Silicone composition for low temperature
The development of silanol-terminated polysiloxanes through Lewis acid-induced polycondensation addresses the limitations of existing silicones in aerospace applications by providing high molecular weight, low glass transition temperature, and cryogenic resistance, ensuring mechanical stability and compatibility with crosslinkers.
Patent Information
- Application Number
- JP2024039763
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Existing silicone materials fail to meet the requirements of aerospace applications at cryogenic temperatures below -100°C, lacking sufficient tensile strength, elongation, and resistance to crystallization-induced hardening, which leads to mechanical failures in space missions.
A method for producing silanol-terminated poly(dimethyl-co-diethyl)siloxane and poly(methylhydro-co-diethyl)siloxane using a Lewis acid-induced polycondensation process with triflate salt and perfluoroborane catalysts, avoiding high reaction temperatures and minimizing cyclic by-products, along with the development of compatible crosslinkers to prevent phase separation.
The method produces polysiloxanes with high molecular weight and low glass transition temperatures, maintaining elasticity and mechanical integrity at cryogenic temperatures, preventing crystallization, and ensuring compatibility with crosslinking agents, thus suitable for aerospace applications.
Smart Images

Figure 2024150403000001 
Figure 2024150403000002 
Figure 2024150403000003
Abstract
Description
[Technical field]
[0001] The present invention relates to reinforced silicone rubber and silicone oil compositions capable of withstanding the extremely low temperatures required for aerospace applications. [Background technology]
[0002] Silicones are organosilicon polymers with the structure of siloxane, characterized by silicon atoms bonded to alkyl groups such as ethyl or methyl groups, trifluoromethyl groups, aryl groups, or other functional groups. Silicone rubber compositions derived from poly(dimethylsiloxane), commonly known as PDMS, are known to withstand temperatures down to -60°C. However, many space applications, such as space exploration missions, require silicone materials that can withstand temperatures well below -100°C and have tensile yield strengths (>3MPa) and elongations at break of more than 300%.
[0003] Poly(diethylsiloxane) (PDIES) is the only polymeric material with a glass transition temperature of -142°C. However, pure PDIES is not suitable for such applications, since it exhibits several crystallization / melting transitions between -142°C and 0°C. The crystallization of silicone is usually accompanied by its hardening, embrittlement, and loss of elasticity. This can degrade or even catastrophically impair the mechanical properties of objects for automotive applications, such as space rovers. It is known from the prior art that the addition of small amounts of phenyl, biphenyl, or diethyl groups (less than 10 mol%) in poly(dimethylsiloxane) prevents the cold crystallization of dimethylpolysiloxane copolymers. In fact, the majority of currently commercially available silicones for space applications (Momentive, Elkem, Nusil, Dow Corning, IOTA, etc.) belong to the family of poly(biphenyl-co-dimethylsiloxane) or poly(methylphenyl-co-dimethylsiloxane). Interestingly, when the biphenyl or methylphenyl content in such copolymers exceeds 10 mol%, the glass transition shifts to higher temperatures, limiting their use at cryogenic temperatures (down to -150 °C). For example, RTV 560, RTV 566, and RTV 567 (methyl-phenyl silicones) sold by Momentive have glass transition temperatures Tg = -115 °C, making these materials unsuitable for lunar south pole missions. It is important to note that cold crystallization of RTV 566 under 25% strain and prolonged waiting at -80 °C (60 hours) increased the elastic modulus from 5 MPa to 240 MPa, which is probably the main cause of mechanical failure and misalignment of the telescope.
[0004] Currently, there are no commercially available silicones that have a relatively high tensile strength (i.e., greater than 4 MPa), an elongation at break greater than 100%, and low temperature resistance below -120°C. The only commercially available silicone is sold by Gelest (EDV-2022), which contains 18-22 mol% poly(diethyl)- and 78-82 mol% poly(dimethylsiloxane), and has a Tg of -131°C. However, this material is not suitable for aerospace applications because it has a relatively low molecular weight (10,000-12,000 g / mol) and may contain cyclic siloxane oligomers that make the material brittle.
[0005] The classical method of silicone synthesis relies on the hydrolysis of dimethyldichlorosilane, resulting in the disilanol H[O-Si(CH3)2] n -OH, hydrochloric acid, and varying amounts of cyclic siloxanes are produced. The hydrochloric acid then acts as a catalyst to condense the disilanols into polydimethylsiloxanes. From there, the silanol-terminated silicones can be polymerized in a variety of ways depending on the desired properties of the final product.
[0006] U.S. Patent No. 4,960,850 describes polycondensation of silanol-terminated polydiorganosiloxane oligomers in the presence of a catalytically effective amount of trifluoromethylsulfonic acid in a closed reaction zone at a temperature of 20°C to 160°C while continuously removing the polycondensation water using a vacuum, and terminating the polycondensation reaction by adding a catalyst-neutralizing amount of cyclopolydiorganosilazane or polydiorganosilazane having diorganoaminosilyl end groups to the reaction liquid. However, trifluoromethylsulfonic acid has a boiling point of 162°C and can be distilled under high vacuum while removing the water.
[0007] Controlled molecular weight silicones are obtained from the ring-opening polymerization (ROP) of cyclic siloxanes. This is a highly controlled method and is also the main method in industry. The above method is relatively easy for the polymerization of a single cyclosiloxane, but it becomes difficult to control when trying to prepare 1:1 poly(dimethyl-cо-diethyl)siloxane by copolymerizing two cyclosiloxanes, for example, decamethylcyclosiloxane (D5Me10) and hexaethylcyclosiloxane (D3Et6). The latter is due to the different distortion of the monomer molecules and the different ring-opening rates between D3Et6 and D5Me10. Ring-opening requires relatively high reaction temperatures of 95-160°C, suitable anionic initiators, end-capping agents, additives, pressure-treated reactors, etc. Silicones usually undergo some degree of back-biting, resulting in the production of various (or fluctuating) amounts of cyclic siloxanes that can be difficult to remove from high-viscosity silicones. Additionally, hexaethylcyclosiloxane is known to preferentially polymerize with itself to form brittle regions in the crosslinked rubber, thus reducing the mechanical properties of the resulting material.
[0008] Another method for synthesizing polysiloxanes from monomeric silane precursors relies on the polycondensation of silane monomers or oligomers in the presence of a perfluoroarylborane catalyst such as B(C6F5)3 (Michael A. Brooks, JB Grande, F. Ganachaud, New Synthetic Strategies for Structured Silicones Using B(C6F5)3. Adv. Polym. Sci. 2011, 235, 161-183). One advantage of this method, known as the Piers-Rubinsztajn reaction, compared to ROP (which relies on cyclic monomers), is that it can be carried out at room temperature and produces much less cyclic products than high-temperature ROP syntheses. However, the main drawback of this method stems from the fact that it can be used to synthesize small amounts of silicones (mmol amounts), but is hardly usable for the synthesis of kg amounts of dimethyl-co-diethyl (1:1) polysiloxane. This is because such reactions are highly exothermic and generate large amounts of gaseous products (typically more than 100 liters of H2, CH4 or CH3-CH3 per kg of silicone). It is clear that any attempt to scale up this reaction would entail serious explosion hazards. Furthermore, another drawback of using the Piers-Rubinsztajn reaction is due to the fact that the borane catalyst must be dissolved in a solvent such as toluene (heptane causes precipitation of the catalyst) since water causes catalyst degradation. The viscosity of the solvent-free silicone synthesis is very simple since the viscosity of the polymer can be checked at any time by visual inspection or by a viscometer, whereas in organic solvents such as toluene, it can be difficult to monitor the progress of the reaction. Furthermore, depending on the structure of the silane precursor (i.e. -OH, -OCH3 or -OCH2CH3), the reaction temperature must be increased to polymerize the monomer. For example, the reaction of the -OCH3 group of dimethoxydimethylsilane with diethylsilane occurs at 22-23 °C, whereas the conversion of -OCH2CH3 to ethane in the presence of B(C6F5)3 requires 70 °C.
[0009] It is known from the prior art that the rate of hydrolysis of a silane depends on its electronic structure, the solvent used, the presence or absence of a catalyst, and the reaction temperature. For example, the hydrolysis of dichlorodimethylsilane in water occurs even at temperatures close to zero, whereas diethoxydimethylsilane is stable at 25° C. and its hydrolysis requires temperatures of 50° C. or higher and, finally, the presence of a suitable acid or base catalyst. Summary of the Invention
[0010] Applicants have discovered that a method of hydrolysis of diethyl / dimethyl / ethylmethylchlorosilanes at low temperatures (1-7°C) reproducibly produces silanol terminated poly(dimethyl-co-diethyl)siloxanes or polymethylethylsiloxanes with average molecular weights Mw-1000 (viscosity 33-36 mPa.s). In the presence of a suitable Lewis acid catalyst, these siloxanes can be conveniently polymerized to high molecular weight PDIES or PEMS (Mw-50000-100000) that have very low glass transition temperatures and do not undergo crystallization / melt transitions at low temperatures. This method does not require high reaction temperatures (above 100°C) and produces a relatively rapid viscosity increase (within minutes) with minimal (ppm) cyclic silicone by-products. The inventive method of PDIES / PEMS synthesis solves the problem of the formation of large amounts of gaseous products (H, methane or ethane) as experienced in the Piers-Rubinsztajn reaction, thus reducing the high exothermicity and explosion hazards as mentioned above.
[0011] Furthermore, another problem to be solved is the compatibility of the crosslinker with vinyl-terminated PDIES. Generally, phenyl-containing crosslinkers are required for crosslinking of phenyl silicones, because phase separation and increased foaming occurs when using classical methylhydrogenpolysiloxane crosslinkers (PHMS) or dimethyl-co-methylhydrogenpolysiloxane crosslinkers. The applicant has noticed a similar phenomenon in the case of dimethyl-co-diethylpolysiloxane. Extensive foaming was observed when vacuum was applied to PDIES / PHMS mixtures in the absence or presence of silica. To solve this crosslinker / diethyl silicone incompatibility problem, the applicant has synthesized a new type of methylhydrogen-co-diethylsiloxane crosslinker that has excellent compatibility with PDIES.
[0012] The present invention therefore relates to a method for the preparation of polysiloxanes containing methyl and ethyl groups, said method comprising the steps of: Step a) hydrolysis reaction of a silanol precursor; Step b) extending the chains of the silanol-terminated siloxane oligomers obtained in step a) by Lewis acid-induced polycondensation by adding a triflate salt catalyst, in particular In(III) triflate, followed by the addition of a perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane. Includes.
[0013] Advantageously, the polysiloxanes containing methyl and ethyl groups are selected from the group consisting of: poly(dimethyl-co-diethyl)siloxanes or poly(methylhydro-co-diethyl)siloxanes of formula (I): [ka] A represents a methyl group or a hydrogen atom; m and n represent the mole percentages of the repeat motifs -O-Si(Me)(A) and -O-Si(Et2), respectively; m=0.5 to 0.8, n=0.2 to 0.5, and m+n=1; p represents the number of both repeating motifs to obtain a weight average molecular weight in the range of 20000 g / mol to 150000 g / mol when A represents a methyl group, and in the range of 300 g / mol to 3500 g / mol when A represents a hydrogen atom. And, poly(ethylmethylsiloxane) of formula (II): [ka] q represents the number of repeat motifs.
[0014] More preferably, the silanol precursor in step a) is selected from among (R1)2 ethylmethylsilane, a mixture of (R1)2 dimethylsilane and (R1)2 diethylsilane, and a mixture of (R1)2 methylsilane and (R1)2 diethylsilane, where R1 represents a chlorine atom, a (C1-C6)alkoxy group (preferably a methoxy group or an ethoxy group), an acetoxy group or an oxime group, advantageously R1 represents a chlorine atom, a methoxy group or an ethoxy group, more preferably R1 represents a chlorine atom.
[0015] In the formulas of the present invention, Me is a methyl group and Et is an ethyl group.
[0016] In the present invention, the terms "included between x and y", "within the range of x to y", "=x to y", and "x to y" are intended to mean that the limits of the range, x and y, are included.
[0017] In the present invention, the term "(C1-C6)alkoxy group" is intended to mean any linear or branched saturated alkoxy group having from 1 to 6 carbon atoms, in particular the OCH3 (methoxy) group and the OCH2CH3 (ethoxy) group.
[0018] The process of the invention is therefore for the preparation of polysiloxanes containing methyl and ethyl groups, preferably poly(dimethyl-co-diethyl)siloxanes or poly(methylhydro-co-diethyl)siloxanes of formula (I) below: [ka] In this formula, A represents a methyl group or a hydrogen atom. m and n represent the mole percentages of the repeat motifs -O-Si(Me)(A) and -O-Si(Et2), respectively; m=0.5 to 0.8, n=0.2 to 0.5, and m+n=1; p represents the number of both repeat motifs to obtain a weight average molecular weight ranging from 20000 g / mol to 150000 g / mol when A represents a methyl group, and represents the number of both repeat motifs to obtain a weight average molecular weight ranging from 300 g / mol to 3500 g / mol when A represents a hydrogen atom. The weight average molecular weight of the polymer can be measured using viscometry (in accordance with ASTM E3116-18 standard of January 25, 2018), 1H NMR, and FTIR.
[0019] Advantageously, m=0.5 to 0.7, n=0.3 to 0.5, and m+m=1, more advantageously, m=0.5 to 0.6, n=0.4 to 0.5, and m+m=1, and even more advantageously, m=n=0.5.
[0020] Specifically, the poly(dimethyl-co-diethyl)siloxane of the present invention has the following formula Ia: [ka] where m, n, and p are as defined above.
[0021] The poly(dimethyl-co-diethyl)siloxanes of formula Ia according to the invention advantageously have a weight-average molecular weight, in particular using the viscometric method according to the ASTM E3116-18 standard of 25 January 2018, in the range of 20 000 g / mol to 150 000 g / mol, more advantageously between 30 000 g / mol to 100 000 g / mol, even more advantageously between 40 000 g / mol to 80 000 g / mol, in particular between 45 000 g / mol to 60 000 g / mol.
[0022] Specifically, the poly(methylhydro-c-diethyl)siloxane of the present invention has the following formula Ib: [ka] where m, n, and p are as defined above.
[0023] The poly(methylhydro-cо-diethyl)siloxanes of formula Ib according to the invention advantageously have a weight-average molecular weight, in particular using the viscometric method according to standard ASTM E3116-18 of 25 January 2018, in the range from 300 g / mol to 3500 g / mol, more advantageously between 500 g / mol and 3000 g / mol, even more advantageously between 1000 g / mol and 2000 g / mol.
[0024] The process of the present invention is also advantageously for preparing poly(ethylmethylsiloxanes) of formula (II): [ka] Here, q represents the number of repeat motifs.
[0025] Advantageously, the poly(ethylmethylsiloxanes) according to the invention have a weight-average molecular weight ranging from 1000 g / mol to 2,000,000 g / mol, in particular using the viscometric method according to standard ASTM E3116-18 of 25 January 2018.
[0026] Step a) in the process of the invention consists of a hydrolysis reaction of a silanol precursor.
[0027] Advantageously, the silanol precursor is selected from among (R1)2 ethylmethylsilane, a mixture of (R1)2 dimethylsilane and (R1)2 diethylsilane, and a mixture of (R1)2 methylsilane and (R1)2 diethylsilane, where R1 represents a chlorine atom, a (C1-C6)alkoxy (advantageously a methoxy or ethoxy group), an acetoxy group or an oxime group, advantageously R1 represents a chlorine atom, a methoxy group or an ethoxy group, more advantageously R1 represents a chlorine atom.
[0028] Thus, advantageously, the silanol precursors are chlorinated or ethoxylated silanol precursors, in particular chlorinated silanol precursors, more advantageously selected from dichloroethylmethylsilane, diethoxyethylmethylsilane, a mixture of dichlorodimethylsilane and dichlorodiethylsilane, a mixture of dichloromethylsilane and dichlorodiethylsilane, a mixture of diethoxydimethylsilane and diethoxydiethylsilane, and a mixture of diethoxymethylsilane and diethoxydiethylsilane, and more advantageously selected from dichloroethylmethylsilane, a mixture of dichlorodimethylsilane and dichlorodiethylsilane, and a mixture of dichloromethylsilane and dichlorodiethylsilane.
[0029] The product obtained after step a) is an oligomer of siloxanes containing methyl and ethyl groups, in particular (dimethyl-co-diethyl)siloxanes or (methylhydro-co-diethyl)siloxanes or ethylmethylsiloxanes, which advantageously have a weight-average molecular weight between 500 g / mol and 3000 g / mol, in particular using the viscometric method according to standard ASTM E3116-18 of 25 January 2018, and more advantageously a weight-average molecular weight between 1000 and 3000 g / mol when A is methyl.
[0030] Possible reaction schemes for step a) (schemes 1 and 2) are as follows: [ka] [ka] wherein A, m, and n are as defined above, and R1 represents a chlorine atom, a C1-C6 alkoxy group (e.g., a methoxy group or an ethoxy group), an acetoxy group, or an oxime group, preferably R1 represents a chlorine atom, a methoxy group, or an ethoxy group, and more preferably R1 represents a chlorine atom.
[0031] In an advantageous embodiment, step a) is carried out at a temperature between 0°C and 40°C, more advantageously at a temperature between 5°C and 35°C.
[0032] In an advantageous embodiment, the reaction is first carried out at a temperature between 0°C and 7°C, advantageously between 5°C and 7°C, followed by increasing the temperature to the range 30-40°C, advantageously 30-35°C.
[0033] More preferably, the reaction is carried out with stirring, and even more preferably, by adding the silanol precursor to the water, particularly dropwise, more preferably at a rate of 1 drop / sec to 5 drops / sec, particularly at a rate of 3 drops / sec.
[0034] In an advantageous embodiment, step a) lasts for 1 to 2 hours.
[0035] In an advantageous embodiment, the molar concentration of water (w) is higher than the molar concentrations of both silanol precursors (a+b): w>a+b
[0036] In a further embodiment, the oligomers obtained in step a) are separated from the HR1, in particular the HCl-containing aqueous phase obtained after carrying out step a), advantageously by heptane extraction, before being used in step b) of the process according to the invention.
[0037] Step b) in the process of the present invention consists in extending the chains of the silanol-terminated siloxane oligomers obtained in step a), advantageously poly(dimethyl-c-diethyl)siloxane oligomers or poly(methylhydro-c-diethyl)siloxane oligomers or ethylmethylsiloxa oligomers, by Lewis acid-induced polycondensation by adding a triflate salt catalyst followed by a perfluoroborane catalyst. Advantageously, the polymer obtained after step b) is a polymer of formula I or II as detailed above.
[0038] Advantageously, the triflate salt catalyst is selected from among In(III) triflate, Bi(III) triflate, Al(III) triflate, and mixtures thereof, and more advantageously, the triflate salt catalyst is In(III) triflate.
[0039] Advantageously, the perfluoroborane catalyst is tris(pentafluorophenyl)borane.
[0040] The reaction schemes (schemes 3 and 4) of step b) using In(III) triflate and perfluoroborane catalyst are as follows: [ka] where A, m, n, and p are as defined above. [ka] where q is as defined above.
[0041] The polymer of formula (I) is an alternating copolymer.
[0042] The polymer of formula (II) is a homopolymer.
[0043] Advantageously, step (b) is carried out at room temperature (20-25° C.).
[0044] In an advantageous embodiment: Firstly, a triflate salt catalyst, in particular In(III) triflate, is added with stirring (step b1), and then the reaction is allowed to proceed without stirring, advantageously for at least 1 to 12 hours. - A perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane, is then added with stirring (step b2), and the reaction is then left to proceed without stirring, advantageously for at least 1 to 12 hours.
[0045] Advantageously, step (b) is carried out in bulk without the use of a solvent.
[0046] In an advantageous embodiment, the triflate salt catalyst, specifically In(III) triflate, is present in an amount of 0.1 mg to 1 mg per gram of oligomer.
[0047] In another advantageous embodiment, the perfluoroborane catalyst, specifically tris(pentafluorophenyl)borane, is present in an amount of 0.1 mg to 1 mg per gram of oligomer.
[0048] In a particular embodiment, step b) is carried out under an inert atmosphere, advantageously under nitrogen.
[0049] The process of the invention may further comprise a step c1) of adding vinyl end groups by reaction of the polymer obtained in step b) with vinyldimethylmethoxysilane or vinyl-1,1,3,3-tetramethyldisiloxane in the presence of a Lewis acid catalyst such as In(III) triflate without a solvent or in toluene as solvent or without a solvent, at a temperature between 20 and 60° C., advantageously step c1) results in the formation of a polymer having formula (III): [ka] A, m, n and p are as defined in formula I; R2=-Si(CH3)2CH=CH2: or a polymer having formula (IV): [ka] q is as defined in formula II, R2=-Si(CH3)2CH=CH2: This is to obtain.
[0050] The polymer of formula (III) is an alternating copolymer.
[0051] The polymer of formula (IV) is a homopolymer.
[0052] Thus, the polymer obtained in step c1) is Poly(dimethyl-c-diethyl)siloxane having the formula (IIIa): [ka] R2, m, n and p are as defined in formula III. Or, Poly(methylhydro-c-diethyl)siloxane having the formula (IIIb): [ka] R2, m, n and p are as defined in formula III. It could be.
[0053] The polymers of formula (IIIa) and formula (IIIb) are alternating copolymers.
[0054] Advantageously, the poly(dimethyl-cо-diethyl)siloxane of formula (IIIa) has a glass transition temperature (Tg) in the range of −130° C. to −142° C., in particular in the range of −135° C. to −141° C., more particularly −139° C., measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014.
[0055] The polysiloxanes of formula (IIIa) more preferably have a weight-average molecular weight, in particular using the viscosity measurement method according to the ASTM E3116-18 standard of 25 January 2018, in the range from 20 000 g / mol to 150 000 g / mol, even more preferably between 30 000 g / mol and 100 000 g / mol, even more preferably between 40 000 g / mol and 80 000 g / mol, in particular between 45 000 g / mol and 50 000 g / mol.
[0056] Advantageously, the poly(methylhydro-cо-diethyl)siloxane of formula (IIIb) has a glass transition temperature (Tg) in the range of -130°C to -146°C, measured by DSC according to the ASTM E1356 standard of May 15, 2014.
[0057] The polysiloxanes of formula (IIIb) more preferably have a weight-average molecular weight, in particular using the viscosity measurement method according to the ASTM E3116-18 standard of 25 January 2018, in the range of 300 g / mol to 3500 g / mol, more preferably between 500 g / mol and 3000 g / mol, and even more preferably between 1000 g / mol and 2000 g / mol.
[0058] Advantageously, the poly(ethylmethylsiloxane) siloxane of formula (IV) has a glass transition temperature (Tg) in the range of -130°C to -142°C, measured by DSC according to the ASTM E1356 standard of May 15, 2014.
[0059] The polysiloxane of formula (IV) more advantageously has a weight-average molecular weight in the range of 20 000 g / mol to 200 000 g / mol, advantageously in the range of 20 000 g / mol to 150 000 g / mol, in particular using the viscosity measurement method according to the ASTM E3116-18 standard of 25 January 2018.
[0060] The reaction schemes of step c1) (schemes 5 and 6) are as follows: [ka] where R2, A, m, n and p are as defined above. [ka] where R2 and q are as defined above.
[0061] In a particular embodiment, the Lewis acid catalyst is a triflate salt, advantageously selected from among In(III) triflate, Bi(III) triflate, Al(III) triflate, and mixtures thereof, more advantageously In(III) triflate, step c1) is carried out without the use of a solvent, more advantageously at a temperature between 50° C. and 70° C., and even more advantageously the catalyst is present in an amount of 0.1 mg to 2 mg per gram of polymer.
[0062] In another particular embodiment, the Lewis acid catalyst is a perfluoroborane catalyst such as B(C6F5)3 and step c1) is carried out without a solvent or with toluene as solvent, more preferably at room temperature (20-25°C), and even more preferably the catalyst is present in an amount of 0.1 mg to 1 mg per gram of polymer.
[0063] In a more particular embodiment, the Lewis acid catalyst is a mixture of a triflate salt and perfluoroborane, advantageously a mixture of In(III) triflate and B(C6F5)3, step c1) is carried out without the use of a solvent, more advantageously at room temperature (20-25°C) and even more advantageously the catalyst is present in an amount of 0.1 mg to 1 mg per gram of polymer.
[0064] In a further particular embodiment, when step c1) is carried out, the catalyst used in step b) is not removed and perfluoroborane, specifically B(C6F5)3, is further added. Advantageously, step c1) is carried out without the use of a solvent and more advantageously at room temperature.
[0065] The process of the invention may comprise a step c2) of adding trialkylsilyl end groups by reaction of the polymer obtained in step b) with a trialkylsilane, in particular trimethylsilane or triethylsilane, more particularly triethylsilane, in the presence of a Lewis acid catalyst such as B(C6F5)3 in toluene as solvent, which step c2) advantageously gives a polymer having formula (V): [ka] A, m, n and p are as defined in formula I; Each R3 is independently a saturated, linear or branched C1-C6 alkyl group, preferably an ethyl group: or a polymer having formula (VI) [ka] q is as defined in formula II; Each R3 is independently a saturated, straight chain, or branched C1-C6 alkyl group: This is to obtain.
[0066] In the present invention, the term "(C1-C6) alkyl group" is intended to mean any linear or branched saturated alkyl group having from 1 to 6 carbon atoms, in particular the CH3 (methyl) group and the CH2CH3 (ethyl) group.
[0067] The polymer of formula (V) is a silicone oil and is an alternating copolymer. The polymer of formula (VI) is a silicone oil and is a homopolymer.
[0068] Advantageously, the poly(dimethyl-cо-diethyl)siloxane of formula (IVa) has a glass transition temperature (Tg) in the range of −130° C. to −145° C., in particular in the range of −135° C. to −142° C., more particularly −136° C., measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014.
[0069] More preferably, said siloxanes have a weight average molecular weight in the range of 40000 g / mol to 65000 g / mol, more preferably still between 45000 g / mol and 55000 g / mol, using the viscosity measurement method according to the ASTM E3116-18 standard of 25 January 2018.
[0070] Advantageously, the poly(ethylmethyl)siloxane of formula (VI) has a glass transition temperature (Tg) in the range of -130°C to -142°C, measured by DSC according to the ASTM E1356 standard of May 15, 2014.
[0071] More advantageously, said siloxanes have a weight average molecular weight in the range of 20000 g / mol to 150000 g / mol using the viscosity measurement method according to the ASTM E3116-18 standard of 25 January 2018.
[0072] The reaction schemes of step c2) (schemes 7 and 8) are as follows: [ka] where R3, A, m, n and p are as defined above. [ka] where R3 and q are as defined above.
[0073] In another particular embodiment, the Lewis acid catalyst is a perfluoroborane catalyst such as B(C6F5)3 and step c2) is carried out without a solvent or with toluene as solvent, more preferably at room temperature (20-25°C), and even more preferably the catalyst is present in an amount of 0.1 mg to 1 mg per gram of polymer.
[0074] In another particular embodiment, the process of the invention further comprises, after step c1) or c), a step d) of removing the catalyst used in steps b) and c1) or in step c), advantageously using aluminium oxide.
[0075] Advantageously, the process of the invention is for producing 50 / 50 poly(dimethyl-co-diethyl)siloxane or 50 / 50 poly(methylhydro-co-diethyl)siloxane.
[0076] The present invention also relates to a poly(dimethyl-co-diethyl)siloxane of formula (IIIa) as defined above, advantageously obtained by the process of the invention, and more advantageously having: a weight-average molecular weight, using the viscometric method according to the ASTM E3116-18 standard of 25 January 2018, in the range of 20 000 g / mоl to 150 000 g / mоl, more preferably between 30 000 g / mоl and 100 000 g / mоl, even more preferably between 40 000 g / mоl and 80 000 g / mоl, in particular between 45 000 g / mоl and 50 000 g / mоl, and / or a glass transition temperature, measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014, in the range of -130°C to -142°C, specifically in the range of -135°C to -141°C, more specifically -139°C.
[0077] The polymer of formula (IIIa) is an alternating copolymer.
[0078] The present invention also relates to a poly(methylhydro-c-diethyl)siloxane of formula (IIIb) as defined above, which is advantageously obtainable by the process of the invention and which more advantageously has: a weight-average molecular weight, using the viscometric method according to the ASTM E3116-18 standard of 25 January 2018, in the range of 300 g / mol to 3500 g / mol, more preferably between 500 g / mol and 3000 g / mol, even more preferably between 1000 g / mol and 2000 g / mol, and / or - The glass transition temperature, measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014, is within the range of -130°C to -146°C.
[0079] The polymer of formula (IIIb) is an alternating copolymer.
[0080] The present invention also relates to a poly(dimethyl-co-diethyl)siloxane of formula (V) as defined above, advantageously obtained by the process of the invention, and more advantageously having: - a weight-average molecular weight, using the viscometric method according to the ASTM E3116-18 standard of 25 January 2018, in the range of 500 g / mol to 150 000 g / mol, advantageously between 1000 g / mol and 3000 g / mol, and / or a glass transition temperature, measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014, in the range of -130°C to -145°C, specifically in the range of -135°C to -142°C, more specifically -139°C.
[0081] The polymer of formula (V) is an alternating copolymer.
[0082] The polymer of formula (V) is a silicone oil.
[0083] The present invention also relates to a composition for making silicone rubber, the composition comprising: - (A) 60 to 94% by weight of vinyl-terminated poly(dimethyl-co-diethyl)siloxane of formula (IIIa) according to the invention; - (B) a reinforcing filler, advantageously 5 to 35% by weight of pyrogenic silica; - (C) 1 to 5% by weight of a crosslinker having a Tg<-130°C, advantageously having formula (IIIb) according to the invention; - (D) a suitable amount of a curing catalyst, advantageously a Pt(0) catalyst such as platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane dissolved in methylvinylcyclosiloxane, and (E) optionally a Pt inhibitor such as 1-ethynyl-1-cyclohexanol
[0084] In this specification, the term "silicone rubber" is understood to mean a material capable of maintaining elasticity in the temperature range of 200 to -140°C.
[0085] The respective amounts of compound (A) (vinyl-terminated poly(dimethyl-c-diethyl)siloxane of formula (IIIa)) and compound (C) (crosslinker) in the composition of the present invention are determined by the ratio of the number of units (R'HSiO2 / 2) and the number of alkenyl groups, and are adjusted taking into account the relative proportion of alkenyl moieties in compound (A) and the relative proportion of units (R'HSiO2 / 2) in compound (C).
[0086] An essential feature of the silicone rubber composition of the present invention is the ratio between the number of units (R'HSiO2 / 2) in the compound (C) introduced into the silicone base composition and the number of diethyl groups in the compound (A) introduced into the rubber composition. According to the present invention, this ratio between the number of units (R'HSiO2 / 2) and the number of alkenyl groups is greater than 3. If the value of this ratio is less than or equal to 3, the composition will have insufficient mechanical and adhesive properties to be used as a self-adhesive PDIES silicone on metal surfaces such as stainless steel or titanium.
[0087] Advantageously, this ratio is greater than 4 and less than 25.
[0088] The curing catalyst is a hydrosilylation catalyst, specifically a platinum Pt(0) catalyst, more specifically complexed with a divinyltetraalkylsiloxane ligand, preferably 1,3-divinyltetramethylsiloxane, such as platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane dissolved in methylvinylcyclosiloxane. Such catalysts are described, for example, in document WO0142258A1. Karstedt's catalyst is most particularly suitable. As in conventional hydrosilylation reactions, the amount of catalyst in the composition is a catalytic amount. By catalytic amount is meant that the amount of platinum is less than 1 molar equivalent relative to the amount of olefinic double bond unsaturation present in the composition. In general, it is sufficient to introduce less than 1000 ppm, preferably more than 30 ppm, of platinum relative to the total mass of compound (A) and compound (C).
[0089] Reaction design of compound (C) (R'HSiO 2 / 2 ) and the hydrosilylation of the alkenyl groups of compound (A) results in crosslinking of the organopolysiloxane to produce a crosslinked silicone rubber composition. Crosslinking is typically initiated by subjecting the silicone rubber composition to a temperature sufficient to cause the hydrosilylation reaction. Crosslinking is typically carried out at temperatures between 15°C and 200°C, for example between 20°C and 150°C, and more preferably between 50°C and 150°C.
[0090] In known methods, the crosslinkable silicone composition generally comprises an inhibitor. Inhibitors are generally used to control the temperature and time of the hydrosilylation crosslinking reaction, thereby further controlling the crosslinking reaction, in particular its initiation and speed. When a crosslinking inhibitor is used, the amount of inhibitor used is preferably 1 to 50,000 ppm, more preferably 20 to 2000 ppm, in particular 100 to 1000 ppm, based on the total mass of compound (A) and compound (C). Inhibitors include acetylene alcohols, such as 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-dodecyn-3-ol, 2-phenyl-3-butyn-2-ol. Preferably, the silicone rubber composition in the present invention comprises an inhibitor.
[0091] The silicone rubber composition according to the invention also has the essential feature of containing a reinforcing filler, advantageously a hydrophobic silica, in particular a pyrogenic silica. In a known manner, the hydrophobic silica is a silica part of whose surface is covered with an organic group, such as an alkyl group. The silica may be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenic silica. Preferably, the silica is 450 ml 2 / g, preferably 80 to 400m 2 / g, particularly preferably 100 to 300m 2 / g, advantageously from 150 to 250 m 2 / g. It is also possible to use mixtures of silicas, such as, for example, Aerosil R 8200, Aerosil R 812 S, Aerosil E 9200 from Evonik or Cab-O-Sil TS 530 from Cabot.
[0092] It is well known that the surface of silica is modified to make it hydrophobic. The surface modification of silica can be achieved in a known manner by reacting silica with a compound having a hydrophobic group, such as a trialkylsilyl group, in particular a trimethylsilyl group. Particularly suitable is silica surface-modified with trimethylsilyl groups. For example, silica modified with hexamethyldisilazane can be mentioned.
[0093] The content of hydrophobic silica is adjusted by those skilled in the art according to its specific surface area and the application of the silicone rubber composition.Preferably, the content of hydrophobic silica in the silicone rubber composition is 5% or more and 35% or less of the total weight of silica, compound (A) and compound (C).Below 5% of the total weight of silica, compound (A) and compound (C), the reinforcing properties of the composition may be insufficient for certain applications.Beyond 35% of the total weight of silica, compound (A) and compound (C), compounding of silicone rubber may be impossible (solid paste obtained when using Wacker silica HDK H2000 or when using more than 20% by weight of Cab-O-Sil TS 530, Aerosil R 8200 or Aerosil E 9200).
[0094] The silicone rubber composition according to the present invention can be prepared by compounding the hydrophobic silica with compound (A), then adding compound (C) with mixing, and finally adding the catalyst. If an inhibitor is used, it is usually added to the mixture of hydrophobic silica and compound (A) before compounding with compound (C).
[0095] The present invention also relates to a silicone rubber obtainable by curing a composition according to the invention, which, as described above, has a glass transition temperature in the range of -130°C to -142°C, advantageously in the range of -135°C to -140°C, in particular -138°C, measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014, and / or does not have a crystallization / melt transition in the range of -140°C to +250°C, measured by DSC in accordance with the ASTM E1356 standard of May 15, 2014.
[0096] More advantageously, the silicone rubber according to the invention has an elongation at break (measured with an INSTRON 34TM-10, France, using the AFNOR NF T 46002 standard, H2, September 1988) of 100% or more, in particular 200% or more, more particularly 300% or more, for example 348%.
[0097] Furthermore, the silicone rubber according to the invention preferably has an elastic modulus, measured according to the French INSTRON 34TM-10 according to the AFNOR NF T 46002 standard of September 1988, of >1 MPa, preferably >3 MPa.
[0098] More preferably, the silicone rubber according to the invention has a Shore A durometer hardness measured in accordance with the ASTM D2240 standard of July 23, 2021 in the range of 35 to 40.
[0099] The present invention also relates to the use of the silicone rubber or poly(dimethyl-co-diethyl)siloxane of formula (V) according to the present invention in the aerospace industry, in particular in space probes. More specifically, the present invention also relates to the use of the poly(dimethyl-co-diethyl)siloxane of formula (V) according to the present invention as a silicone oil for electric motors at low temperatures, in particular below -100°C.
[0100] The invention finally relates to the use of poly(methylhydro-co-diethyl)siloxanes having formula (IIIb) according to the invention as crosslinkers for preparing silicone rubbers.
[0101] The aforementioned and other features of the invention will be better understood on reading the following description of some exemplary embodiments of the invention, given by way of illustration and without limitation. EXAMPLES
[0102] [Example 1: Synthesis of poly(diethyl-co-dimethyl)siloxane (50 / 50) (PDIES-50 / 50)] <Process 1 (Process a)> First, 1 kg of dichlorodiethylsilane (SID3402.0-1KG, Gelest, USA) was distilled at 40-50°C / vacuum degree 20 mbar into a 2 L flask cooled to -79°C using dry ice. The obtained silane was a transparent liquid.
[0103] The synthesis of poly(diethyl-cо-dimethyl)siloxane (50 / 50) was carried out without prior removal of oxygen from the water. An 8 L glass cylinder was placed in an ice bath (polypropylene box) and cooled to 0-5 °C. The reactor was fitted with a bubbler to check eventual gas evolution. Deionized water (3.7 L) was added to the glass reactor, cooled to 5 °C in an ice bath. Agitation was set at 200 rpm. Then, 306 g of diethyldichlorosilane and 251.37 g of dichlorodimethylsilane (ThermoScientific, lot A0439125) were added to a glass column equipped with a Teflon valve (the glass was dried at 100 °C under vacuum and kept under a slight N2 flow). The silanes were mixed with a Teflon bar and dripped into the 3.7 L water at a rate of about 3 drops per second. The temperature of the reaction was maintained at 5-7 °C. Silane hydrolysis was carried out at 300 rpm for 2 hours.
[0104] The reactor was then placed in a polypropylene water bath heated to 40°C, and the temperature of the reaction mixture was adjusted to 30-35°C. The silanol was stirred at 300 rpm for an additional 2 hours. Then, 1.5 L of heptane was added to separate the silanol from the aqueous phase, and a HCl(aq) solution was pumped below the silanol oligomer layer using a silicon tube (slight vacuum). The silanol oligomer was extracted with 1 L of heptane, and the reactor and separatory funnel (500 ml funnel) were washed with an additional 1.5 L of heptane. The silanol oligomer was dried by adding 25 g of MgSO4 and stirring at 200 rpm. The wet MgSO4 was filtered, and the silanol oligomer was kept overnight in 2 L of heptane under nitrogen. The organic solvent was removed using a rotary evaporator at 90°C under vacuum. 313.2 g of silanol oligomer was obtained (theoretical value 369.4 g), the yield was 85%. Viscosity according to the ASTM E3116-18 standard of January 25, 2018: 35 mPa.s (Viscosimeter Model: VSC-N4 (Bioevopeak, China) Measurement range: 20-2,000,000 mPa.s).
[0105] The silanol was placed in a 2 L glass flask and heated to 145° C. for 120 min (air, no vacuum). After 2 h at 145° C., it was cooled to 25° C. (thermostat) and the viscosity was measured. The viscosity was 38 mPa.s. The silanol was purged with nitrogen, sealed in a 1 L container with a silicone septum and stored at −20° C. (to prevent further condensation with water).
[0106] <Process 2 (Process b)> 298 g of silanol oligomer obtained in step 1 was heated at 145°C for 15 min and exposed to vacuum (vacuum < 2 mbar) while hot for 30 min until no more bubbles were observed to form. The silanol oligomer was then poured hot into a dry 1 L flask equipped with a silicon septum, magnetic stirrer and nitrogen flow. Subsequently, 35 mg of indium(III) triflate per 100 g of silanol oligomer was added under nitrogen flow. The catalyst was dispersed in the silanol oligomer by stirring at 500 rpm. The reaction was then allowed to proceed overnight (17 h) in a closed vessel without stirring. An increase in viscosity was observed. The next day, 57 mg of tris(pentafluorophenyl)borane catalyst (Sigma-Aldrich, #442593) was added under nitrogen, mixed at 500 rpm for 5 min and the reaction was allowed to proceed for another 24 h.
[0107] <Process 3 (Process c)> 35 mg of tris(pentafluorophenyl)borane catalyst (Sigma-Aldrich, #442593) was added to the reaction, followed by 1.5 ml of vinyldimethylmethoxysilane (AB106075, ABCR-Germany). The reaction was stirred for 5 minutes and then allowed to continue for an additional 5 hours without stirring. Finally, the reaction product was transferred to a rotary evaporator and the excess vinyldimethylmethoxysilane and other volatiles were removed at 95°C / 30 mbar vacuum.
[0108] <Step 4. Catalyst removal (step d)> The siloxane polymer obtained in step 3 was cooled to room temperature and 150 g of neutral aluminum oxide (#199974, Sigma Aldrich) was added along with 600 ml of heptane. The suspension was stirred at 300 rpm for 20 minutes. The solids were then removed by filtration through a ceramic filter porosity 2, then porosity 4, and finally a 0.45 um PTFE filter. The solvent was removed using a rotary evaporator by heating to 95°C and reducing the vacuum to 30 mbar. Finally, the siloxane polymer was heated at 150°C for 1 hour under a vacuum of <1 mbar (vacuum oven). No significant mass loss was measured by DSC between -80 and 200°C.
[0109] According to ASTM E3116-18 standard on January 25, 2018, Viscosity: 4012 mPa.s, Mw=45000 g / mоl (Viscosimeter Model: VSC-N4 (Bioevopeak, China) Measuring range: 20~2,000,000 mPa.s).
[0110] DSC of this material according to the ASTM E1356 standard of May 15, 2014 showed Tg = -139 °C (2 °C / min, N2) (Model: DSC 3, Mettler Toledo, Switzerland).
[0111] The polydispersity index (PD) by GPC was 1.63.
[0112] The GPC conditions are as follows: GPC (gel permeation chromatography): Agilent 1260 Infinity connected to a 390-MDS detector (Agilent, USA) Refractive index detector: 1260 Infinity RID (Agilent, USA) The heating unit is a Mistral column oven (Spark, Netherland). Column set consists of: 1x Precolumn PSS SDV (PSS / Agilent) 2x columns: Linear XL for PSS SDV analysis (PSS / Agilent) The polymer samples were dissolved in 1 mL of toluene before injection. Toluene, HPLC Plus, for HPLC (#650579-1L, Merck) Test conditions: - Eluent: toluene - Flow rate: 1mL / min - Temperature: 35℃
[0113] The calibration was a conventional calibration of polystyrene narrow band standards ranging from 682 to 130,000 g / mol.
[0114] The software used for Mw calculation was Cirrus GPC Software (Agilent, USA).
[0115] Example 2: Silicone compounding example for the manufacture of silicone rubber 50g Mw45 500g / mol siloxane polymer (synthesized in steps 1 to 4 above) 15g SiO2 (HDK H2000, Wacker Germany) 7g 1-ethynyl-1-cyclohexanol, 99% (E51406, Sigma-Aldrich) (Pt inhibitor) 140mg Pt catalyst* (Platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane complex solution (Sigma Aldrich, #479543) 1.35g HMS-H271 crosslinker (Gelest, USA) (25-30% methylhydro)-dimethylsiloxane copolymer, hydride terminated, 24-60cSt)
[0116] The components were mixed using a mixer at 2000 rpm and cured at 150°C / 1 hour or at room temperature for 24 hours.
[0117] The elastic cross-linked silicone rubber (30 wt% SiO2) has a Tg = -138 °C and showed no crystallization or melting between -150 and +250 °C measured by DSC (Model: DSC 3, Mettler Toledo, Switzerland) according to the ASTM E1356 standard of May 15, 2014. Shore A hardness: 35-40 (measured using HBA100-0 (Kern, Switzerland) according to the ASTM D2240-15 standard of July 23, 2021). Elongation at break: 348% (measured using INSTRON 34TM-10, France, using H2, AFNOR NF T 46002 standard, September 1988).
[0118] [Example 3: Triethylsilyl-terminated poly(dimethyl-co-diethyl)siloxane (50 / 50) silicone oil] Step (a): Hydrolysis A 1 L flask equipped with four inlets, a condenser, a side arm, a vent outlet, and a magnetic stirrer was filled with 370 ml of deionized water. The apparatus was then cooled to 5°C and 30.0 g of dichlorodiethylsilane (Gelest, SID3402.0, Gelest) and 24.6 g of dichlorodimethylsilane (ThermoScientific, #113312500), both cooled to 5°C and mixed, were added dropwise (at a rate of 3 drops per second) over 1 hour. The reaction was stirred at 600 rpm. The reaction temperature was then increased to 30°C and stirred for an additional hour. 500 ml of heptane was added and the silicone was separated from the aqueous phase in a separatory funnel. The organic phase was washed with deionized water until the pH was neutral.
[0119] The reaction product in heptane was transferred to a 1 L flask and the remaining water was dried using 50 g of anhydrous MgSO4. The product was filtered using a high porosity P4 ceramic filter and a 0.45 um PTFE microfilter. Heptane and volatiles were removed using a rotary evaporator at 90°C / vacuum up to 18 mbar. Further vacuum to 1 mbar at room temperature showed no volatiles.
[0120] Step (b): Chain extension The product was transferred to a dry 100 ml round bottom flask equipped with a magnetic stirrer under nitrogen flow. 14 mg of In(III) triflate was then added and stirred for 30 minutes. This was followed by the addition of 14 mg of tris(pentafluorophenyl)borane catalyst (Sigma-Aldrich, #442593) dissolved in 2 ml of anhydrous toluene (Sigma Aldrich, #244511). The reaction was stirred for an additional 30 minutes.
[0121] Process (c2): Finally, 5 ml of triethylsilane (Sigma 230197-25G) and 6.5 mg of tris(pentafluorophenyl)borane were dissolved in 1 ml of toluene. The solution was stirred for 30 min until the foaming ceased. The catalyst was adsorbed on 25 g of neutral Al2O3 with constant stirring at 400 rpm. After stirring the reaction for 10 min, 200 ml of heptane was added and the suspension was filtered through ceramic P2 and P4 filters and then through a 0.45 um PTFE microfilter. The solvent was distilled off at 90°C / vacuum 20 mbar, followed by vacuum <1 mbar at room temperature. The product was characterized by FTIR and Raman spectroscopy. The glass transition Tg=-140°C was measured by DSC under nitrogen flow at a rate of 2°C / min.
[0122] [Example 4: Triethylsilyl-terminated poly(methylhydro-co-diethyl)siloxane (50 / 50) silicone oil (crosslinker)] Step a): Hydrolysis A 1 L flask equipped with four inlets, a condenser, a side arm, a vent outlet, and a magnetic stirrer was purged with a slight nitrogen flow at 25° C. Then, 22 g of diethyldiethoxysilane (Gelest, SID3404) and 16.8 g of methyldiethoxysilane (Sigma-Aldrich, #66612) were added with constant stirring at 400 rpm.
[0123] Steps b) and c1) Finally, 7.5 mg of In(III) triflate catalyst was added directly to the monomer mixture using a Pasteur pipette, followed by the addition of 11 ml of deionized water by pipette at 10 min intervals (3 x 3 ml + 2 ml) while stirring at 29 °C and 400 rpm. After 1 h of stirring, the reaction product was transferred to a 250 ml flask and 25 g of anhydrous MgSO4 was added to dry the water. The product was dissolved in 100 ml of heptane, filtered using a 0.45 um PTFE filter, and volatiles / solvents were removed using a rotary evaporator at 80 °C / vacuum up to 35 mbar. Further reduction in vacuum to 1 mbar at room temperature showed no volatiles.
[0124] To the reaction product obtained in the previous step, 4 mg of tris(pentafluorophenyl)borane catalyst (Sigma-Aldrich, #442593) dissolved in 1 ml of anhydrous toluene (Sigma Aldrich, #244511) and 5 ml of triethylsilane (Sigma 230197-25G) were added under N2 flow and constant stirring at 400 rpm. The solution was stirred for 30 minutes until the generation of bubbles ceased. The borane catalyst was adsorbed on 25 g of neutral Al2O3. After stirring the reaction solution for 10 minutes (magnetic Teflon stir bar), 100 ml of heptane was added and the suspension was filtered through ceramic P2 and P4 filters, followed by a 0.45 um PTFE microfilter. The solvent was evaporated at 90°C / vacuum 20 mbar and vacuum <1 mbar was applied at room temperature. The product (clear liquid) was characterized by FTIR and Raman spectroscopy. The glass transition Tg = -144.7°C was measured by DSC at a rate of 2°C / min under nitrogen flow.
[0125] [Example 5: Synthesis of poly(ethyl-c-methylsiloxane)-PEMS] Step a (hydrolysis) Ethylmethyldichlorosilane (#AB111135, ABCR Germany) was used as received (97% purity) and appeared as a clear pink liquid.
[0126] The synthesis was carried out in an air atmosphere. A 20 L glass reactor was cooled to 5 °C. A 1 L side arm used for the dropwise addition of the silanes was equipped with a bubbler and maintained under a slight nitrogen flow during the silane addition. Deionized water (1.4 L) was cooled and maintained at 4-6 °C during the chlorosilane addition. Agitation was set at 200 rpm. First, 213.0 g (instead of 210 g) of ethylmethyldichlorosilane was added dropwise (3 drops per second) to 1.4 L of water. The temperature of the reaction solution was then gradually increased to 30 °C and stirred at 200 rpm for 2 h 30 min. A transparent silanol layer was formed on the water surface.
[0127] The silanol was extracted with 1.25 L of heptane and dried with 250 g of MgSO4. The heptane was distilled off using a rotary evaporator at 90-95 °C, and then further vacuumed to 1 mbar at room temperature. The viscosity of the resulting silanol was 31.7 mPa.s. The silanol in a 1 L round-bottom flask was then placed in an oven at 145 °C for 20 minutes. The silanol was allowed to cool to room temperature. Subsequently, 100 mg of indium (III) triflate was added with constant stirring at 200 rpm. The silanol was then polymerized over the weekend. 115.0 g of silicone was obtained (theoretical value 131.83 g), a yield of 87%.
[0128] Step b (chain extension) 50 g of the PEMS silanol obtained in step a) was mixed with 50 mg of In(III) triflate (#422151, Sigma-Aldrich), stirred for 5 min at 200 rpm and then polymerized over the weekend (without stirring). The silicone was then stripped of water and volatiles using a rotary evaporator at 95°C under 30 mbar vacuum. The silanol was then mixed with 125 g of anhydrous MgSO4 and dissolved in 400 ml of heptane. The solid was filtered through a P4 ceramic filter and the heptane was distilled off at 95°C. The silanol was heated at 145°C for 10 min under 1 mbar vacuum. The silanol was then cooled to room temperature and 25 mg of tris(pentafluorophenyl)borane was added followed by 2 ml of toluene, mixed for 2 min and kept in a 1 L flask sealed with a silicon septum under N2 atmosphere (without stirring). The silanol was left to polymerize overnight.
[0129] Process c1 The silanol obtained in step b was heated to 95°C under 25 mbar vacuum to remove water and volatiles. Then, 0.33 g of vinyl-1,1,3,3-tetramethyldisiloxane 98% (SIV9097.5, Gelest, USA) and 25 mg of tris(pentafluorophenyl)borane 95% (#442593, Sigma Aldrich) were added, followed by 2 ml of toluene. The silicone was mixed for 5 minutes at 200 rpm and reacted for 2 hours at 25°C. Finally, a vacuum line was connected to distill off the volatiles at 95°C and 30 mbar vacuum. The silicone was diluted with 200 ml of hexane and mixed with 25 g of Al2O3 (neutral alumina) and the suspension was stirred for 10 minutes. The catalyst adsorbed on the alumina was removed by filtration through a ceramic P4 filter and then through a 0.45 um PTFE microfilter. The solvent was removed using a rotary evaporator at 95° C. and the polymer was transferred to a dry 250 ml glass flask and subjected to 150° C. and then 170° C. (20 min each) under a vacuum of 1 mbar. The viscosity was 5500 mPa.s.
[0130] The resulting material was analyzed by DSC. Tg = -141 °C under N2 at 2 °C / min was measured. FTIR and Raman measurements showed the absence of cyclic products. The FTIR and Raman spectra of the product matched the PEMS spectrum calculated with B3LYP / 6-311G (d,p) level) (Gaussian16).
[0131] According to ASTM E3116-18 standard of 25 January 2018 Viscosity: 25 mPa.s, Mw=2000 g / mоl (Viscosimeter Model: VSC-N4 (Bioevopeak, China) - Measurement range: 20~2,000,000 mPa.s).
[0132] The polydispersity index (PD) by GPC was 2.41. The GPC conditions were the same as in Example 1.
[0133] Crosslinking: 5 g PEMS silicone (step c1), 1.5 g SiO2 (HDK H2000), 14 mg Pt(0) tetravinylcyclotetrasiloxane (Sigma Aldrich, #479543), 135 mg HMS H271 (Gelest, USA) at 35 °C / overnight, then 150 °C for 20 min.
[0134] The elastic crosslinked silicone rubber had a Tg of -139°C, and did not crystallize or melt at temperatures between -139 and +250°C.
[0135] No crystallization of silicone was observed from +25 to -130°C at 2°C / min under N2 atmosphere.
Claims
1. Step a) hydrolysis reaction of a silanol precursor; Step b) extending the chains of the silanol-terminated siloxane oligomers obtained in step a) by Lewis acid-induced polycondensation by adding a triflate salt catalyst, in particular In(III) triflate, followed by addition of a perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane. Including, A method for producing polysiloxanes containing methyl and ethyl groups.
2. The polysiloxane containing methyl and ethyl groups is poly(dimethyl-co-diethyl)siloxanes or poly(methylhydro-co-diethyl)siloxanes of formula (I): 【Chemistry 1】 A represents a methyl group or a hydrogen atom; m and n are the repeating motifs -O-Si(Me)(A) and -O-Si(Et 2 ) in mole percent, m=0.5 to 0.8, n=0.2 to 0.5, and m+n=1; p represents the number of both repeating motifs to obtain a weight average molecular weight in the range of 20,000 g / mol to 150,000 g / mol when A represents a methyl group, and to obtain a weight average molecular weight in the range of 300 g / mol to 3500 g / mol when A represents a hydrogen atom. And, a poly(ethylmethylsiloxane) of formula (II): 【Chemistry 2】 q represents the number of repeat motifs Characterized in that it is selected from the group consisting of 2. The method of claim 1.
3. The silanol precursor of step a) is (R1) 2 Ethylmethylsilane, (R1) 2 Dimethylsilane and (R1) 2 A mixture of diethylsilane and (R1) 2 Methylsilane and (R1) 2 and a mixture of diethylsilane, wherein R1 is a chlorine atom, (C 1 -C 6 ) an alkoxy group, an acetoxy group or an oxime group, and preferably R1 represents a chlorine atom, a methoxy group or an ethoxy group; The method of claim 2.
4. the In(III) triflate catalyst is present in an amount of 0.1 mg to 1 mg per gram of oligomer; 4. The method according to any one of claims 1 to 3.
5. Step b) is carried out at room temperature.
5. The method according to any one of claims 1 to 4.
6. characterised in that step b) is carried out in bulk without the use of a solvent, 6. The method according to any one of claims 1 to 5.
7. the poly(dimethyl-co-diethyl)siloxane obtained in step b) has a weight average molecular weight ranging from 20,000 g / mol to 150,000 g / mol; - the poly(methylhydro-co-diethyl)siloxane obtained in step b) has a weight average molecular weight in the range of 300 g / mol to 3500 g / mol; and said poly(ethylmethylsiloxane) obtained in step b) has a weight average molecular weight in the range of 1000 g / mol to 200000 g / mol; Characterized in that 7. The method according to any one of claims 2 to 6.
8. In(III) triflate without solvent or in toluene as solvent or without solvent B(C 6 F 5 ) 3 , or In(III) triflate and B(C 6 F 5 ) 3 and a step c1) of adding vinyl end groups by reaction of the polymer obtained in step b) with vinyldimethylmethoxysilane or vinyl-1,1,3,3-tetramethyldisiloxane in the presence of a Lewis acid catalyst such as a mixture of Advantageously, step c1) is a polymer having formula (III) 【Chemistry 3】 A, m, n and p are as defined in formula I; R 2 =-Si(CH 3 ) 2 CH=CH 2 : or a polymer having formula (IV) 【Chemistry 4】 q is as defined in Formula II; R 2 =-Si(CH 3 ) 2 CH=CH 2 : The purpose of the present invention is to obtain 8. The method according to any one of claims 1 to 7.
9. the poly(dimethyl-co-diethyl)siloxane obtained in step c1) has a glass transition temperature in the range of −130° C. to −142° C., - the poly(methylhydro-co-diethyl)siloxane obtained in step c1) has a glass transition temperature in the range of -130°C to -146°C, and - the poly(ethylmethylsiloxane) obtained in step c1) has a glass transition temperature in the range of -130°C to -142°C, The method according to claim 8.
10. B in toluene as solvent (C 6 F 5 ) 3 and a step c2) of adding trialkylsilyl end groups by reaction of the polymer obtained in step b) with a trialkylsilane in the presence of a Lewis acid catalyst such as Advantageously, step c2) is A polymer having the following formula (V): 【Chemistry 5】 A, m, n and p are as defined in formula I; Each R 3 are each independently saturated, linear, or branched C 1 -C 6 is an alkyl group: or a polymer having formula (VI) 【Chemistry 6】 q is as defined in formula II; Each R 3 are each independently saturated, linear, or branched C 1 -C 6 is an alkyl group: The purpose of the present invention is to obtain 8. The method according to any one of claims 1 to 7.
11. 1. A method for producing 50 / 50 poly(dimethyl-co-diethyl)siloxane or 50 / 50 poly(methylhydro-co-diethyl)siloxane, 11. The method according to any one of claims 2 to 10.
12. of formula (IIIa): R 2 , m, n and p are as defined in formula III. a weight average molecular weight in the range of 20,000 g / mol to 150,000 g / mol, and - Glass transition temperature in the range of -130°C to -142°C having Advantageously, it can be obtained by a method according to any one of claims 8, 9 and 11, Poly(dimethyl-co-diethyl)siloxane.
13. of formula (IIIb): R 2 , m, n and p are as defined in formula III; a weight average molecular weight in the range of 300 g / mol to 3500 g / mol, and - Glass transition temperature in the range of -130°C to -146°C having Advantageously, it can be obtained by a method according to any one of claims 8, 9 and 11, Poly(methylhydro-co-diethyl)siloxane.
14. - the following formula (V): R 3 , A, m, n and p are as defined in claim 10. a weight average molecular weight in the range of 500 g / mol to 150,000 g / mol, and - Glass transition temperature in the range of -130°C to -145°C having Advantageously, it can be obtained by a method according to any one of claims 10 and 11, Poly(dimethyl-co-diethyl)siloxane.
15. - (A) 60 to 94% by weight of vinyl-terminated poly(dimethyl-co-diethyl)siloxane of formula (IIIa) according to claim 12; (B): reinforcing filler, preferably 5 to 35% by weight of pyrogenic silica; - 1 to 5% by weight of (C) a crosslinker having a Tg<-130°C, preferably having the formula (IIIb) according to claim 13; (D): a suitable amount of a curing catalyst, preferably a Pt(0) catalyst such as platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane dissolved in methylvinylcyclosiloxane, and (E): optionally an inhibitor such as 1-ethynyl-1-cyclohexanol; Including, A composition for making silicone rubber.
16. obtainable by curing the composition according to claim 15, and It has a glass transition temperature in the range of -130°C to -142°C, does not have a crystallization / melting transition in the range of -140°C to +250°C, and has an elongation at break of greater than 100%. Silicone rubber.
17. Use of the silicone rubber according to claim 15 or the poly(dimethyl-co-diethyl)siloxane of formula (V) according to claim 14 in the aerospace industry, in particular in space probes.
18. 14. Use of poly(methylhydro-co-diethyl)siloxane having formula (IIIb) according to claim 13 as a crosslinking agent for the preparation of silicone rubber.
Citation Information
Patent Citations
Thermosetting organopolysiloxane composition
JP1981049754A
Elastomer stable at low temperature and preparation thereof
JP1994287304A
Curable organopolysiloxane composition, its cured product and integrated product with substrate
JP2000345046A
Polysiloxane and method for producing the same
JP2006143882A
Method for the condensation polymerization of hydroxyl-terminated polydiorganosiloxanes