Fire-resistant sheet, and construction method of building

The fire-resistant sheet with a thermoplastic resin and foamed intermediate layer thermally expands to form a fireproof layer, addressing the complexity and effectiveness of existing sheets, enhancing fire resistance and ease of installation.

JP2024152237APending Publication Date: 2024-10-25DAIWA HOUSE INDUSTRY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023066303
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing fire-resistant sheets have complex structures and do not effectively enhance the fire resistance of buildings.

Method used

A fire-resistant sheet composed of a first and second layer of non-combustible fibers dispersed in a thermoplastic resin, with an intermediate layer containing a foamed material and a carbonizing agent, which thermally expands to form a heat-insulating layer upon heating.

Benefits of technology

The sheet provides improved fire resistance with a simpler structure, easily installable and cost-effective, forming a robust fireproof layer that protects construction sites from flames.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152237000001_ABST
    Figure 2024152237000001_ABST
Patent Text Reader

Abstract

To provide a fire-resistant sheet which exhibits more favorable fire-resistance with a simple structure, and to provide a construction method of building using the fire-resistant sheet.SOLUTION: A fire-resistant sheet 10 includes: a first layer 11 and a second layer 12 constituted by dispersing incombustible fiber in thermoplastic resin; and an intermediate layer 20 constituted by dispersing a foam material in the thermoplastic resin and arranged between the first layer 11 and the second layer 12. The thickness of the fire-resistant sheet 10 is equal to or greater than 0.5 mm and equal to or less than 5 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fire-resistant sheet and a method for constructing a building. [Background technology]

[0002] A method for improving the fire resistance of a building includes a method of using a fire-resistant covering material. In addition, a fire-resistant sheet may be used as the covering material from the viewpoint of ease of fire-resistant construction. For example, the fire-resistant sheet described in Patent Document 1 is a foamed fire-resistant sheet mainly composed of a synthetic resin with a glass transition temperature of -20 to 20°C, which is flexible and can be easily attached to the construction site of the building by applying an adhesive. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-100879 A Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, there is a demand for fire-resistant sheets that can more effectively improve the fire resistance of buildings while having a simpler structure.

[0005] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a fire-resistant sheet that has a simpler structure and exhibits better fire resistance. Another object of the present invention is to provide a method for constructing a building using the above-mentioned fire-resistant sheet. [Means for solving the problem]

[0006] In order to achieve the above object, the fire-resistant sheet of the present invention has the following configuration. [1] A fire-resistant sheet comprising: a first layer and a second layer formed by dispersing non-flammable fibers or flame-retardant fibers in a thermoplastic resin; and an intermediate layer formed by dispersing a foamed material in a thermoplastic resin and disposed between the first and second layers; and a thickness of the fire-resistant sheet of 0.5 mm or more and 5 mm or less. [2] The fire-resistant sheet according to [1], wherein the intermediate layer has a layer formed by dispersing a foamed material containing a carbonizing agent in a thermoplastic resin. [3] A fire-resistant sheet according to [1] or [2], wherein the intermediate layer has a layer formed by dispersing a foamed material consisting of a mixture of starch and sodium bicarbonate in a thermoplastic resin. [4] The fire-resistant sheet according to any one of [1] to [3], wherein the intermediate layer has a layer formed by dispersing a foaming material containing a foaming agent in a thermoplastic resin. [5] The fire-resistant sheet according to any one of [1] to [4], wherein the intermediate layer has a layer formed by dispersing a foamed material containing unfoamed vermiculite in a thermoplastic resin. [6] The fire-resistant sheet according to any one of [1] to [5], wherein the intermediate layer is formed by dispersing nonflammable fibers or flame-retardant fibers and a foaming material in a thermoplastic resin. [7] The fire-resistant sheet according to any one of [1] to [6], wherein the intermediate layer has a plurality of layers laminated in the thickness direction of the fire-resistant sheet, and each of the plurality of layers has a different foaming initiation temperature. [8] The fire-resistant sheet according to [7], wherein the multiple layers are laminated in an order according to the foaming initiation temperature. [9] A fire-resistant sheet as described in [8], wherein when the fire-resistant sheet is installed, the second layer is attached to the construction site of the building, and the multiple layers are stacked so that the layer having the lower foaming initiation temperature is positioned closer to the first layer.

[0007] The building construction method of the present invention has the following configuration.

[10] A method for constructing a building, comprising attaching the fire-resistant sheet according to any one of [1] to [9] above to a part of the building to be made fire-resistant. Effect of the Invention

[0008] According to the present invention, a fire-resistant sheet having a simpler structure and better fire resistance is provided. In addition, by using the fire-resistant sheet in a building construction project, a good fire-resistant structure can be easily constructed in a target location in the building. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a cross-sectional view of a fire-resistant sheet. [Diagram 2] FIG. 2 is a cross-sectional view of a laminate constituting a fire-resistant sheet, showing the laminate before compression. [Diagram 3] 1 shows the state of a fire-resistant sheet used in an embodiment of the present invention before heating. [Figure 4] 3 shows the state of the fire-resistant sheet used in the examples of the present invention after heating. [Diagram 5] FIG. 13 is a diagram showing test results of an example of the present invention. [Figure 6] FIG. 13 is a diagram showing test results of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The fire-resistant sheet of the present invention and its method of use will be described below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0011] [Application examples of fire-resistant sheets] The fire-resistant sheet of the present invention is used, for example, for the purpose of improving fire resistance in structures such as buildings, specifically for the purpose of meeting the standards for fire-resistant structures (specifically, fire-resistant structures, semi-fire-resistant structures, or fire-prevention structures) stipulated by laws and regulations. Specifically, the fire-resistant sheet is applied to walls, columns, floors, beams, roofs, and the like of buildings and the like to cover the application area. A fire-resistant structure is constructed by covering the application area with the fire-resistant sheet. The application area may be a part made of metal such as steel, or a part made of wood or resin material.

[0012] The method of attaching the fire-resistant sheet to the application site is not particularly limited, but for example, an adhesive may be applied to the application site to form an adhesive layer, and the fire-resistant sheet may be attached to the application site via the adhesive layer. Alternatively, the fire-resistant sheet itself may have an adhesive layer on its back surface, and the back surface may be abutted against the application site to adhere to the application site.

[0013] [Example of fireproof sheet composition] The fire-resistant sheet of the present invention is a sheet body in which a first layer, an intermediate layer, and a second layer are laminated in this order, and is flexible and foldable, and expands in the thickness direction when heated (i.e., has thermal expansion). The fire-resistant sheet of the present invention is compressed in the thickness direction before thermal expansion, specifically, compressed until the thickness of the sheet becomes about 1 / 20 to 1 / 10 of the thickness before compression. As a result, the thickness of the fire-resistant sheet of the present invention is 0.5 mm or more and 5 mm or less.

[0014] That is, the fire-resistant sheet of the present invention is attached to the application site with the first layer, intermediate layer, and second layer each in a compressed state. When the fire-resistant sheet is placed in a high-temperature environment and heated due to a fire or the like, the first layer, intermediate layer, and second layer each thermally expand and are fixed, thereby exerting the fire-resistant performance of the fire-resistant sheet.

[0015] Each layer contained in the fire-resistant sheet of the present invention will now be described. (1st and 2nd layers) The first and second layers are each composed of non-combustible fibers dispersed in a thermoplastic resin, the first layer being placed on the front side (exposed side) of the fire-resistant sheet, and the second layer being placed on the back side (opposite the application area) of the fire-resistant sheet, and are attached to the application area when in use. In each of the first and second layers, the non-combustible fibers are compressed and bound by a binder made of a thermoplastic resin material.

[0016] When the first and second layers are heated during a fire and the temperature of the first or second layer reaches or exceeds a predetermined temperature, the thermoplastic resin binder in that layer softens, releasing the noncombustible fibers that were compressed and restraining them, and the layer expands to its pre-compression thickness. The thickness of the first layer and the second layer (strictly speaking, the thickness in a compressed state) may be the same or different.

[0017] Examples of non-combustible fibers include mineral fibers such as basalt fiber, rock wool, slag wool, glass wool, alumina fiber, silica fiber, glass fiber, silica alumina fiber, metal fibers such as stainless steel fiber and steel wool, and carbon fibers.

[0018] The thermoplastic resin easily imparts flexibility (shapeability) to the first and second layers, which can improve the handleability and ease of application of the entire fire-resistant sheet including the first and second layers. The proportion of the thermoplastic resin in the first and second layers is preferably 0.2% by mass to 50% by mass, more preferably 0.2% by mass to 40% by mass, and particularly preferably 0.2% by mass to 35% by mass, based on the weight of each layer.

[0019] The thermoplastic resin contains at least one component selected from the group consisting of, for example, polyethylene resin, ethylene-vinyl acetate copolymer resin (EVA resin), acrylic resin, polyvinyl chloride resin (PVC resin), etc. Among these, acrylic resin is particularly preferable. The acrylic resin is, for example, a polymer of a monomer component including a (meth)acrylic acid alkyl ester monomer. In this specification, the (meth)acrylic acid alkyl ester means an acrylic acid alkyl ester or a methacrylic acid alkyl ester. The same applies to other similar terms. The (meth)acrylic acid alkyl ester monomer is an ester of (meth)acrylic acid and an aliphatic alcohol, and the number of carbon atoms in the alkyl group of the aliphatic alcohol is, for example, 1 to 18, preferably 1 to 14, more preferably 1 to 10, and even more preferably 1 to 8.

[0020] Specific examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, and tetradecyl (meth)acrylate. The (meth)acrylic acid alkyl ester monomers may be used alone or in combination of two or more kinds. Furthermore, the monomer component for obtaining the acrylic resin may contain a polar group-containing monomer in addition to the above-mentioned (meth)acrylic acid alkyl ester monomer. Examples of polar group-containing monomers include carboxylic acids containing a vinyl group, such as (meth)acrylic acid and itaconic acid; vinyl monomers having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified (meth)acrylate, polyoxyethylene (meth)acrylate, and polyoxypropylene (meth)acrylate; and nitrogen-containing vinyl monomers, such as (meth)acrylonitrile, N-vinylpyrrolidone, N-vinylcaprolactam, N-vinyllaurylolactam, (meth)acryloylmorpholine, (meth)acrylamide, dimethyl(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, and dimethylaminomethyl(meth)acrylate.

[0021] The glass transition temperature (Tg) of the acrylic resin is preferably 5 to 80° C. By setting the glass transition temperature (Tg) within this range, it is possible to impart a certain level of mechanical strength to the fire-resistant sheet while improving moldability, flexibility, etc. From these viewpoints, the glass transition temperature (Tg) of the acrylic resin is more preferably 15 to 70° C., and particularly preferably 25 to 60° C. The glass transition temperature (Tg) of the acrylic resin can be adjusted by appropriately selecting the type or amount of the monomer component used. The glass transition temperature (Tg) of the acrylic resin can be measured, for example, by a differential scanning calorimeter (DSC).

[0022] The acrylic resin is preferably a polymer of a (meth)acrylic acid alkyl ester monomer. Specifically, a polymer of a (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 14 carbon atoms is preferred, a polymer of a (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 10 carbon atoms is more preferred, and a polymer of a (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 8 carbon atoms is particularly preferred. The acrylic resin may be a homopolymer of a (meth)acrylic acid alkyl ester monomer, or a copolymer of two or more kinds of (meth)acrylic acid alkyl ester monomers. Specific examples of suitable acrylic resins include a homopolymer of isobutyl methacrylate, a copolymer of isobutyl methacrylate and methyl methacrylate, and the like. The acrylic resin may be used alone or in combination of two or more kinds.

[0023] The weight average molecular weight of the acrylic resin is preferably 10,000 to 300,000 from the viewpoints of enabling the fire-resistant additive and the like to be appropriately dispersed in the first or second layer and improving moldability and mechanical strength, and from these viewpoints, the weight average molecular weight of the acrylic resin is more preferably 30,000 to 250,000, and particularly preferably 60,000 to 200,000. The weight average molecular weight of the acrylic resin is a weight average molecular weight measured by gel permeation chromatography (GPC) in terms of standard polystyrene. Examples of columns used for measuring the weight average molecular weight by the GPC method include Shodex LF-804 (manufactured by Showa Denko KK).

[0024] (Middle class) The intermediate layer is made by dispersing a foaming material in a thermoplastic resin, and is disposed between the first and second layers. The intermediate layer has thermal expansion properties, and when heated in the event of a fire, the foaming material foams and solidifies to form a heat insulating foaming layer (fireproof layer, carbonized layer).

[0025] The thermoplastic resin plays a role as a binder in the intermediate layer, and contains at least one component selected from the group consisting of polyethylene resin, ethylene vinyl acetate copolymer resin (EVA resin), acrylic resin, polyvinyl chloride resin (PVC resin), etc. Among these, acrylic resin is particularly preferable. The type, glass transition temperature (Tg), weight average molecular weight, and preferred aspects of the acrylic resin are the same as those described for the first layer and the second layer.

[0026] The foam material can be one that expands upon heating to form a porous carbonized layer, and contains one or both of a carbonizing agent and a foaming agent (ie, a mixture of a carbonizing agent and a foaming agent). The carbonizing agent is a component that is carbonized (dehydrated and carbonized) by heating to form the skeleton of the porous structure in the porous carbonized layer. Examples of the carbonizing agent that can be used include polyhydric alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, and polypentaerythritol, polysaccharides, starches such as cornstarch, and substances formed only from carbon, oxygen, and hydrogen, such as expandable graphite.

[0027] The foaming agent has a component that is decomposed or vaporized by heating to generate a non-flammable gas. When the foaming agent is used together with the carbonizing agent, the foaming agent foams the carbonized layer formed by the carbonizing agent with the non-flammable gas derived from the foaming agent, and the carbonized layer has a porous structure. When the foaming agent is dispersed in the binder (thermoplastic resin), the foaming agent foams the binder layer to make the binder layer have a porous structure. The foaming agent is preferably a flame-retardant foaming agent, and phosphates such as ammonium phosphate, ammonium polyphosphate, melamine phosphate, melamine polyphosphate, aluminum polyphosphate, and magnesium polyphosphate phosphate are preferably used as the flame-retardant foaming agent. In addition, sulfamates (such as ammonium sulfamate), carbonates such as sodium hydrogen carbonate, borates (such as ammonium borate), and the like can also be used as the flame-retardant foaming agent.

[0028] The content of the foaming agent in the intermediate layer (more precisely, in each of the layers constituting the intermediate layer) is preferably 0.5 mol to 20.0 mol per mol of the carbonizing agent. When this ratio is 0.5 mol or more, there is an advantage that the carbonized layer and the incinerated layer are particularly easily formed. When this ratio is 20.0 mol or less, there is an advantage that the moldability of the fireproof material is improved. The content of the foaming agent is more preferably 0.5 mol to 10.0 mol per mol of the carbonizing agent, and particularly preferably 1 mol to 4 mol per mol of the carbonizing agent.

[0029] The foaming material may be a material that expands (foams) by itself when heated to form a porous structure, i.e., an expanding agent. Examples of such materials include unexpanded vermiculite, expandable graphite, and expandable sodium silicate.

[0030] A preferred configuration for the intermediate layer is that the intermediate layer is configured by dispersing the foaming material together with non-combustible fibers in a thermoplastic resin (binder) in order to uniformly foam the foaming material in the intermediate layer. The types of non-combustible fibers that can be used for the intermediate layer are the same as those described above for the first and second layers.

[0031] The intermediate layer may be composed of a plurality of layers laminated in the thickness direction of the fire-resistant sheet. In this case, each of the plurality of layers corresponds to one of the following four layers. A layer made by dispersing foam material containing a carbonizing agent in a thermoplastic resin. A layer made by dispersing foaming material containing a foaming agent in a thermoplastic resin. A layer made by dispersing a foam material consisting of a mixture of a carbonizing agent and a foaming agent in a thermoplastic resin. A layer made by dispersing foam material, which expands when heated and forms a porous structure, in a thermoplastic resin.

[0032] The number of layers constituting the intermediate layer is not particularly limited and may be any number. The thickness of each of the layers constituting the intermediate layer (strictly speaking, the thickness in a compressed state) may be uniform among the layers, or may be different among the layers. Which of the above four layers is to be included in the intermediate layer should be determined according to the application of the fire-resistant sheet, for example, the material of the application area. For example, when attaching a fire-resistant sheet to a metal member, the amount of moisture generated from the metal member is very small, so it is better not to include a layer made of a foamed material containing starch, which requires moisture to form a carbonized layer, in the intermediate layer.

[0033] Moreover, it is preferable that the foaming start temperatures of the multiple layers constituting the intermediate layer are different from each other. It is also preferable that the multiple layers are laminated in an order according to the foaming start temperatures. Specifically, in a configuration in which the second layer is attached to the construction site of the building when the fire-resistant sheet is installed, it is preferable that the multiple layers are laminated such that the layer with the lower foaming start temperature is located closer to the first layer. In other words, it is preferable that the multiple layers are laminated in the intermediate layer so that the foaming start temperature becomes higher toward the inside (the construction site side).

[0034] The foaming start temperature is the temperature at which volume expansion (i.e. foaming) begins to occur when the temperature of each layer constituting the intermediate layer is raised from room temperature. The method for measuring the foaming start temperature is not particularly limited, but for example, a sample piece having the same composition as each layer constituting the intermediate layer is heated, and the state is observed visually or otherwise to confirm the temperature at which the sample piece begins to expand, and the temperature at that point may be taken as the foaming start temperature. Alternatively, a sheet having the same composition as each layer constituting the intermediate layer is heated, and the normal force applied from the sheet is measured using a device such as a rheometer (TA Instruments, Discovery HR-2), and the temperature at the point at which the normal force begins to rise may be taken as the foaming start temperature. The foaming initiation temperature of each layer can be adjusted by changing the type of foaming material contained in each layer and the content of the foaming material in each layer.

[0035] The fire-resistant sheet of the present invention may have at least the above-mentioned first layer, intermediate layer, and second layer, and may further have a layer other than these (i.e., a third layer). For example, the third layer may be provided between the first layer and the intermediate layer, or between the second layer and the intermediate layer, or the third layer may be provided on the outside of the first layer or the second layer.

[0036] [Example of the configuration of the fire-resistant sheet according to one embodiment of the present invention] Next, a specific embodiment of the present invention (hereinafter, this embodiment) will be described with reference to the drawings, showing an example of the configuration of a fire-resistant sheet. However, the specific embodiment described below is merely an example for facilitating understanding of the present invention, and does not limit the present invention. In other words, the present invention may be modified or improved without departing from the spirit of the present invention. In addition, the present invention naturally includes its equivalents.

[0037] The fire-resistant sheet according to this embodiment (hereinafter, fire-resistant sheet 10) has a first layer 11 constituting the sheet surface and a second layer 12 constituting the sheet back surface, as shown in Fig. 1. The first layer 11 and the second layer 12 are each formed by dispersing sheet-shaped glass wool or rock wool (e.g., glass fiber) in a thermoplastic resin such as an acrylic resin and binding it.

[0038] Between the first layer 11 and the second layer 12, an intermediate layer 13 is interposed, which is composed of a plurality of layers laminated in the thickness direction of the fireproof sheet 10. In the intermediate layer 31, as shown in FIG. 1, the first intermediate layer 21, the second intermediate layer 22, and the third intermediate layer 23 are arranged in this order from the first layer 11 side. The first intermediate layer 21 is formed by dispersing a foaming material containing a foaming agent and a carbonizing agent, specifically, a foaming material consisting of a mixture of starch and sodium bicarbonate, together with glass wool in acrylic. The second intermediate layer 22 is formed by dispersing a foaming material containing expandable graphite or ammonium polyphosphate as a foaming agent together with glass wool in acrylic resin. The third intermediate layer 23 is formed by dispersing a foaming material containing unfoamed vermiculite together with glass wool in acrylic resin. The configuration of the first intermediate layer 21, that is, the configuration containing a mixture of starch and sodium bicarbonate as a foaming material, is effective when the application site of the fire-resistant sheet 10 is made of a material that generates moisture when heated, such as wood. On the other hand, when the application site is made of a material that generates almost no moisture even when heated, such as metal, the configuration of the first intermediate layer 21 does not need to be adopted.

[0039] The first intermediate layer 21, the second intermediate layer 22, and the third intermediate layer 23 have different foaming start temperatures, specifically, the foaming start temperature of the first intermediate layer 21 (about 140°C), the foaming start temperature of the second intermediate layer 22 (about 200°C), and the foaming start temperature of the third intermediate layer 23 (near 700°C). That is, in the intermediate layer 13, a plurality of layers 21, 22, and 23 are laminated so that the layers with higher foaming start temperatures transition from the front side to the back side of the fire-resistant sheet 10.

[0040] In the fire-resistant sheet 10, each of the layers constituting the first layer 11, the second layer 12, and the intermediate layer 13 is compressed, and the thickness of each layer is shrunk to about 1 / 10 to 1 / 20 of the thickness before compression. To explain in detail, the fire-resistant sheet 10 is formed by compressing the laminate 100 shown in FIG. 2 in the thickness direction. In the laminate 100, the pre-compression first layer 101, the pre-compression first intermediate layer 111, the pre-compression second intermediate layer 112, the pre-compression third intermediate layer 113, and the pre-compression second layer 102 are arranged in this order from the surface side, and the entire laminate 100 is bound by acrylic resin. Each layer in the laminate 100 corresponds to a layer in the same arrangement order in the fire-resistant sheet 10, and the composition of each layer in the laminate 100 is the same as the composition of the layer in the fire-resistant sheet 10 corresponding thereto.

[0041] The laminate 100 is then compressed while being heated until the thickness becomes about 1 / 10 to 1 / 20 of the original thickness. The compressed laminate 100 is then cooled and dried to obtain a thin plate-like fire-resistant sheet 10. The thickness of the fire-resistant sheet 10 is 0.5 mm or more and 5 mm or less. In addition, in the compressed laminate 100, i.e., the fire-resistant sheet 10, a portion of the foamed material contained in the layer constituting the intermediate layer 13 is liquid, and seeps into the glass wool or rock wool constituting the first layer 11 or the second layer 12, and seeps out from the sheet surface (the side opposite the intermediate layer 13).

[0042] The fire-resistant sheet 10 obtained as described above can be easily attached to the construction site of a building, specifically, to the site requiring fire-resistant covering, and can efficiently improve the fire resistance of the construction site. To be more specific, the fire-resistant sheet 10 can be bent or cut to fit the shape of the construction site, so that it can be easily attached appropriately according to the construction site. In other words, the use of the fire-resistant sheet 10 can improve the fire resistance of the construction site more easily and at a lower cost than conventional construction methods such as applying fire-resistant paint to the construction site or wrapping a fire-resistant covering material around the construction site. In addition, when applying fire-resistant paint, it is necessary to adjust the amount of paint applied, and proper adjustment of the amount of paint applied requires specialized knowledge, experience, skill, etc. In contrast, when using the fire-resistant sheet 10, even workers who do not have these skills can apply the sheet appropriately.

[0043] Furthermore, when a fire occurs in a building to which the fire-resistant sheet 10 is applied, the fire-resistant sheet 10 exhibits good fire resistance. To explain in detail, for example, when the fire-resistant sheet 10 attached to a wooden pillar or beam is heated by being exposed to a flame, the foaming material (expandable graphite or ammonium polyphosphate) exuded from the sheet surface foams and becomes fixed. This fixed (carbonized) foaming material forms a protective layer that protects the sheet surface (i.e., the outer surface of the first layer 11 or the second layer 12).

[0044] Then, as the heating progresses and the sheet temperature becomes higher, the acrylic resin, which is the binder, softens, and the glass wool or rock wool that was restrained in a compressed state is released and expands. That is, the compressed glass wool or rock wool tries to restore its pre-compression state. The thickness of the layer after expansion is 10 to 20 times the thickness at the previous stage, that is, the thickness before compression.

[0045] When the fireproof sheet 10 is further heated and the temperature of the fireproof sheet 10 reaches a certain temperature (about 140°C) or higher, the first intermediate layer 21, which is the closest to the first layer 11 among the intermediate layers 13, foams to form a fireproof layer. To explain in detail, the starch as a carbonized layer constituting the first intermediate layer 21 absorbs moisture generated from the part (wood) where the fireproof sheet 10 is attached, heats up, and browns due to the Maillard reaction, and further foams and solidifies (carbonizes) due to carbon dioxide generated with the decomposition of sodium bicarbonate, which is a foaming agent. As a result, a carbonized layer is formed in the glass wool present in the first intermediate layer 21.

[0046] As the fire-resistant sheet 10 heats up and the sheet temperature becomes higher (about 200°C), the second intermediate layer 22, which is located inside the first intermediate layer 21 and adjacent to the first intermediate layer 21, foams to form a fire-resistant layer. To explain in more detail, the foaming agent constituting the second intermediate layer 22, such as expandable graphite or ammonium polyphosphate, expands within the glass wool. Since the melting point of this expanded filler is higher than the glass transition temperature of the glass wool, it maintains the expanded state to form a fire-resistant layer.

[0047] When the fire-resistant sheet 10 is further heated and the sheet temperature reaches a higher temperature (about 700°C), the third intermediate layer 23 adjacent to the second layer 12 foams to form a fire-resistant layer. To explain in detail, unfoamed vermiculite serving as a foaming agent constituting the third intermediate layer 23 expands within the glass wool. Here, since the glass transition temperature of the glass wool and the foaming start temperature of the vermiculite are approximately the same temperature at around 700°C, in a high-temperature environment where the sheet temperature reaches 700°C, the glass wool melts in the third intermediate layer 23 and the vermiculite foams, forming a strong fire-resistant layer.

[0048] As described above, in this embodiment, the first layer 11, the second layer 12, and the intermediate layer 13 of the fireproof sheet 10 in a compressed state thermally expand by heating and restore the thickness before compression, so that the fireproof sheet 10 exhibits good fire resistance. In addition, the intermediate layer 13 has a plurality of layers that foam to form a fireproof layer laminated therein, and the plurality of layers are arranged from the front surface of the sheet toward the back surface of the sheet in order of the lowest foaming start temperature. As a result, when the sheet temperature rises due to heating during a fire, the fireproof layer is formed stepwise from the layer on the front surface side of the sheet (i.e., the side to be heated). As a result, the area where the fireproof sheet 10 is applied can be appropriately protected from flames and the like.

[0049] In addition, in this embodiment, since fiber materials (non-flammable fibers) such as glass wool or rock wool are dispersed in the acrylic resin in each layer of the fireproof sheet 10, a fireproof sheet 10 having a relatively high Young's modulus is obtained. Such a fireproof sheet 10 can be used as a reinforcing material for the construction site. In addition, the reinforcing effect of the fireproof sheet 10 can be further improved by changing the compression ratio of the fireproof sheet 10 or the type and shape (specifically, fiber length) of the fiber material used.

[0050] [Examples of fireproof sheet usage] The fire-resistant sheet of the present invention is used, for example, in the construction of a building, when constructing a fire-resistant structure at a target location (corresponding to a construction location) in the framework of the building. Specifically, in a building construction method, the fire-resistant sheet of the present invention is attached to the surface of the target location to construct a fire-resistant structure at the target location. At this time, the back side of the fire-resistant sheet, i.e., the second layer, is adhered to the surface of the target location.

[0051] By using the fire-resistant sheet of the present invention, a fire-resistant structure can be satisfactorily constructed in a target portion of the building frame, and the construction can be performed more inexpensively and simply than a wet construction method in which a foaming fire-resistant paint or the like is applied to the surface of the target portion. In addition, the fire-resistant sheet can be manufactured in a factory and transported to a construction site (a building construction site) for use, minimizing the work at the construction site. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples. Unless otherwise specified, the contents in the following description are based on mass.

[0053] (Example) In the examples, a fire-resistant sheet having a first layer, a second layer, and an intermediate layer configured under the following conditions was produced. The fire-resistant sheet was produced by compressing a laminate of multiple layers corresponding to the first layer, the second layer, and the intermediate layer until the thickness was reduced to about 1 / 10 of the thickness before compression, and finally producing a sheet with a thickness of 4 mm.

[0054] <First and second layers> The first and second layers were constructed by binding glass fiber sheets in ethylene vinyl acetate copolymer resin. The density and thickness of the glass fiber sheets were 50 g / m 3 , 0.5 mm, and the content of ethylene-vinyl acetate copolymer resin in each of the first and second layers was 30% (30 g was blended per 100 g of the fire-resistant sheet).

[0055] <Middle Class> The intermediate layer was made by dispersing starch (manufactured by Sanwa Starch Industry Co., Ltd., product name: Corn Starch Y), which is a foaming material containing a carbonizing agent, and ammonium polyphosphate and expandable graphite as foaming agents together with glass wool in ethylene-vinyl acetate copolymer resin. The contents of starch, ammonium polyphosphate, expandable graphite, and ethylene-vinyl acetate copolymer resin in the intermediate layer were 35%, 5%, 10%, and 20%, respectively (35g, 5g, 10g, and 20g, respectively, per 100g of fire-resistant sheet).

[0056] <Test> In the examples, a heating test was carried out using the above fire-resistant sheet in the following manner. == Heating test procedure == The fireproof sheet prepared under the above conditions was attached to one surface of a 3.2 mm thick iron plate, and the iron plate was heated on a tabletop stove from the side where the fireproof sheet was attached. During the heating period, thermocouples were fixed to the center of the surface of the iron plate where the fireproof sheet was not attached and to the burner part of the stove, and the temperature change during the heating period was measured using each thermocouple. During the heating period, the iron plate was placed above the stove's trivet and held at a predetermined distance from the stove's burner.

[0057] (Comparative Example) In the comparative example, the heating test was carried out without applying a fire-resistant sheet to the specimen. The procedure of the heating test was the same as in the example.

[0058] (Regarding test results) In the heating test, the fireproof sheet used in the embodiment transitioned from a state before the heating test (see FIG. 3) to a state after the heating test (see FIG. 4). Specifically, ammonium polyphosphate as a foaming agent constituting the intermediate layer seeped out onto the sheet surface, which foamed and became fixed. This fixed (carbonized) foaming agent formed a protective layer that protected the sheet surface (the surface on the heated side). In addition, the expandable graphite as a foaming agent foamed due to heating, and the thickness of the sheet increased, and further heating softened the binding material of the first and second layers, causing the compressed glass fiber sheet to return to its original shape, thereby further increasing the thickness of the sheet. Furthermore, as the heating progressed, the starch in the intermediate layer embraced the foaming agent in the glass wool and solidified, resulting in the formation of a carbonized layer in the sheet.

[0059] The final thickness of the fireproof sheet was about 4 mm before the heating test, and about 22 mm at the end of the heating. The carbonized layer formed in the fireproof sheet also served as a fireproof layer to suppress the penetration of flames and the rise in temperature. As a result, in the heating test, as can be seen by comparing Figures 5 and 6, the degree of rise in the iron plate temperature for the same heating curve is clearly different between the example and the comparative example, and the iron plate temperature at the end of heating in the example is about half of the iron plate temperature at the end of heating in the comparative example.

[0060] As described above, the effects of the present invention are clear from the above-mentioned embodiments. [Explanation of symbols]

[0061] 10 Fireproof sheet 11 1st layer 12 2nd layer 13. Middle Class 21 First Middle Class 22 The second middle class 23 The third middle class 100 Laminate 101 First layer before compression 102 Second layer before compression 111 First intermediate layer before compression 112 Pre-compression second intermediate layer 113 Third intermediate layer before compression

Claims

1. A fire-resistant sheet, A first layer and a second layer formed by dispersing non-flammable fibers in a thermoplastic resin; an intermediate layer disposed between the first layer and the second layer, the intermediate layer being configured by dispersing a foam material in a thermoplastic resin; The fire-resistant sheet has a thickness of 0.5 mm or more and 5 mm or less.

2. The fire-resistant sheet according to claim 1 , wherein the intermediate layer has a layer formed by dispersing the foamed material containing a carbonizing agent in a thermoplastic resin.

3. 2. The fire-resistant sheet according to claim 1, wherein the intermediate layer has a layer formed by dispersing the foam material, which is a mixture of starch and sodium bicarbonate, in a thermoplastic resin.

4. The fire-resistant sheet according to claim 1 , wherein the intermediate layer has a layer formed by dispersing the foam material containing a foaming agent in a thermoplastic resin.

5. The fire-resistant sheet according to claim 1 , wherein the intermediate layer has a layer formed by dispersing the foam material containing unfoamed vermiculite in a thermoplastic resin.

6. The fire-resistant sheet according to claim 1 , wherein the intermediate layer is formed by dispersing non-combustible fibers and the foam material in a thermoplastic resin.

7. The intermediate layer has a plurality of layers laminated in the thickness direction of the fire-resistant sheet, The fire-resistant sheet according to claim 1 , wherein each of the plurality of layers has a different foaming initiation temperature.

8. The fire-resistant sheet according to claim 7 , wherein the plurality of layers are laminated in an order according to the foaming initiation temperature.

9. When the fireproof sheet is installed, the second layer is attached to the construction site of the building; The fire-resistant sheet according to claim 8 , wherein the plurality of layers are laminated such that a layer having a lower foaming initiation temperature is positioned closer to the first layer.

10. A method for constructing a building, comprising attaching the fire-resistant sheet according to any one of claims 1 to 9 to a portion of the building to be made fire-resistant.

Citation Information

Patent Citations

  • Foaming fire-resistant sheet

    JP2022100879A