Soft magnetic alloy particles and inductor using the same

Soft magnetic alloy particles with controlled Ge distribution in amorphous and nanocrystalline phases address the challenge of maintaining high saturation magnetization and improving electromagnetic properties in Fe-based materials, enhancing performance in inductors.

JP2024152624APending Publication Date: 2024-10-25SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024034363
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-03-06
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing Fe-based soft magnetic materials face challenges in maintaining high saturation magnetization characteristics while improving electromagnetic properties due to issues such as non-uniform crystal growth and decreased Fe content when adjusting Si content, which affects magnetization values.

Method used

The development of soft magnetic alloy particles composed of nanocrystals and amorphous Fe and Ge, with specific atomic percentage ranges, where Ge is predominantly present in the amorphous phase, ensuring Ge(a)-Ge(c)>0, and excluding Si, to control nanocrystal size and enhance electromagnetic properties.

Benefits of technology

The solution maintains high saturation magnetization characteristics and improves electromagnetic properties by controlling nanocrystal size and crystallinity, achieving magnetic permeability and core loss within optimal ranges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152624000001_ABST
    Figure 2024152624000001_ABST
Patent Text Reader

Abstract

To provide a printed circuit board having improved connectivity with mounted components and a method for manufacturing the same.SOLUTION: Soft magnetic alloy particles according to the present invention include nanocrystals and amorphous materials, and contain Fe (iron) and Ge (germanium), in which when the average Ge content in the amorphous materials is Ge(a) (at%) and the average Ge content in the nanocrystals is Ge(c) (at%), the relationship Ge(a)-Ge(c)>0 holds.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to soft magnetic alloy particles and inductors using the same. [Background technology]

[0002] Recently, with the miniaturization and high integration of electronic elements, power supply voltages have been decreasing, and as a result, the current value has been increasing to transmit the same amount of power. Therefore, metal inductors that maintain their inductor performance even at high currents have been used, and recently, materials that have high current characteristics among metals, in other words, materials with high saturation magnetization (Ms) values, are being used in order to use higher currents.

[0003] In existing Fe-based soft magnetic materials, the electromagnetic properties have been improved by adjusting the content of elements such as Si to bring magnetostriction close to 0. However, when the Si content is increased, the content of metals such as Fe is reduced, making it difficult to improve the Ms value, which is an issue.

[0004] Also, if the content of metals such as Fe is too high, the Ms value can be increased, but there is a problem that nanocrystals grow locally during heat treatment, which causes uneven crystal growth and impairs the electromagnetic properties of the soft magnetic material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-206836 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the problems of the above-described prior art, and an object of the present invention is to provide soft magnetic alloy particles that can maintain high saturation magnetization characteristics while improving electromagnetic characteristics. Another object of the present invention is to provide an inductor using the above soft magnetic alloy particles.

[0007] However, the problems to be solved by the present invention are not limited to the above-described problems, and can be variously extended within the scope of the technical idea included in the present invention.

Means for Solving the Problems

[0008] The soft magnetic alloy particles according to one aspect of the present invention made to achieve the above object include nanocrystals and amorphous, include Fe (iron) and Ge (germanium), and when the average Ge content in the amorphous is Ge(a) (at%) and the average Ge content in the nanocrystals is Ge(c) (at%), Ge(a) - Ge(c)>0. The soft magnetic alloy particles are represented by the following Composition Formula 1. Composition Formula 1 Fe a Co b Ge c M d In the Composition Formula 1, a, b, c, and d respectively represent the atomic percentage contents (at%) of the corresponding elements, 0 < a ≦ 90, 0 ≦ b ≦ 10, 0 < c ≦ 5, 0 < d ≦ 20, a + b + c + d = 100, and M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

[0009] The M does not include Si. In the above, 0.5 ≦ c ≦ 4 may be satisfied. In the above, 70 ≦ a ≦ 80 may be satisfied. In the above, 2 ≦ b ≦ 6 may be satisfied. In the above, 75 ≦ a + b ≦ 90 may be satisfied. In the above, 10 ≦ d ≦ 20 may be satisfied. In the above, 0.1 ≦ Ge(a) - Ge(c) ≦ 0.7 may be satisfied. M may include B, P, Cu, or a combination thereof. The crystallinity of the soft magnetic alloy particles may be 59% or more and 70% or less. The average crystal size of the nanocrystals may be 20 nm or less.

[0010] An inductor according to one aspect of the present invention made to achieve the above object includes a body containing a magnetic material containing soft magnetic alloy particles, a coil disposed in the body, and an external electrode disposed on an outer surface of the body. The soft magnetic alloy particles include nanocrystals and an amorphous phase, contain Fe (iron) and Ge (germanium), and when the average atomic content of Ge in the amorphous phase is Ge(a) (at%) and the average atomic content of Ge in the nanocrystals is Ge(c) (at%), Ge(a) - Ge(c) > 0. The soft magnetic alloy particles are represented by the following Composition Formula 1. Composition Formula 1 Fe a Co b Ge c M d In Composition Formula 1, a, b, c, and d represent the atomic percentage contents (at%) of the corresponding elements, respectively, where 0 < a ≦ 90, 0 ≦ b ≦ 10, 0 < c ≦ 5, 0 < d ≦ 20, and a + b + c + d = 100, and M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

[0011] M does not include Si. In the above, 0.5 ≦ c ≦ 4 may be satisfied. The crystallinity of the soft magnetic alloy particles may be 59% or more and 70% or less. The average crystal size of the nanocrystals may be 20 nm or less.

[0012] In the inductor, the coil includes a support member and an upper coil and a lower coil disposed on the upper and lower surfaces of the support member, respectively, and the upper coil and the lower coil can be electrically connected through a via that penetrates the support member. In the inductor, the body includes a molded portion, a cover portion arranged on one side of the molded portion, and a core protruding from one side of the molded portion, the coil is arranged between the one side of the molded portion and the cover portion, and the core passes through the coil. In the inductor, the body may include a plurality of magnetic sheets including the magnetic material. Effect of the Invention

[0013] The soft magnetic alloy particles according to the present invention have the effect of improving the electromagnetic properties while maintaining high saturation magnetization properties.

[0014] However, the various and beneficial advantages and effects of the present invention are not limited to the above, and will be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0015] [Figure 1] 1 is a photograph of soft magnetic alloy particles according to an embodiment observed with a transmission electron microscope (TEM). [Diagram 2] 1 is a photograph of conventional soft magnetic alloy particles observed with a transmission electron microscope (TEM). [Diagram 3] FIG. 2 is a diagram showing a line profile (lower part) of quantitative spot analysis by TEM analysis (upper part) of a soft magnetic alloy particle according to an embodiment of the present invention. [Figure 4] FIG. 2 is a diagram showing a line profile (lower part) of quantitative spot analysis by TEM analysis (upper part) of a soft magnetic alloy particle according to an embodiment of the present invention. [Diagram 5]FIG. 2 is a transparent perspective view of an inductor according to an embodiment. [Figure 6] 6 is a cross-sectional view showing a schematic cross section taken along the line II' of FIG. 5. FIG. [Figure 7] FIG. 7 is an enlarged view of region A in FIG. 6. [Figure 8] FIG. 13 is a transparent perspective view of an inductor according to another embodiment. [Figure 9] 9 is a cross-sectional view showing a schematic cross section taken along the line II-II' of FIG. 8. [Figure 10] FIG. 13 is a transparent perspective view of an inductor according to another embodiment. [Figure 11] 11 is a cross-sectional view showing a schematic cross section taken along the line III-III' of FIG. 10. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the present invention will be described in detail with reference to the drawings so that a person having ordinary skill in the art to which the present invention pertains can easily carry out the present invention. In the drawings, parts unnecessary for the explanation are omitted in order to clearly explain the present invention, and the same or similar components are given the same reference numerals throughout the specification. In addition, the drawings are merely for the purpose of making it easy to understand the embodiments disclosed in the present specification, and the technical ideas disclosed in the specification are not limited by the drawings, and all modifications, equivalents, or alternatives included within the ideas and technical scope of the present invention are included. In addition, some components are exaggerated, omitted, or shown roughly in the drawings, and the size of each component does not completely reflect the actual size.

[0017] Throughout the specification, when a part "comprises" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.

[0018] Throughout the specification, the term "stacking direction" refers to the direction in which components are stacked one on top of the other, which is the "thickness direction" perpendicular to the broad surface (principal surface) of a sheet-like component, and corresponds to the T-axis direction in the drawings.

[0019] And, the term "lateral" refers to the direction extending parallel to the broad surface (principal surface) from the periphery of the sheet-like component, which is the "planar direction" and corresponds to the L-axis direction in the drawings.

[0020] The W-axis direction in the drawing is the "width direction."

[0021] Hereinafter, various embodiments and modifications will be described in detail with reference to the drawings.

[0022] [Soft magnetic alloy particles] 1 is a transmission electron microscope (TEM) photograph of a soft magnetic alloy particle according to an embodiment. For reference, the TEM image can be binarized or otherwise used to separate light and dark areas to define the boundary between the amorphous portion and the nanocrystalline portion.

[0023] Referring to FIG. 1, the soft magnetic alloy particles according to one embodiment include nanocrystals and amorphous phases, and contain Fe (iron) and Ge (germanium).

[0024] The soft magnetic alloy particles according to one embodiment are represented by the following composition formula 1.

[0025] [Composition formula 1] Fe a Co b Ge c M d In the above composition formula, a, b, c, and d each represent the atomic percentage content (at%) of the corresponding element, and <a≦90、0≦b≦10、0<c≦5、0<d≦20、a+b+c+d=100である。 M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or combinations thereof.

[0026] In one embodiment, M includes B, P, Cu, or a combination thereof.

[0027] In one embodiment, M does not include Si.

[0028] In composition formula 1, a represents the atomic percentage content of Fe (iron) metal, and it is preferable that 70≦a≦80.

[0029] In the composition formula 1, b represents the atomic percentage content of Co (cobalt) metal, and it is preferable that 2≦b≦6.

[0030] In the composition formula 1, it is preferable that 75≦a+b≦90. If a+b is less than 75, the saturation magnetization value is low and the high current characteristics may be poor, and if a+b is more than 90, it is difficult to control the size of the nanocrystals and the electromagnetic characteristics may be poor.

[0031] In the composition formula 1, it is preferable that 10≦d≦20.

[0032] c indicates the atomic percentage content of Ge (germanium) element, and is preferably 0.5≦c≦4. If c is less than 0.5, it may be difficult to control the size of the nanocrystals, resulting in poor electromagnetic properties, and if c exceeds 4, the content of the metals Fe and Co is relatively low, resulting in a problem that high current properties cannot be ensured.

[0033] As a specific example, the composition formula 1 is Fe 79.4 Co4Ge 0.5 B 10 P 5.5 Cu 0.6 , Fe 79.4 Co4Ge1B 10 P5Cu 0.6 , Fe 79.4 Co4Ge2B 10 P4Cu 0.6 , Fe7 8.4 Co4Ge3B 10 P4Cu 0.6 , or Fe 77.4 Co4Ge4B 10 P4Cu 0.6 may be also possible.

[0034] In one embodiment of the soft magnetic alloy particle, when the average Ge content in the amorphous portion is Ge(a) (at%) and the average Ge content in the nanocrystals is Ge(c) (at%), Ge(a)-Ge(c)>0.

[0035] Ge(a) means the average content (at%) of Ge element relative to all atoms constituting the amorphous part of the soft magnetic alloy grain, and Ge(c) means the average content (at%) of Ge element relative to all atoms constituting the nanocrystalline part of the soft magnetic alloy grain.

[0036] 3 and 4 are diagrams showing a line profile (bottom) of a spot quantitative analysis by TEM analysis (top) of a soft magnetic alloy particle according to an embodiment. For reference, the boundary between the amorphous part and the nanocrystalline part is defined by dividing the light and dark parts by a method such as binarizing the transmission electron microscope (TEM) image. In FIG. 3 and FIG. 4, the relatively bright parts correspond to the nanocrystalline phase, and the relatively dark parts correspond to the amorphous phase.

[0037] Referring to FIGS. 3 and 4, Ge(a) and Ge(c) are measured by line analysis using an Energy Disperse X-Ray Spectrometer (EDS) installed in a Transmission Electron Microscope (TEM).

[0038] Specifically, using the surface of any one nanocrystalline particle as a reference, a line profile was quantitatively analyzed over a 20 nm area inside the nanocrystalline particle and a 200 nm area outside the particle, and the maximum value inside the nanocrystalline particle was compared with the maximum value in the amorphous portion.

[0039] In order to measure the average, the above-described analysis is repeated for 5 or more points, and the average value is calculated.

[0040] 3 and 4, according to an embodiment, in the case of soft magnetic alloy particles that do not contain Si but contain Ge, which has a relatively larger atomic weight than Si, it can be seen that the Ge element is more present in the amorphous state than in the nanocrystals.

[0041] In one embodiment, 0.1 (at%)≦Ge(a)-Ge(c)≦0.7 (at%). If the Ge(a)-Ge(c) value is less than 0.1 (at%), it is difficult to control the size of Ge nanocrystals, resulting in poor electromagnetic properties, whereas if the Ge(a)-Ge(c) value exceeds 0.7 (at%), it is poor in high current properties.

[0042] In one embodiment, the first crystallization temperature (T x1 ) and the second crystallization temperature (T x2 ) may exceed 100°C. x1 ) and the second crystallization temperature (T x2 ) is less than 100°C, T x1 and T x2 As a result, it becomes difficult to obtain a uniform nanocrystalline structure, and the soft magnetic properties deteriorate.

[0043] The amorphous material constituting the soft magnetic alloy particles has at least two exothermic peaks indicating crystallization during the heating process of a DSC curve obtained by differential scanning calorimetry (DSC).

[0044] Among the exothermic peaks, the lowest temperature exothermic peak indicates the first crystallization in which the a-Fe primary phase crystallizes, and the subsequent exothermic peak indicates the second crystallization in which the secondary phase of the Fe-B compound crystallizes.

[0045] Here, the first crystallization onset temperature T x1 is defined as the temperature at the intersection of the first ascending tangent, which is a tangent passing through the point with the steepest positive slope in the first ascending portion from the baseline to the first peak, which is the exothermic peak on the lowest side of the DSC curve, and the baseline.

[0046] In addition, the second crystallization starting temperature Tx2 is defined as the temperature at the intersection of the second ascending tangent, which is a tangent passing through the point with the steepest positive slope in the second ascending portion from the baseline to the second peak, which is the next exothermic peak after the first peak, and the baseline.

[0047] In one embodiment, the soft magnetic alloy grains may have a crystallinity of 40% or more, or 59% or more, or 75% or less, or 70% or less, calculated by the following Equation 1. The soft magnetic alloy grains have a crystallinity of 60%, which improves the crystallinity to a level of 60%, and therefore can achieve advantageous results in terms of high Ms.

[0048] [Formula 1] Crystallinity (%)=[Ic / (Ic+Ia)]×100

[0049] In the above formula 1, Ic is the sum of the integral values ​​of the scattering intensity of the crystalline peaks in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles, and Ia is the sum of the integral values ​​of the scattering intensity of the amorphous halo in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles.

[0050] The degree of crystallinity of soft magnetic alloy particles can be calculated based on a graph obtained by X-ray diffraction spectroscopy. From the X-ray diffraction analysis spectrum, the relationship 2d·sinθ=nλ holds between the wavelength λ and incident angle θ of the incident X-rays and the spacing d of the lattice planes, and this relationship is called the Bragg equation. With this, the lattice spacing d can be calculated when the incident angle is determined.

[0051] However, in amorphous materials, random arrangements rather than regular atomic arrangements appear, so multiple X-ray diffraction patterns do not appear at specific wavelengths, and a wide halo pattern appears in the diffraction angle range of 15° to 35°. If there are no peaks at specific angles in the diffraction angle range of 10° to 60° and a diffuse halo pattern appears, the material can be determined to be amorphous with a crystallinity of 0%. However, the surface of the soft magnetic alloy particles exposed to the X-rays must not contain any contaminants other than organic matter. Only results measured under conditions without factors that affect the diffraction pattern are highly reliable.

[0052] If crystals are present in the soft magnetic alloy particles, one or more crystalline peaks will be present in the range of the measured diffraction angle. The presence of a peak means that, on an X-ray diffraction diagram in which the maximum intensity in the range of diffraction angles 2θ=5° to 50° in an XRD pattern graph is taken as the total area on the vertical axis, the peak can be recognized at least with the naked eye, or the waveform processor can recognize the peak as clearly distinguished from background noise.

[0053] At this time, if the degree of crystallinity is high, the halo region will be reduced, and there will be no halo region in a material with 100% crystallinity. When crystalline and amorphous materials are mixed, the degree of crystallinity can be calculated by calculating the relative ratio of the area of ​​the crystalline peak and the area of ​​the halo region in a graph consisting of the intensity and diffraction angle range.

[0054] The nanocrystals of the soft magnetic alloy particles may be amorphous grains.

[0055] In one embodiment, the nanocrystals of the magnetically soft alloy grains may have an average crystal size of 20 nm or less, for example, 18 nm or less.

[0056] As an example, the average crystal size of nanocrystals can be calculated using the Scherrer equation using the full width at half maximum (FWHM) of the main peak in the XRD graph.

[0057] Alternatively, the average size of the nanocrystals may be determined by measuring the maximum long axis of at least 100 nanocrystals in a scanning electron microscope (SEM) image of a cross section of a soft magnetic alloy particle, creating a size distribution curve, and calculating D50 to determine the average size.

[0058] The soft magnetic alloy particles described above do not contain Si elements, but contain Ge elements having a relatively larger atomic weight than Si elements, and the Ge elements are present in greater amounts in the amorphous state than in the nanocrystals during heat treatment. As a result, the Ge elements act as an inhibitor that prevents the growth of nanocrystals, thereby adjusting the size of the nanocrystals to a certain size or less, thereby improving electromagnetic properties such as magnetic permeability and core loss.

[0059] In addition, by increasing the second crystallization temperature, the heat treatment process window for nanocrystal formation is improved, resulting in uniform nanocrystals and a high crystal fraction, which has the advantage of maintaining high saturation magnetization (Ms) characteristics.

[0060] [Inductor] An example of an inductor 100 including a magnetic material containing the above-mentioned soft magnetic alloy particles will be described below. Types of inductors include thin film inductors, laminated inductors, wire-wound inductors, and wound inductors, and in the following, thin film inductors will be described first.

[0061] Fig. 5 is a schematic perspective view of a thin film inductor according to an embodiment, and Fig. 6 is a schematic cross-sectional view of the inductor shown in Fig. 5 taken along the line I-I' in Fig. 5. A thin film inductor 100 according to an embodiment includes a body 110 including a magnetic material containing soft magnetic alloy particles, a coil 130 disposed within the body, and external electrodes 161, 162 disposed on an outer surface of the body 110.

[0062] The body 110 provides the exterior appearance of the thin film inductor 100 .

[0063] The body 110 has a hexahedral shape including an upper surface and a lower surface facing in the stacking direction of the coils, a side surface facing laterally, and a front surface facing in the width direction, and when mounted on a printed circuit board, the lower surface (the other surface) of the body is the mounting surface. The corners where the surfaces meet may be rounded by grinding or the like.

[0064] The body 110 is formed by forming the coil 130, laminating sheets containing a magnetic material on the upper and lower parts of the coil 130, and then compressing and curing the laminate.

[0065] The body 110 includes a magnetic material, which includes soft magnetic alloy particles according to one embodiment.

[0066] FIG. 7 is an enlarged view of region A in FIG.

[0067] 6 and 7, the magnetic material includes magnetic particles including a resin 20 and coarse magnetic particles 11 or fine magnetic particles 12 dispersed in the resin. As an example, the coarse magnetic particles 11 and the fine magnetic particles 12 are mixed and dispersed at a certain ratio in the resin 20 as a matrix.

[0068] The coarse magnetic particles 11 have an average particle size of 10 μm to 30 μm, and the fine magnetic particles 12 have an average particle size of 1 μm to 10 μm.

[0069] The diameter of the magnetic particles present in the body 110 is measured on a cross section of the body 110. Specifically, a plurality of equally spaced regions (e.g., 10 regions) in the T-axis direction on a LT-direction cross section passing through the center of the body 110 are photographed with a scanning electron microscope, and the diameter of the magnetic particles can be obtained using an image analysis program. In this case, the diameter of the magnetic particles is measured excluding the outer periphery of the body 110, since the magnetic particles may be deformed or destroyed in the compression process or the like. For example, a region corresponding to a length within 5% or 10% of the surface of the body 110 can be excluded.

[0070] The magnetic particles can be any type used in the industry without any restrictions. As an example, the magnetic particles can be made of ferrite or metal-based soft magnetic material.

[0071] The ferrite may include known ferrites such as Mn-Zn ferrite, Ni-Zn ferrite, Ni-Zn-Cu ferrite, Mn-Mg ferrite, Ba ferrite, or Li ferrite.

[0072] The metallic soft magnetic material may be an alloy containing one or more selected from the group consisting of Fe, Si, Cr, Al, and Ni, and may include, for example, Fe-Si-B-Cr amorphous metal particles, but is not limited thereto.

[0073] In one embodiment, the magnetic particles include soft magnetic alloy particles, and in one example, the coarse magnetic particles are soft magnetic alloy particles.

[0074] The resin is an insulating resin, and may include, but is not limited to, an epoxy resin, a polyimide resin, a liquid crystal polymer, or a combination thereof.

[0075] The soft magnetic alloy particles include nanocrystalline and amorphous, and contain Fe (iron) and Ge (germanium).

[0076] The soft magnetic alloy particles are represented by the following composition formula 1. [Composition formula 1] Fe a Co b Ge c M d

[0077] In the above composition formula, a, b, c, and d each represent the atomic percentage content (at%) of the corresponding element, and <a≦90、0≦b≦10、0<c≦5、0<d≦20、a+b+c+d=100であり、 M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or combinations thereof.

[0078] M includes B, P, Cu, or a combination thereof, and does not include Si.

[0079] c indicates the atomic percentage content of Ge (germanium) element, and is preferably 0.5≦c≦4. If c is less than 0.5, it may be difficult to control the size of the nanocrystals, resulting in poor electromagnetic properties, and if c exceeds 4, the content of the metals Fe and Co is relatively low, resulting in a problem that high current properties cannot be ensured.

[0080] In soft magnetic alloy particles, when the average Ge content in the amorphous phase is Ge(a) (at%) and the average Ge content in the nanocrystals is Ge(c) (at%), Ge(a)-Ge(c)>0.

[0081] Ge(a) means the average content (at%) of Ge element relative to all atoms constituting the amorphous part of the soft magnetic alloy grain, and Ge(c) means the average content (at%) of Ge element relative to all atoms constituting the nanocrystalline part of the soft magnetic alloy grain.

[0082] In the inductor 100, the method for measuring Ge(a) and Ge(c) is as follows.

[0083] In a cross-sectional sample (hereinafter referred to as the "cross-sectional sample") cut from the center of the W-axis direction of the inductor body 110 in the L-axis direction and T-axis direction, the soft magnetic alloy particles dispersed in the resin are subjected to line analysis using an EDS (Energy Disperse X-Ray Spectrometer) installed in a transmission electron microscope (TEM).

[0084] A cross-sectional sample of the inductor body 110 is prepared, for example, by immersing the inductor 100 in an epoxy mixture and hardening it, then polishing the sides of the inductor body 110 in the L-axis and T-axis directions to the 1 / 2 point in the W-axis direction, fixing it, and maintaining it in a chamber with a vacuum atmosphere.

[0085] Specifically, the surface of any one nanocrystalline particle contained in the soft magnetic alloy particle is used as a reference, and a line profile is obtained by quantitatively analyzing 20 nm inside the nanocrystalline particle and 200 nm outside the nanocrystalline particle, and the maximum value inside the nanocrystalline particle is compared with the maximum value in the amorphous part. In order to measure the average, the above-described analysis is repeated for 5 points or more, and the average value is calculated.

[0086] The soft magnetic alloy particles preferably have a crystallinity, calculated by the following formula 1, of 40% or more or 59% or more, and 75% or less or 70% or less.

[0087] [Formula 1] Crystallinity (%)=[Ic / (Ic+Ia)]×100

[0088] In the above formula 1, Ic is the sum of the integral values ​​of the scattering intensity of the crystalline peaks in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles, and Ia is the sum of the integral values ​​of the scattering intensity of the amorphous halo in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles.

[0089] Specifically, the crystallinity of the soft magnetic alloy particles can be calculated by Equation 1 after obtaining an XRD graph of the soft magnetic alloy particles from a cross-sectional sample of the inductor body 110. The XRD graph of the soft magnetic alloy particles can be obtained from a sample obtained by crushing and classifying the cross-sectional sample of the body to about 20 μm or more.

[0090] The average crystal size of the nanocrystals contained in the soft magnetic alloy grains may be 20 nm or less, for example, 18 nm or less.

[0091] As an example, the average crystal size of nanocrystals can be calculated using the Scherrer equation using the full width at half maximum (FWHM) of the main peak in the XRD graph.

[0092] Specifically, the average crystal size of the nanocrystals can be calculated using the half-width after obtaining an XRD graph of the soft magnetic alloy particles from a cross-sectional sample of the inductor body 110. The XRD graph of the soft magnetic alloy particles can be obtained through a sample obtained by crushing and classifying the cross-sectional sample of the body to about 20 μm or more.

[0093] As an example, the average crystal size of the nanocrystals can be measured in soft magnetic alloy particles corresponding to coarse magnetic particles having a particle size of 10 μm to 30 μm in a scanning electron microscope (SEM) or transmission electron microscope (TEM) image of a cross-sectional sample of the body. Specifically, in an image of a cross-sectional sample, the center point in the L-axis direction is set as a reference point, and the sizes of the nanocrystals generated inside the coarse magnetic particles observed in a plurality of regions (e.g., 10 regions) at a predetermined interval in the T-axis direction are measured, and the average value can be calculated. The intervals between the plurality of regions can be adjusted according to the scale of the scanning electron microscope (SEM) or transmission electron microscope (TEM) image, and may be equal intervals. In this case, the plurality of regions must be located within the body, and if all 10 points are not located within the body, the position of the reference point is changed or the intervals between the 10 points are adjusted.

[0094] The soft magnetic alloy particles are the same as those described above, so the remaining description will be omitted.

[0095] In one embodiment, an insulating film (not shown) is additionally disposed on the surface of the soft magnetic alloy particles to impart insulating properties and ensure inductance.

[0096] The insulating film may be arranged in one or more layers, up to three layers. As an example, the insulating film may be an organic film including epoxy resin, polyimide resin, liquid crystal polymer, or a combination thereof, or an inorganic film including silicon oxide (SiO), silica (SiO2), alumina (Al2O3), or a metal oxide film such as FeO (iron oxide) or CrO (chromium oxide). When the insulating film is a metal oxide film, the metal oxide film may include, but is not limited to, a metal element contained in the soft magnetic alloy grains.

[0097] The thickness of the insulating film is preferably 1 to 20% of the grain size of the soft magnetic alloy grains.

[0098] If the thickness of the insulating film exceeds 20% of the grain size of the soft magnetic alloy grains, the magnetic permeability and magnetic susceptibility will decrease, so it is preferable to make the thickness as thin as possible.

[0099] The coil 130 is disposed within the body 110 and serves to develop the characteristics of an inductor. For example, when the inductor 100 is used as a power inductor, the coil serves to stabilize the power supply of an electronic device by storing an electric field as a magnetic field and maintaining an output voltage. The coil may be any of a wire-wound type formed by a wire winding method, a thin-film type formed by a thin-film method, and a laminated type formed by a lamination method, but a thin-film type coil will be described below as an example.

[0100] The coil 130 includes an upper coil 131 and a lower coil 132 that are respectively disposed on the upper and lower surfaces of the support member 120. The upper coil 131 and the lower coil 132 are coil layers that are disposed facing each other with the support member 120 as the reference.

[0101] The upper coil 131 and the lower coil 132 are formed as a plated layer on the support member 120 by a plating process or a photolithography method.

[0102] The coil 130 is formed from a material having excellent electrical conductivity, for example, one metal selected from gold (Au), silver (Ag), platinum (Pt), copper (Cu), nickel (Ni), palladium (Pd), aluminum (Al), titanium (Ti), etc., or an alloy of these metals, but any ordinary conductive material can be used without restriction.

[0103] The material and type of the support member 120 are not particularly limited as long as it can support the upper coil 131 and the lower coil 132. For example, the support member 120 may be a copper clad laminate (CCL), a polypropylene glycol (PPG) substrate, a ferrite substrate, or a metal-based soft magnetic substrate. The support member 120 may also be an insulating substrate made of insulating resin. Examples of the insulating resin include thermosetting resins such as epoxy resins, thermoplastic resins such as polyimides, and resins impregnated with reinforcing materials such as glass fibers or inorganic fillers, such as prepreg, ABF (Ajinomoto Build-up Film), FR-4, BT (Bismaleimide Triazine) resin, and PID (Photo Imagable Dielectric) resin. From the viewpoint of maintaining rigidity, an insulating substrate containing glass fibers and epoxy resins may be used, but is not limited thereto.

[0104] Holes are formed through the center of the support member 120 from the top and bottom surfaces, and the holes are filled with a magnetic material to form the core portion 150. By forming the core portion filled with a magnetic material, inductance can be improved.

[0105] The upper coil 131 and the lower coil 132 stacked on both sides of the support member are electrically connected through vias 140 that penetrate the support member 120 .

[0106] The via 140 is formed by forming a through hole using a mechanical drill or a laser drill, and then filling the inside of the through hole with a conductive material by plating.

[0107] The shape and material of the via 140 are not particularly limited as long as it can electrically connect the upper coil 131 on the upper side and the lower coil 132 on the lower side, which are respectively arranged on both sides of the support member 120. Here, the upper side and the lower side are determined based on the stacking direction of the coil patterns in the drawings.

[0108] The vias 140 include a conductive material such as copper (Cu), aluminum (Al), silver (Ag), tin (Sn), gold (Au), nickel (Ni), lead (Pd), or alloys thereof.

[0109] The upper and lower coils 131 , 132 are covered with an insulating layer 133 so as not to come into direct contact with the magnetic material that makes up the body 110 .

[0110] The insulating layer 133 serves to protect the upper and lower coils 131,132.

[0111] The material of the insulating layer 133 may be any material containing an insulating substance, and may include, for example, insulating substances used in ordinary insulating coatings, such as epoxy resin, polyimide resin, liquid crystal crystalline polymer resin, etc., and known photosensitive insulating (Photo Imageable Dielectric: PID) resins may also be used, but are not limited to these.

[0112] The insulating layer 133 is formed by a method such as, but not limited to, vapor phase deposition, and may be formed by laminating insulating films on both sides of the support member.

[0113] The inductor 100 according to the embodiment includes external electrodes 161 and 162 electrically connected to the upper and lower coils 131 and 132 and disposed on the outer surface of the body 110 .

[0114] The external electrodes 161 and 162 are electrically connected to the lead terminals of the upper and lower coils 131 and 132 exposed on both sides of the body 110, respectively.

[0115] When the inductor 100 is mounted in an electronic device, the external electrodes 161 and 162 serve to electrically connect the coil 130 in the inductor to the electronic device.

[0116] The external electrodes 161, 162 are formed using a conductive paste containing a conductive metal, which may be at least one of copper (Cu), nickel (Ni), tin (Sn), and silver (Ag), or an alloy thereof.

[0117] The external electrodes 161, 162 may include a plating layer formed on a paste layer.

[0118] The plating layer includes at least one selected from the group consisting of nickel (Ni), copper (Cu), and tin (Sn). For example, a nickel (Ni) layer and a tin (Sn) layer are formed in sequence.

[0119] The wire-wound inductor 200 and the multilayer inductor 300 will be described in more detail below. Only the configurations of the wire-wound inductor 200 and the multilayer inductor 300 that differ from the thin-film inductor 100 will be described below. The explanation for the thin-film inductor 100 can be applied to the remaining configurations as is.

[0120] FIG. 8 is a schematic diagram showing a see-through perspective view of a wound inductor according to another embodiment, and FIG. 9 is a schematic diagram showing a cross-section in the II-II' direction of FIG. 8, and is a schematic diagram showing a cross-sectional view of the inductor shown in FIG. 8.

[0121] The wire-wound inductor 200 according to one embodiment includes a body 210 including a magnetic material including soft magnetic alloy particles, a coil 230 disposed within the body, and external electrodes 261 , 262 disposed on an external surface of the body 310 .

[0122] In one embodiment, the body 210 includes a molded portion 211, a cover portion 212 disposed on one side of the molded portion 211, and a core 250 protruding from one side of the molded portion 211, the coil 230 being disposed between the one side of the molded portion 211 and the cover portion 212, and the core 250 passing through the coil 230.

[0123] The body 210 of the wire-wound inductor 200 includes a molded part 211, a cover part 212 disposed on one surface of the molded part 211, and further includes a core 250 disposed to protrude from one surface of the molded part 211. In this case, the coil 230 is disposed on one surface of the molded part 211, and has a shape in which the coil 230 surrounds the core 250.

[0124] The body 210 includes a magnetic material, and the magnetic material includes soft magnetic alloy particles according to an embodiment. That is, at least one of the molded part 211, the cover part 212, and the core 250 includes a magnetic material including soft magnetic alloy particles. As an example, the molded part 211 is formed by filling a mold with a magnetic material. As another example, the molded part 211 is formed by filling a mold with a composite material including a magnetic material and a resin. A process of applying high temperature and high pressure to the magnetic material or composite material in the mold is additionally performed, but is not limited thereto. The molded part 211 and the core 250 are integrally formed by the above-mentioned mold, and no boundary is formed between them. The cover part 212 is formed by placing a magnetic composite sheet in which a magnetic material is dispersed in a resin on the molded part 211 and the coil 230, and then applying heat and pressure.

[0125] In the wire-wound inductor 200 , the lead-out portion (not shown) passes through the molded portion 211 and can be connected to the external electrodes 261 , 262 .

[0126] The description of the magnetic material and soft magnetic alloy particles in the body 210 can be applied to the thin film inductor 100 according to an embodiment.

[0127] In the wire-wound inductor 200, the surface of the coil 230 is covered with an insulating layer 231, which serves to provide insulation between the magnetic material of the body 210 and the coil 230. The same description of the insulating layer 133 described above can be applied to the insulating layer 231.

[0128] The wire-wound inductor 200 differs from the thin-film inductor 100 in the configuration of the coil 230 and the presence or absence of a support member.

[0129] The coil 230 is a wound type coil and does not include a support member. The coil 230 is a wound coil formed by winding a metal wire such as a copper wire (Cu-wire) including a metal wire and an insulating layer 231 that covers the surface of the metal wire. The metal wire may be, but is not limited to, a rectangular wire.

[0130] Although coil 230 is shown in FIG. 8 with alpha (α) configuration windings, this is by way of example only and coil 230 may also be edge-wise wound.

[0131] FIG. 10 is a schematic diagram showing a see-through perspective view of a layered inductor according to another embodiment, and FIG. 11 is a schematic diagram showing a cross-section in the III-III' direction of FIG. 10, and is a schematic diagram showing a cross-sectional view of the inductor shown in FIG. 10.

[0132] A stacked inductor 300 according to one embodiment includes a body 310 including a magnetic material including soft magnetic alloy particles, a coil 330 disposed within the body, and external electrodes 361, 362 disposed on an external surface of the body 310, the body 310 including a plurality of magnetic sheets including the magnetic material.

[0133] The description of the magnetic material and soft magnetic alloy particles in the body 310 can be applied to the thin film inductor 100 according to an embodiment.

[0134] As an example, the body 310 is formed by stacking a plurality of magnetic sheets containing a magnetic material in the thickness direction and then sintering the same, and the shape, dimensions, and number of stacked magnetic sheets of the body 310 are not limited to those shown in one embodiment.

[0135] Conductive patterns for forming coils 330 are formed on one surface of the magnetic sheets, and conductive vias for electrically connecting the conductive patterns positioned above and below are formed through the magnetic sheets in the thickness direction.

[0136] Therefore, one end of the conductor pattern formed on each magnetic sheet is electrically connected to each other through the conductive via formed on the adjacent magnetic sheet to form the coil 330.

[0137] The surface of the coil 330 is covered with an insulating layer 331, and the insulating layer 331 functions to provide insulation between the magnetic material of the body 310 and the coil 330. The same description of the insulating layer 133 described above can be applied to the insulating layer 331.

[0138] Both ends of the coil 330 are led out through the body 310 and can be electrically connected to a pair of external electrodes 361 and 362 formed on the body 310 by contacting them, respectively.

[0139] In particular, both ends of the coil 330 are led out through both ends of the body 310, and a pair of external electrodes 361, 362 are formed on both ends of the body 310 through which the coil 330 is led out.

[0140] The conductor pattern can be formed by thick-film printing, coating, vapor deposition, sputtering, etc. of a conductive paste for forming a conductor pattern on a green sheet for forming a magnetic sheet, but is not limited to these methods.

[0141] The conductive vias can be formed by forming through holes in the thickness direction of each sheet and then filling the through holes with a conductive paste or the like, but are not limited to this.

[0142] In addition, the conductive metal contained in the conductive paste for forming the conductor pattern can be one of silver (Ag), palladium (Pd), platinum (Pt), nickel (Ni), and copper (Cu), or an alloy thereof, but the present invention is not limited to this.

[0143] Due to their excellent properties, soft magnetic alloy particles can be included in the body of a thin film, wound, or multilayer inductor as described above, thereby improving the electromagnetic properties while maintaining high saturation magnetization characteristics.

[0144] In addition to the inductors described above, the soft magnetic alloy particles can be used in magnetic products such as transformers, motors, or motor stators.

[0145] Specific examples of the present invention are presented below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and should not be construed as limiting the scope of the present invention.

[0146] [Example]

[0147] (Production Example 1: Production of soft magnetic alloy particles) Fe, Co, Ge, B, P and Cu raw materials are prepared and weighed to obtain the composition formula shown in Table 1 below. The weighed raw materials are mixed and a master alloy is produced using an arc melting method. The produced master alloy is melted and then rapidly cooled in rapid cooling equipment to produce a soft magnetic initial alloy.

[0148] The soft magnetic initial alloy is heat-treated up to the heat treatment temperature (° C.) in Table 1 below to produce soft magnetic alloy particles of Examples 1 to 5 and Comparative Examples 1 to 11 represented by the composition formula in Table 1 below.

[0149] [Table 1]

[0150] (Manufacturing Example 2: Manufacturing of Inductors) A body containing a magnetic material in the form of the soft magnetic alloy particles produced in Production Example 1 dispersed in a resin is produced, and an inductor is produced including the body.

[0151] [Experimental Example]

[0152] (Experimental Example 1: Analysis of the difference in Ge content between the amorphous phase and the crystalline phase) The Ge contents and the difference between the amorphous and crystalline phases of the soft magnetic alloy particles contained in the inductors manufactured in the examples and comparative examples are analyzed.

[0153] The inductor is placed in an epoxy mixture and hardened, after which the sides of the inductor body in the L-axis and T-axis directions are polished to the 1 / 2 point in the W-axis direction, and then fixed and maintained in a vacuum chamber to obtain a cross-sectional sample of the inductor body.

[0154] For the cross-sectional sample of the obtained inductor body, the soft magnetic alloy particles dispersed in the resin are subjected to line analysis using an EDS (Energy Disperse X-Ray Spectrometer) installed in a Transmission Electron Microscope (TEM).

[0155] Specifically, using the surface of any one nanocrystal particle as a reference, we performed spot quantitative analysis of 20 nm inside the nanocrystal particle and 200 nm outside the nanocrystal particle, and compared the maximum value inside the nanocrystal particle with the maximum value in the amorphous part. We performed spot quantitative analysis at six points each, and calculated the average Ge content.

[0156] At this time, the average Ge atomic content (Ge(a), Ge(c)) (unit: at%) in the amorphous phase and the crystalline phase and the content difference (Ge(a)-Ge(c)) (unit: at%) are shown in Table 2 below.

[0157] Referring to Table 2 below, it can be seen that the average Ge atomic content in the amorphous phase (Ge(a)) is higher than the average Ge atomic content in the nanocrystals (Ge(c)). This shows that the Ge element, which has a relatively large atomic weight (compared to the Si element, etc.), remains in the amorphous phase and plays a role in suppressing the growth of nanocrystals in the soft magnetic alloy particles.

[0158] [Table 2]

[0159] (Experimental Example 2: DTA analysis) The soft magnetic alloy particles of the examples and comparative examples are manufactured into ribbons having a thickness of 20 μm using a rapid cooling ribbon equipment, and a DTA analysis is carried out. x1 ) and the second crystallization temperature (T x2 ) and are shown in Table 1.

[0160] Referring to Table 1, in Examples 1 to 5, the second crystallization temperature (T x2 ) increases, the first crystallization temperature (T x1 ) and the second crystallization temperature (T x2 ) exceeds 100°C, improving the heat treatment process window for nanocrystal formation.

[0161] (Experimental Example 3: Crystal size and crystal fraction analysis) First, XRD graphs of soft magnetic alloy particles are obtained from cross-sectional samples of the inductor bodies manufactured in the examples and comparative examples.

[0162] The average crystal size of the nanocrystals contained in the soft magnetic alloy particles is calculated using the Scherrer equation expressed by the following Equation 2, which uses the full width at half maximum (FWHM) of the main peak in the XRD graph. The results are shown in Table 1.

[0163]

number

[0164] In Equation 2, D is the average crystal size, λ is the wavelength of the XRD target, β is the full width at half maximum (FWHM), and θ is the half value of the XRD graph peak 2θ.

[0165] Referring to Table 1, it can be seen that the average crystal size of the nanocrystals is 20 nm or less (about 17 nm level) in Examples 1 to 5. In contrast, it can be seen that the average crystal size of the nanocrystals is more than 20 nm in Comparative Examples 1 to 11.

[0166] In addition, after the XRD analysis, data fitting is performed, and the crystalline fraction is calculated through the area ratio of the amorphous and crystalline regions using Equation 1 described above.

[0167] Referring to Table 1, it can be seen that the crystalline fractions of Examples 1 to 5 are improved to 59% or more. In contrast, it can be seen that the crystalline fractions of Comparative Examples 1 to 11 are less than 59%.

[0168] (Experimental Example 4: Evaluation of electromagnetic characteristics) The magnetic permeability at a frequency of 1 kHz and the core loss under a magnetic field of 0.2 T and 100 kHz were measured and are shown in Table 1.

[0169] Referring to Table 1, it can be seen that Examples 1 to 5 have excellent electromagnetic properties, with a magnetic permeability of 5300 or more and a core loss of 1590 mW / cc or less. In contrast, Comparative Examples 1 to 11 have magnetic permeability of less than 5300 and a core loss of more than 1590 mW / cc, and therefore deteriorated electromagnetic properties.

[0170] Furthermore, referring to Table 1, it can be seen that Examples 1 to 5 exhibit the effects described above, and at the same time, when compared with Comparative Examples 1 to 11, the Ms values ​​are at similar levels.

[0171] Although the preferred embodiment of the present invention has been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the detailed description and drawings of the invention, which of course also fall within the scope of the present invention. [Explanation of symbols]

[0172] 11: Coarse magnetic particles 12: Fine magnetic particles 20: Resin 100, 200, 300: Inductor 110, 210, 310: Body 120: Support member 130, 230, 330: Coil 131: Upper coil 132: Lower coil 133, 231, 331: Insulating layer 140:Beer 150, 250: Core 161, 162, 261, 262, 361, 362: External electrode 211:Mold section 212: Cover part

Claims

1. Includes nanocrystalline and amorphous, includes Fe (iron) and Ge (germanium), When the average Ge content in the amorphous phase is Ge(a) (at%) and the average Ge content in the nanocrystals is Ge(c) (at%), the soft magnetic alloy particles are characterized in that Ge(a)-Ge(c)>0.

2. 2. The soft magnetic alloy particle according to claim 1, wherein the soft magnetic alloy particle is represented by the following composition formula 1: Composition formula 1 Fe a Co b Ge c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at %) of the corresponding element, where 0<a≦90, 0≦b≦10, 0<c≦5, 0<d≦20, and a+b+c+d=100. The M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

3. 3. The soft magnetic alloy particle according to claim 2, wherein said M does not contain Si.

4. 4. Soft magnetic alloy particles according to claim 3, characterized in that 0.5≦c≦4.

5. 4. The soft magnetic alloy particles according to claim 3, wherein 70≦a≦80.

6. 4. The soft magnetic alloy particles according to claim 3, wherein 2≦b≦6.

7. 4. The soft magnetic alloy particles according to claim 3, wherein 75≦a+b≦90.

8. 4. The soft magnetic alloy particles according to claim 3, wherein 10≦d≦20.

9. 4. The soft magnetic alloy particles according to claim 3, wherein 0.1≦Ge(a)−Ge(c)≦0.

7.

10. 4. The soft magnetic alloy particles according to claim 3, wherein M comprises B, P, Cu, or a combination thereof.

11. 4. The soft magnetic alloy particles according to claim 3, characterized in that the crystallinity of the soft magnetic alloy particles is 59% or more and 70% or less.

12. 4. The soft magnetic alloy particle according to claim 3, wherein the nanocrystals have an average crystal size of 20 nm or less.

13. a body including a magnetic material including soft magnetic alloy particles; A coil disposed within the body; an external electrode disposed on an external surface of the body; The soft magnetic alloy grains include nanocrystals and amorphous material, and contain Fe (iron) and Ge (germanium), and when the average Ge atomic content in the amorphous material is Ge(a) (at%) and the average Ge atomic content in the nanocrystals is Ge(c) (at%), the inductor is characterized in that Ge(a)-Ge(c)>0.

14. The inductor according to claim 13 , wherein the soft magnetic alloy grains are represented by the following composition formula 1: Composition formula 1 Fe a Co b Ge c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at %) of the corresponding element, where 0<a≦90, 0≦b≦10, 0<c≦5, 0<d≦20, and a+b+c+d=100. The M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

15. The inductor according to claim 14 , wherein M does not include Si.

16. 16. The inductor of claim 15, wherein 0.5≦c≦4.

17. 16. The inductor according to claim 15, wherein the crystallinity of the soft magnetic alloy grains is 59% or more and 70% or less.

18. 16. The inductor of claim 15, wherein the nanocrystals have an average crystal size of 20 nm or less.

19. The coil includes a support member and an upper coil and a lower coil disposed on an upper surface and a lower surface, respectively, of the support member; The inductor of claim 13 , wherein the upper coil and the lower coil are electrically connected to each other through a via that penetrates the support member.

20. the body includes a molded portion, a cover portion disposed on one surface of the molded portion, and a core protruding from the one surface of the molded portion; The inductor according to claim 13 , wherein the coil is disposed between one surface of the molded portion and the cover portion, and the core passes through the coil.

21. The inductor of claim 13 , wherein the body includes a plurality of magnetic sheets containing the magnetic material.

Citation Information

Patent Citations

  • Laminated inductor

    JP2018206836A