Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

A toner formulation with a binder resin, rhodamine dye, and hindered amine compound addresses fine line reproducibility issues in toners, maintaining image quality by preventing electron transfer and ensuring uniform charging.

JP2024152024AInactive Publication Date: 2024-10-25FUJIFILM CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023065921
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Toner using rhodamine dyes experiences deterioration in fine line reproducibility under certain conditions, leading to poor transfer and scattering of toner images.

Method used

A toner formulation containing a binder resin, a rhodamine dye, and a hindered amine compound, with specific mass ratios and chemical structures, is developed to suppress electron transfer and maintain uniform charging properties.

Benefits of technology

The toner formulation effectively suppresses deterioration in fine line reproducibility, ensuring consistent and high-quality image transfer even under high voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152024000013
    Figure 2024152024000013
  • Figure 2024152024000014
    Figure 2024152024000014
  • Figure 2024152024000001
    Figure 2024152024000001
Patent Text Reader

Abstract

To provide a toner for electrostatic charge image development, an electrostatic charge image developer, a process cartridge, an image forming apparatus, and an image forming method with which a reduction in thin line reproducibility is prevented.SOLUTION: Provided are a toner for electrostatic charge image development having toner particles including a binder resin, a rhodamine pigment, and a hindered amine compound, an electrostatic charge image developer, a process cartridge, an image forming apparatus, and an image forming method.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge, an image forming apparatus, and an image forming method. [Background technology]

[0002] In electrophotographic image formation, an electrostatic image formed on an image carrier is developed with an electrostatic image developer containing a toner for developing electrostatic images (hereinafter also referred to as "toner"). The resulting toner image is then transferred to a recording medium and fixed to form a fixed image.

[0003] In recent years, in the field of electrophotographic image formation, printers for commercial printing, publishing, paper packaging, and the like have been developed, and toners exhibiting various colors have been developed accordingly to improve color reproducibility. As one of such toners, toners using rhodamine dyes as colorants are known. Toners using rhodamine dyes are useful because they have excellent reproducibility of high chroma fluorescent colors, for example, from orange to red or from orange to purple.

[0004] For example, Patent Document 1 discloses a fluorescent toner that utilizes an aqueous fluorescent ink in which fine particles of a polyester resin containing an ionic group in the range of 20 to 1000 eq. / ton and an average particle size of 1 μm or less are finely dispersed in an aqueous medium, the fine particles containing a fluorescent dye that is insoluble or poorly soluble in water and soluble in organic solvents. In Patent Document 1, rhodamine dyes such as chalcoside rhodamine B concentrate, rhodamine B stearate concentrate, and rhodamine B ethyl ester are exemplified as dyes that can be used for fluorescent toners.

[0005] Furthermore, for example, Patent Document 2 discloses "a method for producing a liquid developer containing a binder resin including a resin having an acidic group, a colorant, a basic dispersant, and an insulating liquid, comprising: step I: stirring a raw material including the binder resin, the colorant, and the basic dispersant at a temperature equal to or higher than the glass transition temperature of the binder resin; and step II: dropping 50 to 500 parts by mass of the insulating liquid relative to 100 parts by mass of the stirred product of step I at a temperature equal to or higher than the glass transition temperature of the binder resin to effect phase inversion emulsification, thereby obtaining a dispersion of toner particles." Patent Document 2 lists rhodamine dyes such as rhodamine-B base as examples of colorants for toners. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 07-150098 [Patent Document 2] JP 2018-106145 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, when an image is formed using a toner that uses a rhodamine dye, the reproducibility of thin lines may decrease under certain conditions. Therefore, an object of the present disclosure is to provide a toner for developing electrostatic images, an electrostatic image developer, a process cartridge, an image forming apparatus, and an image forming method, which are capable of suppressing a decrease in fine line reproducibility. [Means for solving the problem]

[0008] Means for solving the above problems include the following aspects. <1> A toner for developing electrostatic images, comprising toner particles containing a binder resin, a rhodamine dye, and a hindered amine compound. <2> The binder resin includes a polyester resin. <1> 2. The toner for developing electrostatic images according to claim 1 . <3> the content of the hindered amine compound relative to the rhodamine dye is 0.1% by mass or more and 200% by mass or less; <1> or <2> 2. The toner for developing electrostatic images according to claim 1 . <4> the total content of the rhodamine dye and the hindered amine compound relative to the toner particles is 0.1% by mass or more and 5% by mass or less; <1> ~ <3> 10. The toner for developing an electrostatic image according to claim 9, <5> The rhodamine dye contains a compound represented by the following general formula (R1): <1> ~ <4> 10. The toner for developing an electrostatic image according to claim 9, [ka] (In general formula (R1), R r1 ~R r7 each independently represents a hydrogen atom, an alkyl group, or an aromatic group; X - represents a counter anion.) <6> The hindered amine compound includes a structure represented by the following general formula (H1): <1> ~ <5> 10. The toner for developing an electrostatic image according to claim 9, [ka] (In general formula (H1), R H1 represents a hydrogen atom, an oxygen atom, an alkyl group, or an alkoxy group; R H2 ~R H6 and R H8 ~R H11 Each independently represents a hydrogen atom or an alkyl group. H2 and R H3 And, R H4 and R H5 And, R H8 and R H9 And, R H10 and R H11At least two combinations of indicate an alkyl group. * indicates the bonding position.) <7> The hindered amine compound contains two or more structures represented by the general formula (H1). <6> 2. The toner for developing electrostatic images according to claim 1 . <8> <1> ~ <7> 2. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1. <9> <1> ~ <7> 13. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 12 and is detachably mountable to an image forming apparatus. <10> <8> and a developing means for developing an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus. <11> An image carrier; A charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; <8> a developing means for developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; A fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <12> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; <8> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 1; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1, Effect of the Invention

[0009] According to the present disclosure, it is possible to provide an electrostatic image developing toner, an electrostatic image developer, a process cartridge, an image forming apparatus, and an image forming method, which are capable of suppressing deterioration in fine line reproducibility. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge that is detachably mounted to the image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment that is an example of the present disclosure will be described. These descriptions and examples are intended to illustrate the embodiment, and are not intended to limit the scope of the embodiment. In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the present disclosure, in which numerical ranges are described in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In the numerical ranges described in the present disclosure, the upper or lower limit of the numerical range may be replaced with values ​​shown in the examples. In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. When an embodiment of the present disclosure is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. In addition, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this. In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified. In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In the present disclosure, "(meth)acrylic" is an expression that includes both acrylic and methacrylic, and "(meth)acrylate" is an expression that includes both acrylate and methacrylate. In this disclosure, "toner for developing electrostatic images" is also referred to as "toner", "electrostatic image developer" is also referred to as "developer", and "carrier for developing electrostatic images" is also referred to as "carrier".

[0012] <Toner for developing electrostatic images> The toner according to the present embodiment has toner particles that contain a binder resin, a rhodamine dye, and a hindered amine compound.

[0013] The toner according to the present embodiment, due to the above-described composition, suppresses the deterioration of thin line reproducibility.

[0014] Conventionally, when an image is formed using a toner that uses a rhodamine dye as in the above Patent Documents 1 and 2, fine line reproducibility may be reduced. The rhodamine dye undergoes partial aggregation of the rhodamine skeleton, resulting in a state in which electron transfer between molecules is likely to occur. When a voltage is applied to the toner in this state by transfer or the like, electron transfer between the rhodamine dye molecules occurs inside the toner, resulting in non-uniform charging of the toner. This results in poor transfer of the toner image, scattering of the toner, and the like, resulting in reduced fine line reproducibility. In particular, when a toner image in which multiple color toners are superimposed or a high-density toner image is transferred, a high voltage is applied to the toner during transfer, causing the above phenomenon to occur and easily deteriorating thin line reproducibility.

[0015] On the other hand, when a hindered amine compound is used in combination with a rhodamine dye, the formation of an association of the rhodamine skeleton in the rhodamine dye is suppressed. It is presumed that the hindered amine compound acts electrostatically on the rhodamine dye. As a result, even if a voltage is applied to the toner during transfer or the like, the chargeability of the toner is less likely to decrease, and transfer failure of the toner image, scattering of the toner, and the like are less likely to occur.

[0016] For the above reasons, the toner according to this embodiment suppresses the deterioration of thin line reproducibility.

[0017] The toner according to this embodiment will be described in detail below.

[0018] The toner according to the exemplary embodiment includes toner particles. The toner may include an external additive, if necessary.

[0019] (Toner particles) The toner particles contain a binder resin, a rhodamine dye, and a hindered amine compound. The toner particles may contain a colorant other than the rhodamine dye, a release agent, and other additives.

[0020] -Rhodamine dye- Rhodamine dyes are compounds having a rhodamine skeleton obtained by condensing aminophenols with phthalic anhydride. Specifically, rhodamine dyes are compounds having a rhodamine skeleton represented by the following formula (R0). In formula (R0), X - indicates a counter anion.

[0021] [ka]

[0022] Examples of rhodamine dyes include rhodamine B, rhodamine 6G, rhodamine 6G6GP, rhodamine 3GO, rhodamine 110, rhodamine 123, rhodamine 560, 6rhodamine 40, rhodamine 800, sulforhodamine B, octadecylrhodamine 101 ester, and rhodamine 19 perchlorate.

[0023] Among these, from the viewpoint of optical properties such as strong absorption and fluorescence, the rhodamine dye preferably contains a compound represented by the following general formula (R1).

[0024] [ka]

[0025] In general formula (R1), R r1 ~R r7 each independently represents a hydrogen atom, an alkyl group, or an aromatic group; X - represents a counter anion.

[0026] R r1 ~R r7 The alkyl group represented by the formula (I) is preferably a straight-chain, branched-chain, or cyclic alkyl group having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a t-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, a dodecyl group, a hexadecyl group, a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a 1-norbornyl group, and a 1-adamantyl group. The aromatic group is preferably an aryl group having a carbon number of 6 to 48, more preferably a carbon number of 6 to 24. Specific examples of the aromatic group include a phenyl group and a naphthyl group.

[0027] R r1 ~R r7When the group represented by is a group that can be further substituted, it may be further substituted with any of the above-mentioned groups. When it has two or more substituents, the substituents may be the same or different.

[0028] X - Examples of the counter anion include a chlorine ion, a bromine ion, an iodine ion, a perchlorate ion, a PF6 ion, a BF4 ion, and an acetate ion. The counter anion is preferably a chlorine ion.

[0029] Specific examples of rhodamine dyes are shown below. In the specific examples, Et represents an ethyl group. 11 represents a cyclohexyl group. Ph represents a phenyl group.

[0030] [ka]

[0031] The rhodamine dyes may be used alone or in combination.

[0032] --Hindered amine compounds-- The hindered amine compound is a compound having a hindered amine structure. Examples of hindered amine compounds are described in "Comprehensive Technology for Polymer Stabilization - Mechanism and Application Development" edited by Yasukazu Ohkatsu, published by CMC. Commercially available hindered amine compounds include Sanol LS-770, Sanol LS-765, and Sanol LS-2626 (all manufactured by Sankyosha), Adeka STAB LA-77, LA-57, LA-52, LA-62, LA-63, LA-67, LA-68, and LA-72 (all manufactured by ADEKA), TINUVIN 123, TINUVIN 144, TINUVIN 622, TINUVIN 765, and TINUVIN 944 (all manufactured by BASF).

[0033] From the viewpoint of suppressing deterioration in fine-line reproducibility, the hindered amine compound preferably contains a structure represented by the following general formula (H1), more preferably contains two or more structures represented by the following general formula (H1), and further preferably contains two or more and three or less structures represented by the following general formula (H1).

[0034] [ka] In general formula (H1), R H1 represents a hydrogen atom, an oxygen atom, an alkyl group, or an alkoxy group; R H2 ~R H6 and R H8 ~R H11 Each independently represents a hydrogen atom or an alkyl group. H2 and R H3 And, R H4 and R H5 And, R H8 and R H9 And, R H10 and R H11 At least two combinations of indicate an alkyl group. * indicates the position of attachment.

[0035] In general formula (H1), R H1 The alkyl group represented by the formula (I) may be a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms. R H1 The alkoxy group represented by the formula (I) includes a substituted or unsubstituted alkoxy group having 1 to 30 carbon atoms.

[0036] R H2 ~R H6 and R H8 ~R H11 The alkyl group represented by the formula (I) may be a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms.

[0037] From the viewpoint of suppressing deterioration in fine-line reproducibility, the hindered amine compound is preferably a compound represented by the following general formulas (H1-A) to (H1-G), and more preferably a compound represented by the following general formula (H1-A).

[0038] [ka]

[0039] [ka]

[0040] In general formulas (H1-A) to (H1-G), R 21 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms (preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms, even more preferably 1 to 3 carbon atoms, and still more preferably 1 or 2 carbon atoms), or -OR 8 R 8 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms (preferably 1 to 12 carbon atoms). R 22 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms (preferably having 1 to 12 carbon atoms, more preferably having 1 to 8 carbon atoms, and even more preferably having 1 to 6 carbon atoms). L 21 represents a single bond, an alkylene group having 1 to 20 carbon atoms (preferably 1 to 10 carbon atoms), or an arylene group having 6 to 20 carbon atoms (preferably 6 to 10 carbon atoms). X 21 and X 22 each independently represents an oxygen atom or -NH-. n represents an integer of 1 to 20 (preferably 1 to 10).

[0041] The hindered amine compounds may be used alone or in combination.

[0042] -Rhodamine dye and hindered amine compound content- The content of the hindered amine compound relative to the rhodamine dye is preferably from 0.08% by mass to 210% by mass, more preferably from 0.1% by mass to 200% by mass, and even more preferably from 50% by mass to 150% by mass. From the viewpoints of increasing the uniformity of the chargeability of the toner and further suppressing a decrease in fine line reproducibility, the content of the hindered amine compound is preferably 0.08% by mass or more (particularly 0.1% by mass or more). On the other hand, from the viewpoint of suppressing decomposition of the hindered amine compound itself and improving fine line reproducibility, the content of the hindered amine compound is preferably 210% by mass or less (particularly 200% by mass).

[0043] The total content of the rhodamine dye and the hindered amine compound in the toner particles is preferably from 0.08% by mass to 6% by mass, more preferably from 0.1% by mass to 5% by mass, and even more preferably from 0.5% by mass to 2% by mass. From the viewpoint of preventing a decrease in fine-line reproducibility while still exhibiting the color of the rhodamine dye, the total content of the rhodamine dye and the hindered amine compound is preferably 0.08% by mass or more (particularly 0.1% by mass or more). On the other hand, from the viewpoint of suppressing deterioration in the color of the rhodamine dye due to aggregation of the rhodamine dye and the hindered amine compound, while also suppressing deterioration in fine-line reproducibility, the total content of the rhodamine dye and the hindered amine compound is preferably 6 mass % or less (particularly 5 mass % or less).

[0044] The contents of the rhodamine dye and the hindered amine compound can be measured, for example, by quantitative determination using LC-MS (liquid chromatography-mass spectrometry).

[0045] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers.

[0046] Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.

[0047] The binder resin preferably contains a polyester resin. Examples of the polyester resin include known polyester resins. The polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. As the polyester resin, a commercially available product or a synthesized product may be used. Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. As the polyvalent carboxylic acid, a trivalent or higher carboxylic acid having a crosslinked or branched structure may be used in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0048] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a trihydric or higher polyhydric alcohol having a crosslinked or branched structure may be used in combination with the diol. Examples of the trihydric or higher polyhydric alcohol include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0049] The glass transition temperature (Tg) of the polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), and more specifically, is determined from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."

[0050] The weight average molecular weight (Mw) of the polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less.

[0051] The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.

[0052] The polyester resin can be obtained by a known production method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a dissolution aid to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the dissolution aid. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility be condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.

[0053] The content of the binder resin is preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the toner particles.

[0054] -Colorants other than rhodamine dyes- Colorants other than rhodamine dyes include color pigments. The color pigment may be any color pigment other than rhodamine dyes, and any known color pigment may be used. Specific examples of color pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 21, 22, 23, 31, 32, 38, 41, 48, 48:1, 48:2, 48:3, 48:4, 49, 52, 53:1, 54, 57:1, 58, 60:1, 63, 64:1, 68, 81:1, 81:4, 83, 88, 89, 112, 1 14, 122, 123, 144, 146, 149, 150, 166, 170, 176, 177, 178, 179, 184, 185, 187, 202, 206, 207, 208, 209, 210, 213, 220, 221, 238, 242, 245, 253, 254, 255, 256, 258, 264, 266, 269, 282, etc., CIPigment Examples of pigments include CI Pigment Violet 19, 23, 32, CI Pigment Orange 13, 16, 38, 43, 62, CI Pigment Yellow 3, 12, 17, 74, 101, 139, 150, 155, 180, 185, and various other pigments. The colorant may be used alone or in combination of two or more kinds.

[0055] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.

[0056] The content of the colorant is preferably from 0.005% by mass to 10% by mass with respect to the toner particles, from the viewpoint of fluorescence intensity.

[0057] --Release agent-- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these. The release agent is preferably a hydrocarbon wax, more preferably paraffin wax or polyethylene wax.

[0058] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."

[0059] The content of the release agent is preferably from 1% by mass to 20% by mass, more preferably from 2% by mass to 20% by mass, and even more preferably from 3% by mass to 15% by mass, based on the toner particles.

[0060] --Other additives-- Examples of other additives include known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.

[0061] -Characteristics of toner particles- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion. The toner particles having a core-shell structure may be composed of a core containing, for example, a binder resin, a rhodamine dye, and a hindered amine compound, and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing a binder resin.

[0062] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 10 μm, and more preferably from 4 μm to 8 μm. The volume average particle size (D50v) of the toner particles is measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5 mass % aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative total is defined as the volume particle size D16v, the number particle size D16p, and the particle size at 50% of the cumulative total as the volume average particle size D50v.

[0063] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.

[0064] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.

[0065] (External additives) Examples of the external additive include inorganic particles. Examples of inorganic particles include SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, and K2O·(TiO2). n , Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, MgSO4, etc.

[0066] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the inorganic particles.

[0067] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate, and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles), and the like.

[0068] The amount of the external additive is preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.

[0069] (Toner manufacturing method) Next, a method for producing the toner according to the present embodiment will be described. The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles. The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). There is no particular limitation on these production methods, and any known production method may be used. Among these, it is preferable to obtain the toner particles by the aggregation and coalescence method. Examples of the aggregation and coalescence method include the methods described in JP-A-2010-97101 and JP-A-2006-154641. An example of the kneading and pulverizing method is the method described in JP-A-2000-267338. An example of the dissolution suspension method is the method described in JP-A-2000-258950.

[0070] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, the toner particles are produced through a step of preparing a resin particle dispersion in which resin particles to be a binder resin are dispersed (resin particle dispersion preparation step), a step of aggregating resin particles (other particles, if necessary) in the resin particle dispersion (in a dispersion after mixing other particle dispersions, if necessary) to form aggregated particles (aggregated particle formation step), and a step of heating the aggregated particle dispersion in which the aggregated particles are dispersed, to fuse and coalesce the aggregated particles, thereby forming toner particles (fusion and coalescence step).

[0071] Here, for example, by using a resin particle dispersion in which resin particles containing a rhodamine dye and a hindered amine compound are dispersed as part of the above-mentioned resin particle dispersion, toner particles containing a binder resin, a rhodamine dye, and a hindered amine compound can be obtained.

[0072] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant other than a rhodamine dye (hereinafter simply referred to as a "colorant") and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may also be used.

[0073] -Resin particle dispersion preparation process- First, a resin particle dispersion in which resin particles serving as a binder resin are dispersed, as well as a colorant particle dispersion in which colorant particles are dispersed and a release agent particle dispersion in which release agent particles are dispersed are prepared.

[0074] Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.

[0075] The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.

[0076] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.

[0077] In the resin particle dispersion, examples of the method for dispersing the resin particles in the dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.

[0078] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is measured by using a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel), and measuring the particle size at which the cumulative distribution is 50% of all particles as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.

[0079] The content of the resin particles in the resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.

[0080] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.

[0081] -Agglomerated particle formation process- Next, the colorant particle dispersion and the release agent particle dispersion are mixed together with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.

[0082] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.

[0083] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.

[0084] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, for example, oxycarboxylic acid such as tartaric acid, citric acid, gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.

[0085] -Fusion / unification process- Next, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles.

[0086] Through the above steps, toner particles are obtained. Note that, after obtaining an aggregated particle dispersion liquid in which aggregated particles are dispersed, the toner particles may be manufactured through a process of further mixing the aggregated particle dispersion liquid with a resin particle dispersion liquid in which resin particles are dispersed, and aggregating the aggregated particles so that the resin particles are further attached to the surfaces of the aggregated particles to form second aggregated particles, and a process of heating the second aggregated particle dispersion liquid in which the second aggregated particles are dispersed to fuse and coalesce the second aggregated particles to form toner particles having a core / shell structure.

[0087] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.

[0088] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.

[0089] <Electrostatic image developer> The electrostatic image developer according to this embodiment contains at least the toner according to this embodiment. The electrostatic image developer according to the present embodiment may be a one-component developer containing only the toner according to the present embodiment, or may be a two-component developer in which the toner is mixed with a carrier.

[0090] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.

[0091] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.

[0092] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin. The coating resin and the matrix resin may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.

[0093] Here, in order to coat the surface of the core material with a coating resin, a method of coating with a coating layer forming solution in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent can be mentioned. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.

[0094] In the two-component developer, the mixture ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.

[0095] <Image forming device / image forming method> An image forming apparatus and an image forming method according to the present embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.

[0096] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.

[0097] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of the image holder after the transfer of the toner image and before charging; and an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge it after the transfer of the toner image and before charging it.

[0098] When the image forming apparatus according to the present embodiment is an intermediate transfer type apparatus, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.

[0099] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge that contains the electrostatic charge image developer according to the present embodiment and has the developing means is preferably used.

[0100] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this example. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted. In the following description, a six-tandem image forming apparatus having six image forming units arranged will be described as an example of the image forming apparatus according to the present embodiment. The tandem image forming apparatus is not limited to this, and may be a five-tandem image forming apparatus having five image forming units arranged, a four-tandem image forming apparatus having four image forming units arranged, or the like.

[0101] 1 is a schematic diagram showing an image forming apparatus according to the present embodiment, which is a 6-tandem type intermediate transfer type image forming apparatus. The pink toner is an example of the toner according to the present embodiment (i.e., a toner having toner particles containing a binder resin, a rhodamine dye, and a hindered amine compound).

[0102] The image forming apparatus shown in Fig. 1 includes first to sixth image forming units 10P, 10Y, 10M, 10C, 10K, and 10G, which are electrophotographic image forming means that output images of each color, pink (P), yellow (Y), magenta (M), cyan (C), and black (K), based on color-separated image data. These image forming units (hereinafter, sometimes simply referred to as "units") 10P, 10Y, 10M, 10C, 10K, and 10G are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10P, 10Y, 10M, 10C, 10K, and 10G may be process cartridges that are detachably attached to the image forming apparatus. An intermediate transfer belt (an example of an intermediate transfer body) 20 is provided below each of the units 10P, 10Y, 10M, 10C, 10K, and 10G and extends through each of the units. The intermediate transfer belt 20 is provided wrapped around a drive roll 22, a support roll 23, and an opposing roll 24 that contact the inner surface of the intermediate transfer belt 20, and runs in a direction from the first unit 10P to the sixth unit 10G. An intermediate transfer body cleaning device 21 is provided on the image bearing surface side of the intermediate transfer belt 20, facing the drive roll 22.

[0103] The developing devices (examples of developing means) 4P, 4Y, 4M, 4C, 4K, 4G of each unit 10P, 10Y, 10M, 10C, 10K, 10G are supplied with pink, yellow, magenta, cyan, black, and green toner contained in toner cartridges 8P, 8Y, 8M, 8C, 8K, 4G, respectively.

[0104] Since the first to sixth units 10P, 10Y, 10M, 10C, 10K, and 10G have the same configuration and operation, the first unit 10P that forms a pink image will be described here as a representative.

[0105] The sixth unit 10P has a photoconductor 1P that acts as an image carrier. Around the photoconductor 1P, there are sequentially arranged a charging roll (an example of a charging means) 2P that charges the surface of the photoconductor 1P to a predetermined potential, an exposure device (an example of an electrostatic image forming means) 3P that exposes the charged surface to a laser beam based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing means) 4P that supplies toner to the electrostatic image to develop it, a primary transfer roll (an example of a primary transfer means) 5P that transfers the developed toner image onto the intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning means) 6P that removes the toner remaining on the surface of the photoconductor 1P after the primary transfer.

[0106] The primary transfer roll 5P is disposed inside the intermediate transfer belt 20, and is provided at a position facing the photoconductor 1P. A bias power supply (not shown) that applies a primary transfer bias is connected to the primary transfer rolls 5P, 5Y, 5M, 5C, 5K, and 5G of each unit. Each bias power supply changes the value of the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).

[0107] Hereinafter, an operation of forming a pink image in sixth unit 10P will be described. First, prior to operation, the surface of the photoconductor 1P is charged to a potential of -600V to -800V by the charging roll 2P.

[0108] The photoconductor 1P has a conductivity (for example, a volume resistivity of 1×10 at 20°C). -6 It is formed by laminating a photosensitive layer on a substrate with a resistivity of Ωcm or less. This photosensitive layer is normally highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam, the resistivity of the portion irradiated with the laser beam changes. Therefore, a laser beam is irradiated from exposure device 3P onto the charged surface of photoconductor 1P in accordance with pink image data sent from a control unit (not shown). As a result, an electrostatic charge image of a pink image pattern is formed on the surface of photoconductor 1P. An electrostatic image is an image formed on the surface of the photoconductor 1P by electrostatic charging. The laser beam from the exposure device 3P reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1P to flow, while the charges remain in the parts not irradiated by the laser beam. This is a so-called negative latent image.

[0109] The electrostatic image formed on the photoconductor 1P rotates to a predetermined development position as the photoconductor 1P travels. At this development position, the electrostatic image on the photoconductor 1P is developed into a toner image by the developing device 4P and made visible.

[0110] The developing device 4P contains an electrostatic image developer including at least pink toner and a carrier. The pink toner is triboelectrically charged by being stirred inside the developing device 4P, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1P. As the surface of the photoconductor 1P passes through the developing device 4P, the pink toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1P, and the latent image is developed with the pink toner. The photoconductor 1P on which the pink toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1P is transported to a predetermined primary transfer position.

[0111] When the pink toner image on the photoconductor 1P is transported to the primary transfer position, a primary transfer bias is applied to the primary transfer roll 5P, and an electrostatic force from the photoconductor 1P to the primary transfer roll 5P acts on the toner image, causing the toner image on the photoconductor 1P to be transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and is controlled by a control unit (not shown) in the first unit 10P to be, for example, +10 μA.

[0112] After the toner image is transferred to the intermediate transfer belt 20, the photoreceptor 1P continues to rotate and comes into contact with a cleaning blade provided in the photoreceptor cleaning device 6P. The toner remaining on the photoreceptor 1P is removed and collected by the photoreceptor cleaning device 6P.

[0113] The intermediate transfer belt 20 is conveyed through the first to sixth image forming units 10P, 10Y, 10M, 10C, 10K, and 10G in order, and the toner images of the respective colors are transferred and superimposed on each other. The intermediate transfer belt 20 onto which the six color toner images have been transferred in multiple layers through the first to sixth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, an opposing roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the opposing roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, and the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.

[0114] After the toner image is transferred to the recording paper P, the intermediate transfer belt 20 continues to run and comes into contact with a cleaning blade provided in the intermediate transfer body cleaning device 21. The toner remaining on the intermediate transfer belt 20 is removed and collected by the intermediate transfer body cleaning device 21. The recording paper P to which the toner image has been transferred is fed into the pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P to form a fixed image.

[0115] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets and the like.

[0116] To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with a resin or the like, art paper for printing, etc. are preferably used. After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.

[0117] <Process cartridge / toner cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus. The process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing means and, as necessary, at least one other means selected from an image carrier, a charging means, an electrostatic image forming means, and a transfer means.

[0118] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted. FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally combining and holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are assembled into a cartridge. In FIG. 2, 109 denotes an exposure device (an example of an electrostatic image forming means), 112 denotes a transfer device (an example of a transfer means), 115 denotes a fixing device (an example of a fixing means), and 300 denotes a recording paper (an example of a recording medium).

[0119] Next, the toner cartridge according to this embodiment will be described. The toner cartridge according to the present embodiment is a toner cartridge that contains the electrostatic image developing toner according to the present embodiment and is detachably attached to an image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing unit provided in the image forming apparatus. The image forming apparatus shown in FIG. 1 is an image forming apparatus having a configuration in which toner cartridges 8Y, 8P, 8M, 8C, 8K, and 8G are detachably attached, and the developing devices 4Y, 4P, 4M, 4C, 4K, and 4G are connected to toner cartridges corresponding to the respective colors by toner supply pipes (not shown). When the toner contained in the toner cartridge becomes low, the toner cartridge is replaced. An example of the toner cartridge according to this embodiment is the toner cartridge 8P, which contains the electrostatic image developing toner according to this embodiment. The toner cartridges 8Y, 8M, 8C, 8K, and 8G contain yellow, magenta, cyan, black, and green toners, respectively. EXAMPLES

[0120] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the following examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.

[0121] <Preparation of polyester resin (1)> Terephthalic acid: 30 parts by mole Fumaric acid: 70 parts by mole Bisphenol A ethylene oxide adduct: 5 mole parts Bisphenol A propylene oxide adduct: 95 parts by mole The above materials were charged into a flask equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour, and 1 part of titanium tetraethoxide was added per 100 parts of the above materials. The temperature was raised to 230°C over 30 minutes while distilling off the generated water, and the dehydration condensation reaction was continued at that temperature for 1 hour, after which the reaction product was cooled. In this way, a polyester resin (1) having a weight average molecular weight of 18,000 and a glass transition temperature of 60° C. was obtained.

[0122] <Preparation of fluorescent colorant particle dispersion (1)> Rhodamine dye (Rhodamine B): 3 parts Hindered amine compound (AT-1): 3 parts Polyester resin (1): 94 parts In a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of the above material were gradually added and dissolved. A 10% by mass aqueous ammonia solution (equivalent to three times the amount by molar ratio of the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was dropped at a rate of 2 parts / min while stirring the mixed liquid. After the dropping was completed, the temperature was returned to room temperature (20°C to 25°C), and bubbling with dry nitrogen was performed for 48 hours while stirring to obtain a resin particle dispersion liquid in which ethyl acetate and 2-butanol were reduced to 1,000 ppm or less. Ion-exchanged water was added to the resin particle dispersion liquid to adjust the solid content to 20% by mass, and a fluorescent colorant particle dispersion liquid (1) was obtained.

[0123] <Preparation of fluorescent colorant particle dispersions (2) to (5)> Fluorescent colorant particle dispersion liquids (2) to (5) were obtained in the same manner as in preparation of fluorescent colorant particle dispersion liquid (1), except that the hindered amine compounds (AT-2) to (AT-4) and (HT-1) were used instead of the hindered amine compound (AT-1) in preparation of fluorescent colorant particle dispersion liquid (1).

[0124] <Preparation of fluorescent colorant particle dispersion (6)> Fluorescent colorant particle dispersion liquid (6) was obtained in the same manner as in preparation of fluorescent colorant particle dispersion liquid (1), except that the hindered amine compound was not added and the number of parts of polyester resin (1) was changed to 96 parts.

[0125] <Preparation of fluorescent colorant particle dispersion (7)> Fluorescent colorant particle dispersion liquid (7) was obtained in the same manner as in preparation of fluorescent colorant particle dispersion liquid (1), except that 6 parts of the rhodamine dye (rhodamine B), 0.0048 parts of the hindered amine compound (AT-1), and 94 parts of the polyester resin (1) were used.

[0126] <Preparation of fluorescent colorant particle dispersion (8)> Fluorescent colorant particle dispersion liquid (8) was obtained in the same manner as in preparation of fluorescent colorant particle dispersion liquid (1), except that 6 parts of the rhodamine dye (rhodamine B), 0.0072 parts of the hindered amine compound (AT-1), and 94 parts of the polyester resin (1) were used.

[0127] <Preparation of fluorescent colorant particle dispersion (9)> Fluorescent colorant particle dispersion liquid (9) was obtained in the same manner as in preparation of fluorescent colorant particle dispersion liquid (1), except that 2.1 parts of the rhodamine dye (rhodamine B), 3.9 parts of the hindered amine compound (AT-1), and 94 parts of the polyester resin (1) were used.

[0128] <Preparation of fluorescent colorant particle dispersion (10)> A fluorescent colorant particle dispersion liquid (10) was obtained in the same manner as in the preparation of the fluorescent colorant particle dispersion liquid (1), except that 1.9 parts of the rhodamine dye (rhodamine B), 4.1 parts of the hindered amine compound (AT-1), and 94 parts of the polyester resin (1) were used.

[0129] <Preparation of fluorescent colorant particle dispersion (11)> Fluorescent colorant particle dispersion liquid (11) was obtained in the same manner as in preparation of fluorescent colorant particle dispersion liquid (1), except that 0.24 parts of the rhodamine dye (rhodamine B), 0.24 parts of the hindered amine compound (AT-1), and 99.53 parts of the polyester resin (1) were used.

[0130] <Preparation of fluorescent colorant particle dispersion (12)> A fluorescent colorant particle dispersion liquid (12) was obtained in the same manner as in the preparation of the fluorescent colorant particle dispersion liquid (1), except that 0.36 parts of the rhodamine dye (rhodamine B), 0.36 parts of the hindered amine compound (AT-1), and 99.29 parts of the polyester resin (1) were used.

[0131] <Preparation of fluorescent colorant particle dispersion (13)> A fluorescent colorant particle dispersion liquid (13) was obtained in the same manner as in the preparation of the fluorescent colorant particle dispersion liquid (1), except that 11.8 parts of the rhodamine dye (rhodamine B), 11.8 parts of the hindered amine compound (AT-1), and 76.33 parts of the polyester resin (1) were used.

[0132] <Preparation of fluorescent colorant particle dispersion (14)> A fluorescent colorant particle dispersion liquid (14) was obtained in the same manner as in the preparation of the fluorescent colorant particle dispersion liquid (1), except that 17.8 parts of the rhodamine dye (rhodamine B), 17.8 parts of the hindered amine compound (AT-1), and 64.50 parts of the polyester resin (1) were used.

[0133] [ka]

[0134] <Preparation of Color Pigment Particle Dispersion (1)> Color pigment (CI Pigment Violet 19): 70 parts Anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 30 parts -Ion-exchanged water: 200 parts The above materials were mixed and dispersed for 10 minutes using a homogenizer (Ultra Turrax T50 manufactured by IKA Corporation). Ion-exchanged water was added so that the solid content in the dispersion was 20% by mass, and a colorant particle dispersion (1) in which colorant particles having a volume average particle size of 140 nm were dispersed was obtained.

[0135] <Preparation of Polyester Resin Particle Dispersion (1)> In a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of polyester resin (1) were gradually added and dissolved, and a 10% by mass aqueous ammonia solution (equivalent to 3 times the amount by molar ratio relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was dropped at a rate of 2 parts / min while stirring the mixed liquid. After the dropping was completed, the temperature was returned to room temperature (20°C to 25°C), and bubbling with dry nitrogen was performed for 48 hours while stirring to obtain a resin particle dispersion in which ethyl acetate and 2-butanol were reduced to 1,000 ppm or less. Ion-exchanged water was added to the resin particle dispersion to adjust the solid content to 20% by mass, and a polyester resin particle dispersion (1) was obtained.

[0136] <Preparation of Release Agent Particle Dispersion (1)> Paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd.): 100 parts Anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA, product name Ultra Turrax T50), and then dispersed using a Manton-Gaulin high-pressure homogenizer (Gaulin), to obtain a release agent particle dispersion (1) (solid content 20% by mass) in which release agent particles having a volume average particle size of 200 nm were dispersed.

[0137] <Example 1> (Preparation of toner particles (1)) Polyester resin particle dispersion (1): 60.8 parts Fluorescent colorant particle dispersion (1): 20 parts Color pigment particle dispersion (1): 0.9 parts Release agent particle dispersion (1): 6 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd.: Neogen RK, solid content: 20%): 1 part The above materials were placed in a round stainless steel flask, and 0.1N (=mol / L) nitric acid was added to adjust the pH to 3.5, and then 30 parts of a nitric acid aqueous solution with a polyaluminum chloride concentration of 10% by mass was added. Next, the mixture was dispersed at a liquid temperature of 30°C using a homogenizer (IKA, product name Ultra Turrax T50), and then heated to 45°C in a heating oil bath and held for 30 minutes. Then, 30.4 parts of polyester resin particle dispersion (1) was added and held for 1 hour, and 0.1N sodium hydroxide aqueous solution was added to adjust the pH to 8.5, and then heated to 84°C and held for 2.5 hours. Next, the mixture was cooled to 20°C at a rate of 20°C / min, and the solid content was filtered off, thoroughly washed with ion-exchanged water, and dried to obtain toner particles (1). The volume average particle size of the toner particles (1) was 7 μm.

[0138] (Preparation of Toner (1)) 100 parts of the obtained toner particles (1) were mixed and blended with 1.5 parts of hydrophobic silica (manufactured by Nippon Aerosil Co., Ltd., RY50) and 1.0 part of hydrophobic titanium oxide (manufactured by Nippon Aerosil Co., Ltd., T805) using a sample mill at 10,000 rpm (revolutions per minute) for 30 seconds. The mixture was then sieved using a vibrating sieve with a mesh size of 45 μm to prepare toner (1) (toner for developing electrostatic images). The volume average particle size of the obtained toner (1) was 7 μm.

[0139] (Preparation of Carrier (1)) Ferrite particles (average particle size 35 μm): 100 parts Toluene: 14 parts Polymethyl methacrylate (MMA, weight average molecular weight 75,000): 5 parts Carbon black (VXC-72, manufactured by Cabot Corporation, volume resistivity: 100 Ω cm or less): 0.2 parts The above materials except for the ferrite particles were dispersed in a sand mill to prepare a dispersion liquid, and this dispersion liquid was placed in a vacuum degassing kneader together with the ferrite particles, and the mixture was dried under reduced pressure while stirring to obtain a carrier (1).

[0140] (Preparation of electrostatic image developer) 8 parts of the toner (1) and 92 parts of the carrier were mixed in a V blender to prepare a developer (1) (electrostatic image developer).

[0141] <Examples 2 to 4, Comparative Examples 1 and 2> Toner particles (2) to (6) were obtained in the same manner as in the preparation of toner particles (1), except that fluorescent colorant particle dispersions (2) to (6) were used instead of the fluorescent colorant particle dispersion (1) in the preparation of toner particles (1). Developers (2) to (6) were then prepared in the same manner as in Example 1 using the obtained toner particles (2) to (6).

[0142] <Example 5: Kneading and grinding method> (Preparation of toner particles) Polyester resin (1): 94 parts Rhodamine dye (Rhodamine B): 0.5 parts Hindered amine compound (AT-1): 0.5 parts Color pigment (CI Pigment Violet 19): 0.8 parts Paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd.): 5.1 parts Copolymerized petroleum resin (A) (C5 petroleum fraction (isoprene) / C5 petroleum fraction (piperylene) / isopropenyl toluene = monomer mass ratio (1.5 / 1.5 / 97), softening point: 125°C): 5 parts The above mixture was kneaded in an extruder and pulverized in a surface pulverizer, after which fine particles and coarse particles were classified in an air classifier to obtain toner particles (7) having a volume average particle size D50 of 8.0 μm.

[0143] (Toner Production) Toner (7) (external additive toner) was prepared by adding 1.0 part of negatively chargeable silica having an average particle size of 40 nm and 0.5 part of negatively chargeable titania having an average particle size of 15 nm to 100 parts of the obtained toner particles (7).

[0144] (Preparation of electrostatic image developer) Next, 100 parts of a carrier made of ferrite with a particle size of 50 μm coated with a styrene-methacrylate copolymer was added to 6 parts of the toner (7) and mixed to produce a developer (7) (electrostatic image developer).

[0145] <Example 6: Styrene acrylic resin / aggregation method> (Preparation of styrene acrylic resin particle dispersion (1)) Styrene: 308 parts n-Butyl acrylate: 100 parts Acrylic acid: 4 parts Dodecanethiol: 6 parts Propanediol diacrylate: 1.5 parts The above components were mixed and dissolved, and the mixture was added to an aqueous solution of 4 parts of anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.: Neogen SC) dissolved in 550 parts of ion-exchanged water to emulsify in a flask, and then, while mixing for 10 minutes, an aqueous solution of 6 parts of ammonium persulfate dissolved in 100 parts of ion-exchanged water was added to the mixture, and nitrogen substitution was performed. The contents were heated in an oil bath while stirring the flask until the contents reached 75°C, and emulsion polymerization was continued for 5 hours. In this way, a styrene-acrylic resin particle dispersion (1) (resin particle concentration: 20%) was obtained in which resin particles having an average particle size of 195 nm and a weight average molecular weight (Mw) of 34,000 were dispersed. The glass transition temperature of the styrene-acrylic resin was 52°C.

[0146] (Preparation of fluorescent colorant particle dispersion (SA1)) Styrene: 308 parts n-Butyl acrylate: 100 parts Acrylic acid: 4 parts Dodecanethiol: 6 parts Propanediol diacrylate: 1.5 parts Rhodamine dye (Rhodamine B) 13.4 parts Hindered amine compound (AT-1) 13.4 parts The above components were mixed and prepared in the same manner as in the styrene-acrylic resin particle dispersion (1), to obtain a fluorescent colorant particle dispersion (SA1) (particle concentration: 20%).

[0147] (Preparation of toner particles (8)) Styrene acrylic resin particle dispersion (1): 60.8 parts Fluorescent colorant particle dispersion (SA1): 20 parts Color pigment particle dispersion (1): 0.9 parts Release agent particle dispersion (1): 6 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd.: Neogen RK, 20%): 1 part The above materials were placed in a round stainless steel flask, and 0.1N (=mol / L) nitric acid was added to adjust the pH to 3.5, and then 30 parts of a nitric acid aqueous solution with a polyaluminum chloride concentration of 10% by mass was added. Next, the mixture was dispersed at a liquid temperature of 30°C using a homogenizer (IKA, product name Ultra Turrax T50), and then heated to 45°C in a heating oil bath and held for 30 minutes. Then, 30.4 parts of styrene acrylic resin particle dispersion (1) was added and held for 1 hour, and 0.1N sodium hydroxide aqueous solution was added to adjust the pH to 8.5, and then heated to 84°C and held for 2.5 hours. Next, the mixture was cooled to 20°C at a rate of 20°C / min, and the solid content was filtered off, thoroughly washed with ion-exchanged water, and dried to obtain toner particles (8). The volume average particle size of the toner particles (8) was 8 μm. Then, using the toner particles (8), a toner (8) and a developer (8) were prepared in the same manner as in Example 1.

[0148] <Examples 7 to 14> Toner particles (9) to (16) were obtained in the same manner as in the preparation of toner particles (1), except that fluorescent colorant particle dispersions (7) to (14) were used instead of the fluorescent colorant particle dispersion (1) in the preparation of toner particles (1). Using the obtained toner particles (9) to (16), developers (9) to (16) were prepared in the same manner as in Example 1.

[0149] <Evaluation method> -Evaluation of fine line reproducibility- As an image forming apparatus, a "Color 1000i Press" manufactured by FUJIFILM Business Innovation Co., Ltd. was prepared, and the developer obtained in each of the Examples and Comparative Examples was filled into the special color developing device. The image forming apparatus was left to stand for 12 hours in an environment of 30° C. and 90% RH, and then 100,000 sheets of a 1% print chart in a special color were formed on A4 paper in the same environment using the image forming apparatus after standing. The following images were formed initially (after printing 10 sheets), after printing 1,000 sheets, after printing 10,000 sheets, after printing 50,000 sheets, after printing 100,000 sheets, and after leaving the sheet for 72 hours after printing 100,000 sheets. A 1on1off image (an image in which 1-dot lines are arranged in parallel at 1-dot intervals) with a resolution of 2,400 dpi (dot per inch) was printed on a total of four layers (toner amount: 4.5 g / cm) of C toner, M toner, Y toner, and toner of this embodiment and comparative example, from the bottom. 2 ) were placed one on top of the other, and a 5 cm x 5 cm chart image perpendicular to the developing direction was formed at the upper left, center, and lower right of an A4 sheet of paper. The line spacing of each chart printed on the obtained sample was observed using a 100x magnifying glass with a scale to see if there were any areas that had become narrower due to toner scattering, or areas that had become wider due to thin lines becoming thinner. Based on the observation results and the line spacing of the observed areas, a grade was given according to the following criteria. The results are shown in Table 1.

[0150] -Evaluation criteria- G1: In all charts, there is no decrease in line spacing due to scattering or increase in line spacing due to thinning. G2: There is a decrease or increase in line spacing, but there is at least one chart with visible thin lines. G3: There is at least one chart where the spacing between thin lines cannot be determined or there are gaps in the thin lines. G4: There are two or more charts where the spacing between thin lines cannot be distinguished or thin lines are missing.

[0151] [Table 1]

[0152] From the above results, it is understood that the toner of this embodiment suppresses the deterioration of thin line reproducibility as compared with the toner of the comparative example. [Explanation of symbols]

[0153] 1P, 1Y, 1M, 1C, 1K, 1G Photoconductor (an example of an image carrier) 2P, 2Y, 2M, 2C, 2K, 2G Charging roll (an example of a charging means) 3P, 3Y, 3M, 3C, 3K, 3G exposure equipment (an example of electrostatic image forming means) 4P, 4Y, 4M, 4C, 4K, 4G developing device (an example of developing means) 5P, 5Y, 5M, 5C, 5K, 5G Primary transfer roll (an example of a primary transfer means) 6P, 6Y, 6M, 6C, 6K, 6G Photoconductor cleaning device (an example of a cleaning means) 8P, 8Y, 8M, 8C, 8K, 8G toner cartridges 10P, 10Y, 10M, 10C, 10K, 10G Image forming unit 20 Intermediate transfer belt (an example of an intermediate transfer body) 21 Intermediate transfer body cleaning device 22 Driving Roll 23 Support roll 24 Opposing Roll 26 Secondary transfer roll (an example of a secondary transfer means) 28 Fixing device (an example of a fixing means) P Recording paper (an example of a recording medium)

[0154] 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of a cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 117 Cabinet 118 Exposure Aperture 200 Process Cartridge 300 Recording paper (an example of a recording medium)

Claims

1. A toner for developing electrostatic images, comprising toner particles containing a binder resin, a rhodamine dye, and a hindered amine compound.

2. 2. The toner for developing electrostatic images according to claim 1, wherein the binder resin comprises a polyester resin.

3. 2. The toner for developing electrostatic images according to claim 1, wherein the content of the hindered amine compound relative to the rhodamine dye is from 0.1% by mass to 200% by mass.

4. 4. The toner for developing electrostatic images according to claim 3, wherein a total content of the rhodamine dye and the hindered amine compound is from 0.1% by mass to 5% by mass based on the toner particles.

5. 2. The toner for developing electrostatic images according to claim 1, wherein the rhodamine dye comprises a compound represented by the following general formula (R1): [Formula 1] In general formula (R1), R r1 ~R r7 each independently represents a hydrogen atom, an alkyl group, or an aromatic group; X - represents a counter anion.

6. The toner for developing electrostatic images according to claim 1 , wherein the hindered amine compound has a structure represented by the following general formula (H1): [chemical 2] In general formula (H1), R H1 represents a hydrogen atom, an oxygen atom, an alkyl group, or an alkoxy group; R H2 ~R H6 and R H8 ~R H11 Each independently represents a hydrogen atom or an alkyl group. H2 and R H3 And, R H4 and R H5 And, R H8 and R H9 And, R H10 and R H11At least two combinations of with indicate an alkyl group. * indicates the bonding position.

7. The toner for developing electrostatic images according to claim 6 , wherein the hindered amine compound contains two or more structures represented by general formula (H1).

8. 8. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1.

9. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 7 and is detachably mountable to an image forming apparatus.

10. a developing unit that contains the electrostatic image developer according to claim 8 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus.

11. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 8 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:

12. a charging step of charging a surface of an image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 8; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,

Citation Information

Patent Citations

  • Water-based fluorescent ink