Method for manufacturing double-sided cooled semiconductor module and double-sided cooled semiconductor device

The use of copper sintered bodies in bonding portions addresses reliability issues in double-sided cooling semiconductor modules by ensuring consistent joint positions and efficient heat dissipation, enabling high-temperature operation and reduced manufacturing costs.

JP2024150645AInactive Publication Date: 2024-10-23RESONAC CORP

Patent Information

Application Number
JP2024117632
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional double-sided cooling semiconductor modules face challenges in maintaining reliability due to increased temperatures and variations in semiconductor element heights, leading to thermal resistance and deteriorated heat dissipation.

Method used

Incorporation of a copper sintered body in the bonding portions between semiconductor elements and substrates, which enhances bonding reliability and maintains consistent joint positions despite height variations, facilitating efficient heat radiation.

Benefits of technology

The solution allows for reliable operation at high temperatures (up to 175°C) with improved thermal conductivity and reduced manufacturing costs, extending the life and consistency of the semiconductor module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150645000001_ABST
    Figure 2024150645000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a double-sided cooled semiconductor module and a double-sided cooled semiconductor device with excellent reliability.SOLUTION: In a method for manufacturing a double-sided cooled semiconductor module 100 with bonding portions 2, 4 including a sintered copper 31, which is a bonding material for bonding semiconductor element 1 and substrates 11a and 11b, the bonding material includes sub-microcopper particles with a volume average particle size of not less than 0.12 μm and not more than 0.8 μm and flake-shaped microcopper particles with a volume average particle size of not less than 1.0 μm and not more than 50 μm, the content of sub-microcopper particles and the content of flake-shaped microcopper particles are not less than 30% and not more than 90% by mass and not less than 10% and not more than 70% by mass, respectively, based on the total mass of metal particles in the bonding material, and the bonding material contains a solvent having a boiling point of 300°C or higher at a rate of 2 mass% or higher, based on the total mass of the bonding material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a double-sided cooled semiconductor module and a method for manufacturing a double-sided cooled semiconductor device. [Background technology]

[0002] A semiconductor device used in an inverter or the like has been proposed that includes a semiconductor module and a cold / heat source. A substrate for conducting electricity with a semiconductor element is disposed inside the semiconductor module, and is joined via a joint formed of a bonding material or the like. The substrate and the cold / heat source are joined by contact or a bonding material, and heat generated from the semiconductor element when electricity is applied is dissipated toward the cold / heat source via the substrate.

[0003] In recent years, due to the demand for smaller, denser, and higher temperature operation of semiconductor devices, the current flowing through the current-carrying substrate and junctions has increased, and the amount of heat generated by the semiconductor element has increased. For this reason, a double-sided cooling type semiconductor module and semiconductor device has been proposed in which substrates are arranged on both sides of the semiconductor element and a cooling / heating source is connected to each substrate (for example, see Patent Document 1 below). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-28040 A Summary of the Invention [Problem to be solved by the invention]

[0005] Due to the recent increasing demand for semiconductor devices to operate at higher temperatures, the maximum temperature of semiconductor elements is increasing, making it difficult to ensure reliability in conventional double-sided cooled semiconductor modules.

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a highly reliable double-sided cooled semiconductor module, a double-sided cooled semiconductor device, and a method for manufacturing a double-sided cooled semiconductor module. [Means for solving the problem]

[0007] In order to solve the above problems, one aspect of the present invention provides a double-sided cooling semiconductor module comprising a semiconductor element, a first substrate provided on one main surface side of the semiconductor element, a second substrate provided on the other main surface side of the semiconductor element, a first bonding portion bonding the semiconductor element to the first substrate, and a second bonding portion bonding the semiconductor element to the second substrate, wherein at least one of the first bonding portion and the second bonding portion includes a copper sintered body.

[0008] In the above double-sided cooling semiconductor module, the joints contain a sintered copper body, which improves the reliability and lifespan of the joints against temperature cycles. Also, the joints contain a sintered copper body, which prevents the joints from increasing thermal resistance in the heat dissipation path from the semiconductor element to the board, thereby preventing the heat generated in the semiconductor element from being degraded, and allows the heat to be efficiently dissipated toward the cold source via the board. Therefore, the above double-sided cooling semiconductor module has excellent reliability.

[0009] The above-mentioned double-sided cooling type semiconductor module may have two or more semiconductor elements.

[0010] However, in a double-sided cooling semiconductor module, when a plurality of semiconductor elements of different heights are mounted, it is necessary to adjust the height by inserting a spacer between at least one of the semiconductor elements and at least one of the substrates, and the accuracy in the height direction required for each component becomes strict. In addition, if the position of the bonding surface of the semiconductor element with the substrate or the distance between the substrates varies due to the variation in the height of each semiconductor element, when the substrate and the semiconductor element are sandwiched during bonding, a surface pressure distribution occurs, and bonding tends to deteriorate. In contrast, in the double-sided cooling semiconductor module according to the present invention, since the bonding portion includes a copper sintered body, it is easy to adjust the position (height) of the bonding surface even when the height of the semiconductor elements varies, and it can be easily suppressed from increasing the manufacturing cost due to additional processing such as the work of selecting semiconductor elements and processing for adjusting the position (height) of the bonding surface.

[0011] The copper sintered body may be a sintered body of a bonding material containing copper particles.

[0012] In the double-sided cooling type semiconductor module, one or more of the first joint portion and the second joint portion may include a spacer.

[0013] Another aspect of the present invention provides a double-sided cooling semiconductor device comprising the double-sided cooling semiconductor module of the present invention described above, and a first cold heat source and a second cold heat source connected to the first substrate and the second substrate of the double-sided cooling semiconductor module, respectively.

[0014] The above-mentioned double-sided cooled semiconductor device is provided with a double-sided cooled semiconductor module according to the present invention, and thus is highly reliable and can be operated at high temperatures.

[0015] Another aspect of the present invention provides a method for manufacturing the double-sided cooling semiconductor module according to the present invention, comprising a first bonding step of sintering a bonding material containing copper particles provided between a first substrate and a semiconductor element, and / or a second bonding step of sintering a bonding material containing copper particles provided between a second substrate and a semiconductor element. Note that when the first bonding step and the second bonding step are provided, the first bonding step and the second bonding step may be performed in this order, in the reverse order, or simultaneously.

[0016] According to the manufacturing method of the double-sided cooling semiconductor module, by including the first bonding process and / or the second bonding process, it becomes easy to adjust the position (height) of the bonding surface even when there is variation in the height of the semiconductor elements, and it is possible to suppress an increase in manufacturing costs due to additional processing such as the selection of semiconductor elements and processing for adjusting the position (height) of the bonding surface. Effect of the Invention

[0017] According to the present invention, it is possible to provide a highly reliable double-sided cooled semiconductor module, a double-sided cooled semiconductor device, and a method for manufacturing a double-sided cooled semiconductor module.

[0018] The double-sided-cooled semiconductor module and double-sided-cooled semiconductor device according to the present invention are capable of operating in high-temperature environments with semiconductor element temperatures of 175°C or higher, which is difficult to achieve with solder bonding. Furthermore, the double-sided-cooled semiconductor module and double-sided-cooled semiconductor device according to the present invention can have a long life and small variation in failure timing. The double-sided-cooled semiconductor module manufacturing method according to the present invention makes it possible to obtain the above-mentioned double-sided-cooled semiconductor module and double-sided-cooled semiconductor device. [Brief description of the drawings]

[0019] [Figure 1] 1 is a schematic cross-sectional view showing an embodiment of a double-sided cooling type semiconductor device; [Diagram 2]FIG. 11 is a schematic cross-sectional view showing another embodiment of a double-sided cooling type semiconductor device. [Diagram 3] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] In this specification, the exemplified materials may be used alone or in combination of two or more, unless otherwise specified. When a plurality of substances corresponding to each component are present in the bonding material, the content of each component in the bonding material means the total amount of the plurality of substances present in the bonding material, unless otherwise specified. A numerical range indicated using "~" indicates a range including the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage may be replaced by the upper limit or lower limit of a numerical range of another stage. In addition, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced by the value shown in the examples. The term "layer" includes a structure having a shape formed on the entire surface as well as a structure having a shape formed on a part of the surface when observed in a plan view.

[0021] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.

[0022] <Double-sided cooling type semiconductor module and double-sided cooling type semiconductor device> The double-sided cooling semiconductor module of this embodiment comprises a semiconductor element, a first substrate provided on one main surface side of the semiconductor element, a second substrate provided on the other main surface side of the semiconductor element, a first bonding portion bonding the semiconductor element to the first substrate, and a second bonding portion bonding the semiconductor element to the second substrate, and at least one of the first bonding portion and the second bonding portion includes a copper sintered body.

[0023] The double-sided cooling type semiconductor module may have two or more semiconductor elements. Also, one or more of the first joint portion and the second joint portion may include a spacer.

[0024] The double-sided cooling type semiconductor device of this embodiment comprises the double-sided cooling type semiconductor module of the above-mentioned embodiment, and a first cold heat source and a second cold heat source connected to the first substrate and the second substrate of this double-sided cooling type semiconductor module, respectively.

[0025] The double-sided cooling type refers to a type in which the direction of heat flow is from the semiconductor element to each of the substrates arranged on both main surfaces of the semiconductor element.

[0026] Hereinafter, the present embodiment will be described with reference to the drawings.

[0027] (1) First embodiment FIG. 1 is a schematic cross-sectional view showing one embodiment of a double-sided cooling type semiconductor device. The double-sided cooling type semiconductor device 101 shown in FIG. 1 includes a double-sided cooling type semiconductor module 100 including a semiconductor element 1, a first substrate 11a provided on one main surface of the semiconductor element 1, a second substrate 11b provided on the other main surface of the semiconductor element, a first joint 2 for joining the semiconductor element 1 and the first substrate 11a, and a second joint 4 for joining the semiconductor element 1 and the second substrate 11b, and a first cold source 21 and a second cold source 22 connected to the first substrate 11a and the second substrate 11b, respectively. In the double-sided cooling type semiconductor module 100 of this embodiment, the first joint 2 is made of a copper sintered body 31, the second joint 4 is made of a copper sintered body 31 and a spacer 41, and the semiconductor element 1 is sealed by a resin member 61.

[0028] The semiconductor element 1 is configured as a power element such as a diode, an IGBT, or a MOSFET that configures a boost converter, an inverter, or the like.

[0029] The resin member 61 that seals the semiconductor element 1 can be made of a synthetic resin such as an epoxy resin.

[0030] Materials for the substrates 11a and 11b include copper, aluminum, nickel, molybdenum, titanium, stainless steel, gold, silver, platinum, etc., from the viewpoint of thermal conductivity and electrical conductivity. Depending on the substrate configuration, it is preferable that an insulating material with good thermal conductivity and heat resistance, such as ceramic, is formed inside the conductive substrate. The substrate may have a substrate to be joined to the semiconductor element and a substrate extending toward the outside, and may have an electric circuit formed by wires 51 connecting these substrates. Materials for the wires 51 include aluminum, copper, gold, etc. The wire diameter of the wires 51 is preferably φ0.04 to 0.4 mm. A bus bar or a clip may be used instead of the wire.

[0031] It is preferable that a metallized layer is provided on the bonding surfaces of the substrates 11a and 11b with the bonding portions 2 and 4. Examples of materials for the metallized layer include nickel, gold, silver, titanium, tungsten, and molybdenum. The metallized layer can be formed by a method such as plating, sputtering, or vapor deposition. The thickness of the metallized layer can be 0.05 μm to 500 μm.

[0032] When insulating layers are provided on the substrates 11a and 11b, it is preferable that the thermal expansion coefficient of the substrates is equal to or close to that of the semiconductor element 1. The thermal expansion coefficient of the substrate is, for example, 3.0×10 -6 ~9.0×10 -6 / K may also be used.

[0033] The copper sintered body 31 may be a sintered body of a bonding material (copper paste) containing copper particles. The bonding material (copper paste) will be described in detail later.

[0034] The spacer 41 can be provided as necessary to adjust the height of the double-sided cooling semiconductor module 100 or the double-sided cooling semiconductor device 101. In this embodiment, the spacer is provided at the second joint 4, but it may be provided at the first joint. Also, multiple spacers may be provided at each joint.

[0035] From the viewpoint of thermal conductivity and electrical conductivity, examples of the material of the spacer 41 include copper, aluminum, nickel, molybdenum, titanium, stainless steel, gold, silver, platinum, and the like.

[0036] In the spacer 41, it is preferable to provide a metallized layer on the bonding surface with the copper sintered body 31. Examples of materials for the metallized layer include nickel, gold, silver, titanium, tungsten, and molybdenum. The metallized layer can be formed by a method such as plating, sputtering, or vapor deposition. The thickness of the metallized layer can be 0.05 μm to 500 μm.

[0037] The cold sources 21 and 22 are made of a material having good thermal conductivity, and may be known materials. The cooling method of the cold sources may be water-cooled, air-cooled, or Peltier. From the viewpoint of cooling performance, the water-cooled method is preferable.

[0038] The cold / heat sources 21 and 22 and the substrates 11a and 11b may be in contact with each other or may be joined by a joining material such as solder, a sintered material, a brazing material, etc. If the substrates 11a and 11b do not have an insulating layer, it is preferable that an insulating layer is provided between the cold / heat sources 21 and 22 and the substrates 11a and 11b.

[0039] (2) Second embodiment Fig. 2 is a schematic cross-sectional view showing another embodiment of the double-sided cooling type semiconductor device. The double-sided cooling type semiconductor device 101 shown in Fig. 2 has the same configuration as the first embodiment of the double-sided cooling type semiconductor device described above, except that there are multiple semiconductor elements.

[0040] In the double-sided cooling type semiconductor device according to the second embodiment, the height (length in the current direction) of the semiconductor element may vary (difference in height or length).

[0041] <Manufacturing method for double-sided cooled semiconductor module> The double-sided cooling semiconductor module according to the present embodiment described above can be manufactured by a method including a first bonding step of sintering a bonding material containing copper particles provided between a first substrate and a semiconductor element, and / or a second bonding step of sintering a bonding material containing copper particles provided between a second substrate and a semiconductor element.

[0042] When manufacturing the double-sided cooling type semiconductor module according to the first embodiment, a bonding material is applied to the bonding position of the substrate 11a with the semiconductor element 1, the semiconductor element 1 is brought into contact with the coating film formed by drying as necessary, using a jig as necessary, and this coating film (bonding layer) is baked (first bonding step), a bonding material is applied to the bonding surface of the semiconductor element 1 with the spacer 41, the spacer 41 is brought into contact with the coating film formed by drying as necessary, using a jig as necessary, a bonding material is applied to the bonding surface of the spacer 41 with the substrate, the substrate 11b is brought into contact with the coating film formed by drying as necessary, using a jig as necessary, and these coating films (bonding layers) are baked (second bonding step). In this embodiment, the baking of the coating film in the first bonding step and the baking of the coating film in the second bonding step may be performed simultaneously.

[0043] The bonding material may be a copper paste containing copper particles and a dispersion medium.

[0044] Copper particles include submicro copper particles and micro copper particles. Submicro copper particles refer to copper particles having a particle size of 0.01 μm or more and less than 1.00 μm. Micro copper particles refer to copper particles having a particle size of 1 μm or more and less than 50 μm.

[0045] The particle size of copper particles can be determined by the following method. The particle size of copper particles can be calculated, for example, from an SEM image. A powder of copper particles is placed on a carbon tape for SEM with a spatula to prepare a sample for SEM. This sample for SEM is observed at 5000 times magnification with an SEM device. A rectangle circumscribing the copper particle in this SEM image is drawn using image processing software, and one side of the rectangle is taken as the particle size of the particle.

[0046] (Submicron copper particles) The submicro copper particles include copper particles having a particle size of 0.12 μm or more and 0.8 μm or less, and for example, copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less can be used. If the volume average particle size of the submicro copper particles is 0.12 μm or more, effects such as reduction in the synthesis cost of the submicro copper particles, good dispersibility, and reduction in the amount of surface treatment agent used can be easily obtained. If the volume average particle size of the submicro copper particles is 0.8 μm or less, the effect of excellent sinterability of the submicro copper particles can be easily obtained. From the viewpoint of further achieving the above effect, the volume average particle size of the submicro copper particles may be 0.15 μm or more and 0.8 μm or less, 0.15 μm or more and 0.6 μm or less, 0.2 μm or more and 0.5 μm or less, or 0.3 μm or more and 0.45 μm or less.

[0047] In the present specification, the volume average particle diameter means a 50% volume average particle diameter. The volume average particle diameter of copper particles can be determined by a method in which raw copper particles or dried copper particles obtained by removing volatile components from a bonding material are dispersed in a dispersion medium using a dispersant, and the resulting dispersion medium is measured using a light scattering particle size distribution measuring device (for example, Shimadzu nanoparticle size distribution measuring device (SALD-7500nano, manufactured by Shimadzu Corporation)). When using a light scattering particle size distribution measuring device, hexane, toluene, α-terpineol, etc. can be used as the dispersion medium.

[0048] The sub-micro copper particles may contain 10% by mass or more of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. From the viewpoint of sintering property of the bonding material, the sub-micro copper particles may contain 20% by mass or more, 30% by mass or more, or 100% by mass of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. When the content ratio of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less in the sub-micro copper particles is 20% by mass or more, the dispersibility of the copper particles is further improved, and the increase in viscosity and the decrease in paste concentration can be further suppressed.

[0049] The content of the sub-micro copper particles may be 20% by mass or more and 90% by mass or less, 30% by mass or more and 90% by mass or less, 35% by mass or more and 85% by mass or less, or 40% by mass or more and 80% by mass or less, based on the total mass of the metal particles contained in the bonding material. If the content of the sub-micro copper particles is within the above range, it is easy to form the bonding part according to the present embodiment described above.

[0050] In addition, when the bonding material of the present embodiment includes submicro copper particles and flaky micro copper particles as copper particles, the content of the submicro copper particles may be 20% by mass or more and 90% by mass or less based on the total mass of the submicro copper particles and the flaky micro copper particles. If the content of the submicro copper particles is 20% by mass or more, the gaps between the flaky micro copper particles can be sufficiently filled, and it is easy to form the bonding part according to the present embodiment described above. If the content of the submicro copper particles is 90% by mass or less, the volumetric shrinkage when the bonding material is sintered can be sufficiently suppressed, and it is easy to form the bonding part according to the present embodiment described above. From the viewpoint of further achieving the above effect, the content of the submicro copper particles may be 30% by mass or more and 85% by mass or less, 35% by mass or more and 85% by mass or less, or 40% by mass or more and 80% by mass or less based on the total mass of the submicro copper particles and the flaky micro copper particles.

[0051] The shape of the submicro copper particles is not particularly limited. The shape of the submicro copper particles can be, for example, spherical, clumpy, needle-like, flake-like, roughly spherical, or aggregates thereof. From the viewpoint of dispersibility and packing, the shape of the submicro copper particles can be spherical, roughly spherical, or flake-like, and from the viewpoint of combustibility, dispersibility, mixability with flake-like microparticles, etc., it can be spherical or roughly spherical.

[0052] From the viewpoints of dispersibility, packing property, and mixability with flake-shaped microparticles, the sub-micro copper particles may have an aspect ratio of 5 or less, or 3 or less. In this specification, the "aspect ratio" refers to the long side / thickness of a particle. The long side and thickness of a particle can be measured, for example, from an SEM image of the particle.

[0053] The submicron copper particles may be treated with a specific surface treatment agent. Examples of the specific surface treatment agent include organic acids having 8 to 16 carbon atoms. Examples of organic acids having 8 to 16 carbon atoms include caprylic acid, methylheptanoic acid, ethylhexanoic acid, propylpentanoic acid, pelargonic acid, methyloctanoic acid, ethylheptanoic acid, propylhexanoic acid, capric acid, methylnonanoic acid, ethyloctanoic acid, propylheptanoic acid, butylhexanoic acid, undecanoic acid, methyldecanoic acid, ethylnonanoic acid, propyloctanoic acid, butylheptanoic acid, lauric acid, methylundecanoic acid, ethyldecanoic acid, propylnonanoic acid, butyloctanoic acid, Saturated fatty acids such as pentylheptanoic acid, tridecanoic acid, methyldodecanoic acid, ethylundecanoic acid, propyldecanoic acid, butylnonanoic acid, pentyloctanoic acid, myristic acid, methyltridecanoic acid, ethyldodecanoic acid, propylundecanoic acid, butyldecanoic acid, pentylnonanoic acid, hexyloctanoic acid, pentadecanoic acid, methyltetradecanoic acid, ethyltridecanoic acid, propyldodecanoic acid, butylundecanoic acid, pentyldecanoic acid, hexylnonanoic acid, palmitic acid, methylpentadecanoic acid, ethyltetradecanoic acid, propyltridecanoic acid, butyldodecanoic acid, pentylundecanoic acid, hexyldecanoic acid, heptylnonanoic acid, methylcyclohexanecarboxylic acid, ethylcyclohexanecarboxylic acid, propylcyclohexanecarboxylic acid, butylcyclohexanecarboxylic acid, pentylcyclohexanecarboxylic acid, hexylcyclohexanecarboxylic acid, heptylcyclohexanecarboxylic acid, octylcyclohexanecarboxylic acid, and nonylcyclohexanecarboxylic acid; octene Examples of the organic acid include unsaturated fatty acids such as benzoic acid, nonenoic acid, methylnonenoic acid, decenoic acid, undecenoic acid, dodecenoic acid, tridecenoic acid, tetradecenoic acid, myristoleic acid, pentadecenoic acid, hexadecenoic acid, palmitoleic acid, and sabienoic acid; and aromatic carboxylic acids such as terephthalic acid, pyromellitic acid, o-phenoxybenzoic acid, methylbenzoic acid, ethylbenzoic acid, propylbenzoic acid, butylbenzoic acid, pentylbenzoic acid, hexylbenzoic acid, heptylbenzoic acid, octylbenzoic acid, and nonylbenzoic acid. The organic acid may be used alone or in combination of two or more.By combining such an organic acid with the sub-micron copper particles, it tends to be possible to achieve both the dispersibility of the sub-micron copper particles and the desorption property of the organic acid during sintering.

[0054] The amount of the surface treatment agent to be applied may be an amount that adheres to the surface of the sub-micro copper particles in one to three molecular layers. This amount depends on the number of molecular layers (n) attached to the surface of the sub-micro copper particles, the specific surface area (Ap) of the sub-micro copper particles (unit: m 2 / g), the molecular weight (Ms) of the surface treatment agent (unit: g / mol), and the minimum coverage area (SS) of the surface treatment agent (unit: m 2 / piece) and Avogadro's number (NA) (6.02 × 10 23 Specifically, the amount of surface treatment agent is calculated according to the formula: Amount of surface treatment agent (mass%) = {(n·Ap·Ms) / (SS·NA+n·Ap·Ms)}×100%.

[0055] The specific surface area of ​​the submicro copper particles can be calculated by measuring the dried submicro copper particles using the BET specific surface area measurement method. The minimum coverage area of ​​the surface treatment agent is 2.05 × 10 -19 m 2 / 1 molecule. In the case of other surface treatment agents, for example, it can be measured by calculation from a molecular model or the method described in "Chemistry and Education" (Katsuhiro Ueda, Sumio Inafuku, Iwao Mori, 40 (2), 1992, p114-117). An example of a method for quantifying the surface treatment agent is shown below. The surface treatment agent can be identified by a thermal desorption gas-gas chromatograph mass spectrometer of the dried powder obtained by removing the dispersing medium from the bonding material, and the carbon number and molecular weight of the surface treatment agent can be determined. The carbon content of the surface treatment agent can be analyzed by carbon content analysis. Examples of carbon content analysis methods include high-frequency induction heating furnace combustion / infrared absorption method. The amount of the surface treatment agent can be calculated from the carbon number, molecular weight and carbon content of the identified surface treatment agent using the above formula.

[0056] The treatment amount of the surface treatment agent may be 0.07% by mass or more and 2.1% by mass or less, 0.10% by mass or more and 1.6% by mass or less, or 0.2% by mass or more and 1.1% by mass or less.

[0057] Submicro copper particles can be commercially available. Commercially available submicro copper particles include, for example, CH-0200 (manufactured by Mitsui Mining & Smelting Co., Ltd., volume average particle diameter 0.36 μm), HT-14 (manufactured by Mitsui Mining & Smelting Co., Ltd., volume average particle diameter 0.41 μm), CT-500 (manufactured by Mitsui Mining & Smelting Co., Ltd., volume average particle diameter 0.72 μm), and Tn-Cu100 (manufactured by Taiyo Nippon Sanso Co., Ltd., volume average particle diameter 0.12 μm).

[0058] (Micro copper particles) The micro copper particles include copper particles having a particle size of 1.0 μm to 50 μm, and for example, copper particles having a volume average particle size of 1.0 μm to 50 μm can be used. The volume average particle size of the micro copper particles may be 2.0 μm to 20 μm, 2.0 μm to 10 μm, 3.0 μm to 20 μm, or 3.0 μm to 10 μm.

[0059] The shape of the micro copper particles may be, for example, spherical, blocky, needle-like, flake-like, roughly spherical, or an aggregate thereof. Among these, flake-like is preferred. The flake-like includes flat shapes such as plate-like and scale-like.

[0060] The flake-shaped micro copper particles include copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more. For example, copper particles having an average maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be used. If the average maximum diameter and aspect ratio of the flake-shaped micro copper particles are within the above range, the volume shrinkage when the bonding material is sintered can be sufficiently reduced, and it becomes easy to form the bonding part according to the above-mentioned embodiment. From the viewpoint of further achieving the above effect, the average maximum diameter of the flake-shaped micro copper particles may be 1 μm or more and 10 μm or less, or 3 μm or more and 10 μm or less. The maximum diameter and average maximum diameter of the flake-shaped micro copper particles can be measured, for example, from an SEM image of the particles, and are obtained as the major axis X and the average major axis Xav of the flake-shaped structure described later.

[0061] The flake-shaped micro copper particles may contain 50% by mass or more of copper particles having a maximum diameter of 1 μm or more and 20 μm or less. From the viewpoints of orientation in the bonded body, reinforcing effect, and filling property of the bonding paste, the flake-shaped micro copper particles may contain 70% by mass or more, 80% by mass or more, or 100% by mass of copper particles having a maximum diameter of 1 μm or more and 20 μm or less. From the viewpoint of suppressing bonding failure, it is preferable that the flake-shaped micro copper particles do not contain particles having a size exceeding the bonding thickness, such as particles having a maximum diameter exceeding 20 μm.

[0062] A method for calculating the major axis X of a flake-shaped micro copper particle from an SEM image is exemplified. A powder of flake-shaped micro copper particles is placed on a carbon tape for SEM with a spatula to prepare a sample for SEM. This sample for SEM is observed at 5000 times magnification with an SEM device. A rectangle circumscribing the flake-shaped micro copper particle in the SEM image is drawn with image processing software, and the long side of the rectangle is taken as the major axis X of the particle. This measurement is performed on 50 or more flake-shaped micro copper particles using multiple SEM images, and the average major axis value Xav is calculated.

[0063] The aspect ratio of the flaky micro copper particles may be 4 or more, or may be 6 or more. If the aspect ratio is within the above range, the flaky micro copper particles in the bonding material are oriented approximately parallel to the bonding surface, thereby suppressing the volumetric shrinkage when the bonding layer (bonding material) is sintered, and it becomes easy to form the bonding part according to the present embodiment described above.

[0064] The shape of the flake-shaped micro copper particles according to this embodiment can also be specified by parameters of the major axis (average maximum diameter) X, the middle axis (width) Y, and the minor axis (thickness) T. The major axis X is the distance between two parallel planes selected so that the distance between the two parallel planes is maximum among the two parallel planes circumscribing the flake-shaped micro copper particles in the three-dimensional shape of the flake-shaped micro copper particles. The middle axis Y is the distance between two parallel planes that are perpendicular to the two parallel planes that give the major axis X and that are selected so that the distance between the two parallel planes is maximum among the two parallel planes circumscribing the flake-shaped micro copper particles. The minor axis T is the distance between two parallel planes that are perpendicular to the two parallel planes that give the major axis X and the two parallel planes that give the middle axis Y, and that are selected so that the distance between the two parallel planes is maximum among the two parallel planes circumscribing the flake-shaped micro copper particles.

[0065] The average value Xav of the major axis may be 1 μm or more and 50.0 μm or less, 1 μm or more and 20 μm or less, or 3 μm or more and 10 μm or less. When Xav is within the above range, in the bonded body produced by sintering the bonding material, the sintered body of the bonding material can be easily formed with an appropriate thickness.

[0066] The ratio (aspect ratio) of the average major axis Xav to the average minor axis Tav may be 4.0 or more, 6.0 or more, or 10.0 or more. When Xav / Tav is within the above range, the flake-shaped micro copper particles in the bonding material are easily oriented substantially parallel to the bonding surface, and the volumetric shrinkage when the bonding material is sintered can be suppressed, making it easy to ensure the bonding strength of the bonded body produced by sintering the bonding material.

[0067] The ratio of the average major axis Xav to the average middle axis Yav, Xav / Yav, may be 2.0 or less, 1.7 or less, or 1·5 or less. If Xav / Yav is within the above range, the shape of the flaky micro copper particles becomes a flaky particle having a certain area, and the flaky micro copper particles in the bonding material are easily oriented approximately parallel to the bonding surface, so that the volumetric shrinkage when the bonding material is sintered can be suppressed, and it is easy to ensure the bonding strength of the bonded body produced by sintering the bonding material. If Xav / Yav exceeds 2.0, it means that the shape of the flaky micro copper particles approaches a long and thin line shape.

[0068] The ratio Yav / Tav of the average medium diameter Yav to the average short diameter Tav may be 2.5 or more, 4.0 or more, or 8.0 or more. When Yav / Tav is within the above range, the flake-shaped micro copper particles in the bonding material are easily oriented substantially parallel to the bonding surface, the volumetric shrinkage when the bonding material is sintered can be suppressed, and the bonding strength of the bonded body produced by sintering the bonding material can be easily ensured.

[0069] The content of the flake micro copper particles may be 1% by mass or more and 90% by mass or less, 10% by mass or more and 70% by mass or less, or 20% by mass or more and 50% by mass or less, based on the total mass of the metal particles. If the content of the flake micro copper particles is within the above range, it is easy to form the joint according to the present embodiment described above.

[0070] When the bonding material of the present embodiment includes submicro copper particles and flaky micro copper particles as copper particles, the total content of the submicro copper particles and the flaky micro copper particles may be 80% by mass or more based on the total mass of the metal particles. If the total content of the submicro copper particles and the flaky micro copper particles is within the above range, it is easy to form the bonding part according to the present embodiment. From the viewpoint of further achieving the above effect, the total content of the submicro copper particles and the flaky micro copper particles may be 90% by mass or more, 95% by mass or more, or 100% by mass based on the total mass of the metal particles.

[0071] In the flake-shaped micro copper particles, the presence or absence of treatment with a surface treatment agent is not particularly limited. From the viewpoint of dispersion stability and oxidation resistance, the flake-shaped micro copper particles may be treated with a surface treatment agent. The surface treatment agent may be one that is removed during bonding. Examples of such surface treatment agents include aliphatic carboxylic acids such as palmitic acid, stearic acid, arachidic acid, and oleic acid; aromatic carboxylic acids such as terephthalic acid, pyromellitic acid, and o-phenoxybenzoic acid; aliphatic alcohols such as cetyl alcohol, stearyl alcohol, isobornylcyclohexanol, and tetraethylene glycol; aromatic alcohols such as p-phenylphenol; alkylamines such as octylamine, dodecylamine, and stearylamine; aliphatic nitriles such as stearonitrile and decanenitrile; silane coupling agents such as alkylalkoxysilanes; and polymer treatment materials such as polyethylene glycol, polyvinyl alcohol, polyvinylpyrrolidone, and silicone oligomers. The surface treatment agent may be used alone or in combination of two or more.

[0072] The amount of the surface treatment agent may be more than one molecular layer on the particle surface. The amount of the surface treatment agent varies depending on the specific surface area of ​​the flaky micro copper particles, the molecular weight of the surface treatment agent, and the minimum coverage area of ​​the surface treatment agent. The amount of the surface treatment agent is usually 0.001% by mass or more. The specific surface area of ​​the flaky micro copper particles, the molecular weight of the surface treatment agent, and the minimum coverage area of ​​the surface treatment agent can be calculated by the above-mentioned method.

[0073] By using sub-micro copper particles and flaky micro copper particles in combination, the volumetric shrinkage when the bonding material is sintered is suppressed, making the bonding material less likely to peel off from the bonding surface when sintered, making it easier to achieve sufficient bonding strength and reliability when bonding semiconductor elements, etc.

[0074] In the bonding material of this embodiment, the content of micro copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is preferably 50 mass % or less, more preferably 40 mass % or less, and even more preferably 30 mass % or less, based on the total amount of flake-shaped micro copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more. By limiting the content of micro copper particles having an average maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2, the flake-shaped micro copper particles in the bonding material are easily oriented approximately parallel to the bonding surface, and the volume shrinkage when the bonding material is sintered can be more effectively suppressed. This makes it easier to form the bonding part according to the present embodiment described above. In order to make such effects even easier to obtain, the content of micro copper particles having an average maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 may be 20 mass % or less, or 10 mass % or less, based on the total amount of flaky micro copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more.

[0075] The flake-shaped micro copper particles according to the present embodiment can be commercially available. Examples of commercially available flake-shaped micro copper particles include MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd., average maximum diameter 4.1 μm), 3L3 (manufactured by Fukuda Metal Foil & Powder Co., Ltd., volume maximum diameter 7.3 μm), 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd., average maximum diameter 5.8 μm), and 2L3 (manufactured by Fukuda Metal Foil & Powder Co., Ltd., average maximum diameter 9 μm).

[0076] In the bonding material of this embodiment, the micro copper particles to be blended include flake-shaped micro copper particles having a maximum diameter of 1 μm or more and an aspect ratio of 4 or more, and the content of the micro copper particles having a maximum diameter of 1 μm or more and an aspect ratio of less than 2 is 50% by mass or less, preferably 30% by mass or less, based on the total amount of the flake-shaped micro copper particles. When using commercially available flake-shaped micro copper particles, those having a maximum diameter of 1 μm or more and an aspect ratio of 4 or more, including flake-shaped micro copper particles, and having a maximum diameter of 1 μm or more and an aspect ratio of less than 2 may be selected as the flake-shaped micro copper particles having a content of 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total amount of the flake-shaped micro copper particles.

[0077] The bonding material may contain metal particles other than copper particles, such as nickel, silver, gold, palladium, platinum, etc.

[0078] The volume average particle size of the other metal particles may be 0.01 μm or more and 10 μm or less, 0.01 μm or more and 5 μm or less, or 0.05 μm or more and 3 μm or less. When the other metal particles are contained, the content thereof may be less than 20 mass% or may be 10 mass% or less based on the total mass of the metal particles contained in the bonding material from the viewpoint of obtaining sufficient bonding properties. The other metal particles may not be contained. The shape of the other metal particles is not particularly limited.

[0079] By including metal particles other than copper particles in the bonding material of the present embodiment, a sintered metal layer in which multiple types of metals are dissolved or dispersed can be obtained, and the mechanical properties of the bonded portion, such as yield stress and fatigue strength, are improved, and connection reliability is likely to be improved. In addition, by adding multiple types of metal particles, the bonded portion formed is likely to have improved bonding strength and connection reliability with respect to adherends such as semiconductor elements and substrates.

[0080] (dispersion medium) The dispersion medium is not particularly limited, and may be volatile. Examples of volatile dispersion media include monohydric and polyhydric alcohols such as pentanol, hexanol, heptanol, octanol, decanol, ethylene glycol, diethylene glycol, propylene glycol, butylene glycol, α-terpineol, and isobornylcyclohexanol (MTPH); ethylene glycol butyl ether, ethylene glycol phenyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol isobutyl ether, diethylene glycol hexyl ether, triethylene glycol methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl ether, diethylene glycol isopropyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl ether, propylene glycol propyl ether, and dipropylene glycol. Examples of the esters include methyl ether, dipropylene glycol ethyl ether, dipropylene glycol propyl ether, dipropylene glycol butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol methyl ether, and tripropylene glycol dimethyl ether; esters such as ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl ether acetate (DPMA), ethyl lactate, butyl lactate, γ-butyrolactone, and propylene carbonate; acid amides such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide; aliphatic hydrocarbons such as cyclohexane, octane, nonane, decane, and undecane; aromatic hydrocarbons such as benzene, toluene, and xylene; mercaptans having an alkyl group having 1 to 18 carbon atoms; and mercaptans having a cycloalkyl group having 5 to 7 carbon atoms.Examples of mercaptans having an alkyl group having 1 to 18 carbon atoms include ethyl mercaptan, n-propyl mercaptan, i-propyl mercaptan, n-butyl mercaptan, i-butyl mercaptan, t-butyl mercaptan, pentyl mercaptan, hexyl mercaptan, and dodecyl mercaptan. Examples of mercaptans having a cycloalkyl group having 5 to 7 carbon atoms include cyclopentyl mercaptan, cyclohexyl mercaptan, and cycloheptyl mercaptan.

[0081] The content of the dispersion medium may be 5 to 50 parts by mass, with the total mass of the metal particles contained in the bonding material being 100 parts by mass. If the content of the dispersion medium is within the above range, the bonding material can be adjusted to a more appropriate viscosity, and sintering of the copper particles is less likely to be hindered.

[0082] In the present embodiment, the dispersion medium preferably contains a solvent having a boiling point of 300° C. or higher. From the viewpoint of not impeding sintering and densification during sintering of the coating film (bonding layer) and being quickly evaporated and removed when the bonding temperature is reached, the boiling point of the solvent having a boiling point of 300° C. or higher may be 300° C. or higher and 450° C. or lower, 305° C. or higher and 400° C. or lower, or 310° C. or higher and 380° C. or lower.

[0083] It is preferable to select a solvent having a boiling point of 300° C. or higher that has a structure with high affinity for the surface of metal particles in order to improve the dispersibility of the metal particles contained therein. When the metal particles are surface-treated with a surface treatment agent containing an alkyl group, it is preferable to select a solvent having an alkyl group. Examples of such solvents having a boiling point of 300°C or higher include isobornylcyclohexanol (MTPH, manufactured by Nippon Terpene Co., Ltd.), butyl stearate, Exepar BS (manufactured by Kao Corporation), stearyl stearate, Exepar SS (manufactured by Kao Corporation), 2-ethylhexyl stearate, Exepar EH-S (manufactured by Kao Corporation), isotridecyl stearate, Exepar TD-S (manufactured by Kao Corporation), isooctadecanol, Fine Oxocol 180 (manufactured by Nissan Chemical Industries, Ltd.), Fine Oxocol 180T (manufactured by Nissan Chemical Industries, Ltd.), 2-hexyldecanol, Fine Oxocol 1600 (manufactured by Nissan Chemical Industries, Ltd.), tributyrin, tetraethylene glycol, heptadecane, octadecane, nonadecane, eicosane, heneicosane, docosane, methylheptadecane, tridecyl Examples of the cyclohexane, tetradecylcyclohexane, pentadecylcyclohexane, hexadecylcyclohexane, undecylbenzene, dodecylbenzene, tetradecylbenzene, tridecylbenzene, pentadecylbenzene, hexadecylbenzene, heptadecylbenzene, nonylnaphthalene, diphenylpropane, octyl octanoate, methyl myristate, ethyl myristate, methyl linoleate, methyl stearate, triethylene glycol bis(2-ethylhexanoic acid), tributyl citrate, pentylphenol, dibutyl sebacate, oleyl alcohol, cetyl alcohol, methoxyphenethyl alcohol, benzylphenol, hexadecanenitrile, heptadecyl nitrile, benzyl benzoate, and cinmethylin.

[0084] From the viewpoint of improving dispersibility, it is preferable to select a solvent having a boiling point of 300°C or higher that has a Hansen solubility parameter close to that of the surface treatment agent. Since organic acids, organic amines, hydroxyl group-containing polymers, polyvinylpyrrolidone, etc. are easy to handle as surface treatment agents, it is preferable that the solvent having a boiling point of 300°C or higher has at least one group selected from the group consisting of hydroxyl groups, ether groups, and ester groups. The Hansen solubility parameters can be searched, for example, from the database at the end of the handbook, or searched / calculated using the database and simulation integrated software HSPiP.

[0085] The content of the solvent having a boiling point of 300° C. or more can be 2% by mass or more based on the total mass of the bonding material. The content of the solvent having a boiling point of 300° C. or more can be 2.2% by mass or more, 2.3% by mass or more, or 2.4% by mass or more based on the total mass of the bonding material. If the content of the solvent having a boiling point of 300° C. or more is within the above range, when the coating film (bonding layer) of this embodiment is sintered, a certain amount of the solvent can remain in the bonding layer, and the flexibility and adhesion of the bonding material between the members can be easily maintained, and even if the members used for bonding have different thermal expansion coefficients, they tend to be bonded without peeling. The upper limit of the content of the solvent having a boiling point of 300° C. or more is not particularly limited. From the viewpoint of suppressing the time until the dispersion medium is removed at the sintering temperature and shortening the sintering time, it may be 9% by mass or less based on the total mass of the bonding material.

[0086] In addition, in the bonding material of this embodiment, the content of the solvent having a boiling point of 300°C or more may be 15% by volume or more, 17% by volume or more, or 23% by volume or more based on the total volume of the bonding material. If the content of the solvent having a boiling point of 300°C or more is within the above range, when the coating film (bonding layer) of this embodiment is sintered, a certain amount of the solvent can remain in the coating film (bonding layer), and the flexibility and adhesion of the bonding material between the members are easily maintained, and even if the members used for bonding have different thermal expansion coefficients, they tend to be bonded without peeling. The upper limit of the content of the solvent having a boiling point of 300°C or more is not particularly limited. From the viewpoint of suppressing the time until the dispersion medium is removed at the sintering temperature and shortening the sintering time, it may be 60% by volume or less based on the total volume of the bonding material.

[0087] The type of dispersion medium contained in the bonding material can be analyzed, for example, by gas chromatography-mass spectrometry of high-temperature desorbed gas and TOF-SIMS. As another analytical method, the supernatant obtained by separating the particle components by centrifugation may be identified by ordinary organic analysis, for example, FT-IR, NMR, liquid chromatography, or a combination of these. The ratio of the types of dispersion medium can be quantified by liquid chromatography, NMR, etc.

[0088] (Additives) If necessary, the bonding material may contain appropriate additives such as a wetting improver such as a nonionic surfactant or a fluorine-based surfactant; an antifoaming agent such as silicone oil; and an ion trapping agent such as an inorganic ion exchanger.

[0089] (Preparation of bonding material) The bonding material may be prepared by mixing the above-mentioned submicro copper particles, micro copper particles, other metal particles, and any additives in a dispersion medium. After mixing the components, a stirring process may be performed. The bonding material may be adjusted in maximum particle size by a classification operation.

[0090] The bonding material may be prepared by mixing sub-micro copper particles, a surface treatment agent, and a dispersion medium in advance, performing a dispersion treatment to prepare a dispersion of sub-micro copper particles, and further mixing micro copper particles, other metal particles, and any additives. By using such a procedure, the dispersibility of the sub-micro copper particles is improved, and the mixability with the micro copper particles is improved, and the performance of the bonding material is further improved. The dispersion of the sub-micro copper particles may be classified to remove aggregates.

[0091] Methods for applying the bonding material include stencil printing, dispenser, screen printing, transfer printing, offset printing, jet printing, jet dispenser, needle dispenser, comma coater, slit coater, die coater, gravure coater, slit coat, letterpress printing, intaglio printing, gravure printing, soft lithography, bar coat, applicator, particle deposition method, spray coater, spin coater, dip coater, and electrodeposition coating.

[0092] The thickness of the coating film may be 1 μm or more and 1000 μm or less, 10 μm or more and 1000 μm or less, 10 μm or more and 500 μm or less, 50 μm or more and 200 μm or less, 10 μm or more and 3000 μm or less, 15 μm or more and 500 μm or less, 20 μm or more and 300 μm or less, 5 μm or more and 500 μm or less, 10 μm or more and 250 μm or less, or 15 μm or more and 150 μm or less.

[0093] From the viewpoint of the effect of absorbing the variation in height of the semiconductor element or the variation in the distance between the substrates, and from the viewpoint of printing accuracy, the thickness is preferably 10 μm or more and 1000 μm or less. When the thickness of the coating film is 10 μm or more, it becomes easy to obtain the effect of absorbing the variation in height, and when it is 1000 μm or less, it becomes easy to ensure the printing accuracy.

[0094] The coating film may be dried by leaving it at room temperature, by heating, or by drying under reduced pressure. For example, a hot plate, a hot air dryer, a hot air heating furnace, a nitrogen dryer, an infrared ray dryer, an infrared heating furnace, a far-infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, a hot plate press device, etc. may be used for drying by heating or drying under reduced pressure. The drying temperature and time may be appropriately adjusted according to the type and amount of the dispersion medium used. The drying temperature and time may be, for example, 50°C or higher and 180°C or lower for 1 minute to 120 minutes.

[0095] The coating film (bonding layer) can be sintered by a heat treatment, which can be performed using, for example, a hot plate, a hot air dryer, a hot air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far-infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, or the like.

[0096] The gas atmosphere during sintering may be an oxygen-free atmosphere from the viewpoint of suppressing oxidation. The gas atmosphere during sintering may be a reducing atmosphere from the viewpoint of removing surface oxides of copper particles. Examples of the oxygen-free atmosphere include the introduction of an oxygen-free gas such as nitrogen or a rare gas, or a vacuum. Examples of the reducing atmosphere include a pure hydrogen gas, a mixed gas of hydrogen and nitrogen such as forming gas, nitrogen containing formic acid gas, a mixed gas of hydrogen and a rare gas, and a rare gas containing formic acid gas.

[0097] From the viewpoint of reducing thermal damage to the components constituting the power card or double-sided cooling module and improving the yield, the maximum temperature reached during the heat treatment may be 250° C. or higher and 450° C. or lower, 250° C. or higher and 400° C. or lower, or 250° C. or higher and 350° C. or lower. If the maximum temperature reached is 200° C. or higher, sintering tends to proceed sufficiently when the maximum temperature is held for 60 minutes or less.

[0098] The time for which the maximum temperature is maintained may be 1 minute or more and 60 minutes or less, or may be 1 minute or more and less than 40 minutes, or may be 1 minute or more and less than 30 minutes, from the viewpoint of volatilizing all of the dispersion medium and improving the yield.

[0099] In this embodiment, from the viewpoint of reducing the bonding material mainly composed of copper particles and reducing thermal stress occurring between the substrate and the semiconductor element, it is preferable to heat the bonding material at 350° C. or less in hydrogen having a concentration of 1% or more.

[0100] The coating film (bonding layer) can be sintered under a load of 0 to 100 MPa. In this embodiment, bonding can be performed without pressure. In this specification, "without pressure" means a state in which the members to be bonded are subjected to a pressure of 0.01 MPa or less in addition to the weight of the members to be bonded.

[0101] When the bonding material (copper paste) contains copper particles and a dispersion medium, the copper particles include sub-micro copper particles having a volume average particle size of 0.01 μm or more and 0.8 μm or less, and micro copper particles having a volume average particle size of 2.0 μm or more and 50 μm or less, the sum of the content of the sub-micro copper particles and the content of the micro copper particles is 80 mass % or more based on the total mass of the metal particles contained in the bonding material, the content of the sub-micro copper particles is 30 mass % or more and 90 mass % or less based on the total mass of the sub-micro copper particles and the micro copper particles, and the content of the micro copper particles is 10 mass % or more and 50 mass % or less based on the total mass of the metal particles contained in the bonding material, sufficient bonding strength can be obtained even when bonding is performed without applying pressure.

[0102] The reason for the above is that by containing sub-micro copper particles and micro copper particles in a specific ratio in the bonding material, it is possible to sufficiently suppress the volumetric shrinkage during sintering caused by the surface protective agent or dispersion medium while maintaining sufficient sinterability, thereby ensuring the strength of the sintered body and improving the bonding strength with the adherend surface.

[0103] In addition, since the above-mentioned bonding material can obtain the above-mentioned effects by using submicro copper particles and micro copper particles, it has the advantage that it can be supplied more cheaply and stably than a bonding material mainly composed of expensive copper nanoparticles.

[0104] Furthermore, the micro copper particles are preferably flake-shaped. Using flake-shaped micro copper particles makes it easier to reduce the thermal stress occurring between the semiconductor element and the substrate. The reason for this effect is that the micro copper particles in the bonding material are oriented approximately parallel to the bonding surface, thereby suppressing the volumetric shrinkage when the bonding material is sintered, the overlapping area of ​​the flake-shaped micro copper particles is increased, thereby improving the bonding strength, and the flake-shaped micro copper particles align the sub-micro copper particles to obtain a reinforcing effect.

[0105] After bonding, the bonding material (copper paste) becomes a sintered copper body (porous body).

[0106] 3 is an enlarged cross-sectional view of a bonding portion according to this embodiment. The copper sintered body for bonding a substrate and a semiconductor element, or a semiconductor element and a spacer, is a sintered body of a bonding layer formed from a bonding material containing copper particles and a dispersion medium, in which the copper particles contain submicro copper particles and micro copper particles, and is a porous body containing a structure 31(a) derived from submicro copper particles, a structure 31(b) derived from copper particles of flaky micro copper particles as micro copper particles, and pores 31(c).

[0107] In this embodiment, the bonding layer formed from the bonding material of the embodiment described above is heated at 350° C. or less in hydrogen with a concentration of 1% or more, and the volume resistivity, thermal conductivity, and adhesive strength are each 1×10 -5 Ω·cm or less, 50W·m -1 ·K -1 By including such a sintered body in the joint, it is possible to realize a double-sided cooling type semiconductor module with excellent reliability.

[0108] The volume resistivity is calculated by the following formula. ρ=A R / L Here, ρ is the electrical resistivity per unit volume (volume resistivity) (Ω m), R is the resistance of the sintered body (Ω), and A is the cross-sectional area of ​​the sintered body (m 2 ), and L is the thickness of the sintered body (m).

[0109] The thermal conductivity can be calculated from the thermal diffusivity, specific heat capacity, and density of the joint. For example, the thermal diffusivity of the joint is measured by the laser flash method (LFA467, Netsch), and the thermal conductivity of the joint at 25°C [W / (m K)] can be calculated by multiplying this thermal diffusivity by the specific heat capacity measured by a differential scanning calorimeter (DSC8500, PerkinElmer), and the density obtained in the same manner as above.

[0110] The bonding strength can be measured using a universal bond tester (4000 series, manufactured by DAGE) or the like.

[0111] The joint may include a structure 31(b) derived from flake-like copper particles oriented approximately parallel to the interface with the electrode, and the copper content in the joint may be 65 volume % or more, based on the volume of the joint.

[0112] The structure derived from the copper particles of the flake-shaped micro copper particles according to this embodiment, i.e., the flake-shaped structure in the sintered copper having a flake-shaped structure, may have a ratio of major axis to thickness of 5 or more. The number average major axis of the flake-shaped structure may be 2 μm or more, 3 μm or more, or 4 μm or more. If the shape of the flake-shaped structure is within this range, the reinforcing effect of the flake-shaped structure contained in the joint is improved, and the double-sided cooling type semiconductor module becomes even more reliable.

[0113] The major axis and thickness of the flake-like structure can be determined, for example, from an SEM image of the bonded body (copper sintered body and semiconductor element or substrate). The following is an example of a method for measuring the major axis and thickness of the flake-like structure from an SEM image. The bonded body is poured with epoxy casting resin so that the entire sample is filled, and then hardened. The cast sample is cut near the cross section to be observed, the cross section is polished, and CP (cross section polisher) processing is performed. The cross section of the sample is observed at 5000 times with an SEM device. A cross-sectional image (e.g., 5000x) of the bonded structure is obtained, and a dense continuous part that is linear, rectangular, or ellipsoidal is taken as the longest line contained within this part, and the longest line perpendicular to this is taken as the thickness. If the longest axis is 1 μm or more and the longest axis / thickness ratio is 4 or more, the flake-like structure is considered to have a flake-like structure, and the longest axis and thickness of the flake-like structure can be measured using image processing software with a length measurement function. The average values ​​can be obtained by calculating the number average of 20 or more randomly selected points.

[0114] The major axis of the flake-like structure is given as the distance between two parallel straight lines that are selected so that the distance between the two parallel straight lines is the maximum among two parallel straight lines that circumscribe the flake-like structure, and the thickness of the flake-like structure is given as the distance between two parallel planes that are selected so that the distance between the two parallel planes is the maximum among two parallel planes that are perpendicular to the two parallel straight lines that give the major axis and circumscribe the flake-like structure.

[0115] The image processing software is not particularly limited, and for example, Microsoft PowerPoint (Microsoft Corporation) and ImageJ (National Institutes of Health) can be used.

[0116] The content ratio of the flake-like structures to the entire structure can be calculated by determining the cross-sectional area of ​​the bonded body from an SEM image of the bonded body, determining the cross-sectional area of ​​the flake-like structures from the major axis and thickness of the flake-like structures measured by the above-mentioned method, and dividing the total cross-sectional area of ​​the flake-like structures by the cross-sectional area of ​​the bonded body. In the bonded part according to this embodiment, the content ratio of the flake-like structures to the entire structure determined by the above-mentioned method may be 10 to 40%, 15 to 35%, or 20 to 30%.

[0117] The copper content (volume ratio) in the joint can be 65% by volume or more based on the volume of the joint. If the copper content in the joint is within the above range, it is possible to suppress the formation of large voids inside the joint and the sintered copper connecting the flake-shaped structures from becoming sparse. Therefore, if the copper content in the joint is within the above range, sufficient thermal conductivity is obtained and the bonding strength between the copper sintered body and the semiconductor element or substrate is improved, and the bonded body has excellent connection reliability. The copper content in the joint may be 67% by volume or more, or may be 70% by volume or more based on the volume of the joint. The copper content in the joint may be 90% by volume or less based on the volume of the joint from the viewpoint of ease of manufacturing process.

[0118] When the composition of the material that constitutes the joint is known, the copper content in the joint can be found, for example, by the following procedure. First, the joint is cut out into a rectangular parallelepiped, and the length and width of the joint are measured with a vernier caliper or external shape measuring device, and the thickness is measured with a film thickness meter to calculate the volume of the joint. The apparent density M1 (g / cm3) is calculated from the volume of the cut out joint and the weight of the joint measured with a precision balance. 3 ) is calculated. The calculated M1 and the density of copper, 8.96g / cm 3 Using these values, the copper content (volume %) in the joint can be calculated from the following formula (2). Copper content in joint (volume %) = [(M1) / 8.96] × 100 (2)

[0119] In this embodiment, after the first and second bonding steps, an electric circuit can be formed by inserting wires into the substrate, and then sealing can be performed with a resin member.

[0120] Thereafter, the cold and heat sources 21 and 22 may be abutted against the substrates 11a and 11b or bonded with a bonding material to produce a double-sided cooling type semiconductor device.

[0121] Furthermore, the manufacturing method for the double-sided cooling semiconductor module according to this embodiment may include a third bonding process in which a bonding material is applied to the bonding surface of the semiconductor element of one of the components or to the bonding position of the spacer of the other component with the semiconductor element, and then the two components are brought together and the coating of the bonding material (bonding layer) is fired.

[0122] For example, when manufacturing the double-sided cooling semiconductor module according to the second embodiment, in the third bonding step, it is preferable to abut the semiconductor element and the spacer while applying pressure in a direction in which the two components approach each other, and / or to bake the coating film (bonding layer) of the bonding material while applying pressure in a direction in which the semiconductor element and the spacer approach each other. By applying pressure in this manner, even if there is variation in the heights of the multiple semiconductor elements 1, the bonding layer having shape followability can provide sufficient bonding between each semiconductor element 1 and the substrate 11 and the spacer 41. In addition, it is possible to reduce variation in the thickness of the double-sided cooling semiconductor module after bonding. EXAMPLES

[0123] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0124] In this example, in order to evaluate the reliability of the joint in the joint, a joint between a lead frame and a Si chip was produced, and a power cycle test was performed using this joint.

[0125] The following materials were prepared to prepare the bonding material: [Metal particles] 3L3N (manufactured by Fukuda Metal Foil and Powder Co., Ltd., shape: flake, 50% volume average particle size: 6.1 μm) CH-0200 (manufactured by Mitsui Mining & Smelting Co., Ltd., shape: pseudo-spherical, surface treatment agent: lauric acid (dodecanoic acid), surface treatment amount: 0.973 mass% (based on the total mass of CH-0200), 50% volume average particle size: 0.36 μm, content of copper particles having a particle size of 0.1 μm or more and less than 1 μm: 100 mass%, content of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less: 100 mass%) Zinc flakes (Aifa Aesar, 325mesh, product name Zinc Flake) AgC239 (manufactured by Fukuda Metal Foil and Powder Co., Ltd., shape: flake, 50% volume average particle size: 7 μm) [Dispersion medium] Hydroterpineol (manufactured by Nippon Terpene Chemical Co., Ltd.) Tributyrin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Isobornylcyclohexanol (Tersolv MTPH, product name, manufactured by Nippon Terpene Chemical Co., Ltd.) Butyl stearate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0126] (zygote 1) 1.215 g of dihydroterpineol, 0.18 g of tributyrin, 2.067 g of CH-0200, 1.531 g of 3L3N, and 0.5 g of zinc flakes were added to an agate mortar and mixed until no dry powder remained, and the mixture was transferred to a plastic bottle. The sealed plastic bottle was stirred for 2000 min using a planetary vacuum mixer (Planetary Vacuum Mixer ARV-310, manufactured by Thinky Corporation). -1 (2000 rpm) for 2 minutes. The obtained paste-like mixed liquid (metal paste) was used as bonding material 1. The concentration of bonding material 1 (the ratio of the total content of CH-0200, 3L3N, and zinc flakes to the total amount of bonding material 1) was 88 mass%.

[0127] The obtained bonding material 1 was applied to a lead frame (bonding size: 19 × 25 × 3 mm) that had been electrolytically plated with Ni, using a metal squeegee to a printing thickness of 200 μm in an area (5.7 mm × 5.7 mm) that was the same size as the chip to be mounted by stencil printing. Next, a Si chip (Schottky barrier diode, SIDC32D170H, manufactured by Infinion) was mounted directly on the bonding material 1 applied to the lead frame so that the opposite side to the surface on which the plating film was applied was in contact with the bonding material 1 applied. Next, this was set in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas was flowed at 1 L / min to replace the air with argon gas. Thereafter, the temperature was raised to 300 ° C. over 30 minutes while flowing hydrogen gas at 500 mL / min, and sintering was performed under the conditions of 300 ° C. for 60 minutes, forming a sintered copper layer as a bonding part between the lead frame and the Si chip. Thereafter, the argon gas was changed to 0.3 L / min to cool the sample, and the sample was taken out into the air at 50°C or less. Next, in order to prevent the sintered copper layer from oxidizing during the test, polyimide resin (HIMAL (HL-1210) manufactured by Hitachi Chemical Co., Ltd.) was applied with a brush to the sintered copper protruding from the periphery of the Si chip, the sample was placed on a hot plate, and after covering with a Buchner funnel, it was provisionally dried at 50°C for 10 minutes while blowing N2 gas, and then it was fully dried at 200°C for 60 minutes. In this way, a sample of the bonded body 1 was produced.

[0128] (zygote 2) 1.26 g of butyl stearate and 0.54 g of isobornylcyclohexanol were placed in a plastic bottle and stirred with a mix rotor for 60 minutes to prepare mixed solution 1. Next, 18.2 g of AgC239 and mixed solution 1 were added to an agate mortar and mixed until no dry powder remained, and then transferred to a new plastic bottle. The sealed plastic bottle was stirred for 2000 min using a planetary vacuum mixer (Planetary Vacuum Mixer ARV-310, manufactured by Thinky Corporation). -1 (2000 rpm) for 1 minute. The resulting paste-like mixed liquid (metal paste) was used as the bonding material 2. The concentration of the bonding material 2 (the ratio of the content of AgC239 to the total amount of the bonding material 2) was 91 mass %.

[0129] The obtained bonding material 2 was applied to a lead frame (joint size: 19×25×3 mm) that had been electrolytically plated with Ag, using a metal squeegee to a printing thickness of 100 μm in an area (5.7 mm×5.7 mm) that was the same size as the chip to be mounted by stencil printing. Next, a Si chip (Schottky barrier diode, SIDC32D170H, manufactured by Infinion) was mounted directly on the bonding material 2 applied to the lead frame so that the opposite side to the surface on which the plating film was applied was in contact with the applied bonding material 2. Next, this was dried on a hot plate at 180° C. for 20 minutes, and then set in a thermocompression bonding device (manufactured by Ayumi Kogyo Co., Ltd.) and sintered in air under conditions of 1 minute of heating, 5 minutes at 300° C., and 20 MPa, forming a sintered silver layer between the lead frame and the Si chip as a bonding part. After that, the load was removed, and the sample was taken out at 50° C. or less. In this way, a sample of the bonding body 2 was produced.

[0130] (zygote 3) Sheet-shaped lead solder (Senju Metal Industry Co., Ltd., Pb Ag1.5 Sn0.5, thickness 100μm) was cut into an area (5.7mm x 5.7mm) the same size as the chip to be mounted, and mounted on a lead frame (joint size: 19 x 25 x 3mm). Next, a Si chip (Schottky barrier diode, SIDC32D170H, manufactured by Infinion) was mounted directly on the mounted sheet-shaped lead solder so that the opposite side to the plated surface was in contact with the mounted sheet-shaped lead solder. Next, this was set in a thermocompression bonding device (manufactured by Ayumi Industry Co., Ltd.) and subjected to reduction treatment in formic acid at 250°C for 15 minutes, and then heated in N2 until it reached 380°C. After confirming that the temperature had been reached and the solder had melted, a vacuum replacement was performed and voids in the molten solder were removed. Then, N2 gas replacement was performed while slowly cooling, and a solder layer was formed between the lead frame and the Si chip as a joint. Then, the sample was taken out at 50°C or less. In this manner, a sample of the bonded body 3 was prepared.

[0131] <Reliability evaluation of joints> The bonded assembly obtained above was subjected to the following power cycle test. [Power cycle test] The fabricated sample was clamped with a spring jig under a load of 0.3 MPa and set in a power cycle test device (custom-made product). The maximum value of the chip heat generation temperature (junction temperature, Tj) estimated from the diode characteristics (Tj max The sample was energized so that the chip temperature was 100°C (Tj min ), the conditions under which a temperature difference (ΔTj) occurs in the junction in a short time were derived. The current and time at this time were set as the test conditions, and this was repeated until the sample failed. For failure judgment, when the same current as at the start was applied to the sample, a failure was judged to have occurred when the junction temperature Tj changed by ±10% or more, and the number of cycles at this time was set as the number of failure cycles. This test was performed on n=10 samples, and a Weibull distribution analysis was performed on the obtained number of failure cycles. This Weibull distribution analysis was used to derive the relationship between the number of failure cycles and the cumulative failure rate, and the power cycle life of each junction was evaluated. The cumulative failure rate means the proportion of samples that have failed at a certain number of cycles among all samples of the same configuration.

[0132] The results of the Weibull distribution analysis for the power cycle test are summarized in Table 1. The evaluation items in the table have the following meanings. Average number of cycles: The average number of cycles to failure when multiple passer cycle tests are performed (n = 10 or more for each sample). Shape parameter m: An index for estimating the failure occurrence factor. When m<1, it indicates a random failure, and when m≧1, it indicates a failure due to deterioration. Scale parameter η: Number of failure cycles at a cumulative failure rate of 63.2%. Characteristic lifetime (vs. conjugate 3) (times): Magnification when the scale parameter η of conjugate 3 is set to 1.

[0133] [Table 1]

[0134] It was confirmed that the bonded body 1, which was bonded under pressure-free conditions using sintered copper with excellent heat dissipation properties, exhibited a characteristic life 14.2 times longer than that of the bonded body 3 using solder. In addition, the bonded body 1 has a larger characteristic life and a larger value of the shape parameter m than the bonded body 2 bonded with sintered silver, indicating that the bonded body 1 has a long life and small variation in failure timing.

[0135] According to the double-sided cooling type semiconductor module and the double-sided cooling type semiconductor device of the present invention, the reliability can be improved by using a sintered copper body at the joint between the semiconductor element and the substrate. [Explanation of symbols]

[0136] 1...semiconductor element (power device), 11a, 11b...substrate (lead frame), 21, 22...heat source, 31...copper sintered body, 41...spacer, 51...wire, 61...resin member, 100, 100'...double-sided cooled semiconductor module (power card), 101...double-sided cooled semiconductor device.

Claims

1. A method for manufacturing a double-sided cooling type semiconductor module comprising: a semiconductor element; a first substrate provided on one main surface side of the semiconductor element; a second substrate provided on the other main surface side of the semiconductor element; a first bonding portion bonding the semiconductor element to the first substrate; and a second bonding portion bonding the semiconductor element to the second substrate, wherein at least one of the first bonding portion and the second bonding portion includes a copper sintered body, and the copper sintered body is a sintered body of a bonding material including copper particles, A first bonding step of sintering a bonding material containing copper particles provided between the first substrate and the semiconductor element, and / or a second bonding step of sintering a bonding material containing copper particles provided between the second substrate and the semiconductor element, The bonding material includes sub-micro copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less, and flake-shaped micro copper particles having a volume average particle size of 1.0 μm or more and 50 μm or less, The content of the submicro copper particles and the content of the flaky micro copper particles are 30% by mass or more and 90% by mass or less and 10% by mass or more and 70% by mass or less, respectively, based on the total mass of the metal particles contained in the bonding material; A method for manufacturing a double-sided cooling type semiconductor module, wherein the bonding material contains a solvent having a boiling point of 300°C or higher in a proportion of 2 mass% or more based on the total mass of the bonding material.

2. The method for manufacturing a double-sided cooled semiconductor module according to claim 1 , wherein the double-sided cooled semiconductor module has two or more semiconductor elements.

3. The method for manufacturing a double-sided cooling type semiconductor module according to claim 1 , wherein one or more of the first bonding portion and the second bonding portion include a spacer.

4. 4. The method for manufacturing a double-sided cooling type semiconductor module according to claim 1, wherein the first bonding step and / or the second bonding step are performed without applying pressure.

5. A method for manufacturing a double-sided cooling type semiconductor device comprising: a double-sided cooling type semiconductor module including a semiconductor element, a first substrate provided on one main surface side of the semiconductor element, a second substrate provided on the other main surface side of the semiconductor element, a first bonding portion bonding the semiconductor element to the first substrate, and a second bonding portion bonding the semiconductor element to the second substrate; and a first cold / heat source and a second cold / heat source connected to the first substrate and the second substrate, respectively, of the double-sided cooling type semiconductor module, A method for producing a double-sided cooled semiconductor device, comprising the steps of: obtaining the double-sided cooled semiconductor module by the method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Copper paste for bonding and semiconductor device

    JP2018152176A

  • Power module

    JP2019021864A

  • Copper paste for pressureless bonding, bonded body and semiconductor device

    WO2018131095A1

  • Semiconductor device

    JP2017028040A

Cited By

  • Semiconductor device and heat dissipation member, and methods for manufacturing same

    WO2026121259A1

  • Semiconductor device and power conversion device using same

    WO2026154838A1