Electrophotographic receptor, process cartridge, and electrophotographic device

By integrating a polymer with a specific structural unit in the undercoat layer, the electrophotographic photoreceptor addresses potential fluctuations, ensuring stable image quality during high-volume and high-speed printing.

JP2024152030APending Publication Date: 2024-10-25CANON KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023065930
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Conventional electrophotographic photoreceptors experience significant potential fluctuations during high-volume and high-speed printing, leading to deteriorated image quality due to insufficient electron transport ability and charge accumulation.

Method used

Incorporating a polymer with a specific structural unit into the undercoat layer, characterized by the presence of perylene imide and electron-withdrawing groups, to enhance electron mobility and prevent aggregation, thereby stabilizing the potential.

Benefits of technology

The solution effectively suppresses potential fluctuations, maintaining image quality and stability during repeated high-volume and high-speed printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152030000048
    Figure 2024152030000048
  • Figure 2024152030000049
    Figure 2024152030000049
  • Figure 2024152030000001
    Figure 2024152030000001
Patent Text Reader

Abstract

To provide an electrophotographic receptor capable of suppressing a potential variation.SOLUTION: An electrophotographic receptor includes a support, an undercoat layer, and a photosensitive layer in this order. The undercoat layer includes a polymer having a structural unit represented by the following formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, a process cartridge, and an electrophotographic apparatus. [Background technology]

[0002] In recent years, there has been a demand for electrophotographic apparatuses capable of forming higher quality images, and it is desirable to provide apparatuses which can output images with high stability in quality even when used repeatedly. In electrophotographic photoreceptors used in electrophotographic processes, a technique is known in which an undercoat layer containing an electron transport material is provided between the support and the photosensitive layer in order to suppress charge injection from the support side to the photosensitive layer side and to suppress the occurrence of image defects such as black spots. Patent Document 1 describes an electrophotographic photoreceptor having a photosensitive layer containing a copolymer of a structure having a carboxyl group and a structure having electron transport ability. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-198014 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been a demand for large-volume and high-speed printing in electrophotographic processes. According to studies by the present inventors, it has been found that in the electrophotographic photoreceptor described in Patent Document 1, when large-volume and high-speed printing are performed, the potential fluctuation may become large. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide an electrophotographic photoreceptor capable of suppressing potential fluctuations. [Means for solving the problem]

[0005] The above object can be achieved by the present invention, which is described below. That is, the electrophotographic photoreceptor according to the present invention is an electrophotographic photoreceptor having a support, an undercoat layer, and a photosensitive layer in this order, The undercoat layer is characterized in that it contains a polymer having a structural unit represented by the following formula (1). [ka] (In formula (1), R 11 ~R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, X represents a structure represented by the following formula (2), (3), (4) or (5). [ka] (In formula (2), R 21 ~R 28 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 2 represents a structure represented by the following formula (2-1), (2-2), (2-3), (2-4) or (2-5), [ka] In formula (2-2), R 61 and R 62 each independently represents a methyl group or a trifluoromethyl group. However, R 21 ~R 28 , R 61 and R 62 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. [ka] (In formula (3), R 31 ~R 38 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 3 represents a structure represented by the following formula (3-1), (3-2), (3-3), (3-4) or (3-5), [ka] In formula (3-2), R 71 and R 72 each independently represents a methyl group or a trifluoromethyl group. However, R 31 ~R 38 , R 71 and R 72 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. [ka] (In formula (4), R 41 ~R 44 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group. However, R 41 ~R 44 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. [ka] (In formula (5), R 51 ~R 58 is a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, or R 81 represents a group represented by R 81 is a halogen atom, a substituted or unsubstituted alkyl group having one or more carbon atoms, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted cycloalkyl group. However, R51 , R 52 , R 55 and R 56 At least one of the following is R 81 and other R 51 ~R 58 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. Effect of the Invention

[0006] According to the present invention, it is possible to provide an electrophotographic photoreceptor capable of suppressing potential fluctuations. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a diagram showing an example of a layer structure of an electrophotographic photoreceptor according to the present invention. [Diagram 2] 1 is a diagram showing an example of a schematic configuration of an electrophotographic apparatus provided with a process cartridge having an electrophotographic photosensitive member according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below with reference to preferred embodiments. When performing large-volume and high-speed printing, the potential fluctuation may become large in a conventional electrophotographic photoreceptor. The following is considered to be the cause of this. Electrophotographic photoreceptors are required to have high sensitivity and high durability in order to handle large-volume and high-speed printing, and therefore, charge generating substances having higher sensitivity are used as the charge generating substances contained in electrophotographic photoreceptors. As the charge generating material becomes more sensitive, the amount of generated charge increases, but in conventional electrophotographic photoreceptors, the electron transport capacity is insufficient, and it is considered that when images are repeatedly output, charges are retained in the exposed parts of the photosensitive layer, causing potential fluctuations. When the potential fluctuations in the exposed parts of the electrophotographic photoreceptor become large, the density of the image becomes lighter after repeated use than at the beginning, and the image quality deteriorates.

[0009] The present inventors have investigated the inclusion of a highly π-conjugated perylene imide at a high concentration in order to increase the mobility of electrons in order to suppress potential fluctuations. However, there are cases where the mobility of the electron transport material is not sufficiently increased by merely forming a film containing a high concentration of perylene imide. One of the reasons for this is the rigid planar structure of perylene imide. Perylene imide has a rigid planar structure, so that molecules tend to stack closely together, and form aggregation sites in the film, resulting in non-uniform distribution, which is thought to be a hindrance to improving the mobility.

[0010] Therefore, the present inventors have further studied and found that by using a polymer having a specific unit in addition to perylene imide as an electron transport material, perylene imides can be present at an appropriate distance from each other in the film, and the formation of aggregation sites can be suppressed. Furthermore, by using the above polymer as an electron transport material, the mobility of electrons was improved. The reason why the above problems in the prior art can be solved by using the above polymer as an electron transport material is considered to be as follows. An electron-withdrawing group is introduced into a specific unit of the above polymer. The present inventors presume that this reduces the electron density of the perylene imide moiety in the above polymer, thereby suppressing stacking of the perylene imide moiety. The present inventors also presume that the specific unit has a non-planar structure, thereby suppressing stacking of molecular chains. It is believed that the above mechanism has enabled the suppression of potential fluctuations. Specifically, the present inventors have found that the problems in the conventional technology can be solved by using an electrophotographic photoreceptor having an undercoat layer characterized by containing, as an electron transport material, a polymer having a structural unit represented by the formula (1) described below.

[0011] The configuration of the electrophotographic photoreceptor according to the present invention will be described in detail below. [Electrophotographic photoreceptor] The electrophotographic photoreceptor according to the present invention has a support, an undercoat layer, and a photosensitive layer in this order. Fig. 1 is a diagram showing an example of the layer structure of the electrophotographic photoreceptor according to the present invention. In Fig. 1, 101 is a support, 102 is an undercoat layer, 103 is a charge generating layer, 104 is a charge transport layer, and 105 is a photosensitive layer (laminated type photosensitive layer). The method for producing the electrophotographic photoreceptor according to the present invention includes a method in which the coating liquid for each layer described below is prepared, coated in the desired order, and dried. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoint of efficiency and productivity. The support and each layer will be described below.

[0012] <Support> In the present invention, the electrophotographic photoreceptor has a support. In the present invention, the support is preferably a conductive support having electrical conductivity. The shape of the support may be a cylinder, a belt, a sheet, or the like. Among them, a cylindrical support is preferable. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, or the like. The support is preferably made of a metal, a resin, or a glass. Examples of the metal include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among them, an aluminum support using aluminum is preferable. Furthermore, the resin or glass may be made conductive by a process such as mixing with or coating with a conductive material.

[0013] <Conductive layer> In the present invention, a conductive layer may be provided on the support. By providing the conductive layer, scratches and irregularities on the surface of the support can be concealed and light reflection on the surface of the support can be controlled. The conductive layer preferably contains conductive particles and a resin. The conductive particles may be made of a material such as metal oxide, metal, or carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure having a core particle and a coating layer that covers the core particle. Examples of the core particle include titanium oxide, barium sulfate, zinc oxide, etc. Examples of the coating layer include metal oxides such as tin oxide. Furthermore, when a metal oxide is used as the conductive particles, the volume average particle size thereof is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like.

[0014] The thickness of the conductive layer is preferably from 1 μm to 50 μm, and particularly preferably from 3 μm to 40 μm. The conductive layer can be formed by preparing a coating solution for the conductive layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the coating solution for the conductive layer include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser.

[0015] <Undercoat layer> The electrophotographic photoreceptor according to the present invention has an undercoat layer on the support or the conductive layer. In the present invention, the undercoat layer is obtained by forming a coating film of a coating solution for the undercoat layer containing a polymer having a structural unit represented by the following formula (1) and drying the coating film by heating. The temperature during drying by heating is preferably 50 to 200°C. In the present invention, the undercoat layer contains, as an electron transporting material, a polymer having a structural unit represented by the following formula (1). [ka] (In formula (1), R 11 ~R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, X represents a structure represented by the following formula (2), (3), (4) or (5).

[0016] [ka] (In formula (2), R 21 ~R 28 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z2 represents a structure represented by the following formula (2-1), (2-2), (2-3), (2-4) or (2-5), [ka] In formula (2-2), R 61 and R 62 each independently represents a methyl group or a trifluoromethyl group. However, R 21 ~R 28 , R 61 and R 62 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group.

[0017] [ka] (In formula (3), R 31 ~R 38 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 3 represents a structure represented by the following formula (3-1), (3-2), (3-3), (3-4) or (3-5), [ka] In formula (3-2), R 71 and R 72 each independently represents a methyl group or a trifluoromethyl group. However, R 31 ~R 38 , R 71 and R 72 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group.

[0018] [ka] (In formula (4), R 41 ~R 44 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group. However, R41 ~R 44 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group.

[0019] [ka] (In formula (5), R 51 ~R 58 is a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, or R 81 represents a group represented by R 81 is a halogen atom, a substituted or unsubstituted alkyl group having one or more carbon atoms, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted cycloalkyl group. However, R 51 , R 52 , R 55 and R 56 At least one of the following is R 81 and other R 51 ~R 58 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group.

[0020] In the structural unit represented by formula (1), examples of the substituent that the substituted alkyl group has include an aryl group, a halogen atom, a nitro group, a cyano group, and a trifluoromethyl group. Examples of the substituent on the substituted aryl group include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group. Examples of the substituent on the substituted alkoxy group include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group. Examples of the substituent that the substituted thiol group has include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group. Examples of the substituent on the substituted amino group include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, a hydroxyalkyl group, an aryl group, and an alkoxy group. Furthermore, examples of the substituent that the substituted alkynyl group may have include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group.

[0021] In the structural unit represented by formula (1), specific examples of the substituted or unsubstituted alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a cyclopentyl group, an n-hexyl group, a 1-methylpentyl group, a 4-methyl-2-pentyl group, a 3,3-dimethylbutyl group, a 2-ethylbutyl group, a cyclohexyl group, a hexyl group, an isohexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, a henicosyl group, a triacontyl group, a benzyl group, and a trityl group. Specific examples of the substituted or unsubstituted alkynyl group include an ethynyl group, a propynyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, and an octynyl group. Specific examples of the substituted or unsubstituted aryl group include a phenyl group, a biphenylyl group, a fluorenyl group, a 1-naphthyl group, a 2-naphthyl group, and a tolyl group. Specific examples of the substituted or unsubstituted alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a tert-butoxy group, a phenoxy group, a pentyloxy group, a cyclohexyloxy group, a benzyloxy group, an allyloxy group, and a 1-naphthyloxy group. Examples of the substituted or unsubstituted thiol group include a thiol group (sulfanyl group), a methylthio group, an ethylthio group, a propylthio group, a butylthio group, a pentylthio group, a hexylthio group, a heptylthio group, an octylthio group, and a phenylthio group. Specific examples of the substituted or unsubstituted amino group include an amino group, a methylamino group, a dimethylamino group, a trimethylamino group, an ethylamino group, a diethylamino group, a propylamino group, an isopropylamino group, a butylamino group, a pentylamino group, a hexylamino group, a heptylamino group, an octylamino group, a phenylamino group, and a pyrrolidinyl group.

[0022] Specific examples of the perylene imide structure in the structural unit represented by formula (1) are shown below. [ka] [ka] [ka]

[0023] From the viewpoint of forming a film state in which the perylene imide structure is uniformly distributed in the undercoat layer and from the viewpoint of improving the electron mobility, R 11 ~R 18at least one of the is preferably a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group having 20 carbon atoms or less, a substituted or unsubstituted thiol group having 20 carbon atoms or less, a substituted or unsubstituted amino group having 20 carbon atoms or less, a substituted or unsubstituted alkyl group having 20 carbon atoms or less, a substituted or unsubstituted alkynyl group having 20 carbon atoms or less, or a substituted or unsubstituted aryl group having 20 carbon atoms or less.

[0024] Specific examples of the structure represented by formula (2) are shown below. In the structure represented by formula (2), R 21 ~R 28 , R 61 and R 62 (When the structure represented by formula (2) does not have the structure represented by formula (2-2), R 21 ~R 28 At least one of) represents a nitro group, a cyano group, or a trifluoromethyl group. [ka]

[0025] From the viewpoint of forming a film state in which the perylene imide structure is uniformly distributed in the undercoat layer and from the viewpoint of increasing the mobility of electrons, R 21 ~R 28 , and R in formula (2-2) 61 and R 62 At least one of these is preferably a trifluoromethyl group.

[0026] Specific examples of the structure represented by formula (3) are shown below. In the structure represented by formula (3), R 31 ~R 38 , R 71 and R 72 (When the structure represented by formula (3) does not have the structure represented by formula (3-2), R 31 ~R 38 At least one of) represents a nitro group, a cyano group, or a trifluoromethyl group. [ka]

[0027] From the viewpoint of forming a film state in which the perylene imide structure is uniformly distributed in the undercoat layer and from the viewpoint of increasing the mobility of electrons, R 31 ~R 38 , and R in formula (3-2) 71 and R 72 At least one of these is preferably a trifluoromethyl group.

[0028] Specific examples of the structure represented by formula (4) are shown below. [ka]

[0029] From the viewpoint of forming a film state in which the perylene imide structure is uniformly distributed in the undercoat layer and from the viewpoint of increasing the electron mobility, R 41 ~R 44 At least one of these is preferably a trifluoromethyl group.

[0030] Specific examples of the structure represented by formula (5) are shown below. [ka]

[0031] From the viewpoint of forming a film state in which the perylene imide structure is uniformly distributed in the undercoat layer and from the viewpoint of increasing the electron mobility, R 51 ~R 58 At least one of these is preferably a trifluoromethyl group.

[0032] Examples of polymer compounds having a structural unit represented by formula (1) are shown in Table 1 below. [Table 1]

[0033] The weight average molecular weight of the polymer having the structural unit represented by formula (1) is preferably 30,000 or less. In the present invention, the content ratio of the polymer having a structural unit represented by formula (1) relative to the total mass of the undercoat layer is preferably 30 mass% or more, and more preferably 50 mass% or more, from the viewpoint of improving the electron mobility in the undercoat layer. The thickness of the undercoat layer is preferably from 0.1 μm to 10 μm, and more preferably from 0.5 μm to 5 μm. The undercoat layer controls charge injection at the interface and also functions as an adhesive layer. The undercoat layer in the present invention has a function of transporting charges of the same polarity as the charge polarity of the surface of the electrophotographic photoreceptor. Specifically, the charge polarity of the surface of the electrophotographic photoreceptor is negative, and the undercoat layer has a negative charge transport function, i.e., an electron transport function, and its electron mobility is 10 -7 cm 2 / V·sec or more is preferable, and 10 -6 cm 2 / V·sec or more. In order to maintain the surface potential of the electrophotographic photoreceptor, the volume resistivity of the undercoat layer is 1×10 10 It is preferable that the resistivity is Ω·cm or more, and more preferably 1×10 12 Ω·cm or more.

[0034] The coating liquid for forming the undercoat layer according to the present invention may contain a crosslinking agent in addition to the electron transport material. As the crosslinking agent, any known material can be used, specifically, the compounds described in "Crosslinking Agent Handbook" edited by Shinzo Yamashita and Tosuke Kaneko, published by Taiseisha (1981) can be mentioned.

[0035] In the present invention, the crosslinking agent is preferably an isocyanate compound having an isocyanate group or a blocked isocyanate group, or an amine compound having an N-methylol group or an alkyl-etherified N-methylol group. An isocyanate compound having 2 to 6 isocyanate groups or blocked isocyanate groups is preferred. Examples of the isocyanate compound as the crosslinking agent include the isocyanate compounds shown below, but the present invention is not limited thereto. In addition, the isocyanate compounds shown below may be used in combination. Examples of the isocyanate compound include isocyanurate modified products, biuret modified products, allophanate modified products, and adduct modified products with trimethylolpropane or pentaerythritol of diisocyanates such as triisocyanate benzene, triisocyanate methylbenzene, triphenylmethane triisocyanate, lysine triisocyanate, tolylene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, xylylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, methyl-2,6-diisocyanate hexanoate, and norbornane diisocyanate. The blocked isocyanate group is -NHCOX 1 (X 1 X is a protecting group). 1 may be any protecting group that can be introduced into an isocyanate group. Examples of commercially available isocyanate compounds include isocyanate-based crosslinking agents such as Duranate MFK-60B, SBA-70B, 17B-60P, SBN-70D, and SBB-70P manufactured by Asahi Kasei Corporation, and Desmodur BL3175 and BL3475 manufactured by Sumika Bayer Urethane Co., Ltd. The amine compound as the crosslinking agent preferably has an N-methylol group or an alkyl-etherified N-methylol group.More preferably, the amine compound has a plurality (two or more) of N-methylol groups or alkyl-etherified N-methylol groups.For example, the amine compound may include methylolated melamine, methylolated guanamine, methylolated urea derivatives, methylolated ethylene urea derivatives, methylolated glycoluril, and compounds in which the methylol moiety is alkyl-etherified, and derivatives thereof. Examples of commercially available amine compounds (crosslinking agents) include Super Melami No. 90 (manufactured by NOF Corp. (formerly Nippon Oil & Fats)), Super Bekkamin® TD-139-60, L-105-60, L127-60, L110-60, J-820-60, and G-821-60 (manufactured by DIC Corp.), U-Ban 2020 (Mitsui Chemicals), Sumitex Resin M-3 (manufactured by Sumitomo Chemical Co., Ltd. (formerly Sumitomo Chemical Co., Ltd.)), and Ni Examples of such compounds include Karac MW-30, MW-390, and MX-750LM (manufactured by Sanwa Chemical Co., Ltd.), Super Beckamin(R) L-148-55, 13-535, L-145-60, and TD-126 (manufactured by DIC Corporation), Nikalac BL-60 and BX-4000 (manufactured by Sanwa Chemical Co., Ltd.), Nikalac MX-280, Nikalac MX-270, and Nikalac MX-290 (manufactured by Sanwa Chemical Co., Ltd.).

[0036] The coating liquid for forming the undercoat layer according to the present invention may contain a thermoplastic resin having a polymerizable functional group in addition to the electron transport material and the crosslinking agent. Examples of the thermoplastic resin include polyacetal resin, polyolefin resin, polyester resin, polyether resin, polyamide resin, etc. Examples of the polymerizable functional group of the thermoplastic resin include a hydroxyl group, a thiol group, an amino group, and a methoxy group. Furthermore, the thermoplastic resin is preferably a thermoplastic resin having a repeating unit consisting of -(CH2-CH2-O)n- (n is an integer of 2 or more and 200 or less), -(CH2-CH3CH-O)n- (n is an integer of 2 or more and 200 or less), or -(CH2-CH2-O-CH2-CH2-SS)n- (n is an integer of 2 or more and 50 or less). Thermoplastic resins having a polymerizable functional group that are commercially available include, for example, polyether polyol resins such as AQD-457, AQD-473 (all manufactured by Nippon Polyurethane Industry Co., Ltd.), GP-400, and GP-700 (all manufactured by Sanyo Chemical Industries, Ltd. and Sannix); Phthalkid W2343 (manufactured by Hitachi Chemical Co., Ltd.), Watersol S-118, CD-520, Beckolite M-6402-50, and M-6201-40IM (all manufactured by DIC), Haridip WH-1188 (manufactured by Harima Chemical Co., Ltd.), ES3604, and ES6538 (all manufactured by Nippon Polyurethane Industry Co., Ltd.); Examples of such resins include polyester polyol resins such as those manufactured by U-PICA; polyacrylic polyol resins such as Burnock WE-300 and WE-304 (both manufactured by DIC); polyvinyl alcohol resins such as Kuraray Poval PVA-203 (manufactured by Kuraray); polyvinyl acetal resins such as BX-1, BM-1, and KS-5 (both manufactured by Sekisui Chemical Co., Ltd.); polyamide resins such as Toresin FS-350 (manufactured by Nagase Chemtex); polyamine resins such as Luccamide (manufactured by DIC); and polythiol resins such as QE-340M (manufactured by Toray). Among these, polyvinyl acetal resins having a polymerizable functional group and polyester polyol resins having a polymerizable functional group are preferred from the viewpoint of polymerizability. The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0037] <Photosensitive layer> The photosensitive layer of an electrophotographic photoreceptor is mainly classified into (1) a multi-layer type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The multi-layer type photosensitive layer has a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer has a photosensitive layer containing both a charge generation material and a charge transport material.

[0038] (1) Laminated photosensitive layer The laminated photosensitive layer includes a charge generating layer and a charge transport layer.

[0039] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin. Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable.

[0040] The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds. The thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm. The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0041] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin. Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred. The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer. Examples of the resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10.

[0042] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles. The thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm. The charge transport layer can be formed by preparing a coating solution for the charge transport layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred.

[0043] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming a coating film of this, and drying it. The charge generating material, the charge transporting material and the resin are the same as the examples of materials in "(1) Multi-layer type photosensitive layer" above.

[0044] <Protective layer> In the present invention, a protective layer may be provided on the photosensitive layer. By providing the protective layer, durability can be improved. The protective layer preferably contains conductive particles and / or a charge transport material, and a resin. The conductive particles include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide. Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred. Examples of the resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among them, polycarbonate resin, polyester resin, and acrylic resin are preferable.

[0045] The protective layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the reaction include thermal polymerization, photopolymerization, and radiation polymerization. Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an acrylic group and a methacrylic group. A material having a charge transport function may be used as the monomer having a polymerizable functional group. The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, abrasion resistance improvers, etc. Specific examples of the additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles. The thickness of the protective layer is preferably from 0.5 μm to 10 μm, and more preferably from 1 μm to 7 μm. The protective layer can be formed by preparing a coating solution for the protective layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0046] [Process cartridges, electrophotographic devices] The process cartridge according to the present invention is characterized in that it integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably attachable to the main body of the electrophotographic apparatus. The electrophotographic apparatus according to the present invention is characterized by comprising the electrophotographic photosensitive member described above, as well as a charging means, an exposing means, a developing means and a transferring means.

[0047] FIG. 2 shows an example of a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. A cylindrical electrophotographic photoreceptor 1 is driven to rotate around an axis 2 at a predetermined peripheral speed in the direction of the arrow. The surface of the electrophotographic photoreceptor 1 is charged to a predetermined positive or negative potential by a charging means 3. Although the figure shows a roller charging method using a roller-type charging member, a corona charging method, a proximity charging method, an injection charging method, or other charging methods may be adopted. Exposure light 4 is irradiated from an exposure means (not shown) onto the charged surface of the electrophotographic photoreceptor 1, and an electrostatic latent image corresponding to the target image information is formed. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 1 is developed with toner contained in a developing means 5, and a toner image is formed on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor 1 is transferred to a transfer material 7 by a transfer means 6. The transfer material 7 to which the toner image has been transferred is transported to a fixing means 8, where the toner image is fixed, and the transfer material is printed out outside the electrophotographic device. The electrophotographic device may have a cleaning means 9 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 1 after transfer. Also, a so-called cleanerless system may be used in which the deposits are removed by the developing means 5 or the like without separately providing the cleaning means 9. The electrophotographic apparatus may have a charge eliminating mechanism that eliminates charge on the surface of the electrophotographic photoreceptor 1 by pre-exposure light 10 from a pre-exposure means (not shown). Also, in order to mount and remove the process cartridge 11 according to the present invention to the main body of the electrophotographic apparatus, a guide means 12 such as a rail may be provided. The electrophotographic photoreceptor of the present invention can be used in laser beam printers, LED printers, copiers, facsimiles, and combination machines thereof. EXAMPLES

[0048] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples without departing from the gist of the present invention. In the following description of the examples, "parts" are based on mass unless otherwise specified.

[0049] First, a synthesis example of a polymer (electron transport material) having a structural unit represented by formula (1) will be shown. [Synthesis example of a polymer having a structural unit represented by formula (1) (example of compound: PIP-1)] 50 parts of N-methylpyrrolidone were mixed with 1.96 parts of 3,4,9,10-perylenetetracarboxylic dianhydride (Tokyo Chemical Industry Co., Ltd.) and 1.99 parts of 2,2-bis(4-aminophenyl)hexafluoropropane (Tokyo Chemical Industry Co., Ltd.). The mixture was heated to 180°C while stirring, and reacted for 48 hours, after which the mixture was cooled. The cooled mixture was then poured into 50 ml of water, and the precipitate was filtered off. The precipitate was washed with hot water and then dried to obtain 3.3 parts of a polymer (PIP-1) having a structural unit represented by formula (1). The compound obtained was identified by NMR. For identification, measurements were performed using a 1H-NMR (400MHz, JMN-EX400, JEOL) with a solvent CDCl3. As a result, the peak positions of the target compound were confirmed to be δ8.6-7.8 ppm (broad m, perylene moiety) and δ7.5-7.8 ppm (broad m, phenyl moiety linked to imide nitrogen). The weight-average molecular weight of the obtained polymer was 11072 (Table 2). The weight-average molecular weight (Mw) was measured by GPC (gel permeation chromatography) using HLC-8220 manufactured by Tosoh Corporation, and expressed as a polystyrene equivalent value.

[0050] [Synthesis example of a polymer having a structural unit represented by formula (1) (example of compound: PIP-29)] 50 parts of N-methylpyrrolidone were mixed with 1.96 parts of 3,4,9,10-perylenetetracarboxylic dianhydride (Tokyo Chemical Industry Co., Ltd.) and 1.87 parts of 2,2'-bis(trifluoromethyl)benzidine (Tokyo Chemical Industry Co., Ltd.). The mixture was heated to 180°C while stirring, and reacted for 72 hours, after which the mixture was cooled. The cooled mixture was then poured into 50 ml of water, and the precipitate was filtered off. The precipitate was washed with hot water and then dried to obtain 3.2 parts of a polymer (PIP-29) having a structural unit represented by formula (1). The compound obtained was identified by NMR. For identification, measurements were performed using a solvent CDCl3 by 1H-NMR (400MHz, JMN-EX400, JEOL). As a result, the peak positions of the target compound were confirmed to be δ8.6-7.8 ppm (broad m, perylene moiety) and δ7.5-7.9 ppm (broad m, phenyl moiety linked to imide nitrogen). The weight average molecular weight of the obtained polymer was 16256 (Table 2). The weight average molecular weight (Mw) was measured by GPC (gel permeation chromatography) using HLC-8220 manufactured by Tosoh Corporation, and expressed as a polystyrene equivalent value. A synthesis example of an electron transport material used in a comparative example will be described below.

[0051] [Synthesis example of electron transport material (D01)] The following materials were prepared: 1.96 parts of 3,4,9,10-perylenetetracarboxylic dianhydride (Tokyo Chemical Industry Co., Ltd.) 4,4'-Diaminodiphenyl ether (Tokyo Chemical Industry Co., Ltd.) 0.95 parts 0.038 parts of 3,5-diaminobenzoic acid (Tokyo Chemical Industry Co., Ltd.) These were mixed with 100 parts of dimethylacetamide under a nitrogen atmosphere, stirred at room temperature for 1 hour, and then refluxed for 8 hours. The resulting precipitate was then filtered and washed with acetone to obtain 0.82 parts of electron transport material (D01). The product obtained was in the form of particles.

[0052] [Example 1] [Manufacturing of electrophotographic photoreceptors] <Support> An aluminum cylinder with a length of 260.5 mm and a diameter of 30 mm was prepared. This aluminum cylinder was machined (JIS B 0601:2014, ten-point average roughness Rzjis: 0.8 μm), and the machined aluminum cylinder was used as a support (conductive support).

[0053] <Undercoat layer> Next, 5 parts of the exemplary compound (PIP-1) as an electron transport material was dissolved in a mixed solvent of 48 parts of chloroform and 24 parts of o-xylene. The obtained coating solution for the undercoat layer was dip-coated on the support, and the obtained coating film was heated at 170°C for 40 minutes and dried to form an undercoat layer with a thickness of 1.5 µm.

[0054] <Charge generation layer> Next, hydroxygallium phthalocyanine crystals (charge generating material) having peaks at Bragg angles (2θ±0.2°) of 7.5°, 9.9°, 12.5°, 16.3°, 18.6°, 25.1°, and 28.3° in CuKα characteristic X-ray diffraction were prepared. 10 parts of this hydroxygallium phthalocyanine crystal, 5 parts of polyvinyl butyral resin (trade name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.), and 250 parts of cyclohexanone were placed in a sand mill using glass beads with a diameter of 1 mm, and dispersed for 2 hours. Next, 250 parts of ethyl acetate were added to this to prepare a coating liquid for a charge generating layer. This coating liquid for a charge generating layer was applied by dip coating on the undercoat layer to form a coating film, and the resulting coating film was dried at a temperature of 95° C. for 10 minutes to form a charge generating layer having a thickness of 0.15 μm.

[0055] <Charge transport layer> The following materials were prepared: 5 parts of a charge transport material represented by the following formula (B-1): [ka] 5 parts of a charge transport material compound represented by the following formula (B-2): [ka] Polycarbonate resin (product name: Iupilon Z-400, manufactured by Mitsubishi Engineering Plastics) 10 parts These were dissolved in a mixed solvent of 25 parts of orthoxylene / 25 parts of methyl benzoate / 25 parts of dimethoxymethane to prepare a coating solution for the charge transport layer. The charge transport layer coating liquid thus prepared was dip-coated onto the charge generation layer to form a coating film, and the coating film was dried by heating at a temperature of 120° C. for 30 minutes to form a charge transport layer having a thickness of 25 μm.

[0056] [evaluation] <Evaluation of potential fluctuation> A laser beam printer (product name: Laser Jet Enterprise M609dn) manufactured by Hewlett-Packard was used to evaluate the potential fluctuation. For the evaluation, the laser beam printer was modified so that it could operate at a process speed of 370 mm / s, with variable charging conditions, and variable laser exposure. The potential fluctuation was evaluated as follows. The manufactured electrophotographic photoreceptor was mounted in the above-mentioned laser beam printer and placed in an environment of normal temperature and normal humidity (23° C. / 50% RH). The initial drum surface potential was −500 V for the non-exposed area, and the exposure light amount was 0.3 μJ / cm. 2 After passing 10,000 sheets, the potential of the exposed portion was measured. The surface potential was measured by modifying the cartridge, attaching a potential probe (model 6000B-8, Trek Japan) to the development position, and measuring the potential at the center of the drum using a surface potential meter (model 344, Trek Japan). During paper feed, a text image with a print rate of 1% was printed on A4-sized plain paper, and 10,000 sheets of image were output. The potential fluctuation was evaluated by calculating the amount of fluctuation between the initial state and after 10,000 sheets had been fed. The results are shown in Table 2.

[0057] Evaluation of Electron Mobility The electron mobility was determined by the time of flight method. It is known that the electron mobility depends on the electric field strength. 7 The values ​​used were those in V / m. The specific measurement method is as follows. First, for the evaluation of electron mobility, the coating liquid for the undercoat layer was applied to an aluminum sheet with a wire bar and dried at 160°C for 10 minutes to form an undercoat layer with a thickness of 5.0 μm. Then, the coating liquid for the charge generation layer was applied with a wire bar and dried at 100°C for 10 minutes to form a charge generation layer with a thickness of 0.2 μm to prepare a measurement sample. The measurement sample thus prepared was sandwiched between glass transparent electrodes coated with a conductive material such as ITO coating to form a circuit consisting of a power supply and a resistor for measuring current. Next, an electric field of 3.0×10 7 After applying a voltage adjusted to V / m, the sample was irradiated with light from the transparent electrode side. At this time, the electrons generated in the charge generation layer were injected into the undercoat layer, and the current waveform when they traveled through the undercoat layer by hopping conduction was observed with an oscilloscope to obtain the travel time (t) of the carriers traveling within the sample. The speed (v=d / t) was calculated from this travel time (t) and the thickness (d) of the sample. Since the speed (v) is the product (v=μE) of the electron mobility (μ) and the electric field strength (E), the electron mobility (μ) in the sample was calculated by dividing the speed (v) by the electric field strength (E). The obtained electron mobility is shown in Table 2. The volume resistivity was also measured using the measurement samples prepared in the same manner. The results are shown in Table 2.

[0058] [Examples 2 to 8, 13 to 44, 49 to 80, 85 to 300] Electrophotographic photoreceptors were produced and evaluated in the same manner as in Example 1, except that the electron transport material in Example 1 was changed to one shown in Tables 2 to 6. The results are shown in Tables 2 to 6.

[0059] [Example 9] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Example 1, except that the undercoat layer was formed as follows. The results are shown in Table 2.

[0060] <Undercoat layer> The following materials were prepared: 8 parts of exemplary compound (PIP-1) as electron transport material 4.01 parts of a blocked isocyanate compound (product name: SBB-70P (solid content 70%, isocyanate:blocking group=6.7:3.3 (mass ratio), manufactured by Asahi Kasei)) as an isocyanate compound 0.12 parts of styrene-acrylic resin (product name: UC-3920, manufactured by Toagosei) These were dissolved in a mixed solvent consisting of 48 parts of 1-butanol and 24 parts of acetone. The obtained coating liquid for the undercoat layer was dip-coated onto a support, and the obtained coating film was heated at 170° C. for 40 minutes to be cured (polymerized) to form an undercoat layer with a thickness of 1.5 μm.

[0061] [Examples 10 to 12, 45 to 48, 81 to 84] In Example 9, the electron transport material was changed to the electron transport material shown in Tables 2 and 3. In addition, the content ratio of the electron transport material, the isocyanate compound, and the resin in the undercoat layer was changed, and the content ratio (mass%) of the electron transport material in the undercoat layer was changed as shown in Tables 2 and 3. The ratio between the isocyanate compound and the resin was kept constant. Except for that, an electrophotographic photoreceptor was produced in the same manner as in Example 9, and evaluated in the same manner. The results are shown in Tables 2 and 3.

[0062] [Example 301] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Example 1, except that the support was changed to that described below, a conductive layer was formed on the support as described below, and an undercoat layer was further formed on the conductive layer as described below. The results are shown in Table 6.

[0063] <Support> An aluminum cylinder having a diameter of 30 mm and a length of 260.5 mm was used as a support (cylindrical support).

[0064] <Conductive layer> An anatase-type titanium oxide having an average primary particle size of 200 nm was used as the substrate, and a titanium niobium sulfate solution containing 33.7 parts of titanium in terms of TiO2 and 2.9 parts of niobium in terms of Nb2O5 was prepared. 100 parts of the substrate was dispersed in pure water to prepare a suspension of 1000 parts, which was then heated to 60°C. The titanium niobium sulfate solution and 10 mol / L sodium hydroxide were dropped into the suspension over 3 hours so that the pH of the suspension was 2 to 3. After the entire amount was dropped, the pH was adjusted to near neutral, and a polyacrylamide-based flocculant was added to precipitate the solids. The supernatant was removed, filtered, washed, and dried at 110°C to obtain an intermediate containing 0.1 mass% of organic matter derived from the flocculant in terms of C. This intermediate was calcined in nitrogen at 750°C for 1 hour, and then calcined in air at 450°C to produce titanium oxide particles. The resulting particles had a volume average particle size (average primary particle size) of 220 nm as determined by a particle size measurement method using a scanning electron microscope. Next, a phenolic resin (phenolic resin monomer / oligomer) was used as a binder (product name: Plyofen J-325, manufactured by DIC, resin solid content: 60%, density after curing: 1.3 g / cm 2 50 parts of this phenol resin was dissolved in 35 parts of 1-methoxy-2-propanol as a solvent to obtain a solution. To this solution, 60 parts of titanium oxide particles were added, and the mixture was placed in a vertical sand mill using 120 parts of glass beads with an average particle size of 1.0 mm as a dispersion medium, and dispersion treatment was carried out for 4 hours under conditions of a dispersion temperature of 23±3°C and a rotation speed of 1500 rpm (circumferential speed of 5.5 m / s) to obtain a dispersion. The glass beads were removed from this dispersion using a mesh. Next, the following materials were prepared: 0.01 part silicone oil as a leveling agent (product name: SH28 PAINT ADDITIVE, manufactured by Toray Dow Corning) Silicone resin particles (product name: KMP-590, manufactured by Shin-Etsu Chemical Co., Ltd., average particle size: 2 μm, density: 1.3 g / cm) were used as a surface roughening agent. 3 ) 8 copies These were added to the dispersion liquid after removing the glass beads, stirred, and filtered under pressure using PTFE filter paper (product name: PF060, manufactured by Advantec Toyo) to prepare a coating liquid for the conductive layer. The conductive layer coating liquid thus prepared was dip-coated onto the above-mentioned support to form a coating film, and the coating film was heated at 150° C. for 20 minutes to be cured, thereby forming a conductive layer having a thickness of 25 μm.

[0065] <Undercoat layer> The following materials were prepared: 8 parts of exemplary compound (PIP-1) as electron transport material 4.01 parts of a blocked isocyanate compound (product name: SBB-70P (solid content 70%, isocyanate:blocking group=6.7:3.3 (mass ratio), manufactured by Asahi Kasei)) as an isocyanate compound 0.12 parts of styrene-acrylic resin (product name: UC-3920, manufactured by Toagosei) These were dissolved in a mixed solvent of 48 parts of 1-butanol and 24 parts of acetone. The obtained coating liquid for undercoat layer was dip-coated onto the conductive layer, and the obtained coating film was heated at 170° C. for 40 minutes to be cured (polymerized) to form an undercoat layer with a thickness of 1.5 μm.

[0066] [Example 302] The support was changed to the one described below, and a conductive layer was formed on the support as follows. Then, an undercoat layer, a charge generating layer, and a charge transport layer similar to those in Example 1 were formed in this order on the conductive layer to produce an electrophotographic photoreceptor, which was evaluated in the same manner as in Example 1. The results are shown in Table 6.

[0067] <Support> An aluminum cylinder having a diameter of 30 mm and a length of 260.5 mm was used as a support (cylindrical support).

[0068] <Conductive layer> An anatase-type titanium oxide having an average primary particle size of 200 nm was used as the substrate, and a titanium niobium sulfate solution containing 33.7 parts of titanium in terms of TiO2 and 2.9 parts of niobium in terms of Nb2O5 was prepared. 100 parts of the substrate was dispersed in pure water to prepare a suspension of 1000 parts, which was then heated to 60°C. The titanium niobium sulfate solution and 10 mol / L sodium hydroxide were dropped into the suspension over 3 hours so that the pH of the suspension was 2 to 3. After the entire amount was dropped, the pH was adjusted to near neutral, and a polyacrylamide-based flocculant was added to precipitate the solids. The supernatant was removed, filtered, washed, and dried at 110°C to obtain an intermediate containing 0.1 mass% of organic matter derived from the flocculant in terms of C. This intermediate was calcined in nitrogen at 750°C for 1 hour, and then calcined in air at 450°C to produce titanium oxide particles. The resulting particles had a volume average particle size (average primary particle size) of 220 nm as determined by a particle size measurement method using a scanning electron microscope. Next, a phenolic resin (phenolic resin monomer / oligomer) was used as a binder (product name: Plyofen J-325, manufactured by DIC, resin solid content: 60%, density after curing: 1.3 g / cm 2 50 parts of this phenol resin was dissolved in 35 parts of 1-methoxy-2-propanol as a solvent to obtain a solution. To this solution, 60 parts of titanium oxide particles were added, and the mixture was placed in a vertical sand mill using 120 parts of glass beads with an average particle size of 1.0 mm as a dispersion medium, and dispersion treatment was carried out for 4 hours under conditions of a dispersion temperature of 23±3°C and a rotation speed of 1500 rpm (circumferential speed of 5.5 m / s) to obtain a dispersion. The glass beads were removed from this dispersion using a mesh. Next, the following materials were prepared: 0.01 part silicone oil as a leveling agent (product name: SH28 PAINT ADDITIVE, manufactured by Toray Dow Corning) Silicone resin particles (product name: KMP-590, manufactured by Shin-Etsu Chemical Co., Ltd., average particle size: 2 μm, density: 1.3 g / cm) were used as a surface roughening agent. 3 ) 8 copies These were added to the dispersion liquid after removing the glass beads, stirred, and filtered under pressure using PTFE filter paper (product name: PF060, manufactured by Advantec Toyo) to prepare a coating liquid for the conductive layer. The conductive layer coating liquid thus prepared was dip-coated onto the above-mentioned support to form a coating film, and the coating film was heated at 150° C. for 20 minutes to be cured, thereby forming a conductive layer having a thickness of 25 μm.

[0069] [Comparative Example 1] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Example 1, except that the method of forming the undercoat layer in Example 1 was changed as follows. The results are shown in Table 7. <Undercoat layer> 40 parts of the electron transport material (D01) and 500 parts of distilled water, 300 parts of methanol, and 8 parts of triethylamine as a dispersion medium were mixed and dispersed for 2 hours in a sand mill using glass beads with a diameter of 1 mm to prepare a coating solution for an undercoat layer. The obtained coating solution for an undercoat layer was dip-coated on a support, and the obtained coating film was heated at 120°C for 10 minutes and dried to form an undercoat layer with a thickness of 1.5 μm. [ka] The ratio of the repeating units in the electron transporting substance (D01) is indicated by mol %.

[0070] [Comparative Examples 2 to 5] In Example 9, the electron transport material was changed to an electron transport material (D01). In addition, the content ratio of the electron transport material, the isocyanate compound, and the resin in the undercoat layer was changed so that the content ratio (mass%) of the electron transport material in the undercoat layer became the value shown in Table 7. The ratio between the isocyanate compound and the resin was kept constant. Except for that, an electrophotographic photoreceptor was produced in the same manner as in Example 9, and was evaluated in the same manner. The results are shown in Table 7.

[0071] [Comparative Examples 6 and 7] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Comparative Example 1, except that the electron transport material (D01) in Comparative Example 1 was changed to have a weight average molecular weight shown in Table 7. The results are shown in Table 7.

[0072] [Comparative Examples 8 to 11] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Comparative Example 3, except that the electron transport material (D01) in Comparative Example 1 was changed to the electron transport materials (D02) to (D05) shown in Table 7. The structures of the electron transport materials (D02) to (D05) used in Comparative Examples 8 to 11 are shown below. The results are shown in Table 7. [ka]

[0073] [Table 2]

[0074] [Table 3]

[0075] [Table 4]

[0076] [Table 5]

[0077] [Table 6]

[0078] [Table 7]

[0079] The disclosure according to an embodiment of the present invention includes the following configuration. (Configuration 1) An electrophotographic photoreceptor having a support, an undercoat layer, and a photosensitive layer in this order, The electrophotographic photoreceptor comprises an undercoat layer containing a polymer having a structural unit represented by the following formula (1): [ka] (In formula (1), R 11 ~R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, X represents a structure represented by the following formula (2), (3), (4) or (5). [ka] (In formula (2), R 21 ~R 28 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 2 represents a structure represented by the following formula (2-1), (2-2), (2-3), (2-4) or (2-5), [ka] In formula (2-2), R 61 and R 62 each independently represents a methyl group or a trifluoromethyl group. However, R 21 ~R 28 , R 61 and R 62 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. [ka] (In formula (3), R 31~R 38 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 3 represents a structure represented by the following formula (3-1), (3-2), (3-3), (3-4) or (3-5), [ka] In formula (3-2), R 71 and R 72 each independently represents a methyl group or a trifluoromethyl group. However, R 31 ~R 38 , R 71 and R 72 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. [ka] (In formula (4), R 41 ~R 44 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group. However, R 41 ~R 44 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. [ka] (In formula (5), R 51 ~R 58 is a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, or R 81 represents a group represented by R 81 is a halogen atom, a substituted or unsubstituted alkyl group having one or more carbon atoms, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted cycloalkyl group. However, R51 , R 52 , R 55 and R 56 At least one of the following is R 81 and other R 51 ~R 58 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. (Configuration 2) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the content of the polymer having the structural unit represented by the formula (1) in the undercoat layer is 50% by mass or more based on the total mass of the undercoat layer. (Configuration 3) R in formula (1) 11 ~R 18 at least one of the above is a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group having 20 carbon atoms or less, a substituted or unsubstituted thiol group having 20 carbon atoms or less, a substituted or unsubstituted amino group having 20 carbon atoms or less, a substituted or unsubstituted alkyl group having 20 carbon atoms or less, a substituted or unsubstituted alkynyl group having 20 carbon atoms or less, or a substituted or unsubstituted aryl group having 20 carbon atoms or less. (Configuration 4) R in Equation (2) 21 ~R 28 , R in formula (2-2) 61 and R 62 , R in Equation (3) 31 ~R 38 , R in formula (3-2) 71 and R 72 , R in Equation (4) 41 ~R 44 , and R in formula (5) 51 ~R 58 4. The electrophotographic photoreceptor according to any one of configurations 1 to 3, wherein at least one of the groups is a trifluoromethyl group. (Configuration 5) 5. The electrophotographic photoreceptor according to any one of configurations 1 to 4, wherein the polymer having the structural unit represented by formula (1) has a weight average molecular weight of 30,000 or less. (Configuration 6) The volume resistivity of the undercoat layer is 1×10 106. The electrophotographic photoreceptor according to any one of configurations 1 to 5, which has a resistivity of Ω·cm or more. (Configuration 7) A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of Configurations 1 to 6 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus. (Configuration 8) 7. An electrophotographic apparatus comprising: an electrophotographic photoreceptor according to any one of Configurations 1 to 6; a charging unit, an exposing unit, a developing unit, and a transferring unit. [Explanation of symbols]

[0080] 101:Support 102: Undercoat layer 103: Charge generating layer 104: Charge transport layer 105: Photosensitive layer 1: Electrophotographic photoreceptor 2: Axis 3: Charging means 4: Image exposure light 5: Developing method 6: Transfer method 7: Transfer material 8: Image fixing means 9: Cleaning means 10: Pre-exposure light 11: Process cartridge 12: Guidance means

Claims

1. An electrophotographic photoreceptor having a support, an undercoat layer, and a photosensitive layer in this order, The electrophotographic photoreceptor comprises an undercoat layer containing a polymer having a structural unit represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 11 ~R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, X represents a structure represented by the following formula (2), (3), (4) or (5): 【Chemistry 2】 (In formula (2), R 21 ~R 28 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 2 represents a structure represented by the following formula (2-1), (2-2), (2-3), (2-4) or (2-5), 【Chemistry 3】 In formula (2-2), R 61 and R 62 each independently represents a methyl group or a trifluoromethyl group. However, R 21 ~R 28 , R 61 and R 62 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. 【Chemistry 4】 (In formula (3), R 31 ~R 38 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, Z 3 represents a structure represented by the following formula (3-1), (3-2), (3-3), (3-4) or (3-5), 【Chemistry 5】 In formula (3-2), R 71 and R 72 each independently represents a methyl group or a trifluoromethyl group. However, R 31 ~R 38 , R 71 and R 72 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. 【Chemistry 6】 (In formula (4), R 41 ~R 44 each independently represents a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group. However, R 41 ~R 44 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group. 【Chemistry 7】 (In formula (5), R 51 ~R 58 is a hydrogen atom, a nitro group, a cyano group, or a trifluoromethyl group, or R 81 represents a group represented by R 81 is a halogen atom, a substituted or unsubstituted alkyl group having one or more carbon atoms, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted cycloalkyl group. However, R 51 , R 52 , R 55 and R 56 At least one of 81 and other R 51 ~R 58 At least one of represents a nitro group, a cyano group, or a trifluoromethyl group.

2. 2. The electrophotographic photoreceptor according to claim 1, wherein the content of the polymer having the structural unit represented by formula (1) is 50% by mass or more based on the total mass of the undercoat layer.

3. R in formula (1) 11 ~R 18 2. The electrophotographic photoreceptor according to claim 1, wherein at least one of the is a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group having 20 carbon atoms or less, a substituted or unsubstituted thiol group having 20 carbon atoms or less, a substituted or unsubstituted amino group having 20 carbon atoms or less, a substituted or unsubstituted alkyl group having 20 carbon atoms or less, a substituted or unsubstituted alkynyl group having 20 carbon atoms or less, or a substituted or unsubstituted aryl group having 20 carbon atoms or less.

4. R in formula (2) 21 ~R 28 , R in formula (2-2) 61 and R 62 , R in formula (3) 31 ~R 38 , R in formula (3-2) 71 and R 72 , R in formula (4) 41 ~R 44 , and R in formula (5) 51 ~R 58 2. The electrophotographic photoreceptor according to claim 1, wherein at least one of is a trifluoromethyl group.

5. 2. The electrophotographic photoreceptor according to claim 1, wherein the polymer having the structural unit represented by formula (1) has a weight average molecular weight of 30,000 or less.

6. The volume resistivity of the undercoat layer is 1×10 10 2. The electrophotographic photoreceptor according to claim 1, which has a surface area of ​​Ω·cm or more.

7. 7. A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of claims 1 to 6 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

8. 7. An electrophotographic apparatus comprising: the electrophotographic photoreceptor according to claim 1; a charging unit, an exposing unit, a developing unit, and a transferring unit.

Citation Information

Patent Citations

  • Electrophotographic photosensitive member, process cartridge, and electrophotographic apparatus