Precast prestressed concrete product
By incorporating Portland cement, pulverized blast furnace slag, and an ettringite-forming early demolding agent, the precast prestressed concrete product maintains strength and workability, enabling higher slag replacement ratios and reduced carbon dioxide emissions.
Patent Information
- Application Number
- JP2023066626
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Increasing the replacement ratio of pulverized blast furnace slag in concrete to reduce carbon dioxide emissions is hindered by decreased initial strength and increased viscosity, which affects the workability and production efficiency of precast and prestressed concrete products.
A precast prestressed concrete product comprising Portland cement, pulverized blast furnace slag, and an ettringite-forming early demolding agent, with a replacement ratio of 50% to 90% by mass and an added amount of early demolding agent between 10 to 30 kg/m³, maintaining a water binder ratio of 30% to 42% by mass, to ensure initial strength and workability.
The solution maintains initial strength and workability of precast prestressed concrete products, allowing for higher slag replacement ratios without compromising production efficiency, thereby reducing carbon dioxide emissions.
Smart Images

Figure 2024152436000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to precast prestressed concrete products. [Background technology]
[0002] As part of measures to combat climate change, all industries are being asked to reduce emissions of carbon dioxide, a greenhouse gas. The construction industry emits a large amount of carbon dioxide during business activities such as material procurement, construction, and demolition. Concrete materials emit large amounts of carbon dioxide due to the use of fossil fuels and decarbonation in limestone during the cement manufacturing process. Decarbonizing the construction industry and reducing its environmental impact are major challenges in order to realize a sustainable society.
[0003] One method for reducing carbon dioxide emissions during concrete production is to replace part of the cement with ground granulated blast furnace slag, an industrial by-product, thereby reducing the amount of cement used (see, for example, Patent Document 1).
[0004] On the other hand, in the case of precast, prestressed concrete products manufactured in factories, it is desirable to shorten the age at which the concrete is removed from the form (age at which prestress is introduced) in order to increase the operating rate of the factory. However, it is known that the initial strength decreases as the amount of granulated blast furnace slag substituted for cement increases. Therefore, when concrete mixed with the above-mentioned granulated blast furnace slag is used for precast, prestressed concrete products, there is a problem that it is difficult to ensure the initial strength and to shorten the age at which the concrete is removed from the form (age at which prestress is introduced). Therefore, in order to prevent the decrease in the initial strength of concrete mixed with granulated blast furnace slag, it has been attempted to use granulated blast furnace slag with a high degree of fineness and to reduce the water-binder ratio (for example, Patent Document 2).
[0005] Also, in order to improve the delay in strength development, a method is known in which an admixture with an early demolding effect and a setting-accelerating effect is added to an ettringite-based concrete expansive additive that is generally used to prevent cracks in concrete products (e.g., Non-Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-114176 A [Patent Document 2] JP 2019-48742 A [Non-patent literature]
[0007] [Non-Patent Document 1] Study on the fundamental properties of hardened cement using expansive early demolding agent; 76th Annual Conference of the Japan Society of Civil Engineers V-17 2021 Summary of the Invention [Problem to be solved by the invention]
[0008] From the viewpoint of reducing the environmental impact of concrete, it is desirable to increase the substitution rate of ground granulated blast furnace slag for cement. However, as the substitution rate of ground granulated blast furnace slag increases, the early strength decreases, and so there is a problem that it is difficult to increase the substitution rate of ground granulated blast furnace slag in precast, prestressed concrete products, which require a certain early strength for the introduction of prestress.
[0009] Furthermore, as in Patent Document 2, if the water-binder ratio is reduced and the fineness of the ground granulated blast furnace slag is increased in order to ensure a specified initial strength, the viscosity of the fresh concrete increases and workability decreases, so there is a problem that the replacement rate of the ground granulated blast furnace slag is limited to the range that is feasible for work.
[0010] Therefore, an object of the present invention is to provide a precast, prestressed concrete product which can compensate for the decrease in initial strength and ensure excellent workability, while employing approximately the same water-binder ratio and the same curing method as when only Portland cement is used (said replacement rate = 0 mass%), even when the replacement rate of ground granulated blast furnace slag is increased. [Means for solving the problem]
[0011] In order to solve the above problems, one embodiment of the concrete product disclosed herein is a precast, prestressed concrete product, which contains at least water, a binder consisting of Portland cement and ground granulated blast furnace slag, an ettringite-forming early-removal agent, fine aggregate, and coarse aggregate, in which the replacement rate of the ground granulated blast furnace slag to cement is 50% by mass or more and 90% by mass or less, and the amount of the ettringite-forming early-removal agent added is 10 kg / m 3 More than 30kg / m 3 The present invention is characterized in that:
[0012] The Portland cement is preferably a high early strength Portland cement.
[0013] The water-binder ratio, which is the ratio of the water to the binder, is preferably 30% by mass or more and 42% by mass or less.
[0014] The compressive strength of the concrete at 1 day is 35N / mm 2 More preferably, it is equal to or greater than this. Effect of the Invention
[0015] According to the present invention, even if the replacement rate of ground granulated blast furnace slag in precast, prestressed concrete products is increased, it is possible to compensate for the decrease in initial strength and ensure excellent workability while employing approximately the same water-binder ratio and the same curing method as in the case where only Portland cement is used (said replacement rate = 0 mass%). [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a diagram showing the relationship between the elapsed time of concrete undergoing a steam curing process and the set temperature of the steam curing. [Diagram 2] 1 is a graph showing the relationship between the binder-water ratio B / W and the compressive strength of concrete at one day when the replacement rate A / B is 0 mass%. [Diagram 3] Graph showing the relationship between the amount of early demolding agent FDE added and the compressive strength of concrete at one day of age, when the water-binder ratio is 32% by mass and the replacement rate A / B is 90% by mass. [Figure 4] A graph showing the relationship between the replacement rate A / B and the compressive strength of concrete at one day of age, when the water-binder ratio is 32 mass% and the amount of early demolding agent FDE added is 0 kg / m3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Embodiment) Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. Note that the same elements are designated by the same numbers or symbols throughout the description of the embodiments. The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present invention, its application, or its uses.
[0018] In this specification, "fresh concrete" refers to concrete in a state from immediately after mixing the ingredients until the start of setting.
[0019] <Concrete products> The concrete product according to this embodiment (also simply referred to as "concrete" in this specification) is a precast, prestressed concrete product manufactured in a factory.
[0020] The concrete contains water W, a binder B consisting of Portland cement C and ground granulated blast furnace slag A, an ettringite-forming early demolding material FDE, fine aggregate S, and coarse aggregate G.
[0021] [Portland cement] The Portland cement C is not particularly limited, and general Portland cements such as ordinary Portland cement, high-early-strength Portland cement, and ultra-high-early-strength Portland cement can be used.
[0022] The Portland cement C is preferably a high-early-strength Portland cement.
[0023] [Grained blast furnace slag] The type and fineness of the ground granulated blast furnace slag A are not specified, but it is preferable that it conforms to JIS A 6206 "ground granulated blast furnace slag for concrete". The density is not intended to be limited, but is, for example, 2 to 5 g / cm 3 In addition, the specific surface area can be set to 5000 to 10000 cm 2 Particularly preferred is ground granulated blast furnace slag with a molecular weight of 6000 or 8000 / g.
[0024] By using ground granulated blast furnace slag A as part of binder B, the amount of Portland cement C used can be reduced, contributing to a reduction in carbon dioxide emissions.
[0025] [Early demolding material] For the rapid demolding material FDE, an ettringite-forming rapid demolding material is used.
[0026] The specific surface area of the early demolding material FDE is, but is not limited to, for example, 2500 cm 2 / g or more 6000cm 2 / g or less, preferably 4500 cm 2 / g or more 5500cm 2 / g or less.
[0027] [Inflatable material] The concrete product may contain an expansive material EX. The expansive material EX is not particularly limited, and any known general expansive material can be used.
[0028] [Water, aggregates and additives] The water W is not particularly limited, and water used in general concrete, such as tap water, can be used. The amount of water W added to the concrete is not particularly limited, and may be the amount used in general concrete, for example, 100 to 200 kg / m 3 etc. can be used.
[0029] The fine aggregate S is not particularly limited, and may be any fine aggregate generally used in concrete. For example, natural aggregates such as sand, crushed sand, and porous aggregate may be used. For the coarse aggregate G, natural aggregates such as gravel and crushed stone may be used.
[0030] Concrete may contain various additives such as water reducing agents, air-entraining agents, high-performance water reducing agents, high-performance air-entraining water reducing agents, and shrinkage reducing agents. The additives may be added to concrete by being contained in water W, for example. The amount of additives added to concrete is appropriately adjusted depending on the function of the additive, but may be, for example, 2 to 10 kg / m 3 It can be said that:
[0031] [Water binder ratio] The ratio of water W to binder B, that is, the water-binder ratio W / B of concrete is preferably 30% by mass or more and 42% by mass or less, more preferably more than 30% by mass and 42% by mass or less, even more preferably 31% by mass or more and 41% by mass or less, and particularly preferably 31% by mass or more and 35% by mass or less. By setting the water-binder ratio W / B in the above range, it is possible to improve workability while compensating for the initial strength reduction.
[0032] [Amount of binder added] The amount of binder B added to the concrete may be adjusted in relation to the amount of water W added so that the water-binder ratio W / B falls within the above range.
[0033] [Replacement rate] In this specification, "the replacement ratio A / B of ground granulated blast furnace slag A to cement" means the ratio of Portland cement replaced by ground granulated blast furnace slag A when all of binder B is Portland cement. Specifically, "the replacement ratio A / B of ground granulated blast furnace slag A to cement" is expressed as the content (mass%) of ground granulated blast furnace slag A in binder B. The replacement ratio A / B is 50 mass% or more and 90 mass% or less, more preferably 60 mass% or more and 90 mass% or less, and particularly preferably 70 mass% or more and 90 mass% or less. The larger the replacement ratio A / B, the more the amount of Portland cement C used can be reduced, and therefore the greater the reduction in carbon dioxide emissions.
[0034] [Amount of early demolding agent added] The amount of FDE added to concrete for rapid demolding is 10 kg / m 3 More than 30kg / m 3 Less than 10kg / m 3 More than 25kg / m 3 By setting the amount of the quick demolding agent FDE to the above range, sufficient early strength can be ensured even if the water-binder ratio W / B exceeds 30 mass% and the replacement rate A / B is increased. Thus, compensation for the decrease in early strength and excellent workability can be achieved at the same time.
[0035] [Amount of expansion agent added] The amount of expansion agent EX added to concrete is 30kg / m 3 It is preferable that the density is less than 10 kg / m 3 More than 30kg / m 3 By setting the amount of the expansion additive EX to the above range, cracks in concrete products can be effectively suppressed.
[0036] <Concrete manufacturing method> The manufacturing method of concrete includes, but is not limited to, for example, a mixing process for measuring and mixing the above-mentioned materials contained in concrete, i.e., at least water W, binder B consisting of cement C and ground granulated blast furnace slag A, early-release material FDE, fine aggregate S, and coarse aggregate G, a pouring process for pouring the mixed fresh concrete inside a formwork, a steam curing process for steam curing the fresh concrete, a form removal process for removing the formwork, and a moist curing process for moist curing the concrete with water or the like supplied from outside after removing the formwork.
[0037] In the steam curing process, the outside air of the fresh concrete is kept (prepared) at a standard temperature (e.g., 20°C), then heated (e.g., 25°C / 3 hours), kept at the highest temperature (e.g., 45°C), and then cooled (e.g., 25°C / 6 hours). In this way, in the steam curing process, the temperature of the outside air is changed in response to the temperature change caused by the heat generated by hydration of the fresh concrete, which promotes hardening through the hydration reaction and allows the concrete to develop strength early. The humidity of the outside air can be, for example, 95% by mass.
[0038] <Compressive strength of concrete> The compressive strength of concrete at one day, i.e., its initial strength, is 35N / mm 2 It is preferable that the resistance is 40.6N / mm or more. 2 The concrete compressive strength targeted in the experimental examples described below was determined to be 40.6 N / mm2, taking into account the variability of experimental values, so as to ensure that most experimental values would not fall below the initial strength. 2 That's all.
[0039] As a result, precast, prestressed concrete products with an increased replacement rate of ground granulated blast furnace slag can be prestressed the day after concrete is poured, just like when only Portland cement is used (replacement rate = 0 mass%).
[0040] <Experimental Example> Next, specific experimental examples will be described.
[0041] 1. Test conditions [Preparation of test pieces] Test pieces (diameter 10×20 cm) for the compressive strength test described below were prepared using the following materials, composition and conditions.
[0042] -material- Portland cement C: High early strength Portland cement (density 3.14 g / cm 3 ) Ground granulated blast furnace slag A: Ground granulated blast furnace slag 6000 (density 2.91 g / cm 3 , Specific surface area: approx. 6000cm 2 / g) Rapid demolding material FDE: Ettringite formation system (density 2.55g / cm 3 ) Expansion material EX: Ettringite and lime composite (density 3.08g / cm 3 ) Water W: Tap water Fine aggregate S: Equal amounts of land sand and crushed sand are mixed. Land sand (from Namegata City, surface dry density 2.58g / cm 3 , water absorption rate 2.58% by mass) Crushed sand (Kanuma City, surface dry density 2.62g / cm 3 , water absorption rate 1.14% by mass) Coarse aggregate G: Crushed stone 2005 (Kanuma City, surface dry density 2.64g / cm 3 , water absorption rate 0.64% by mass) High-performance water reducing agent SP: Polycarboxylic acid type Air Entraining AgentAE: Anionic Surfactant -Composition- Water binder ratio W / B: 32% by mass, 36% by mass, 41% by mass Substitution rate A / B: 0% by mass, 50% by mass, 60% by mass, 70% by mass, 80% by mass, 90% by mass Early demolding material FDE: 0kg / m 3 , 10kg / m 3 , 20kg / m 3 Expandable material EX: 0kg / m 3 , 10kg / m 3 , 20kg / m 3, 30kg / m 3 Amount of water added (standard: concrete): 160 kg / m 3 Amount of coarse aggregate G added (standard: concrete): 985 kg / m 3 The unit fine aggregate content was adjusted according to the amount of early demolding agent (FDE) added.
[0043] The target slump flow at the end of mixing was 50±7.5 cm, and the target air content was 4.5±1.5%, which were adjusted by the amount of high-performance water reducing agent SP and air entraining agent AE added.
[0044] -Production procedure- The above materials were mixed in the above-mentioned proportions according to the following procedure.
[0045] That is, Portland cement C, ground granulated blast furnace slag A and fine aggregate S were mixed using a mixer and dry mixed for 45 seconds, then water W containing admixtures was added and the first mixing was carried out for 90 seconds, and then coarse aggregate G was added and the second mixing was carried out for 60 seconds.
[0046] The mixed fresh concrete was then poured into a circular formwork measuring φ10 x 20 cm, and steam curing was carried out in a variable temperature chamber as follows.
[0047] FIG. 1 is a diagram showing the relationship between the elapsed time (hours) of concrete undergoing a steam curing process and the set temperature (° C.) for the steam curing.
[0048] Specifically, as shown in Figure 1, the material was first placed at 20°C for 3 hours, then heated to 45°C over 3 hours, held at 45°C for 4 hours, and then cooled to 20°C over 6 hours. The humidity during the steam curing period was 95% by mass.
[0049] Then, the form was removed 24 hours after the fresh concrete was poured (form was removed when the material was aged one day). In this way, test pieces aged one day were obtained.
[0050] [Compressive strength test] The compressive strength test was carried out in accordance with JIS A 1108.
[0051] [Target properties] The target properties of precast, prestressed concrete products were as follows:
[0052] Target compressive strength at 1 day = 40.6N / mm 2 Slump flow = 50 ± 7.5 cm Air volume = 4.5 ± 1.5% 2. Test Results The test results of the compressive strength test are shown in Table 1 and Figs.
[0053] [Table 1]
[0054] The binder water ratio B / W is the mass ratio of binder B to water W. In addition, in Table 1, the replacement rate A / B is 90 mass%, and the amount of the early demolding agent FDE and the amount of the expansion agent EX are both 20 kg / m 3 There are two samples of 1 day old concrete. The difference in the 1 day old compressive strength of these two samples is due to the difference in the amount of air contained in the samples. In other words, the more air contained in the sample, the lower the compressive strength.
[0055] (1) Replacement ratio A / B = 0% by mass (high-early-strength Portland cement only) Figure 2 shows the relationship between the binder-water ratio B / W (water-binder ratio W / B) and the compressive strength of concrete at one day (N / mm2) when the replacement rate A / B is 0 mass%, i.e., when only high-early-strength Portland cement is used as binder B. 2 ) is a graph showing the relationship between
[0056] As shown in Figure 2, as B / W increases, i.e., as W / B decreases, the compressive strength increases.
[0057] (2) Difference in replacement rate A / B Figure 4 shows the amount of FDE added for early demolding = 0 kg / m 3 The replacement ratio A / B and the compressive strength of concrete at 1 day (N / mm 2 ) The water-binder ratio W / B is 32 mass%.
[0058] As shown in FIG. 4, it can be seen that as the replacement ratio A / B increases, the compressive strength decreases.
[0059] (3) Difference in amount of FDE added as early demolding agent Figure 3 shows the relationship between the amount of early demolding agent FDE added and the compressive strength (N / mm 2 ) The water-binder ratio W / B is 32 mass%.
[0060] As shown in Figure 3, as the amount of early demolding agent FDE added increases, the compressive strength at one day increases.
[0061] 3. Data Completion From the results of Figs. 2 to 4, approximate formulas F1, F2, and F6 shown in these figures and Table 2 were calculated.
[0062] [Table 2]
[0063] Based on the approximate formulas F1, F2, and F6, the compressive strength was calculated for cases where the water-binder ratio W / B, the replacement rate A / B, and the amount of early demolding agent FDE added were different, and the compressive strength test was not conducted. The results are shown in Table 3.
[0064] [Table 3]
[0065] As shown in Table 3, it is found that adding an early demolding agent FDE and increasing the amount added is effective from the viewpoint of compensating for the decrease in compressive strength at one day in concrete mixed with ground granulated blast furnace slag A. It is also found that as the amount of early demolding agent FDE added increases, it is possible to increase the water-binder ratio W / B and the replacement rate A / B of ground granulated blast furnace slag A.
[0066] In particular, when the water-binder ratio W / B is 33% by mass or more and less than 37% by mass, preferably 35% by mass or more and 36% by mass or less, the compressive strength of the concrete at one day of age is 40.8 N / mm 2 In order to achieve the above, the amount of FDE added as an early demolding agent is set at 30 kg / m 3 By so doing, the substitution ratio A / B can be set to 80 mass % or less.
[0067] Furthermore, when the water-binder ratio W / B is 30% by mass or more and less than 33% by mass, preferably 31% by mass or more and 32% by mass or less, the compressive strength of the concrete at one day of age is 40.8 N / mm 2 From the viewpoint of achieving the above, the amount of the early demolding agent FDE added is 10 kg / m 3 More than 30kg / m 3 By setting it to be equal to or less than 1, the substitution ratio A / B can be set to be equal to or less than 90 mass %.
[0068] From the viewpoint of reducing carbon dioxide emissions, it is desirable to increase the replacement ratio A / B as much as possible while still achieving the desired early strength.
[0069] <Features and Effects> The concrete according to this embodiment is a precast, prestressed concrete product, which contains water, a binder made of Portland cement and ground granulated blast furnace slag, an ettringite-forming early-removal agent, fine aggregate, and coarse aggregate, in which the replacement rate of the ground granulated blast furnace slag to the cement is 50% by mass or more and 90% by mass or less, and the amount of the ettringite-forming early-removal agent added is 10 kg / m 3 More than 30kg / m 3 The present invention is characterized in that:
[0070] Since the concrete contains ground granulated blast furnace slag A, the amount of Portland cement C used can be reduced, and carbon dioxide emissions can be reduced. In addition, concrete containing ground granulated blast furnace slag A tends to have a lower initial strength as the replacement rate A / B increases, but the inclusion of an ettringite-forming early-release agent can compensate for the decrease in initial strength. Furthermore, while the concrete containing ground granulated blast furnace slag A traditionally ensured initial strength by reducing the water-binder ratio W / B, the inclusion of an ettringite-forming early-release agent makes it possible to compensate for the decrease in initial strength, and therefore the water-binder ratio W / B can be increased. This suppresses the increase in viscosity of fresh concrete and improves workability.
[0071] Although the preferred embodiments of the present invention have been described in detail above, the concrete and the method for producing concrete according to the present invention are not limited to the above-described embodiments, and various modifications and changes are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0072] A. Ground granulated blast furnace slag B Binding material A / B substitution rate C Portland cement S Fine aggregate G Coarse aggregate W water W / B water binder ratio B / W binder water ratio
Claims
1. A precast, prestressed concrete product comprising: The present invention comprises at least water, a binder consisting of Portland cement and ground granulated blast furnace slag, an ettringite-forming rapid demolding agent, fine aggregate, and coarse aggregate, the substitution rate of the ground granulated blast furnace slag to the cement being 50% by mass or more and 90% by mass or less, and the amount of the ettringite-forming rapid demolding agent added is 10 kg / m 3 More than 30kg / m 3 is less than or equal to A precast, prestressed concrete product characterized by:
2. The Portland cement is a high-early-strength Portland cement.
2. The precast prestressed concrete product of claim 1.
3. The water-binder ratio, which is the ratio of the water to the binder, is 30% by mass or more and 42% by mass or less.
3. A precast prestressed concrete product according to claim 1 or claim 2.
4. The compressive strength of the concrete product at one day of age is 35 N / mm 2 That's all.
3. A precast prestressed concrete product according to claim 1 or claim 2.
Citation Information
Patent Citations
Concrete material
JP2014114176A
High strength concrete and production method of high strength concrete
JP2019048742A