Resin foam and foam member
A resin foam with reduced petroleum-derived resin content and plant-derived polyolefin composition addresses the challenge of carbon dioxide emissions and shock absorption, offering superior protection for thin electronic devices.
Patent Information
- Application Number
- JP2024019555
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-02-13
- Publication Date
- 2024-10-25
AI Technical Summary
Existing resin foams used in electronic device cushioning materials face challenges in reducing carbon dioxide emissions and achieving excellent shock absorption properties, particularly as devices become thinner and components smaller.
A resin foam with a petroleum-derived resin content of 50% by weight or less, optimized through a specific density formula, and incorporating plant-derived polyolefin resins, such as polypropylene, to achieve low apparent density and controlled cell structure for enhanced shock absorption.
The solution results in a resin foam that reduces carbon dioxide emissions while providing excellent shock absorption properties, flexibility, and adaptability to narrow clearances, suitable for protecting smaller electronic components.
Smart Images

Figure 2024152611000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin foam and a foam member. [Background technology]
[0002] Foam materials are often used as cushioning materials for protecting the screens, substrates, and electronic components of electronic devices. In recent years, in response to the trend toward thinner electronic devices, there is a demand for narrower clearances in the areas where cushioning materials are arranged. Furthermore, as electronic devices become smaller and more multifunctional, there is a trend toward smaller electronic components being used, and there is a demand for thinner cushioning materials (foam materials) that have excellent shock absorption properties. In addition, in response to the increasing demand for environmental consideration in recent years, there is a demand for reduced carbon dioxide emissions from the above-mentioned cushioning materials (foam materials). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP2017-186504A [Patent Document 2] JP2015-034299A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a resin foam that can contribute to reducing carbon dioxide emissions and has excellent impact absorption properties. [Means for solving the problem]
[0005] [1] A resin foam according to an embodiment of the present invention is a resin foam having a cell structure, in which a content ratio a of a petroleum-derived resin is 50% by weight or less and which satisfies the following formula (1): [Apparent density (g / cm 3)] < -0.0025 × [content of petroleum-derived resin a (%)] + 0.48 ··· (1) [2] In the resin foam according to the above item [1], the aspect ratio of the cells contained in the resin foam may be 4 or less. [3] The resin foam according to the above [1] or [2], wherein the 50% compressive load of the resin foam is 40 N / cm 2 It may be the following. [4] The resin foam according to any one of [1] to [3] above, wherein the 25% compressive load of the resin foam is 25 N / cm 2 It may be the following. [5] In the resin foam according to any one of the above [1] to [4], the resin foam may have an average cell diameter of 200 μm or less. [6] The resin foam according to any one of [1] to [5] above, wherein the resin foam has an apparent density of 0.4 g / cm 3 It may be the following. [7] In the resin foam according to any one of the above [1] to [6], the resin foam may have a coefficient of variation of cell diameter of 0.6 or less. [8] The resin foam according to any one of [1] to [7] above may contain a plant-derived polyolefin resin. [9] The resin foam described in [8] above may contain a plant-derived polyolefin as the plant-derived polyolefin-based resin, and the plant-derived polyolefin may have a melt flow rate at a temperature of 230°C of less than 20 g / 10 min.
[10] In the resin foam according to any one of [1] to [9] above, the plant-derived polyolefin may have a melt tension of 10 cN or more.
[11] In the resin foam of [8] above, the plant-derived polyolefin may have a die swell ratio of 1.5 or less at a melting point +20°C.
[12] The resin foam according to any one of the above [1] to
[11] , wherein the resin composition forming the resin foam may have a die swelling ratio of 1.5 or less at a melting point + 20°C of the resin composition.
[13] The resin foam according to any one of [8] to
[12] above may contain a plant-derived polypropylene-based polymer as the plant-derived polyolefin-based resin.
[14] In the resin foam described in any one of [8] to
[13] above, the plant-derived polyolefin-based resin may be a mixture of a polyolefin other than a polyolefin-based elastomer and a polyolefin-based elastomer, and the polyolefin may be a plant-derived polyolefin, and the polyolefin-based elastomer may be a plant-derived polyolefin-based elastomer or a petroleum-derived polyolefin-based elastomer.
[15] The resin foam according to any one of [1] to
[14] above may have a heat-meltable layer on one or both sides.
[16] A foam member according to one embodiment of the present invention comprises a resin foam layer composed of a resin foam described in any one of [1] to
[15] above, and a pressure-sensitive adhesive layer arranged on at least one side of the resin foam layer. Effect of the Invention
[0006] According to the present invention, it is possible to provide a resin foam which can contribute to reducing carbon dioxide emissions and has excellent impact absorption properties. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of a foam member according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A. Resin foam A-1. Overview of resin foam In the resin foam according to the embodiment of the present invention, the content ratio a of the petroleum-derived resin is 50% by weight or less, and the following formula (1) is satisfied. [Apparent density (g / cm 3 )] < -0.0025 × [content of petroleum-derived resin a (%)] + 0.48 ··· (1) The content ratio a of the petroleum-derived resin is a content ratio based on the total amount of resin constituting the resin foam.
[0009] The resin foam has a bubble structure (cell structure). Examples of the bubble structure (cell structure) include a closed cell structure, an open cell structure, and a semi-open and semi-closed cell structure (a cell structure in which a closed cell structure and an open cell structure are mixed). Preferably, the cell structure of the resin foam is a semi-open and semi-closed cell structure. Typically, the resin foam of the present invention is obtained by foaming a resin composition. The resin composition is a composition containing at least a resin that constitutes the resin foam.
[0010] According to an embodiment of the present invention, the content ratio a of the petroleum-derived resin is set to the above range, and the apparent density (g / cm 3 ) and the content ratio a (%) of the petroleum-derived resin satisfy the above relationship, a resin foam with reduced carbon dioxide emissions can be provided. Furthermore, according to the present invention, by focusing on the apparent density and the content ratio a of the petroleum-derived resin and optimizing the relationship between them, it is possible to achieve both reduced carbon dioxide emissions and impact absorption properties. The above resin foam is advantageous in that it is thin yet has excellent impact absorption properties and flexibility. In other words, one of the major achievements of the present invention is that it has achieved improved impact absorption properties while at the same time reducing carbon dioxide emissions.
[0011] In the resin foam, the content ratio a of the petroleum-derived resin is preferably less than 45% by weight, and more preferably less than 40% by weight. If the content is within such a range, the above-mentioned effects become prominent.
[0012] Preferably, the resin foam contains a plant-derived resin. More preferably, the resin foam contains a plant-derived polyolefin-based resin. Even more preferably, the resin foam contains a plant-derived polypropylene-based resin. If a plant-derived polypropylene-based resin is used, the above effects become more pronounced, and further, a resin foam having excellent heat resistance can be obtained.
[0013] In addition, the biomass ratio (the ratio of sample carbon to standard modern carbon) of petroleum-derived resins and plant-derived resins is 14 The resins derived from petroleum are classified according to their C concentration. 14 It does not contain C (radioactive carbon-14, half-life 5730 years). On the other hand, plant-derived resins are 14 C (radioactive carbon-14, half-life 5730 years). The biomass ratio of the resin derived from the above plants is preferably 50% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. 14 The concentration of C can be measured by accelerator mass spectrometry.
[0014] In the resin foam, the content b of the plant-derived resin is preferably more than 50% by weight, more preferably 45% by weight or more, and further preferably 40% by weight or more. If it is within such a range, the above-mentioned effects become remarkable.
[0015] In one embodiment, the value calculated by "-0.0025 x [content ratio a (%) of petroleum-derived resin] + 0.48" may be preferably 0.01 or more, 0.03 or more, or 0.05 or more. Also, the value calculated by "-0.0025 x [content ratio a (%) of petroleum-derived resin] + 0.48" may be 0.5 or less, 0.4 or less, or 0.3 or less.
[0016] A-2. Characteristics of resin foam The apparent density of the resin foam is preferably 0.4 g / cm 3 More preferably, it is 0.3 g / cm or less. 3 More preferably, it is 0.2 g / cm or less. 3 More preferably, it is 0.1 g / cm or less. 3 More preferably, it is 0.08 g / cm or less. 3 More preferably, it is 0.05 g / cm or less. 3 More preferably, it is 0.04 g / cm or less. 3 More preferably, it is 0.03 g / cm or less. 3The apparent density of the resin foam is preferably 0.01 g / cm or less. 3 More preferably, it is 0.02 g / cm 3 More preferably, it is 0.03 g / cm 3 That is all. The foamability can be judged by the apparent density. In the present invention, by setting the apparent density in the above range, a resin foam excellent in flexibility and impact absorption can be obtained even though it is a thin layer. In addition, it is possible to reduce carbon dioxide emissions. The method for measuring the apparent density will be described later.
[0017] The resin foam has a cell ratio of preferably 97% or less, more preferably 96% or less. The resin foam has a cell ratio of preferably 30% or more, more preferably 50% or more, and even more preferably 60% or more. Within such a range, a resin foam having appropriate flexibility can be obtained.
[0018] The cell density of the resin foam is preferably 30 cells / mm 2 More preferably, 50 pieces / mm 2 More preferably, 70 pieces / mm 2 More preferably, 80 pieces / mm 2 More preferably, 90 pieces / mm 2 More preferably, it is 100 pieces / mm 2 More preferably, the number is 110 / mm 2 More preferably, 120 pieces / mm 2 This is the above. Within this range, a resin foam having favorable flexibility and excellent punching processability can be obtained. Furthermore, the higher the cell number density, the easier it is to store energy when compressed, and a resin foam having excellent compression recovery force can be obtained. The upper limit of the cell number density of the resin foam is preferably 400 cells / mm 2 and more preferably 350 pieces / mm 2 and more preferably 300 pieces / mm 2 and more preferably 250 pieces / mm 2and particularly preferably 200 pieces / mm 2 The cell number density of a resin foam is the cell number density in a cross section observed in a randomly selected cross section of the resin foam, and can be determined by image analysis of the cross section of the resin foam.
[0019] The average bubble diameter (average cell diameter) of the resin foam is preferably 200 μm or less, more preferably 155 μm or less, even more preferably 145 μm or less, even more preferably 130 μm or less, even more preferably 110 μm or less, even more preferably 90 μm or less, even more preferably 80 μm or less, and even more preferably 70 μm or less. Within such a range, a resin foam having excellent impact absorption properties can be obtained. In one embodiment, the average bubble diameter (average cell diameter) of the resin foam is 90 μm or less. Furthermore, the average bubble diameter (average cell diameter) of the resin foam is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 40 μm or more. When the average bubble diameter (average cell diameter) is within the above range, a resin foam having excellent flexibility and stress dispersion and preferably exhibiting impact absorption properties can be obtained. Furthermore, a resin foam having excellent compression recovery, punching processability, and resistance to repeated impacts can be obtained. A method for measuring the average bubble diameter will be described later.
[0020] The maximum bubble diameter (cell diameter) of the resin foam is preferably 400 μm or less, more preferably 300 μm or less, even more preferably 250 μm or less, even more preferably 220 μm or less, even more preferably 170 μm or less, even more preferably 150 μm or less, even more preferably 130 μm or less, even more preferably 120 μm or less, even more preferably 110 μm or less, and even more preferably 100 μm or less. The maximum bubble diameter (cell diameter) of the resin foam is preferably 40 μm or more, more preferably 60 μm or more, even more preferably 70 μm or more, and particularly preferably 80 μm or more. Within such a range, a resin foam having particularly excellent impact absorption properties can be obtained. In one embodiment, the maximum bubble diameter (cell diameter) of the resin foam is 170 μm or less.
[0021] The coefficient of variation of the bubble diameter (cell diameter) of the resin foam is preferably 0.6 or less, more preferably 0.55 or less, even more preferably 0.5 or less, even more preferably 0.45 or less, and even more preferably 0.40 or less. Within such a range, deformation due to impact becomes uniform, local stress load is prevented, and a resin foam having excellent stress dispersion and particularly excellent impact absorption properties can be obtained. The smaller the coefficient of variation, the more preferable it is, and the lower limit is, for example, 0.15 (preferably 0.1, more preferably 0.01). A method for measuring the coefficient of variation of the bubble diameter will be described later.
[0022] When the cell structure of the resin foam is a semi-open, semi-closed cell structure, the proportion of the closed cell structure therein is preferably 40% or less, more preferably 30% or less. In this specification, the proportion of the closed cell structure of the resin foam is determined, for example, by immersing a measurement object in water in an environment of a temperature of 23°C and a humidity of 50%, measuring the mass thereafter, and then sufficiently drying the object in an oven at 80°C, and then measuring the mass again. In addition, since open cells can retain moisture, the mass of the open cells is measured and determined.
[0023] The aspect ratio of the bubbles in the resin foam is preferably 4 or less, more preferably 3 or less, even more preferably 2 or less, still more preferably 1.5 or less, and particularly preferably 1.3 or less. Within such a range, a resin foam having excellent impact absorption properties can be provided. The aspect ratio of the bubbles in the resin foam is, for example, 1 or more, and preferably greater than 1.1. A method for measuring the aspect ratio of the bubbles in the resin foam will be described later.
[0024] The thickness of the bubble walls (cell walls) of the resin foam is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, particularly preferably 0.7 μm or more, and most preferably 1 μm or more. The thickness of the bubble walls (cell walls) of the resin foam is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 5 μm or less, particularly preferably 4 μm or less, and most preferably 3 μm or less. If it is within such a range, a resin foam having appropriate strength can be obtained. Such a resin foam has excellent punching processability, and is prevented from being torn, generating dust, remaining pieces, etc. during punching. If the thickness of the bubble walls is within the above range, a resin foam having excellent flexibility and stress dispersion can be obtained. The thickness of the bubble walls can be measured by capturing an enlarged image of the bubble part of the resin foam and analyzing the image using the analysis software of the measuring instrument.
[0025] The 50% compression load of the resin foam is preferably 40 N / cm 2 More preferably, it is 20 N / cm 2 or less, and more preferably 10 N / cm 2 More preferably, it is 5 N / cm 2 More preferably, it is 4 N / cm or less. 2 More preferably, it is 3N / cm or less. 2 More preferably, it is 2N / cm or less. 2Within this range, a resin foam having preferable flexibility and impact absorption properties can be obtained. The lower limit of the 50% compression load of the resin foam is, for example, 0.5 N / cm 2 The 50% compression load of a resin foam is the stress (N) when it is compressed to 50% of its compression ratio per unit area (1 cm 2 ) converted.
[0026] The 25% compression load of the resin foam is preferably 25N / cm 2 More preferably, it is 15 N / cm 2 or less, and more preferably 10 N / cm 2 More preferably, it is 6 N / cm or less. 2 More preferably, it is 5 N / cm 2 More preferably, it is 3N / cm or less. 2 More preferably, it is 2 N / cm or less. 2 or less, and more preferably 1.5 N / cm 2 Within this range, a resin foam having preferable flexibility and impact absorption properties can be obtained. The lower limit of the 25% compression load of the resin foam is, for example, 0.5 N / cm 2 The 25% compression load of a resin foam is the stress (N) when it is compressed to 50% of its compression ratio per unit area (1 cm 2 ) converted.
[0027] The thickness of the resin foam is preferably 8000 μm or less, more preferably 5000 μm or less, even more preferably 4000 μm or less, and particularly preferably 2000 μm or less. The thickness of the resin foam is preferably 100 μm or more, more preferably 200 μm or more, even more preferably 300 μm or more, and particularly preferably 400 μm or more. If the thickness is within such a range, a fine and uniform cell structure can be formed, which is advantageous in that excellent impact absorption properties can be exhibited.
[0028] The thickness change rate of the resin foam when compressed is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less. Within such a range, a resin foam having good recovery properties and excellent punching processability can be obtained. In this specification, the "thickness change rate of the resin foam when compressed" refers to the thickness change rate when the resin foam and the adhesive are laminated, pressed and bonded together by rolling three times back and forth with a 5 kg roller, and left for 30 minutes, and is the change rate calculated by the following formula. Thickness change rate during crimping [%] = (thickness before crimping - thickness after crimping) / thickness before crimping) x 100
[0029] The impact absorption of the resin foam is preferably 40% or more, more preferably 55% or more, further preferably 60% or more, particularly preferably 70% or more, and most preferably 80% or more. The impact absorption is measured as follows. A test specimen is formed by placing a resin foam, double-sided tape (product number: No. 5603W, manufactured by Nitto Denko), and a PET film (product number: Diafoil MRF75, manufactured by Mitsubishi Plastics) in that order on top of the impact force sensor. A 66g iron ball is dropped onto the test specimen from a height of 50cm above the PET film, and the impact force F1 is measured. · Also, drop an iron ball directly onto the impact force sensor as described above to measure the impact force F0 of the blank. Calculate the shock absorption (%) from F1 and F0 using the formula (F0-F1) / F0×100.
[0030] The stress retention of the resin foam is preferably 60% or more, more preferably 63% or more. The stress retention of the resin foam is preferably 100% or less, more preferably 95% or less. Within such a range, a resin foam can be obtained that has excellent stress dispersion properties and can exhibit excellent impact absorption even in a thin film. In this specification, the stress retention is the ratio of the tensile strength immediately after stretching to the tensile strength after holding for 120 seconds after stretching (tensile strength after holding for 120 seconds / stress retention immediately after stretching×100) when a resin foam (width 10 mm×length 100 mm) is stretched by 20% in the length direction at a speed of 300 m / min.
[0031] In one embodiment, a resin having a die swell ratio of 1.5 or less at a melting point (melting point of the resin constituting the resin foam) +20°C is used as the resin constituting the resin foam. That is, in one embodiment, the die swell ratio of the resin forming the resin foam at a melting point +20°C before foaming is 1.5 or less. By using a resin having a die swell ratio in the above range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The die swell ratio of the resin forming the resin foam at a melting point +20°C before foaming is preferably 1.5 or less, more preferably 1.25 or less. The lower limit of the die swell ratio of the resin (before foaming) is, for example, 1.05 (preferably 1.02, more preferably 1.01). In addition, the die swell ratio at melting point +20°C of the resin constituting the resin foam (i.e., the resin after foaming) is preferably 1.5 or less, more preferably 1.25 or less, and even more preferably 1.1 or less. The lower limit of the die swell ratio of the resin (after foaming) is, for example, 1.05 (preferably 1.02, more preferably 1.01). In this specification, the die swell ratio means a value obtained by dividing the diameter of the resin discharged when a measurement target sample (resin, resin composition) in a molten state is discharged from a die by the diameter of the die. The die swell ratio is calculated by measuring the diameter of the obtained string-like molded product obtained by extruding a resin in a molten state at melting point +20°C using a die with a length of 10 mm and an aperture of 1 mmφ at a shear rate of 20 mm / s, and calculating the diameter of the molded product (mm) / die aperture (mm). In addition, the melting point of the resin is measured by the peak top temperature of the endothermic peak obtained by differential scanning calorimetry (DSC) measurement. Differential scanning calorimetry (DSC) is measured using a differential scanning calorimeter (e.g., trade name "Q-2000", TA Instruments) under conditions of a sample weight of 3 mg and a heating rate of 10°C / min. When there are two or more peaks, the peak top temperature on the higher temperature side is regarded as the melting point.
[0032] The melt tension of the resin constituting the resin foam is preferably 10 cN or more, more preferably 15 cN or more, even more preferably 20 cN or more, and particularly preferably 25 cN or more. The melt tension of the resin constituting the resin foam is preferably 50 cN or less, more preferably 45 cN or less. Within this range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The melt tension is the melt tension at the melting point of the compound to be measured +20°C. The method for measuring the melt tension is as follows.
[0033] -Method of measuring melt tension of resin The sample to be measured (resin, resin composition) is extruded into a molten strand at an extrusion speed of 8.8 mm / min using a twin capillary rheometer "RH7-2" (manufactured by Rosand Precision) at a temperature 20°C higher than the melting point of the resin and with an orifice diameter of 1 mmφ. The strand is then taken up at a take-up speed of 0.5 m / min. The take-up speed is then increased in increments of 0.1 m / min. The melt tension at which the strand of resin breaks is taken as the "melt tension."
[0034] The resin foam may have any suitable shape depending on the purpose. A typical example of such a shape is a sheet, in which case the resin foam of the present invention may be treated as a resin foam layer.
[0035] When the resin foam is in the form of a sheet (i.e., in the form of a resin foam layer), the thickness is preferably 5000 μm or less, more preferably 4000 μm or less, even more preferably 3000 μm or less, and particularly preferably 2500 μm or less. The thickness of the resin foam is preferably 30 μm or more, more preferably 35 μm or more, even more preferably 40 μm or more, and even more preferably 45 μm or more. The resin foam of the present invention can exhibit excellent impact absorption even if it is thin. Such a resin foam can be suitably used as a protective material applied to a small clearance.
[0036] The resin foam of the present invention may have a heat-melting layer on one or both sides thereof. A resin foam having a heat-melting layer can be obtained, for example, by rolling a resin foam (or a precursor of a resin foam) using a pair of heating rolls heated to a temperature equal to or higher than the melting temperature of the resin composition constituting the resin foam.
[0037] The bubble ratio (cell ratio) of the heat melting layer is preferably 30% or less, more preferably 20% or less, even more preferably 10% or less, particularly preferably 5% or less, and most preferably 0%. The thickness of the heat melting layer is preferably 0.60 mm or less, more preferably 0.40 mm or less, and even more preferably 0.20 mm or less. The thickness of the heat melting layer is preferably 0.05 mm or more, more preferably 0.07 mm or more, and even more preferably 0.09 mm or more.
[0038] A-3. Method for forming resin foam The resin foam can be formed by any suitable method as long as the effect of the present invention is not impaired. A representative example of such a method is a method of foaming a resin composition containing a resin material (polymer). The resin composition contains any suitable resin material (polymer).
[0039] In one embodiment, a resin composition having a die swell ratio of 1.5 or less (preferably 1.25 or less) at the melting point of the resin composition + 20°C is used. Within this range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The lower limit of the die swell ratio of the resin composition is, for example, 1.05 (preferably 1.02, more preferably 1.01). The melting point of the resin composition means the melting point of the compound having the highest melting point among the compounds in the resin composition.
[0040] The melt tension of the resin composition is preferably 10 cN or more, more preferably 15 cN or more, even more preferably 20 cN or more, and particularly preferably 25 cN or more. The melt tension of the resin composition is preferably 50 cN or less, more preferably 45 cN or less. Within such a range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. As described above, the melt tension is the melt tension at the melting point of the compound to be measured (i.e., the resin composition) + 20°C, and the melting point of the resin composition is the melting point of the compound having the highest melting point among the compounds in the resin composition.
[0041] Examples of the polymer include acrylic resins, silicone resins, urethane resins, polyolefin resins, ester resins, rubber resins, etc. The polymers may be used alone or in combination of two or more.
[0042] The content of the polymer is preferably 30 parts by weight or more, more preferably 35 parts by weight or more, and even more preferably 40 parts by weight or more, based on 100 parts by weight of the resin composition. The content of the polymer is preferably 95 parts by weight or less, more preferably 90 parts by weight or less, even more preferably 80 parts by weight or less, and particularly preferably 60 parts by weight or less, based on 100 parts by weight of the resin composition. Within such a range, a resin foam having excellent flexibility and stress dispersion can be obtained.
[0043] In one embodiment, a polyolefin resin is used as the polymer.
[0044] As the polyolefin resin, preferably, a plant-derived polyolefin resin is used, more preferably, a plant-derived polypropylene resin is used. A plant-derived polyolefin resin (preferably, a propylene resin) and a petroleum-derived polyolefin resin may be used in combination.
[0045] The content of the polyolefin resin is preferably 50 parts by weight to 100 parts by weight, more preferably 70 parts by weight to 100 parts by weight, even more preferably 90 parts by weight to 100 parts by weight, particularly preferably 95 parts by weight to 100 parts by weight, and most preferably 100 parts by weight, relative to 100 parts by weight of the above polymer.
[0046] The polyolefin resin is preferably at least one selected from the group consisting of polyolefins and polyolefin elastomers, and more preferably, polyolefins and polyolefin elastomers are used in combination. The polyolefins and polyolefin elastomers may each be used alone or in combination of two or more. In this specification, the term "polyolefin" does not include "polyolefin elastomers".
[0047] When polyolefin and polyolefin elastomer are used in combination as the polyolefin resin, the weight ratio of polyolefin to polyolefin elastomer (polyolefin / polyolefin elastomer) is preferably 1 / 99 to 99 / 1, more preferably 10 / 90 to 90 / 10, further preferably 20 / 80 to 80 / 20, and particularly preferably 30 / 70 to 70 / 30. In one embodiment, the weight ratio of polyolefin to polyolefin elastomer (polyolefin / polyolefin elastomer) is preferably 25 / 75 to 75 / 25, more preferably 35 / 65 to 65 / 35. Within such a range, a resin foam can be obtained that has excellent compression recovery, suppresses shape changes (particularly thickness changes) before and after punching during punching, has appropriate strength, and is excellent in punching processability.
[0048] In one embodiment, a plant-derived polyolefin (preferably a polypropylene-based polymer) is used as the polyolefin, and a plant-derived or petroleum-derived polyolefin-based elastomer is used as the polyolefin-based elastomer. In this case, the weight ratio of the polyolefin (i.e., plant-derived polyolefin) is preferably 50% by weight or more, more preferably 53% by weight or more, even more preferably 60% by weight or more, and even more preferably 70% by weight or more, based on the total weight of the polyolefin and the polyolefin-based elastomer. Within such a range, the effects of the present invention are remarkable. The upper limit of the weight ratio of the polyolefin (i.e., plant-derived polyolefin) is, for example, 99% (preferably 100%) based on the total weight of the polyolefin and the polyolefin-based elastomer.
[0049] As the polyolefin, any suitable polyolefin may be adopted as long as it does not impair the effects of the present invention. Examples of such polyolefins include linear polyolefins and branched (branched) polyolefins. In one embodiment, a branched polyolefin is used as the polyolefin-based resin. In this embodiment, only a branched polyolefin may be used as the polyolefin, or a branched polyolefin and a linear polyolefin may be used in combination. By using a branched polyolefin, a resin foam having a small average cell diameter and excellent impact absorption properties can be obtained. The content of the branched polyolefin is preferably 30 parts by weight or more, more preferably 50 parts by weight or more, relative to 100 parts by weight of the polyolefin. The content of the branched polyolefin is preferably 100 parts by weight or less, more preferably 80 parts by weight or less, relative to 100 parts by weight of the polyolefin.
[0050] The polyolefin may be used alone or in combination of two or more. When one type of polyolefin is used, a plant-derived polyolefin may be used as the polyolefin. When two or more types of polyolefins are used, at least one of them may be a plant-derived polyolefin. The content of the plant-derived polyolefin is preferably 50 parts by weight or more, more preferably 80 parts by weight or more, and even more preferably 90 parts by weight or more, based on 100 parts by weight of the polyolefin blend. It is particularly preferable that all of the polyolefins used are plant-derived polyolefins. As described above, the plant-derived polyolefin is 14 It refers to polyolefins containing C (radioactive carbon-14, half-life 5730 years).
[0051] The polyolefin may be, for example, a polymer containing a structural unit derived from an α-olefin. The polyolefin may be composed of only a structural unit derived from an α-olefin, or may be composed of a structural unit derived from an α-olefin and a structural unit derived from a monomer other than an α-olefin. When the polyolefin is a copolymer, any suitable copolymerization form may be adopted as the copolymerization form. For example, a random copolymer, a block copolymer, etc. may be mentioned.
[0052] The α-olefin that can constitute the polyolefin is preferably, for example, an α-olefin having 2 to 8 carbon atoms (preferably 2 to 6, more preferably 2 to 4) (e.g., ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, etc.). Only one type of α-olefin may be used, or two or more types of α-olefins may be used.
[0053] Examples of monomers other than α-olefins constituting polyolefins include ethylenically unsaturated monomers such as vinyl acetate, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, vinyl alcohol, etc. The monomers other than α-olefins may be of only one type or of two or more types.
[0054] Specific examples of polyolefins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene (propylene homopolymer), copolymers of ethylene and propylene, copolymers of ethylene and an α-olefin other than ethylene, copolymers of propylene and an α-olefin other than propylene, copolymers of ethylene, propylene and an α-olefin other than ethylene and propylene, and copolymers of propylene and an ethylenically unsaturated monomer.
[0055] In one embodiment, a polypropylene-based polymer having a propylene-derived structural unit is used as the polyolefin. Examples of the polypropylene-based polymer include polypropylene (propylene homopolymer), a copolymer of ethylene and propylene, and a copolymer of propylene and an α-olefin other than propylene, and preferably polypropylene (propylene homopolymer). The polypropylene-based polymer may be used alone or in combination of two or more kinds.
[0056] The plant-derived polyolefin is preferably a plant-derived polypropylene-based polymer. The plant-derived polypropylene-based polymer may be a homopolymer of plant-derived propylene, or may be a copolymer of plant-derived propylene and other monomers. In the case of a copolymer, the content of the structural unit based on plant-derived propylene in the copolymer is preferably 50 parts by weight or more, more preferably 70 parts by weight or more, based on 100 parts by weight of the plant-derived polypropylene-based polymer.
[0057] The plant-derived polypropylene-based polymer may be polypropylene produced using biomass as a raw material. For example, it may be a polypropylene-based polymer produced using biopropylene produced by dehydrating propanol produced by fermentation. It may also be a polypropylene-based polymer produced using biopropylene produced during a synthesis reaction of bioethylene. It may also be a polypropylene-based polymer produced using biopropylene synthesized from bioethanol.
[0058] The melt flow rate (MFR) of the polyolefin at a temperature of 230°C is preferably 0.25 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.35 g / 10 min or more. The melt flow rate (MFR) of the polyolefin at a temperature of 230°C is preferably 20 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 6 g / 10 min or less, even more preferably 5 g / 10 min, particularly preferably 1 g / 10 min or less, and most preferably 0.6 g / 10 min or less. In this specification, the melt flow rate (MFR) refers to the MFR measured at a temperature of 230°C and a load of 2.16 kgf (21.2 N) based on ISO1133 (JIS-K-7210). In one embodiment, the die swell ratio and shear viscosity of the resin are controlled by the melt flow rate of the polyolefin constituting the resin foam.
[0059] The melt flow rate (MFR) of the plant-derived polyolefin at a temperature of 230°C is preferably less than 20g / 10min, more preferably less than 10g / 10min, even more preferably less than 6g / 10min, even more preferably less than 5g / 10min, particularly preferably less than 1g / 10min, and most preferably 0.6g / 10min or less. The melt flow rate (MFR) of the plant-derived polyolefin at a temperature of 230°C is preferably 0.25g / 10min or more, more preferably 0.3g / 10min or more, and even more preferably 0.35g / 10min or more. If it is within such a range, the effect of the present invention becomes remarkable. It is particularly advantageous in that a resin foam having excellent impact absorption properties can be obtained.
[0060] In one embodiment, the die swell ratio of the plant-derived polyolefin at melting point +20°C is 1.5 or less (preferably 1.25 or less). Within this range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide. The lower limit of the die swell ratio of the plant-derived polyolefin is, for example, 1.05 (preferably 1.02, more preferably 1.01).
[0061] The melt tension of the plant-derived polyolefin is preferably 10 cN or more, more preferably 15 cN or more, even more preferably 20 cN or more, and particularly preferably 25 cN or more. The melt tension of the plant-derived polyolefin is preferably 50 cN or less, more preferably 45 cN or less. Within this range, a resin foam containing small bubbles and having a low density can be obtained. Such a resin foam has excellent impact absorption properties. It is also advantageous in that it emits less carbon dioxide.
[0062] The weight average molecular weight of the polyolefin is preferably 50,000 or more, more preferably 55,000 or more, and even more preferably 60,000 or more. The weight average molecular weight of the polyolefin is 120,000 or less, more preferably 110,000 or less, and even more preferably 100,000 or less. Within such a range, the die swell ratio and shear viscosity of the resin can be preferably adjusted. Furthermore, the molecular weight distribution (weight average molecular weight / number average molecular weight) of the polyolefin is preferably 7 to 10, more preferably 6 to 9. Within such a range, the die swell ratio and shear viscosity of the resin can be preferably adjusted. The weight average molecular weight and number average molecular weight can be determined by gel permeation chromatography measurement (solvent: tetrahydrofuran, polystyrene equivalent).
[0063] As the polyolefin-based elastomer, any suitable polyolefin-based elastomer may be adopted within the scope of not impairing the effects of the present invention. Examples of such polyolefin-based elastomers include so-called non-crosslinked thermoplastic olefin-based elastomers (TPOs) such as ethylene-propylene copolymers, ethylene-propylene-diene copolymers, ethylene-vinyl acetate copolymers, polybutene, polyisobutylene, chlorinated polyethylene, elastomers in which a polyolefin component and a rubber component are physically dispersed, and elastomers in which a polyolefin component and a rubber component have a microphase separation structure; dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) which are multiphase polymers obtained by dynamically heat treating a mixture containing a resin component A (olefin-based resin component A) forming a matrix and a rubber component B forming a domain in the presence of a crosslinking agent, and which have a sea-island structure in which crosslinked rubber particles are finely dispersed as domains (island phases) in the resin component A which is a matrix (sea phase); and the like.
[0064] The polyolefin-based elastomer preferably contains a rubber component. Examples of such rubber components include those described in JP-A-08-302111, JP-A-2010-241934, JP-A-2008-024882, JP-A-2000-007858, JP-A-2006-052277, JP-A-2012-072306, JP-A-2012-057068, JP-A-2010-241897, JP-A-2009-067969, and JP-A-03 / 002654.
[0065] Specific examples of elastomers having a microphase-separated structure of a polyolefin component and an olefin-based rubber component include elastomers made of polypropylene resin (PP) and ethylene-propylene rubber (EPM), elastomers made of polypropylene resin (PP) and ethylene-propylene-diene rubber (EPDM), etc. The weight ratio of the polyolefin component to the olefin-based rubber component (polyolefin component / olefin-based rubber) is preferably 90 / 10 to 10 / 90, more preferably 80 / 20 to 20 / 80.
[0066] Dynamically crosslinked thermoplastic olefin elastomers (TPV) generally have a higher elastic modulus and smaller compression set than non-crosslinked thermoplastic olefin elastomers (TPO), which gives them good recovery properties and allows them to show excellent recovery properties when made into resin foams.
[0067] As described above, dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) are obtained by dynamically heat treating a mixture containing a resin component A (olefin-based resin component A) that forms a matrix and a rubber component B that forms domains, in the presence of a crosslinking agent. These TPVs are multiphase polymers having an island-sea structure in which crosslinked rubber particles are finely dispersed as domains (island phases) in resin component A, which is the matrix (sea phase).
[0068] Examples of dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) include those described in JP-A-2000-007858, JP-A-2006-052277, JP-A-2012-072306, JP-A-2012-057068, JP-A-2010-241897, JP-A-2009-067969, and JP-A-03 / 002654.
[0069] As the dynamically crosslinked thermoplastic olefin-based elastomer (TPV), commercially available products may be used, such as "Zeotherm" (manufactured by Zeon Corporation), "Thermorun" (manufactured by Mitsubishi Chemical Corporation), and "Sarlink 3245D" (manufactured by Toyobo Co., Ltd.).
[0070] The polyolefin elastomer preferably has a melt flow rate (MFR) of 1.5 g / 10 min or more at 230° C., more preferably 2 g / 10 min or more. The polyolefin elastomer preferably has a melt flow rate (MFR) of 25 g / 10 min or less at 230° C., more preferably 20 g / 10 min or less, and even more preferably 15 g / 10 min. In this way, the melt tension of the polyolefin elastomer is preferably adjusted, and as a result, the effect of the present invention becomes remarkable.
[0071] In one embodiment, two or more polyolefin-based elastomers having different melt flow rates (MFR) at 230° C. within the above range are used in combination. In this case, a polyolefin-based elastomer (low MFR polyolefin-based elastomer) having a melt flow rate (MFR) at 230° C. of preferably 1.5 g / 10 min or more and less than 8 g / 10 min (more preferably 2 g / 10 min to 5 g / 10 min) can be used in combination with a polyolefin-based elastomer (high MFR polyolefin-based elastomer) having a melt flow rate (MFR) at 230° C. of preferably 8 g / 10 min to 25 g / 10 min (more preferably 9 g / 10 min to 20 g / 10 min, and even more preferably 10 g / 10 min to 20 g / 10 min). In this way, the melt tension of the polyolefin-based elastomer is preferably adjusted, and as a result, the effects of the present invention become remarkable.
[0072] The blending ratio of the low MFR polyolefin elastomer to the high MFR polyolefin elastomer (low MFR polyolefin elastomer / high MFR polyolefin elastomer; weight ratio) is preferably 1.5 to 5, more preferably 1.8 to 3.5, and particularly preferably 2 to 3. Within such a range, the melt tension of the polyolefin elastomer can be preferably adjusted, and as a result, the effects of the present invention become remarkable.
[0073] The melt tension of the polyolefin-based elastomer is preferably 5 cN or more, more preferably 10 cN or more. The melt tension of the polyolefin-based elastomer is preferably 50 cN or less. In one embodiment, the die swell ratio and shear viscosity of the resin are controlled by the melt tension of the polyolefin-based elastomer constituting the resin foam.
[0074] The JIS A hardness of the polyolefin elastomer is preferably 30° or more, more preferably 40° or more, even more preferably 45° or more, and most preferably 50° or more. The JIS A hardness of the polyolefin elastomer is preferably 95° or less, more preferably 90° or less, even more preferably 88° or less, particularly preferably 85° or less, and most preferably 83°. The JIS A hardness is measured based on ISO7619 (JIS K6253).
[0075] In one embodiment, the resin foam (i.e., the resin composition) may further contain a filler. By including a filler, it is possible to form a resin foam that requires a large amount of energy to deform the cell walls, and the resin foam exhibits excellent impact absorption properties. Furthermore, by including a filler, it is possible to form a fine and uniform cell structure, which is advantageous in that excellent impact absorption properties can be exhibited. Only one type of filler may be used alone, or two or more types may be used in combination.
[0076] The content of the filler is preferably 10 parts by weight or more, more preferably 30 parts by weight or more, and even more preferably 50 parts by weight or more, based on 100 parts by weight of the polymer constituting the resin foam. The content of the filler is preferably 150 parts by weight or less, more preferably 130 parts by weight or less, and even more preferably 100 parts by weight or less, based on 100 parts by weight of the polymer constituting the resin foam. If the content is within such a range, the above-mentioned effect becomes remarkable.
[0077] In one embodiment, the filler is an inorganic material. Examples of materials constituting the inorganic filler include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, silicon nitride, boron nitride, crystalline silica, amorphous silica, metal (e.g., gold, silver, copper, aluminum, nickel), carbon, graphite, etc.
[0078] In one embodiment, the filler is an organic material. Examples of materials constituting the organic filler include polymethylmethacrylate (PMMA), polyimide, polyamideimide, polyetheretherketone, polyetherimide, and polyesterimide.
[0079] A flame retardant may be used as the filler. Examples of the flame retardant include bromine-based flame retardants, chlorine-based flame retardants, phosphorus-based flame retardants, and antimony-based flame retardants. From the viewpoint of safety, a non-halogen, non-antimony-based flame retardant is preferably used.
[0080] Examples of non-halogen, non-antimony flame retardants include compounds containing aluminum, magnesium, calcium, nickel, cobalt, tin, zinc, copper, iron, titanium, boron, etc. Examples of such compounds (inorganic compounds) include hydrated metal compounds such as aluminum hydroxide, magnesium hydroxide, magnesium oxide-nickel oxide hydrate, and magnesium oxide-zinc oxide hydrate.
[0081] The filler may be subjected to any suitable surface treatment, such as a silane coupling treatment or a stearic acid treatment.
[0082] The bulk density of the filler is preferably 0.8 g / cm 3 More preferably, it is 0.6 g / cm or less. 3or less, and more preferably 0.4 g / cm 3 or less, and particularly preferably 0.3 g / cm 3 Within this range, the filler can be contained with good dispersibility, and the effect of adding the filler can be fully exhibited even with a small filler content. A resin foam with a small filler content is advantageous in that it is highly foamed, flexible, and has excellent stress dispersion and appearance. The lower limit of the bulk density of the filler is, for example, 0.01 g / cm. 3 and preferably 0.05 g / cm 3 and more preferably 0.1 g / cm 3 It is.
[0083] The number average particle diameter (primary particle diameter) of the filler is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. Within such a range, the filler can be contained with good dispersibility and a uniform cell structure can be formed. As a result, a resin foam with excellent stress dispersion and appearance can be obtained. The lower limit of the number average particle diameter of the filler is, for example, 0.1 μm. The number average particle diameter of the filler can be measured using a particle size distribution meter (MicrtracII, Microtrack Bell Co., Ltd.) using a suspension prepared by mixing 1 g of filler in 100 g of water as a sample.
[0084] The specific surface area of the filler is preferably 2 m 2 / g or more, more preferably 4m 2 / g or more, more preferably 6m 2 Within this range, the filler can be incorporated with good dispersibility and a uniform cell structure can be formed. As a result, a resin foam with excellent stress dispersion and appearance can be obtained. The upper limit of the specific surface area of the filler is, for example, 20 m 2 The specific surface area of the packing material can be measured by the BET method, that is, by adsorbing a molecule with a known adsorption area onto the packing material surface at a low temperature using liquid nitrogen, and measuring the amount of the molecule adsorbed.
[0085] The resin composition may contain any other appropriate components as long as the effects of the present invention are not impaired. Such other components may be one type only, or two or more types. Examples of such other components include rubber, resins other than the polymers blended as the resin material, softeners, aliphatic compounds, antiaging agents, antioxidants, light stabilizers, weathering agents, UV absorbers, dispersants, plasticizers, carbon, antistatic agents, surfactants, crosslinking agents, thickeners, rust inhibitors, silicone compounds, tension modifiers, shrinkage inhibitors, flow modifiers, gelling agents, curing agents, reinforcing agents, foaming agents, foam nucleating agents, colorants (pigments, dyes, etc.), pH adjusters, solvents (organic solvents), thermal polymerization initiators, photopolymerization initiators, lubricants, crystal nucleating agents, crystallization accelerators, vulcanizing agents, surface treatment agents, and dispersion aids.
[0086] As described above, the resin foam is typically obtained by foaming a resin composition. As the foaming method (a method for forming bubbles), a method usually used in foam molding, such as a physical method or a chemical method, can be adopted. That is, the resin foam may typically be a foam formed by foaming using a physical method (physical foam), or a foam formed by foaming using a chemical method (chemical foam). The physical method is generally a method in which a gas component such as air or nitrogen is dispersed in a polymer solution and bubbles are formed by mechanical mixing (mechanical foam). The chemical method is generally a method in which cells are formed by gas generated by thermal decomposition of a foaming agent added to a polymer base, to obtain a foam.
[0087] The resin composition to be subjected to foam molding may be prepared, for example, by mixing the components using any appropriate melt kneading device, such as an open-type mixing roll, a non-open-type Banbury mixer, a single-screw extruder, a twin-screw extruder, a continuous kneader, or a pressure kneader.
[0088] Forming a resin foam: One example of embodiment 1 for forming a resin foam is a form in which a resin foam is formed through a step (step A) of mechanically foaming an emulsion resin composition (an emulsion containing a resin material (polymer) and the like). Examples of foaming devices include high-speed shear devices, vibration devices, and pressurized gas discharge devices. Of these foaming devices, high-speed shear devices are preferred from the viewpoints of miniaturizing the bubble diameter and producing a large volume. This one example of embodiment 1 for forming a resin foam is applicable to formation from any resin composition.
[0089] From the viewpoint of film-forming properties, the solids concentration of the emulsion is preferably high. The solids concentration of the emulsion is preferably 30% by weight or more, more preferably 40% by weight or more, and even more preferably 50% by weight or more.
[0090] The bubbles generated by mechanical stirring are gases that have been taken into the emulsion. Any suitable gas may be used as the gas as long as it is inert to the emulsion and does not impair the effects of the present invention. Examples of such gases include air, nitrogen, and carbon dioxide.
[0091] The resin foam of the present invention can be obtained by applying the foamed emulsion resin composition (bubble-containing emulsion resin composition) onto a substrate and drying it (Step B). Examples of the substrate include a release-treated plastic film (such as a release-treated polyethylene terephthalate film), a plastic film (such as a polyethylene terephthalate film), and the like.
[0092] In step B, any appropriate method may be adopted as the coating method and drying method as long as the effects of the present invention are not impaired. Step B preferably includes a preliminary drying step B1 in which the bubble-containing emulsion resin composition applied to the substrate is dried at 50° C. or higher and lower than 125° C., and a main drying step B2 in which the composition is further dried at 125° C. or higher and 200° C. or lower.
[0093] By providing the preliminary drying step B1 and the main drying step B2, it is possible to prevent the coalescence of bubbles and the bursting of bubbles due to a sudden rise in temperature. In particular, in a foamed sheet having a small thickness, the coalescence and bursting of bubbles due to a sudden rise in temperature is likely to occur, so providing the preliminary drying step B1 is very significant. The temperature in the preliminary drying step B1 is preferably 50°C to 100°C. The time for the preliminary drying step B1 is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes. The temperature in the main drying step B2 is preferably 130°C to 180°C or less, more preferably 130°C to 160°C. The time for the main drying step B2 is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes.
[0094] Forming a resin foam: embodiment 2 In one embodiment 2 of forming a resin foam, a foam is formed by foaming a resin composition with a foaming agent. As the foaming agent, a foaming agent usually used for foam molding can be used, and from the viewpoint of environmental protection and low pollution to the foamed object, it is preferable to use a high-pressure inert gas.
[0095] As the inert gas, any suitable inert gas may be adopted as long as it is inert to the resin composition and can be impregnated. Examples of such inert gas include carbon dioxide, nitrogen gas, and air. These gases may be used in combination. Among these, carbon dioxide is preferred from the viewpoint of a large amount of impregnation into the resin material (polymer) and a fast impregnation speed.
[0096] The inert gas is preferably in a supercritical state. That is, it is particularly preferable to use carbon dioxide in a supercritical state. In a supercritical state, the solubility of the inert gas in the resin composition is increased, making it possible to mix the inert gas at a high concentration, and the inert gas becomes highly concentrated when the pressure is suddenly lowered, so that more bubble nuclei are generated, and the density of the bubbles formed by the growth of the bubble nuclei is larger than in other states even if the porosity is the same, so that fine bubbles can be obtained. The critical temperature of carbon dioxide is 31°C, and the critical pressure is 7.4 MPa.
[0097] Examples of the method for forming a foam by impregnating a resin composition with a high-pressure inert gas include a gas impregnation step in which an inert gas is impregnated under high pressure into a resin composition containing a resin material (polymer), a depressurization step in which the pressure is reduced after the gas impregnation step to foam the resin material (polymer), and a heating step in which bubbles are grown by heating as necessary. In this case, a previously molded unfoamed molded body may be impregnated with an inert gas, or a molten resin composition may be impregnated with an inert gas under pressure and then molded during depressurization. These steps may be performed by either a batch method or a continuous method. That is, the resin composition may be molded into an appropriate shape such as a sheet to form an unfoamed resin molded body, and then the unfoamed resin molded body is impregnated with a high-pressure gas and foamed by releasing the pressure, or the resin composition may be kneaded with a high-pressure gas under pressure, and molded and foamed at the same time by releasing the pressure.
[0098] An example of producing a foam by the batch method is shown below. For example, a resin sheet for foam molding is produced by extruding a resin composition using an extruder such as a single screw extruder or a twin screw extruder. Alternatively, the resin composition is uniformly kneaded using a kneader equipped with blades such as a roller, a cam, a kneader, or a Banbury type, and pressed to a predetermined thickness using a hot plate press or the like to produce an unfoamed resin molded body. The unfoamed resin molded body thus obtained is placed in a high-pressure container, and high-pressure inert gas (such as carbon dioxide in a supercritical state) is injected to impregnate the unfoamed resin molded body with the inert gas. When the inert gas is sufficiently impregnated, the pressure is released (usually to atmospheric pressure), and bubble nuclei are generated in the resin. The bubble nuclei may be allowed to grow at room temperature as they are, or may be allowed to grow by heating in some cases. As a heating method, known or commonly used methods such as a water bath, an oil bath, a heated roll, a hot air oven, far infrared rays, near infrared rays, and microwaves can be used. After the bubbles are grown in this manner, the foam can be obtained by rapidly cooling the foam with cold water or the like to fix the shape. The unfoamed resin molded product to be foamed is not limited to a sheet-like product, and various shapes can be used depending on the application. The unfoamed resin molded product to be foamed can be produced by other molding methods such as extrusion molding, press molding, and injection molding.
[0099] An example of producing a foam by a continuous method is shown below. For example, a resin composition is kneaded using an extruder such as a single-screw extruder or a twin-screw extruder while injecting (introducing) a high-pressure gas (particularly an inert gas, or further carbon dioxide) to sufficiently impregnate the resin composition with the high-pressure gas in a kneading impregnation step, and the resin composition is extruded through a die or the like provided at the tip of the extruder to release the pressure (usually to atmospheric pressure), and foaming and foaming are simultaneously performed in a molding decompression step to form the foam. In addition, when foaming in a continuous method, a heating step for growing bubbles by heating may be provided as necessary. After the bubbles are grown in this way, the shape may be fixed by rapidly cooling with cold water or the like as necessary. The high-pressure gas may be introduced continuously or discontinuously. In addition, in the kneading impregnation step and the molding decompression step, for example, an extruder or an injection molding machine may be used. In addition, as a method of heating when growing bubble nuclei, any appropriate method such as a water bath, an oil bath, a heat roll, a hot air oven, far infrared rays, near infrared rays, and microwaves may be used. The foam may have any suitable shape, such as a sheet, a prismatic shape, a cylindrical shape, or an irregular shape.
[0100] The amount of gas mixed when foaming the resin composition is preferably 2% by weight to 10% by weight, more preferably 2.5% by weight to 8% by weight, and even more preferably 3% by weight to 6% by weight, based on the total amount of the resin composition, in order to obtain a highly foamed resin foam.
[0101] The pressure when the resin composition is impregnated with the inert gas can be appropriately selected in consideration of operability and the like. For example, such a pressure is preferably 6 MPa or more (for example, 6 MPa to 100 MPa), and more preferably 8 MPa or more (for example, 8 MPa to 50 MPa). In addition, the pressure when carbon dioxide in a supercritical state is used is preferably 7.4 MPa or more from the viewpoint of maintaining the supercritical state of carbon dioxide. If the pressure is lower than 6 MPa, the bubble growth during foaming is remarkable, and the bubble diameter becomes too large, so that a preferable average cell diameter (average bubble diameter) may not be obtained. This is because, when the pressure is low, the amount of gas impregnated is relatively small compared to that at high pressure, and the bubble nucleation rate decreases and the number of bubble nuclei formed decreases, so that the amount of gas per bubble increases conversely and the bubble diameter becomes extremely large. In addition, in a pressure range lower than 6 MPa, the bubble diameter and bubble density change significantly even with a small change in the impregnation pressure, so that it is easy to make it difficult to control the bubble diameter and bubble density.
[0102] The temperature in the gas impregnation step varies depending on the type of inert gas used and the type of components in the resin composition, and can be selected from a wide range. In consideration of operability, the temperature is preferably 10°C to 350°C. The impregnation temperature when impregnating an inert gas into an unfoamed molded body is preferably 10°C to 250°C, more preferably 40°C to 230°C, in the batch process. In addition, the impregnation temperature when extruding a molten polymer impregnated with a gas to simultaneously perform foaming and molding is preferably 60°C to 350°C in the continuous process. When carbon dioxide is used as the inert gas, the temperature during impregnation is preferably 32°C or higher, more preferably 40°C or higher, in order to maintain a supercritical state.
[0103] In the depressurizing step, the depressurizing speed is preferably 5 MPa / sec to 300 MPa / sec in order to obtain uniform fine bubbles.
[0104] The heating temperature in the heating step is preferably 40°C to 250°C, and more preferably 60°C to 250°C.
[0105] In one embodiment, after obtaining a foamed structure through a predetermined process (for example, after obtaining a resin foam by the method of <Embodiment 1> or <Embodiment 2>), the foamed structure is thinned and then rolled to obtain a resin foam. Through such a process, a resin foam with an appropriately adjusted aspect ratio can be obtained. Also, a resin foam with a small thickness (for example, 0.2 mm or less) can be obtained.
[0106] The foam structure can be thinned using any suitable slicer. The thickness of the foam structure after thinning is preferably 0.01 mm or more, more preferably 0.05 mm or more, even more preferably 0.1 mm or more, and particularly preferably 0.15 mm or more. The upper limit of the thickness of the foam structure after thinning is preferably 3 mm or less, more preferably 2 mm or less, even more preferably 1.5 mm or less, even more preferably 1 mm or less, even more preferably 0.8 mm or less, and particularly preferably 0.5 mm or less. Within such a range, the number of bubbles in the resin foam is particularly preferably adjusted, making it difficult for crushing to occur due to punching, and therefore a resin foam with particularly excellent punching processability can be obtained.
[0107] The roll used in the rolling is preferably a heated roll. The temperature of the roll is preferably 150°C to 250°C, more preferably 160°C to 230°C.
[0108] The rolling ratio of the foamed structure (thickness after rolling / thickness before rolling×100) is preferably 80% or less, more preferably 10% to 80%, further preferably 20% to 75%, and particularly preferably 30% to 75%. Within such a range, a resin foam with an appropriately adjusted aspect ratio can be obtained.
[0109] B. Foam material 1 is a schematic cross-sectional view of a foam member according to one embodiment. The foam member 100 has a resin foam layer 10 and a pressure-sensitive adhesive layer 20 disposed on at least one side of the resin foam layer 10. The resin foam layer 10 is composed of the above-mentioned resin foam.
[0110] The thickness of the resin foam layer of the foamed material is preferably 30 μm or more, more preferably 35 μm or more, even more preferably 40 μm or more, and particularly preferably 45 μm or more. The thickness of the resin foam layer of the foamed material is preferably 5000 μm or less, more preferably 4000 μm or less, even more preferably 3000 μm or less, and more preferably 2500 μm or less. When the thickness of the resin foam layer is within the above range, the resin foam layer can easily follow even a small clearance. When the thickness of the resin foam layer is within the above range, the bubbles can be uniformly contained, and excellent impact absorption properties can be exhibited.
[0111] The thickness of the adhesive layer is preferably 5 μm or more, more preferably 6 μm or more, even more preferably 7 μm or more, and particularly preferably 8 μm or more. The thickness of the adhesive layer is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and most preferably 50 μm or less. When the thickness of the adhesive layer is within the above range, the foam material of the present invention can exhibit excellent impact absorption properties.
[0112] The adhesive layer may be a layer made of any suitable adhesive. Examples of the adhesive constituting the adhesive layer include rubber-based adhesives (synthetic rubber-based adhesives, natural rubber-based adhesives, etc.), urethane-based adhesives, acrylic urethane-based adhesives, acrylic-based adhesives, silicone-based adhesives, polyester-based adhesives, polyamide-based adhesives, epoxy-based adhesives, vinyl alkyl ether-based adhesives, fluorine-based adhesives, and rubber-based adhesives. The adhesive constituting the adhesive layer is preferably at least one selected from acrylic-based adhesives, silicone-based adhesives, and rubber-based adhesives. Such adhesives may be of only one type or of two or more types. The adhesive layer may be of one layer or of two or more layers.
[0113] When classified according to the adhesive form, examples of the adhesive include emulsion type adhesives, solvent type adhesives, ultraviolet cross-linking type (UV cross-linking type) adhesives, electron beam cross-linking type (EB cross-linking type) adhesives, hot melt type adhesives, etc. Such adhesives may be of only one type or of two or more types.
[0114] The water vapor permeability of the adhesive layer is preferably 50 (g / (m 2 24 hours) or less, and more preferably 30 (g / (m 2 24 hours) or less, and more preferably 20 (g / (m 2 24 hours) or less, and particularly preferably 10 (g / (m 2 When the water vapor permeability of the pressure-sensitive adhesive layer is within the above range, the foam sheet of the present invention is not affected by moisture and can stabilize the impact absorption properties.
[0115] The adhesive constituting the adhesive layer may contain any appropriate other component within a range that does not impair the effects of the present invention.
[0116] Examples of the other components include other polymer components, softeners, antiaging agents, curing agents, plasticizers, fillers, antioxidants, thermal polymerization initiators, photopolymerization initiators, ultraviolet absorbers, light stabilizers, colorants (pigments, dyes, etc.), solvents (organic solvents), surfactants (e.g., ionic surfactants, silicone-based surfactants, fluorine-based surfactants, etc.), crosslinking agents (e.g., polyisocyanate-based crosslinking agents, silicone-based crosslinking agents, epoxy-based crosslinking agents, alkyl etherified melamine-based crosslinking agents, etc.), etc. The thermal polymerization initiator and the photopolymerization initiator can be included in the material for forming the polymer component.
[0117] The foamed material of the present invention can be produced by any appropriate method, such as a method of producing the foamed material of the present invention by laminating a resin foam layer and a pressure-sensitive adhesive layer, or a method of producing the foamed material of the present invention by laminating a material for forming a pressure-sensitive adhesive layer and a resin foam layer, and then forming a pressure-sensitive adhesive layer by a curing reaction or the like. EXAMPLES
[0118] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The test and evaluation methods in the examples are as follows. The term "parts" means "parts by weight" unless otherwise specified, and the term "%" means "% by weight" unless otherwise specified.
[0119] <Evaluation method> (1) Apparent density The density (apparent density) of the resin foam was calculated as follows. The resin foam obtained in the examples and comparative examples was punched out to a size of 20 mm x 20 mm to prepare a test piece, and the dimensions of the test piece were measured with a vernier caliper. Next, the weight of the test piece was measured with an electronic balance. Then, the density was calculated according to the following formula. Apparent density (g / cm 3 ) = weight of test piece / volume of test piece (2) 25% compression load Measured according to the compression hardness measurement method for resin foams described in JIS K 6767. Specifically, the resin foams obtained in the examples and comparative examples were cut into test pieces of 30 mm × 30 mm size, and the stress (N) when compressed to a compression rate of 25% at a compression speed of 10 mm / min was measured per unit area (1 cm 2 ) per 25% compression load (N / cm 2 ) was decided. (3) 50% compression load Measured according to the compression hardness measurement method for resin foams described in JIS K 6767. Specifically, the resin foams obtained in the examples and comparative examples were cut into test pieces of 30 mm × 30 mm size, and the stress (N) when compressed to a compression rate of 50% at a compression speed of 10 mm / min was measured per unit area (1 cm 2 ) per 50% compression load (N / cm 2 ) was decided. (4) Average bubble diameter (average cell diameter), maximum bubble diameter (maximum cell diameter), and coefficient of variation of bubble diameter (cell diameter) The resin foam was cut with a razor blade in the direction perpendicular to the main surface of the resin foam (thickness direction), and a digital microscope (product name "VHX-500", manufactured by Keyence Corporation) was used as a measuring instrument to capture an image of the cut surface of the resin foam. The image was analyzed using the instrument's analysis software to determine the number-average bubble diameter (average cell diameter) and maximum bubble diameter (maximum cell diameter). The number of bubbles in the captured enlarged image was about 400. The standard deviation was calculated from all the cell diameter data, and the coefficient of variation was calculated using the following formula. Coefficient of variation = standard deviation / average bubble size (average cell size) (5) Bubble diameter aspect ratio A digital microscope (product name "VHX-2000, manufactured by Keyence Corporation) was used as a measuring instrument to measure the aspect ratio of the cells in the resin foams obtained in the examples and comparative examples by the following method. The resin foam is cut with a razor blade in the direction perpendicular to the main surface of the resin foam (thickness direction), and the cut surface is measured with a microscope (for example, Keyence's "VHX-2000") to obtain a predetermined area (3 mm2 The area was observed at a magnification of 100x, and the length of each bubble in the thickness direction and the length perpendicular to the thickness direction were measured. Similar measurements were made for all bubbles present within a given area. The aspect ratio of the bubbles was calculated by dividing the length perpendicular to the thickness direction by the length in the thickness direction. The same calculation was performed for all bubbles, and the average value was taken as the "aspect ratio of the bubbles in the resin foam." (6) Melt tension The resin (plant-derived polypropylene polymer) contained in the resin foam was extruded into a molten strand shape at an extrusion speed of 8.8 mm / min using a twin capillary rheometer "RH7-2" (manufactured by Rosand Precision) at a temperature 20°C higher than the melting point of the plant-derived polypropylene polymer and an orifice diameter of 1 mmφ, and the strand was taken up at a take-up speed of 0.5 m / min. The take-up speed was increased by 0.1 m / min, and the melt tension at which the strand-shaped resin broke was recorded as the "melt tension." (7) Die swell ratio Using an extensional viscometer (product name "RH-7", Malvern Instruments) as a measuring instrument, a sample (size: 5 mm square) was placed in a cylinder at a temperature 20°C higher than the melting point of the resin constituting the resin foam, and allowed to melt for 7 minutes. The molten material was then extruded at a shear rate of 20 mm / s into a die with a length of 10 mm and an aperture of 1 mmφ, and the diameter of the resulting string-like molded product was measured using a digital caliper (product name "CD67-s PM", Mitutoyo Corporation), and the die swell ratio was calculated from the following formula. Die swell ratio = diameter of molded product (mm) / die aperture (mm) As the above samples, the plant-derived polypropylene-based polymer contained in the resin foam and the resin composition forming the resin foam were used, and the die swell ratios of these samples were measured. (8) Shock absorption A test specimen was formed by placing a resin foam, double-sided tape (product number: No. 5603W, manufactured by Nitto Denko), and a PET film (product number: Diafoil MRF75, manufactured by Mitsubishi Plastics) in that order on the impact force sensor. A 66g iron ball was dropped onto the test specimen from a height of 50cm above the PET film to measure the impact force F1. In addition, an iron ball was dropped directly onto the impact force sensor as described above to measure the impact force F0 of the blank. The impact absorption (%) was calculated from F1 and F0 using the formula (F0-F1) / F0×100. (9) CO2 emissions from raw materials [kg / m 2 ] When the amount of CO2 generated when producing petroleum-derived resin is 1.8 kg / kg-resin and the amount of CO2 generated when producing plant-derived resin is 1.0 kg / kg-resin, and the weight of petroleum-derived resin contained in 1 m2 of foam is wp and the weight of plant-derived resin is wb, the amount of CO2 generated from the raw materials for the foam can be calculated as 1.8 x wp + 1.0 x wb.
[0120] Example 1 56 parts by weight of a plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF", MFR: 0.85g / 10min), 49 parts by weight of a polyolefin elastomer A (melt flow rate (MFR): 15g / 10min), 10 parts by weight of magnesium hydroxide, 1 part by weight of stearic acid monoglyceride, and 10 parts by weight of carbon black were kneaded at a temperature of 200°C using a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were placed in a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 MPa (12 MPa after injection) in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 5.2 parts by weight per 100 parts by weight of resin. After being fully saturated with carbon dioxide gas, the mixture was cooled to a temperature suitable for foaming, extruded from a die, and sliced to a thickness of 1.0 mm to obtain a sheet-shaped resin foam. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0121] Example 2 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 65 parts by weight, the amount of polyolefin elastomer A was 35 parts by weight, and the amount of carbon dioxide gas injected was 5.5 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0122] Example 3 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 65 parts by weight, and the amount of polyolefin elastomer A was 35 parts by weight. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0123] Example 4 A resin foam was obtained in the same manner as in Example 2, except that the amount of carbon dioxide gas injected was 5.8 parts by weight per 100 parts by weight of the resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0124] Example 5 65 parts by weight of a plant-derived polypropylene polymer (manufactured by Borealis, trade name "BA110CF", MFR: 0.85g / 10min), 35 parts by weight of a polyolefin elastomer A (melt flow rate (MFR): 15g / 10min), 10 parts by weight of magnesium hydroxide, 1 part by weight of stearic acid monoglyceride, and 10 parts by weight of carbon black were kneaded at a temperature of 200°C using a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were placed in a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 MPa (12 MPa after injection) in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 5.8 parts by weight per 100 parts by weight of resin. After being fully saturated with carbon dioxide gas, the mixture was cooled to a temperature suitable for foaming, extruded from a die, and sliced to a thickness of 2.0 mm to obtain a sheet-shaped resin foam. Furthermore, the foamed structure was passed between the rolls (the gap between the rolls) of a pair of rolls, one of which was heated to 200° C., to obtain a 1.0 mm thick resin foam B. The gap between the rolls was set so that a 1.0 mm thick resin foam B was obtained.
[0125] Example 6 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of a plant-derived polypropylene polymer (manufactured by SABIC, product name "Rely 61EK61PS", MFR: 0.3 g / 10 min) was used, and the amount of carbon dioxide gas injected was 5.5 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0126] Example 7 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of a plant-derived polypropylene polymer (manufactured by SABIC, product name "Rely 71EK71PS", MFR: 0.3 g / 10 min) was used, and the amount of carbon dioxide gas injected was 5.5 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0127] Example 8 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 75 parts by weight, the amount of polyolefin elastomer A was 25 parts by weight, and the amount of carbon dioxide gas injected was 5.2 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0128] Example 9 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 75 parts by weight, the amount of polyolefin elastomer A was 25 parts by weight, and the amount of carbon dioxide gas injected was 5.4 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0129] Example 10 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 65 parts by weight, the amount of polyolefin elastomer A was 35 parts by weight, and the amount of carbon dioxide gas injected was 6.2 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0130] Example 11 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was 65 parts by weight, the amount of polyolefin elastomer A was 35 parts by weight, and the amount of carbon dioxide gas injected was 6.4 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0131] Comparative Example 1 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of a plant-derived polypropylene polymer (manufactured by Borealis, product name "BC250MO", MFR: 4g / 10 min) was used, and the amount of carbon dioxide gas injected was 5.5 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0132] Comparative Example 2 A resin foam was obtained in the same manner as in Example 1, except that the amount of plant-derived polypropylene polymer (manufactured by Borealis, product name "BA110CF") was changed to 65 parts by weight, and 65 parts by weight of a plant-derived polypropylene polymer (manufactured by Borealis, product name "BB125MO", MFR: 1.3 g / 10 min) was used, and the amount of carbon dioxide gas injected was 5.5 parts by weight per 100 parts by weight of resin. The obtained resin foam was subjected to the above-mentioned evaluations, and the results are shown in Table 1.
[0133] [Table 1] [Industrial Applicability]
[0134] The resin foam of the present invention can be suitably used, for example, as a cushioning material for electronic devices. [Explanation of symbols]
[0135] 100 Foam material 10 Resin foam layer (resin foam) 20 Adhesive layer
Claims
1. A resin foam having a cell structure, A resin foam having a petroleum-derived resin content a of 50% by weight or less and satisfying the following formula (1): [Apparent density (g / cm 3 ) ]<−0.0025×[content a (%) of petroleum-derived resin] + 0.48 ... (1)
2. The resin foam according to claim 1 , wherein the resin foam has an aspect ratio of cells of 4 or less.
3. The 50% compression load of the resin foam is 40 N / cm 2 The resin foam according to claim 1 , wherein:
4. The 25% compression load of the resin foam is 25 N / cm 2 The resin foam according to claim 1 , wherein:
5. The resin foam according to claim 1 , wherein the resin foam has an average cell diameter of 200 μm or less.
6. The apparent density of the resin foam is 0.4 g / cm 3 The resin foam according to claim 1 , wherein:
7. The resin foam according to claim 1 , wherein the resin foam has a coefficient of variation of cell diameter of 0.6 or less.
8. The resin foam according to claim 1 , comprising a plant-derived polyolefin resin.
9. The plant-derived polyolefin-based resin includes a plant-derived polyolefin, The resin foam according to claim 8 , wherein the plant-derived polyolefin has a melt flow rate at 230° C. of less than 20 g / 10 min.
10. The resin foam according to claim 1 , wherein the plant-derived polyolefin has a melt tension of 10 cN or more.
11. The resin foam according to claim 8 , wherein the plant-derived polyolefin has a die swell ratio of 1.5 or less at a melting point +20° C. of the plant-derived polyolefin.
12. The resin foam according to claim 1 , wherein the resin composition forming the resin foam has a die swelling ratio of 1.5 or less at a melting point +20° C. of the resin composition.
13. The resin foam according to claim 8 , wherein the plant-derived polyolefin-based resin comprises a plant-derived polypropylene-based polymer.
14. the plant-derived polyolefin-based resin is a mixture of a polyolefin other than a polyolefin-based elastomer and a polyolefin-based elastomer, As the polyolefin, a plant-derived polyolefin is used, As the polyolefin-based elastomer, a plant-derived polyolefin-based elastomer or a petroleum-derived polyolefin-based elastomer is used. The resin foam according to claim 8.
15. The resin foam according to claim 1 , having a heat-fusible layer on one or both sides.
16. A foam member comprising: a resin foam layer formed from the resin foam according to claim 1; and a pressure-sensitive adhesive layer disposed on at least one side of the resin foam layer.
Citation Information
Patent Citations
Impact absorption material
JP2015034299A
Foam for buffer material and buffer material
JP2017186504A
Cited By
Resin foam and foam member
WO2026126973A1
Resin foam and foam member
WO2026127016A1