Sliding member

A grooved surface on the duplex stainless steel base material disperses stress, addressing microcrack issues in the build-up layer, ensuring the sliding member's durability and crack resistance.

JP2024151680AInactive Publication Date: 2024-10-25OSAKA FUJI CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023065227
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional sliding members with duplex stainless steel base material and nickel/cobalt alloy layers face issues with microcracks due to residual stress during overlay layer formation, especially when using methods like powder plasma arc welding or laser cladding.

Method used

A grooved surface on the duplex stainless steel base material is used, with adjacent grooves aligned without gaps, to disperse stress and prevent microcracks in the build-up layer, comprising a nickel alloy lower layer and cobalt alloy surface layer.

Benefits of technology

The grooved surface design effectively suppresses microcrack formation in the build-up layer, enhancing the durability and integrity of the sliding member by distributing residual stress, thereby preventing cracks from starting points.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151680000001_ABST
    Figure 2024151680000001_ABST
Patent Text Reader

Abstract

To provide a sliding member having a structure in which microcracks are unlikely to be generated in a build-up layer when the build-up layer is formed on a surface of a two-phase stainless steel, which is a base material.SOLUTION: In a sliding member in which a build-up layer 2 consisting of a nickel alloy underlayer 2a and a cobalt alloy surface layer 2b is provided on a surface of a two-phase stainless steel base material 1, the base material surface on which the build-up layer is formed is made a grooved surface in which adjacent groove parts 1a are aligned without gaps, to suppress generation of microcracks in the build-up layer with stress dispersion by the groove parts.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sliding member that is provided on the sliding surfaces of various pumps, such as centrifugal pumps, mixed flow pumps, and axial flow pumps, as well as various valves and various screws, where metal members rub against each other, to suppress the occurrence of seizing on the sliding surfaces. [Background technology]

[0002] Conventionally, as a sliding member of this type, a member using duplex stainless steel as a base material, on the surface of which is formed a build-up layer consisting of a nickel alloy underlayer and a cobalt alloy surface layer, is known (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-166237 A [Patent Document 2] JP 2018-187647 A Summary of the Invention [Problem to be solved by the invention]

[0004] The duplex stainless steel that constitutes the base material of the sliding members is a two-phase stainless steel that is a 1:1 mixture of austenitic stainless steel and ferritic stainless steel. It has high strength, excellent corrosion resistance, and excellent resistance to stress corrosion cracking, and is therefore used as a base material for the sliding surfaces of various pumps, such as centrifugal pumps, mixed flow pumps, and axial flow pumps, as well as various valves, various screws, and other components where metals rub against each other.

[0005] When a cobalt alloy is deposited as a build-up layer on the surface of this duplex stainless steel base material, a lower layer of nickel alloy with a low carbon content is deposited between the surface cobalt alloy layer and the surface of the duplex stainless steel base material, thereby suppressing the penetration of carbon from the surface cobalt alloy into the duplex stainless steel base material.

[0006] However, since build-up on the surface of duplex stainless steel is performed by powder plasma arc welding, laser cladding, thermal spraying, or the like, there has been a problem that when forming the build-up layer, microcracks are likely to occur in the build-up layer due to residual stress, making it difficult to obtain a build-up layer with high strength.

[0007] Therefore, an object of the present invention is to provide a sliding member having a structure in which microcracks are unlikely to occur in a buildup layer when the buildup layer is formed on the surface of the base material, duplex stainless steel. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention provides a sliding member having a build-up layer formed on the surface of a duplex stainless steel base material, the build-up layer being composed of a nickel alloy underlayer and a cobalt alloy surface layer, and is characterized in that the base material surface on which the build-up layer is formed is a grooved surface in which adjacent grooves are aligned without any gaps.

[0009] The groove depth of the adjacent grooves is set to be not less than 40 μm and not more than 300 μm.

[0010] The cross-sectional shape of the groove may be an arc shape or a V shape. Effect of the Invention

[0011] When forming a build-up layer on the surface of duplex stainless steel by laser cladding or the like, if the surface of the base material, duplex stainless steel, is smooth, residual stress will concentrate on the smooth parts of the build-up layer and tend to become the starting points for cracks.

[0012] In this invention, by making the surface of the base material, duplex stainless steel, into a grooved surface in which adjacent grooves are lined up without any gaps, the occurrence of microcracks in the buildup layer can be suppressed by stress dispersion caused by the grooves. [Brief description of the drawings]

[0013] [Figure 1]1 is an enlarged schematic cross-sectional view of an example of a sliding member according to the present invention; [Diagram 2] 11 is an enlarged schematic cross-sectional view of another example of a sliding member according to the present invention; FIG. [Diagram 3] 1 is a micrograph of a cross section of a sliding member in which an experiment was conducted to determine whether cracks would occur in the buildup layer depending on differences in the depth of a groove formed on the surface of the base material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings.

[0015] FIG. 1 is an enlarged schematic cross-sectional view of a sliding member according to the present invention.

[0016] The sliding member according to the present invention has a build-up layer 2 made of a nickel alloy underlayer 2a and a cobalt alloy surface layer 2b formed on the surface of a base material 1 made of duplex stainless steel.

[0017] The thickness of the nickel alloy lower layer 2a is 1 mm to 1.5 mm, the thickness of the cobalt alloy surface layer 2b is 1.5 mm to 2.0 mm, and the total thickness of the buildup layer 2 is about 2.5 to 3.5 mm.

[0018] The nickel alloy constituting the lower layer 2a may be an Inconel alloy, a Hastelloy alloy, or the like.

[0019] As the cobalt alloy constituting the surface layer 2b, a Stellite alloy, a Triballoy alloy, an Inconel alloy containing carbide, or the like can be used.

[0020] It is preferable to use a laser cladding method and a plasma arc welding method to provide the lower layer 2a and the surface layer 2b on the surface of the duplex stainless steel, which is the base material 1. As another method, in addition to thermal spraying, powder plasma spraying, laser cladding and thermal spraying can also be combined.

[0021] The surface of the base material 1 on which the buildup layer 2 is formed is formed into a grooved surface in which adjacent groove portions 1a are arranged without any gaps.

[0022] The depth d of the groove 1a is set to 40 μm or more. If the depth of the groove 1a is 40 μm or less, the surface of the base material 1 on which the pre-buildup layer 2 is formed becomes flat, and residual stress is concentrated in the buildup layer 2 built up on the flat surface, which makes it easy for microcracks to occur in the buildup layer 2. These microcracks are likely to become the starting points for cracks in the buildup layer 2.

[0023] The depth d of the groove 1a is set to a maximum of 300 μm or less. The reason for this is that when the build-up layer 2 is formed on the surface of the duplex stainless steel base material 1 by laser processing, low heat input and low dilution build-up conditions are set in order to suppress the thermal effects and dilution (penetration) of the duplex stainless steel base material 1, and therefore, if the surface of the base material 1 becomes uneven, poor fusion tends to occur.

[0024] The surface of the base material 1 of the present invention is formed into a grooved surface in which adjacent grooves 1a are lined up without any gaps, so that no flat portion is formed between adjacent grooves 1a. By forming the surface of the base material 1 into a grooved surface in which adjacent grooves 1a are lined up without any gaps, the grooves 1a distribute the stress of the buildup layer 2 when the buildup layer 2 is formed, so that the occurrence of microcracks is suppressed, and cracks originating from the microcracks are less likely to occur in the buildup layer 2.

[0025] The grooved surface, in which adjacent grooves 1a are aligned without any gaps, can be achieved by lathe machining using a round or triangular tip.

[0026] When the surface of the base material 1 is turned on a lathe using a round tip, a groove portion 1a having an arc-shaped cross section as shown in FIG. 1 can be formed, and when the surface of the base material 1 is turned on a lathe using a triangular tip, a groove portion 1a having a V-shaped cross section as shown in FIG. 2 can be formed.

[0027] Figure 3 is a micrograph of an experiment conducted to determine whether cracks would occur in the buildup layer 2 when grooves 1a with depths of 10 μm, 20 μm, 30 μm, 40 μm, 100 μm, and 200 μm were machined using a round tip on the surface of the base material 1, which was a duplex stainless steel, and a buildup layer 2 was formed on the grooved surface by laser cladding.

[0028] In the experiment of FIG. 3, the nickel alloy constituting the lower layer 2a of the buildup layer 2 is a Hastelloy alloy having a thickness of 1.0 mm, and the cobalt alloy constituting the surface layer 2b is a Stellite alloy having a thickness of 1.5 mm.

[0029] As shown in FIG. 3, when the depth of the groove portion 1a was 10 μm, 20 μm, and 30 μm, cracks occurred in the buildup layer 2, but when the depth of the groove portion 1a was 40 μm, 100 μm, and 200 μm, no cracks occurred in the buildup layer 2.

[0030] This invention is not limited to the above-described embodiments, and can of course be embodied in various other forms without departing from the spirit of the invention. The scope of the invention is indicated by the claims, and further includes the equivalent meanings set forth in the claims, and all modifications within the scope of the claims. [Explanation of symbols]

[0031] 1: Base material 1a:Groove 2: Overlay layer 2a: Lower layer 2b: Surface layer

Claims

1. A sliding member having a build-up layer made of a nickel alloy underlayer and a cobalt alloy surface layer on the surface of a duplex stainless steel base material, the slide member being characterized in that the base material surface on which the build-up layer is formed is a grooved surface in which adjacent grooves are aligned without any gaps.

2. 2. The sliding member according to claim 1, wherein the adjacent grooves have a groove depth of 40 μm or more and 300 μm or less.

3. 3. The sliding member according to claim 1, wherein the groove has a cross-sectional shape of a circular arc.

4. 3. The sliding portion according to claim 1, wherein the groove has a V-shaped cross section. Material.

Citation Information

Patent Citations

  • Coated member, and overlaying structure

    JP2012166237A

  • Slide member

    JP2018187647A