Recycled composite semipermeable membrane and element

The composite semipermeable membrane, utilizing recycled polysulfone and biopolyester, addresses the need for decarbonization by reducing CO2 emissions while maintaining separation efficiency.

JP2024152172AInactive Publication Date: 2024-10-25TORAY INDUSTRIES INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023066208
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The increasing demand for decarbonization and recycling in various fields necessitates the development of composite semipermeable membranes that utilize recycled materials to reduce CO2 emissions.

Method used

A composite semipermeable membrane is developed using a support membrane containing recycled polysulfone and a separation functional layer, which includes a base material and a porous support layer made from recycled polyester or biopolyester, integrated with a water collection pipe, supply side channel material, and permeation side channel material.

Benefits of technology

The use of recycled materials reduces CO2 emissions by incorporating recycled polysulfone and biopolyester, maintaining effective separation performance while minimizing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152172000001_ABST
    Figure 2024152172000001_ABST
Patent Text Reader

Abstract

To provide a composite semipermeable membrane which can reduce a CO2 emission amount.SOLUTION: A composite semipermeable membrane is produced from a support membrane containing recycled polysulfone.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite semipermeable membrane useful for selective separation of a liquid mixture and an element comprising the same. [Background technology]

[0002] Regarding the separation of mixtures, there are various techniques for removing substances (e.g. salts) dissolved in a solvent (e.g. water). In recent years, the use of membrane separation methods as an energy- and resource-saving process has expanded.

[0003] Membranes used in membrane separation methods include microfiltration membranes, ultrafiltration membranes, nanofiltration membranes, reverse osmosis membranes, etc. These membranes are used, for example, to obtain drinking water from seawater, brackish water, water containing harmful substances, etc., to produce ultrapure water for industrial use, to treat wastewater, and to recover valuable materials.

[0004] Nanofiltration membranes and reverse osmosis membranes are generally made of composite semipermeable membranes having a nonwoven fabric substrate, a porous support layer thereon, and a separation functional layer containing crosslinked polyamide thereon. Patent Document 1 discloses a reverse osmosis filter module having a reverse osmosis membrane, a feed spacer, a tricot filtration channel, and a tube. In the reverse osmosis filter module, the reverse osmosis membrane, the feed spacer, and the tricot filtration channel are wrapped around the tube. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2019-514665 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the demand for decarbonization has increased, and recycling or reuse is required in various fields. The present invention aims to provide a composite semipermeable membrane containing recycled materials or an element (module) having the same. [Means for solving the problem]

[0007] The present invention for solving the above problems includes the following configurations. [1] A composite semipermeable membrane comprising a support membrane containing regenerated polysulfone and a separation functional layer. [2] The composite semipermeable membrane according to the above [1], wherein the support membrane has a substrate and a porous support layer containing recycled polysulfone. [3] The composite semipermeable membrane according to [1] or [2] above, wherein the support membrane has a porous support layer and a substrate containing at least one of recycled polyester and biopolyester. [4] A water collection pipe, a feed-side flow passage material, a permeation-side flow passage material, and the composite semipermeable membrane according to any one of [1] to [3] above, The feed-side passage material, the composite semipermeable membrane, and the permeate-side passage material are stacked and wrapped around the water collection pipe. element. [5] The element according to the above [4], wherein the permeate side flow passage material contains at least one of recycled polyester and biopolyester. Effect of the Invention

[0008] Since the composite semipermeable membrane and element of the present invention contain recycled polysulfone, it is possible to reduce CO2 emissions. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a composite semipermeable membrane. [Diagram 2] FIG. 2 is a partially developed perspective view showing an example of a spiral separation membrane element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described in detail.

[0011] In this specification, "mass" is synonymous with "weight." In addition, in this specification, "to" means that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0012] 1.Composite semipermeable membrane The composite semipermeable membrane 1 described below comprises a support membrane and a separation functional layer located on the support membrane.

[0013] (Support membrane) The support membrane supports the separating functional layer 12 and imparts physical strength to the composite semipermeable membrane 1. The support membrane contains at least regenerated polysulfone.

[0014] The support membrane may include a substrate 14 and a porous support layer 13, as shown in Figure 1. The substrate 14 preferably includes at least one of recycled polyester and biopolyester, and the porous support layer 13 preferably includes recycled polysulfone.

[0015] (base material) As the substrate 14, it is preferable to use a fibrous substrate in terms of strength, roughness forming ability, and fluid permeability.

[0016] As the substrate 14, either a long fiber nonwoven fabric or a short fiber nonwoven fabric can be preferably used.

[0017] The substrate 14 preferably contains at least one of polyolefin, polyester, and cellulose. Polyolefin and polyester are preferred because they are highly effective at retaining their shape against pressure and tension. The substrate preferably contains at least one of recycled polyester and biopolyester, as this can reduce the CO2 emissions associated with the production of the substrate.

[0018] (porous support layer) The porous support layer 13 serves as a base for forming a separation functional layer, and does not itself have substantial separation performance for ions, etc.

[0019] The size and distribution of the pores in the porous support layer 13 are not particularly limited, but a porous support layer having, for example, uniform and fine pores, or gradually larger fine pores from the surface on which the separation functional layer is formed to the other surface, and in which the size of the fine pores on the surface on which the separation functional layer is formed is 0.1 nm or more and 100 nm or less, is preferred.

[0020] The porous support layer 13 can be obtained by casting a solution containing a polymer onto a substrate.

[0021] The porous support layer 13 preferably contains polysulfone, which has high chemical, mechanical and thermal stability and is easy to mold.

[0022] A solution of polysulfone in N,N-dimethylformamide (hereinafter referred to as DMF) is cast to a certain thickness onto tightly woven polyester cloth or polyester nonwoven fabric, and then wet-coagulated in water to obtain a support membrane with most of its surface having fine pores with diameters of several tens of nanometers or less.

[0023] The thickness of the porous support layer 13 affects the strength of the composite semipermeable membrane obtained and the packing density when it is made into an element. In order to obtain sufficient mechanical strength and packing density, the thickness of the support membrane is preferably in the range of 30 μm to 300 μm, more preferably in the range of 100 μm to 220 μm.

[0024] The morphology of the porous support layer 13 can be observed by a scanning electron microscope, a transmission electron microscope, or an atomic force microscope. For example, when observing by a scanning electron microscope, the porous support layer is peeled off from the substrate, and then cut by freeze fracturing to obtain a sample for cross-sectional observation. This sample is thinly coated with platinum, platinum-palladium, or ruthenium tetrachloride, preferably ruthenium tetrachloride, and observed by a high-resolution field emission scanning electron microscope (UHR-FE-SEM) at an accelerating voltage of 3 to 15 kV. As the high-resolution field emission scanning electron microscope, an S-900 type electron microscope manufactured by Hitachi, Ltd., or the like, can be used.

[0025] The thickness of the porous support layer 13 is preferably in the range of 20 μm to 100 μm. When the thickness of the porous support layer is 20 μm or more, good pressure resistance can be obtained and a uniform support membrane without defects can be obtained, so that a composite semipermeable membrane including such a porous support layer can exhibit good salt removal performance. If the thickness of the porous support layer exceeds 100 μm, the amount of unreacted substances remaining during production increases, which may reduce the amount of permeated water and reduce chemical resistance.

[0026] (Recycled polyester) Recycled polyester refers to polyester that is remanufactured by collecting used PET bottles, films, fibers, etc., cleaning, crushing, and flaking them, and using them as raw materials. Depending on the raw materials and process used for recycling, using recycled polyester can reduce CO2 emissions by 40 to 50% compared to non-recycled polyester.

[0027] (Biopolyester) Biopolyester refers to polyester made from raw materials that contain biomass (renewable organic resources derived from living organisms and not fossil resources). Polyester is produced by polymerizing terephthalic acid, which is produced from paraxylene, and ethylene glycol. Depending on the percentage of bio-based raw materials and the process, the use of biopolyester can reduce CO2 emissions by 25-60% compared to non-biopolyester.

[0028] (separation functional layer) Among the components of the composite semipermeable membrane 1, it is the separating functional layer 12 that substantially has the ability to separate solutes.

[0029] A polyamide separation functional layer formed by polycondensing a polyfunctional amine and a polyfunctional acid halide, an organic-inorganic hybrid functional layer, etc., is preferably used as the separation functional layer 12, because of its excellent performance in separating components in the raw fluid. These separation functional layers can be formed by polycondensing a monomer on a porous support layer.

[0030] The separation functional layer 12 preferably contains a polyamide. The polyamide is formed by interfacial polycondensation of a polyfunctional amine and a polyfunctional acid halide on a support membrane (on the porous support layer 13 if the support membrane includes the porous support layer 13) by a known method. For example, a polyfunctional amine aqueous solution is applied to the porous support layer, the excess amine aqueous solution is removed with an air knife or the like, and then an organic solvent solution containing a polyfunctional acid halide is applied to produce the polyamide.

[0031] The separation functional layer 12 may have an organic-inorganic hybrid structure containing an Si element, etc. The separation functional layer 12 having an organic-inorganic hybrid structure may be, for example, the following compounds (A) and (B): (A) a silicon compound in which a reactive group having an ethylenically unsaturated group and a hydrolyzable group are directly bonded to a silicon atom, and (B) A compound other than the compound (A) having an ethylenically unsaturated group Specifically, the separation functional layer may contain a condensate of the hydrolyzable group of the compound (A) and a polymer of the ethylenically unsaturated group of the compound (A) and / or (B). That is, the separation functional layer may contain A polymer formed by condensation and / or polymerization of only compound (A), Polymers formed by polymerization of only compound (B), and Copolymer of compound (A) and compound (B) The copolymer may contain at least one polymer selected from the group consisting of the following. The polymer includes a condensation product. In the copolymer of the compound (A) and the compound (B), the compound (A) may be condensed via a hydrolyzable group.

[0032] The hybrid structure can be formed by a known method. An example of the method for forming the hybrid structure is as follows. A reaction liquid containing compound (A) and compound (B) is applied to a porous support layer. After removing excess reaction liquid, a heat treatment may be performed to condense the hydrolyzable groups. The ethylenically unsaturated groups of compound (A) and compound (B) may be polymerized by heat treatment, electromagnetic wave irradiation, electron beam irradiation, or plasma irradiation. In order to increase the polymerization rate, a polymerization initiator, a polymerization promoter, etc. may be added when forming the separation functional layer.

[0033] In addition, for any of the separation functional layers, the surface of the membrane may be hydrophilized, for example, with an alcohol-containing aqueous solution or an alkaline aqueous solution, before use.

[0034] 2.Separation membrane element (overview) Separation membrane elements come in various shapes, but they have in common that raw water is supplied to one side of the separation membrane and permeated fluid is obtained from the other side. Separation membrane elements are formed with many bundled separation membranes to increase the membrane area per separation membrane element, that is, to increase the amount of permeated fluid obtained per separation membrane element. Various shapes of separation membrane elements have been proposed depending on the application and purpose, such as spiral type, hollow fiber type, plate-and-frame type, rotating flat membrane type, and flat membrane integrated type.

[0035] For example, a spiral separation membrane element is widely used for reverse osmosis filtration. The spiral separation membrane element includes a water collection pipe and a separation membrane unit wound around the water collection pipe. The separation membrane unit is formed by stacking a feed-side flow path material that supplies raw water (i.e., water to be treated) as feed water to the separation membrane surface, a separation membrane that separates components contained in the raw water, and a permeation-side flow path material that guides the permeated fluid that has permeated the separation membrane and been separated from the feed-side fluid to the water collection pipe. The spiral separation membrane element is preferably used because it can apply pressure to the raw water and therefore can extract a large amount of permeated fluid. A spiral-type separation membrane element using a composite semipermeable membrane includes at least a water collection pipe, a separation membrane, a feed-side flow path material, and a permeate-side flow path material.

[0036] In the spiral separation membrane element 5 shown in FIG. 2, a polymer net is used as the feed-side flow passage material 2 that forms the flow passage on the feed side. In addition, a tricot with a finer spacing than the feed-side flow passage material 2 is used as the permeation-side flow passage material 4 in order to prevent the composite semipermeable membrane 1 from sagging and to form the flow passage on the permeation side. The permeation-side flow passage material 4 and the composite semipermeable membrane 1 that is superimposed on both sides of the permeation-side flow passage material 4 and adhered in an envelope-like manner form an envelope-like membrane 3. The inside of the envelope-like membrane 5 constitutes the permeation-side flow passage. The envelope-like membrane 5 that is alternately laminated with the feed-side flow passage material 2 has a predetermined portion on the opening side adhered to the outer circumferential surface of the water collection tube 6 and is spirally wound. The direction of the x-axis shown in FIG. 1 is the longitudinal direction of the water collection tube 6. The direction of the y-axis is perpendicular to the longitudinal direction of the water collection tube 6.

[0037] (Supply side channel material) The feed-side channel material is used to secure a channel for the feed water and to disturb the feed water. The shape of the feed-side channel material is not particularly limited, and may have a continuous shape or a discontinuous shape. Examples of channel materials having a continuous shape include materials such as films and nets. Here, the continuous shape means that the channel material is substantially continuous over the entire range. The continuous shape may include a portion where the channel material is discontinuous to the extent that no problems such as a decrease in the amount of water produced are caused. The material of the feed-side channel material is not particularly limited, and may be the same material as the separation membrane or a different material.

[0038] (Permeate side channel material) In the envelope-shaped membrane 5, the separation membranes 3 are stacked with their permeate side surfaces facing each other, and a permeate-side channel material 4 is disposed between the separation membranes 3, forming a permeate-side channel. The material of the permeate-side channel material is not limited, and tricot, nonwoven fabric, a porous sheet with protrusions attached, a film with a concave-convex shape and perforations, and a concave-convex nonwoven fabric can be used. In addition, protrusions that function as the permeate-side channel material may be attached to the permeate side of the separation membrane.

[0039] The material of the polymer that is the material of the permeate side flow passage material is not particularly limited as long as it maintains the shape of the permeate side flow passage material and causes little elution of components into the permeate water, and examples thereof include polyamides such as nylon, polyesters, polyacrylonitriles, polyolefins such as polyethylene and polypropylene, polyvinyl chloride, polyvinylidene chloride, polyfluoroethylene, and other synthetic resins, but polyolefins and polyesters are preferred in terms of strength that can withstand high pressures and hydrophilicity, and polyesters are particularly preferred. Furthermore, from the viewpoint of CO2 emissions, it is more preferred to use recycled polyesters or biopolyesters.

[0040] When the sheet-like material is composed of a plurality of fibers, the fibers may have, for example, a polypropylene / polyethylene core-sheath structure.

[0041] 3. Method for regenerating polysulfone in the support membrane A method for reusing polysulfone in a support membrane will be described below. In the following method, a used composite semipermeable membrane may be used, or a support membrane before a separation functional layer is formed, or a composite semipermeable membrane that is out of specification and has not been used may be used.

[0042] (Cleaning process) Since organic or inorganic impurities contained in the raw water are attached to the used composite semipermeable membrane, it is preferable to wash it with an acid or an alkali. As the acid, inorganic acids such as dilute hydrochloric acid, dilute sulfuric acid, phosphoric acid, nitric acid, and sodium hydrogen sulfite, and organic acids such as an aqueous oxalic acid solution and an aqueous citric acid solution can be used alone or in a mixture of two or more. As the alkali, an aqueous sodium hydroxide solution, an aqueous sodium hypochlorite solution, and an aqueous sodium carbonate solution can be used alone or in a mixture of two or more. For washing, a method of immersing the composite semipermeable membrane in an aqueous acid or alkali solution alone or alternately for a certain period of time, or a method of circulating an acid or alkali within the separation membrane element can be used.

[0043] In order to improve the cleaning efficiency, the chemical cleaning may be combined with physical cleaning such as backflow cleaning using a pump or air cleaning using a blower.

[0044] Since the support membrane or unused composite semipermeable membrane may contain impurities such as organic solvents, it is preferable to wash the membrane with a water-soluble organic solvent and then rinse the membrane with water.

[0045] (Process for removing the substrate) When the support membrane includes a substrate and a porous support layer, the substrate and the porous support layer (which may be a laminate of a separation functional layer and a porous support layer) are separated to isolate the porous support layer. Specifically, the substrate may be peeled off from the porous support layer, or the porous support layer (which may be a laminate with a separation functional layer) may be ground to separate it from the substrate. Grinding may be performed using a grinder, a sander, a blaster, or the like. Peeling is particularly preferred because it can remove the substrate efficiently while suppressing noise, odor, and dust in a shorter time than grinding.

[0046] The peeling can be performed by supplying a high-pressure fluid to the permeable side of the composite semipermeable membrane (the surface of the separation functional layer in the composite semipermeable membrane, or the surface of the support membrane facing the porous support layer), or by peeling the interface between the substrate and the porous support layer manually or using a film peeling device, or by using a combination of these methods.

[0047] Furthermore, the step of removing the substrate contained in the composite semipermeable membrane may be carried out either before or after the step of removing the separating functional layer from the composite semipermeable membrane, which will be described later.

[0048] (Step of removing the separation functional layer) To isolate the porous support layer from the composite semipermeable membrane, a step of removing the separation functional layer from the laminate of the porous support layer and the separation functional layer is carried out. As a removal method, a method of disassembling the separation functional layer or a method of removing the separation functional layer from the porous support layer by grinding can be used. The specific grinding method is as described above. Disassembly can remove the separation functional layer more easily and efficiently than grinding.

[0049] The decomposition can be performed by contacting the separation functional layer with a chemical that decomposes the separation functional layer but does not decompose the porous support layer, by decomposing the separation functional layer by plasma treatment, or by depolymerization using subcritical water. However, decomposition of the separation functional layer with a chemical is particularly preferred because it can be performed in a short time and at low cost.

[0050] As for the chemicals used for decomposing the separation functional layer, in the case where the separation functional layer is a polyamide separation functional layer formed by polycondensation of a polyfunctional amine and a polyfunctional acid halide, a chemical capable of oxidatively decomposing an amide bond is preferable, and for example, a chlorine-based chemical such as an aqueous sodium hypochlorite solution or an aqueous calcium hypochlorite solution, or an alkaline chemical such as hydrogen peroxide or sodium hydroxide can be used, and these can be used alone or as a mixture of two or more kinds. Among them, the method of removing the separation functional layer by the chlorine decomposition method using an aqueous sodium hypochlorite solution or an aqueous calcium hypochlorite solution is preferable because it is possible to remove the separation functional layer most simply and efficiently while suppressing chemical changes in the polysulfone to be regenerated.

[0051] The method of measuring the presence or absence of chemical changes in polysulfone can be performed by molecular weight distribution measurement, elemental analysis, melting point measurement, differential scanning calorimetry, heat weight loss analysis, nuclear magnetic resonance spectroscopy, infrared spectroscopy, ultraviolet spectroscopy, etc., but it can also be confirmed by processing the recycled polysulfone resin into its original shape and comparing its physical properties before and after the regeneration process. However, no matter which method is used, measurement errors will occur, so in analyses such as molecular weight distribution measurement, elemental analysis, melting point measurement, differential scanning calorimetry, heat weight loss analysis, nuclear magnetic resonance spectroscopy, infrared spectroscopy, and ultraviolet spectroscopy, the error is within 5%, and in the case of processing the recycled polysulfone resin into its original shape and comparing its physical properties before and after the regeneration process, an error of about 10% can be considered to be no chemical change.

[0052] As the pH of the chlorine-based aqueous solution used becomes more acidic, the proportion of the active species, hypochlorous acid, increases and the decomposition efficiency of the separation functional layer increases; however, at the same time, there is a higher risk of promoting corrosion of piping and equipment. Therefore, the pH is preferably in the range of 6.0 to 9.0, and more preferably in the range of 6.5 to 7.5.

[0053] The effective chlorine concentration of the chlorine-based aqueous solution used is preferably in the range of 1% to 15%, more preferably in the range of 3 to 10%, which allows efficient decomposition of the separating functional layer while suppressing decomposition of the chemical itself.

[0054] The higher the temperature of the chlorine-based aqueous solution used, the higher the decomposition efficiency. However, if the temperature is too high, gas will be generated or the decomposition of the chemical itself will be accelerated, making it difficult to control the concentration. Therefore, the temperature is preferably in the range of 10°C to 60°C, and more preferably in the range of 20°C to 40°C.

[0055] The decomposition of the separation functional layer with chemicals can be achieved by a method of immersing the composite semipermeable membrane obtained by disassembling the separation membrane element in an aqueous solution of a chlorine-based chemical for a certain period of time, by continuously or intermittently applying a chlorine-based aqueous solution to the surface of the composite semipermeable membrane, or by circulating an aqueous solution of a chlorine-based chemical within the separation membrane element to remove the separation functional layer.

[0056] The pH, available chlorine concentration, treatment temperature and treatment method of the above chlorine-based aqueous solution can be arbitrarily set depending on the degree of polymerization and thickness of the separating functional layer of the composite semipermeable membrane used.

[0057] (Process for crushing the porous support layer) In order to efficiently dissolve the polysulfone in the solvent, it is preferable to crush the isolated porous support layer before dissolving. A crusher or pulverizer such as a ball mill, a high-speed cutter mill, a roll crusher, a rotary cutter, or a hydraulic cutter is usually used to crush the porous support layer, but it is particularly preferable to use a crushing means such as a high-speed cutter mill, a rotary cutter, or a hydraulic cutter, since it can be crushed finely. In addition, it is preferable to dry the porous support layer to be crushed in advance, since it can be crushed more uniformly.

[0058] By dissolving the crushed particles in a solvent, a polysulfone solution can be obtained in a short period of time.

[0059] 4. Formation of a porous support layer containing recycled polysulfone An isolated porous support layer (i.e., regenerated polysulfone) can be used as at least a part of the resin forming the porous support layer. It is used by dissolving it in a solvent such as DMF, similar to the method for producing a porous support membrane.

[0060] As in the above-mentioned method for forming the porous support layer, the solvent for dissolving the regenerated polysulfone is exemplified by DMF. Since the polysulfone solution obtained by dissolving the regenerated polysulfone in a solvent may contain impurities, a substrate, and a part of the separation functional layer that were not completely removed in the isolation step of the porous support layer, it is preferable to carry out a purification step to remove these impurities. Centrifugation and / or filtration can be used to purify the polysulfone resin solution. Filtration, which can be inexpensive and continuously purified, is particularly preferable. The filter material used for filtration may be any filter material that is not affected by solvents such as DMF and can remove impurities remaining in the regenerated polysulfone resin solution, and may be a felt filter, a membrane filter, a glass filter, a metal mesh, or the like, used alone or in combination.

[0061] The purified regenerated polysulfone resin solution can be poured onto a substrate to a certain thickness and wet-coagulated in water to regenerate a porous support membrane, similar to the method for producing the porous support membrane described above.

[0062] As a method for forming a separation functional layer on a porous support layer containing recycled polysulfone, the above-mentioned method such as interfacial polymerization can be used.

[0063] 5. Use of composite semipermeable membranes The composite semipermeable membrane can be used in applications such as medical care, pharmaceutical production, food production, water treatment, etc. When used, the composite semipermeable membrane may be incorporated into a fluid separation device.

[0064] The fluid separation device includes one or more modules, and a pump or the like that supplies raw water to the modules. The module includes the above-mentioned elements connected in series or parallel, and a pressure vessel that houses the elements. The fluid separation device can separate the raw water into permeate and concentrated water.

[0065] The higher the operating pressure of the fluid separation device, the higher the salt rejection rate, but the more energy required for operation is required. Also, taking into consideration the durability of the composite semipermeable membrane, the operating pressure when the treated water is passed through the composite semipermeable membrane is preferably 0.1 MPa or more and 10 MPa or less. As the supply water temperature increases, the salt rejection rate decreases, but as the temperature decreases, the membrane permeation flux also decreases, so a temperature of 5°C or more and 45°C or less is preferable. In addition, as the pH of the supply water increases, there is a risk of magnesium scale formation in the case of supply water with a high salt concentration such as seawater, and there is also concern about membrane deterioration due to high pH operation, so operation in the neutral region is preferable.

[0066] Examples of raw water include seawater, brine, wastewater, and other liquid mixtures containing 500 mg / L to 100 g / L of TDS (Total Dissolved Solids) and 0.1 mg / L to 1000 mg / L of nonionic substances. Generally, TDS refers to the total dissolved solids content and is expressed as "weight / volume" or "weight ratio." By definition, it can be calculated from the weight of the residue left after evaporating a solution filtered through a 0.45 micron filter at a temperature of 39.5 to 40.5°C, but it is more convenient to convert it from the practical salinity (S). EXAMPLES

[0067] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0068] <Example> (Membrane desalination rate) Water to be evaluated, adjusted to a temperature of 25°C, pH of 7, and a sodium chloride concentration of 35,000 ppm, was supplied to the composite semipermeable membrane at an operating pressure of 5.5 MPa to perform membrane filtration. The electrical conductivity of the supply water and the permeated water was measured using an electrical conductivity meter manufactured by DKK-TOA Corporation to obtain the practical salinity, i.e., NaCl concentration, of each. The salt rejection rate was calculated based on the NaCl concentration thus obtained and the following formula. Here, the sodium chloride concentration (ppm) means the concentration based on mass.

[0069] Membrane salt rejection rate (%) = 100 × {1-(NaCl concentration in permeate water / NaCl concentration in feed water)} (membrane flux) In the test described above, the amount of water that permeates the membrane of the feed water (NaCl aqueous solution) is measured, and the value converted to the amount of water that permeates (cubic meters) per day per square meter of membrane surface is called the membrane permeation flux (m 3 / m 2 / day).

[0070] (Element salt rejection rate) Evaluation water adjusted to a temperature of 25°C, pH 7, and sodium chloride concentration of 35,000 ppm was supplied to the spiral separation membrane element at an operating pressure of 5.5 MPa to perform membrane filtration. The electrical conductivity of the supply water and the permeate was measured using an electrical conductivity meter manufactured by DKK-TOA Corporation to obtain the practical salinity, i.e., NaCl concentration, of each. The salt rejection rate was calculated based on the NaCl concentration thus obtained and the following formula. Here, sodium chloride concentration (ppm) refers to the concentration based on mass.

[0071] Element salt rejection rate (%) = 100 x {1 - (NaCl concentration in permeate water / NaCl concentration in feed water)} (Amount of water produced) In the test described above, the amount of permeated water was measured while the spiral-type separation membrane element was in operation, and the amount of permeated water (cubic meters) per day was calculated as the amount of water produced (m 3 The data are expressed as 100 mg / day.

[0072] (CO2 emissions) CO2 emissions were calculated based on the CO2 emission unit of each component's material and the amount of components used, taking into account CO2 emissions from electricity, steam, and water used.

[0073] (Preparation of recycled polysulfone) Dilute sulfuric acid adjusted to pH 1 was passed through the used spiral separation membrane element at room temperature (20°C), and the pump was stopped and the element was left to stand for 24 hours. The inside of the element was then rinsed with RO water, and an aqueous solution of sodium hydroxide adjusted to pH 14 was passed through and circulated at room temperature (20°C), after which the pump was stopped and the element was left to stand for 24 hours. The inside of the element was then rinsed with RO water to remove impurities adhering to the composite semipermeable membrane.

[0074] After washing, the filament windings and end plates of the separation membrane element were removed, and the composite semipermeable membrane was cut out from the separation membrane leaf so as to remove the adhesive portion. The cut composite semipermeable membrane was passed through a film peeling device to remove the substrate contained in the composite semipermeable membrane.

[0075] The composite semipermeable membrane with the substrate removed was immersed in an aqueous sodium hypochlorite solution with an available chlorine concentration of 5% adjusted to pH 7 for 24 hours at room temperature (20°C), and then rinsed with RO water to decompose and remove the polyamide separation functional layer.

[0076] The porous support layer from which the polyamide separation function layer had been decomposed and removed was dried and then pulverized with a high-speed cutter mill to obtain recycled polysulfone resin.

[0077] The ground regenerated polysulfone resin was then dissolved in 15.0% by weight of polysulfone in N,N-dimethylformamide (DMF), which was then filtered and purified using a 400-mesh SUS metal plain weave filter and a PTFE membrane filter with a pore size of 1 μm. 2 The purified regenerated polysulfone resin solution was cast at room temperature (25°C) to a thickness of 180 μm onto a 1000-milliliter roll of 10000 cc / sec, and then immediately immersed in pure water and left for 5 minutes to produce a roll of porous support membrane (thickness 130 μm) made of a fiber-reinforced polysulfone support membrane.

[0078] (Preparation of composite semipermeable membrane / spiral-type separation membrane element) The surface of the polysulfone layer of the porous support membrane was immersed in an aqueous solution containing 1.6% by mass of m-PDA and 1.0% by weight of ε-caprolactam for 2 minutes, then slowly pulled up vertically. Excess aqueous solution was removed from the surface of the support membrane by blowing nitrogen from an air nozzle.

[0079] Then, a n-decane solution containing 0.08% by mass of trimesoyl chloride was applied so that the surface of the membrane was completely wetted, and the membrane was left to stand for 1 minute. Excess solution was then removed from the membrane by air blowing, and the membrane was washed with hot water at 80°C for 1 minute to obtain a composite separation membrane roll. The separation membrane sheet was then cut and folded so that one side was open. Between the sheets, a net (thickness: 800 μm, pitch: 5 mm × 5 mm) was continuously laminated as a feed-side flow passage material. A urethane adhesive was applied to both ends of the perforated water collection pipe of the separation membrane sheet in the longitudinal direction, and the sheets were then stacked to form a spiral separation membrane element with an effective area of ​​36 m. 2 Twenty-six envelope-shaped membranes with a width of 930 mm were prepared so that the

[0080] Then, a predetermined portion of the opening side of the envelope-shaped membrane was attached to the outer periphery of a perforated water collection pipe, and further wound in a spiral shape to produce a wound body. After wrapping a film around the outer periphery of the wound body and fixing it with tape, the edges were cut, end plates were attached, and filament winding was performed to produce an 8-inch element.

[0081] Example 1 The composite semipermeable membrane was placed in a pressure cell and evaluated under the above-mentioned conditions, with the results shown in Table 1. In addition, the spiral-wound separation membrane element was placed in a pressure vessel and evaluated under the above-mentioned conditions, with the results shown in Table 1.

[0082] (Examples 2 to 7) A composite semipermeable membrane and a spiral-type separation membrane element were produced in the same manner as in Example 1, except that the members were as shown in Tables 1 and 2.

[0083] The composite semipermeable membrane was placed in a pressure cell and evaluated under the above-mentioned conditions, and the results are shown in Tables 1 and 2. In addition, the separation membrane element was placed in a pressure vessel and each performance was evaluated under the same conditions as in Example 1, and the results are shown in Tables 1 and 2.

[0084] Comparative Example 1 A composite semipermeable membrane and a spiral-type separation membrane element were produced in the same manner as in Example 1, except that the members were as shown in Table 2.

[0085] The composite semipermeable membrane was placed in a pressure cell and evaluated under the above-mentioned conditions, with the results shown in Table 2. In addition, the spiral-wound separation membrane element was placed in a pressure vessel and each performance was evaluated under the above-mentioned conditions, with the results shown in Table 2.

[0086] [Table 1]

[0087] [Table 2]

[0088] As is clear from the results shown in Tables 1 and 2, the composite semipermeable membranes and separation membrane elements of Examples 1 to 7 were able to reduce CO2 emissions while maintaining separation performance. [Industrial Applicability]

[0089] The composite semipermeable membrane and element of the present invention can be suitably used, in particular, for water purification or desalinization of brackish water or seawater.

[0090] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention. [Explanation of symbols]

[0091] 1 Composite semipermeable membrane 12 Separation functional layer 13 Porous support layer 14 Base material 2 Supply side channel material 3 Envelope membrane 4 Permeate side channel material 5 Spiral type separation membrane element 6 Water collection pipe 7 Supply water 8 Permeate water 9 Concentrated water

Claims

1. A composite semipermeable membrane comprising a support membrane containing regenerated polysulfone and a separation functional layer.

2. The support membrane has a substrate and a porous support layer comprising recycled polysulfone. The composite semipermeable membrane according to claim 1.

3. The support membrane has a porous support layer and a substrate comprising at least one of recycled polyester and biopolyester; The composite semipermeable membrane according to claim 1 or 2.

4. A water collection pipe, a feed-side flow path material, a permeation-side flow path material, and the composite semipermeable membrane according to any one of claims 1 to 3, The feed-side passage material, the composite semipermeable membrane, and the permeate-side passage material are stacked and wrapped around the water collection pipe. element.

5. The element according to claim 4 , wherein the permeate side flow path material contains at least one of recycled polyester and biopolyester.