Fixed guide shoe, inclined rolling mill with the same, and method for manufacturing seamless steel pipe

The fixed guide shoe with a controlled composition and structure effectively addresses heat cracks in inclined rolling mills, enhancing productivity and reducing costs by suppressing thermal stress and crack propagation.

JP2024150951AActive Publication Date: 2024-10-24JFE STEEL CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023064010
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

Existing fixed guide shoes in inclined rolling mills suffer from heat cracks due to rapid heating and cooling, leading to splitting or breakage, which decreases seamless steel pipe productivity and increases manufacturing costs due to high alloying element content.

Method used

A fixed guide shoe with a specific component composition (C: 0.35 to 0.45%, Si: 0.70 to 1.3%, Mn: 0.2 to 0.7%, Cr: 5.0 to 10%, optionally Mo: 0.9 to 1.5%, Ni: 0.01 to 2.0%, V: 0.5 to 1.6%) and a structure with a carbide area ratio of 6% or less, along with a linear expansion coefficient of 1.5×10^-5 1/℃ or less, to suppress thermal stress and crack propagation.

Benefits of technology

The solution provides excellent heat crack resistance, reducing guide shoe replacement frequency and increasing seamless steel pipe productivity while lowering manufacturing costs by minimizing alloying elements like Cr and Ni.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150951000002
    Figure 2024150951000002
  • Figure 2024150951000003
    Figure 2024150951000003
  • Figure 2024150951000004
    Figure 2024150951000004
Patent Text Reader

Abstract

To provide a fixed guide shoe excellent in heat crack resistance and excellent in productivity of a seamless steel pipe.SOLUTION: A fixed guide shoe installed in an inclined rolling mill, the fixed guide shoe having a component composition containing, by mass percent, C:0.35-0.45%, Si:0.70-1.3%, Mn:0.2-0.7%, and Cr:5.0-10%, and a remainder consists of Fe and an unavoidable impurity and a tissue having areal ratio of carbide is 6% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fixed guide shoe installed in a tilt rolling mill, and more particularly to a fixed guide shoe having excellent heat crack resistance and excellent productivity for seamless steel pipes. [Background technology]

[0002] Figure 1 shows a schematic diagram of the steps of the Mannesmann plug mill process, which is one of the methods for manufacturing seamless steel pipes. As shown in Figure 1, a billet is heated in a rotary heating furnace and then pierced with a piercer to obtain a blank pipe. The blank pipe is then elongated and rolled in an elongator and plug mill to reduce its wall thickness, and then it is rounded with a reeler to flatten the inner surface of the blank pipe. The rounded blank pipe is then heated in a reheating furnace and sizing rolled to the specified outer diameter using a sizer to produce a seamless steel pipe.

[0003] Figure 2 shows an example of an inclined rolling mill used in the production of seamless steel pipes, with Figure 2(a) being a schematic diagram showing the configuration of a piercer and Figure 2(b) being a schematic diagram showing the configuration of an elongator. The piercer and elongator each have two rolls whose rotation axes are inclined relative to each other and a plug positioned between them. The piercer rolls the billet and the elongator rolls the blank pipe using the plug.

[0004] In such a piercer or elongator, a fixed guide shoe (fixed guide shoe) or a disk roll type guide shoe (disk roll type guide shoe) is installed as a tube guide to prevent the billet or raw tube from swinging during rolling. Figure 3 is an example of an inclined rolling mill equipped with a fixed guide shoe, and is a front view of the area where the rolls and plugs of the inclined rolling mill (piercer or elongator) are located, viewed from the rolling direction.

[0005] During rolling, the fixed guide shoe comes into contact with the material being rolled, which is heated to a high temperature. Therefore, the fixed guide shoe is rapidly heated during rolling by heat conduction from the material being rolled, and is rapidly cooled by cooling water after rolling. Repeated rapid heating and cooling can cause heat cracks in the fixed guide shoe, which can cause it to break or fracture. This requires replacing the fixed guide shoe with a new one, which reduces the productivity of seamless steel pipes.

[0006] Methods for suppressing heat cracks in guide shoes have been studied in the past. For example, Patent Document 1 discloses a guide shoe for seamless pipe piercing and rolling that contains, by weight, 0.5-2.0% C, 0.1-3.0% Si, 5-20% Mn, 20-40% Cr, and 10-20% Ni, or further contains at least one of 0.10-6.0% Mo, 0.10-6.0% W, 0.01-3.0% Nb, 0.02-3.0% V, 0.001-0.2% B, and 0.005-0.2% N, with the balance being substantially Fe. Patent Document 2 discloses a heat treatment method for a guide shoe for rolling seamless steel pipes, in which a tool steel consisting of 0.2-0.5% C, ≦1.6% Si, ≦1.1% Mn, 30-60% Ni, 25-31% Cr, ≦0.02% P, ≦0.02% S, the balance being Fe and unavoidable impurities, is heat treated in an air atmosphere at 1200-1280°C for 30-180 minutes, and subsequently heat treated in an air atmosphere at 700-900°C for 7-10 hours. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 5-17849 [Patent Document 2] JP 2007-308781 A Summary of the Invention [Problem to be solved by the invention]

[0008] The techniques described in Patent Documents 1 and 2 above are effective in suppressing heat cracks in the guide shoe, but the guide shoes proposed in these documents contain a high content of alloy elements, which increases the manufacturing costs.

[0009] SUMMARY OF THE PRESENT EMBODIMENT In view of the above problems, an object of the present invention is to provide a fixed guide shoe which has excellent heat crack resistance and excellent productivity for producing seamless steel pipes. [Means for solving the problem]

[0010] The inventors investigated the cause of the generation of heat cracks in fixed guide shoes as shown in Fig. 3. As a result, they discovered that Cr carbides, which are M7C3 type carbides that precipitate in the fixed guide shoes, serve as a propagation path for heat cracks, and that the cause is the generation of thermal stress that becomes the starting point of heat cracks when the material is subjected to repeated rapid heating and cooling.

[0011] The inventors therefore considered that it would be possible to eliminate the propagation path of heat cracks by suppressing Cr carbides, and to reduce the thermal stress that is the starting point of heat cracks by using a fixed guide shoe with a low linear expansion coefficient. The present invention was made based on the above findings, and the gist of the present invention is as follows.

[0012] [1] A fixed guide shoe installed on a tilt rolling mill, A composition containing, by mass%, C: 0.35-0.45%, Si: 0.70-1.3%, Mn: 0.2-0.7%, Cr: 5.0-10%, with the balance being Fe and unavoidable impurities; A fixed guide shoe having a structure in which the area ratio of carbides is 6% or less. [2] The fixed guide shoe described in [1], wherein the component composition further contains, in mass percent, one or more selected from Mo: 0.9 to 1.5%, Ni: 2.0% or less, and V: 0.5 to 1.6%. [3] The linear expansion coefficient at 800°C is 1.5×10 -5The fixed guide shoe according to [1] or [2], wherein the thermal expansion coefficient is 1 / ℃ or less. [4] A tilt rolling mill comprising the fixed guide shoe according to any one of [1] to [3]. [5] A method for producing a seamless steel pipe using the inclined rolling mill described in [4] above. Effect of the Invention

[0013] According to the present invention, a fixed guide shoe having excellent heat crack resistance and excellent productivity for seamless steel pipes can be provided.

[0014] According to the present invention, when a seamless steel pipe is manufactured using a tilt rolling mill equipped with a fixed guide shoe, the occurrence of heat cracks that cause breakage or rupture of the fixed guide shoe can be suppressed or reduced, the frequency of replacing the fixed guide shoe can be reduced, and the productivity of seamless steel pipes can be improved. In addition, by using an inexpensive fixed guide shoe with a reduced content of alloy elements such as Cr and Ni, the manufacturing cost of seamless steel pipes can be reduced and the productivity of seamless steel pipes can be improved. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic diagram showing the steps of the Mannesmann plug mill process. [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of the piercer and elongator. [Diagram 3] FIG. 3 is a front view of a region where the rolls and plugs of a tilt rolling mill equipped with fixed guide shoes are present, as viewed from the rolling direction. [Figure 4] FIG. 4 is an explanatory diagram for explaining the positions at which the samples for structure observation and the samples for linear expansion coefficient measurement were taken. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below.

[0017] The fixed guide shoe of the present invention has the following component composition: In the following, % indicating the content of each component means mass % unless otherwise specified.

[0018] C: 0.35-0.45% C is an important element that affects the strength characteristics of fixed guide shoes. To obtain good strength characteristics, the C content must be 0.35% or more. This allows appropriate strength characteristics to be obtained. On the other hand, if the C content is too high, excessive Cr carbides will precipitate, reducing heat crack resistance. Therefore, the C content must be 0.45% or less.

[0019] Silicon: 0.70 to 1.3% Silicon is an effective element for improving the strength characteristics of fixed guide shoes. To obtain this effect, the silicon content must be 0.70% or more. On the other hand, if the silicon content is too high, it may become embrittled in hot conditions, making it unsuitable for use as a tool. Therefore, the silicon content must be 1.3% or less.

[0020] Mn: 0.2-0.7% Mn is effective in improving strength properties. To obtain this effect, the Mn content must be 0.2% or more. On the other hand, if the Mn content is too high, residual austenite remains and fatigue strength decreases. In addition, Mn is known as a carbide forming element, and if the amount of Mn added is too high, the amount of Cr carbide precipitated increases and heat crack resistance decreases. Therefore, the Mn content must be 0.7% or less.

[0021] Cr: 5.0~10% Cr is an element with excellent high-temperature strength properties. To obtain this effect, the Cr content must be 5.0% or more. On the other hand, if the Cr content is too high, excessive Cr carbides, which are M7C3 type carbides, will precipitate, leading to a decrease in heat crack resistance. Therefore, the Cr content must be 10% or less.

[0022] The above are the basic components (essential components) in the composition of the fixed guide shoe of the present invention. In the composition, the balance other than the above basic components can be Fe and inevitable impurities.

[0023] The above-mentioned composition may further contain one or more elements selected from Mo, Ni and V within the following ranges.

[0024] Mo: 0.9-1.5% Mo is effective for improving heat resistance. In order to obtain this effect, when Mo is contained, the Mo content is preferably 0.9 to 1.5%.

[0025] Ni: 2.0% or less Ni is effective for toughness. To obtain this effect, when Ni is contained, the Ni content is preferably 2.0% or less. Also, when Ni is contained, the Ni content is preferably 0.01% or more.

[0026] V: 0.5-1.6% V is effective in improving strength characteristics, and in order to obtain this effect, when V is contained, the V content is preferably 0.5 to 1.6%.

[0027] Carbide in the structure of the fixed guide shoe: Area ratio is 6% or less Although the precipitation of M7C3 type carbides can provide excellent wear resistance, as the amount of carbides increases, they develop into a net shape, which becomes a path for the propagation of heat cracks, causing a decrease in heat crack resistance. For this reason, the fixed guide shoe is to have a structure in which the area ratio of M7C3 type carbides is 6% or less. The structure observation of the fixed guide shoe is performed as follows. A sample of 30 mm x 15 mm x 10 mm for structure observation is taken at a depth of 10 mm (see Figure 4) from the surface of the fixed guide shoe (the surface on the side that comes into contact with the rolled material). The metal structure is revealed by polishing a surface parallel to the above surface and etching it with a Virela, and observed with an optical microscope (magnification: 200 times). At this time, the carbides show a white color, and the area ratio (area%) of the white area to the entire observation area is calculated by image analysis. Metal structure photographs of five fields of view are taken, the area ratio of each carbide is measured, and the average value is taken as the area ratio of the carbide in the structure of the fixed guide shoe.

[0028] Linear expansion coefficient of fixed guide shoe at 800℃: 1.5×10 -5 1 / ℃ or less The thermal stress that causes heat cracks increases with an increase in the linear expansion coefficient. Therefore, in order to reduce the thermal stress, the linear expansion coefficient of the fixed guide shoe is set to 1.5×10 -5 It is desirable to keep the coefficient of linear expansion at 800°C or less. The coefficient of linear expansion is measured as follows: A sample for measuring the coefficient of linear expansion, measuring 4 mm in diameter and 10 mm in length, is taken from a position 10 mm deep (see Figure 4) from the surface of the fixed guide shoe (the surface that comes into contact with the rolled material). The sample is heated at a heating rate of 100°C / sec using a Formaster testing machine to measure the change in length of the sample, and the coefficient of linear expansion at 800°C is calculated.

[0029] The steel structure of the fixed guide shoe of the present invention preferably has martensite as the main phase, with retained austenite being less than 1.0% in area ratio. In the present invention, the main phase means a phase that occupies 50% or more in area ratio. The area ratio of the main phase is preferably 60% or more, and more preferably 75% or more. The steel structure of the fixed guide shoe of the present invention can be determined by cutting out a sample for structure observation from a location (see FIG. 4) located at a depth of 10 mm from the surface of the fixed guide shoe (the surface on the side in contact with the rolled material) and observing the surface of the sample by a known method.

[0030] The fixed guide shoe of the present invention can be manufactured by, although not limited to, preparing molten steel having the above-mentioned composition and casting it into a predetermined shape of the fixed guide shoe by the V process. EXAMPLES

[0031] Next, the present invention will be described in detail with reference to the following examples. However, the present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention, and all such modifications are included in the technical scope of the present invention.

[0032] A molten steel having the composition shown in Table 1 was prepared, and a fixed guide shoe was cast by the V process. The fixed guide shoe was then installed in a piercer, which is a tilt rolling machine (piercing rolling machine), and a billet having an outer diameter of 230 mm and a material of API 5CTL80 was heated to 1290°C and pierced and rolled. A sample for structural observation was separately taken from a position 10 mm deep from the surface of the fixed guide shoe produced, and the area ratio of carbides was measured according to the above-mentioned method. A sample for measuring the linear expansion coefficient, having a diameter of 4 mm and a length of 10 mm, was also taken from a position 10 mm deep from the surface of the fixed guide shoe (the surface on the side in contact with the rolled material) according to the above-mentioned method, and the linear expansion coefficient was measured. Carbides were obtained by image analysis. The linear expansion coefficient was calculated by measuring the change in length of a sample having a size of 4 mm in diameter and 10 mm in length by heating the sample at a heating rate of 100°C / sec using a Formaster testing machine, and the linear expansion coefficient at 800°C was calculated.

[0033] Heat crack resistance was evaluated by visually inspecting the surface of the fixed guide shoe after the piercing and rolling. Those that showed no heat cracks were deemed to have excellent heat crack resistance.

[0034] As can be seen from Table 1, by satisfying the conditions of the present invention, a fixed guide shoe with excellent heat crack resistance can be obtained. This makes it possible to suppress or reduce the occurrence of heat cracks that cause the fixed guide shoe to break or fracture, reduce the frequency of replacing the fixed guide shoe, and increase the productivity of seamless steel pipes. In addition, by using an inexpensive fixed guide shoe with a reduced content of alloy elements such as Cr and Ni, the manufacturing cost of seamless steel pipes can be reduced and the productivity of seamless steel pipes can be increased.

[0035] [Table 1]

Claims

1. A fixed guide shoe installed on a tilt rolling mill, A composition containing, by mass%, C: 0.35 to 0.45%, Si: 0.70 to 1.3%, Mn: 0.2 to 0.7%, Cr: 5.0 to 10%, with the balance being Fe and unavoidable impurities; A fixed guide shoe having a structure in which the area ratio of carbides is 6% or less.

2. The fixed guide shoe according to claim 1, wherein the component composition further contains, in mass percent, one or more selected from Mo: 0.9 to 1.5%, Ni: 2.0% or less, and V: 0.5 to 1.6%.

3. The linear expansion coefficient at 800°C is 1.5 x 10 -5 2. The fixed guide shoe of claim 1, wherein the temperature is 1 / °C or less.

4. The linear expansion coefficient at 800°C is 1.5 x 10 -5 3. The fixed guide shoe of claim 2, wherein the temperature is 1 / °C or less.

5. A tilt rolling mill comprising the fixed guide shoe according to any one of claims 1 to 4.

6. A method for producing a seamless steel pipe by using the inclined rolling mill according to claim 5.

Citation Information

Patent Citations

  • JP1975102517A

  • Casting tool

    JP1986157655A

  • Guide shoe for piercing and rolling seamless pipe and manufacture of the same

    JP1993017849A

  • Ni-base superalloy

    JP1996085838A

  • Tool steel for hot working excellent in wear resistance, and tool steel product

    JP1998298709A