Manufacturing method of metal carbide and hydrocarbon and carbon-containing member

A method using molten salts and carbon electrodes at lower temperatures efficiently produces metal carbide and hydrocarbons, addressing energy inefficiencies and CO2 emissions in traditional methods, achieving high yields and low-temperature hydrocarbon production.

JP2024152637AInactive Publication Date: 2024-10-25DAIKIN INDUSTRIES LTD +1

Patent Information

Application Number
JP2024048286
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-03-25
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing metal carbide require high temperatures, leading to low energy efficiency and significant CO2 emissions, and existing carbon sources for metal carbide production yield low metal carbide, with limited experimental data supporting improved yields using carbon dioxide.

Method used

A method involving a molten salt containing alkali or alkaline earth metal ions, using a carbon electrode to produce metal carbide at lower temperatures (800°C or lower) by applying a voltage, followed by hydrolyzing the metal carbide to obtain hydrocarbons, utilizing electrodes made of glassy carbon, natural graphite, or highly oriented pyrolytic graphite.

Benefits of technology

The method enables rapid and efficient production of metal carbide and hydrocarbons at lower temperatures, with high yields and reduced CO2 emissions, producing hydrocarbons like acetylene efficiently.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152637000001_ABST
    Figure 2024152637000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method capable of efficiently obtaining a metal carbide through a prompt progress of a reaction at a comparatively low temperature, a method of manufacturing hydrocarbon from the obtained metal carbide, and a carbon-containing member carrying the metal carbide.SOLUTION: A manufacturing method of a metal carbide includes: preparing a molten salt containing at least one kind of first metal ion selected from a group consisting an alkali metal ion and an alkaline earth metal ion; preparing an electrode containing carbon; and applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing a carbide of the first metal.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing metal carbides and hydrocarbons, and to a carbon-containing component. [Background technology]

[0002] Acetylene is an industrially important substance as a raw material for various organic compounds. Acetylene is usually obtained by the reaction of metal carbide (mainly calcium carbide) with water.

[0003] Calcium carbide is generally obtained by heating a mixture of quicklime (calcium oxide) and coke to a high temperature in an electric furnace (for example, Patent Document 1). Patent Document 2 proposes, with regard to the production of calcium carbide, to previously briquette coke and mix it with quicklime. Patent Document 3 proposes a method for producing lithium carbide by reacting metallic lithium obtained by melt electrolysis of lithium chloride with carbon powder such as carbon black. Non-Patent Document 1 proposes a method for producing lithium carbide by reacting metallic lithium obtained by molten salt electrolysis of lithium hydroxide with a carbon source such as carbon dioxide. Non-Patent Document 2 proposes a method for producing lithium carbide by reacting metallic lithium with carbon. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Unexamined Patent Publication No. 178412 / 1983 [Patent Document 2] JP 2018-35328 A [Patent Document 3] Japanese Patent Application Publication No. 2-256626 [Non-patent literature]

[0005] [Non-Patent Document 1] McEnaney JM, Rohr BA, Nielander AC, Singh AR, King LA, Norskov JK, Jaramillo TF, “A cyclic electrochemical strategy to produce acetylene from CO2, CH4, or alternative carbon sources.”, Sustain Energy Fuels 4:2, 752-2759 (2020) [Non-Patent Document 2] Uwe Ruschewitz, “Binary and ternary carbides of alkali and alkaline-earth metals”, Coordination Chemistry Reviews 244, 115-136 (2003) Summary of the Invention [Problem to be solved by the invention]

[0006] To produce metal carbide, it is usually necessary to heat the raw material to 2000°C or higher. Therefore, there is a problem that the energy efficiency is low and a large amount of carbon dioxide is generated. In addition, in Patent Documents 1 to 3, carbon itself is used as the carbon source of metal carbide. In Non-Patent Document 1, it is described that when carbon dioxide is used as the carbon source, the yield of lithium carbide does not exceed 20% in theory, but the yield of lithium carbide can be increased by using carbon as the carbon source. However, no experimental data supporting this is shown. In Non-Patent Document 2, it is described that amorphous carbon or graphite is used as the carbon source, but in order to produce crystalline lithium carbide, it is necessary to contact metallic lithium vapor at 800°C to 900°C or to contact metallic lithium in an arc melting furnace at approximately 3500°C or higher.

[0007] The present disclosure aims to provide a production method in which a reaction proceeds quickly at a relatively low temperature (for example, 800° C. or lower) and metal carbide can be efficiently obtained. The present disclosure further provides a method for producing hydrocarbons from the obtained metal carbide. In addition, the present disclosure provides a carbon-containing member carrying metal carbide. [Means for solving the problem]

[0008] The present disclosure includes the following aspects. [1] Preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; Providing an electrode comprising carbon; and applying a voltage to the molten salt using the electrodes to obtain a metal carbide composition containing a carbide of the first metal.

[0009] [2] The method for producing metal carbide according to the above [1], wherein the molten salt is substantially free of carbonate ions.

[0010] [3] The method for producing metal carbide according to the above [1] or [2], wherein the electrode contains at least one selected from the group consisting of glassy carbon, natural graphite, isotropic graphite, highly oriented pyrolytic graphite, plastic formed carbon and conductive diamond.

[0011] [4] The method for producing metal carbide according to any one of the above [1] to [3], wherein the electrode contains highly oriented pyrolytic graphite.

[0012] [5] The method for producing metal carbide according to any one of the above [1] to [4], wherein the molten salt contains at least one of a halide ion and an oxide ion as an anion.

[0013] [6] The method for producing metal carbide according to any one of the above [1] to [5], wherein the molten salt contains both halide ions and oxide ions as anions.

[0014] [7] The method for producing metal carbide according to the above [5] or [6], wherein the molten salt contains chloride ions as the halide ions.

[0015] [8] The method for producing metal carbide according to the above [5] or [6], wherein the molten salt contains a fluoride ion as the halide ion.

[0016] [9] The method for producing a metal carbide according to any one of the above [1] to [8], wherein the metal carbide composition further contains at least one selected from the group consisting of carbon, an elemental substance, a halide, a carbonate, an oxide, a hydride and a peroxide of the first metal.

[0017]

[10] The method for producing metal carbide according to any one of the above [1] to [9], wherein the molten salt contains, as the first metal ion, at least one selected from the group consisting of lithium ions, sodium ions, and potassium ions, and calcium ions.

[0018]

[11] Preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; Providing an electrode comprising carbon; applying a voltage to the molten salt using the electrodes to obtain a metal carbide composition containing a carbide of the first metal; and a first metal carbide being hydrolyzed to obtain a hydrocarbon-containing gas;

[0019]

[12] The method for producing hydrocarbons according to the above

[11] , wherein the hydrocarbon is acetylene.

[0020]

[13] The method for producing hydrocarbons according to

[11] or

[12] above, wherein the gas contains acetylene as the hydrocarbon and further contains at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

[0021]

[14] A substrate comprising carbon; a metal carbide composition supported on the substrate, the metal carbide composition including a carbide of at least one first metal selected from the group consisting of alkali metals and alkaline earth metals. Effect of the Invention

[0022] According to the present disclosure, it is possible to provide a production method in which a reaction proceeds quickly at a relatively low temperature and metal carbide can be efficiently obtained, a method for producing hydrocarbons from the obtained metal carbide, and a carbon-containing member supporting metal carbide. [Brief description of the drawings]

[0023] [Figure 1] 1 is a flow chart illustrating a method for producing metal carbide according to the present disclosure. [Diagram 2] 1 is a flow chart illustrating a method for producing hydrocarbons according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] In the method for producing metal carbide disclosed herein, a voltage is applied to a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions to obtain metal carbide. According to the method using this molten salt, the reaction proceeds quickly at a relatively low temperature of 800° C. or less, and metal carbide can be obtained efficiently.

[0025] The present disclosure also includes a method for obtaining hydrocarbons by hydrolyzing the metal carbides obtained by the above-mentioned method, which can efficiently obtain high-purity hydrocarbons.

[0026] The present disclosure encompasses a carbon-containing component having a metal carbide supported thereon, the carbon-containing component being useful in the production of hydrocarbons.

[0027] [Metal carbide manufacturing method] The method for producing metal carbide according to the present disclosure includes preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, preparing an electrode containing carbon, and applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing a carbide of the first metal. According to the method according to the present disclosure, the first metal carbide can be obtained in high yield. Figure 1 is a flow chart showing the method for producing metal carbide according to the present disclosure.

[0028] (I) Preparation of molten salt (S11) A molten salt containing a first metal ion is prepared. The first metal ion is a metal source for the target metal carbide. The molten salt is prepared by ionizing a salt containing the first metal ion (first metal salt). It is not necessary that the entire first metal salt is ionized. For convenience, the metal salt contained in the electrolytic bath is referred to as a molten salt, even if it is not completely ionized.

[0029] (First metal ion) The first metal ion is at least one selected from the group consisting of alkali metal ions and alkaline earth metal ions. Carbides of alkali metals and alkaline earth metals, also known as acetylides, are easily hydrolyzed to produce acetylene, and are of high industrial value.

[0030] The alkali metal may be at least one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs) and francium (Fr). The alkali metal may be at least one selected from the group consisting of Li, Na, K, Rb and Cs. The alkali metal may in particular be at least one selected from the group consisting of Li, Na, K and Cs.

[0031] The alkaline earth metal may be at least one selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba) and radium (Ra). The alkaline earth metal may be at least one selected from the group consisting of Mg, Ca, Sr and Ba.

[0032] In terms of industrial value, the first metal ion may include an alkaline earth metal ion. The first metal ion may include an alkali metal ion together with an alkaline earth metal ion. The alkali metal ion has an excellent function as an electrolyte, such as facilitating the ionization of an alkaline earth metal salt, promoting the generation of an alkaline earth metal ion, lowering the melting point of the molten salt, and enabling electrolysis at a lower temperature. The first metal ion may include at least one selected from the group consisting of Li, Na, K, Rb, and Cs ions as an alkali metal ion, and at least one selected from the group consisting of Be, Mg, Ca, Sr, and Ba ions as an alkaline earth metal ion. In particular, it may include at least one of Li, Na, and K ions, and Ca ions.

[0033] The amount of the first metal ion contained in the molten salt is not particularly limited. From the viewpoint of reaction efficiency, the number of moles of the first metal ion is preferably 1 mol% or more, more preferably 2 mol% or more, and particularly preferably 3 mol% or more, based on the total number of moles of cations in the electrolytic bath. The number of moles of the first metal ion is preferably 20 mol% or less, more preferably 15 mol% or less, and particularly preferably 10 mol% or less, based on the total number of moles of cations in the electrolytic bath. In one embodiment, the number of moles of the first metal ion is 1 mol% or more and 20 mol% or less, based on the total number of moles of cations in the electrolytic bath.

[0034] (other metal ions) The molten salt may contain metal ions (second metal ions) other than the first metal ions. The second metal ions are not particularly limited as long as the first metal carbide, which is the target substance, can be stably precipitated. It is preferable that the salt of the second metal ions is ionized at a temperature of 800° C. or less.

[0035] The second metal may be at least one selected from the group consisting of rare earth elements, aluminum (Al), gallium (Ga), indium (In), thallium (Tl), zinc (Zn), cadmium (Cd), gold (Au), silver (Ag) and copper (Cu). The rare earth elements may be scandium (Sc), yttrium (Y), lanthanide elements and actinide elements.

[0036] (anion) Examples of counter ions (anions) of the first and second metal ions include halide ions, sulfate ions, phosphate ions, nitrate ions, acetate ions, carboxylate ions, and oxide ions (O 2- ) is at least one selected from the group consisting of:

[0037] The anion may include at least one of a halide ion and an oxide ion. In particular, the anion may include both a halide ion and an oxide ion. While an oxide of a first metal is easy to obtain, its melting temperature tends to be high. A halide of a first metal is generally used as a molten salt. However, the halide ion may generate a halogen gas at the anode, which has a high oxidizing power (and may cause corrosion). When the molten salt includes both a halide ion and an oxide ion, the melting temperature of the molten salt can be lowered while suppressing the generation of halogen gas.

[0038] The halogen includes at least one selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I) and astatine (At). The halogen may be at least one selected from the group consisting of F, Cl, Br and I, and may be, in particular, F and / or Cl.

[0039] The first metal salt used in the preparation of the molten salt is, for example, a first metal salt containing an alkaline earth metal ion, specifically, CaO, CaCl 2 , CaF 2 , CaBr 2 , CaI 2 , CaH 2 , Ca 3 P 2 Specific examples of the first metal salt containing an alkali metal ion include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI.

[0040] The molten salt is carbonate ion (CO 3 2-) is preferably substantially free of carbonate ions. If the molten salt contains carbonate ions, it will react with electrons generated by the discharge of the first metal (Formula 1) and carbon will be easily produced. This will reduce the yield of the first metal carbide. If the molten salt is substantially free of carbonate ions, such side reactions are suppressed and the yield of the first metal carbide will be increased. (Formula 1) 2CO 3 2- +8e - → 2C+6O 2-

[0041] "Substantially free of carbonate ions" allows the presence of carbonate ions to an extent that they are not involved in the electrolytic reaction. The molten salt may contain, for example, about 1.0 mol% or less of carbonate ions. The carbonate ion concentration in the molten salt may be 0.5 mol% or less, 0.3 mol% or less, or 0 mol%.

[0042] (II) Preparation of carbon-containing electrodes (S12) An electrode containing carbon (hereinafter, sometimes referred to as a "carbon electrode") is prepared. The carbon electrode functions as a cathode during electrolysis. The carbon contained in the carbon electrode serves as a carbon source for the target metal carbide.

[0043] The carbon may be present at least on the surface of the carbon electrode. The surface of the carbon electrode is the portion that can come into contact with the first metal ion.

[0044] The raw material of the carbon electrode may be, for example, at least one carbon material selected from the group consisting of glassy carbon (GC), graphite, isotropic graphite, highly oriented pyrolytic graphite (HOPG), plastic formed carbon (PFC) and conductive diamond. Among them, from the viewpoint of Faraday efficiency, it may be a carbon material having a high degree of crystallinity, and may be HOPG. Other examples of carbon materials having a high degree of crystallinity include graphene, carbon nanotubes, carbon nanohorns, and carbon fibers. The carbon electrode may be obtained by molding the above carbon material, for example, a woven fabric, a nonwoven fabric, or a felt-like material.

[0045] Alternatively, the carbon electrode may be a molded body of a metal such as Ag, Cu, Ni, Pb, Hg, Tl, Bi, In, Sn, Cd, Au, Zn, Pd, Ga, Ge, Fe, Pt, Ru, Ti, Cr, Mo, W, V, Nb, Ta, Zr, or an alloy thereof, coated with the above-mentioned carbon material. The carbon electrode may not include the first metal.

[0046] The material of the other electrode (anode) is not particularly limited. Examples of the material of the anode include Pt, conductive metal oxides, and the above-mentioned carbon materials. Examples of electrodes made of conductive metal oxides include transparent conductive electrodes called ITO electrodes in which a mixed oxide of indium and tin is formed on glass, electrodes called DSA electrodes (trademark of De Nora Permelec Electrodes, Inc.) in which an oxide of a platinum group metal such as ruthenium or iridium is formed on a substrate such as titanium, and La 1-x Sr x FeO 3-δ (0≦x≦0.5 (particularly, 0.1≦x≦0.5), 0≦δ≦0.5), etc. Among them, conductive metal oxide anodes are preferred because they are less likely to be consumed due to oxidation reactions.

[0047] (III) Application of voltage (S13) Next, a voltage is applied to the molten salt. Carbon is reduced at the cathode (C≡C 2- ) reacts with the first metal ion to obtain a composition containing the first metal carbide (metal carbide composition). The application of voltage can also promote ionization of the first metal salt that has not been ionized in the molten salt.

[0048] When the first metal is Ca, calcium carbide (CaC 2 ) is produced (Equation 2). Calcium carbide is typically deposited on the cathode. On the cathode, calcium metal may be further produced by a side reaction (Equation 3). Some or all of the calcium metal produced in this side reaction may further react to form calcium carbide. (Formula 2) Ca 2++2C +2e - → CaC 2 (Formula 3) Ca 2+ +2e - → Ca

[0049] The voltage is applied at a temperature at which the molten salt can be maintained in a molten state. The temperature of the electrolytic bath may be, for example, 350° C. or higher, or 400° C. or higher. The temperature of the electrolytic bath may be, for example, 800° C. or lower, or 700° C. or lower. According to the present disclosure, the reaction proceeds at such a relatively low temperature, and therefore the energy efficiency is high.

[0050] The applied voltage is set so that the cathode potential is lower (more noble) than the potential (Emc) at which the first metal is deposited on the carbon electrode. This can further improve the selectivity of the first metal carbide. If the cathode potential is excessively high (more noble), the desired first metal carbide is difficult to generate. If the cathode potential is excessively low (more noble), the first metal carbide is generated, but a metal contained in the molten salt whose redox potential in the molten salt is higher (more noble) than the set cathode potential is deposited. If the molten salt contains multiple metals whose redox potentials are close to each other, an alloy of multiple metals may be deposited depending on the set cathode potential. The potential Emc can be determined by performing cyclic voltammetry measurement in the molten salt to be used using the carbon electrode (e.g., a HOPG electrode).

[0051] The set current value when constant current electrolysis is performed may be appropriately set so that the cathode potential during electrolysis falls within the above-mentioned potential range.

[0052] The metal carbide composition includes a carbide of a first metal. The first metal carbide is a main component of the metal carbide composition. The main component is a component that occupies 50 mass% or more of the total mass of the metal carbide composition. The content ratio of the first metal carbide may be 80 mass% or more, or 90 mass% or more, of the mass of the metal carbide composition. The content ratio of the first metal carbide may be 99.9 mass% or less, or 99 mass% or less, of the mass of the metal carbide composition. In one embodiment, the content ratio of the first metal carbide is 80 mass% or more and 99.9 mass% or less of the mass of the metal carbide composition.

[0053] The metal carbide composition is usually obtained in a state supported on a cathode (strictly speaking, a substrate derived from a carbon electrode used as a cathode). When a molten salt having excellent solubility of the first metal carbide is used, the first metal carbide is obtained in a state where it is partially or entirely dissolved in the molten salt. If the first metal carbide is dissolved in the molten salt in advance, the first metal carbide obtained by electrolysis is easily precipitated on the carbon electrode, and is easily obtained in a state where it is supported on a substrate derived from the carbon electrode.

[0054] The metal carbide composition may include at least one selected from the group consisting of carbon, an elemental, halide, carbonate, oxide, hydride, and peroxide of a first metal. The metal carbide composition may further include at least one selected from the group consisting of an elemental, halide, carbonate, oxide, and carbide of a second metal.

[0055] The metal carbide composition may further include at least one selected from the group consisting of solidified electrolytes (other metal salts), halides, oxides, metals, and hydrates of the materials constituting the device.

[0056] The carbon contained in the metal carbide composition is at least one selected from the group consisting of nanocarbon materials such as graphite, amorphous carbon, glassy carbon, carbon nanotube, diamond, nanodiamond, graphene, etc. By continuing the electrolysis of the above method, the first metal carbide can be further obtained from the carbon contained in the metal carbide composition. In this case, the yield can be further increased.

[0057] The presence of the first metal carbide, the first metal itself, compounds containing the first metal, and other impurities can be confirmed and their quantities can be determined, for example, by Raman spectroscopy and X-ray diffraction (XRD) analysis of the composition.

[0058] [Carbon-containing materials] The present disclosure encompasses a carbon-containing component comprising a substrate comprising carbon and a metal carbide composition supported on the substrate, the metal carbide composition comprising at least one carbide of a first metal selected from the group consisting of alkali metals and alkaline earth metals. The carbon-containing component according to the present disclosure can be utilized in the production of hydrocarbons.

[0059] The carbon-containing member can be obtained by, for example, the above-mentioned method for producing a metal carbide. That is, the carbon-containing member can correspond to the carbon electrode obtained by electrolyzing the above-mentioned molten salt using the above-mentioned carbon electrode. In this case, the substrate is derived from the above-mentioned carbon electrode.

[0060] The metal carbide composition may be supported on at least a portion of the surface of the substrate. The surface of the substrate typically corresponds to the portion of the carbon electrode that was in contact with the first metal ion. Supported includes a state in which at least a portion of the surface of the substrate is covered with the metal carbide composition.

[0061] However, the carbon contained in the carbon electrode is consumed as a carbon source for the first metal carbide, and then precipitates again as the first metal carbide. Therefore, the substrate usually does not retain the original shape of the carbon electrode. In addition, the carbon electrode may contain metal carbide. Therefore, it may not be possible to clearly distinguish between the metal carbide contained in the carbon electrode before electrolysis and the metal carbide generated by electrolysis. In this case, for example, it is possible to confirm whether or not the carbon-containing member according to the present disclosure is one that is described below.

[0062] When an elemental analysis is performed by energy dispersive X-ray analysis (EDX) on a cross section passing through the center (or center of gravity) of a carbon-containing member, the first metal and carbon are detected on the cross section. Since the substrate (carbon electrode) does not usually contain the first metal, the detection of the first metal and carbon can be safely considered to indicate the presence of the first metal carbide. Furthermore, when the concentration of the first metal is higher near the outer edge than near the center in the cross section, it can be safely considered that the substrate and the metal carbide composition supported thereon are present. This is because carbon present on the outer side of the carbon electrode is usually more likely to react (to become the first metal carbide) than the center. According to the above method, even if the boundary between the substrate and the metal carbide composition is not clear, it can be confirmed whether the component is a carbon-containing component according to the present disclosure.

[0063] [Method of producing hydrocarbons] The present disclosure encompasses a method for producing hydrocarbons from a first metal carbide. That is, the method for producing hydrocarbons according to the present disclosure includes preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, preparing an electrode containing carbon (carbon electrode), applying a voltage to the molten salt using the carbon electrode to obtain a metal carbide composition containing the carbide of the first metal, and hydrolyzing the carbide of the first metal to obtain a gas containing a hydrocarbon. Figure 2 is a flowchart showing the method for producing hydrocarbons according to the present disclosure.

[0064] (1) Preparation of molten salt (S21) The molten salt is prepared in the same manner as in the preparation of the molten salt (S11) in the above-mentioned method for producing metal carbide.

[0065] (2) Preparation of carbon-containing electrodes (S22) A carbon electrode is prepared in the same manner as in (II) Preparation of carbon-containing electrode (S12) in the above-mentioned method for producing metal carbide.

[0066] (3) Application of voltage (S23) A voltage is applied to the molten salt in the same manner as in the voltage application (S13) in the above-mentioned method for producing a metal carbide, thereby obtaining a composition containing a first metal carbide.

[0067] (4) Hydrolysis of metal carbides (S24) Next, the first metal carbide is brought into contact with water to be hydrolyzed. This results in a gas containing the target hydrocarbon. According to the present disclosure, the Faraday efficiency e for the production of hydrocarbons is improved. Hydrocarbons usually have low solubility in water. Therefore, the produced hydrocarbons are quickly discharged into the gas phase and collected.

[0068] The first metal carbide may be isolated from the metal carbide composition and hydrolyzed. The isolation is performed, for example, by a method of pulverizing the metal carbide composition and utilizing the difference in specific gravity. Alternatively, the metal carbide composition may be hydrolyzed as it is. For example, an electrode (which may be the "carbon-containing member" according to the present disclosure) on which the metal carbide composition is precipitated is brought into contact with water as it is. In this case, the second metal carbide that may be contained in the metal carbide composition may also be hydrolyzed to generate hydrocarbons.

[0069] The resulting hydrocarbons include, for example, methane, ethane, ethylene, acetylene (C 2 H 2), methylacetylene, propane, propylene, butane, and butene. When an isolated first metal carbide is used or when the amount of impurities (particularly simple metals) contained in the composition is small, acetylene is obtained as the main component. The main component is a component that accounts for 50% by mass or more of the total mass of the gas recovered. Acetylene is an industrially important hydrocarbon.

[0070] The gas obtained may contain impurities such as water vapor, hydrogen, nitrogen, and oxygen in addition to hydrocarbons. The amount of impurities is preferably 10% by mass or less, more preferably 1% by mass or less, of the gas recovered. The amount of impurities may be 0.0001% by mass or more, or may be 0.001% by mass or more, of the gas recovered. In one embodiment, the amount of impurities is 0.0001% by mass or more and 1% by mass or less of the gas recovered.

[0071] The resulting gas contains acetylene as a hydrocarbon, and may further contain at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

[0072] The presence of hydrocarbons and impurities can be confirmed and their quantity can be determined, for example, by gas chromatography mass spectrometry (GC-MS analysis) of the recovered gas, Fourier transform infrared absorption spectrometry (FT-IR analysis) equipped with a gas cell, or ultraviolet-visible absorption spectrometry (UV-Vis analysis).

[0073] The amount of water to be brought into contact with the composition is appropriately set according to the mass of the composition. The amount of water is, for example, an amount equal to or more than the amount required for hydrolysis of the metal carbide and metal contained in the composition. In addition, it is desirable to use an amount of water that allows the entire composition to be immersed and that takes into consideration evaporation due to heat generated during hydrolysis.

[0074] Hydrolysis of the first metal carbide produces a hydroxide of the first metal along with hydrocarbons. For example, the hydrolysis of calcium carbide produces calcium hydroxide along with acetylene (Equation 4). (Formula 4) CaC2 +2H 2 O → C 2 H 2 +Ca(OH) 2

[0075] Although the embodiments of the present disclosure have been described above in detail, the present disclosure is not limited thereto.

[0076] In the above embodiment, the carbon electrode is exemplified by a metal molded body coated with a carbon material and an electrode obtained by forming a carbon material, but is not limited thereto. The carbon electrode may be an electrode (typically a metal electrode) on which a composition containing carbon is deposited (hereinafter referred to as a "third carbon electrode"). The third carbon electrode may be obtained, for example, by electrolyzing a molten salt containing a first metal ion derived from a first metal carbonate and a carbonate ion. The third carbon electrode may also be obtained, for example, by electrolyzing a molten salt containing a first metal ion in the presence of a carbonate ion derived from carbon dioxide. In these cases, the third carbon electrode is obtained as a cathode after the electrolysis. EXAMPLES

[0077] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto.

[0078] [Example 1-1] (Manufacturing of metal carbides) Eutectic composition of LiCl, KCl, CaCl 2 (LiCl / KCl / CaCl 2 = 52.3 mol% / 11.6 mol% / 36.1 mol%), with 3.0 mol% CaO mixed (i.e., LiCl / KCl / CaCl 2 / CaO=50.8 mol% / 11.3 mol% / 35.0 mol% / 2.9 mol%), and dried in vacuum at 200°C and 100 Pa or less for 24 hours or more. Each of these mixed salts was placed in a glass container, set in an electric furnace, and heated to 450°C. 2 -CaO molten salt was obtained.

[0079] Next, a working electrode (1 cm × 1.5 cm HOPG), a counter electrode (coiled platinum wire), and a reference electrode (Ag + A lid (Ag+ / Ag) was attached to the container and the container was sealed with the lid. Next, a voltage was applied for 30 minutes using a potentio-galvanostat while maintaining the potential of the working electrode relative to the reference electrode at 0.3 V. It was confirmed that a deposit was formed on the working electrode. All experimental operations were performed in a glove box maintained in a high-purity argon atmosphere. The potential of the working electrode was measured between the reference electrode (Ag+ / Ag) and the cathode, and calibrated based on the Li-Ca alloy deposition potential.

[0080] (Hydrocarbon production) The precipitate was placed in a sealed test tube. Pure water was added to the test tube in small amounts at room temperature (23°C) to hydrolyze the precipitate. The total amount of water added was 2.5 ml. After confirming that bubbles were being generated in the test tube, the test tube was left to stand until the bubbles were no longer observed. Next, 100 μl (microliters) of gas was collected from the test tube using a gas-tight syringe.

[0081] Using a gas chromatograph (GC) device, GC-MS analysis was performed on the obtained gas, and the main components were found to be C 2 H 2 It was confirmed that methane, ethane, and hydrogen were produced as by-products. Other components included water, carbon dioxide, nitrogen, oxygen, and argon. The amount of each component produced was also confirmed. 2 H 2 The mass fraction of was well above 50 mass%. 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0082] C 2 H 2 The Faraday efficiency for gas production was calculated to be about 0.7%. The higher the Faraday efficiency for hydrocarbon gas production, the higher the Faraday efficiency for metal carbide production.

[0083] [Example 1-2] The deposit and the hydrocarbon were obtained in the same manner as in Example 1, except that the potential of the working electrode relative to the reference electrode was maintained at 0.1 V and the voltage was applied for 30 minutes. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It is understood that this includes 2 H 2 The faradaic efficiency for gas production was calculated to be approximately 8.8%.

[0084] [Examples 1-3 to 1-6] Precipitates and hydrocarbons were obtained in the same manner as in Example 1-1, except that constant current electrolysis was performed while maintaining the current density at the value shown in Table 1. The hydrocarbons contained C as the main component. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 In Examples 1-4, the molten salt was previously prepared using CaC 2 was added in an amount of 2.0 mol % to the molten salt.

[0085] [Table 1]

[0086] [Examples 2-1 to 2-5] A deposit and a hydrocarbon were obtained in the same manner as in Example 1-1, except that graphite was used as the working electrode and electrolysis was performed under the conditions shown in Table 2. The hydrocarbon contained C as the main component. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0087] [Table 2]

[0088] [Examples 3-1 and 3-2] A deposit and a hydrocarbon were obtained in the same manner as in Example 1-1, except that GC was used as the working electrode and electrolysis was performed under the conditions shown in Table 3. The hydrocarbon contained C as the main component. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0089] [Table 3]

[0090] [Examples 4-1 to 4-7] Molten salts include NaCl, KCl, and CaCl 2 (NaCl / KCl / CaCl 2 = 33.4 mol% / 11.6 mol% / 55.0 mol%), 3.0 mol% CaO and 7.0 mol% CaC 2 Mixtures of NaCl, KCl, and CaCl 2 / CaO / CaC 2 A precipitate and a hydrocarbon were obtained in the same manner as in Example 1-1, except that electrolysis was performed under the conditions shown in Table 4 using a mixture of Ag and a reference electrode (Ag + The potential between the cathode and the Na-K-Ca alloy deposition potential was measured and calibrated. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0091] [Table 4]

[0092] [Examples 5-1 to 5-12] Molten salts include NaCl, KCl, and CaCl 2 (NaCl / KCl / CaCl 2 Precipitates and hydrocarbons were obtained in the same manner as in Example 1-1, except that electrolysis was performed under the conditions shown in Table 5 using a molten salt of CaC (=33.4 mol% / 11.6 mol% / 55.0 mol%) and a graphite working electrode at 550°C. 2 was added to the molten salt at 1.0 mol%. In Examples 5-6 to 5-12, CaC 2 was added in an amount of 7.0 mol % to the molten salt.

[0093] The amount of gas generated by hydrolysis (mL) and the C calculated by analyzing the gas 2 H 2 The Faraday efficiency of the production is shown in Table 5. Tables 6 to 8 also show the gas production amount and the Faraday efficiency. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0094] [Table 5]

[0095] [Examples 6-1 to 6-10] Precipitates and hydrocarbons were obtained in the same manner as in Example 5-1, except that GC (glassy carbon) was used as the working electrode and electrolysis was performed under the conditions shown in Table 6. In Examples 6-3 to 6-5, CaC 2 was added to the molten salt at 1.0 mol%. In Examples 6-6 to 6-10, CaC2 The main component of the hydrocarbon was C. 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0096] [Table 6]

[0097] [Examples 7-1 to 7-4] Precipitates and hydrocarbons were obtained in the same manner as in Example 5-1, except that HOPG (highly oriented pyrolytic graphite) was used as the working electrode and electrolysis was performed under the conditions shown in Table 7. In Examples 7-3 and 7-4, CaC 2 was added to the molten salt at 1.0 mol %. Hydrocarbons are mainly composed of C 2 H 2 It was confirmed that it contains C 2 H 2 Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0098] [Table 7]

[0099] [Examples 8-1 to 8-5] A precipitate and a hydrocarbon were obtained in the same manner as in Example 5-1, except that PFC (plastic formed carbon) was used as the working electrode and electrolysis was performed under the conditions shown in Table 8. In Examples 8-1 to 8-5, CaC 2 was added in an amount of 7.0 mol % to the molten salt. Hydrocarbons are mainly composed of C 2 H 2 It was confirmed that it contains C 2 H 2Since gas is being generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0100] [Table 8]

[0101] C 2 H 2 The faradaic efficiency of formation, e, was calculated as follows: First, the C in the collected gas was calculated from the total peak area and the calibration curve obtained from the GC-MS analysis. 2 H 2 The volume ratio of the gas phase in the collection vessel and the volume of the gas phase were calculated. 2 H 2 From the volume ratio of C 2 H 2 Finally, the volume of the generated C 2 H 2 The Faraday efficiency e (%) was calculated using the following formula, assuming that the temperature was at standard conditions (0°C, 101 kPa).

number

[0102] As can be seen from Tables 1 to 8, the desired first metal carbide was obtained by both constant potential electrolysis and constant current electrolysis. In particular, when HOPG with a high degree of crystallinity was used as the working electrode, acetylene (first metal carbide) was obtained with high faradaic efficiency. 2 By using molten salt, it was possible to obtain hydrocarbons from the precipitate with higher Faraday efficiency. 2 It is desirable to add CaC 2 This is believed to be because the dissolution of the molten salt was suppressed. [Industrial Applicability]

[0103] The production method of the present disclosure is useful in various fields because the reaction proceeds quickly at a relatively low temperature and metal carbide can be efficiently obtained.

Claims

1. Preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; Providing an electrode comprising carbon; and applying a voltage to the molten salt using the electrodes to obtain a metal carbide composition containing a carbide of the first metal.

2. The method for producing metal carbide according to claim 1 , wherein the molten salt is substantially free of carbonate ions.

3. 2. The method for producing metal carbide according to claim 1, wherein the electrode comprises at least one selected from the group consisting of glassy carbon, natural graphite, isotropic graphite, highly oriented pyrolytic graphite, plastic formed carbon, and conductive diamond.

4. The method for producing metal carbide according to claim 1 , wherein the electrode comprises highly oriented pyrolytic graphite.

5. 2. The method for producing metal carbide according to claim 1, wherein the molten salt contains at least one of a halide ion and an oxide ion as an anion.

6. 2. The method for producing metal carbide according to claim 1, wherein the molten salt contains both halide ions and oxide ions as anions.

7. 7. The method for producing metal carbide according to claim 5, wherein the molten salt contains chloride ions as the halide ions.

8. 7. The method for producing metal carbide according to claim 5, wherein the molten salt contains fluoride ions as the halide ions.

9. 2. The method for producing metal carbide according to claim 1, wherein the metal carbide composition further comprises at least one selected from the group consisting of carbon, an elemental substance, a halide, a carbonate, an oxide, a hydride, and a peroxide of the first metal.

10. 2. The method for producing metal carbide according to claim 1, wherein the molten salt contains, as the first metal ions, one selected from the group consisting of lithium ions, sodium ions, and potassium ions, and calcium ions.

11. Preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; Providing an electrode comprising carbon; applying a voltage to the molten salt using the electrodes to obtain a metal carbide composition containing a carbide of the first metal; and hydrolyzing the carbide of the first metal to obtain a gas containing hydrocarbons.

12. The method for producing hydrocarbons according to claim 11, wherein the hydrocarbon is acetylene.

13. 13. The method for producing hydrocarbons according to claim 11 or 12, wherein the gas contains acetylene as the hydrocarbon, and further contains at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

14. A substrate comprising carbon; a metal carbide composition supported on the substrate, the metal carbide composition comprising a carbide of at least one first metal selected from the group consisting of alkali metals and alkaline earth metals.

Citation Information

Patent Citations

  • Method for preparing calcium carbide through electrolysis

    CN116288415A

  • Electrolytic preparation of calcium carbide

    US2952591A

  • Method for producing metal carbide, method for producing hydrocarbon, and metal carbide composition

    WO2023058619A1

  • Method for producing metal carbide and hydrocarbon, and metal carbide composition

    WO2023058620A1

  • Production of calcium carbide by blast furnace process

    JP1986178412A

Cited By