotive force and generates electricity.
[0004] As a cathode catalyst, for example, a Pt-supported carbon catalyst in which Pt particles are supported on carbon has been proposed, but this Pt-supported carbon catalyst has a problem with durability. Specifically, there is a problem that the Pt particles supported on the carbon aggregate or dissolve into the electrolyte layer, which leads to a decrease in the performance of the fuel cell.
[0005] Patent Document 1 reports catalyst particles having carbon particles carrying Pt, with Sn oxide disposed on the Pt particles. It is described that the specific surface area of the platinum particles is increased and the tin oxide on the Pt surface suppresses the aggregation of the Pt particles, resulting in both high activity and good durability.
[0006] In addition, in Non-Patent Document 1, Pt-SnO2 particles are produced by heat-treating carbon particles carrying a PtSn alloy and separating them into a Pt phase and a SnO2 phase. It is reported that electrons are donated from the SnO2 phase to the Pt phase, improving the activity of Pt and suppressing oxidation. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] WO2014 / 136798 publication [Non-patent literature]
[0008] [Non-Patent Document 1] small,2020,16,2005048. Summary of the Invention [Problem to be solved by the invention]
[0009] However, in an evaluation of power generation using a membrane electrode assembly containing Pt-SnO2 catalyst particles, there were problems with the SnO2 placed on the Pt surface being hydrophilic, making the catalyst layer prone to flooding, and the heat treatment to form the SnO2 phase reducing the crystallinity of the carbon and increasing the electronic resistance, resulting in poorer IV characteristics than a membrane electrode assembly containing Pt catalyst particles.
[0010] The present inventors have found that by bringing Pt-SnO2 particles into contact with an ionic liquid, flooding can be suppressed and the IV characteristics can be improved.
[0011] In view of the above, an object of the present invention is to provide a catalyst particle, a membrane electrode assembly, and a fuel cell which are excellent in IV characteristics of the membrane electrode assembly. [Means for solving the problem]
[0012] [1] A catalyst particle comprising: a conductive support; and metal particles supported on the conductive support, the metal particles containing Pt and Sn, some or all of the Sn in the metal particles being in the form of an oxide, and at least a portion of a surface of the metal particles being in contact with an ionic liquid. [2] The catalyst particles according to [1], wherein the conductive support is made of carbon, and the peak intensity ratio (G / D ratio) of G band to D band measured by Raman spectroscopy is 1.2 or more and 2.2 or less at a laser wavelength of 532 nm. [3] The catalyst particles according to [1] or [2], wherein the atomic ratio of Pt to Sn in the metal particles is in the range of 3:1 to 10:1. [4] The catalyst particles according to any one of [1] to [3], wherein the ionic liquid is an imidazolium salt. [5] The catalyst particles according to [4], wherein the ionic liquid is 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. [6] The catalyst particles according to [4], wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. [7] A membrane electrode assembly comprising a polymer electrolyte membrane and a cathode electrode catalyst layer, the cathode electrode catalyst layer comprising the catalyst particles according to any one of [1] to [6]. [8] The membrane electrode assembly according to [7], wherein the cathode side electrode catalyst layer further contains a conductive auxiliary. [9] The membrane electrode assembly according to [8], wherein the conductive auxiliary is vapor-grown carbon fiber.
[10] A fuel cell comprising the membrane electrode assembly according to [7], [8] or [9]. Effect of the Invention
[0013] According to one aspect of the present invention, it is possible to provide a catalyst particle, a membrane electrode assembly for a fuel cell, and a fuel cell, which are excellent in IV characteristics. [Brief description of the drawings]
[0014] [Figure 1] 1 is an explanatory diagram showing a schematic diagram of an entire catalyst particle according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an explanatory diagram illustrating a schematic view of the vicinity of the surface of the conductive support in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. <Overall structure of catalyst particles> FIG. 1 is an explanatory diagram showing a schematic view of the entire catalyst particle according to an embodiment of the present invention.
[0016] 1, a catalyst particle 1 according to this embodiment includes a conductive support 2, a plurality of metal particles 3 supported on the conductive support 2, and an ionic liquid 4. Each of the above-mentioned components will be described in detail below.
[0017] (Conductive carrier) There is no particular limitation on the material of the conductive support 2, so long as it is particles of a conductive material. The conductive support 2 is preferably carbon particles. In particular, it is preferable that the conductive support is carbon particles having a peak intensity ratio (G / D ratio) of G band to D band by Raman spectroscopy of 1.2 to 2.2. Also, it is preferable that the conductive support 2 is carbon particles having the above-mentioned peak intensity ratio (G / D ratio) of 1.6 or more. In this embodiment, the wavelength of the laser light used in Raman spectroscopy is 532 nm. In this embodiment, the G band by Raman spectroscopy is a wavelength of 1580 cm -1 The Raman peak located around 1360 cm is called the D band. -1 This refers to the Raman peaks located near If the peak intensity ratio (G / D ratio) is less than 1.2, the electronic resistance is high and the degree of improvement in the IV characteristics may be small. If the peak intensity ratio (G / D ratio) is more than 2.2, the crystallinity of the carbon particles is high and it may be difficult to support metal particles.
[0018] (metal particles 3) The metal particles 3 used in the catalyst particles 1 contain Pt and Sn, and at least a part or all of the Sn is an oxide. The Sn oxide is SnO x The oxidation state of Sn is not specifically specified because it varies depending on the catalyst synthesis conditions, MEA fabrication conditions, and power generation conditions; however, fully oxidized SnO2 is desirable because it is chemically stable.
[0019] The ratio (atomic ratio) of the metal elements in the metal particles 3 may be Pt:Sn=3:1 to 10:1. If the amount of Sn is more than Pt:Sn=3:1, Sn and its oxides themselves are not active, so the number of active Pt sites decreases and the overall catalytic activity decreases. If the amount of Sn is less than Pt:Sn=10:1, the effect of improving the activity of Pt by the Sn oxides cannot be obtained.
[0020] The metal particles 3 may have a PtSn alloy phase and a Sn oxide phase, but preferably have a Pt phase 3a and a Sn oxide phase 3b as shown in Fig. 2. It is preferable that the metal particles 3 have a Pt phase 3a and a Sn oxide phase 3b, and that the Sn oxide phase 3b is dispersed within the Pt phase 3a.
[0021] It is preferable that at least a part of the Sn oxide phase 3 b is exposed on the surface of the metal particle 3 .
[0022] By heat treating PtSn alloy particles in an oxidizing atmosphere such as an oxygen-containing atmosphere, metal particles containing Pt and Sn having an Sn oxide phase can be obtained. In particular, when heat treatment is performed under conditions in which there is sufficient oxygen, the Pt phase 3a and SnO x It is possible to easily obtain metal particles 3 that are phase-separated into a phase (for example, an SnO2 phase) 3b.
[0023] Heat treatment of PtSn alloy to form Pt phase and SnO x By separating the phases, SnO x The phase can be selectively provided on the Pt particles, and SnO x This promotes electron donation from the catalyst to Pt, thereby increasing the catalytic activity of Pt.
[0024] (Ionic Liquid) The ionic liquid is in contact with the surfaces of the metal particles 3. By having the surfaces of the Pt phase of the metal particles 3 in contact with the ionic liquid, the generation of oxides derived from water is suppressed, and flooding in the membrane electrode assembly is also suppressed. The ionic liquid may further be in contact with the surface and the interior of the conductive support 2 .
[0025] Although there is no particular limitation on the ionic liquid 5, it is preferably an imidazolium salt. An imidazolium salt is a salt of a cation having an imidazole ring structure and a counter anion. Examples of the cation are as follows. R and R' are independently -CH3, -C2H5, -C3H7, -C4H9, -CH 13 ,-CH2-CH=CH2. [ka]
[0026] An example of a counter anion is Cl. - ,Br - , I - ,BF4 - ,PF6 - , FSI((FSO2)2N - ),TFSI((CF3SO2)2N - ). In particular, the ionic liquid 5 preferably contains 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. As the alkyl moiety, methyl, ethyl, propyl, butyl, pentyl, heptyl, hexyl, octyl, nonyl, decyl, etc. are used. As the alkyl moiety, butyl is particularly preferable. In other words, the ionic liquid 5 is more preferably 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
[0027] (Catalyst particle composition) The ratio of the metal particles supported in the catalyst particle 1 may be 30 parts by mass or more and 60 parts by mass or less, based on 100 parts by mass of the total of the conductive support and the metal particles. 50 parts by mass is particularly preferable. If it is less than 30 parts by mass, the catalyst layer thickness of the membrane electrode assembly increases, and the IV characteristics may not improve easily. If it is more than 60 parts by mass, it becomes difficult to disperse and support the metal particles on the conductive support, and the metal particles may aggregate and become large, resulting in a decrease in mass activity.
[0028] The amount of the ionic liquid 5 in the catalyst particle 1 (the amount of impregnation of the ionic liquid 5) may be equivalent to a volume of 15 vol% or more and 80 vol% or less of the pore volume of the conductive support 2 and the metal particle 3. More specifically, the content of the ionic liquid 5 in the catalyst particle 1 is preferably within a range of 30 vol% or more and 60 vol% or less of the pore volume of the conductive support 2 and the metal particle 3 of the catalyst particle 1, and more preferably within a range of 45 vol% or more and 55 vol% or less. The pore volume in the conductive support 2 and the metal particle 3 of the catalyst particle 1 can be determined, for example, by a low-temperature nitrogen adsorption method. In this embodiment, the total volume of pores from 2 nm to 100 nm is used as the pore volume. If the amount of impregnation of the ionic liquid 5 is less than 15 vol% of the pore volume of the catalyst particle, the ionic liquid 5 may not have a sufficient effect on the oxygen reduction activity. Furthermore, if the amount of ionic liquid 5 impregnated is more than 80 vol% of the pore volume of the catalyst particle, the ionic liquid 5 cannot be stably retained in the catalyst particle 1, and some of the ionic liquid 5 may flow out during the manufacturing process or preparation process of the catalyst particle 1, or during power generation of a fuel cell incorporating an electrode using the catalyst particle 1. Furthermore, if the amount of ionic liquid 5 impregnated is large, oxygen is less likely to permeate from the ionic liquid layer to the metal particle surface, increasing resistance and possibly deteriorating IV performance.
[0029] [Method of manufacturing catalyst particles] The above catalyst particles can be produced as follows.
[0030] A conductive support carrying PtSn alloy particles is prepared. Any known synthesis method may be used. Next, the conductive support carrying PtSn alloy particles is heat-treated in an oxygen atmosphere such as air to obtain catalyst particles having a Pt phase or a PtSn phase and an Sn oxide phase. Increasing the heat treatment temperature promotes phase separation between the metal layer of the PtSn alloy particles and the Sn oxide phase, but this tends to decrease the G / D ratio of the conductive support, so it is preferable to appropriately adjust the heat treatment temperature and time.
[0031] Next, the conductive support carrying the catalyst particles is impregnated with an ionic liquid. Specifically, the conductive support carrying the catalyst particles is impregnated with a solution of the ionic liquid, and then the solvent is removed. An example of the solvent is acetonitrile. This causes the ionic liquid to adhere to the surface of the metal particles.
[0032] <Membrane electrode assembly for fuel cells> The fuel cell membrane electrode assembly according to this embodiment includes a polymer electrolyte membrane and a catalyst layer (electrode catalyst layer) containing the above-mentioned catalyst particles 1. The fuel cell membrane electrode assembly according to this embodiment includes, for example, a polymer electrolyte membrane and a pair of catalyst layers that contain the catalyst particles 1 and sandwich the polymer electrolyte membrane from above and below. The catalyst layer on the anode side does not need to contain the above-mentioned catalyst particles 1, and only the catalyst layer on the cathode side may contain the above-mentioned catalyst particles 1.
[0033] The polymer electrolyte membrane is made of a polymer material having proton conductivity, and for example, a fluorine-based electrolyte membrane or a hydrocarbon-based polymer electrolyte membrane can be used. As the fluorine-based polymer electrolyte membrane, for example, Nafion (registered trademark) manufactured by DuPont, Flemion (registered trademark) manufactured by Asahi Glass Co., Ltd., Aciplex (registered trademark) manufactured by Asahi Kasei Corporation, Gore Select (registered trademark) manufactured by Gore, etc. can be used. In addition, as the hydrocarbon-based polymer electrolyte membrane, for example, an electrolyte membrane such as sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, or sulfonated polyphenylene can be used. The thickness of the polymer electrolyte membrane can be, for example, 0.05 to 0.25 mm.
[0034] The catalyst layer may further contain a conductive auxiliary agent other than the above-mentioned catalyst particles. Examples of the conductive auxiliary agent include vapor grown carbon fiber (VGCF), thin-layer graphene, and carbon nanotube (CNT), and VGCF is particularly preferable.
[0035] The content of the linear material such as VGCF in the catalyst layer is preferably in the range of 0.1 to 45 parts by mass, more preferably in the range of 1 to 30 parts by mass, and even more preferably in the range of 10 to 20 parts by mass, relative to 100 parts by mass of the entire catalyst layer. If the content of the fibrous material in the catalyst layer is within the above numerical range, it is possible to impart even better electronic conductivity to the catalyst layer and contribute to maintaining the structure of the catalyst layer.
[0036] The catalyst layer may further contain an ionomer (polymer electrolyte). The ionomer in the catalyst layer may be the same type as the ionomer in the polymer electrolyte membrane, or may be different. The amount of ionomer used in the catalyst layer according to this embodiment may be such that the ratio of the ionomer mass to the mass of catalyst particle 1 (ionomer mass / (total mass of conductive support, metal particles, and ionic liquid)) is 0.2 or more and 0.4 or less. If this ratio is lower than 0.2, proton conduction may be insufficient, resistance may be high, and IV performance may be deteriorated. If the ratio is higher than 0.4, the number of pores in the catalyst layer may be reduced, water discharge and oxygen diffusion may be insufficient, and IV performance may be deteriorated.
[0037] <Fuel cell> The fuel cell according to this embodiment includes the above-mentioned membrane electrode assembly. The fuel cell according to this embodiment includes, for example, a pair of gas diffusion layers, each of which is disposed to face each of the catalyst layers of the above-mentioned membrane electrode assembly. The gas diffusion layers and the catalyst layers form a cathode (positive electrode) and an anode (negative electrode).
[0038] (Effects of this embodiment) The catalyst particles 1 according to this embodiment have the following effects. (1) In the catalyst particle 1 and the membrane electrode assembly according to this embodiment, The metal particles contain Pt and Sn, some or all of the Sn in the metal particles is in the form of an oxide, and at least a portion of the surface of the metal particles is in contact with the ionic liquid.
[0039] With such a configuration, the oxidation of Pt is suppressed by the presence of the Sn oxide phase in the metal particles, improving durability. Further, by bringing an ionic liquid into contact with at least a part of the surface of the metal particles, the hydrophilicity of the metal particle surface due to the SnOx phase is suppressed, and floating in the catalyst layer of the membrane electrode assembly can be suppressed.
[0040] (2) The electrode catalyst layer according to an example of the present embodiment contains the above-described catalyst particles 1 and a conductive auxiliary agent. With such a configuration, the decrease in electron conductivity accompanying the decrease in the crystallinity of carbon due to the heat treatment during the synthesis of the catalyst particles can be compensated for by the conductive auxiliary agent.
[0041] [Examples] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the examples at all.
[0042] <Synthesis of Pt particle-supported carbon (catalyst A)> The Pt particle-supported carbon was synthesized according to a known method, had a Pt loading of Pt / C = 50 / 50 (wt / wt), and a carbon support having a G band / D band ratio of 1.6 or more from Raman spectroscopy was used.
[0043] <Synthesis of PtSn alloy particle-supported carbon (catalyst B)> The PtSn alloy particle-supported carbon was synthesized according to a known method, had a PtSn loading of PtSn / C = 50 / 50 (wt / wt), and a carbon support having a G band / D band ratio of 1.6 or more from Raman spectroscopy was used. The atomic ratio of the PtSn alloy particles was 3:1. Also, a part of the Sn in the PtSn alloy particles was partially oxidized in the working environment to become SnO x and was present.
[0044] <Synthesis of carbon (catalyst C) supporting metal particles in which the SnO2 phase is dispersed in the Pt phase> The synthesized PtSn alloy particle-supported carbon (catalyst B) was heat-treated in air (at 200°C to 400°C for 1 hour) to synthesize carbon supporting metal particles in which the SnO2 phase was dispersed in the Pt phase.
[0045] <Synthesis of ionic liquid-impregnated catalyst particles (Catalyst D)> The synthesized PtSn alloy particle-supported carbon (catalyst B) was added to acetonitrile and ultrasonically dispersed for 30 minutes, after which an ionic liquid was added in an amount equal to 50% of the pore volume of the PtSn alloy particle-supported carbon. After stirring overnight with a stirrer, the acetonitrile was removed with an evaporator to obtain ionic liquid-impregnated catalyst particles (catalyst D).
[0046] <Synthesis of ionic liquid-impregnated catalyst particles (Catalyst E)> Carbon carrying metal particles (Pt phase with SnO2 phase dispersed therein) (catalyst C) was added to acetonitrile and ultrasonically dispersed for 30 minutes, after which ionic liquid was added in an amount equal to 50% of the pore volume of the carbon carrying metal particles. After stirring overnight with a stirrer, the acetonitrile was removed with an evaporator to obtain ionic liquid-impregnated catalyst particles (catalyst E).
[0047] Example 1 Following the procedure described in <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, ionic liquid was brought into contact with heat-treated catalyst C to synthesize ionic liquid-impregnated catalyst particles (catalyst E). The ionic liquid used was 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio of the carbon was evaluated by Raman spectroscopy and found to be 1.1. The catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt particle-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0048] Example 2 Except for the different type of supported carbon starting material, catalyst E was produced in the same manner as in Example 1. Specifically, catalyst C, which had been heat-treated according to <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, was contacted with an ionic liquid to synthesize ionic liquid-impregnated catalyst particles (catalyst E). 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. The catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt particle-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0049] Example 3 Except for the different type of supported carbon starting material, catalyst E was produced in the same manner as in Example 1. Specifically, catalyst C, which had been heat-treated according to <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, was contacted with an ionic liquid to synthesize ionic liquid-impregnated catalyst particles. 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.7. The catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0050] Example 4 Following the procedure described in <Synthesis of ionic liquid-impregnated catalyst particles (catalyst D)>, ionic liquid was brought into contact with PtSn alloy particle-supported carbon (catalyst B) that had not been heat-treated, to synthesize ionic liquid-impregnated catalyst particles (catalyst D). The ionic liquid used was 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The atomic ratio of Pt to Sn in the PtSn alloy particles was 3:1. The G / D ratio was evaluated to be 2.0 by Raman spectroscopy. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst D) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0051] Example 5 Except for the different type of carbon support starting material, catalyst E was produced in the same manner as in Example 4. Specifically, ionic liquid was brought into contact with PtSn alloy particle-supported carbon (catalyst B) that had not been heat-treated, following the procedure of <Synthesis of ionic liquid-impregnated catalyst particles (catalyst D)>, to synthesize ionic liquid-impregnated catalyst particles (catalyst D). 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. PtSn alloy particles with an atomic ratio of Pt to Sn of 3:1 were used. The G / D ratio was evaluated by Raman spectroscopy and found to be 2.2. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst D) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0052] Example 6 Catalyst E was produced in the same manner as in Example 2, except that the atomic ratio of the starting material PtSn alloy particles was different. Specifically, ionic liquid was brought into contact with catalyst C, which had been heat-treated according to <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, to synthesize ionic liquid-impregnated catalyst particles (catalyst E). 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 2:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. The catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. 2The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0053] Example 7 Catalyst E was produced in the same manner as in Example 2, except that the atomic ratio of the starting material PtSn alloy particles was different. Specifically, ionic liquid was brought into contact with catalyst C, which had been heat-treated according to <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, to synthesize ionic liquid-impregnated catalyst particles (catalyst E). 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 10:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. The catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0054] Example 8 Catalyst E was produced in the same manner as in Example 2, except that the atomic ratio of the starting material PtSn alloy particles was different. Specifically, ionic liquid was brought into contact with catalyst C, which had been heat-treated according to <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, to synthesize ionic liquid-impregnated catalyst particles (catalyst E). 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 11:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. The catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0055] Example 9 Ionic liquid-impregnated catalyst particles (catalyst E) were produced in the same manner as in Example 2. Specifically, ionic liquid was brought into contact with catalyst C, which had been subjected to heat treatment according to <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>, to synthesize ionic liquid-impregnated catalyst particles (catalyst E). 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. 2 The catalyst ink was applied so that the thickness became 100 nm, and then dried to obtain a cathode-side catalyst layer. Subsequently, Pt-supported carbon (Catalyst A), an ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the side opposite to the cathode-side catalyst layer so that the platinum amount was 0.05 mg / cm 2 and dried to form an anode-side catalyst layer, thereby fabricating a membrane electrode assembly.
[0056] (Comparative Example 1) Pt-supported carbon (Catalyst A) was synthesized according to <Synthesis of Pt-Supported Carbon (Catalyst A)>. When the G / D ratio was evaluated by Raman spectroscopic analysis, it was 1.7. Pt-supported carbon (Catalyst A) and an ionomer were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink without adding VGCF. The catalyst ink was applied to the electrolyte membrane so that the platinum amount was 0.2 mg / cm 2 and dried to obtain a cathode-side catalyst layer. Subsequently, Pt-supported carbon (Catalyst A), an ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the side opposite to the cathode-side catalyst layer so that the platinum amount was 0.05 mg / cm 2 and dried to form an anode-side catalyst layer, thereby fabricating a membrane electrode assembly.
[0057] (Comparative Example 2) Heat treatment was performed according to <Synthesis of Carbon Supported with Metal Particles in which SnO2 Phase was Dispersed in Pt Phase (Catalyst C)> to synthesize catalyst particles (Catalyst C). The atomic ratio of Pt to Sn of the metal particles was 3:1. When the G / D ratio was evaluated by Raman spectroscopic analysis, it was 1.2. Catalyst particles (Catalyst C) and an ionomer were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink without adding VGCF. The catalyst ink was applied to the electrolyte membrane so that the platinum amount was 0.2 mg / cm 2 and dried to obtain a cathode-side catalyst layer. Next, Pt-supported carbon (catalyst A), ionomer, and VGCF were added to a mixed solution containing water, IPA, and ethanol to prepare a catalyst ink. The catalyst ink was applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. 2 The catalyst ink was applied so that the thickness of the anode electrode became 10 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.
[0058] <Membrane electrode assembly evaluation> The fabricated membrane electrode assembly, gasket, and GDL (Gas Diffusion Layer) were incorporated into a JARI standard cell, and the IV characteristics were evaluated under the power generation conditions described in "Common Fundamental Technology for Cell Evaluation and Analysis," part of NEDO's Basic Technology Development for Promoting the Practical Application of Polymer Electrolyte Fuel Cells. For durability testing, a load response of 6,000 cycles was conducted, as described in the "Common Fundamental Technology for Cell Evaluation Analysis" in the Development of Fundamental Technology for Promoting the Practical Application of Polymer Electrolyte Fuel Cells, conducted by the New Energy and Industrial Technology Development Organization (NEDO). After the durability test, the IV characteristics were evaluated again.
[0059] [Table 1]
[0060] The columns "Voltage before durability" and "Voltage after durability" in Table 1 indicate the voltages of 1.5 A / cm2 in IV measurements before and after the durability tests in Examples 1 to 9 and Comparative Example 2. 2 The values shown are comparisons of the voltage at that time with the corresponding voltage in Comparative Example 1. Examples in which the voltage was improved by 50 mV or more compared to Comparative Example 1 are marked with ⊚, examples in which the voltage was improved within the range of the same to 50 mV or less are marked with ◯, and examples in which the voltage was lower than in Comparative Example 1 are marked with ×.
[0061] Examples 1 to 9 show that the voltage before and after durability is improved by impregnating the catalyst particles with an ionic liquid, compared with Comparative Example 2. Furthermore, it is shown that the voltage before durability is further improved when the G / D ratio of the carbon used as the conductive support is in the range of 1.2 to 2.2. Furthermore, Examples 2 and 9 show that the voltage before and after durability is improved when VGCF is added as a conductive auxiliary. Examples 2, 6, 7, and 8 show that the voltage before durability is further improved when the element ratio of Pt to Sn is 3:1 to 10:1. [Industrial Applicability]
[0062] The fuel cell electrode material according to the present invention is used as an electrode for the power sources of various portable electronic devices, automobiles, and household electrical appliances. [Explanation of symbols]
[0063] 1...catalyst particles, 2...conductive support (carbon), 3...metal particles, 4...ionic liquid.
Claims
1. A catalyst particle comprising: a conductive support; and metal particles supported on the conductive support, the metal particles containing Pt and Sn, a part or all of the Sn in the metal particles being in the form of an oxide, and at least a part of a surface of the metal particles being in contact with an ionic liquid.
2. 2. The catalyst particle according to claim 1, wherein the conductive support is made of carbon, and the peak intensity ratio (G / D ratio) of G band to D band by Raman spectroscopy is 1.2 or more and 2.2 or less at a laser wavelength of 532 nm.
3. 3. The catalyst particles according to claim 1 or 2, wherein the atomic ratio of Pt to Sn in the metal particles is in the range of 3:1 to 10:
1.
4. 3. The catalyst particles according to claim 1, wherein the ionic liquid is an imidazolium salt.
5. 5. The catalyst particles according to claim 4, wherein the ionic liquid is 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
6. 5. The catalyst particles according to claim 4, wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
7. A membrane electrode assembly including a polymer electrolyte membrane and a cathode-side electrode catalyst layer, The cathode side electrode catalyst layer comprises the catalyst particles according to claim 1 .
8. The membrane electrode assembly in accordance with claim 7 , wherein the cathode side electrode catalyst layer further comprises a conductive auxiliary.
9. 9. The membrane electrode assembly of claim 8, wherein the conductive aid is vapor grown carbon fiber.
10. A fuel cell comprising the membrane electrode assembly of claim 7.
Citation Information
Patent Citations
Catalyst for solid polymer fuel cell cathodes and method for producing catalyst for solid polymer fuel cell cathodes
WO2014136798A1