Pellicle and pellicle assembly
The pellicle assembly with three-dimensional structures, adhesive borders, and controlled thermal expansion materials addresses contamination and stress issues in EUV lithography, enhancing reliability and pattern quality.
Patent Information
- Application Number
- JP2024113899
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-09-12
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2038-06-08
AI Technical Summary
Existing pellicles in EUV lithographic apparatuses face challenges due to the reflective nature of patterning devices, vacuum environment, and the need for effective particle contamination protection, which are not adequately addressed by conventional pellicle designs.
A pellicle assembly with three-dimensional expansion structures, adhesive borders, actuators for space control, and materials with controlled thermal expansion coefficients to manage stress and contamination, along with a tracking device for monitoring pellicle condition.
Enhances pellicle lifespan and reliability by managing stress, reducing contamination, and providing real-time monitoring, thus maintaining pattern integrity in EUV lithography.
Smart Images

Figure 2024150564000001_ABST
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS)
[0001] This application claims priority to European Application No. 17176205.7 filed June 15, 2017, and European Application No. 17190503.7 filed September 12, 2017, which applications are incorporated by reference in their entireties into this specification.
[0002]
[0002] The present invention relates to a pellicle and a pellicle assembly. The pellicle assembly may comprise a pellicle and a frame supporting the pellicle. The pellicle may be suitable for use with a patterning device of a lithographic apparatus. The present invention finds particular, but not exclusive, use in connection with EUV lithographic apparatus and tools. [Background technology]
[0003]
[0003] A lithographic apparatus is a machine configured to apply a desired pattern onto a substrate. Lithographic apparatus can be used, for example, in the manufacture of integrated circuits (ICs). A lithographic apparatus can, for example, project a pattern from a patterning device (e.g. mask) onto a layer of radiation-sensitive material (resist) provided on the substrate.
[0004]
[0004] The wavelength of radiation used by a lithographic apparatus to project a pattern onto a substrate determines the minimum size of features that can be formed on the substrate. To form smaller features on a substrate than conventional lithographic apparatus (which may use electromagnetic radiation having a wavelength of, for example, 193 nm), lithographic apparatus using EUV radiation, which is electromagnetic radiation having a wavelength in the range of 4-20 nm, may be used.
[0005]
[0005] In a lithographic apparatus, a patterning device may be used to impart a pattern to a radiation beam. The patterning device may be protected from particle contamination by a pellicle. The pellicle may be supported by a pellicle frame.
[0006]
[0006] The use of pellicles in lithography is well known and established. A typical pellicle in a DUV lithography apparatus is a membrane located away from the patterning device and out of the focal plane of the lithography apparatus in use. Because the pellicle is out of the focal plane of the lithography apparatus, contamination particles that land on the pellicle are out of focus of the lithography apparatus. Therefore, images of the contamination particles are not projected onto the substrate. Without the presence of a pellicle, contamination particles that land on the patterning device would be projected onto the substrate and introduce defects into the projected pattern.
[0007]
[0007] It would be desirable to use a pellicle in an EUV lithography apparatus. EUV lithography differs from DUV lithography in that it is typically performed in a vacuum and the patterning device is generally reflective rather than transmissive.
[0008]
[0008] It would be desirable to provide a pellicle and / or pellicle assembly that overcomes or mitigates one or more problems associated with the prior art. Embodiments of the invention described herein may be used in an EUV lithography apparatus. Embodiments of the invention may also be used in a DUV lithography apparatus or another form of lithography apparatus. Summary of the Invention
[0009] According to a first aspect described herein, there is provided a pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, the pellicle assembly further comprising one or more three-dimensional expansion structures that enable the pellicle to expand under stress.
[0010]
[0010] This can improve the life and reliability of the pellicle assembly.
[0011] At least one of the three-dimensional extended structures may be formed in a pellicle frame and thereby applied to the pellicle. For example, the three-dimensional extended structure may also be applied to the pellicle by forming the three-dimensional extended structure in a pellicle frame and depositing the pellicle on the pellicle frame.
[0012]
[0012] At least one of the three-dimensional expanding structures may form a spring. For example, the spring may comprise at least one V-shaped configuration formed within the pellicle frame. At least one of the structures may comprise a plurality of springs formed within the pellicle frame and arranged around a central portion of the pellicle. The central portion of the pellicle is the portion of the pellicle that is not in direct contact with the frame. In this way, the stress within the pellicle may be more precisely controlled. At least one of the springs may be a leaf spring.
[0013]
[0013] At least one of the three-dimensional extended structures may be present in the center of the pellicle.
[0014]
[0014] The frame may include a substrate, and the pellicle assembly may include at least one spring layer between the substrate and the pellicle. The at least one spring may be formed in the spring layer. The addition of the leaf spring further enhances the ability to select a desired stress within the pellicle.
[0015]
[0015] At least one of the three-dimensional expanding structures may comprise a herringbone pattern, which may extend across the entire pellicle or across an outer (eg, non-image field) portion of the pellicle.
[0016]
[0016] The at least one three-dimensional extending structure may provide roughness across the surface of the pellicle.
[0017] According to a second aspect described herein, there is provided a pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached. The surface comprises at least one adhesive boundary for reducing adhesive spreading. Providing an adhesive boundary reduces the tendency of the adhesive to spread and thus reduces contamination of the space between the patterning device and the pellicle.
[0018]
[0018] At least one adhesive boundary may comprise a circular boundary. Additionally or alternatively, at least one adhesive boundary may comprise a line boundary. By providing a circular boundary, the adhesive will be applied within the circular boundary and will spread and center within the circular boundary, but the amount of adhesive that spreads beyond the circular boundary is reduced. In this way, the precision with which the adhesive can be applied may be beneficially increased.
[0019]
[0019] The line boundary may be positioned adjacent to an edge of the pellicle frame, the edge of the frame adjacent to a central portion of the pellicle, where the central portion of the pellicle is that portion of the pellicle that is not in direct contact with the pellicle frame.
[0020]
[0020] The line boundary may be located between the circular boundary and the center of the pellicle.
[0021]
[0021] At least one boundary may comprise a groove in the frame.
[0022]
[0022] The pellicle assembly may include an adhesive that is generally concentric with a circular boundary.
[0023]
[0023] According to a third aspect described herein, there is provided a pellicle assembly comprising a pellicle frame, a pellicle, and one or more actuators for moving the pellicle assembly towards and away from a patterning device. In this manner, a space between the pellicle and the patterning device may be opened and closed to allow processing of the space. For example, when open, the space may be flushed, while when closed, the space may be sealed and pressure controlled.
[0024]
[0024] The actuator may be configured to transition the pellicle assembly between a closed configuration in which a substantially sealed volume is formed between the pellicle and the patterning device, and an open configuration in which the volume between the pellicle and the patterning device is fluidly connected to the surrounding environment.
[0025]
[0025] According to a fourth aspect described herein, there is provided a pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached. The pellicle frame comprises a first material having a first coefficient of thermal expansion (CTE) and a second material having a second coefficient of thermal expansion. In this manner, the overall CTE of the pellicle frame can be tailored and selected to reduce (or increase) the difference with respect to the CTE of the pellicle. The difference in CTE between the pellicle and the pellicle frame introduces stresses in the pellicle during fabrication and after processing (such as annealing). By controlling the overall CTE of the pellicle frame, the amount of stress in the pellicle can be controlled.
[0026]
[0026] The first material may comprise silicon. The first material may comprise a plurality of pores, and the second material is located within the plurality of pores. In other embodiments, the first material may comprise one or more channels, and the second material may be provided within the one or more channels.
[0027] The second material may at least partially surround the first material.
[0028]
[0028] The second material may comprise a metal, for example the second material may comprise aluminium and / or molybdenum.
[0029] According to a fifth aspect described herein, there is provided a pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, the pellicle frame being bonded to the pellicle. The pellicle may be an annealed pellicle, and the frame may be bonded to the pellicle after such annealing.
[0030]
[0030] The pellicle frame may comprise a material having a coefficient of thermal expansion (CTE) lower than that of silicon. For example, the pellicle frame may comprise a glass-ceramic material such as Zerodur®.
[0031]
[0031] The pellicle frame may be bonded to the pellicle using a bonding procedure that operates at a temperature less than approximately 160 degrees Celsius. In this manner, a pellicle frame comprising silicon may be used while achieving a non-operating stress (i.e., pre-stress) in the pellicle of approximately 200 MPa. The pellicle frame may be bonded to the pellicle using at least one of optical compression bonding, hydrogen bonding, gold diffusion bonding, or anodic bonding. Any other bonding method may be used, it being understood that the particular bonding method operates at a temperature that produces the desired prestress in the pellicle after fabrication. By way of example only, other examples of bonding include mechanical (e.g., bolts, fasteners, etc.), ceramic green body bonding (wherein two pieces of ceramic material in the green state are bonded during sintering to become a monolithic part) (also known as co-fired bonding), direct bonding, glass bonding, atomic diffusion bonding, and laser ablation assisted bonding.
[0032]
[0032] The pellicle frame may be formed in a single piece, i.e., the pellicle frame may not include multiple pieces connected (e.g., via adhesive or mechanical retention means) to form a whole. In this manner, the number of interfaces between components of the pellicle assembly is reduced, thereby reducing particulate contamination.
[0033]
[0033] The pellicle frame may be provided with an inert coating to reduce outgassing.
[0034]
[0034] The pellicle of any of the above aspects may comprise molybdenum disilicide (MoSi2). The stress within the pellicle may be in the range of 100 MPa to 250 MPa, such as approximately 200 MPa, at room temperature.
[0035]
[0035] The pellicle may comprise a graphite-based material. The stress within the pellicle may be in the range of 300 MPa to 450 MPa, for example approximately 400 MPa, at room temperature.
[0036] According to a sixth aspect described herein, there is provided a lithographic apparatus arranged to project a pattern from a patterning device onto a substrate, wherein a pellicle according to any of the previous aspects is arranged adjacent to the patterning device to prevent particles from contacting the patterning device.
[0037] According to a seventh aspect described herein, there is provided a method of manufacturing a pellicle assembly, the method comprising depositing a pellicle on a substrate, coupling a pellicle frame to the pellicle such that the pellicle is between the pellicle frame and the substrate, and etching the substrate to leave the pellicle and the pellicle frame.
[0038]
[0038] The pellicle frame may be bonded to the pellicle at a temperature below 160 degrees Celsius.
[0039]
[0039] The method may further comprise annealing the pellicle after depositing the pellicle on the substrate and prior to bonding the pellicle frame to the pellicle.
[0040]
[0040] According to an eighth aspect described in the present specification, a pellicle assembly is provided comprising a pellicle frame defining a surface to which the pellicle is attached, and a computer readable and writable tracking device is provided on or within the pellicle frame.
[0041]
[0041] The tracking device may be configured to store a unique identifier for the pellicle and / or the pellicle assembly.
[0042]
[0042] The tracking device may be configured to store operational data indicative of the pellicle's usage history and / or information specific to that pellicle, such as parameters measured offline (eg, transmission, reflectance, etc.).
[0043]
[0043] According to a ninth aspect described in the present specification, there is provided a lithographic apparatus comprising a controller arranged to project a pattern from a patterning device onto a substrate, the controller comprising a processor configured to execute computer readable instructions to cause a transceiver arrangement to read from and write to a tracking device of a pellicle assembly according to the eighth aspect.
[0044]
[0044] The computer readable instructions may be configured to cause the processor to obtain one or more operational data items from the tracking device and determine whether the one or more operational data items exceed a threshold.
[0045]
[0045] The computer readable instructions may be configured to cause the processor to, in response to determining that one or more operational data items exceed a threshold, cause the lithographic apparatus to unload the pellicle assembly.
[0046]
[0046] The computer readable instructions may be configured to cause the processor to write data to the tracking device indicating that the pellicle assembly has been unloaded from the transceiver arrangement.
[0047]
[0047] The computer readable instructions may be configured to cause the processor to cause the transceiver to record operational data about the tracking device during use of the lithographic apparatus in response to a determination that one or more operational data items do not exceed a threshold value.
[0048]
[0048] According to a tenth aspect described in the present specification, there is provided a pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is mounted, the pellicle being configured to exhibit one or more wrinkles in use, the one or more wrinkles being configured to reflect a portion of an incident radiation beam away from the substrate.
[0049] The pellicle may be configured such that the wrinkles form a maximum angle with respect to a plane defined by the surface of the patterning device of greater than 35 mrad.
[0050]
[0050] The pellicle may be configured such that the wrinkles form a maximum angle with respect to a plane defined by the surface of the patterning device of less than 300 mrad.
[0051]
[0051] The pellicle may be configured to reflect approximately 0.4% of the radiation beam incident on it in use.
[0052] According to an eleventh aspect described herein, there is provided a pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, and one or more tension layers provided on the surface of the pellicle and extending inwardly beyond an inner edge of the pellicle frame, the one or more tension layers acting to stiffen the pellicle assembly and maintain tension in the pellicle.
[0053]
[0053] At least one of the one or more tensile layers may be provided on an upper side of the pellicle such that the pellicle is disposed between the tensile layer and the frame. At least one of the one or more tensile layers may be provided on a lower side of the pellicle. The one or more tensile layers may include a first tensile layer provided on an upper side of the pellicle and a second tensile layer provided on a lower side of the pellicle.
[0054] At least one of the one or more tensile layers may include a first portion extending inwardly from an inner edge of the pellicle frame and a second portion extending outwardly from the inner edge of the pellicle frame, the second portion being longer than the first portion. In this manner, a majority of the tensile layer may be in communication with the pellicle frame (either directly or through the pellicle), thereby further strengthening the pellicle assembly.
[0055] At least one of the one or more tensile layers may have a multi-layer construction.
[0056] According to a twelfth aspect described herein, there is provided a lithographic apparatus comprising a pellicle assembly according to the eleventh aspect, arranged to project a pattern from a patterning device onto a substrate.
[0057]
[0057] According to a thirteenth aspect described herein, there is provided a dynamic gas lock for a lithographic apparatus comprising a pellicle assembly according to any one of the pellicle assemblies described above.
[0058]
[0058] It will be appreciated that features described in relation to one or more of the above aspects may be utilized in combination with other aspects. [Brief description of the drawings]
[0059]
[0059] Embodiments of the present invention will now be described, by way of example only, with reference to the accompanying schematic drawings in which:
[0060] [Figure 1] 1 illustrates a schematic representation of a lithography system comprising a lithography apparatus including a pellicle assembly. [Diagram 2] 1 illustrates a schematic of a pellicle assembly. [Diagram 3] 1A-1D show schematic stages in the construction of a pellicle assembly having a tensioning structure that allows the pellicle to be tensioned under stress. [Figure 4] 4 shows a schematic top view of the pellicle of FIG. 3; [Diagram 5] 4 is a graph showing how pellicle stress varies with stiffness of the extended structure shown in FIG. 3. [Figure 6] 1A-1D show schematic diagrams of stages in the construction of a pellicle assembly having different extension structures. [Figure 7] 1 illustrates a schematic of a pellicle assembly having multiple extending structures. [Figure 8] 1 shows a substrate that has been etched to provide an expanding structure that operates in two dimensions. [Figure 9] 1 shows a substrate with a herringbone extension structure. [Figure 10] 1 illustrates a schematic of a pellicle assembly having a herringbone extension structure along the edge of the pellicle assembly. [Figure 11] 1 illustrates a schematic of a pellicle assembly having a herringbone extension structure across the surface of the pellicle. [Figure 12] 1 shows a schematic of a pellicle having a herringbone extension structure. [Figure 13] 13A-13C are schematic diagrams illustrating mechanical bending of a pellicle assembly to reduce tension in the pellicle. [Figure 14] 13A-B illustrate schematic diagrams of mechanical bending of a pellicle assembly to increase tension in the pellicle. [Figure 15] 1A-1C show schematic diagrams of a pellicle configuration having tension structures provided by surface roughness. [Figure 16] 13A-13C show schematic diagrams of alternative configurations of a pellicle having extending structures provided by surface roughness; [Figure 17] 1 illustrates a schematic of a pellicle frame with an adhesive boundary. [Figure 18] 1 shows a pellicle frame with an adhesive boundary. [Figure 19a] 1 shows the pellicle assembly in an open configuration. [Figure 19b] 1 shows the pellicle assembly in a closed configuration. [Figure 19c] 19b shows the pellicle assembly of FIG. 19b after flushing the surrounding volume. [Figure 20a] 1A-1D illustrate schematic stages in the manufacture of a pellicle frame according to one embodiment. [Figure 20b] 1A-1D illustrate schematic stages in the manufacture of a pellicle frame according to one embodiment. [Figure 20c] 1A-1D illustrate schematic stages in the manufacture of a pellicle frame according to one embodiment. [Figure 21a] 13A-13C are schematic diagrams illustrating alternative examples of pellicle frames; [Figure 21b] 13A-13C are schematic diagrams illustrating alternative examples of pellicle frames; [Figure 22] 1 illustrates a schematic diagram of a pellicle assembly having a pellicle frame according to one embodiment. [Figure 23a] 5A-5C are schematic diagrams illustrating stages in the manufacture of a pellicle assembly according to another embodiment; [Figure 23b] 5A-5C are schematic diagrams illustrating stages in the manufacture of a pellicle assembly according to another embodiment; [Figure 24] 24 is a graph showing how prestress in a pellicle varies with bonding temperature in the method shown in FIG. 23. [Diagram 25]10 illustrates a schematic representation of the reflection of radiation from a pellicle towards a substrate; [Figure 26] 13A and 13B illustrate schematic reflections of radiation from a wrinkled pellicle away from a substrate. [Figure 27a] 1A-1C illustrate schematic diagrams of example pellicle assembly configurations reinforced by application of at least one tensile layer. [Figure 27b] 1A-1C illustrate schematic diagrams of example pellicle assembly configurations reinforced by application of at least one tensile layer. [Figure 27c] 1A-1C illustrate schematic diagrams of example pellicle assembly configurations reinforced by application of at least one tensile layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0061]
[0060] Figure 1 shows a lithography system including a pellicle assembly 15 according to an embodiment described herein. The lithography system comprises a radiation source SO and a lithography apparatus LA. The radiation source SO is configured to generate an extreme ultraviolet (EUV) radiation beam B. The lithography apparatus LA comprises an illumination system IL, a support structure MT configured to support a patterning device MA (e.g. a mask), a projection system PS, and a substrate table WT configured to support a substrate W. The illumination system IL is configured to condition the radiation beam B before it is incident on the patterning device MA. The projection system is configured to project the radiation beam B (now patterned by the mask MA) onto the substrate W. The substrate W may include a previously formed pattern. In that case, the lithography apparatus aligns the patterned radiation beam B with the pattern previously formed on the substrate W.
[0062]
[0061] The source SO, the illumination system IL, and the projection system PS may all be constructed and arranged such that they may be isolated from the external environment. A gas (e.g. hydrogen) at a pressure below atmospheric pressure may be provided in the source SO. A vacuum may be provided in the illumination system IL and / or the projection system PS. A small amount of gas (e.g. hydrogen) at a pressure significantly below atmospheric pressure may be provided in the illumination system IL and / or the projection system PS.
[0063]
[0062] The source SO may take any form, for example of the type that may be referred to as a laser-produced plasma (LPP) source. In an alternative example, the source SO may comprise one or more free electron lasers. The one or more free electron lasers may be configured to emit EUV radiation that may be provided to one or more lithographic apparatus.
[0064]
[0063] From a radiation source SO, a radiation beam B enters an illumination system IL configured to condition the radiation beam. The illumination system IL may include a faceted field mirror device 10 and a faceted pupil mirror device 11. The faceted field mirror device 10 and the faceted pupil mirror device 11 together provide a radiation beam B having a desired cross-sectional shape and a desired angular distribution. The radiation beam B passes through the illumination system IL and is incident on a patterning device MA held by a support structure MT. The patterning device MA is protected by a pellicle 19 which is held in place by a pellicle frame 17. The pellicle 19 and the pellicle frame 17 together form a pellicle assembly 15. The patterning device MA (which may for example be a mask) reflects and patterns the radiation beam B. The illumination system IL may include other mirrors or devices in addition to or instead of the faceted field mirror device 10 and the faceted pupil mirror device 11.
[0065]
[0064] Following reflection from the patterning device MA, the patterned radiation beam B enters a projection system PS. The projection system comprises a number of mirrors arranged to project the radiation beam B onto a substrate W held by a substrate table WT. The projection system PS may apply a demagnification to the radiation beam, forming an image having smaller features than corresponding features on the patterning device MA. For example, a demagnification of 4 may be applied. The patterned radiation beam incident on the substrate W may comprise a strip of radiation. The strip of radiation may also be referred to as an exposure slit. During a scanning exposure, the movement of the substrate table WT and the support structure MT may be such that the exposure slit travels over the exposure field of the substrate W. Although in Figure 1 the projection system PS has two mirrors, the projection system may comprise any number of mirrors, for example six mirrors.
[0066]
[0065] The radiation source SO shown in Figure 1 may include components not shown. For example, the radiation source may be provided with a spectral filter. The spectral filter may be substantially transparent for EUV radiation but substantially blocking radiation of other wavelengths, such as infrared radiation.
[0067]
[0066] As briefly mentioned above, the pellicle assembly 15 includes a pellicle 19 disposed adjacent to the patterning device MA. The pellicle 19 is provided in the path of the radiation beam B such that the radiation beam B passes through the pellicle 19 both when approaching the patterning device MA from the illumination system IL and when reflected by the patterning device MA towards the projection system PS. The pellicle 19 comprises a thin membrane that is substantially transparent to EUV radiation (but will absorb small amounts of EUV radiation). The pellicle 19 acts to protect the patterning device MA from particle contamination. The pellicle 10 may be referred to herein as an EUV transparent pellicle.
[0068]
[0067] While efforts will be made to maintain a clean environment inside the lithographic apparatus LA, particles may still be present inside the lithographic apparatus LA. In the absence of the pellicle 19, particles may build up on the patterning device MA. Particles on the patterning device MA may adversely affect the pattern imparted to the radiation beam B and therefore the pattern transferred to the substrate W. The pellicle 19 provides a barrier between the patterning device MA and the environment within the lithographic apparatus LA to prevent particles from building up on the patterning device MA.
[0069] In use, the pellicle 19 is positioned a sufficient distance from the patterning device MA such that particles incident on the surface of the pellicle 19 are not in the focal plane of the radiation beam B. This spacing between the pellicle 19 and the patterning device MA acts to reduce the extent to which particles on the surface of the pellicle 19 impart a pattern to the radiation beam B. It will be appreciated that if a particle is present in the radiation beam B but not in the focal plane of the radiation beam B (i.e. not on the surface of the patterning device MA), then the image of the particle will not be in focus at the surface of the substrate W. In some embodiments the spacing between the pellicle 19 and the patterning device MA may be, for example, about 2 mm to 3 mm (e.g. about 2.5 mm). In some embodiments, the spacing between the pellicle 19 and the patterning device may be adjustable, as described in further detail below.
[0070]
[0069] Figure 2 is a more detailed schematic diagram of a cross section of the pellicle assembly 15 and the patterning device MA. The patterning device MA includes a pattern surface 24. The pellicle frame 17 supports the pellicle 19 around a periphery of the pellicle 19. The pellicle frame 17 may include an attachment mechanism 22 configured to allow the pellicle frame to be removably attachable to the patterning device MA (i.e., to allow the pellicle frame to be attachable to and detachable from the patterning device MA). The attachment mechanism 22 is configured to engage with an attachment feature (not shown) provided on the patterning device MA. The attachment feature may be, for example, a protrusion extending from the patterning device MA. The attachment mechanism 22 may include, for example, a locking member that engages with the protrusion to secure the pellicle frame 17 to the patterning device MA. Note that although referred to herein as a pellicle frame, the pellicle frame 17 may also be referred to elsewhere as a pellicle boundary. The pellicle frame 17 (or "border") may also be attached to the mask via a further pellicle frame. For example, see FIG. 4B of patent application WO2016079051, which shows an arrangement with a pellicle membrane 19, a border 20 (which in some configurations may correspond to a general, rather than specific, component in the position of "frame 17" in the present application), and an additional frame 17 attached to the patterning device MA via attachment mechanisms as shown in FIGS. 12 and 31 of WO2016079051. Multiple attachment mechanisms and associated attachment features may be provided. The attachment mechanisms may be distributed around the pellicle frame 17 (e.g. two on one side of the frame and two on the other side of the frame). Associated attachment features may be distributed around the periphery of the patterning device MA.
[0071]
[0070] A contamination particle 26 is shown diagrammatically in Figure 2. The contamination particle 26 is incident on the pellicle 19 and is retained by the pellicle 19. The pellicle 19 retains the contamination particle sufficiently far from the patterned surface 24 of the mask MA so that the contamination particle is not imaged onto the substrate by the lithographic apparatus LA.
[0072]
[0071] A pellicle assembly according to one embodiment of the present invention may enable a mask pattern (on a patterning device) to be provided which remains substantially defect-free during use (the mask pattern being protected from contamination by the pellicle).
[0073]
[0072] The pellicle assembly 15 may be constructed by depositing the pellicle 19 (which may be made of polysilicon (pSi), for example) directly onto a substrate that provides the frame 17. The substrate may be, for example, a silicon wafer. After deposition of the pellicle 19 film, the substrate may be selectively back-etched to remove a central portion of the substrate, leaving only the outer periphery, to form the frame 17 for supporting the pellicle 19. The pellicle 19 may have a thickness of, for example, on the order of 15 to 50 nm.
[0074]
[0073] The pellicle 19 requires some "prestress" (i.e., some stress that exists in the pellicle 19 when not in use and is therefore not exposed to radiation and gas pressure during the scanning operation). The prestress in the pellicle 19 allows the pellicle 19 to withstand pressure differences caused by temperature and gas pressure changes during the scanning operation. However, too much prestress will shorten the overall life of the pellicle assembly 15. Therefore, it is desirable to give the pellicle 19 a minimum prestress (in the xy plane shown) to limit the deflection (in the y direction) for a given pressure on the pellicle 19. If the pellicle 19 deflects too much in the y direction, the pellicle 19 may break and / or contact other components in the area around the pellicle 19.
[0075]
[0074] The pre-stress of the pellicle 19 is preferably limited because the stress in the pellicle 19 is preferably significantly lower than the ultimate tensile stress or yield strength of the material forming the pellicle 19. To increase the life and reliability of the pellicle 19, the margin between the stress and the ultimate tensile stress should be as large as possible.
[0076]
[0075] Prestress may be built into the pellicle 19 through one or more mechanisms including stoichiometry, hydrogenation, crystal size control, doping, and coefficient of thermal expansion (CTE) mismatch during deposition of the pellicle 19 on the wafer 17. The pellicle 19 may also include multiple layers (e.g., a capping layer to protect the pellicle 19 from hydrogen radicals, etc.) Due to CTE mismatch between layers of the pellicle 19 portion of the pellicle assembly 15 and the heteroepitaxy process by which different layers of the pellicle 19 may be deposited, the stress in each layer of the multi-layer pellicle 19 may be different.
[0077]
[0076] The use of stoichiometry, hydrogenation, crystal size selection (i.e. number of grain boundaries), doping, etc. will all affect the chemical stability of the layers of the pellicle 19. In general, the processes used to fabricate the pellicle 19 may result in the desired prestress (if the desired prestress is relatively high), but the use of the techniques outlined above may be such that the pellicle 19 does not have the most stable configuration from a thermochemical standpoint. For example, a pellicle constructed from molybdenum disilicide (MoSi2) oxidizes exponentially faster as a function of prestress. Also, in complementary metal oxide semiconductor (CMOS) based fabrication processes using the methods outlined above, it is generally difficult to obtain a prestress below a value of 600 MPa. In some embodiments, it is desirable to obtain a pellicle 19 having a prestress on the order of 100-200 MPa.
[0078]
[0077] Furthermore, the pellicle frame 17 is generally inflexible compared to the pellicle 19, resulting in internal stresses in addition to the desired prestress. Thus, a prestress of, say, 100 MPa in the pellicle 19 will in reality be a prestress of 100 MPa plus or minus the deviation caused by the pellicle frame 15. In other words, some parts of the pellicle 19 may be under higher stress than other parts, resulting in pellicle 19 having greater points of mechanical weakness.
[0079]
[0078] The average prestress in the pellicle 19 is approximately the same in both the x and y dimensions as shown. In one embodiment, it is desirable to prevent wrinkles with high angles (between the xy plane and the z dimension) (on the order of 300 mrad). One approach to reduce high angle local wrinkles is by reducing the prestress in the scan (x) direction. The stress in the scan (x) direction is adjusted to a Poisson's ratio ν (approximately 0.17-0.25 for MoSi2) and a y-direction stress σ to prevent buckling at rest. y It only needs to be a small amount larger than the multiplication of σ x =ν*σ y It is.
[0080] During exposure, the stress σ in the non-scanning (y) direction y is the stress in the scan (x) direction σ x However, σ x is ν*σ y, the buckling modes that may occur within the exposure slit on the pellicle 19 will be lower in order, and therefore the likelihood of local high wrinkle angles will be lower. The lowest buckling mode is one period of a sine, i.e., a single wrinkle. It takes energy to pull the pellicle 19 into a higher buckling mode (i.e., to cause the pellicle 19 to contain multiple wrinkles). The more energy that is present, the more likely it is that, for example, imperfections in the pellicle 192 will locally pull the pellicle 192 to a (locally) high angle. Thus, in embodiments employing the techniques described herein, the amount of prestress in the scan direction may be reduced.
[0081]
[0080] It is desirable to decouple the internal microstructure of the pellicle 19 from the prestress within the pellicle 19. That is, it is beneficial to control the prestress of the pellicle 19 mechanically (or externally) rather than through the internal microstructure of the pellicle 19. This allows the pellicle 19 to be manufactured to be as chemically inert as possible, while still allowing the prestress within the pellicle 19 to be tuned to a desired level.
[0082]
[0081] Figure 3 illustrates diagrammatically the stages of fabrication of a pellicle assembly 35 according to an embodiment. The pellicle assembly 35 is fabricated by etching two notches 36, 37 that will provide a frame in a substrate 38 (e.g. a silicon wafer), as shown in Figure 3a. As shown in Figure 3b, a pellicle 19 is deposited on the notched substrate 38. The substrate 38 is then back-etched to provide the pellicle assembly 35 with a frame 39, as shown in Figure 3c. After back-etching, the notches 36, 37 become the frame 39 that comprises two tension structures (e.g. a V-shaped configuration) 36', 37' in the form of leaf springs. The leaf springs 36', 37' reduce the pre-stress of the pellicle 19 in the x-dimension (i.e. the scanning direction).
[0083]
[0082] The length and thickness of the leaf springs 36', 37' can be controlled by adjusting the depth of the notches 36, 37 (i.e., their extent in the z dimension) and their location on the xy plane of the substrate 38. In this way, the stress reduction provided by the leaf springs 36', 37' can be controlled. Also, the stiffness of the leaf springs can be adjusted independently in both the scanning (x) and non-scanning (y) dimensions. For example, as shown in FIG. 4, the notches can be positioned on the substrate to provide lower stress in the scanning direction (x) than in the non-scanning direction (y). In particular, in FIG. 4, the notches 40, 41 are positioned closer (in the x dimension) to the desired image field 42, thereby resulting in a relatively flexible leaf spring. Meanwhile, the notches 43, 44 can be positioned further away (in the y dimension) from the desired image field 42 to create a stiffer leaf spring.
[0084]
[0083] Figure 5 is a graph showing how the stress in the pellicle varies as a function of the stiffness of the leaf springs (such as leaf springs 36', 37'). Figure 5 shows that by varying the stiffness of leaf springs 36', 37', it is possible to control the prestress in the pellicle over a wide range.
[0085]
[0084] Thus, the use of one or more tensioning structures can increase the margin between the prestress in the pellicle after fabrication and the ultimate tensile stress of the pellicle, thereby improving the life and reliability of the pellicle. Also, in the event of a catastrophic failure of the pellicle, the reduced tension provided by the tensioning structures means that less elastic energy is stored in the pellicle. Thus, there is less likelihood that a break in the pellicle will result in the release of pellicle debris into other areas of the lithographic apparatus.
[0086]
[0085] Although Figures 3 and 4 show the extension structure with a single notch, it will be understood that extension structures with additional notches and / or other patterns may be etched into the substrate from which the pellicle frame is formed to provide extension structures with different properties. In this way, pellicles with different prestresses may be provided. In some embodiments, additional layers may be utilized in the manufacture of a pellicle assembly to provide more complex extension structures. For example, Figure 6 illustrates a schematic of stages in the manufacture of a pellicle assembly 55 (Figure 6d). The pellicle assembly 55 is manufactured by etching serrations 51, 52 into a substrate 53 (e.g., a silicon wafer). A spring layer 54 is deposited on the substrate 53 such that the spring layer 54 is received within and takes the shape of the serrations 51, 52. The spring layer 54 may be formed of a metal such as, for example, copper, gold, silver, etc. In other embodiments, the spring layer 54 may be formed of other materials such as SiOx, SiN, or MoSi. Between the substrate 53 and the spring layer 54, a shield layer 56 is deposited over the desired image field. The shield layer 53 need not be deposited within the serrations 51, 52. Removal of the shield layer 53 after deposition of the spring layer 54 results in the arrangement shown in FIG. 6c, where the spring layer 54 is generally restricted to the area within the serrations 51, 52. A pellicle layer 57 is deposited over the spring layer 54 and the substrate 53. Back-etching of the substrate 53 results in a pellicle assembly 55 having two extending structures 58, 59. The properties of the spring layer 54, in addition to the properties of the serrations 51, 52 (e.g. depth, width), may be selected to obtain a desired prestress in the pellicle 57, resulting in a pellicle frame with a very low stiffness level. Although a single spring layer 54 is shown in the exemplary arrangement of FIG. 6, it will be understood that in other embodiments, two or more spring layers may be provided. If two or more spring layers are provided, the spring layers may be of different materials.
[0087]
[0086] In some embodiments, the substrate and / or spring layer may be etched to isolate the extension structures from each other. In a theoretically ideal arrangement, the pellicle may be suspended from the pellicle frame by an infinite number of extension structures (e.g., springs), with each extension structure having no internal connection to any of the other extension structures. While it is not possible to provide an infinite number of extension structures, it will be understood from the teachings herein that different etching patterns may be utilized to isolate each extension structure from each other extension structure within the general techniques described above. Figure 7 shows a schematic top view of a pellicle frame 75, where the frame 70 is etched to provide a plurality of isolated extension structures in the form of springs 71 supporting the pellicle 72.
[0088]
[0087] While the above examples describe tension structures that operate in a single dimension, stretching along the x-axis in Figures 3 and 6, in other embodiments tension structures can be formed that operate in multiple dimensions to control stress in the pellicle in both the x- and z-dimensions. Figure 8 is a photograph showing a perspective view of a substrate that has been etched to provide tension structures that operate in both the x- and z-dimensions shown.
[0089] In one embodiment, the pellicle frame may be etched to provide what is referred to as a "herringbone" pattern. This comprises sawtooth (or zigzag) structures in the xy, zy and zx planes. Figure 9a is a photograph showing a membrane 80 with an outer contour shown generally by a dashed outline 81. Referring to Figure 9b, the membrane 80 is folded to provide a herringbone structure 80'. It can be seen that the herringbone structure 80' makes the membrane 80 smaller than the outer contour 81.
[0090]
[0089] The herringbone structure can be utilized in multiple ways within the pellicle assembly. In one embodiment, the herringbone structure is applied to the exterior of the pellicle assembly. With reference to Figure 10, the pellicle assembly 90 comprises a pellicle 91 having an image field (or central) portion 92 and an extending structure in the form of a herringbone portion 93 at the frame (or edge) portion of the pellicle assembly 90. In Figure 10, the herringbone structure is illustrated diagrammatically by hatching. The edge 93 of the herringbone pattern may be constructed by the techniques described above with reference to Figure 6, for example using different etching patterns.
[0091]
[0090] In another embodiment, the entire surface of the pellicle may be formed with a herringbone structure. Referring to FIG. 11, a pellicle assembly 100 is shown in which the entire pellicle 101, including the image field portion 102, has a herringbone structure (schematically illustrated by hatching). By forming the entire pellicle 101 with a herringbone structure as in the exemplary arrangement of FIG. 11, the entire surface of the pellicle 101 contributes to reducing the prestress of the entire pellicle 101. In a test, a pellicle with a herringbone pattern was modeled using a finite element method. The results showed that, compared to a pellicle without a herringbone structure, the average stress in the pellicle can be reduced by a factor of 10 or more, while the maximum stress experienced by any part of the pellicle is reduced by a factor of 6 or more.
[0092]
[0091] When the herringbone structure is applied over the entire surface of the pellicle (or at least over a majority of the surface of the pellicle), the pellicle can be formed such that the total prestress is zero Pa. In an exemplary embodiment, the out-of-plane structure (i.e., the extent in the z dimension of the extended structure) is on the order of 0.1 mm to 0.5 mm, and the herringbone pattern has a spatial frequency of 0.2 mm to 1 mm. In such an embodiment, the pellicle after construction will have no prestress because the additional surface area provided by the herringbone structure (compared to a flat pellicle) is orders of magnitude greater than the shrinkage of the pellicle during fabrication. Surprisingly, it has been found that, while a pellicle without prestress would typically flex unacceptably in use (i.e., the flexure would bring particles on the pellicle into the focal plane), the herringbone structure has an additional advantage in that it introduces significant bending stiffness to the pellicle in at least one direction compared to a flat pellicle. Referring to FIG. 12, a pellicle 120 having a herringbone structure is illustrated. The herringbone structure of pellicle 120 provides a relatively high bending stiffness for bending about axis 121, and a lower bending stiffness about axis 122 resulting in reduced deflection of pellicle 120. The bending stiffness provided by the herringbone structure reduces out-of-plane deviations (e.g., deflection in the z dimension) during use.
[0093]
[0092] Thus, the use of one or more tensioning structures with herringbone structures throughout the pellicle or on the outer (e.g., frame, edge, or non-image field) portions of the pellicle can increase the margin between the pre-stress in the pellicle after fabrication and the ultimate tensile stress of the pellicle, thereby improving the life and reliability of the pellicle. Also, in the event of catastrophic failure of the pellicle, the reduced tension provided by the herringbone structure means that less elastic energy is stored in the pellicle. Thus, there is less likelihood that a break in the pellicle will result in the release of pellicle debris into other areas of the lithographic apparatus.
[0094]
[0093] The herringbone pattern can be formed in the pellicle generally using the method described above. That is, the herringbone pattern can be first etched into the substrate (e.g., a silicon wafer) before deposition of the pellicle on the substrate and before back-etching the substrate. In contrast to the method described above with reference to Figures 3 and 6, to provide herringbone over the entire surface of the pellicle, the entire surface of the substrate can be pre-etched, rather than only the outer portion of the substrate that forms the pellicle frame. In another embodiment, the stress of the pellicle can be adjusted by introducing localized portions of the herringbone pattern only where it is expected that the pellicle will be exposed to thermal loads in use.
[0095]
[0094] In one embodiment, the stress in the pellicle may be controlled through mechanical bending of the substrate prior to depositing the pellicle material on the substrate. For example, referring to FIG. 13a, the substrate 130 may be mechanically bent into a bow-shaped shape. The pellicle 131 may be deposited on the outer (convex) surface of the bow-shaped substrate 130 (FIG. 13b). Finally, the mechanical load in the substrate 130 may be released, thereby introducing mechanical compression into the pellicle 131 (FIG. 13c). Due to the mechanical compression introduced into the pellicle 131, the tension in the pellicle 131 with further manufacturing steps (e.g., back etching, annealing, etc.) will be lower than if the pellicle 131 was initially deposited on a flat substrate.
[0096] Bending the substrate before depositing the pellicle material on the substrate can also be used to increase tension. For example, referring to FIG. 14a, the substrate 140 can be mechanically bent into a bow shape. Then, the pellicle 141 can be deposited on the inner (concave) surface of the bow-shaped substrate 140 (FIG. 14b). Finally, the mechanical load in the substrate 140 can be released, thereby introducing mechanical tension.
[0097]
[0096] The stress mechanically added to or removed from a pellicle as a function of the radius of curvature of the substrate on which the pellicle is deposited during manufacture can, in some embodiments, be calculated similarly to "Stony's Equation."
number
[0098]
[0097] It should be understood that the control of stress in a pellicle through mechanical bending is not limited to a single layer, but can be reproduced for each additional layer of the pellicle deposited on the substrate. In this manner, the stress of each individual layer of the pellicle can be tailored as desired. Also, the use of mechanical bending can be used to control stress in more than one direction. For example, the substrate can be mechanically bent in multiple different directions. The bending direction can be different for different layers of the pellicle.
[0099]
[0098] Additionally, a feedback loop may be provided with sensors (not shown) to measure the forces generated during pellicle deposition as the pellicle layer grows thicker. The mechanical bending of the substrate can then be controlled based on that feedback to ensure the same stress throughout the thickness of the pellicle layer. Feedback may be particularly beneficial in the first atomic layers of the pellicle, since stress develops differently in the first atomic layers than in the "bulk" of the pellicle.
[0100]
[0099] Above, with reference to Figs. 11 and 12, it was described that a herringbone pattern can be created across the pellicle surface. In an alternative embodiment, other patterns or random "roughness" can be introduced into the pellicle during manufacture to reduce the final prestress of the pellicle. Similar to the method described above, to introduce "roughness" into the pellicle, roughness can be introduced onto the surface of the substrate onto which the pellicle is deposited. A number of mechanisms can be used to introduce roughness onto the surface of the substrate. For example, with reference to Fig. 15, a low-temperature plasma-enhanced chemical vapor deposition (PECVD) oxide layer 152 (e.g., silicon dioxide) can be provided on the surface of a silicon substrate 150. The PECVD oxide layer 152 provides a back "etch stop" layer onto which the pellicle 151 is deposited. Low-temperature PECVD oxide has an inherent roughness that is much greater than silicon. The pellicle 151 will have this roughness when deposited on the PECVD oxide layer 152.
[0101] [000100] In another embodiment, potassium hydroxide (KOH) may be used to etch the surface of a silicon substrate on which the pellicle will be deposited. Specifically, a resist may first be deposited on the silicon substrate, and the deposited resist may be lithographically patterned. For example, a checkerboard pattern may be formed in the resist. After lithographically patterning in the resist, the silicon may be etched (e.g., with KOH). For example, the silicon may be etched to create an inverted pyramid shape, which provides the desired roughness. The resist may then be removed and the substrate cleaned. The cleaned substrate may be oxidized by thermal oxidation to round off sharp edges created during etching and create an "etch stop." The pellicle may then be deposited on the oxidized substrate ready for regular pellicle fabrication.
[0102] [000101] It will be appreciated that other etchants may be used. For example, in other embodiments, an isotropic dry or wet etch may be used. In another embodiment, the roughness may be created by isotropic etching of silicon dioxide prior to removal of the resist.
[0103] [000102] The addition of "roughness" to a pellicle may be limited to portions of the pellicle rather than provided across the entire surface of the pellicle. For example, similar to the way in which springs were created in the embodiments described with reference to Figures 3 and 6, roughness may be added to the pellicle along one or more edges of the pellicle, or in other portions of the pellicle. For example, the stress in the pellicle may be tailored by introducing localized portions of roughness only where it is expected that the pellicle will be exposed to thermal loads in use.
[0104] [000103] The lateral dimension of the features created by the addition of roughness or pattern to the pellicle is preferably greater than the thickness of the pellicle. For example, with reference to Figure 16, the lateral dimension X of the features (shown in the exemplary arrangement of Figure 16 as forming a triangular pattern) is greater than the thickness y of the pellicle layer 161.
[0105] [000104] In some embodiments, the dimensions and configuration of the roughness added to the pellicle may be selected to provide approximately 0.045-0.095% extra surface area across the pellicle than would be provided by a flat pellicle. Once the pellicle is free-standing (e.g., after other steps in the manufacture of the pellicle assembly, such as back-etching), stresses will be reduced compared to those provided by a flat pellicle due to the extra surface area scaled with the Young's modulus of the pellicle material.
[0106] [000105] The pellicle may be attached to the pellicle frame using adhesive. Manually dispensing the small amount of adhesive needed to attach the pellicle to the pellicle frame may be difficult due to process variations and operator inaccuracies. For example, problems can occur when too much adhesive is applied (process variations) and when the adhesive is placed too far from the inside of the frame. Capillary action between the frame and the pellicle can lead to migration of the adhesive inside the enclosed volume between the pellicle and the patterning device MA. Adhesive in the enclosed volume can lead to serious contamination of the patterning device.
[0107] [000106] Figure 17 shows a schematic of a pellicle frame 171. The pellicle frame comprises a frame boundary having an inner edge 174. The central portion of the pellicle is beyond the inner edge 174 and is not in direct contact with the frame. The frame boundary is provided with a circular boundary 172. The circular boundary 172 is engraved into the material of the frame, which may be silicon for example. By providing a circle engraved into the frame boundary, it has been found that this provides a centering function for the adhesive dispensed into the central area of the circus. An adhesive drop with a high contact angle will start wetting immediately after dispensing. The circular boundary 172 acts as a barrier that causes the adhesive to self-center within the boundary 172.
[0108] [000107] An additional border 173 is also provided. In the embodiment shown, the additional border 173 takes the form of a straight line engraved into the frame 171. This additional border 173 acts as an additional barrier if too much adhesive is applied. Figure 18a is a photograph showing the centering effect of the circular border 172, where it can be seen that the adhesive 180 forms a generally centered circular spot of adhesive that is generally concentric with the circular border 172. In the embodiment shown, the diameter of the circular border 172 is on the order of 1.4 mm.
[0109] [000108] The circular border 172 and the additional border 173 may be provided by etching the substrate. For example, the borders 172, 173 may be laser etched into a silicon substrate.
[0110] [000109] Figure 18b is a photograph showing a situation where a dot of adhesive 181 contains too much adhesive applied to the pellicle frame 171. In Figure 18b it can be seen that the additional boundary 173 acts as a further barrier preventing the adhesive 181 from spreading beyond the inner boundary 174 of the frame and contaminating the enclosed volume between the pellicle and the patterning device MA.
[0111] [000110] Providing the circular boundary 172 and / or additional boundary 173 reduces the risk of adhesive reaching the enclosed volume and increases the ease and accuracy of dispensing the adhesive, which may be done manually.
[0112] [000111] It will be appreciated that the pellicle frame to which the pellicle is attached is relatively rigid compared to the pellicle itself. The rigidity of the frame, combined with the pre-stress applied to the pellicle as described above, can cause problems with the pellicle wrinkling as the temperature increases during the scanning operation. During a scan, the temperature can increase by up to several hundred degrees Celsius.
[0113] [000112] In one embodiment, a mechanism is provided for translating the pellicle frame towards and away from the patterning device MA to close and open the area between the pellicle and the patterning device MA. Referring to Figure 19, a pellicle assembly 190 is shown together with the patterning device MA. The pellicle assembly 190 comprises a pellicle frame 191 and a pellicle 192. An actuator (not shown) is provided for translating the pellicle assembly along the z dimension as shown. In Figure 19a, the pellicle assembly is shown in an open configuration, with the pellicle assembly 190 spaced away from the patterning device MA. In the open configuration, the pressure in the volume between the pellicle 192 and the patterning device MA is the same, labelled P1 in Figure 19a.
[0114] [000113] It will be appreciated that the actuator may take any suitable form as will be apparent to one skilled in the art.
[0115] [000114] The actuators are configured to enable the pellicle assembly 190 to transition to a closed configuration by translating the pellicle assembly 190 towards the patterning device MA until the pellicle frame 191 is in physical contact with the patterning device MA. In the closed configuration, the volume between the patterning device MA and the pellicle 192 is physically separated from the external environment surrounding the patterning device MA. The pellicle frame 191 may include a sealing member (not shown) on a surface 193 that is arranged to contact the patterning device MA. The patterning device MA may include a corresponding sealing member (not shown) to interface with the pellicle frame 191.
[0116] [000115] In Figure 19a, the pressure in the enclosed volume between pellicle 192 and patterning device MA is still at pressure P1, the same as the pressure around the patterning device MA.
[0117] [000116] During the scanning operation, pellicle assembly 190 may be transitioned to a closed configuration and gas may be flushed from the environment surrounding patterning device MA and pellicle assembly 190, thereby reducing the pressure of the environment surrounding patterning device MA. As illustrated in Figure 19c, after flushing the surrounding areas, the pressure in the volume between patterning device MA and pellicle 192 will be greater than the pressure surrounding patterning device MA (labeled P2 in Figure 19c). Thus, pellicle 192 will bow away from patterning device MA in the z dimension.
[0118] [000117] Prior to transitioning the pellicle assembly 190 from the open to the closed configuration, the ambient pressure surrounding the patterning device MA (labeled P1 in Figure 19a) may be selectively adjusted. For example, in some embodiments this pressure may be brought to approximately 2 Pa through the introduction of a gas such as hydrogen gas.
[0119] [000118] By increasing the pressure between the patterning device MA and the pellicle 192, the thermal connection to the patterning device is improved. This allows for more cooling by conduction through the gas in the volume between the patterning device MA and the pellicle 192. To reduce the pressure difference across the pellicle 192, pressure may also be increased from the opposite side of the pellicle 192. In this way, the pressure difference across the pellicle 192, and therefore the tension in the pellicle 192, is controlled.
[0120] [000119] By ensuring that the tension in pellicle 192 induced by the difference in pressures P1, P2 is greater than the tension in pellicle 192 induced by frame 191, pellicle 192 will wrinkle significantly less than when exposed to the high thermal loads during scanning operations. Also, by closing the volume between pellicle 192 and patterning device MA, liquids cannot enter that volume during scanning operations.
[0121] [000120] In the above embodiment, it is shown that the substrate on which the pellicle is deposited can be a crystalline silicon wafer. There are many reasons for the trend in the art to use crystalline silicon as a pellicle substrate, including the fact that the industry has a wealth of experience processing crystalline silicon wafers. Also, the coefficient of thermal expansion (CTE) of crystalline silicon wafers (2.6 μm / m / K) matches the CTE of polycrystalline pellicle materials (approximately 4 μm / m / K), so that thermal stresses introduced during the manufacturing process are relatively small. Therefore, crystalline silicon has quickly become the default surface to grow pellicles, even when the pellicles are constructed from materials with different CTEs than the polycrystalline pellicle materials.
[0122] [000121] In some embodiments, the pellicle may be constructed from MoSi2 with a CTE of approximately 8 μm / m / K or a graphite-based material with a CTE of approximately 1 μm / m / K. As discussed above, upon annealing at high temperatures (e.g., approximately 800 degrees Celsius) to improve the microstructure of the pellicle, the internal stresses within the pellicle assembly are small (e.g., close to zero). However, upon cooling (e.g., to room temperature), a large CTE mismatch occurs between the pellicle and the substrate, resulting in stress accumulation that contributes to the large prestress within the pellicle assembly, as discussed above.
[0123] [000122] In one embodiment, the CTE of the pellicle frame is tailored by fabricating the pellicle frame from a composite material. Referring to Figure 20a, there is shown a silicon wafer 200 which forms the pellicle frame of the pellicle assembly. It will be appreciated that in other embodiments the substrate may be a different material.
[0124] [000123] A boundary area 201 is defined on the substrate 200 that defines the edge of the pellicle frame. Although the boundary area 201 is shown in FIG. 20a as having a generally rectangular shape, it should be understood that other shapes may be used. For example, a circular shaped pellicle frame may be particularly beneficial in some embodiments as it may introduce less stress concentration within the pellicle. Portions of silicon are removed from within the boundary area 201 of the substrate 200 to form an area 202 that includes one or more regions for receiving another material. The removed areas are filled with a second (or filler) material having a different CTE than silicon to form a synthesis area 203. Construction of a pellicle assembly using the substrate 200 may then proceed as normal. The synthesis area 203 ensures that the pellicle frame of a pellicle assembly constructed using the substrate 200 has a desired CTE. The CTE may be tailored by selecting the filler material and the manner in which the filler material is distributed within the boundary area 201.
[0125] [000124] For example, in one embodiment, silicon may be removed from boundary region 201 as a continuous band 210, as shown in Figure 21a. In an alternative embodiment, boundary region 201 may be perforated to define a plurality of holes 215. A filler material may then be applied to fill the holes. It will be understood that the arrangements shown in Figures 21a and 21b are exemplary only and material may be removed from boundary region 201 in any arrangement.
[0126] [000125] In one embodiment, after filling, the filler material may partially or completely surround the border area. Figure 22 shows a cross section of a pellicle assembly 223 with filler material 220 in and around holes in a silicon substrate 221, thereby surrounding the silicon substrate 221. Together, the silicon substrate 221 and filler material 220 form a pellicle frame 222. In Figure 22, the substrate is back-etched to form a pellicle assembly 223 having a pellicle 224.
[0127] [000126] Using filler material, the CTE of the pellicle frame can be increased or decreased to increase or decrease the prestress in the pellicle.
[0128] [000127] The filler material may be any suitable material having a different CTE than the substrate material on which the pellicle is deposited (silicon in one example) and the substrate material forming the pellicle frame. By way of example only, the filler material may be a material having a relatively high CTE. Preferably, the filler material is a ductile material. Preferably, the filler material is a material that does not outgas. In one exemplary embodiment, the filler material is a metal. In one particular example, the filler material is aluminum or molybdenum. In one embodiment, different amounts of substrate may be removed at different portions of the interface. In this manner, additional localized control over prestress within the pellicle assembly may be achieved.
[0129] [000128] As mentioned above, once the filler material is added to the substrate, all other process steps for manufacturing the pellicle assembly may be beneficially left unchanged so that the use of the composite frame may be easily introduced into existing manufacturing processes. In one embodiment, rather than utilizing a substrate to form the pellicle frame, the pellicle frame may be bonded to the pellicle in a separate operation. In that case, the substrate may be completely etched away (so that no portion of the substrate remains in the pellicle assembly). An exemplary pellicle assembly 230 is shown in FIG. 23 during construction, where a pellicle 231 is deposited on a substrate 232. The substrate may be, for example, crystalline silicon. After being deposited on the substrate 232, the pellicle 231 may be annealed by conventional pellicle manufacturing methods. However, after annealing, a frame 233 may be bonded to the pellicle 231. The frame 233 is bonded to the side of the pellicle opposite the side that is in contact with the substrate 232. The substrate is then entirely back-etched to remove the substrate, leaving behind pellicle assembly 230 comprising pellicle 231 and frame 234. In this manner, the prestress in the pellicle after fabrication depends on the difference in CTE between pellicle 231 and frame 234 and the temperature at which bonding of frame 234 to pellicle 231 occurred.
[0130] [000129] It will be appreciated that the term "bonded" is used herein to differentiate from processes in which a pellicle is deposited on a substrate, i.e., in conventional arrangements, the pellicle is attached to the substrate after it has been deposited thereon, as opposed to the present arrangement in which the frame is bonded to the pellicle after it has been annealed.
[0131] [000130] Frame 234 may be constructed from any material such that the CTE of frame 234 may be selected depending on the desired properties of the pellicle assembly, such as prestress. Additionally, the method (and thus the temperature) of bonding frame 234 may be selected to further obtain the desired properties of pellicle assembly 230. For example, in one embodiment, pellicle frame 234 may comprise a lithium aluminosilicate glass ceramic, such as Zerodur® from Schott AG. Zerodur has a very low CTE and therefore little or no stretch, resulting in very low forces on the pellicle and patterning device MA.
[0132] [000131] In one embodiment, the frame 234 may comprise silicon, and it may be desirable to provide a prestress in the pellicle 231 in the range of 100 to 250 MPa, for example approximately 200 MPa. To achieve a prestress of approximately 200 MPa, the frame 234 may be bonded to the pellicle 231 at a temperature below approximately 160 degrees Celsius. For example, bonding techniques such as optical compression bonding and hydrogen bonding may be used, which operate at temperatures of approximately 20 to 25 degrees Celsius. Other exemplary bonding techniques that may be used with a silicon frame to achieve a prestress of approximately 200 MPa include gold diffusion bonding (operating at a temperature of approximately 50 degrees Celsius) and anodic bonding (operating at a temperature of approximately 160 degrees Celsius).
[0133] [000132] It will be appreciated that different bonding temperatures may be selected if different amounts of prestress are desired in the pellicle 231. FIG. 24 is a graph showing how the prestress in a MoSi pellicle increases with the temperature at which the silicon frame is bonded to the pellicle. It will be appreciated that the desired prestress may be determined depending on a number of factors, including, for example, the configuration of the pellicle 231. By way of example, in one embodiment using a graphite-based pellicle 231, a prestress in the range of 300 MPa to 450 MPa, e.g., 400 MPa, may be desired, and the material of the pellicle frame 234 and the temperature of bonding may be selected accordingly. Specifically, the prestress σ in the pellicle 231 at a given temperature T may be determined by the following equation:
number
[0134] [000133] The method described with reference to FIG. 23 may further be advantageous in that the frame may be constructed in any desired size and shape. In other construction methods of the pellicle assembly, a pellicle frame formed from an etched substrate on which the pellicle is grown may be assembled onto a further frame for placement on a patterning device. The method described with reference to FIG. 23 advantageously avoids further construction (e.g., gluing, assembly) and reduces the number of interfaces between components, thereby reducing particle generation that may cause contamination and reducing stresses on the pellicle 231 during manufacture. That is, the pellicle frame may be formed from a single piece rather than by remaining substrate boundaries and adding further frame elements. Also, construction of the frame 234 may be simpler than other pellicle assembly construction techniques. For example, the pellicle frame 234 may be machined or machined from a single piece of frame material.
[0135] [000134] In one embodiment, the pellicle frame 234 may be coated with a chemically inert coating prior to bonding to the pellicle 231. In this manner, outgassing of the pellicle frame 234 may be reduced or eliminated.
[0136] [000135] In one embodiment, the entire pellicle frame 234 may be coated with a chemical coating that is resistant to the etch used to etch the substrate 232. The entire pellicle assembly 230 may then be constructed and cleaned prior to etching the substrate 232, thereby improving yield.
[0137] [000136] In the examples described above with reference to Figures 23 and 24, it was described that the frame 234 may comprise silicon. However, in other embodiments, the frame may comprise a material other than silicon. For example, the frame 234 may comprise at least one of aluminum, titanium, beryllium, aluminum nitride, Zerodur®, silicon oxide, and silicon carbide. The choice of frame material may be selected depending on the bonding temperature and the desired pellicle prestress.
[0138] [000137] In an embodiment, the pre-stress of the pellicle may be selected such that the pellicle is wrinkled in a particular manner (e.g. has wrinkles of a particular desired size) to improve the performance of the lithographic apparatus. Referring to Figure 25, a patterning device MA is shown protected by a pellicle 302. A radiation beam 304 passes through the pellicle 302 and is incident on the patterning device MA. A patterned radiation beam 306 reflects from the patterning device MA, passes through the pellicle 302 and is incident on a desired area of the substrate 308. However, the pellicle 302 is not completely transparent to the radiation beam 304. A portion of the radiation beam 304 is absorbed by the pellicle 302, while a portion 310 is reflected from the pellicle 302. The reflected portion 310 may be, for example, on the order of 0.4% of the radiation beam 304. The reflected portion 310 does not follow the same path as the patterned radiation beam 306 and therefore does not impinge on the desired area of the substrate 308. Also, because the reflected portion 310 does not interact with the patterning device MA in any way, the reflected portion 310 is not patterned in the desired pattern. Thus, the reflected beam 306 may cause overlay errors and / or reduced contrast.
[0139] [000138] In one embodiment, the pellicle properties are selected to cause the development of wrinkles that reflect at least a portion of an incident radiation beam along a path of propagation that does not intersect the substrate. Figure 26 shows a similar arrangement to that shown in Figure 25, with identical components having the same reference numbers. However, in Figure 26, the pellicle 402 is configured to wrinkle to cause the reflective portion 310 to follow a path that does not intersect the substrate 308. Thus, in the embodiment of Figure 26, the portion 310 does not result in reduced contrast or overlay error. It will be appreciated that it will not be possible to prevent all reflections from the pellicle 402 onto the substrate (e.g. portions reflected from the peaks of the wrinkle valleys), but by selecting an appropriate wrinkle, the amount of radiation reflected from the pellicle onto the substrate can be reduced.
[0140] [000139] The quality of the wrinkles in pellicle 402 may be controlled using any of the techniques described herein for controlling the pre-stress present in pellicle 402. The temperature of pellicle 402 may also be controlled. In one embodiment, the pre-stress and temperature of pellicle 402 are selected to produce wrinkles at room temperature having an angle α greater than approximately 35 mrad with respect to a plane defined by the surface of the pellicle, although it will be appreciated that the desired angle of the wrinkles may vary depending on the optical path length between the patterning device and the substrate.
[0141] [000140] In one embodiment, pellicle 402 is exposed to a pre-stress of approximately 240 MPa. In one embodiment, pellicle 402 may be heated to an operating temperature (e.g., during a patterning operation) of approximately 200-450°C. In an exemplary embodiment in which pellicle 402 is heated to approximately 450°C with a pre-stress of approximately 240 MPa, pellicle 402 may exhibit wrinkles having a maximum local angle α of up to approximately 40 mrad and a wrinkle height Wh on the order of 10 μm. However, it will be understood that in general, the wrinkle height may vary and may depend on the material composition of the pellicle. In one embodiment in which the wavelength of radiation beam 304 is on the order of 13.5 nm, the pellicle may be configured to exhibit wrinkles having a minimum height on the order of 10 μm. In general, it might be expected that wrinkles in the pellicle 402 may enhance absorption of the incident radiation beam 304, but it has been found that an increase in absorption of the radiation beam 304 due to wrinkles having a local angle of less than approximately 300 mrad will be satisfactory.
[0142] [000141] A pellicle may have a finite amount of time during which it is effective and / or the likelihood of failure is within a desired threshold. For example, for some pellicles, after a certain amount of use, the pellicle may be close enough to failure that it may be preferable to avoid use. If the pellicle were to catastrophically fail, the elastic energy stored within the pellicle may result in the pellicle breaking, which in turn may result in the ejection of pellicle debris into other areas of the lithographic apparatus, thereby resulting in downtime of the lithographic apparatus.
[0143] [000142] To allow a decision to be made as to whether a pellicle should be used, in one embodiment, a wirelessly readable and writable tracking device is provided within the pellicle frame of the pellicle. For example, the pellicle frame may include a Near Field Communication (NFC) chip (such as an RFID "tag"). For example, the tracking device may be attached within the pellicle frame at the time of manufacture or attachment to the patterning device. The tracking device comprises a serial number that uniquely identifies the pellicle and / or pellicle assembly. The tracking device may also store operational data that may be used to track the operational history of the pellicle. For example, the operational data may include the number of exposures the pellicle has been exposed to, the time of manufacture, the total amount of radiation (e.g., based on the number of exposures and the known power of each exposure), and / or any other information that may be used to determine whether the pellicle has reached the end of its useful life. The tracking device may also store pellicle specific information, such as a list of parameter values (e.g., EUV transmission, reflectance, etc.) that have been measured offline.
[0144] [000143] When the pellicle / patterning device combination is loaded into the lithographic apparatus, a transceiver arrangement (e.g., comprising a single transceiver or separate receivers and transmitters) provided in the lithographic apparatus may read (i.e., by a controller) the serial number and operational data of the pellicle. The controller may determine whether one or more particular items of operational data exceed a threshold. For example, the controller may determine whether the number of exposures the pellicle has been exposed to or the time since manufacture exceed a threshold. If the controller determines that one or more of the operational data items exceed a threshold, the lithographic apparatus may unload the pellicle / patterning device combination. The controller may further cause the transceiver to write data to a tracking chip to mark the pellicle as unusable or to indicate that it has been rejected for use by a particular lithographic apparatus.
[0145] [000144] If it is determined that a particular operational data item does not exceed its corresponding threshold, the controller tracks usage of the pellicle during operation. For example, the controller may record the number of exposures the pellicle has been exposed to and may cause the transceiver to write that data to a tracking device. The tracking data may be written to the tracking device at the time of use or during an unload operation where the pellicle / patterning device is removed from the lithographic apparatus.
[0146] [000145] Once removed from the lithographic apparatus, the tracking device in the pellicle / patterning device combination may be read to determine if the pellicle has been marked as unusable or if one or more of the operational data items exceed a threshold value, after which it may be determined whether to replace the patterning device pellicle.
[0147] [000146] Figures 27a-c illustrate schematic diagrams of other arrangements by which the pellicle assembly may be strengthened to prevent breakage during use or manufacture. With reference to Figure 27a, pellicle assembly 500 comprises a pellicle frame 502 supporting a pellicle 504. Pellicle frame 502 may be manufactured, for example, as described above. A tensile layer 506 is applied to the "front" or "top" side of pellicle arrangement 500 (i.e., such that pellicle 504 is disposed between tensile layer 506 and pellicle frame 502). It will be appreciated that tensile layer 506 may be provided on pellicle 504 in any suitable manner (e.g., by any form of deposition or by growing tensile layer 506 on pellicle 504).
[0148] [000147] When viewed in cross section as shown in FIG. 27a, the tensile layer 506 extends laterally inwardly beyond (e.g., over or across) the inner edge 508 of the pellicle frame 502. The location of the inner edge 508 of the pellicle frame is typically a weak point of the pellicle assembly and is a location where the pellicle assembly is often exposed to mechanical failure. The presence of the tensile layer 506 extending over the weak point of edge 508 acts to maintain tension in the pellicle 504 and to strengthen the pellicle assembly 500. In this manner, the tensile layer 506 allows the pellicle 504 to be exposed to additional pretension than would be possible without the presence of the tensile layer 506. As detailed above, applying an appropriate and sufficient level of pretension to the pellicle 504 improves the optical properties of the pellicle assembly by preventing wrinkling. The tensile layer 508 preferably extends inwardly over only the non-optically active portions of the pellicle 504. That is, the tensile layer 508 preferably does not extend inwardly to an extent that would overlap the beam path of the radiation beam B. As in the arrangement shown in FIG. 27a, it is preferred (but not essential) that the tensile layer 508 extend outwardly from the edge 508 more than it extends inwardly from the edge 508 to provide greater strength. Thus, as shown in FIG. 27a, the tensile layer 506 comprises a first portion 506a extending inwardly from the edge 508 and a second, larger portion 506b extending outwardly from the edge 508.
[0149] [000148] As shown with reference to pellicle assembly 510 of FIG. 27b, a tensile layer 512 may instead be applied to the "bottom" or "lower surface" of pellicle 504. Similar to tensile layer 506 of pellicle assembly 500, tensile layer 512 of pellicle assembly 510 extends across the interior boundary between pellicle frame 502 and pellicle 504, thereby strengthening pellicle assembly 510. In the arrangement of FIG. 27b, a first portion 512a of tensile layer 506 extends inwardly from edge 508 and a second, larger portion 512b extends outwardly from edge 508. Also, in arrangement 510, second portion 512b extends over multiple sides of pellicle frame 502. Specifically, in the example of Figure 27a, second portion 512b extends over all exposed surfaces of pellicle frame 504 (e.g., all surfaces other than the "top" surface to which pellicle 504 is applied). In this manner, tensile layer 512 can, among other things, strengthen pellicle assembly 510 and allow for higher pre-tensioning of pellicle 504.
[0150] [000149] Further, as shown in FIG. 27c, the pellicle assembly 514 may comprise both a tensile layer 506 and a tensile layer 512. The tensile layer may comprise any suitable material. For example, the tensile layer may comprise a metal layer with good adhesion such as molybdenum (Mo), ruthenium (Ru), e.g. aluminum (Al), titanium (Ti), tantalum (Ta), vanadium (V), chromium (Cr), niobium (Nb), hafnium (Hf), tungsten (W), oxides such as TiO2, Ta2O5, nitrides such as TiN, TaN, CrN, SiN, or carbides such as TiC, TaC, SiC. In general, any material that adheres well and can be deposited with sufficient tensile stress (determined by the specific requirements of a particular application) may be used. The tensile layer may also comprise a multi-layer structure with each layer comprising a different material. For example, the tensile layer may include a capping or protective layer over the tensile layer. By way of example only, the tensile layer may include a first layer of molybdenum to provide tension and a second layer of ZrO2 to act as a protective layer. Additionally, a tensile layer provided earlier (such as tensile layer 506) may have a different structure and composition than a tensile layer provided later (such as tensile layer 512). This advantageously allows different materials to be used to match different operating conditions "above" and "below" the pellicle 504. It will also be appreciated that the thickness of the tensile layer and the distance it extends on either side of edge 508 may be selected depending on the particular material used.
[0151] [000150] In general, the above-described arrangements provide a pellicle assembly in which the stress under non-operating conditions (e.g., pre-stress) may be selected depending on the application requirements. For example, if it is desired to provide a lower pre-tension than is currently available, the life of the pellicle may be improved while allowing the desired thermo-chemistry. That is, the above-described techniques allow for decoupling the thermo-chemistry of the pellicle and the pre-stress present in the pellicle after manufacture of the pellicle assembly. Also, in the event of a catastrophic failure of the pellicle, the reduced tension that may be obtained by the above-disclosed configurations means that less elastic energy is stored in the pellicle. Thus, there is less likelihood that a break in the pellicle will result in the release of pellicle debris to other areas of the lithographic apparatus, thereby reducing downtime of the lithographic apparatus. Furthermore, while the above-described arrangements are described with respect to a pellicle used to protect a patterning device MA, it should be understood that the above-described pellicle assemblies described herein may be used in other applications, both in relation to lithography and more broadly. For example, the above-described arrangements may be used to provide a pellicle assembly for use in a dynamic gas lock.
[0152] [000151] In an embodiment, the present invention may form part of a mask inspection apparatus. The mask inspection apparatus may illuminate a mask with EUV radiation and monitor radiation reflected from the mask using an imaging sensor. The image received by the imaging sensor is used to determine whether defects are present on the mask. The mask inspection apparatus may include optics (e.g. mirrors) configured to receive EUV radiation from an EUV radiation source and form it into a radiation beam that is directed towards the mask. The mask inspection apparatus may further include optics (e.g. mirrors) configured to collect EUV radiation reflected from the mask and form an image of the mask on the imaging sensor. The mask inspection apparatus may include a processor configured to analyze the image of the mask on the imaging sensor and to determine from the analysis whether any defects are present on the mask. The processor may be further configured to determine whether the detected mask defects will cause unacceptable defects in an image projected onto a substrate when the mask is used by the lithographic apparatus.
[0153] [000152] In an embodiment the invention may form part of a metrology apparatus. The metrology apparatus may be used to measure the alignment of a projected pattern formed in a resist on a substrate relative to a pattern already present on the substrate. This measurement of relative alignment may be referred to as overlay. The metrology apparatus may, for example, be located immediately adjacent to a lithographic apparatus and may be used to measure overlay before the substrate (and resist) are processed.
[0154] [000153] Although specific reference may be made in the text to embodiments of the invention in the context of a lithographic apparatus, embodiments of the invention may be used in other apparatus. Embodiments of the invention may form part of a mask inspection apparatus, a metrology apparatus, or any apparatus that measures or processes objects such as wafers (or other substrates) or masks (or other patterning devices). These apparatus may be generally referred to as lithography tools. Such lithography tools may utilise vacuum or atmospheric (non-vacuum) conditions.
[0155] [000154] The term "EUV radiation" may be considered to encompass electromagnetic radiation having a wavelength in the range of 4 to 20 nm, for example in the range of 13 to 14 nm. EUV radiation may have a wavelength less than 10 nm, for example in the range of 4 to 10 nm, such as 6.7 nm or 6.8 nm.
[0156] [000155] Although it is described above that the source SO may be a laser-produced plasma LPP source, any suitable source may be used to generate EUV radiation. For example, the EUV-emitting plasma may be generated by converting a fuel (e.g. tin) into a plasma state using an electrical discharge. This type of source may be referred to as a discharge-produced plasma (DPP) source. The electrical discharge may be generated by a power supply, which may form part of the source or may be a separate entity connected to the source SO via an electrical connection.
[0157] [000156] Although specific reference may be made in the text to the use of the lithographic apparatus in the manufacture of ICs, it should be understood that the lithographic apparatus described herein may have other applications. Other possible applications include the manufacture of integrated optical systems, guidance and detection patterns for magnetic domain memories, flat panel displays, liquid crystal displays (LCDs), thin film magnetic heads, etc.
[0158] [000157] Although specific embodiments of the invention have been described above, it will be appreciated that the invention may be practiced otherwise than as described. The above description is illustrative and not limiting. Thus, it will be apparent to one skilled in the art that modifications may be made to the invention as described without departing from the scope of the claims set out below.
Claims
1. 1. A pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, The pellicle assembly comprises one or more three-dimensional expanding structures that enable the pellicle to expand under stress.
2. The pellicle assembly of claim 1 , wherein at least one of said three-dimensional expanding structures is formed within said pellicle frame and thereby applied to said pellicle.
3. The pellicle assembly of claim 1 or 2, wherein at least one of the three-dimensional extension structures forms a spring.
4. The pellicle assembly of claim 3 , wherein said spring comprises at least one V-shaped formation formed within said pellicle frame.
5. 5. The pellicle assembly of claim 1, wherein the at least one structure comprises a plurality of springs formed within the pellicle frame and positioned around a central portion of the pellicle.
6. The pellicle assembly of claim 2 or any claim dependent thereon, wherein the at least one spring is a leaf spring.
7. The pellicle assembly of claim 1 , wherein at least one of the three-dimensional extension structures is present in a central portion of the pellicle.
8. The pellicle assembly of claim 7 , wherein the frame comprises a substrate, and the pellicle assembly comprises at least one spring layer between the substrate and the pellicle, and wherein at least one spring is formed within the spring layer.
9. The pellicle assembly of claim 1 , wherein the at least one three-dimensional extended structure comprises a herringbone pattern.
10. 10. The pellicle assembly of claim 9, wherein the at least one three-dimensional expanding structure comprises a herringbone pattern that extends across a majority of an entire surface of the pellicle.
11. 11. The pellicle assembly of claim 1, wherein the at least one three-dimensional extending structure provides roughness across the entire surface of the pellicle.
12. 1. A pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, A pellicle assembly, wherein the surface comprises at least one adhesive boundary for reducing adhesive spreading.
13. The pellicle assembly of claim 12 , wherein the at least one adhesive boundary comprises a circular boundary.
14. The pellicle assembly of claim 12 or 13, wherein the at least one adhesive boundary comprises a line boundary.
15. The pellicle assembly of claim 14 , wherein the line boundary is disposed adjacent an edge of the frame, the edge of the frame adjacent a center portion of the pellicle.
16. 146. A pellicle assembly according to claim 14 or 145, depending from claim 13, wherein the line boundary is disposed between the circular boundary and a center of the pellicle.
17. The pellicle assembly of claim 12 , wherein the at least one boundary comprises a groove in the frame.
18. 18. The pellicle assembly of claim 12, wherein the pellicle assembly comprises an adhesive generally concentric with the circular boundary.
19. A pellicle frame; A pellicle and one or more actuators that move the pellicle assembly toward and away from a patterning device; A pellicle assembly comprising:
20. 20. The pellicle assembly of claim 19, wherein the actuator is configured to transition the pellicle assembly between a closed configuration in which a substantially sealed volume is formed between the pellicle and a patterning device, and an open configuration in which a volume between the pellicle and the patterning device is in fluid communication with an ambient environment.
21. 1. A pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, The pellicle assembly, wherein the pellicle frame comprises a first material having a first coefficient of thermal expansion and a second material having a second coefficient of thermal expansion.
22. The pellicle assembly of claim 21 , wherein the first material comprises silicon.
23. 23. The pellicle assembly of claim 21 or 22, wherein the first material comprises a plurality of pores, and the second material is located within the plurality of pores.
24. 24. The pellicle assembly of claim 21, 22 or 23, wherein the second material at least partially surrounds the first material.
25. 25. The pellicle assembly of any one of claims 21 to 24, wherein the second material comprises a metal.
26. 1. A pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, The pellicle frame is coupled to the pellicle, a pellicle assembly.
27. 27. The pellicle frame of claim 26, wherein said pellicle is an annealed pellicle and said pellicle frame is bonded to said pellicle after annealing.
28. 28. The pellicle assembly of claim 26 or 27, wherein the pellicle frame comprises a material having a coefficient of thermal expansion (CTE) lower than that of silicon.
29. 30. The pellicle assembly of claim 26, 27 or 28, wherein the pellicle frame comprises a glass-ceramic material.
30. 30. The pellicle assembly of any of claims 26 to 29, wherein the pellicle frame is bonded to the pellicle using a bonding procedure operating at a temperature of less than approximately 160 degrees Celsius.
31. 31. The pellicle assembly of any of claims 26 to 30, wherein the pellicle frame is bonded to the pellicle using at least one of optical compression bonding, hydrogen bonding, gold diffusion bonding, or anodic bonding.
32. 32. The pellicle assembly of any one of claims 26 to 31, wherein the pellicle frame is formed in a single piece.
33. 33. The pellicle assembly of any of claims 26-32, wherein the pellicle frame comprises an inert coating to reduce outgassing.
34. 34. The pellicle assembly of any one of claims 26 to 33, wherein the pellicle frame does not comprise silicon.
35. 35. The pellicle assembly of any one of claims 26 to 34, wherein the pellicle frame comprises at least one of aluminum, titanium, beryllium, aluminum nitride, Zerodur®, silicon oxide, and silicon carbide.
36. 1. A pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, when irradiated with a radiation beam to pattern a substrate to be patterned, the pellicle comprises one or more wrinkles and partially reflects the radiation beam; The one or more wrinkles are configured to reflect a portion of the radiation beam away from the substrate to be patterned.
37. 37. The pellicle assembly of claim 36, wherein the pellicle is configured such that the wrinkles form a maximum angle with a plane defined by the surface of the patterning device that is greater than 35 mrad.
38. The pellicle is configured such that the wrinkles form a maximum angle with respect to a plane defined by the surface of the patterning device of less than 300 mrad.
38. The pellicle assembly of claim 36 or 37.
39. 39. A pellicle assembly according to claim 36, 37 or 38, wherein the pellicle is configured, in use, to reflect approximately 0.4% of an incident radiation beam.
40. The pellicle is made of molybdenum disilicide (MoSi 2 40. The pellicle assembly of claim 1, wherein the average stress within the pellicle is in the range of 100 MPa to 250 MPa at room temperature.
41. 41. The pellicle assembly of claim 1, wherein the pellicle comprises a graphite-based material and the average stress within the pellicle is in the range of 300 MPa to 450 MPa at room temperature.
42. 42. A lithographic apparatus arranged to project a pattern from a patterning device onto a substrate, the lithographic apparatus comprising a pellicle assembly according to any one of claims 1 to 41 arranged adjacent to the patterning device to prevent particles from contacting the patterning device.
43. 1. A method of manufacturing a pellicle assembly, comprising: depositing a pellicle on a substrate; coupling the pellicle frame to the pellicle such that the pellicle is between the pellicle frame and the substrate; Etching the substrate to leave the pellicle and the pellicle frame. A method comprising:
44. 44. The method of claim 43, wherein the pellicle frame is bonded to the pellicle at a temperature below 160 degrees Celsius.
45. 45. The method of claim 43 or 44, further comprising annealing the pellicle after depositing the pellicle on the substrate and prior to bonding the pellicle frame to the pellicle.
46. 1. A pellicle assembly comprising a pellicle frame defining a surface to which the pellicle is attached, A pellicle assembly, wherein a computer readable and writable tracking device is provided on or in said pellicle frame.
47. 47. The pellicle assembly of claim 46, wherein the computer readable and writable tracking device is configured to store an identifier for the pellicle and / or the pellicle assembly.
48. 48. A pellicle assembly according to claim 46 or 47, wherein the computer tracking device is configured to store operational data indicative of a usage history of the pellicle and / or specific characteristics of the pellicle.
49. 50. A lithographic apparatus arranged to project a pattern from a patterning device onto a substrate, comprising: a controller having a processor configured to execute computer readable instructions to cause a transceiver arrangement to read from and write to a tracking device of a pellicle assembly according to any one of claims 46 to 48.
50. 50. The lithographic apparatus of claim 49, wherein the computer readable instructions are configured to cause the processor to obtain one or more items of operational data from the tracking device and determine whether the one or more items of operational data exceed a threshold.
51. 51. The lithographic apparatus of claim 50, wherein the computer readable instructions are configured to: cause the processor to, in response to determining that the one or more operational data items exceed a threshold, cause the lithographic apparatus to unload the pellicle assembly.
52. 52. The lithographic apparatus of claim 51, wherein the computer readable instructions are configured to cause the processor to write data to the tracking device indicating that the pellicle assembly has been unloaded at the transceiver arrangement.
53. 53. The lithographic apparatus of claim 50 or 52, wherein the computer readable instructions are configured to: cause the processor to, in response to determining that the one or more operational data items do not exceed the threshold, cause the transceiver to record operational data for the tracking device during use of the lithographic apparatus.
54. a pellicle frame defining a surface to which the pellicle is attached; one or more tension layers in mechanical communication with the pellicle and extending inwardly beyond an inner edge of the pellicle frame; A pellicle assembly comprising:
55. 55. The pellicle assembly of claim 54, wherein at least one of the one or more tensile layers is provided on an upper side of the pellicle such that the pellicle is disposed between the tensile layer and the frame.
56. 56. The pellicle assembly of claim 54 or 55, wherein at least one of the one or more tensile layers is provided on an underside of the pellicle.
57. 57. The pellicle assembly of claim 54, 55 or 56, wherein the one or more tensile layers comprise a first tensile layer provided on an upper side of the pellicle and a second tensile layer provided on a lower side of the pellicle.
58. 58. The pellicle assembly of any one of claims 54 to 57, wherein at least one of the one or more tensile layers comprises a first portion extending inward from the inner edge of the pellicle frame and a second portion extending outward from the inner edge of the pellicle frame, the second portion being longer than the first portion.
59. 58. The pellicle assembly of any one of claims 54 to 57, wherein at least one of the one or more tensile layers comprises a multi-layer structure.
60. 60. A lithographic apparatus arranged to project a pattern from a patterning device onto a substrate, comprising a pellicle assembly according to any one of claims 54 to 59 positioned adjacent to the patterning device to prevent particles from contacting the patterning device.
61. A dynamic gas lock for a lithographic apparatus comprising a pellicle assembly according to any one of claims 1 to 41, 46 to 48 or 54 to 59.
Citation Information
Patent Citations
Mask, exposure method, and device manufacturing method
JP2010078921A
Pellicle frame, manufacturing method thereof, and pellicle
JP2012220532A
Method for adjusting lithographic mask flatness using thermally induced pellicle stress
US20060146313A1
Cited By
Method of manufacturing pellicle for 3㎚ EUV lithography
KR103003072B1