Method for producing foam sheet

By controlling the discharge, adjustment, and drying processes within specific parameters, the method addresses the challenge of continuous foam sheet production, resulting in high-performance urethane foam sheets with improved hydrophilicity.

JP2024152017APending Publication Date: 2024-10-25INOAC TECHN CENT
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023065904
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing methods face challenges in continuously producing foam sheets with excellent performance.

Method used

A method involving specific manufacturing conditions, including a discharging step, an adjusting step, and a drying step, where the composition is discharged at a predetermined line speed, adjusted to a predetermined thickness and width, and dried in an oven, adhering to certain time and ratio formulas to ensure optimal foam formation.

Benefits of technology

Enables the production of urethane foam sheets with enhanced performance, particularly hydrophilic foam, suitable for applications requiring water absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152017000002
    Figure 2024152017000002
  • Figure 2024152017000003
    Figure 2024152017000003
  • Figure 2024152017000004
    Figure 2024152017000004
Patent Text Reader

Abstract

To provide a method for producing a foam sheet that enables continuous production of a foam sheet with superior performance.SOLUTION: A method for producing a foam sheet disclosed herein includes a discharge step for discharging a composition that contains a first liquid containing a urethane prepolymer and a second liquid containing water toward a line flowing at a predetermined line speed; an adjustment step for adjusting the composition discharged onto the line so as to have a predetermined thickness and width; and a drying step for drying the composition that has undergone the adjustment step within a dry furnace, where the composition has a gel time TG fulfilling formula 1.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a foamed sheet. [Background technology]

[0002] Hydrophilic urethane foam is widely used in applications where absorbency (amount and speed of water absorption) is required, such as initial wound dressings, cosmetics, incontinence products, wipes, and seedling culture media.

[0003] Patent Document 1 discloses a hydrophilic urethane foam having excellent thermal comfort and the like, which uses a hydrophilic isocyanate-terminated prepolymer obtained by using a reactive component containing a specific isocyanate component and the like. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-534727 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0005] However, in the conventional techniques, it is sometimes difficult to continuously produce foamed sheets.

[0006] Therefore, an object of the present invention is to provide a method for producing a foamed sheet, which enables continuous production of a foamed sheet having excellent performance. [Means for solving the problem]

[0007] The present inventors have conducted extensive research and found that the above problems can be solved by setting the production conditions of a foamed sheet to satisfy specific conditions. That is, the present invention is as follows.

[0008] Certain aspects of the present disclosure include: A discharge step of discharging a composition including a first liquid including a urethane prepolymer and a second liquid including water toward a line flowing at a predetermined line speed; an adjusting step of adjusting the composition discharged onto the line to a predetermined thickness and width; a drying step of drying the composition after the adjusting step in a drying oven; Including, The gel time T of the composition G The method for producing a foamed sheet is characterized in that the following formula 1 is satisfied: (Formula 1) 0.7≦T G / T T <1.2 T T is the time it takes for the composition to be transported from the point where it was dispensed to the exit of the drying oven.

[0009] Cream Time T of the composition C is the residence time T defined as S It is preferable that it is longer than . (residence time T S ) The time from when the composition is discharged to when it reaches a predetermined width through the adjustment process is called the residence time T S Let us assume that. Cream Time T of the composition C However, it is preferable that the time is 15 seconds or more and 60 seconds or less. The adjusting step is preferably a step of adjusting the width of the composition to 300 mm or more.

[0010] According to the present invention, it is possible to provide a urethane foam having excellent performance. In particular, according to the present invention, it is possible to provide a urethane foam having excellent performance that can be preferably used as a hydrophilic foam. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram of a production line for the method of producing a foamed sheet. [Diagram 2]FIG. 2(1) is a conceptual side view showing the state of the composition in the preparation process, and FIG. 2(2) is its conceptual top view. [Diagram 3] 3(1) and 3(2) are conceptual top views showing modified examples of the ejection process and the adjustment process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, when an upper limit value and a lower limit value are separately described, it is deemed that a numerical range combining any upper limit value and any lower limit value is substantially disclosed.

[0013] In the following, unless otherwise specified, various measurements are carried out at room temperature (23° C.).

[0014] <<< Manufacturing method of foam sheet >>>

[0015] The method for producing a foam sheet according to the present disclosure includes a step of reacting a urethane prepolymer with water to obtain a foam sheet.

[0016] More specifically, the method for producing the foamed sheet includes: A discharge step of discharging a composition including a first liquid including a urethane prepolymer and a second liquid including water toward a line flowing at a predetermined line speed; an adjusting step of adjusting the composition discharged onto the line to a predetermined thickness and width; a drying step of drying the composition after the adjusting step in a drying oven; It is preferred that the compound contains

[0017] Hereinafter, each step will be described mainly with reference to FIG. 1, which is a schematic diagram of a production line (hereinafter, simply referred to as a line) relating to the method for producing a foamed sheet.

[0018] <<Discharge process>> The discharge step is a step of discharging a composition 110 containing a first liquid containing a urethane prepolymer and a second liquid containing water from a discharge part 15 onto a line flowing at a predetermined line speed. Note that the step of "discharging a composition onto a line" shown here also includes a step of "discharging a composition onto a substrate flowing along the line." The substrate is, for example, an undercarrier 21 described below.

[0019] In the manufacturing method of the present disclosure, the water contained in the second liquid reacts with the urethane prepolymer contained in the first liquid to generate carbon dioxide gas, which then causes foaming. Specific examples of the first liquid containing the urethane prepolymer and the second liquid containing water will be described later.

[0020] The first liquid containing a urethane prepolymer is stored in a first liquid tank 11. The second liquid containing water is stored in a second liquid tank 12. The first liquid stored in the first liquid tank 11 is sent to the mixing section 13 by a pump (not shown). Similarly, the second liquid stored in the second liquid tank 12 is sent to the mixing section 13 by a pump (not shown). In this manner, the first liquid and the second liquid are filled in the mixing section 13. In the mixing section 13, the first liquid and the second liquid are stirred using a known stirring means such as a mixer as necessary, and a mixture of the first liquid and the second liquid is formed. This mixture is sent to the discharge section 15 as a composition 110 by a pump (not shown).

[0021] The stirring step can be carried out using a known stirring means such as a mixer.

[0022] The stirring conditions in the stirring step may be appropriately selected depending on the viscosity of the composition, the components to be mixed, and the like.

[0023] Since the reactivity between the first liquid and the second liquid can be easily controlled, the temperature at which the contents of the first liquid tank 11, the second liquid tank 12, and the mixing section 13 are kept warm is preferably 10° C. or higher, 15° C. or higher, 20° C. or higher, or 25° C. or higher, and is preferably 40° C. or lower, or 35° C. or lower. A specific temperature is, for example, 30° C.

[0024] The mixing ratio of the first liquid to the second liquid may be appropriately adjusted depending on the raw materials used, etc. For example, the ratio of the first liquid to the second liquid (first liquid / second liquid) is 100 / 50 to 100 / 10, or 100 / 40 to 100 / 20, etc.

[0025] Next, the composition 110, which is a mixture of the first liquid and the second liquid, is discharged from the discharge section 15 onto the line. In the present disclosure, the discharge section 15 is a cylindrical or tubular member, and the composition 110 is sent out onto the line in a substantially cylindrical shape. In the discharge process according to the present disclosure, the composition 110 is discharged onto the continuous undercarrier 21, and the composition 110 moves from the upstream to the downstream of the line along the movement of the undercarrier 21. In the discharge process, the undercarrier 21 may be provided on a movable member (such as a roller or conveyor, not shown), and the composition 110 may be further discharged onto the undercarrier 21, and the undercarrier 21 and the composition 110 discharged onto the undercarrier 21 may move from the upstream to the downstream of the line at a predetermined speed along the movement of the movable member. Such a speed at which the undercarrier 21 is sent out and the moving speed of the movable member (the speed at which the composition 110 moves along the line) are referred to as the line speed.

[0026] As shown in FIG. 1, in the discharge process according to the present disclosure, the undercarrier 21 is pulled out from an undercarrier delivery section 31 in which the undercarrier 21 is rolled, and provided on a line.

[0027] The undercarrier 21 is usually a film-like member. It is preferable to use an undercarrier 21 that is difficult for the composition 110 to penetrate and has low elasticity. The undercarrier 21 may be subjected to an appropriate surface treatment such as a release treatment, a sand mat treatment, or a chemical mat treatment. The undercarrier 21 is not particularly limited, and a PET sheet, a PP sheet, a PE sheet, a paper-based sheet (e.g., release paper), etc. can be used.

[0028] The line speed may be set in consideration of the conditions in the adjusting step and drying step described below. The line speed is, for example, preferably 0.1 m / min or more, 0.5 m / min or more, 1.0 m / min or more, or 2.0 m / min or more, and preferably 50 m / min or less, 20 m / min or less, or 10 m / min or less. Under such conditions, a foamed sheet having excellent performance is easily obtained, and the productivity of the foamed sheet can be increased.

[0029] In the present disclosure, a method has been shown in which the first liquid and the second liquid are mixed in advance in the mixing section 13. However, it is also possible to feed the first liquid and the second liquid directly to the discharge section 15 without providing the mixing section 13, form a mixture of the first liquid and the second liquid inside the discharge section 15, and discharge it from the discharge section 15.

[0030] The viscosity (25°C viscosity) of composition 110 is preferably 100 mPa·s or more, 200 mPa·s or more, 500 mPa·s or more, 1,000 mPa·s or more, or 1,500 mPa·s or more, and is preferably 5,000 mPa·s or less, 4,500 mPa·s or less, 4,000 mPa·s or less, 3,500 mPa·s or less, or 3,000 mPa·s or less. By setting the viscosity of composition 110 within such a range, it becomes easy to mold a foam, and a foam sheet with excellent performance can be easily obtained.

[0031] FIG. 1 shows a form in which the angle of the line at the position (discharge position S) where the composition is discharged from the discharge part 15 has an inclination angle θ with respect to the horizontal direction. In other words, in FIG. 1, the undercarrier 21 is sent to the discharge position S along a line inclined upwards (at the discharge position S, the undercarrier 21, which is the discharge surface of the composition, is inclined with respect to the horizontal direction). Thereafter, the inclination of the line is eliminated from the vicinity beyond the discharge position S, and the line is configured to move in the horizontal direction. At this time, the inclination angle θ of the line (the angle formed by the horizontal direction and the inclination of the line) is not particularly limited. From the viewpoint of preventing the composition 110 discharged from the discharge part 15 from flowing back to the discharge part 15, it is preferable that the inclination angle θ is +15° or less, +10° or less, +5° or less, +1° or less, or +0° or less. The inclination angle θ being 0° means that the line has no inclination at the discharge position S. In FIG. 1, a configuration in which the undercarrier send-out section 31 side is downward and the discharge position S side is upward (upward slope configuration) is shown, but a configuration in which the undercarrier send-out section 31 side is upward and the discharge position S side is downward (downward slope configuration) is also possible. In this case, the inclination angle θ is less than 0°. Specifically, the inclination angle θ may be less than 0°, 1° or less, 2° or less, or 5° or less, or may be -15° or more, or -10° or more, or the like. That is, the inclination angle θ may be in a free range (for example, -15 to +15°, etc.) based on the horizontal direction.

[0032] 1 shows a method of discharging the composition 110 from above downward, but the discharging method is not limited to this. For example, when the composition 110 is a highly viscous composition, it is also possible to carry out the discharging step by discharging the composition 110 horizontally with the discharge part 15 turned sideways while the undercarrier 21 is moving vertically.

[0033] In addition, components other than the urethane prepolymer and water (other components) may be used as raw materials for the foamed sheet. When using other components, it is preferable to have the other components contained in the first liquid in advance, but the other components may be contained in the second liquid, or a third liquid containing the other components as a composition separate from the first and second liquids may be prepared, and the first, second, and third liquids may be mixed in the mixing section 13 to form a mixture (composition 110).

[0034] <<Adjustment process>> The adjustment step is a step of adjusting the thickness and width of the composition 110 discharged onto the line (onto the undercarrier 21) using the height adjustment means 40 to obtain the adjusted composition 120. Thus, in the present disclosure, the composition 110 after the adjustment step is referred to as the adjusted composition 120.

[0035] 1, the adjustment step according to the present disclosure has a lower roller 41 and an upper roller 42 as a height adjustment means 40 for the composition 110. That is, in the adjustment step according to the present disclosure, the composition 110 discharged from the discharge portion 15 is passed through the gap between the lower roller 41 and the upper roller 42, thereby adjusting the composition 110 to a predetermined thickness.

[0036] Fig. 2(1) is a conceptual side view showing how the height of the composition 110 is adjusted by passing the composition 110 through the gap between the lower roller 41 and the upper roller 42, and Fig. 2(2) is its conceptual top view. Note that in this figure, the under carrier 21 and the top carrier 22 are not shown.

[0037] As shown in FIG. 2(1), the gap between the lower roller 41 and the upper roller 42 is adjusted to be thinner than the thickness H1 of the composition 110 after being discharged from the discharge section 15. The composition 110 sandwiched between the undercarrier 21 and the top carrier 22 is rolled to a thickness H2, which is the same thickness as the width of the gap between the lower roller 41 and the upper roller 42 (or a thickness close to the width of the gap), by passing through this gap. At this time, the composition 110 that has reached the position of the lower roller 41 and the upper roller 42 is stopped by the upper roller 42 and the lower roller 41, and a part of it stays near the upper roller 42. As shown in FIG. 2(2), the composition 110 stopped by the upper roller 42 and the lower roller 41 is pushed out and spread in a direction (CD direction, width direction) perpendicular to the line direction (MD direction) by the pressure of the subsequent composition 110 fed along the line. Unless conditions are met in which the composition 110 blocked by the upper roller 42 and the lower roller 41 flows back upstream in the line direction (conditions such as the discharge amount of the composition 110 being too large or the line speed being too fast, causing a delay in the processing of the adjustment step), the flow rate (discharge amount) of the composition 110 discharged from the discharge section 150 and the flow rate of the adjustment composition 120 after passing through the lower roller 41 and the upper roller 42 are substantially the same. Therefore, the width W2 of the adjustment composition 120 is determined based on the flow rate of the composition 110, the height H2 of the adjustment composition 120, the line speed, etc.

[0038] As described above, the adjusted composition 120 formed by passing through the height adjusting means 40 (the gap formed by the lower roller 41 and the upper roller 42) has a thickness H2 smaller than the thickness H1 of the composition 110 after being discharged from the discharge portion 15, and a width W2 larger than the width W1 of the composition 110 after being discharged from the discharge portion 15. That is, the adjusted composition 120 moves downstream in the line in a state adjusted to be thinner and wider than the composition 110.

[0039] The thickness H2 of the adjusting composition 120 can be adjusted by changing the conditions set by the height adjusting means 40 (the width of the gap between the lower roller 41 and the upper roller 42 in FIG. 1), etc. Also, the width H2 of the adjusting composition 120 can be adjusted by changing the conditions set by the height adjusting means 40 (the width of the gap between the lower roller 41 and the upper roller 42 in FIG. 1), the line speed, the discharge amount of the composition 110, etc.

[0040] As described above, the adjustment process can also be described as a process of deforming composition 110, which has a thickness H1 and a width W1, to obtain an adjusted composition 110 having a thickness H2 that is less than the thickness H1 of composition 110 and a width W2 that is greater than the width W1 of composition 110.

[0041] In the adjustment process according to the present disclosure, as shown in FIG. 1, the top carrier 22 is laminated on the upper side of the composition 110 immediately before the composition 110 contacts the height adjustment means 40 (upper roller 42). That is, in the adjustment process according to the present disclosure, the adjustment process is performed in a state in which the composition 110 is sandwiched between the top carrier 22 and the undercarrier 21. In this way, by using not only the undercarrier 21 but also the top carrier 22 in the adjustment process, the height of the composition 110 is adjusted in a state in which it is sandwiched so as to be in close contact with the top carrier 22 and the undercarrier 21, so that the height H2 and the surface state of the obtained adjusted composition 120 are easily homogenized.

[0042] As shown in FIG. 1, in the adjustment process according to the present disclosure, the top carrier 22 is pulled out from a top carrier delivery section 32 in which the top carrier 22 is rolled, and provided on a line.

[0043] The top carrier 22 is usually a film-like member. It is preferable to use a top carrier 22 that is difficult for the composition 110 to penetrate and has low elasticity. The top carrier 22 may be subjected to an appropriate surface treatment such as a release treatment, a sand mat treatment, or a chemical mat treatment. The top carrier 22 is not particularly limited, and a PET sheet, a PP sheet, a PE sheet, a paper-based sheet (e.g., release paper), etc. can be used.

[0044] The adjusting step may be a step that does not use the top carrier 22. When the foamed sheet 130 is produced without using the top carrier 22, the top carrier delivery section 32 is not necessary.

[0045] Here, composition 110 is a mixture containing a first liquid containing a urethane prepolymer and a second liquid containing water, and this mixture undergoes a curing reaction over time between the isocyanate groups in the urethane prepolymer and the water.

[0046] In this case, Cream Time T of composition 110 C is the residence time T defined as S It is preferable that it is longer than .

[0047] Residence time T S The time from when the composition 110 is discharged onto the line to when it reaches a predetermined width (width W2) through the adjustment process is called the residence time T S As described above, during the adjustment process, the composition 110 held up by the height adjustment means 40 spreads in the CD direction due to the pressure of the following compositions 110 being sent one after another along the line. SThis can also be expressed as the time required from when the composition 110 is discharged until when the composition 110 reaches the outermost part in the CD direction of the height adjusting means 40 (corresponding to the edge of the adjusting composition 120 in the CD direction). The residence time can be calculated using parameters such as the height H2 of the adjusting composition 120 (or the width of the gap between the lower roller 41 and the upper roller 42), the line speed, the discharge amount of the composition 110, and the viscosity of the composition 110, but it can also be easily measured as an actual value measured visually.

[0048] Composition 110 Cream Time T C This refers to the time from when the first liquid and the second liquid are mixed at a raw material temperature of 30°C and an ambient temperature of 23°C, and 100 g of the mixture discharged from the discharge portion 15 is collected into a 1 L cup, until the mixture starts to foam and the liquid level of the mixture in the cup rises (starts to expand). Furthermore, when the composition 110 contains other components, these are mixed in advance with the first liquid.

[0049] Cream Time T C is the residence time T S By making the length longer than this, the curing reaction of composition 110 is less likely to occur before the adjustment process is completed, so that the resulting foamed sheet is less likely to crack or break cells, and a foamed sheet with excellent performance can be obtained.

[0050] In addition, the residence time T S Cream Time T of composition 110 C Ratio of (T C / T S ) is preferably more than 1.0, 1.1 or more, or 1.2 or more, and is preferably 1.6 or less, or 1.5 or less, or 1.4 or less. Under such conditions, a foamed sheet having excellent performance is easily obtained, and the productivity of the foamed sheet can be increased.

[0051] Composition 110 Cream Time T CSpecifically, the cream time T of the composition 110 is preferably 15 seconds or more, 20 seconds or more, or 25 seconds or more, and is preferably 60 seconds or less, 55 seconds or less, or 50 seconds or less. C By setting the content of the cream time T in this range, it is easy to obtain a foamed sheet having excellent properties. C can be easily adjusted by the pH of the second liquid, and the pH of the second liquid can be adjusted by a pH adjuster as described below. Thus, the method for producing a foamed sheet according to the present disclosure preferably includes a pH adjustment step of adding a pH adjuster to the second liquid to adjust the pH of the second liquid. In other words, in a composition (composition for producing a foam) including a first liquid containing a urethane prepolymer and a second liquid containing water, the second liquid preferably contains a pH adjuster.

[0052] In the adjustment process of the present disclosure, a form in which a lower roller 41 and an upper roller 42 are used as a means 40 for adjusting the height of the composition 110 has been described, but a known means (e.g., a slit-shaped member, a knife-shaped member, etc.) depending on the viscosity, etc. of the composition 110 may also be used as the means 40 for adjusting the height of the composition 110.

[0053] The height H2 of the adjusting composition 120 may be adjusted according to the height of the foamed sheet to be manufactured. Specifically, the height H2 of the adjusting composition 120 is preferably 1.0 mm or more, 1.5 mm or more, or 2.0 mm or more, and is preferably 10.0 mm or less, 8.0 mm or less, or 5.0 mm or less.

[0054] The width W2 of the adjusting composition 120 may be adjusted according to the width of the foamed sheet to be manufactured. Specifically, the width W2 of the adjusting composition 120 is preferably 100 mm or more, 200 mm or more, 300 mm or more, or 500 mm or more. The upper limit of the width W2 of the adjusting composition 120 is not particularly limited, and is, for example, 10 m, 5 m, or 1 m.

[0055] <<Examples of changes to the discharge process and adjustment process>> Here, in FIG. 1, the discharge part 15 is a cylindrical or tubular member, and a configuration in which only one such member is provided on the line is shown, but the configuration of the discharge part 15 is not limited to this.

[0056] 3(1) and 3(2) are conceptual top views showing modified examples of the ejection process and the adjustment process.

[0057] As shown in FIG. 3(1), the discharge step may be a step of discharging a plurality of discharge parts (discharge parts 15-1, 15-2, and 15-3) in parallel and discharging compositions (compositions 110-1, 110-2, and 110-3) from each discharge part. In this case, the compositions (compositions 110-1, 110-2, and 110-3) discharged from each discharge part are blocked by the height adjustment means 40, and adjacent compositions 110 are joined and integrated, and the height is adjusted to form a wide adjusted composition 120. In this way, by dispersing the composition 110 fed to the adjustment step in the CD direction by providing a plurality of discharge parts 15, the composition 120 that is retained near the height adjustment means (upper roller 42) during the adjustment step is less likely to flow back to the upstream side in the line direction, or the retention time T S On the other hand, when only one discharge portion 15 is provided, the composition 110 spreads evenly in the CD direction as a continuous composition during the preparation step (there is no junction between the compositions), which is advantageous in that streaks are less likely to occur in the obtained preparation composition 120.

[0058] When a plurality of discharge parts 15 are provided, the number of the discharge parts 15 is not particularly limited. When a plurality of discharge parts 15 are provided, the discharge amount of the composition 110 in each discharge part 15 does not have to be the same, and the installation positions of each discharge part 15 do not have to be arranged in parallel in the CD direction (the distance to the height adjustment means 40 may be different for each discharge part 15). Furthermore, when three or more discharge parts 15 are provided, the distance between each discharge part 15 does not have to be constant.

[0059] Furthermore, as shown in Fig. 2(2), the discharge part 15 may be a member capable of discharging over a wide range in the CD direction. Specifically, when the discharge part 15 is a die 15A as shown in Fig. 2(2), the composition 110 discharged from the die 15A is blocked by the height adjusting means 40 and spreads in the CD direction (CD direction), forming a wide adjusted composition 120 having a uniform height. In this way, by using a member capable of discharging over a wide range in the CD direction, such as the die 15A, as the discharge part 15, it is easy to obtain a wider adjusted composition 120, or the residence time T S This is advantageous in that the time required for the measurement can be shortened.

[0060] <<Drying process>> The drying step is a step in which the adjusted composition 120 obtained through the adjusting step is sent to a drying oven 50, the adjusted composition 120 is dried, and a foamed sheet 130 is obtained.

[0061] The drying oven 50 is, for example, a box-shaped drying oven extending along the line direction. Although not shown, the drying oven 50 has a cylindrical structure with an inlet and an outlet, and the adjusting composition 120 sandwiched between the under-carrier 21 and the top carrier 22 can flow down inside the drying oven 50.

[0062] The drying method in the drying oven 50 is not particularly limited and may be heat drying, air drying, reduced pressure drying, a combination of these, etc. The drying oven used in the drying step is, for example, a microwave oven, a high-frequency induction heating oven, a hot air drying oven, etc.

[0063] The drying conditions in the drying oven 50 can be appropriately changed depending on the height H2 of the adjusted composition 120, the line speed, etc. The drying temperature is, for example, 15°C or higher, 25°C or higher, 40°C or higher, 50°C or higher, 60°C or higher, 80°C or higher, etc. The drying temperature condition is, for example, 120°C, etc. The drying temperature may be changed inside the drying oven 50. For example, the drying temperature may be lowered near the entrance of the drying oven 50 and higher near the exit of the drying oven 50.

[0064] After the drying step is performed, or in the drying furnace 50, a film removing step of removing the top carrier 22 may be performed. In the film removing step, for example, the under-carrier 21 and the top carrier 22 may be removed by winding them up from the foamed sheet 130 using a film removing means such as the top carrier winding unit 33. Moreover, the foamed sheet 130 with a film may be manufactured without carrying out such a film removing step. Moreover, when the foamed sheet 130 is manufactured without using the top carrier 22, or when the foamed sheet 130 with a film is manufactured, the film removing means such as the top carrier winding part 33 is not necessary.

[0065] Here, the gel time T of the composition 110 G It is preferable that the following formula 1 is satisfied. (Formula 1) 0.7≦T G / T T <1.2

[0066] Gel time T of composition 110 G This indicates the time from the time the mixture is collected until the reaction of the mixture stops (the time until the mixture hardens and the tackiness of the upper surface of the formed foam disappears) when the first liquid and the second liquid are mixed at a raw material temperature of 30°C and an ambient temperature of 23°C, and 100 g of the mixture discharged from the discharge part 15 is collected in a 1 L cup. When the resin foam forming composition contains other components, the other components are mixed in advance with the first liquid.

[0067] Total time T T is the time required for the composition 110 to be transported from the discharged position (discharge position S) to the exit position (exit position E) of the drying oven 50 (through the adjustment process and drying process). T is the distance from the discharge position S to the exit position E (the length from the discharge position S to the adjustment means, the distance from the adjustment means to the drying oven 50, and the length of the drying oven 50 itself), the residence time T S , and the line speed.

[0068] Gel time T of composition 110 G and total time T T When the above relationship is satisfied, the reaction of the adjusting composition 120 is sufficiently carried out and drying is also sufficiently carried out, making it easier to obtain a foamed sheet having excellent performance.

[0069] Gel time T of composition 110 G The gel time T of the composition 110 is preferably 160 seconds or more, 170 seconds or more, or 180 seconds or more, and is preferably 320 seconds or less, 300 seconds or less, or 250 seconds or less. G can be easily adjusted by the pH of the second liquid.

[0070] Total time T T Although it differs depending on the manufacturing equipment, it is, for example, 170 seconds or more, 180 seconds or more, or 200 seconds or more, and 320 seconds or less, 300 seconds or less, or 250 seconds or less.

[0071] In addition, Cream Time T of composition 110 C Gel time T of composition 110 G The ratio (T G / T C ) is preferably 3.0 or more, 4.5 or more, 5.0 or more, 5.2 or more, or 5.5 or more, and is preferably 12.0 or less, 10.0 or less, 8.0 or less, or 6.5 or less. By using such a composition 110, it is possible to increase the productivity, etc., when continuously producing a foamed sheet.

[0072] After the drying step, a step of winding up the foamed sheet 130 and a step of processing the foamed sheet 130 (for example, cutting) may be further provided.

[0073] <<<<Foam sheet>>>> The foamed sheet obtained as described above has excellent properties (for example, excellent hydrophilicity) as a result of adjusting the production conditions.

[0074] The structure / physical properties / characteristics, raw materials (the first and second liquids used in the discharging step), applications, etc. of the foamed sheet obtained by the production method of the present disclosure will be described below.

[0075] <<<Physical properties / characteristics of foam sheets>>> <<density>> The density of the foam sheet is not particularly limited, but is preferably 50 kg / m 3 More than 60kg / m 3 More than 70kg / m 3 More than 80kg / m 3 It is preferable that the resistance is 150 kg / m or more. 3 Below 120kg / m 3 Less than or equal to 100kg / m 3 It is preferable that:

[0076] The density of the foamed sheet can be measured according to JIS K7222:2005 "Foamed plastics and rubber - Determination of apparent density". Specifically, the density of the foamed sheet can be obtained by processing the foamed sheet into a length of 50 mm x width of 50 mm, measuring the thickness and mass, and dividing the measured mass by the volume.

[0077] <<Water absorption rate>> The foamed sheet preferably has a water absorption speed, measured by the following method, of 3 sec or less, less than 1.5 sec, or less than 1 sec. (Measurement method) 8.4 g of sodium chloride and 0.4 g of potassium chloride are diluted with distilled water to make 1 L of solution, which is used as the evaluation liquid. At an ambient temperature of 25°C, 0.2 cc of the evaluation liquid at 37°C is dropped from a height of 1 cm onto a foam sheet (thickness, for example, 3 mm), and the water absorption rate is the time from when the evaluation liquid is dropped until the evaluation liquid is completely absorbed by the foam sheet.

[0078] <<Water absorption>> The foamed sheet preferably has a water absorption, as measured by the following method, of more than 15 g / g, more than 17 g / g, more than 18 g / g, or 20 g / g or more.

[0079] (Measurement method) 8.4 g of sodium chloride and 0.4 g of potassium chloride are diluted with distilled water to make 1 L of solution, which is used as the evaluation liquid. A foamed sheet of 50 mm x 50 mm (thickness, for example, 3 mm) is used as a test piece. Measure the mass A of the test piece in a dry state. The test piece is immersed in the evaluation liquid having 40 times the mass of A at 37°C for 30 minutes. After immersion in the evaluation liquid for 30 minutes, the test piece is taken out of the evaluation liquid and hung for 20 seconds, and then the mass B of the test piece is measured. Calculate the amount of water absorption using the following formula. Water absorption amount = (mass B - mass A) / mass A

[0080] <<Water retention rate>> The foamed sheet preferably has a water retention rate of more than 50% or more than 60%, as measured by the following method.

[0081] (Measurement method) 8.4 g of sodium chloride and 0.4 g of potassium chloride are diluted with distilled water to make 1 L of solution, which is used as the evaluation liquid. A foamed sheet of 50 mm x 50 mm (thickness, for example, 3 mm) is used as a test piece. Measure the mass A of the test piece in a dry state. The test piece is immersed in the evaluation liquid having 40 times the mass of A at 37°C for 30 minutes. After immersion in the evaluation liquid for 30 minutes, the test piece is taken out of the evaluation liquid and hung for 20 seconds, and then the mass B of the test piece is measured. After hanging for 20 seconds, a load of 40 mmHg is applied to the test piece. After the load is applied, measure the mass C of the test piece two minutes later. Calculate the water retention rate using the following formula. Water retention rate = (mass C - mass A) / (mass B - mass A) × 100

[0082] <<Swelling rate>> The foamed sheet preferably has a swelling ratio, measured by the following method, of 300% or less, 250% or less, or 200% or less. (Measurement method) 8.4 g of sodium chloride and 0.4 g of potassium chloride are diluted with distilled water to make 1 L of solution, which is used as the evaluation liquid. The dimensions of the test piece when dry are measured, and the volume A is calculated. The test piece is immersed in the evaluation liquid having a mass 40 times the mass of the test piece (the above-mentioned mass A) at 37° C. for 30 minutes. After immersion in the evaluation liquid for 30 minutes, the test piece is taken out from the evaluation liquid, the dimensions of the test piece are measured, and the volume B is calculated. The swelling ratio is calculated using the following formula. Swelling ratio = volume B / volume A x 100

[0083] <<<Raw materials for foam sheets>>> As described above, the foamed sheet is produced from the first liquid containing the urethane prepolymer and the second liquid containing water. As described above, a component (other component) other than the urethane prepolymer and water may be used as a raw material for the foamed sheet. In this case, it is preferable that the other component is contained in the first liquid. Each of these will be explained below.

[0084] <<1st liquid>> The first liquid contains a urethane prepolymer. The urethane prepolymer is obtained by reacting a polyol with a polyisocyanate. In other words, the urethane prepolymer is a reaction product of a polyol and a polyisocyanate. More specifically, the urethane prepolymer is an isocyanate-terminated urethane prepolymer obtained by a urethane reaction between a polyol and a polyisocyanate such that the polyisocyanate is in excess.

[0085] <Polyol> The polyol used in the production of the urethane prepolymer is not particularly limited and can be freely selected.

[0086] Examples of the polyol include polyester polyol, polycarbonate polyol, polyether polyol, and polyester ether polyol.

[0087] Examples of polyester polyols include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and azelaic acid, aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, alicyclic dicarboxylic acids such as hexahydrophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid, and acid esters or acid anhydrides thereof, and ethylene glycol, 1,3-propylene glycol, 1,2-propylene ... Examples of the polyols include polyester polyols such as polypropylene glycol obtained by a dehydration condensation reaction with lactone monomers such as ε-caprolactone and methylvalerolactone; and polyester polyols such as ε-caprolactone and methylvalerolactone obtained by ring-opening polymerization of lactone monomers such as ε-caprolactone and methylvalerolactone.

[0088] Examples of polycarbonate polyols include those obtained by reacting at least one of polyhydric alcohols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1,8-octanediol, 1,9-nonanediol, and diethylene glycol with diethylene carbonate, dimethyl carbonate, diethyl carbonate, and the like.

[0089] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc., which are obtained by polymerizing cyclic ethers such as ethylene oxide (EO), propylene oxide, tetrahydrofuran, etc., and copolyethers thereof. Polyether polyols can also be obtained by polymerizing the above-mentioned cyclic ethers using polyhydric alcohols such as glycerin and trimethylolethane.

[0090] Examples of polyester ether polyols include those obtained by a dehydration condensation reaction of aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and azelaic acid; aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as hexahydrophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; or acid esters or acid anhydrides of these acids with glycols such as diethylene glycol or propylene oxide adducts, or mixtures thereof.

[0091] The polyols may be used alone or in combination.

[0092] The polyol is preferably a diol and / or a triol.

[0093] When it is desired to improve the water absorption property of the obtained foamed sheet, a method of using a random type polyether polyol as the polyol can be mentioned. More specifically, by containing 50 mass % or more, 60 mass % or more, 70 mass % or more, 80 mass % or more, or 90 mass % or more of the random type polyether polyol in the total polyol constituting the urethane prepolymer, a foamed sheet with better water absorption property can be obtained.

[0094] The random type polyether polyol contains ethylene oxide. Here, the random type of the random type polyether polyol indicates that it is a random copolymer. That is, the random type polyether polyol indicates a polyether polyol in which ethylene oxide and propylene oxide are randomly copolymerized. Note that the polyether polyol in which ethylene oxide and propylene oxide are block copolymerized is called a block type polyether polyol.

[0095] The random type polyether polyol preferably has a ratio of ethylene oxide per molecule of the random type polyether polyol (hereinafter, sometimes referred to as the random type polyether polyol EO content) of 20.0 mass % or more, 25.0 mass % or more, or 30.0 mass % or more.

[0096] The random type polyether polyol preferably contains a diol compound and a triol compound.

[0097] The average number of functional hydroxyl groups in the entire random type polyether polyol is not particularly limited, but is preferably more than 2.0 and less than 3.0, or 2.4 or more and 2.7 or less.

[0098] The number average molecular weight of the polyol is preferably 200-5,000, 300-4,500, or 400-4,000.

[0099] The raw material for the urethane prepolymer may contain a monool other than the polyol as an alcohol component, as long as the effect of the invention is not impaired.

[0100] <Polyisocyanate> The polyisocyanate is not particularly limited and can be freely selected.

[0101] The polyisocyanate may be difunctional or trifunctional or higher.

[0102] Examples of bifunctional polyisocyanates include: Aromatic compounds such as 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 2,4'-diphenylmethane diisocyanate (2,4'-MDI), 2,2'-diphenylmethane diisocyanate (2,2'-MDI), hydrogenated MDI, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, polymethylene polyphenyl polyisocyanate, 1,5-naphthalene diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, and tetramethylxylene diisocyanate (TMXDI); Alicyclic ones such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and methylcyclohexane diisocyanate; Examples of the isocyanate include alkylene-based isocyanates such as butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, and lysine diisocyanate.

[0103] Examples of tri- or higher functional polyisocyanates include 1-methylbenzene-2,4,6-triisocyanate, 1,3,5-trimethylbenzene-2,4,6-triisocyanate, biphenyl-2,4,4'-triisocyanate, diphenylmethane-2,4,4'-triisocyanate, methyldiphenylmethane-4,6,4'-triisocyanate, 4,4'-dimethyldiphenylmethane-2,2',5,5'tetraisocyanate, triphenylmethane-4,4',4"-triisocyanate, polymeric MDI, lysine ester triisocyanate, 1,3,6-hexamethylene triisocyanate, 1,6,11-undecane triisocyanate, bicycloheptane triisocyanate, and 1,8-diisocyanatomethyloctane.

[0104] The polyisocyanate may also include modified products and derivatives thereof.

[0105] The polyisocyanates can be used alone or in combination.

[0106] The polyisocyanate preferably contains an aliphatic isocyanate. More specifically, the aliphatic isocyanate is preferably contained in an amount of 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more of the total polyisocyanate constituting the urethane prepolymer.

[0107] The amount of polyisocyanate can be adjusted so that the average functional number of hydroxyl groups in the polyol and the NCO% of the urethane prepolymer are within the desired ranges. The amount of polyisocyanate can be, for example, 10 to 40% by mass or 20 to 35% by mass, assuming that the total amount of polyol and polyisocyanate is 100% by mass.

[0108] <Other ingredients> The other components include resin components other than the urethane prepolymer and known additives, such as catalysts (e.g., amine catalysts, organometallic catalysts, etc.), surfactants (foam stabilizers, etc.), antioxidants, ultraviolet absorbers, antibacterial agents, etc.

[0109] <<Second liquid>> The second liquid contains water. When the water contained in the second liquid reacts with the urethane prepolymer contained in the first liquid, carbon dioxide gas is generated, and the carbon dioxide gas causes foaming.

[0110] The pH of the second liquid is preferably less than 7.0, 6.8 or less, 6.5 or less, 6.3 or less, or 6.0 or less. The lower limit of the pH of the second liquid is not particularly limited, but is, for example, 5.0 or 5.5. By setting the pH of the second liquid in such a range, the gel time T G Cream Time TC The pH of the second liquid is a value measured using a commercially available pH measuring device (a handy pH meter manufactured by HORIBA).

[0111] The pH of the second liquid can be adjusted by using an appropriate pH adjuster (e.g., sodium phosphate, sodium acetate, potassium acetate, citric acid, sodium citrate, potassium citrate, sodium benzoate, potassium benzoate, potassium carbonate, sodium bicarbonate, sodium carbonate, etc.).

[0112] The second liquid may contain a foaming agent other than water.

[0113] <<<Applications of foam sheets>>> A preferred form of the foam sheet according to the present disclosure is a hydrophilic urethane foam. More specifically, the foam sheet can be preferably used for absorbing water, such as wipe materials, seedling culture media, sanitary products, and medical devices (particularly wound dressings). EXAMPLES

[0114] EXAMPLES Hereinafter, the method for producing a foamed sheet and the foamed sheet will be specifically described with reference to examples and comparative examples, but the present invention is not limited to the following.

[0115] <<<<Example 1>>>> A foam sheet was produced using the production line shown in FIG.

[0116] <<<Raw materials>>> <<1st liquid>> As raw materials, 24.3 parts by mass of polyol I, 24.3 parts by mass of polyol II, 25.8 parts by mass of polyethylene glycol, 25.6 parts by mass of polyisocyanate, and a catalyst in an amount of 20 ppm based on the total amount of Liquid 1 were weighed into a reaction vessel, heated to a temperature range of 55°C ± 5°C, and reacted for 4 hours to produce a composition containing a prepolymer, which was used as Liquid 1. The viscosity of the prepolymer is shown in Table 1. <Polyol I> Random type polyol Ethylene oxide / propylene oxide copolymer Average number of functional groups 2 Number average molecular weight 1000 EO content 50% by mass Hydroxyl value: 112.1 mg KOH / g <Polyol II> Random type polyol Ethylene oxide / propylene oxide copolymer Average number of functional groups 3 Number average molecular weight 1500 EO content 70% by mass Hydroxyl value: 112.1 mg KOH / g <peg100> Polyethylene glycol Average number of functional groups 2 Number average molecular weight 1000 EO content 100% by mass Hydroxyl value: 113mgKOH / g <Polyisocyanate> Hexamethylene diisocyanate (HDI) <Catalyst> TIB Chemical KAT 716LA

[0117] <<Second liquid>> Water was used as the second liquid, and a small amount of a pH adjuster was added to adjust the pH of the second liquid to the values ​​shown in Table 1.

[0118] <<<Discharge process>>> The first and second liquids were stirred and mixed in the blending ratio shown in Table 1 to form a composition. Next, using only one cylindrical discharge part, the inclination angle of the discharge part was set to 10°, and the composition was discharged from the discharge part onto the undercarrier. The line speed, the discharge amount of the composition, the cream time and the gel time of the composition are as shown in Table 1. Release paper was used as the undercarrier.

[0119] <<<Adjustment process>>> The composition on the undercarrier was passed between vertically arranged roll members to adjust the thickness and width of the composition so that the molded product had the thickness shown in Table 1. The width of the gap between the roll members was 0.25 mm. Note that a top carrier was placed on the composition before the composition was passed between the roll members. Release paper was used as the top carrier.

[0120] <<<Drying process>>> The composition after the preparation process was sent to a drying oven and dried by heating at 80-100°C. After drying, the top carrier was removed to produce a foamed sheet. The thickness and density of the obtained foamed sheet (molded product) are shown in Table 1.

[0121] The total time T required for the composition to move from the discharged position to the outlet of the drying oven is T was 247.5 seconds.

[0122] <<<<Examples 2-3, Comparative Example 1, Comparative Example 2>>>> Foam sheets according to Examples 2 and 3, Comparative Example 1, and Comparative Example 2 were produced in the same manner as in Example 1, except that the production conditions were changed to those shown in Table 1.

[0123] <<<<Example 4-6>>>> The foamed sheets according to Examples 4 to 6 were produced in the same manner as in Example 1, except that the composition discharge method and discharge amount were changed to those shown in Table 1. Specifically, in Example 4, two discharge parts spaced apart were used, in Example 5, two discharge parts spaced apart were used, and in Example 6, a die-shaped wide discharge part was used. For Examples 4 and 5, the total discharge amount of all the discharge parts is shown in Table 1.

[0124] <<<<Evaluation>>>> The obtained foamed sheet (molded article) was evaluated for its width, appearance, water absorption rate, water absorption amount, water retention rate, and swelling rate. The methods for measuring the density, water absorption rate, water absorption amount, water retention rate, and swelling rate of the molded article were as described above.

[0125] The width, appearance, water absorption and water retention of the molded product were scored based on the following criteria, and the scores were totaled to make an overall judgment.

[0126] <<<Width>>> (Evaluation Criteria) 1 point: Less than 500mm 2 points: 500mm or more

[0127] <<<Water absorption>>> (Evaluation Criteria) 0 points: 15g / g or less (or cannot be evaluated) 1 point: over 15g / g

[0128] <<<Water retention rate>>> (Evaluation Criteria) 0 points: 50% or less (or unable to evaluate) 1 point: over 50%

[0129] <<<Appearance>>> The surface of the foam sheet was observed. (Evaluation Criteria) 0 points: Cells are uneven, missing, or not cured properly 1 point: No uneven foaming, cells are uniform

[0130] <<<Overall rating>>> ×: Total score 2 points or less △: Total score 3~4 points ○: Total points 5 points

[0131] [Table 1]

Claims

1. a discharge step of discharging a composition including a first liquid including a urethane prepolymer and a second liquid including water toward a line flowing at a predetermined line speed; an adjusting step of adjusting the composition discharged onto the line to a predetermined thickness and width; a drying step of drying the composition after the adjusting step in a drying oven; Including, The gel time T of the composition G A method for producing a foamed sheet, characterized in that the following formula 1 is satisfied: (Formula 1) 0.7≦T G / T T <1.2 T T is the time it takes for the composition to be transported from the point where it is dispensed to the exit of the drying oven.

2. Cream Time T of the composition C is the residence time T defined as S The method for producing a foamed sheet according to claim 1, wherein the length of the foamed sheet is longer than the length of the foamed sheet. (Residence time T S ) The time from when the composition is discharged to when it reaches a predetermined width through the adjustment process is called the residence time T S Let us assume that.

3. Cream Time T of the composition C The method for producing a foamed sheet according to claim 1, wherein the foaming time is from 15 seconds to 60 seconds.

4. The method for producing a foamed sheet according to any one of claims 1 to 3, wherein the adjusting step is a step of adjusting the width of the composition to be 300 mm or more.

Citation Information

Patent Citations

  • Hydrophilic prepolymer for polyurethane foam

    JP2017534727A