Optical cable and composite cable
The composite cable design with a specific volume ratio and melting point configuration addresses the weight and transmission loss issues of plastic optical fibers, achieving a lightweight and efficient optical cable.
Patent Information
- Application Number
- JP2023065131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Optical cables using plastic optical fibers face issues of increased weight due to the optical properties of plastic fibers and require reduced transmission loss.
A composite cable design incorporating a plastic optical fiber surrounded by a tube with a volume ratio of 10% to 50% and a melting point higher than the glass transition temperature of the plastic optical fiber, along with an electrical signal cable and a sheath, to maintain flexibility and reduce transmission loss.
The design results in a lightweight optical cable with reduced transmission loss and improved handling characteristics.
Smart Images

Figure 2024151633000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to optical cables and composite cables. [Background technology]
[0002] An optical cable including an optical fiber is known (see, for example, Patent Document 1). In the optical cable described in Patent Document 1, the material of the optical fiber includes glass. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-132647 A Summary of the Invention [Problem to be solved by the invention]
[0004] From the standpoint of ease of handling, attempts are being made to make plastic optical fibers by replacing the optical fiber material with plastic.
[0005] However, in the above-mentioned configuration, due to the optical characteristics of the plastic optical fiber, the optical fiber becomes large, and therefore the optical cable becomes heavy.
[0006] On the other hand, optical cables are required to have reduced transmission loss.
[0007] The present invention provides an optical cable and a composite cable that are lightweight yet capable of reducing transmission loss. [Means for solving the problem]
[0008] The present invention (1) includes an optical cable comprising a plastic optical fiber and a tube surrounding the plastic optical fiber, the volume ratio of the plastic optical fiber in the tube being 10% or more and 50% or less.
[0009] The present invention (2) includes the optical cable according to (1), in which the number of the plastic optical fibers is four.
[0010] The present invention (3) includes the optical cable according to (1) or (2), in which the melting point of the tube is lower than the glass transition temperature of the plastic optical fiber.
[0011] The present invention (4) includes a composite cable comprising an optical cable according to any one of (1) to (3), an electric signal cable, and a sheath surrounding the optical cable and the electric signal cable. Effect of the Invention
[0012] The optical cable and composite cable of the present invention are lightweight and yet capable of reducing transmission loss. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view of a composite cable comprising an embodiment of the optical cable of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (definition) In this specification, the "volume ratio of the plastic optical fiber in the tube" means the ratio calculated by "volume of the plastic optical fiber / volume of the internal space of the tube." Also, the "volume ratio of the plastic optical fiber in the tube" is synonymous with the "cross-sectional area of the plastic optical fiber or the cross-sectional area inside the tube" in a cross section perpendicular to the longitudinal direction of the optical cable.
[0015] 1. One embodiment With reference to FIG. 1, a composite cable comprising an embodiment of the optical cable of the present invention will be described.
[0016] 1.1 Composite cable 1 The composite cable 1 has a substantially circular shape in a cross-sectional view. The cross-sectional view is taken along a cross section perpendicular to the extension direction of the composite cable 1. In this embodiment, the composite cable 1 includes an optical cable 2, an electric signal cable 3, and a sheath 4.
[0017] 1.2 Optical Cable 2 The optical cable 2 is disposed inside the composite cable 1. The optical cable 2 has a substantially circular shape in a cross-sectional view. In this embodiment, the optical cable 2 includes a plurality of plastic optical fibers (hereinafter, sometimes referred to as POF) 21, a tube 22, and a fiber material 23.
[0018] 1.2.1 Plastic Optical Fiber21 Each of the multiple plastic optical fibers 21 has a substantially circular cross section. The plastic optical fibers 21 are flexible. The plastic optical fibers 21 include a core (not shown), a clad (not shown), an overclad (not shown), and a coloring layer (not shown) in this order toward the outside in the radial direction. The clad is a single layer or multiple layers. The radial direction is included in the orthogonal direction. Examples of materials for the plastic optical fibers 21 include resins. Examples of resins include polycarbonate resins, acrylic resins, and epoxy resins.
[0019] 1.2.1.1 Glass transition temperature of plastic optical fiber21 Plastic optical fiber 21 (specifically, overclad) of The glass transition temperature is, for example, 80° C. or higher, preferably 90° C. or higher, and, for example, 130° C. or lower, preferably 120° C. or lower. The glass transition temperature of the plastic optical fiber 21 (specifically, the overclad) is determined by differential scanning calorimetry. The overclad is the layer with the largest area in the cross-sectional area of the plastic optical fiber 21. The overclad is also a shape-maintaining layer that maintains the outer shape of the plastic optical fiber 21.
[0020] 1.2.1.2 Sizes of plastic optical fibers 21 The size of the plastic optical fiber 21 is not limited as long as it satisfies the volume ratio described below. The outer diameter of the plastic optical fiber 21 is, for example, 0.05 mm or more, preferably 0.15 mm or more, and for example, 0.50 mm or less, preferably 0.35 mm or less.
[0021] 1.2.1.3 Number of plastic optical fibers 21 The plastic optical fiber 21 may be singular or plural. When the plastic optical fiber 21 is plural, the number of the plastic optical fibers 21 is, for example, 2 or more, for example, 3 or more, and for example, 8 or less, preferably 6 or less. The number of the plastic optical fibers 21 is preferably 4. If the number of the plastic optical fibers 21 is 4, it is possible to transmit a large amount of data, reduce transmission loss, and make the optical cable 2 lightweight.
[0022] 1.2 Tube 22 The tube 22 surrounds a plurality of plastic optical fibers 21. In this embodiment, the tube 22 has a substantially circular shape in a cross-sectional view. The tube 22 may be referred to as an optical cord.
[0023] Examples of the material of the tube 22 include resin. Examples of the resin include polyethylene resin, acrylic resin, epoxy resin, vinyl resin, and polyimide resin. From the viewpoints of processability and handling, polyethylene resin is preferable.
[0024] 1.2.1 Tube 22 size The size of the tube 22 is adjusted so that the "volume ratio of the plastic optical fiber 21 in the tube 22" described below is a desired ratio. The inner diameter of the tube 22 is, for example, 0.2 mm or more, preferably 0.5 mm or more, and, for example, 2.0 mm or less, preferably 1.0 mm or less. The thickness of the tube 22 is, for example, 0.02 mm or more, preferably 0.1 mm or more, and, for example, 0.5 mm or less, preferably 0.3 mm or less.
[0025] 1.2.2 Volume ratio of the plastic optical fiber 21 in the tube 22 In the present invention, the volume ratio of the plastic optical fiber 21 in the tube 22 is 10% or more and 50% or less.
[0026] If the volume ratio of the plastic optical fibers 21 in the tube 22 is less than 10%, there is a limit to how thin the multiple plastic optical fibers 21 can be, and the tube 22 becomes excessively large. This makes the optical cable 2 heavy. Specifically, the mass of the optical cable 2 per unit length increases.
[0027] If the volume ratio of the plastic optical fiber 21 in the tube 22 exceeds 50%, the transmission loss increases. Also, if the volume ratio of the plastic optical fiber 21 in the tube 22 exceeds 50%, the plastic optical fiber 21 becomes excessively thick. As a result, the optical cable 2 becomes heavy.
[0028] The volume ratio of the plastic optical fiber 21 in the tube 22 is preferably 13% or more, and is preferably 45% or less, more preferably 40% or less, even more preferably 30% or less, particularly preferably 20% or less, and further preferably 15% or less. In other words, the volume ratio of the plastic optical fiber 21 in the tube 22 is preferably 13% or more and 45% or less, more preferably 13% or more and 40% or less, even more preferably 13% or more and 30% or less, particularly preferably 13% or more and 20% or less, and most preferably 13% or more and 15% or less.
[0029] The "volume ratio of the plastic optical fibers 21 in the tube 22" is calculated as the ratio of the volume of the plastic optical fibers 21 to the volume inside the tube 22. The volume inside the tube 22 is calculated from the inner diameter and length of the tube 22. The volume of the plastic optical fibers 21 is calculated from the number of the plastic optical fibers 21, the outer diameter and length of the plastic optical fibers 21. When there are multiple plastic optical fibers 21, the sum of the volumes of the plastic optical fibers 21 is the volume of the plastic optical fibers 21. The volume inside the tube 22 includes the volume of the fiber material 23, which will be described next.
[0030] 1.2.3 Melting Point of Tube 22 The melting point of the tube 22 exceeds, for example, the glass transition temperature of the plastic optical fiber 21. The melting point of the tube 22 is, for example, 70° C. or higher, preferably 85° C. or higher, and, for example, 110° C. or lower, preferably 100° C. or lower. The melting point of the tube 22 is determined by differential scanning calorimetry.
[0031] If the melting point of the tube 22 is lower than the glass transition temperature of the plastic optical fiber 21, even if the tube 22 is heated so as to melt during extrusion molding production of the optical cable 2, it is possible to prevent the elastic modulus of the plastic optical fiber 21 from decreasing, and the plastic optical fiber 21 can be arranged in a desired shape within the tube 22. In other words, a highly reliable plastic optical fiber 21 can be formed and arranged within the tube 22.
[0032] 1.2.4 Textile materials23 The fiber material 23 covers the surfaces of the multiple plastic optical fibers 21 inside the tube 22. The fiber material 23 fills the inside of the tube 22. An example of a material for the fiber material 23 is aramid resin. A specific example of the fiber material 23 is high tensile fiber. In this embodiment, the fiber material 23 does not melt when heated, for example.
[0033] 1.3 Electrical signal cables3 The electric signal cable 3 is disposed inside the composite cable 1. The electric signal cable 3 is adjacent to the optical cable 2 in a cross-sectional view. The electric signal cable 3 has an elliptical or circular shape in a cross-sectional view. The electric signal cable 3 includes a pair of signal lines 31A, 31B and an electric cord 32.
[0034] 1.3.1 Pair of signal lines 31A, 31B The pair of signal wires 31A, 31B are disposed inside the electric signal cable 3. Each of the pair of signal wires 31A, 31B has a circular shape in a cross-sectional view. The pair of signal wires 31A, 31B are adjacent to each other in a cross-sectional view. Each of the pair of signal wires 31A, 31B includes a core wire 310 and a coating material 311, which are arranged in this order toward the outside in the radial direction. The core wire 310 has a circular shape in a cross-sectional view. An example of a material for the core wire 310 is copper. The coating material 311 is disposed on the circumferential surface of the core wire 310. An example of a material for the coating material 311 is resin.
[0035] 1.3.2 Electrical cord 32 The electric cord 32 surrounds the pair of signal lines 31A and 31B. The electric cord 32 has an elliptical or circular ring shape in a cross-sectional view. The electric cord 32 is made of, for example, resin.
[0036] 1.4 Sheath 4 The sheath 4 is the outermost layer of the composite cable 1. The sheath 4 surrounds the optical cable 2 and the electric signal cable 3. The sheath 4 has a substantially circular ring shape in a cross-sectional view. Examples of the material of the sheath 4 include resin. Examples of the resin include polyvinyl chloride resin.
[0037] 1.5 Manufacturing method of composite cable 1 Next, a method for manufacturing the composite cable 1 will be described.
[0038] In this method, first, the optical cable 2 and the electric signal cable 3 are prepared.
[0039] To prepare the optical cable 2, first, a plurality of plastic optical fibers 21 are prepared. After that, the plurality of plastic optical fibers 21 are assembled so as to be disposed inside the tube 22 (hereinafter, sometimes referred to as "multi-core coding"). At this time, the plurality of plastic optical fibers 21 and the tube 22 are both heated by extrusion molding. The heating temperature is at least a temperature at which the tube 22 melts, specifically, for example, 150°C or higher and, for example, 200°C or lower. At this time, the plurality of plastic optical fibers 21 are covered by extruding the fiber material 23 simultaneously with the plastic optical fibers 21 so as to be filled inside the tube 22.
[0040] Thereafter, the optical cable 2 and the electric signal cable 3 are assembled to form an assembly, and the assembly is surrounded by a sheath 4 .
[0041] 2. Effects In this embodiment, since the volume ratio of the plastic optical fiber 21 in the tube 22 is 10% or more, the tube 22 can be made small, and therefore the optical cable 2 can be made lightweight.
[0042] Furthermore, since the volume ratio of the plastic optical fiber 21 in the tube 22 is 50% or less, the transmission loss of the optical cable 2 can be reduced and the plastic optical fiber 21 can be prevented from becoming excessively thick, thereby making the optical cable 2 lighter.
[0043] 3. Modifications In the following modifications, the same components and steps as those in the above-described embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted. In addition, each modification can achieve the same effects as those in the above-described embodiment, unless otherwise specified. Furthermore, the embodiment and the modifications can be appropriately combined.
[0044] Although not shown, the composite cable 1 further includes a control wire and a ground wire. The control wire and the ground wire are surrounded by a sheath 4.
[0045] The optical cable 2 is a device that can be distributed as a single component and is industrially applicable. In other words, the optical cable 2 does not have to be provided in the composite cable 1. EXAMPLES
[0046] The present invention will be described in more detail below with reference to examples. Note that the present invention is not limited to the examples. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "not more than" or "less than") or lower limit (a numerical value defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0047] <Examples 1 to 5, Comparative Example 1, and Comparative Example 2> <Optical cable 2 manufacturing> An optical cable 2 having the size shown in Table 1 was manufactured.
[0048] Example 1 The tube 22 shown in Table 1 was prepared, and the optical cable 2 was produced using the tube 22. The specific procedure is as follows.
[0049] A mold was used to extrude the tube 22 into a cylindrical shape. Four plastic optical fibers 21 with an outer diameter of 0.25 mm and a fiber material 3 made of high tensile fiber were introduced into the cylindrical portion. In this manner, the optical cable 2 was produced.
[0050] Thereafter, the optical cable 2 and the electric signal cable 3 were assembled to form an assembly, and the assembly was surrounded by a sheath 4. In this manner, the composite cable 1 was produced.
[0051] The overcladding of the plastic optical fiber 21 is made of polycarbonate resin (manufacturer: SABIC Japan, LLC). The glass transition temperature of the overcladding determined by differential scanning calorimetry was 110°C.
[0052] The tube 22 is made of polyethylene resin. The melting point of the tube 22 determined by differential scanning calorimetry (manufacturer: Mettler Toledo) is: 95 The temperature was ℃.
[0053] The molding temperature for multi-core coding was 150°C.
[0054] (Examples 2 to 5, Comparative Examples 1 and 2) A composite cable 1 was produced in the same manner as in Example 1. However, the extrusion speed of the tube 22 using a mold and the like were changed.
[0055] <Evaluation> The increase rate of the transmission loss of the optical cable 2 was obtained by measuring the optical loss using an optical pulse tester (product name: LOR201 manufactured by Luciol Corporation).
[0056] [Table 1] [Explanation of symbols]
[0057] 1 Composite Cable 2 Optical cable 3 Electrical signal cables 4 Sheath 21 Plastic Optical Fiber 22 Tube
Claims
1. Plastic optical fiber, a tube surrounding the plastic optical fiber; An optical cable, wherein the volume ratio of the plastic optical fiber in the tube is 10% or more and 50% or less.
2. The optical cable according to claim 1 , wherein the number of said plastic optical fibers is four.
3. 3. The optical cable according to claim 1, wherein the melting point of the tube is lower than the glass transition temperature of the plastic optical fiber.
4. The optical cable according to claim 3; An electrical signal cable; a sheath surrounding the optical cable and the electrical signal cable; A composite cable comprising: