Polyimide tube
The polyimide tube with carbon nanotubes addresses the issue of tearing in fixing belts by maintaining high thermal conductivity and mechanical strength, ensuring durability and performance during paper jams.
Patent Information
- Application Number
- JP2023065037
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-12
AI Technical Summary
Existing fixing belts in image forming devices are prone to tearing when a paper jam occurs due to the forceful removal of jammed paper, compromising thermal conductivity and mechanical integrity.
A polyimide tube containing carbon nanotubes is used as a base layer in the fixing belt, ensuring a thermal conductivity of 1.00 W/mK or more in the longitudinal direction, a longitudinal-to-circumferential thermal conductivity ratio of 1.05 or more, and a tensile modulus-breaking test force product of 4000.0 kgf²/mm², enhancing resistance to tearing.
The polyimide tube with carbon nanotubes maintains high thermal conductivity and mechanical strength, preventing tearing during paper jams and suppressing excessive temperature rise, thereby improving the durability and performance of fixing belts.
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide tube that can be suitably used for a fixing belt mounted in an image forming apparatus or the like. [Background technology]
[0002] In electrophotographic image forming devices such as copiers and printers, an unfixed toner image formed on a recording medium such as recording paper is fixed by a fixing device. This method involves feeding a transfer paper with a thermal ink temporarily attached to the surface of the fixing belt between a fixing belt with a heater on the back side and a press roller, melting and fixing the thermal ink to the transfer paper, and at the same time strengthening the fixation by pressing.
[0003] A method is known in which a base layer of a fixing belt contains a filler with excellent thermal conductivity (high thermal conductive filler) in order to improve the thermal conductivity of the fixing belt, thereby improving the fixing performance, shortening the waiting time after power-on, reducing power consumption, and increasing the fixing speed.
[0004] In order to solve such problems, a resin tubular object has been proposed in the past (see, for example, JP 2006-330405 A) which is "a resin tubular object based on a heat-resistant resin and which is characterized in that it contains 1 to 25 volume parts of a filler having a thermal conductivity of more than 60 W / mk" (see, for example, JP 2006-330405 A). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-330405 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when a paper jam occurs inside an image forming device, the user must remove the fixing device and pull out the jammed paper from the paper transport path to clear the jam. However, if the user tries to pull out the paper forcibly, a load is placed on the fixing members, etc., which can cause the belt end to tear. Therefore, there is a demand for a polyimide tube that can be used for fixing belts, etc., that is resistant to tearing when a jam occurs while maintaining thermal conductivity.
[0007] An object of the present invention is to provide a polyimide tube that has excellent thermal conductivity and is suitable for use in a fixing belt or the like, and is resistant to tearing caused by paper being pulled out when a jam occurs. [Means for solving the problem]
[0008] The polyimide tube of the present invention is a polyimide tube comprising a polyimide resin, Carbon Nanotubes The polyimide tube In the film thickness direction The thermal conductivity is 1.00 W / mK or more, the longitudinal thermal conductivity / circumferential thermal conductivity ratio of the thermal conductivity is 1.05 or more, and the product of the longitudinal tensile modulus and the breaking test force in the tensile test is 4000.0 kgf 2 / mm 2 That's all.
[0009] The tensile modulus of the polyimide tube in the longitudinal direction is 700 kgf / mm 2 That's all. Effect of the Invention
[0010] By using the polyimide tube of the present invention, it is possible to provide a polyimide tube that has excellent thermal conductivity and is usable for a fixing belt, etc., that is not easily torn when a paper is pulled out when a jam occurs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The polyimide tube according to the embodiment of the present invention is a polyimide tube containing a polyimide resin, Carbon Nanotubes The polyimide tube In the film thickness direction The thermal conductivity is 1.00 W / mK or more, the longitudinal thermal conductivity / circumferential thermal conductivity ratio of the thermal conductivity is 1.05 or more, and the product of the longitudinal tensile modulus and the breaking test force in the tensile test is 4000.0 kgf 2 / mm 2 The polyimide tube of the present invention can be suitably used as a base layer of a fixing belt provided in an image forming apparatus. The longitudinal direction in the present invention refers to a direction perpendicular to the circumferential direction of the tube.
[0012] The polyimide tube according to the present embodiment has the above physical properties, and therefore has high thermal conductivity, making it difficult for the tube to break when a jam occurs and paper is pulled out. In addition, the longitudinal thermal conductivity / circumferential thermal conductivity increases the longitudinal thermal conductivity, and when the tube is used as a fixing belt, it can prevent the belt end from overheating due to the passage of paper. The reason for this is presumed to be as follows.
[0013] The polyimide tube according to the embodiment of the present invention is Carbon Nanotubes By including In the film thickness direction The thermal conductivity is 1.00W / mK or more, and the longitudinal thermal conductivity / circumferential thermal conductivity ratio is 1.05 or more. Carbon Nanotubes By orienting the fusing belt, the thermal conductivity in the longitudinal direction is increased, which reduces temperature unevenness in the longitudinal direction that occurs between the belts when paper passes through, thereby preventing excessive heating at the ends of the fusing belt where paper does not pass.
[0014] In addition, the product of the tensile modulus in the longitudinal direction and the breaking test force in the tensile test is 4000.0 kgf 2 / mm 2By setting the value to this or higher, it is possible to prevent tears caused by forcibly pulling out paper when a jam occurs. If a user tries to forcibly pull out paper when a jam occurs, the load applied in the longitudinal direction deforms the end of the fixing belt, which is thought to cause tears to occur at the end of the fixing belt. The product of the longitudinal tensile modulus and the breaking test force in the tensile test is 4000.0 kgf 2 / mm 2 This is believed to prevent deformation and tearing of the fixing belt edge. The breaking test force is the test force at the time of breakage at the maximum inclination in accordance with JIS P8113.
[0015] The polyimide tube according to the embodiment of the present invention has a tensile modulus of elasticity in the longitudinal direction of 700 kgf / mm 2 More preferably, it is 710 kgf / mm 2 That's all.
[0016] Next, the polyimide resin used in the present embodiment may be, for example, an imidized product of polyamic acid (polyamic acid), which is a polymer of tetracarboxylic dianhydride and diamine compound.Specific examples of polyimide resins include those obtained by polymerizing equimolar amounts of tetracarboxylic dianhydride and diamine compound in a solvent to obtain a polyamic acid solution, and then imidizing the polyamic acid.
[0017] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,3,3'4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,3 ,3',4'-Benzophenonetetracarboxylic dianhydride, 3,3',4,4'-Benzophenonetetracarboxylic dianhydride (BTDA), Bis(3,4-dicarboxyphenyl)sulfone dianhydride, Bis(2,3-dicarboxyphenyl)methane dianhydride, Bis(3,4-dicarboxyphenyl)methane dianhydride, 1.05-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1.05-bis(3,4-dicarboxyphenyl)ethane dianhydride, 2,2-bis[3,4-(dicarboxyphenoxy)phenyl]propane dianhydride diphthalic anhydride (BPADA), 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, oxydiphthalic anhydride (ODPA), bis(3,4-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfoxide dianhydride, thiodiphthalic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 1,2,7,8-phenanthrenetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 9 Examples of the dianhydride include aromatic tetracarboxylic dianhydrides such as 1,9-bis[4-(3,4'-dicarboxyphenoxy)phenyl]fluorene dianhydride, cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 2,3,4,5-tetrahydrofuran tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, 3,4-dicarboxy-1-cyclohexyl succinic dianhydride, and 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic dianhydride. Two or more of these tetracarboxylic dianhydrides may be used in combination.Among these tetracarboxylic dianhydrides, pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 2,2-bis[3,4-(dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), and oxydiphthalic anhydride (ODPA) are particularly preferred.
[0018] Specific examples of diamine compounds include paraphenylenediamine (PPD), metaphenylenediamine (MPDA), 2,5-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 2,2-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-diaminodiphenylmethane, 4,4 '-Diaminodiphenylmethane (MDA), 2,2-bis-(4-aminophenyl)propane, 3,3'-diaminodiphenyl sulfone (33DDS), 4,4'-diaminodiphenyl sulfone (44DDS), 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether (34ODA), 4,4'-diaminodiphenyl ether ( ODA), 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 1,3-bis(3-aminophenoxy)benzene (133APB), 1,3-bis(4-aminophenoxy)benzene (134APB), 1,4-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]sulfone (B Examples of aromatic diamines include bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis(3-aminophenyl)1.05,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)1.05,1,3,3,3-hexafluoropropane, and 9,9-bis(4-aminophenyl)fluorene.
[0019] Among them, from the viewpoints of durability, thermal conductivity, and flexural durability, preferred polyimide resins include polyimide resins made of 3,3',4,4'-biphenyltetracarboxylic dianhydride and p-phenylenediamine (BPDA-PPD), polyimide resins made of 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-diaminodiphenyl ether (BPDA-ODA), and polyimide resins made of pyromellitic dianhydride and 4,4'-diaminodiphenyl ether (PMDA-ODA), and these polyimide resins may be combined.
[0020] Examples of organic polar solvents that dissolve the tetracarboxylic dianhydride and diamine compound to obtain the polyimide resin include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, hexamethylphosphoric triamide, 1,2-dimethoxyethane, diglyme, triglyme, and the like. Among these diamines, N,N-dimethylacetamide (DMAC) and N-methyl-2-pyrrolidone (NMP) are particularly preferred. These organic polar solvents may be used alone or in combination. In addition, aromatic hydrocarbons such as toluene and xylene may be mixed with the organic polar solvent.
[0021] Books Other heat conductive particles may be added to the extent that the strength and thermal conductivity of the invention are not impaired.
[0022] The polyimide tube of the present invention is a seamless tubular layer mainly composed of polyimide resin and Carbon Nanotubes In the polyimide tube according to the embodiment of the present invention, the thickness of the tube is preferably 30 μm or more and 100 μm or less from the viewpoint of mechanical properties, and more preferably 50 μm or more and 80 μm or less from the viewpoint of ease of manufacture and the flexibility required when used in a fixing belt or the like.
[0023] Next, a method for manufacturing a fixing belt using the polyimide tube of the present invention will be described in detail. The fixing belt using the polyimide tube of the present invention is mainly manufactured through a polyamic acid solution preparation step, a base layer molding step (the polyimide tube of the present invention), a primer layer formation step, a release layer molding step, a baking step, and a demolding step.
[0024] (1) Polyamic acid solution preparation process In the polyamic acid solution preparation step, the polyimide precursor solution prepared as follows is added with the above-mentioned Carbon Nanotubes The polyamic acid solution is obtained by adding the above. Carbon Nanotubes There is no particular limitation on the method of adding Carbon Nanotubes In addition to adding it directly, Carbon Nanotubes may be added.
[0025] Examples of organic polar solvents that can prepare the polyamic acid solution include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, hexamethylphosphoric triamide, 1,2-dimethoxyethane, diglyme, triglyme, etc. Among these diamines, N,N-dimethylacetamide (DMAC) and N-methyl-2-pyrrolidone (NMP) are particularly preferred. These organic polar solvents may be used alone or in combination. In addition, aromatic hydrocarbons such as toluene and xylene may be mixed with the organic polar solvent.
[0026] In the present embodiment, it is preferable to use 4,4'-diaminodiphenyl ether as the diamine and pyromellitic dianhydride as the tetracarboxylic dianhydride, and it is particularly preferable to use paraphenylenediamine as the diamine and 3,3',4,4'-biphenyltetracarboxylic dianhydride as the tetracarboxylic dianhydride. The polyimide resin obtained from these monomers has excellent mechanical properties and is tough, and does not soften or melt like a thermoplastic resin even when the temperature of the fixing belt increases, and has excellent heat resistance and mechanical properties. In addition, a polyamic acid solution consisting of the diamine and tetracarboxylic acid is combined to form a polyimide resin having mechanical properties such as flexibility, and can be used preferably.
[0027] If necessary, a resin such as polyamideimide or polyethersulfone may be added to the polyamic acid solution within the scope of the present invention.
[0028] The polyamic acid solution may contain known additives such as dispersants, solid lubricants, antisettling agents, leveling agents, surface conditioners, moisture absorbents, antigelling agents, antioxidants, UV absorbers, light stabilizers, plasticizers, antiskinning agents, surfactants, antistatic agents, antifoaming agents, antibacterial agents, antifungal agents, preservatives, thickeners, etc. Furthermore, the polyamic acid solution may contain a dehydrating agent and an imidization catalyst in amounts greater than or equal to the stoichiometric amount.
[0029] It is preferable that the polyamic acid solution is subjected to a treatment such as filtration and degassing before use.
[0030] (2) Base layer (polyimide tube) molding process The tubular article of the present invention is obtained by using an apparatus equipped with a slit head positioned on the outside of a core body at a predetermined gap with the outer diameter of the core body, extruding a coating precursor solution from the outside from the slit head onto the outer surface of the core body at a controlled predetermined extrusion speed, cast-molding the coating precursor solution to a predetermined film thickness on the outer surface of the core body while moving the core body, retaining the cast coating on the core body until it is at least in a state where it can retain its strength as a tubular article, and separating the core body and the coating. As an alternative method, a precursor solution is applied to the outer surface of the core, and then a die is run over the outer surface of the core at a speed of 100 mm / s or more. Carbon Nanotubes can be oriented longitudinally.
[0031] (3) Primer layer formation process In the primer layer forming process, the core on which the base layer is formed is dipped in a primer liquid containing a dispersoid containing a fluororesin and a water-soluble heat-resistant resin, and the primer liquid is uniformly applied to the outer peripheral surface of the base layer. The primer layer is a layer that serves to bond the base layer and the release layer, and is composed of an adhesive resin such as a fluororesin or an acrylic resin, a water-soluble heat-resistant resin such as a water-soluble polyamideimide resin or a water-soluble polyimide resin, and the like. Then, the base layer (with the core) with the primer liquid is heated. The heating temperature at this time is preferably a temperature at which the solvent volatilizes but the imidization of the polyimide precursor does not proceed, for example, a temperature within a range of 320°C or less.
[0032] (4) Release layer forming process In the release layer forming process, a fluororesin dispersion liquid is applied, and then the coating is dried to form a coating of the fluororesin dispersion liquid on the primer layer. Examples of fluororesins include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), and tetrafluoroethylene-hexafluoropropylene copolymer (FEP), which may be used alone or in combination.
[0033] (5) Firing process In the baking step, the product obtained in the release layer forming step is baked to obtain a fixing belt. The baking temperature at this time is preferably in the range of 300°C to 450°C. The treatment time is preferably in the range of 30 minutes to 2 hours. This is because the imidization of the base material layer is completed and the fluororesin of the release layer is baked simultaneously, which not only shortens the manufacturing time of the fixing belt and improves the thermal efficiency, but also increases the adhesive strength of each layer.
[0034] (6) Demolding process In the demolding process, the fixing belt is removed from the core.
[0035] <Features of the fixing belt> In image forming devices using a general fixing belt, the fixing belt is used to melt and fix toner to a recording medium such as paper. Therefore, the fixing belt is heated by a heater provided inside the fixing belt, and when a recording medium such as paper passes through, the heat is absorbed by the recording medium, creating a temperature difference between the passing part and the non-passing part, and the non-passing part is prone to overheating. Carbon Nanotubes By orienting the film, the thermal conductivity in the longitudinal direction is improved, so the temperature is kept uniform and excessive heating can be suppressed. Carbon Nanotubes By orienting the toner particles in the longitudinal direction, it is possible to prevent the end portions of the fixing belt from being torn due to deformation caused by a load being applied in the longitudinal direction due to forcible pulling out in the event of a jam.
[0036] The fixing belt of the present embodiment may have an elastic layer between the base layer and the release layer.
[0037] <Examples and Comparative Examples> The fixing belt according to the present embodiment will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples. EXAMPLES
[0038] 1. Preparation of the fixing belt First, a mold having an outer diameter of 18 mm and a length of 500 mm and having a release-treated surface was prepared.
[0039] Next, in a polyamic acid solution (composition: 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) / paraphenylenediamine (PPD):pyromellitic dianhydride (PMDA) / 4,4'-diaminodiphenyl ether (ODA) = 97.5:2.5 ratio, solid content 18.8 parts by mass), Nika Carbon nanotubes (VGCF-H manufactured by Showa Denko KK) were added to the polyamic acid solution so that the amount was 17.0 parts by volume relative to the solid content of the polyamic acid solution, and the polyamic acid solution was stirred until the carbon nanotubes were uniformly dispersed, yielding a polyamic acid solution with a viscosity of 900 poise.
[0040] Next, using an apparatus equipped with a slit head positioned at a predetermined gap with the outer diameter of the ship mold, the polyamic acid solution was discharged from the slit head onto the outer surface of the mold from the outside while controlling the discharge speed at a predetermined discharge speed, and the polyamic acid solution was applied to the outer surface of the mold while moving the core at a speed of 100 mm / s. After that, as a drying process, the mold was placed in a 120°C oven and dried for 30 minutes, after which the temperature was raised to 200°C over 20 minutes, maintained at the same temperature for 20 minutes, and cooled to room temperature to produce a substrate layer.
[0041] Next, the primer liquid was applied to the surface of the substrate layer and dried at 150° C. for 10 minutes to prepare a primer layer.
[0042] Then, the PFA dispersion was coated on the dried primer layer, and after drying at room temperature for 30 minutes, the temperature was gradually increased to 350°C and baked at 350°C for 30 minutes to obtain the intended fixing belt with a base layer thickness of 60 μm.
[0043] 2. Physical property evaluation (1) Measurement of the thermal conductivity of the base layer With reference to JIS R2616, only the base layer of the fixing belt was cut into a 2 cm x 2 cm piece, a transistor was attached to one side of the base layer via thermal conductive grease, and a heat sink (made of aluminum) was attached to the other side via thermal conductive grease, and an electric current was applied to raise the temperature until the temperature of the transistor reached 60°C, and the base layer was heated at 60°C for 3 minutes, and the temperature A of the transistor surface and the temperature B of the base layer surface with the heat sink attached were measured using a thermocouple. The power consumption at this time was measured, and the thermal resistance was calculated from the temperature of each surface and the power consumption using the following formula. Thermal resistance = (Temperature A of the transistor surface - Temperature B of the substrate layer surface) / Power consumption Using the thermal resistance calculated above, the thermal conductivity was calculated according to the following formula. Thermal conductivity = film thickness of substrate layer / (cross-sectional area of transistor x thermal resistance) The thermal conductivity of the substrate layer was 1.10 W / mK. Next, the thermal conductivity in the longitudinal and circumferential directions was measured by placing an aluminum rod (width 15 mm, thickness 5 mm, length 60 mm) covered with insulation on a hot plate, and cutting a film consisting of only the polyimide layer into a 1.5 cm x 1.5 cm square on top of it. This was then layered so that the thickness of the film was 5 mm in the longitudinal and circumferential directions, and the polyimide film covered with insulation was then placed on top of it. The temperatures above and below the aluminum plate and above and below the layered film were measured with thermocouples. In addition, a cooling fan was attached to the top of the film, and the measurement was performed with the hot plate temperature set to 180°C. From the measurement results, the thermal conductivity was calculated using the following formula. λf=((λa×ΔTa / La)×(Lf / ΔTf) λf: Thermal conductivity of film, λa: Thermal conductivity of aluminum rod, ΔTf: Temperature difference between top and bottom of film, ΔTa: Temperature difference between top and bottom of aluminum rod, Lf: Film thickness, La: Aluminum rod length As a result of the measurement, it was confirmed that the longitudinal thermal conductivity / circumferential thermal conductivity ratio was 1.05. Carbon Nanotubes It was confirmed that the film was oriented in the longitudinal direction.
[0044] (2) Measurement of tensile modulus and breaking test force The fixing belt was cut open and punched out in the longitudinal direction with a JIS-3 dumbbell (JIS K6301) to prepare a sample. The sample was tested using a Shimadzu Autograph AGS-50A with a chuck distance of 30 mm and a pulling speed of 50 mm / min, and the tensile modulus of maximum inclination and the test force at break were measured in accordance with JIS P8113. As a result, the tensile modulus was 982 kgf / mm 2 The breaking test force is 7.2 kgf, and the product of the tensile modulus and the breaking test force is 7070.4 kgf 2 / mm 2 It was also confirmed that the tape was difficult to tear even when it was repeatedly jammed and pulled out forcefully. EXAMPLES
[0045] next ,mosquito A fixing belt was obtained in the same manner as in Example 1, except that carbon nanotubes (VGCF-H manufactured by Showa Denko KK) were added in an amount of 21.0 parts by volume relative to the solid content of the polyamic acid solution.
[0046] The thermal conductivity of the obtained fixing belt was 1.45 W / mK, the longitudinal thermal conductivity / circumferential thermal conductivity ratio was 1.05, and the tensile modulus was 976 kgf / mm 2 The breaking test force is 6.6 kgf, and the product of the tensile modulus and the breaking test force is 6441.6 kgf 2 / mm 2 It was also confirmed that the tape was difficult to tear even when it was repeatedly jammed and pulled out forcefully. EXAMPLES
[0047] Next, in a polyamic acid solution (composition: 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) / paraphenylenediamine (PPD): pyromellitic dianhydride (PMDA) / 4,4'-diaminodiphenyl ether (ODA) = 80:20 ratio, (solid content 17.0 parts by mass) NikaCarbon nanotubes (VGCF-H manufactured by Showa Denko K.K.) were added in an amount of 26.0 parts by volume relative to the solid content of the polyamic acid solution, and the polyamic acid solution was stirred until the carbon nanotubes were uniformly dispersed to obtain a polyamic acid solution with a viscosity of 900 poise. A fixing belt was obtained in the same manner as in Example 1, except that the thickness of the substrate was 70 μm.
[0048] The thermal conductivity of the obtained fixing belt was 1.85 W / mK, the longitudinal thermal conductivity / circumferential thermal conductivity ratio was 1.06, and the tensile modulus was 932 kgf / mm 2 The breaking test force is 5.6 kgf, and the product of the tensile modulus and the breaking test force is 5219.2 kgf. 2 / mm 2 It was also confirmed that the tape was difficult to tear even when it was repeatedly jammed and pulled out forcefully. EXAMPLES
[0049] next ,mosquito A fixing belt was obtained in the same manner as in Example 3, except that carbon nanotubes (VGCF-H manufactured by Showa Denko KK) were added in an amount of 30.0 parts by volume relative to the solid content of the polyamic acid solution.
[0050] The thermal conductivity of the obtained fixing belt was 2.20 W / mK, the longitudinal thermal conductivity / circumferential thermal conductivity ratio was 1.07, and the tensile modulus was 923 kgf / mm 2 The breaking test force is 5.4 kgf, and the product of the tensile modulus and the breaking test force is 4984.2 kgf. 2 / mm 2 It was also confirmed that the tape was difficult to tear even when it was repeatedly jammed and pulled out forcefully.
[0051] Comparative Example 1 Next, boron nitride (MBN-010T manufactured by Mitsui Chemicals) was added as inorganic particles to a polyamic acid solution (composition: 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) / paraphenylenediamine (PPD):pyromellitic dianhydride (PMDA) / 4,4'-diaminodiphenyl ether (ODA) = 80:20 ratio (solid content 18.8 parts by mass) in an amount of 40.0 parts by volume relative to the solid content of the polyamic acid solution, and the polyamic acid solution was stirred until the boron nitride was uniformly distributed, thereby obtaining a polyamic acid solution with a viscosity of 900 poise. A fixing belt was obtained in the same manner as in Example 1, except for this.
[0052] The thermal conductivity of the obtained fixing belt was 1.05 W / mK, the longitudinal thermal conductivity / circumferential thermal conductivity ratio was 1.00, and the tensile modulus was 915 kgf / mm 2 The breaking test force is 4.0, and the product of the tensile modulus and the breaking test force is 3660.0 kgf 2 / mm 2 It was confirmed that this is the case.
Claims
1. A polyimide tube comprising a polyimide resin, the polyimide resin containing inorganic particles, the polyimide tube having a thermal conductivity of 1.00 W / mK or more, a longitudinal thermal conductivity / circumferential thermal conductivity ratio of the thermal conductivity being 1.05 or more, and a product of a longitudinal tensile modulus and a breaking test force in a tensile test being 4000.0 kgf 2 / mm 2 A polyimide tube characterized by the above.
2. The tensile modulus of the polyimide tube in the longitudinal direction is 700 kgf / mm 2 2. The polyimide tube according to claim 1, wherein the polyimide tube is a polyimide tube having a thickness of 100 nm or less.
3. 3. The polyimide tube according to claim 1, wherein the inorganic particles are one selected from the group consisting of carbon nanofibers and carbon nanotubes.
4. A fixing belt, comprising the polyimide tube according to claim 1 as a base layer.
Citation Information
Patent Citations
Heating fixing belt, its manufacturing method and image fixing device
JP2007272223A
Fixing belt and fixing device
JP2014228729A
Fixing device and image forming apparatus
JP2016012072A
Fixing member and heat fixing device
JP2019211701A
Resin tube and fixing belt
JP2006330405A