Packaging base paper

A softwood pulp-based paper with carboxymethylcellulose and polyacrylamide resin coating addresses the issue of tearing and puncture resistance, ensuring durable paper packaging for sealed containers.

JP2024152443AActive Publication Date: 2024-10-25HOKUETSU CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023066639
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

Existing paper packaging materials lack sufficient strength to resist tearing when folded or punctured by sharp objects, making them unsuitable for sealed containers due to potential leakage during distribution.

Method used

A packaging base paper composed primarily of softwood pulp with a disintegration freeness of 440 to 690 ml (CSF), coated with a metal salt of carboxymethylcellulose and containing a polyacrylamide resin, achieving high resistance to punctures and tears.

Benefits of technology

The paper exhibits excellent tensile and puncture strength, maintaining integrity during distribution and replacing plastic packaging by providing a durable, tear-resistant sealed container.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152443000001
    Figure 2024152443000001
Patent Text Reader

Abstract

To provide a packaging base paper which is resistant to tearing even when folded and is resistant to tearing even when it comes into contact with a sharp object or a protruding object.SOLUTION: A problem of the present invention is solved by a packaging base paper made of a base paper mainly composed of pulp, in which 70 mass% or more of the pulp is softwood pulp, the macerated freeness is 440 to 690 ml (CSF), the formation index measured by the total β-ray ground is 1 or less, and a metal salt of carboxymethylcellulose is applied to at least one surface of the base paper.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging base paper that is resistant to tearing even when folded and to tearing even when it comes into contact with a sharp object or a protruding object. [Background technology]

[0002] In recent years, the problem of plastic waste has become more serious. It is said that the world's plastic production exceeds 400 million tons per year, and among these, the packaging container sector produces a particularly large amount of plastic, which is the main cause of plastic waste. The most commonly used plastics for packaging containers are polyethylene terephthalate (PET), which is used for beverage bottles, polyethylene (PE), which is used for laminating plastic bags and containers, and polypropylene (PP). Plastic does not decompose for a long time, and the waste turns into microplastics in the natural environment, causing serious adverse effects on the ecosystem. In particular, marine pollution by microplastics is severe, and it is said that the plastic waste cannot be recovered. In the future, it will be necessary for the global environment to reduce the use of plastic.

[0003] In response to this problem, there is a growing movement to replace plastic packaging with packaging made of paper materials. For example, in the case of sealed packaging, various products are available in which a laminate or heat seal layer is provided on a paper base material. However, since paper is more easily broken than plastic materials, there are problems such as the paper being easily torn at the fold if the strength against bending is insufficient, and the paper being easily punctured or torn by contact with sharp objects or protrusions during distribution. If such problems occur, the contents will leak, making it unsuitable as a sealed container.

[0004] To avoid such problems, it is necessary to increase the strength of the paper, particularly its folding endurance and resistance to contact with sharp objects or protrusions; however, no technology for increasing the aforementioned resistance has been reported to date.

[0005] As a technique for imparting strength to a paper base material, Patent Document 1 proposes a wrapping paper characterized by adding 0.01 to 3.0 mass% of carboxymethylcellulose with a substitution degree of 0.3 to 0.6 in order to obtain excellent sizing properties and paper strength in wet and dry states. Patent Document 2 also proposes an impregnated paper impregnated with an impregnating resin characterized by comprising an acrylic acid ester copolymer having a glass transition temperature (Tg) of -30 to +30°C, which contains 75 to 98 mass% of structural units derived from 10 to 100 mass% methyl acrylate and 0 to 90 mass% methyl methacrylate and / or ethyl acrylate, and 2 to 15 mass% of structural units derived from one or more monomers selected from (meth)acrylamide, N-alkyl-substituted (meth)acrylamide, and (meth)acrylic acid, in order to obtain excellent internal bond strength and folding endurance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-027399 A [Patent Document 2] JP 2005-281431 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the wrapping paper described in Patent Document 1 has low resistance (puncture strength) to contact with sharp objects or protrusions, and has problems such as being easily punctured or torn during distribution, etc. Furthermore, the invention described in Patent Document 2 has a problem in that it needs to be impregnated with a large amount of resin in order to obtain excellent strength, and the amount of plastic used is too large.

[0008] The present invention has been made in consideration of such problems, and an object of the present invention is to provide a packaging base paper that has high strength against bending, excellent resistance to contact with sharp objects or protrusions, and retains strength that makes it difficult to tear even during distribution after packaging the contents. [Means for solving the problem]

[0009] The packaging base paper of the present invention is characterized in that it is made of a base paper mainly composed of pulp, 70% by mass or more of the pulp is softwood pulp (hereinafter also referred to as "N pulp"), and the disintegration freeness of the packaging base paper is 440 to 690 ml (CSF). Furthermore, the present invention is characterized in that it has at least two or more of the following four features. It is characterized in that at least one surface of the base paper is coated with a metal salt of carboxymethylcellulose, preferably a sodium salt of carboxymethylcellulose (sodium carboxymethylcellulose) (Item A). Furthermore, the present invention is characterized in that the formation index measured by the total β-ray radiation is 1 or less (Item B), contains a polyacrylamide resin (Item C), and has a density of 0.55 to 0.90 g / cm 3 (Item D). The packaging base paper of the present invention having two or more of Items A to D can provide a sealed container that has high resistance (puncture strength) to contact with sharp objects or protrusions and is difficult to break even after packaging the contents. In the present invention, the sealed container includes not only containers that are relatively airtight, such as retort pouches for food, but also containers that are permeable to gas but that do not allow solid or liquid foreign matter to enter and that can prevent loss, efflorescence, deliquescence, or evaporation of the contents under normal handling, transportation, or storage conditions.

[0010] The packaging base paper of the present invention preferably contains a paper strength enhancer and / or a sizing agent. The packaging base paper of the present invention may further contain a sizing agent. With this configuration, carboxymethyl cellulose is easily distributed on the surface of the base paper, and a packaging base paper with higher puncture strength can be obtained. The packaging base paper of the present invention may also contain a paper strength enhancer. This allows a packaging base paper with high puncture strength to be obtained. The paper strength enhancer may be a polyacrylamide resin or something other than a polyacrylamide resin.

[0011] In addition, in the packaging base paper of the present invention, the coating amount of the metal salt of carboxymethyl cellulose is 0.1 to 1.2 g / m2 in terms of solid content per one side of the base paper. 2 The packaging base paper of the present invention may further contain a sizing agent. This allows the packaging base paper to have higher puncture strength. The packaging base paper of the present invention may further contain a sizing agent. This configuration allows the carboxymethyl cellulose to be easily distributed on the surface of the base paper, and allows the packaging base paper to have higher puncture strength.

[0012] The packaging base paper of the present invention may also have a base paper of two or more layers. This configuration makes it easier to obtain a base paper with good texture, and allows for a packaging base paper with higher puncture strength. The packaging base paper of the present invention may further contain a sizing agent. This configuration allows for a packaging base paper with higher puncture strength. The packaging base paper of the present invention has a basis weight of 50 to 150 g / m2. 2 This makes it possible to obtain a packaging base paper with high puncture strength. 2 More than 0.095N / g / m 2 More preferably, 0.100N / g / m 2 It is preferable that the puncture strength per unit basis weight is equal to or greater than 100 g / m2. A sealed container made of such a packaging base paper is resistant to breakage even when subjected to impact during distribution after packaging the contents, making it suitable for storage and transportation, and is particularly suitable as a container for liquids and powders. Here, the puncture strength according to the present invention is the strength specified in "7.5 Puncture Strength Test" of "JIS Z 1707:2019 General Rules for Food Packaging Plastic Films", and the puncture strength per unit basis weight is obtained by dividing the puncture strength by the U.S. basis weight.

[0013] Furthermore, in the packaging base paper of the present invention, the content of the polyacrylamide resin may be 0.1 to 0.9% by mass relative to the pulp in the base paper. This configuration allows the packaging base paper to have higher puncture strength. Furthermore, in the packaging base paper of the present invention, the mass average molecular weight of the polyacrylamide resin may be 350,000 to 3,700,000. This configuration allows the packaging base paper to have higher puncture strength.

[0014] Furthermore, in the method for producing packaging base paper of the present invention, a pulp slurry is prepared in which 70% by mass or more of the pulp is softwood pulp, and then the concentration of the raw material at the papermaking machine inlet (raw material concentration) is set to 0.1 to 0.9% by mass, and paper is made using a papermaking machine. The obtained base paper is then impregnated with an aqueous carboxymethyl cellulose solution and dried to produce the packaging base paper of the present invention having a disintegration freeness of 440 to 690 ml (CSF).

[0015] Furthermore, in the method for producing packaging base paper of the present invention, a pulp slurry is prepared in which 70% or more by mass of the pulp is softwood pulp, and then a raw material slurry is prepared containing 0.1 to 0.9 parts by mass of a polyacrylamide-based resin per 100 parts by mass of the pulp slurry. The raw material slurry obtained is used to make paper in a papermaking machine, and the obtained base paper is then impregnated with an aqueous carboxymethyl cellulose solution and dried to produce the packaging base paper of the present invention having a disintegration freeness of 440 to 690 ml (CSF).

[0016] Furthermore, in the method for manufacturing packaging paper of the present invention, a pulp slurry is prepared in which 70% or more by mass of the pulp is softwood pulp, and then a raw material slurry is prepared which contains 0.1 to 0.9 parts by mass of a polyacrylamide-based resin per 100 parts by mass of the pulp slurry. The obtained raw material slurry is used to make paper in a papermaking machine with a raw material concentration at the papermaking machine inlet of the papermaking machine (raw material concentration) of 0.1 to 0.9% by mass, thereby producing packaging paper of the present invention having a disintegrated freeness of 440 to 690 ml (CSF).

[0017] Furthermore, in the method for producing packaging base paper of the present invention, a pulp slurry is prepared in which 70% or more by mass of the pulp is softwood pulp, and then a raw material slurry is prepared which contains 0.1 to 0.9 parts by mass of a polyacrylamide-based resin per 100 parts by mass of the pulp slurry. Using the obtained raw material slurry, paper is made in a papermaking machine with a raw material concentration at the papermaking machine inlet (raw material concentration) of 0.1 to 0.9% by mass, and then the obtained base paper is impregnated with an aqueous carboxymethyl cellulose solution and dried to produce packaging base paper of the present invention having a disintegrated freeness of 440 to 690 ml (CSF).

[0018] Furthermore, the method for producing packaging base paper of the present invention preferably includes a step of calendering the dried packaging base paper at a linear pressure of 10 to 100 kg / cm and / or with 1 to 3 nips. Effect of the Invention

[0019] The packaging base paper of the present invention has excellent tensile strength and is not only resistant to tearing, but also has high strength against bending and high puncture strength, for example, a puncture strength per unit basis weight of 0.087 N / g / m 2 Since the paper has a high elasticity of 100% or more, it has excellent resistance to impacts during distribution after packaging of the contents, and can therefore be suitably used as sealed containers such as packaging bags, and can also be suitably used as a base paper for replacing part or all of conventional plastic packaging with paper packaging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Next, the present invention will be described in detail with reference to the embodiments, but the present invention is not limited to these descriptions. Various modifications of the embodiments may be made as long as the effects of the present invention are achieved.

[0021] The packaging base paper used in the present invention is mainly composed of pulp. Examples of the pulp used here include unbleached wood chemical pulp, such as hardwood unbleached kraft pulp (LUKP), softwood unbleached kraft pulp (NUKP), hardwood unbleached sulfite pulp (LUSP), and softwood unbleached sulfite pulp (NUSP), bleached wood chemical pulp, such as hardwood bleached kraft pulp (LBKP), softwood bleached kraft pulp (NBKP), hardwood bleached sulfite pulp (LBSP), and softwood bleached sulfite pulp (NBSP), and mechanical pulp, such as thermomechanical pulp (TMP), refiner ground pulp (RGP), and groundwood pulp (GP). The proportion of pulp in the packaging base paper of the present invention is not particularly limited, but is preferably 90% by mass or more, for example, 90 to 99% by mass of pulp in the packaging base paper. It is possible to reduce the proportion of pulp by adding a filler or other bulking agent, but this is not desirable because it also leads to a decrease in various strengths of the paper.

[0022] In the present invention, 70% by mass or more of the pulp is softwood pulp. It is preferably 75% by mass or more, 80% by mass or more, and more preferably 85% by mass or more. For example, it is preferable that the softwood pulp in the total pulp is 70 to 100% by mass, further 75 to 100% by mass, 80 to 100% by mass, 85 to 100% by mass, 90 to 100% by mass, for example, 95 to 100% by mass. If pulp other than softwood pulp is used, hardwood pulp is preferable from the viewpoint of cost, etc., and for example, it is preferable to use hardwood bleached kraft pulp (LBKP). For example, pulp containing 70 to 100 mass% of softwood pulp and 30 to 0 mass% of hardwood pulp may be used, and further pulp containing 75 to 100 mass% of softwood pulp and 25 to 0 mass% of hardwood pulp, 80 to 100 mass% of softwood pulp and 20 to 0 mass% of hardwood pulp, 85 to 100 mass% of softwood pulp and 15 to 0 mass% of hardwood pulp, 90 to 100 mass% of softwood pulp and 10 to 0 mass% of hardwood pulp, or pulp containing 95 to 100 mass% of softwood pulp and 5 to 0 mass% of hardwood pulp may be used. The softwood pulp is not particularly limited, and may be NUKP, NUSP, NBKP, or NBSP. Among these, NUKP is more preferable because it is easier to improve strength properties such as folding endurance. If the proportion of softwood pulp in the total pulp is less than 70% by mass, it becomes difficult to satisfy the strength against folding, and the proportion of long fiber pulp in the paper decreases, making it impossible to obtain sufficient puncture strength.

[0023] In the present invention, the disintegration freeness of the packaging base paper is set to 440 to 690 ml (CSF). It is preferably 500 to 670 ml (CSF), and more preferably 530 to 650 ml (CSF). By setting the disintegration freeness of the packaging base paper within this range after making 70 mass % or more of the total pulp in the base paper softwood pulp, the puncture strength can be further improved. When the disintegration freeness value of the base paper before the metal salt of carboxymethylcellulose is applied becomes small, for example, when it falls below 500 ml (CSF), the puncture strength tends to decrease, which is different from the various strengths such as tensile strength, whose numerical value increases when fibrillation is advanced to a certain degree. Therefore, it is difficult to adjust the balance between these various strengths and the puncture strength only by the freeness of the pulp, but this can be solved by applying a metal salt of carboxymethylcellulose. That is, even if the base paper has a relatively small disintegration freeness value of 440 to 530 ml (CSF), the puncture strength can be improved by applying a metal salt of carboxymethylcellulose, and it is easy to balance the strength with various strengths such as tensile strength and tear strength. The effect of improving the puncture strength by applying a metal salt of carboxymethylcellulose tends to be greater the smaller the disintegration freeness (the smaller the puncture strength of the base paper before the application of carboxymethylcellulose), but it is also observed even when the disintegration freeness value is in the relatively large range of 531 to 690 ml. If the disintegration freeness of the packaging base paper is less than 440 ml (CSF), the pulp becomes too fibrillated, which may result in a poor effect on improving the puncture strength. Conversely, if the disintegration freeness exceeds 690 ml (CSF), the pulp is not sufficiently fibrillated, which results in a poor effect on improving the puncture strength. The disintegrated freeness herein refers to the Canadian Standard Freeness (Canadian Standard Pulp Freeness) value measured according to the method of JIS P 8121-2: 2012 using a pulp slurry obtained by disintegrating according to the method of JIS P 8220-1: 2012. Examples of the metal salt of carboxymethylcellulose used in the present invention include sodium salt, lithium salt, potassium salt, magnesium salt, calcium salt, etc., with sodium salt being preferred.Metal salts of carboxymethylcellulose are generally referred to as carboxymethylcellulose, and in this specification, metal salts of carboxymethylcellulose are also referred to as "carboxymethylcellulose" or "CMC", and when it is necessary to specify the metal species of the metal salt, they are referred to as sodium carboxymethylcellulose, etc.

[0024] The method of beating the raw pulp is not particularly limited, and any beating machine such as a beater, a Jordan, a deluxe finer, or a double disc refiner may be used alone or in combination.

[0025] The packaging base paper of the present invention uses the above-mentioned pulp, and is characterized by having at least two of the following four features. That is, it is characterized by having a metal salt of carboxymethylcellulose, preferably a sodium salt of carboxymethylcellulose (sodium carboxymethylcellulose) coated on at least one surface of the base paper (Feature A). Furthermore, the present invention is characterized by having a formation index of 1 or less measured by the total β-ray radiation (Feature B), containing a polyacrylamide resin (Feature C), and having a density of 0.55 to 0.90 g / cm. 3 The packaging base paper of the present invention having two or more of the features A to D can provide a sealed container that has high resistance (puncture strength) to contact with sharp objects or protrusions and is difficult to break even after packaging the contents. Any combination of two or more of the features A to D is sufficient, and each of these features has an effect of improving resistance (puncture strength) to contact with sharp objects or protrusions. The puncture strength improving effects of each of these features do not interfere with each other, and the puncture strength can be improved additively by combining two or more of the features A, B, C, and D. That is, the packaging base paper of the present invention having two or more of the features A, B, C, and D has sufficient puncture strength, but a packaging base paper having three or more, or even four or more, of the features A, B, C, and D can provide a packaging base paper with better puncture strength.

[0026] That is, the embodiment of the packaging paper of the present invention includes at least the following forms. One embodiment of the present invention is a packaging base paper that combines items A and B, and is characterized in that it is made of a base paper whose main component is pulp, in which 70% or more by mass of the pulp is softwood pulp, has a disintegration freeness of 440 to 690 ml (CSF), has a formation index measured by the total β-ray material of 1 or less, and has a metal salt of carboxymethylcellulose applied to at least one side of the base paper.

[0027] One embodiment of the present invention is a packaging base paper that combines items A and C, characterized in that it is made of a base paper whose main component is pulp, in which 70% or more by mass of the pulp is softwood pulp, has a disintegration freeness of 440 to 690 ml (CSF), contains a polyacrylamide resin, and has a metal salt of carboxymethylcellulose applied to at least one surface of the base paper.

[0028] As one embodiment of the present invention, by combining items A and D, the pulp is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp, the defibrated freeness is 440 to 690 ml (CSF), and the density is 0.55 to 0.90 g / cm 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

[0029] One embodiment of the present invention is a packaging base paper that combines items B and C, and is characterized in that it is made of a base paper whose main component is pulp, in which 70% or more by mass of the pulp is softwood pulp, has a disintegration freeness of 440 to 690 ml (CSF), has a formation index of 1 or less measured by the total β-ray material, and contains a polyacrylamide resin.

[0030] As one embodiment of the present invention, by combining items B and D, the paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the macerated freeness is 440 to 690 ml (CSF), the formation index measured by the total β-ray material is 1 or less, and the density is 0.55 to 0.90 g / cm 3 The packaging base paper is characterized in that

[0031] As one embodiment of the present invention, by combining items C and D, a paper liner made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the paper liner has a disintegration freeness of 440 to 690 ml (CSF), contains a polyacrylamide resin, and has a density of 0.55 to 0.90 g / cm 3 The packaging base paper is characterized in that

[0032] Furthermore, it is more preferable that the packaging base paper of the present invention has three or more of the characteristics of items A to D. That is, it is possible to obtain a sealed container that has more excellent resistance (puncture strength) to contact with sharp objects or protrusions and is less likely to break even after packaging the contents. As one embodiment of the present invention, by combining items A, B, and C, it is a packaging base paper that is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, has a disintegration freeness of 440 to 690 ml (CSF), has a formation index measured by the total of β-rays of 1 or less, contains a polyacrylamide resin, and has a metal salt of carboxymethylcellulose applied to at least one surface of the base paper.

[0033] As one embodiment of the present invention, by combining items A, B, and D, the paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the macerated freeness is 440 to 690 ml (CSF), the formation index measured by the total β-ray material is 1 or less, and the density is 0.55 to 0.90 g / cm 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

[0034] As one embodiment of the present invention, by combining items A, C, and D, a paper liner made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the paper liner has a disintegration freeness of 440 to 690 ml (CSF), contains a polyacrylamide resin, and has a density of 0.55 to 0.90 g / cm 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

[0035] As one embodiment of the present invention, by combining items B, C, and D, the paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the defibrated freeness is 440 to 690 ml (CSF), the formation index measured by the total β-ray material is 1 or less, a polyacrylamide resin is contained, and the density is 0.55 to 0.90 g / cm 3 The packaging base paper is characterized in that

[0036] In the most preferred embodiment of the present invention, by combining items A, B, C, and D, the paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the defibrated freeness is 440 to 690 ml (CSF), the formation index measured by the total β-ray material is 1 or less, a polyacrylamide resin is contained, and the density is 0.55 to 0.90 g / cm 3 The packaging base paper is characterized in that at least one surface of the base paper is coated with a metal salt of carboxymethyl cellulose. In this embodiment, the puncture strength per unit basis weight is 0.095 N / g / m 2 Thus, a packaging base paper having extremely excellent puncture strength can be obtained.

[0037] In the packaging base paper of the present invention, it is preferable that carboxymethylcellulose is applied to at least one surface of the base paper (item A). By applying carboxymethylcellulose to the surface of the base paper, the effects of reinforcing interfiber bonds, filling gaps between fibers, and providing strength through a coating are obtained, improving folding strength and breaking elongation as well as puncture strength. Furthermore, the higher the moisture content of the paper, the higher the puncture strength of the paper. Since carboxymethylcellulose has high water retention, it is expected to have the effect of maintaining high moisture in the paper, and therefore it is expected to improve puncture strength.

[0038] The packaging base paper of the present invention preferably has a moisture content (hereinafter sometimes referred to as "equilibrium moisture content") of 6.5 to 8.5% by mass after conditioning for 24 hours in a 23°C x 50% RH environment. More preferably, it is 7.0 to 8.0% by mass. It has an effect of improving puncture strength. If the equilibrium moisture content is less than 6.5% by mass, the effect of improving puncture strength may be poor. Conversely, even if the equilibrium moisture content exceeds 8.5% by mass, the effect of improving puncture strength will plateau, but in order to make the equilibrium moisture content 8.5% by mass or more, it is necessary to impart excessive water retention to the paper, which may reduce the suitability for processing into packaging bags, etc. Note that when the packaging base paper of the present invention is conditioned for 24 hours in a 40°C x 90% RH environment, for example, the moisture content may be about 12% by mass, but it has been found that even in this case, the puncture strength is good. Therefore, a container using the packaging base paper of the present invention can be a container with sufficient puncture strength even in a high humidity environment.

[0039] The carboxymethyl cellulose used in the present invention may have, for example, a degree of substitution of 0.6 to 0.7, a degree of polymerization of 220 to 250, and a molecular weight of 47,000 to 135,000. The molecular weight is particularly preferably 47,000 to 54,000. Within the above ranges, the cellulose ester is easily dissolved in water, has a low viscosity, and therefore has good workability, is easily permeated and impregnated uniformly into the base paper, and tends to improve puncture strength.

[0040] The method of applying carboxymethylcellulose is not particularly limited, and various known coating devices or impregnation devices can be used, for example, size press method, dipping method, coater method, spray method, etc. Application methods that can be used include. By attaching carboxymethylcellulose to the surface of the base paper, the surface strength of the paper is improved, and the resistance to rubbing and puncture is improved, so that the paper can be suitably used as a packaging base paper. The amount of carboxymethylcellulose attached to the base paper is 0.1 to 1.2 g / m2 in terms of solid content per side of the base paper. 2 , for example, 0.2 to 1.0 g / m 2 More preferably, the thickness is 0.3 to 0.8 g / m 2 0.1g / m 2 If the thickness is less than 1.2 g / m, it is difficult to obtain the effect of providing strength through the coating or the effect of maintaining a high equilibrium moisture content, and there is a risk that the improvement in puncture strength will be inferior. 2 If the moisture content exceeds 100%, the equilibrium moisture content of the paper can be increased, but the stiffness of the packaging base paper may become too high, making the paper more susceptible to cracking and tearing, and the suitability for processing into packaging bags and the like may also decrease. In the present invention, carboxymethyl cellulose can be applied to both sides of the base paper to produce packaging base paper with higher puncture strength. For example, 0.2 to 2.2 g / m2 in terms of solid content is applied to both sides of the base paper using an impregnation device. 2 , preferably 0.4 to 2.0 g / m 2 , more preferably 0.5 to 1.5 g / m 2 By impregnating the paper with carboxymethyl cellulose, a packaging base paper with higher puncture strength can be obtained.

[0041] The drying method after coating the base paper with carboxymethyl cellulose is not particularly limited, and may be an air drying method represented by hot air drying such as a multi-cylinder dryer method, a Yankee dryer method, or an air dryer method, or a radiation drying method represented by an infrared device.

[0042] The packaging base paper of the present invention preferably has a formation index of 1 or less as measured by the total β-rays (item B). By making the formation index of 1 or less as measured by the total β-rays, the number of areas with locally low puncture strength can be reduced, and the packaging base paper can be made less likely to tear. The formation index is preferably 0.8 or less, more preferably 0.6 or less. If the formation index exceeds 1, the unevenness of the formation, i.e., the unevenness of the basis weight, becomes large, and the base paper locally has areas with high and low basis weights. As a result, the puncture strength also varies locally, and the areas with poor puncture strength may be easily torn when contacted with sharp objects or protrusions. The lower limit of the formation index is not particularly limited, but is preferably 0.3 or more, more preferably 0.5 or more. If the formation index is reduced, the unevenness of the basis weight is reduced, and the variation in puncture strength can be suppressed, while if the formation index is reduced too much, the effect of improving the puncture strength will reach a plateau, and manufacturing problems may occur, such as the need to drastically reduce the raw material concentration described below. Furthermore, the elongation rate of the base paper decreases, which may impair the suitability for processing when the base paper needs to be elongated, such as when it is processed into a bag shape.

[0043] As a method for making the formation index measured by the total β-rays less than 1, it is preferable to improve the formation of the base paper by lowering the concentration of the raw material at the inlet of the papermaking machine, i.e., the concentration of the raw material slurry (mass of raw material slurry / mass of water+mass of raw material slurry, hereinafter also referred to as raw material concentration), thereby reducing the formation index. The raw material concentration is preferably 0.9% by mass or less, more preferably 0.5% by mass or less, and even better 0.3% by mass or less. In the case of a cylinder papermaking machine, the raw material concentration in the vat at the inlet of the papermaking machine corresponds to the raw material concentration, and in the case of a Fourdrinier papermaking machine, the inlet concentration of the head box corresponds to the raw material concentration. If the raw material concentration is too high, it becomes difficult to adjust the formation, and as a result, the formation index is likely to exceed 1. In this way, it is preferable to adjust the formation index by the raw material concentration, but if the raw material concentration is less than 0.1% by mass, the sheet becomes difficult to peel off from the wire and the yield on the wire also decreases, so 0.1% by mass is the actual lower limit. It is more preferable that the lower limit of the raw material concentration is 0.15% by mass. In particular, in the case of multi-layer papermaking, it is preferable that the raw material concentrations of the front and back layers are within this range. In addition, when making paper using a Fourdrinier papermaking machine, the use of a shaking device improves the formation and the formation index can be reduced. In addition, depending on the conditions of use, the formation index can be reduced by using a retention aid or a coagulant such as aluminum sulfate. Therefore, in the manufacturing method of the packaging base paper of the present invention, a packaging base paper having an appropriate formation index can be obtained by adjusting the pulp slurry, and then making the paper using a papermaking machine with the concentration of the raw material at the papermaking machine inlet (raw material concentration) set to 0.1 to 0.9% by mass.

[0044] As described above, the packaging base paper of the present invention contains a relatively large amount of softwood pulp and has a relatively high numerical range of disintegration freeness. In order to simply improve the formation, it is better to contain more hardwood pulp than softwood pulp, advance the beating of the pulp, and set the disintegration freeness in a relatively low range. However, these actions result in a decrease in puncture strength that exceeds the effect of improving the formation. The packaging base paper of the present invention contains 70% by mass or more of softwood pulp, and has a disintegration freeness of 440 to 690 ml (CSF), while being a base paper with good formation, thereby improving the puncture strength.

[0045] The formation index used in the measurement of the formation index in the present invention is a β-ray ground total, that is, a ground total using a β-ray radiation source, which indicates the distribution of the U.S. basis weight (sometimes called basis weight). The widely used ground total is based on light transmission, but it is not suitable for evaluating the formation because the pulp components, the type and amount of filler, the hue, the whiteness, the degree of beating of the pulp, etc. are variable factors. The formation index measured using the β-ray ground total is an index of the difference in basis weight (referred to as unit basis weight) measured at a diameter of 1 mm of the packaging base paper. If the formation index measured using the β-ray ground total is 1 or less, the local basis weight difference is small. On the other hand, if the formation index measured using the β-ray ground total exceeds 1, the local basis weight difference becomes large and the puncture strength becomes low in the part with a small unit basis weight. Therefore, good formation is important for the packaging base paper of the present invention.

[0046] The packaging base paper of the present invention preferably contains a dry strength enhancer as a paper strength enhancer, and can contain polyacrylamide as the dry strength enhancer (item C). As the polyacrylamide (polyacrylamide-based resin), an amphoteric polyacrylamide-based resin, which has particularly excellent fixation properties, is preferable. With this configuration, high folding strength is obtained, and strength against bending is increased. In addition, a sealed container can be obtained that has high resistance (puncture strength) to contact with sharp objects or protrusions, and is difficult to break even after the contents are packaged.

[0047] Furthermore, in the packaging base paper of the present invention, the content of the polyacrylamide resin may be 0.1 to 0.9% by mass relative to the pulp in the base paper. This configuration allows the packaging base paper to have higher puncture strength. Furthermore, in the packaging base paper of the present invention, the mass average molecular weight of the polyacrylamide resin may be 350,000 to 3,700,000. This configuration allows the packaging base paper to have higher puncture strength.

[0048] The packaging base paper of the present invention may further contain a dry strength enhancer other than polyacrylamide resin. Examples of such dry strength enhancers include starches such as oxidized starch, cationic starch, or modified starch, vegetable gum, polyvinyl alcohol, modified polyvinyl alcohol, rubber latex, polyethylene oxide, polyamide resin, and the like, and one or more of these may be used. Among these, polyacrylamide resins, particularly amphoteric polyacrylamide resins with excellent fixability, are preferred. There are no particular limitations on the method of applying these to the base paper, and an internal addition method or an external addition method may be used, but adding them to the pulp slurry (internal addition) makes it easier to obtain a base paper with excellent puncture strength.

[0049] The content of the dry strength agent in the packaging base paper is preferably 0.10 to 2.2 parts by mass, more preferably 0.12 to 1.0 parts by mass, relative to 100 parts by mass of pulp. More preferably, it is 0.15 to 0.8 parts by mass. If it is less than 0.1 parts by mass, the effect of improving the puncture strength may be poor. On the other hand, if it exceeds 2.2 parts by mass, agglomerates derived from the strength agent may be generated in the papermaking machine, causing stains on the paper.

[0050] In the present invention, the packaging base paper may further contain a sizing agent. As the sizing agent that can be used here, one or more of paraffin wax-based sizing agents, microcrystalline wax-based sizing agents, carnauba (carnauba wax)-based sizing agents, alkyl ketene dimer-based sizing agents, rosin-based sizing agents, alkenyl succinic anhydride-based sizing agents, styrene acrylic-based sizing agents, etc. may be used. In the packaging base paper of the present invention, carboxymethyl cellulose may be applied to the surface of the base paper. In this case, by including a sizing agent in the base paper, the carboxymethyl cellulose is inhibited from penetrating into the inside of the base paper and is more likely to remain on the surface of the base paper. As a result, a packaging base paper with higher puncture strength can be obtained. The method of applying the sizing agent to the base paper is not particularly limited, and an internal addition method or an external addition method can be used, but it is preferable to add the sizing agent to the pulp slurry (internal addition). When external addition is used, it is preferable to apply the carboxymethyl cellulose after applying the sizing agent to the base paper. The content of the sizing agent is preferably 0.1 to 0.5 parts by mass, more preferably 0.15 to 0.35 parts by mass, relative to 100 parts by mass of pulp. In the present invention, for example, it is preferable to add a rosin-based sizing agent, preferably a modified rosin emulsion, in an amount of 0.1 to 0.5 parts by mass relative to 100 parts by mass of pulp.

[0051] The packaging base paper of the present invention may contain various papermaking materials such as wet strength agents, aluminum sulfate, fillers, retention aids, coloring dyes, coloring pigments, bulking agents, etc., within the scope of not impairing the intended effects of the present invention. As the filler, one or more known fillers such as hydrated silicic acid, white carbon, talc, kaolin, clay, calcium carbonate, titanium oxide, aluminosilicate, calcined clay, barium sulfate, synthetic resin fillers, etc. may be used. For example, 0.1 to 2.0 parts by mass of aluminum sulfate may be contained per 100 parts by mass of pulp.

[0052] In this embodiment, the density of the base paper is 0.55 to 0.90 g / cm 3(item D). By setting the density in this range, it is difficult for sharp objects such as needles to penetrate and the base material is less likely to crack, so that high puncture strength can be obtained. The density is 0.60 to 0.85 g / cm 3 More preferably, it is 0.65 to 0.80 g / cm 3 It is more preferable that the density is 0.55 g / cm. Normally, when comparing base papers of the same basis weight, the strengths of paper such as tensile strength and folding endurance tend to decrease as the density decreases, but there is an optimum density range for puncture strength, and if the density is too high or too low, the puncture strength decreases. Therefore, in this embodiment, in order to obtain a packaging base paper that has high puncture strength while maintaining a balance with other strengths, the density is set to the above range. The density of the base paper is 0.55 g / cm. 3 If the density is less than 0.90 g / cm, not only will the paper's strengths, such as tensile strength, decrease, impairing its suitability for processing, but the puncture strength will also tend to decrease. 3 Above this value, the cushioning properties decrease, and the puncture strength also decreases.

[0053] The method of adjusting the density of the base paper is not particularly limited, but includes calendaring. The calendaring method is not particularly limited and can be selected from known methods such as super calendaring, gloss calendaring, shoe nip calendaring, and soft calendaring. The temperature, line pressure, and number of nips in the calendaring can be appropriately set within a range in which the target density can be obtained. By increasing the density by calendaring, the smoothness of the base paper is increased, resulting in a packaging base paper with better printability. On the other hand, the density increases as the line pressure and number of nips in the calendaring increase, so the density can be adjusted by appropriately adjusting them. In order to obtain an appropriate density in the present invention, the line pressure is preferably 10 to 100 kg / cm, and the number of nips is preferably 1 to 3 nips.

[0054] Another method for adjusting the density is to use a multi-layer paper. In the present invention, it is preferable that the packaging base paper is made by combining two or more layers. When made in multiple layers, the density tends to be higher than when made in a single layer. Furthermore, by using such a configuration, unevenness in the formation can be suppressed, and the packaging base paper can be made to have better puncture strength. If uneven formation is present, the base paper is prone to tearing at the thin formation areas, and there is a risk of localized areas with poor puncture strength, so it is more preferable to reduce uneven formation. In order to reduce uneven formation, a base paper with a relatively large basis weight, for example, one with a basis weight of 60 g / m2, is used. 2 When the basis weight exceeds 100 g / m2, it is better to make multiple layers by reducing the basis weight per layer rather than making a single layer. When making multiple layers, the number of layers is preferably 3 or more, and more preferably 4 or more. There is no particular upper limit on the number of layers, but the packaging base paper of the present invention has a basis weight of 50 to 150 g / m2. 2 In some cases, the number of layers may be in the range of 7 or less, and preferably 6 or less.

[0055] In the present invention, the method of making the base paper is not particularly limited, and the base paper can be made using a conventionally known papermaking machine such as a cylinder papermaking machine, a short wire papermaking machine, a fourdrinier papermaking machine, or a combination of these papermaking machines. The drying method in the papermaking machine is not particularly limited, and the multi-cylinder dryer method, the Yankee dryer method, the air drying method represented by hot air drying, and the radiation drying method represented by an infrared device can be used. Among them, the multi-cylinder dryer method or the Yankee dryer method is preferred, and the Yankee dryer method is more preferred. By drying using the Yankee dryer method, the mirror surface of the Yankee dryer is transferred to one side of the base paper, resulting in a paper with a one-sided gloss, and a packaging base paper with better puncture strength can be obtained.

[0056] In this embodiment, the basis weight of the packaging base paper is 50 to 150 g / m 2 More preferably, it is 70 g / m 2 ~130g / m 2 , e.g., 75 g / m 2 ~85g / m 2or 80 g / m 2 ~110g / m 2 Within this range, the paper has excellent folding strength and puncture resistance while maintaining suitability for processing into packaging bags, etc. The basis weight is 50 g / m 2 If it is less than 150g / m, the bending and puncture strength may be poor. 2 If it exceeds this value, the puncture strength will be high, but the stiffness will also be too high, which may reduce the suitability for processing into packaging bags, etc.

[0057] Furthermore, the present invention relates to a method for producing packaging paper, and the embodiment of the method includes at least the following aspects. One embodiment of the present invention relates to a method for producing packaging base paper, which comprises preparing a pulp slurry in which 70% by mass or more of the pulp is softwood pulp, then making the raw material concentration at the paper machine inlet to 0.1-0.9% by mass (raw material concentration) with a paper machine, and then impregnating the obtained base paper with an aqueous carboxymethylcellulose solution and drying it. This allows for the production of the packaging base paper of the present invention, which satisfies items A and B, and has a formation index of 1 or less measured by total β-ray radiation, at least one side of the base paper is coated with a metal salt of carboxymethylcellulose, and a disaggregated freeness of 440-690 ml (CSF).

[0058] One embodiment of the present invention relates to a method for producing a packaging base paper, which comprises preparing a pulp slurry in which 70% by mass or more of the pulp is softwood pulp, then preparing a raw material slurry containing 0.1 to 0.9 parts by mass of a polyacrylamide resin per 100 parts by mass of the pulp slurry, and using the raw material slurry to make paper using a papermaking machine, and then impregnating the obtained base paper with an aqueous carboxymethylcellulose solution and drying. This allows for the production of the packaging base paper of the present invention, which contains a polyacrylamide resin, has a metal salt of carboxymethylcellulose applied to at least one side of the base paper, has a disintegration freeness of 440 to 690 ml (CSF), and includes items A and C.

[0059] One embodiment of the present invention relates to a method for producing packaging base paper, which comprises preparing a pulp slurry in which 70% by mass or more of the pulp is softwood pulp, then preparing a raw material slurry containing 0.1-0.9 parts by mass of polyacrylamide resin per 100 parts by mass of the pulp slurry, and using the raw material slurry obtained to make paper in a papermaking machine with a raw material concentration at the papermaking machine inlet of the papermaking machine (raw material concentration) of 0.1-0.9% by mass. This allows for the production of packaging base paper of the present invention, which has a formation index of 1 or less measured in total for β-rays, contains polyacrylamide resin, and has a disintegration freeness of 440-690 ml (CSF), and includes items B and C.

[0060] One embodiment of the present invention relates to a method for producing a packaging base paper, which comprises preparing a pulp slurry in which 70% by mass or more of the pulp is softwood pulp, then preparing a raw material slurry containing 0.1-0.9 parts by mass of a polyacrylamide resin and preferably 0.1-0.5 parts by mass of a sizing agent per 100 parts by mass of the pulp slurry after preparing the pulp slurry, and using the obtained raw material slurry to make a paper with a concentration of the raw material at the paper machine inlet (raw material concentration) of 0.1-0.9% by mass, and then impregnating the obtained base paper with an aqueous carboxymethylcellulose solution and drying it. This allows for the production of a packaging base paper of the present invention, which has a formation index of 1 or less measured by the total of β-rays, contains a polyacrylamide resin, has a metal salt of carboxymethylcellulose applied to at least one side of the base paper, and has a disaggregated freeness of 440-690 ml (CSF), and includes items A, B, and C.

[0061] The method for producing packaging base paper preferably includes calendering the dried packaging base paper at a linear pressure of 10 to 100 kg / cm and / or with 1 to 3 nips, thereby achieving a density of 0.55 to 0.90 g / cm. 3 In the manufacturing method of the present invention, the pulp is beaten in an appropriate range to prepare a pulp slurry so that the packaging base paper has a dissolved freeness of 440 to 690 ml (CSF).

[0062] The packaging base paper of the present invention has a puncture strength per unit basis weight of 0.087 N / g / m 2 It is preferable that the value is equal to or greater than 0.095 N / g / m 2 More preferably, it is 0.100 N / g / m or more. 2 It is most preferable that the tensile strength is 6.0 kN / m or more. For example, the tensile strength of the packaging base paper of the present invention is preferably 6.0 kN / m to 10.0 kN / m. The puncture strength of the packaging base paper of the present invention is preferably 7.00 N or more, and more preferably 7.50 N or more. With this strength, the packaging base paper can be excellent in physical strength, difficult to break, has high strength against bending, and has excellent resistance to impact during distribution after packaging of the contents, and can be suitably used as a base paper for replacing part or all of conventional plastic packaging with paper packaging. Furthermore, the packaging base paper of the present invention can be used as a bag-shaped sealed container by applying, for example, an adhesive or a resin with heat sealability, and directly processing the bag to form a sealed container. It is also possible to laminate one side with polyethylene or the like and then processing the bag to form a sealed container. Applying such a laminate results in the use of plastic materials, but the amount of plastic is reduced by making a part of the sealed container from paper. The form of the bag making process is not particularly limited, and depending on the application, for example, pillow packaging, caramel packaging, or a combination of these can be adopted. Thus, the packaging base paper of the present invention is suitable as a packaging base paper for sealed containers, and is particularly suitable as a packaging base paper for bag-shaped sealed containers.

[0063] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" refers to "solid parts" unless otherwise specified. The number of parts added is a value calculated based on the solid content.

[0064] Example 1 <Base paper manufacturing> 100 parts of beaten softwood bleached kraft pulp was dispersed in water to prepare a pulp slurry, and 0.2 parts of a polyacrylamide resin with a mass average molecular weight (Mw) of 3 million as a dry paper strength agent, 0.25 parts of a sizing agent (product name: AL1300 / manufactured by Seiko PMC Co., Ltd., modified rosin emulsion), and 0.5 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. The obtained raw material slurry was used to make paper using a fourdrinier paper machine to obtain a single-layer base paper. The inlet concentration (raw material concentration) of the head box was 0.2% by mass.

[0065] <Coating> A carboxymethylcellulose (indicated as "CMC" in the table) aqueous solution (product name: SG Cellogen PR, sodium carboxymethylcellulose, Daiichi Kogyo Seiyaku Co., Ltd., degree of substitution 0.6-0.7, degree of polymerization 220-250, molecular weight 47000-54000) was applied to the obtained base paper using a two-roll size press, and the base paper was dried at 130°C in a rotary dryer to obtain the desired packaging base paper. The amount of carboxymethylcellulose attached to the base paper was 1.12 g / m2 in terms of solid content on both sides of the base paper. 2 (0.56g / m per side 2 After drying, no calendaring was performed. The basis weight of the resulting packaging base paper was 80.8 g / m 2 The packaging base paper has a freeness of 600mlCSF and a density of 0.62g / cm 3 It was.

[0066] Example 2 In the preparation of the pulp slurry in Example 1, 75 parts of beaten softwood bleached kraft pulp and 25 parts of beaten hardwood bleached kraft pulp were used, and the amount of carboxymethyl cellulose attached was 1.00 g / m2 in terms of solid content on both sides of the base paper. 2 (0.50g / m per side 2 The packaging base paper was obtained in the same manner as in Example 1, except that the weight per unit area was changed to 100.0 g / m. The basis weight of the obtained packaging base paper was 80.0 g / m. 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.60g / cm 3 It was.

[0067] Example 3 A packaging base paper was obtained in the same manner as in Example 1, except that a three-ply paper was made, and after drying, a calendar treatment was performed with a linear pressure of 80 kg / cm and one nip. The basis weight of the obtained packaging base paper was 80.8 g / m 2 The packaging base paper has a freeness of 600mlCSF and a density of 0.79g / cm 3 It was.

[0068] Example 4 A packaging base paper was obtained in the same manner as in Example 3, except that no polyacrylamide resin was added as a dry strength agent and no carboxymethyl cellulose was applied. The basis weight of the obtained packaging base paper was 77.7 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.79g / cm 3 It was.

[0069] Example 5 A packaging base paper was obtained in the same manner as in Example 1, except that carboxymethyl cellulose was not applied. The basis weight of the obtained packaging base paper was 80.5 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.59g / cm 3 It was.

[0070] Example 6 In Example 1, the amount of carboxymethyl cellulose attached to the base paper was 1.15 g / m2 in terms of solid content on both sides of the base paper. 2 (0.575g / m per side 2 ) and no polyacrylamide resin was added as a dry strength agent to obtain a packaging base paper in the same manner as in Example 1. The basis weight of the obtained packaging base paper was 81.1 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.62g / cm 3 It was.

[0071] Example 7 A packaging base paper was obtained in the same manner as in Example 3, except that after drying, calendaring was performed at a linear pressure of 150 kg / cm and 3 nips. The basis weight of the obtained packaging base paper was 80.8 g / m 2 The packaging base paper has a freeness of 600mlCSF and a density of 0.96g / cm 3 It was.

[0072] Example 8 100 parts of beaten softwood bleached kraft pulp was dispersed in water to prepare a pulp slurry, and 0.2 parts of a dry strength agent (product name: DA4104 / Seiko PMC, polyacrylamide resin) with a mass average molecular weight (Mw) of about 1 million, 0.5 parts of a sizing agent (product name: AL1300 / Seiko PMC, modified rosin emulsion), and 1.2 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. The obtained raw material slurry was used to make paper using a Fourdrinier papermaking machine to obtain a single-layer base paper. The inlet concentration (raw material concentration) of the head box was 1.0 mass%. Then, a 1% concentration starch aqueous solution was added to both sides of the base paper at a solid content of 2.0 g / m2 using a two-roll size press. 2 (1.0g / m per side 2 After drying, the mixture was calendered at a linear pressure of 80 kg / cm and one nip to obtain the desired packaging base paper. The basis weight of the resulting packaging base paper was 81.3 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.75g / cm 3 It was.

[0073] Example 9 <Base paper manufacturing> 100 parts of beaten softwood unbleached kraft pulp was dispersed in water to prepare a pulp slurry, and 0.2 parts of a dry strength agent (product name: DA4104 / Seiko PMC, polyacrylamide resin) with a mass average molecular weight (Mw) of about 1 million, 0.25 parts of a sizing agent (product name: AL1300 / Seiko PMC, modified rosin emulsion), and 0.5 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. Paper was made from the obtained raw material slurry using a standard square sheet machine, and then dried at 120°C in a hot air dryer and calendered with a linear pressure of 80 kg / cm and one nip to obtain a paper weight of 81.0 g / m2. 2 A base paper of the above formula was obtained.

[0074] <Coating> The obtained base paper was impregnated with an aqueous solution of carboxymethylcellulose (product name: SG Cellogen PR, sodium carboxymethylcellulose, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., degree of substitution 0.6-0.7, degree of polymerization 220-250, molecular weight 47000-54000) and dried at 130°C in a rotary dryer to obtain the intended packaging base paper. The amount of carboxymethylcellulose attached to the base paper was 1.0 g / m2 in terms of solid content on both sides of the base paper. 2 (0.5g / m per side 2 The basis weight of the resulting packaging base paper was 82.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.70g / cm 3 It was.

[0075] Example 10 In Example 9, the carboxymethyl cellulose aqueous solution was not applied, and the polyvinyl alcohol aqueous solution (shown as "PVA" in the table) was applied at a solid content of 4.0 g / m2 on both sides of the base paper. 2 (2.0g / m per side 2 A packaging base paper was obtained in the same manner as in Example 9, except that the base paper was impregnated with cellulose acetate. The basis weight of the obtained packaging base paper was 85.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.70g / cm 3 It was.

[0076] Example 11 100 parts of beaten softwood bleached kraft pulp was dispersed in water to prepare a pulp slurry, and 0.2 parts of a dry paper strength agent (product name: DA4104 / Seiko PMC, polyacrylamide resin) with a mass average molecular weight (Mw) of about 1 million, 0.5 parts of a sizing agent (product name: AL1300 / Seiko PMC, modified rosin emulsion), and 1.2 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. The obtained raw material slurry was used to make paper using a fourdrinier papermaking machine to obtain a single-layer base paper. The inlet concentration (raw material concentration) of the head box was 0.2% by mass. After drying, the paper was calendered at a linear pressure of 80 kg / cm and a nip count of 1 nip to obtain the desired packaging base paper. The resulting packaging base paper had a basis weight of 81.3 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.75g / cm 3 It was.

[0077] Example 12 Packaging base paper was obtained in the same manner as in Example 11, except that a two-layer base paper was obtained using a cylinder paper machine instead of a Fourdrinier paper machine. The same raw material slurry was used for the base paper, and two layers were made together so that each layer had the same basis weight. The raw material concentration in the vat at the inlet of the cylinder paper machine was 0.2 mass% for both layers. The basis weight of the obtained packaging base paper was 79.4 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.75g / cm 3 It was.

[0078] (Example 13) Packaging base paper was obtained in the same manner as in Example 11, except that a three-layer base paper was obtained using a cylinder paper machine instead of a Fourdrinier paper machine. The same raw material slurry was used for the base paper, and three layers were made together so that each layer had the same basis weight. The raw material concentration in the vat at the inlet of the cylinder paper machine was 0.2 mass% for all three layers. The basis weight of the obtained packaging base paper was 79.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.77g / cm 3 It was.

[0079] Example 14 <Manufacture of base paper> 100 parts of beaten softwood bleached kraft pulp was dispersed in water to prepare a pulp slurry, and 0.25 parts of a sizing agent (product name: AL1300 / manufactured by Seiko PMC, modified rosin emulsion) and 0.5 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. The raw material slurry obtained was used to make paper using a standard square sheet machine, and then dried at 120°C in a hot air dryer to produce a paper with a basis weight of 80 g / m. 2 A single layer base paper was obtained. <Coating> The resulting base paper was coated with a starch aqueous solution and dried at 130°C in a rotary dryer to obtain the intended packaging base paper. The amount of starch attached to the base paper was 1g / m on both sides of the base paper. 2 The basis weight of the resulting packaging base paper was 81.0 g / m 2 The freeness of the packaging paper is 580ml and the density is 0.62g / cm 3 It was.

[0080] Example 15 A packaging base paper was obtained in the same manner as in Example 3, except that the coating of the carboxymethyl cellulose aqueous solution was not performed. The basis weight of the obtained packaging base paper was 80.5 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.79g / cm 3 It was.

[0081] (Example 16) Packaging base paper was obtained in the same manner as in Example 1, except that no polyacrylamide resin was added as a dry strength agent and the inlet concentration in the head box was 1.0 mass%. The basis weight of the obtained packaging base paper was 81.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.62g / cm 3 It was.

[0082] (Example 17) A packaging base paper was obtained in the same manner as in Example 3, except that the aqueous carboxymethyl cellulose solution was not applied, and after drying, calendaring was performed at a linear pressure of 150 kg / cm and 3 nips. The basis weight of the obtained packaging base paper was 80.6 g / m2 The packaging base paper has a freeness of 580mlCSF and a density of 0.96g / cm 3 It was.

[0083] (Example 18) A packaging base paper was obtained in the same manner as in Example 1, except that a polyacrylamide resin was not added as a dry strength agent, and after drying, calendaring was performed at a linear pressure of 150 kg / cm and 3 nips. The basis weight of the obtained packaging base paper was 81.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.96g / cm 3 It was.

[0084] (Example 19) In Example 1, the amount of carboxymethyl cellulose attached to the base paper was 1.15 g / m2 in terms of solid content on both sides of the base paper. 2 (0.575g / m per side 2 A packaging base paper was obtained in the same manner as in Example 1, except that the inlet concentration in the head box was 1.0 mass%, and the paper was dried and then calendered with a linear pressure of 150 kg / cm and 3 nips. The basis weight of the obtained packaging base paper was 80.3 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.96g / cm 3 It was.

[0085] Comparative Example 1 A packaging base paper was obtained in the same manner as in Example 1, except that the degree of beating of the softwood bleached kraft pulp was adjusted. The basis weight of the obtained packaging base paper was 81.3 g / m 2 , disintegration freeness is 420mlCSF, density is 0.61g / cm 3 The amount of carboxymethyl cellulose attached to the base paper was 1.0 g / m2 in terms of solid content on both sides of the base paper. 2 (0.5g / m per side 2 ) was.

[0086] Comparative Example 2 A packaging base paper was obtained in the same manner as in Example 1, except that 50 parts of beaten bleached softwood kraft pulp and 50 parts of beaten bleached hardwood kraft pulp were used in the preparation of the pulp slurry in Example 1. The basis weight of the obtained packaging base paper was 81.3 g / m 2 , disintegration freeness is 580mlCSF, density is 0.62g / cm 3 The amount of carboxymethyl cellulose attached to the base paper was 1.0 g / m2 in terms of solid content on both sides of the base paper. 2 (0.5g / m per side 2 ) was.

[0087] Comparative Example 3 70 parts of beaten bleached softwood kraft pulp and 30 parts of beaten bleached hardwood kraft pulp were dispersed in water to prepare a pulp slurry, and 0.25 parts of a sizing agent (product name: AL1300 / manufactured by Seiko PMC, modified rosin emulsion) and 0.5 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. The obtained raw material slurry was used to make paper using a Fourdrinier papermaking machine to obtain a single-layer base paper. The inlet concentration (raw material concentration) of the head box was 0.2% by mass. After drying, the paper was subjected to a calendar treatment at a linear pressure of 150 kg / cm and 3 nips to obtain a packaging base paper. The resulting packaging base paper had an average basis weight of 80.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.96g / cm 3 It was.

[0088] Comparative Example 4 <Base paper manufacturing> 70 parts of beaten bleached softwood kraft pulp and 30 parts of beaten bleached hardwood kraft pulp were dispersed in water to prepare a pulp slurry, and 0.25 parts of a sizing agent (product name: AL1300 / manufactured by Seiko PMC, modified rosin emulsion) and 0.5 parts of aluminum sulfate were added to the pulp slurry to obtain a raw material slurry. Using the obtained raw material slurry, a single-layer base paper was obtained by papermaking using a fourdrinier papermaking machine. The inlet concentration (raw material concentration) of the head box was 1.0% by mass. After drying, the paper was calendered at a linear pressure of 150 kg / cm and 3 nips.

[0089] <Coating> A carboxymethylcellulose aqueous solution (product name: SG Cellogen PR, sodium carboxymethylcellulose, Daiichi Kogyo Seiyaku Co., Ltd., substitution degree 0.6-0.7, polymerization degree 220-250, molecular weight 47000-54000) was applied to the obtained base paper using a two-roll size press, and the base paper was dried at 130°C in a rotary dryer to obtain the intended packaging base paper. The amount of carboxymethylcellulose attached to the base paper was 1.00 g / m2 in terms of solid content on both sides of the base paper. 2 (0.50g / m per side 2 The basis weight of the resulting packaging base paper was 80.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.96g / cm 3 It was.

[0090] Comparative Example 5 70 parts of beaten bleached softwood kraft pulp and 30 parts of beaten bleached hardwood kraft pulp were dispersed in water to prepare a pulp slurry, and 0.2 parts of a polyacrylamide resin with a mass average molecular weight (Mw) of 3 million was added as a dry paper strength enhancer to the pulp slurry, 0.25 parts of a sizing agent (product name: AL1300 / manufactured by Seiko PMC Co., Ltd., modified rosin emulsion), and 0.5 parts of aluminum sulfate were added to obtain a raw material slurry. The obtained raw material slurry was used to make paper using a fourdrinier papermaking machine to obtain a single-layer base paper. The inlet concentration (raw material concentration) of the head box was 1.0% by mass. After drying, the paper was subjected to a calendar treatment at a linear pressure of 150 kg / cm and 3 nips to obtain a packaging base paper. The resulting packaging base paper had a basis weight of 80.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.96g / cm 3 It was.

[0091] Comparative Example 6 70 parts of beaten bleached softwood kraft pulp and 30 parts of beaten bleached hardwood kraft pulp were dispersed in water to prepare a pulp slurry, to which 0.25 parts of a sizing agent (product name: AL1300 / manufactured by Seiko PMC, modified rosin emulsion) and 0.5 parts of aluminum sulfate were added to obtain a raw material slurry. The obtained raw material slurry was used to make paper on a Fourdrinier papermaking machine to obtain a single-layer base paper. The inlet concentration (raw material concentration) in the head box was 1.0% by mass. No calendering was performed. The U.S. basis weight of the obtained packaging base paper was 80.0 g / m 2 The packaging base paper has a freeness of 580mlCSF and a density of 0.62g / cm 3 It was.

[0092] The obtained packaging base paper was evaluated by the following method. The obtained results are shown in Table 1. In addition, although the results are not shown here, the tensile strength was also measured, and it was confirmed that for Examples 1 to 19, the tensile strength in the machine direction was 6.0 kN / m or more.

[0093] (formation index) The texture index was measured and calculated using a β-ray fabric total tester manufactured by Ambertec under the following measurement conditions. Measurement conditions: Measurement area 70mm x 70mm, measurement pitch 3.5mm x 3.5mm Calculation method: Formation index = STD ÷ (grammage weight) 1 / 2 In this case, STD is the standard deviation of mass from the basis weight. The smaller the formation index, the better the formation.

[0094] (Puncture strength) Using an Autograph Precision Universal Tester (AGS-10kNX: manufactured by Shimadzu Corporation), measurements were taken according to the following method in accordance with "7.5 Puncture Strength Test" in "JIS Z 1707:2019 General Rules for Food Packaging Plastic Films." The test pieces of packaging base paper were conditioned for 24 hours at 23°C x 50% rh. 1. The test piece was fixed in a jig and a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm was pierced at a test speed of 50 mm / min, and the maximum force (N) until the needle penetrated was measured. 2. Each test piece was pierced at 15 points, and the average value was taken as the piercing strength (N).

[0095] (Puncture strength per unit basis weight) The puncture strength per unit basis weight was calculated using the following formula (1). The puncture strength tends to be proportional to the basis weight, and in this embodiment, the comparison is made based on the puncture strength per unit basis weight. Formula (1): Puncture strength (N) / grams weight (g / m 2 ) = puncture strength per unit basis weight (N / g / m 2 )

[0096] (Tensile strength) The tensile strength (kN / m) of the packaging base paper was measured according to the method specified in JIS P 8113 "Paper and paperboard - Test methods for tensile properties - Part 2: Constant speed extension method."

[0097] Table 1 shows an overview of the configuration of the packaging base paper obtained in each Example and Comparative Example and the evaluation results. The packaging base paper obtained in each Example of the present invention, which has two or more characteristics out of Items A to D, had excellent puncture strength. Here, the packaging papers of Examples 1 to 3 and 9, which have all four of Items A to D, have a puncture strength per unit basis weight of 0.095 to 0.116 N / g / m 2 This is the most preferred embodiment of the present invention. Furthermore, the packaging papers of Examples 5 to 7, 10 to 13, and 15, which have any three of the above four items, were packaging base papers with excellent puncture strength, with puncture strength per unit basis weight of 0.089 to 0.099. Furthermore, the packaging papers of Examples 4, 8, 14, and 16 to 19, which have any two of the above four items, were packaging base papers with excellent puncture strength, with puncture strength per unit basis weight of 0.088 to 0.096. Furthermore, although the results are not shown here, the tensile strength was also sufficient for practical use (longitudinal strength of 6.0 kN / m or more).

[0098] In contrast, the packaging papers of Comparative Examples 3 to 6, which had only one of the above four items, did not have sufficient puncture strength. Considering these Examples and Comparative Examples 3 to 6, it was found that none of the above four items A to D was particularly effective in improving puncture strength, and the four items contributed to improving puncture strength on average. In contrast, the packaging base paper obtained in Comparative Example 1 had low disintegration freeness and poor puncture strength. The packaging base paper obtained in Comparative Example 2 had poor puncture strength because the N pulp content was too low.

[0099] [Table 1]

Claims

1. The packaging base paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the macerated freeness is 440 to 690 ml (CSF), the formation index measured by the total β-ray ground is 1 or less, and at least one surface of the base paper is coated with a metal salt of carboxymethylcellulose.

2. The packaging base paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, the pulp has a disintegrated freeness of 440 to 690 ml (CSF), contains a polyacrylamide resin, and has a metal salt of carboxymethylcellulose applied to at least one surface of the base paper.

3. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegrated freeness of 440 to 690 ml (CSF) and a density of 0.55 to 0.90 g / cm 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

4. The packaging base paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, has a disintegrated freeness of 440 to 690 ml (CSF), has a formation index of 1 or less as measured by the total β-ray material, and contains a polyacrylamide resin.

5. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegrated freeness of 440 to 690 ml (CSF), a formation index measured by the total β-ray material is 1 or less, and a density of 0.55 to 0.90 g / cm 3 The packaging base paper is characterized by:

6. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegration freeness of 440 to 690 ml (CSF), contains a polyacrylamide resin, and has a density of 0.55 to 0.90 g / cm. 3 The packaging base paper is characterized by:

7. The packaging base paper is made of a base paper mainly composed of pulp, in which 70% by mass or more of the pulp is softwood pulp, has a disintegrated freeness of 440 to 690 ml (CSF), has a formation index of 1 or less measured by total β-ray ground, contains a polyacrylamide resin, and has a metal salt of carboxymethylcellulose applied to at least one surface of the base paper.

8. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegrated freeness of 440 to 690 ml (CSF), a formation index measured by the total β-ray material is 1 or less, and a density of 0.55 to 0.90 g / cm 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

9. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegration freeness of 440 to 690 ml (CSF), contains a polyacrylamide resin, and has a density of 0.55 to 0.90 g / cm. 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

10. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegrated freeness of 440 to 690 ml (CSF), a formation index measured by the total of β-rays is 1 or less, contains a polyacrylamide resin, and has a density of 0.55 to 0.90 g / cm. 3 The packaging base paper is characterized by:

11. The paper is made of a base paper mainly composed of pulp, and 70% by mass or more of the pulp is softwood pulp. The paper has a disintegrated freeness of 440 to 690 ml (CSF), a formation index measured by the total of β-rays is 1 or less, contains a polyacrylamide resin, and has a density of 0.55 to 0.90 g / cm. 3 and a metal salt of carboxymethyl cellulose is applied to at least one surface of the base paper.

12. The packaging base paper according to any one of claims 1 to 11, further comprising a paper strength agent and / or a sizing agent.

13. The puncture strength per unit weight is 0.087 N / g / m 2 The packaging base paper according to any one of claims 1 to 11, characterized in that

14. Basis weight: 50-150g / m 2 The packaging base paper according to any one of claims 1 to 11,

15. The coating amount of the metal salt of carboxymethyl cellulose is 0.1 to 1.2 g / m2 in terms of solid content per one side of the base paper. 2 The packaging base paper according to any one of claims 1 to 3, 7 to 9 and 11,

16. The packaging base paper according to any one of claims 1 to 3, 7 to 9 and 11, wherein the metal salt of carboxymethylcellulose is sodium carboxymethylcellulose.

17. The packaging base paper according to any one of claims 2, 4, 6, 7, and 9 to 11, wherein the content of the polyacrylamide resin is 0.1 to 0.9% by mass relative to the pulp in the base paper.

18. The packaging base paper according to any one of claims 2, 4, 6, 7, and 9 to 11, characterized in that the polyacrylamide resin has a mass average molecular weight (Mw) of 350,000 to 3,700,000.

19. 12. The packaging base paper according to any one of claims 1 to 11, characterized in that the base paper is a combination of two or more layers.

20. The packaging base paper according to any one of claims 1 to 11, characterized in that the softwood pulp is softwood unbleached kraft pulp (NUKP).

21. A method for producing packaging base paper having a disintegrated freeness of 440 to 690 ml (CSF) is characterized in that a pulp slurry is prepared in which 70 mass % or more of the pulp is softwood pulp, then the concentration of the raw material at the papermaking machine inlet (raw material concentration) is set to 0.1 to 0.9 mass %, paper is made in a papermaking machine, and the obtained base paper is impregnated with an aqueous carboxymethyl cellulose solution and dried.

22. A method for producing packaging base paper having a disintegrated freeness of 440 to 690 ml (CSF) is characterized by preparing a pulp slurry in which 70 mass % or more of the pulp is softwood pulp, then preparing a raw material slurry containing 0.1 to 0.9 parts by mass of a polyacrylamide-based resin per 100 parts by mass of the pulp slurry, making paper using the obtained raw material slurry in a papermaking machine, and then impregnating the obtained base paper with an aqueous carboxymethyl cellulose solution and drying it.

23. A method for producing packaging base paper having a disintegrated freeness of 440 to 690 ml (CSF), comprising the steps of: preparing a pulp slurry in which 70 mass % or more of the pulp is softwood pulp; then preparing a raw material slurry containing 0.1 to 0.9 mass parts of a polyacrylamide-based resin per 100 mass parts of the pulp slurry; and using the obtained raw material slurry to make paper in a papermaking machine with a raw material concentration at the papermaking machine inlet of 0.1 to 0.9 mass %.

24. A method for producing packaging base paper having a disintegrated freeness of 440 to 690 ml (CSF), comprising the steps of: preparing a pulp slurry in which 70 mass % or more of the pulp is softwood pulp; preparing a raw material slurry containing 0.1 to 0.9 mass parts of a polyacrylamide-based resin per 100 mass parts of the pulp slurry; using the obtained raw material slurry to make paper in a papermaking machine with a raw material concentration at the papermaking machine inlet of 0.1 to 0.9 mass % (raw material concentration); and impregnating the obtained base paper with an aqueous carboxymethyl cellulose solution and drying.

25. The method for producing packaging base paper according to any one of claims 21 to 24, comprising calendering the dried packaging base paper at a linear pressure of 10 to 100 kg / cm and / or at a nip number of 1 to 3.

Citation Information

Patent Citations

  • Kraft paper

    JP2010229564A

  • Method for producing kraft paper

    JP2013217005A

  • Paper-made barrier packaging material

    JP2014173201A

  • Kraft paper and method of producing kraft paper

    JP2015021209A

  • Method for producing pattern paper

    JP2016169445A