Metal mold, method for manufacturing the same, and method for manufacturing molded product using the same
A multilayer plating film on a conductive metal base material addresses peelability and water repellency issues in molds, enabling efficient production of rubber and resin products with fine protrusions.
Patent Information
- Application Number
- JP2024063544
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-25
AI Technical Summary
Existing molds for manufacturing rubber and resin products with fine protrusions suffer from poor peelability, leading to potential damage and reduced water repellency due to inadequate multilayer plating films.
A mold with a multilayer plating film featuring a porous plating layer and a surface plating layer, composed of specific metals like Ni, Co, W, Cr, Rh, Ru, or Pd, is used to create a conductive metal base material with controlled pore diameters and thicknesses, enhancing peelability and water repellency.
The mold achieves high productivity in manufacturing rubber and resin products with numerous fine protrusions, ensuring excellent releasability and high water repellency.
Smart Images

Figure 2024152677000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a mold on which a multilayer plating film having many holes is formed, and a method for manufacturing a molded product using the mold. [Background technology]
[0002] It is known that forming many fine protrusions on the surface of rubber or resin molded products can provide water- and oil-repellent properties and change the coefficient of friction. A known method for manufacturing molded products with such fine protrusions is to mold rubber or resin using a mold with many holes on the surface.
[0003] Patent Document 1 describes that gloves with hair-like protrusions formed on the surface obtained by molding polyvinyl chloride using a hand mold with a porous Ni plating layer formed on the surface dry easily when wet and are less likely to get dirty.
[0004] However, the hand mold described in Patent Document 1 does not have sufficient releasability of the resin after molding, which can cause the molded product to be damaged when peeled off, or the plating layer to peel off and adhere to the molded product, reducing its water repellency. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2022-64122 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a mold on which a multilayer plating film having many holes is formed and which has excellent releasability for rubber molded articles and resin molded articles, a method for manufacturing the mold, and a method for manufacturing the molded articles with high productivity, in which many fine protrusions are formed on the surface and which have high water repellency. [Means for solving the problem]
[0007] The above-mentioned problem is solved by providing a mold having a multilayer plating film having many holes formed on a base material made of a conductive metal, wherein the multilayer plating film is formed by forming a porous plating layer mainly composed of Ni on the base material, and then forming a surface plating layer mainly composed of Ni, Co, W, Cr, Rh, Ru, Ir, or Pd on the porous plating layer, wherein the average diameter of the holes formed in the multilayer plating film is 1 to 300 μm in area-weighted average value, the thickness of the porous plating layer is 1 to 500 μm, and the thickness of the surface plating layer is 0.01 to 150 μm.
[0008] The multilayer plating film is formed by forming a porous plating layer mainly composed of Ni on the substrate, forming an intermediate plating layer mainly composed of Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir or Ru on the porous plating layer, and forming a surface plating layer mainly composed of Ni, Co, W, Cr, Rh, Ru, Ir or Pd on the intermediate plating layer, and it is preferable that the thickness of the intermediate plating layer is 0.01 to 150 μm.
[0009] The above problem is solved by a method for manufacturing the mold, which comprises a porous plating step of forming the porous plating layer in a plating solution containing Ni ions, and a surface plating step of forming the surface plating layer in a plating solution containing Ni ions, Co ions, W ions, Cr ions, Rh ions, Ru ions, Ir ions, or Pd ions, and the porous plating layer is formed by plating at 10 A / dm 2 The above-mentioned problems can also be solved by providing a method for manufacturing a mold, in which the mold is formed by electroplating at a cathode current density of at least 1000 volts.
[0010] A preferred embodiment of the mold is a method for producing a molded product having a large number of protrusions formed on the surface thereof by filling the mold with rubber or resin, curing or solidifying the rubber or resin, and then releasing the obtained molded product from the mold. [Effects of the Invention]
[0011] The mold of the present invention, on which a multilayer plating film having many holes is formed, has excellent releasability for rubber molded articles and resin molded articles. According to the mold manufacturing method of the present invention, such molds can be manufactured with high productivity. Furthermore, by using such molds, many fine protrusions are formed on the surface, and rubber molded articles and resin molded articles having high water repellency can be manufactured with high productivity. [Brief explanation of the drawings]
[0012] [Figure 1] 1 shows optical microscope images of the surfaces of multilayer plating films formed on molds in Examples 1 to 4. [Figure 2] 1 shows optical microscope images of the surfaces of multilayer plating films formed on molds in Examples 5 and 6 and Comparative Example 1. [Figure 3] 1 shows optical microscope images and laser microscope images of the surfaces of silicone rubber sheets (surfaces peeled from the mold) in Examples 1 to 4. [Figure 4] 1 shows optical microscope images and laser microscope images of the surfaces (surfaces peeled from the mold) of the silicone rubber sheets or polypropylene sheets in Examples 5 and 6 and Comparative Example 1. DETAILED DESCRIPTION OF THE INVENTION
[0013] The mold of the present invention comprises a substrate made of a conductive metal and a multilayer plating film having numerous pores formed thereon. The multilayer plating film is formed by forming a porous plating layer primarily composed of Ni on the substrate, and then forming a surface plating layer primarily composed of Ni, Co, W, Cr, Rh, Ru, Ir, or Pd on the porous plating layer. The average diameter of the pores formed in the multilayer plating film is 1 to 300 μm in area-weighted average value, the thickness of the porous plating layer is 1 to 500 μm, and the thickness of the surface plating layer is 0.01 to 150 μm. The mold exhibits excellent releasability for rubber molded articles and resin molded articles. Therefore, by using such a mold, numerous fine protrusions are formed on the surface, enabling the efficient production of rubber molded articles and resin molded articles having high water repellency.
[0014] The method for manufacturing the mold is not particularly limited, but may include a porous plating step of forming the porous plating layer in a plating solution containing Ni ions, and a surface plating step of forming the surface plating layer in a plating solution containing Ni ions, Co ions, W ions, Cr ions, Rh ions, Ru ions, Ir ions, or Pd ions, and the porous plating layer is formed by plating at 10 A / dm in a solution containing 0.01 to 1 mol / L of Ni ions and having a pH of 6 or more. 2 A method of forming the layer by electroplating at a cathode current density of the above or similar is preferred.
[0015] The substrate used in the present invention may be made of any conductive metal, and the material is not particularly limited. Examples of suitable metals include Fe, Al, Cu, and alloys containing these as the main component, with Fe and alloys containing Fe as the main component being preferred. Examples of alloys containing Fe as the main component include stainless steel, alloy tool steel (SKD material, etc.), structural carbon steel (SCM material, etc.), and aging-treated steel (maraging steel, etc.). In the present invention, "mainly composed" means that the material is contained in an amount of 50% by mass or more. The shape of the substrate is not particularly limited and may be appropriately determined depending on the molded product.
[0016] The substrate used in the present invention may be a multilayer structure. In this case, the surface on which the multilayer plating film is formed, i.e., the surface layer, is required to be a layer made of a conductive metal, and the other layers may be layers made of a conductive metal, or layers made of a nonmetallic material such as ceramics or resin, or layers made of a semi-metallic material with low conductivity such as silicon. The semi-metallic material here refers to a material that exhibits a certain degree of conductivity but is not conductive enough to be subjected to conventional electroplating. The surface layer made of a conductive metal of the multilayer structure may be formed by a common method used before electroplating a non-metallic material, such as electroless Ni plating to form a plating layer mainly composed of Ni.
[0017] In the porous plating step, a porous plating layer containing Ni as a main component is formed on the substrate made of the conductive metal in a plating solution containing Ni ions. The plating solution used to form the porous plating layer preferably contains 0.01 to 1 mol / L of Ni ions. If the Ni ion content is less than 0.01 mol / L, the strength of the porous plating layer may be reduced. The Ni ion content is more preferably 0.05 mol / L or more, and even more preferably 0.08 mol / L or more. On the other hand, if the Ni ion content exceeds 1 mol / L, it may be impossible to form a porous plating layer on the substrate. The Ni ion content is more preferably 0.8 mol / L or less, and even more preferably 0.5 mol / L or less. In this case, the plating solution may contain metal ions other than Ni ions as long as the effects of the present invention are not impaired. However, it is preferable that the plating solution contains 0.01 to 1 mol / L of Ni ions and is substantially free of metal ions other than Ni ions. This is because if the plating solution contains metal ions other than Ni ions, the corrosion resistance of the resulting porous plating layer may be reduced. From this perspective, the Ni content in the porous plating layer is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more.
[0018] The pH of the plating solution is preferably 6 or higher. If the pH of the plating solution is less than 6, a uniform porous plating layer may not be formed. The pH of the plating solution is more preferably 7 or higher, even more preferably 7.5 or higher, and particularly preferably 8 or higher. On the other hand, there is no particular upper limit to the pH, and the pH is usually 14 or lower, preferably 12 or lower, and more preferably 9.5 or lower.
[0019] The method for adjusting the pH of the plating solution to the above range is not particularly limited, and examples thereof include adding ammonia; metal hydroxides such as sodium hydroxide; or metal carbonates such as sodium bicarbonate to the plating solution. As described above, it is undesirable for the plating solution to contain metal ions other than Ni ions. Using ammonia to adjust the pH can prevent the plating solution from containing metal ions other than Ni ions. From this perspective, it is preferable that the plating solution be a solution whose pH is adjusted to 6 or higher using ammonia. The ammonia referred to here does not include ammonia that has dissociated into ammonium ions. When adjusting the pH using ammonia, the method is not particularly limited, and examples include adding an aqueous ammonia solution to the plating solution or blowing ammonia gas into the plating solution.
[0020] In this case, the plating solution preferably contains 0.2 to 30 mol / L of ammonia. The ammonia content here refers to the value obtained by calculating the ammonia concentration per 1 L of plating solution from the number of moles of ammonia added to the plating solution. If the ammonia content is less than 0.2 mol / L, the pH of the plating solution may not reach 6 or higher. The ammonia content is more preferably 0.3 mol / L or higher, and even more preferably 0.5 mol / L or higher. On the other hand, if the ammonia content exceeds 30 mol / L, the production cost may increase and the working environment may deteriorate due to odor, making industrial implementation difficult. The ammonia content is more preferably 20 mol / L or lower, and even more preferably 10 mol / L or lower.
[0021] The plating solution preferably contains 0.2 to 10 mol / L of at least one ion selected from the group consisting of ammonium ions and alkali metal ions. If the content of the ions is less than 0.2 mol / L, the solution resistance of the plating solution increases, and the temperature of the plating solution rises in a short period of time when electroplating Ni at a high current density, which may make continuous production of plated products difficult. The content of the ions is more preferably 0.5 mol / L or more. On the other hand, if a plating solution containing more than 10 mol / L of the ions is to be obtained, a large amount of ammonium salt or alkali metal salt must be dissolved as an ion source of the ammonium ions and alkali metal ions, which may increase production costs. The content of the ions is more preferably 5 mol / L or less.
[0022] The type of counter anion for the Ni ion, ammonium ion, and alkali metal ion is not particularly limited. Examples of counter anions include halide ions such as chloride ions; sulfate ions; sulfamate ions; acetate ions; nitrate ions; and citrate ions. From the viewpoints of availability and low cost, the plating solution preferably contains, as the counter anion, at least one ion selected from the group consisting of chloride ions, sulfate ions, sulfamate ions, and acetate ions, and more preferably contains chloride ions and / or sulfate ions.
[0023] The cathode current density when electroplating the substrate is 10A / dm 2 Here, the cathode current density is the current value applied to the substrate (cathode) when electroplating Ni, expressed as the current density per 1 dm of the substrate. 2 This is the value converted to the current value per cathode current density of 10A / dm 2 If the cathode current density is less than 12 A / dm, it may be impossible to form a uniform porous plating layer. 2 On the other hand, there is no particular upper limit to the cathode current density, and the cathode current density is usually 1000 A / dm 2less than 500 A / dm 2 or less, more preferably 300 A / dm 2 The following is the result.
[0024] The plating time is not particularly limited and can be set appropriately so that the porous plating layer has the desired thickness. The temperature of the plating solution is also not particularly limited, but if the temperature is too high, there is a concern that the composition of the plating solution will change due to evaporation of the solvent, so the temperature is usually 50°C or less.
[0025] Furthermore, the method for forming the porous Ni plating layer described in WO 2015 / 060449 can also be used as the method for forming the porous plating layer.
[0026] The thickness of the porous plating layer thus formed must be 1 to 500 μm. If the thickness is less than 1 μm, the protrusions formed on the molded article obtained using the mold will be too short, resulting in insufficient water repellency, and the porous plating layer will become brittle and easily peel off from the substrate. The thickness of the porous plating layer is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. On the other hand, if the thickness of the porous plating layer exceeds 500 μm, the manufacturing cost will increase. The thickness of the porous Ni plating layer is preferably 300 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less. Here, the thickness of the porous plating layer means the thickness from the substrate surface to the protrusions of the porous plating layer, and is measured by the method described in the examples.
[0027] In the surface plating step, a surface plating layer containing Ni, Co, W, Cr, Rh, Ru, Ir, or Pd as a main component is formed on the porous plating layer in a plating solution containing Ni ions, Co ions, W ions, Cr ions, Rh ions, Ru ions, Ir ions, or Pd ions. Among these, a layer containing Ni or Cr as a main component is preferred. The content of Ni, Co, W, Cr, Rh, Ru, Ir, or Pd in the surface plating layer is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more.
[0028] The plating method for forming the surface plating layer is not particularly limited, and electroplating can be performed using a known electroplating bath. For example, plating baths used to form a surface plating layer mainly composed of Ni include Watts bath, Wood's bath, Ni sulfamate bath, and organic acid Ni bath; plating baths used to form a surface plating layer mainly composed of Cr include trivalent chromium plating baths such as oxalic acid bath, sulfate bath, and chloride bath, and hexavalent chromium plating baths such as Sargent bath, mixed catalyst bath, HEEF bath, and fluoride bath. The current density and plating time are appropriately set so that the surface plating layer has a desired thickness. Examples of surface plating layers formed by electroplating include surface plating layers whose main component is Ni, such as electrolytic Ni plating layers, electrolytic Ni-W alloy plating layers, electrolytic Ni-Co alloy plating layers, electrolytic Ni-Mn alloy plating layers, electrolytic Ni-Mo alloy plating layers, electrolytic Ni-Sn alloy plating layers, electrolytic Ni-Fe alloy plating layers, and PTFE (polytetrafluoroethylene) composite electrolytic Ni plating layers (electrolytic Ni plating with PTFE particles dispersed in it); surface plating layers whose main component is W, such as electrolytic W-Ni alloy plating layers; surface plating layers whose main component is Co, such as electrolytic Co-Ni alloy plating layers; surface plating layers whose main component is Cr, such as Cr plating layers and Cr-C alloy plating layers; and surface plating layers whose main component is Pd, such as Pd-Ni alloy plating layers.
[0029] The surface plating layer may be formed by electroless plating. Examples of surface plating layers formed by electroless plating include electroless Ni plating layers, electroless Ni-P plating layers, electroless Ni-B plating layers, electroless Ni-WP plating layers, electroless Ni-WB plating layers, electroless Ni-Co-P plating layers, electroless Ni-Sn-P plating layers, and surface plating layers containing Ni as a main component, such as a PTFE composite electroless Ni plating layer (electroless Ni plating layer with PTFE particles dispersed therein).
[0030] The thickness of the surface plating layer thus formed must be 0.01 to 150 μm. If the thickness of the surface plating layer is less than 0.01 μm, the multilayer plating film will easily peel off from the substrate, and the releasability of rubber molded products and resin molded products will be insufficient. The thickness of the surface plating layer is preferably 0.1 μm or more, more preferably 0.5 μm or more. On the other hand, if the surface plating layer is too thick, the manufacturing cost will increase. The thickness of the surface plating layer is preferably 120 μm or less, more preferably 80 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and particularly preferably 20 μm or less. In the present invention, the thickness of the surface plating layer refers to the thickness calculated by dividing the weight of the deposit containing Ni, Co, W, Cr, Rh, Ru, Ir, Pd, or the like deposited by the surface plating treatment by the density of the deposit and the plating area, and is measured by the method (gravimetric method) described in the examples. Here, the plating area does not take into account the surface irregularities.
[0031] In order to obtain a reinforcing effect for the multilayer plating film and further improve the releasability of rubber molded products and resin molded products, it is preferable to form an intermediate plating layer mainly composed of Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir, or Ru between the porous plating layer and the surface plating layer. That is, the multilayer plating film is preferably formed by forming the porous plating layer on the substrate, forming an intermediate plating layer mainly composed of Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir, or Ru on the porous plating layer, and then forming the surface plating layer on the intermediate plating layer. Even if pores less than 1 μm in diameter remain in the porous plating layer, protrusions that contribute to the water repellency of rubber molded products and resin molded products are not formed. Forming the intermediate plating layer is thought to further improve releasability without reducing water repellency because the pores are filled with precipitates. Among these, a layer mainly composed of Cu is preferred as the intermediate plating layer. The content of Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir, or Ru in the intermediate plating layer is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more. The intermediate plating layer may be a single layer or a multilayer. An example of the latter is a multilayer plating film formed by forming a first intermediate plating layer mainly composed of Cu on the porous plating layer, forming a second intermediate plating layer mainly composed of Ni on the first intermediate plating layer, and forming a top plating layer mainly composed of Cr on the second intermediate plating layer. Forming such a second intermediate plating layer suppresses Cu elution from the first intermediate plating layer due to the strongly acidic chromium plating solution (Sargent bath) used to form the top plating layer.
[0032] After the porous plating step and before the surface plating step, an intermediate plating step can be performed in which an intermediate plating layer containing Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir, or Ru as a primary component is formed on the porous plating layer in a plating solution containing Cu ions, Sn ions, Zn ions, Co ions, Fe ions, Pd ions, Ni ions, Ir ions, or Ru ions. The plating method used to form the intermediate plating layer is not particularly limited, and electroplating can be performed using a known electroplating bath. For example, plating baths used to form an intermediate plating layer containing Cu as a primary component include a Cu sulfate bath and a Cu pyrophosphate bath, with a Cu sulfate bath being preferred. Plating baths used to form an intermediate plating layer containing Ni as a primary component include those described above as being used to form the surface plating layer. The current density and plating time are appropriately set so that the intermediate plating layer has the desired film thickness. The intermediate plating layer may also be formed by electroless plating.
[0033] The thickness of the intermediate plating layer thus formed (total thickness if the intermediate plating layer is multilayered) is 0.01 to 150 μm. If the thickness of the intermediate plating layer is less than 0.01 μm, the multilayer plating film will easily peel off from the substrate, and the releasability of rubber molded products and resin molded products will be insufficient. The thickness of the intermediate plating layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 3 μm or more, even more preferably 5 μm or more, and particularly preferably 7 μm or more. On the other hand, a thick surface plating layer increases manufacturing costs. The thickness of the intermediate plating layer is preferably 120 μm or less, more preferably 80 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and particularly preferably 20 μm or less. In the present invention, the thickness of the intermediate plating layer refers to the thickness calculated by dividing the weight of the deposit containing Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir, Ru, etc., deposited by the intermediate plating process by the density of the deposit and the plating area, and is measured by the method (gravimetric method) described in the examples. Here, the plating area does not take into account the surface irregularities.
[0034] The multilayer plating film may be formed by forming only the porous plating layer, the intermediate plating layer, and the top plating layer, or may further include layers other than these layers as long as the effects of the present invention are not impaired. Examples of the other layers include an undercoat plating layer (e.g., an electroless Ni plating layer) formed between the substrate and the porous plating layer.
[0035] Specific layer configurations of the multilayer plating film include: Porous plating layer / Cu electroplating layer (first intermediate) / Ni electroplating layer (second intermediate) / Cr electroplating layer (surface) Porous plating layer / Cu electroplating layer (middle) / Ni electroplating layer (surface) Porous plating layer / electro Cu plating layer (middle) / electroless Ni plating layer (surface) Porous plating layer / Cr plating layer (surface), Porous plating layer / PTFE composite electroless Ni plating (surface), etc.
[0036] The thickness of the multilayer plating film thus obtained is preferably 10 to 1000 μm. If the thickness is less than 10 μm, the protrusions formed on the molded product obtained using the mold may be too short, resulting in insufficient water repellency, or the porous plating layer may become brittle and easily peel off from the substrate. The thickness of the multilayer plating film is more preferably 20 μm or more, even more preferably 30 μm or more, even more preferably 40 μm or more, and particularly preferably 50 μm or more. On the other hand, if the thickness of the multilayer plating film exceeds 1000 μm, the multilayer plating film becomes brittle and the production cost increases. The thickness of the multilayer plating film is more preferably 500 μm or less, even more preferably 300 μm or less, and particularly preferably 150 μm or less. Here, the thickness of the multilayer plating film refers to the thickness from the substrate surface to the protrusions of the multilayer plating film.
[0037] The average diameter of the pores formed in the multilayer plating film must be 1 to 300 μm in area-weighted average value. If the average diameter of the pores is less than 1 μm, protrusions will not be formed on the resulting rubber or resin molded product, resulting in insufficient water repellency. The average diameter of the pores is preferably 5 μm or more, more preferably 10 μm or more. On the other hand, if the average diameter of the pores exceeds 300 μm, the resulting rubber or resin molded product will have insufficient water repellency and the strength of the multilayer plating film will be reduced. The average diameter of the pores is preferably 200 μm or less, more preferably 150 μm or less. Here, the average diameter of the pores is obtained by selecting multiple pores from a laser microscope photograph of the surface of the plated product, measuring the diameters of the pores, and calculating the area-weighted average. If the pores are not circular, the equivalent circle diameter is used as the diameter.
[0038] The depth of the pores formed in the multilayer plating film is preferably 1 to 200 μm. By having the pore depth in this range, the water repellency of the resulting molded article is further improved. The depth is more preferably 5 μm or more, and even more preferably 10 μm or more. The pore depth is measured by the method described in the Examples.
[0039] The spacing between holes formed in the multilayer plating film is preferably 0.1 to 1000 μm. By having the spacing within this range, the water repellency of the resulting molded article is further improved. The spacing is more preferably 1 μm or more, even more preferably 3 μm or more, and particularly preferably 5 μm or more. On the other hand, the spacing is more preferably 500 μm or less, even more preferably 300 μm or less, and particularly preferably 200 μm or less. The spacing between holes here refers to the distance between the central axes of two adjacent holes. The spacing between holes is measured by the method described in the Examples.
[0040] The mold of the present invention, which has a multilayer plating film with many holes formed thereon, has excellent releasability for rubber molded articles and resin molded articles. By using such a mold, many fine protrusions are formed on the surface, and rubber molded articles and resin molded articles with high water repellency can be produced with good productivity.
[0041] A preferred embodiment of the mold is a method for producing a molded product having a large number of protrusions formed on the surface thereof by filling the mold with rubber or resin, curing or solidifying the rubber or resin, and then releasing the obtained molded product from the mold.
[0042] The rubber or resin material is not particularly limited, and examples of rubber include silicone rubber, ethylene-propylene-diene terpolymer rubber, acrylonitrile-butadiene copolymer rubber, chloroprene rubber, chlorosulfonated polyethylene rubber, ethylene-propylene copolymer rubber, acrylic rubber, hydrin rubber, styrene-butadiene copolymer rubber, isobutylene-isoprene copolymer rubber, natural rubber, isoprene rubber, butadiene rubber, urethane rubber, and fluorine-based rubber. Examples of resins include epoxy resins; polyurethanes; polyamides such as nylon 6 and nylon 66; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyolefins such as polyethylene and polypropylene; polyacetal; acrylic resins such as polymethyl methacrylate; polycarbonate; polyvinyl chloride; styrene-based resins such as polystyrene and ABS; fluoropolymers; polyphenylene sulfide; polyether ether ketone; polyphenylene ether; polysulfone; polyethersulfone; polyimide; polyetherimide; thermoplastic elastomers such as olefin-based thermoplastic elastomers, urethane-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers.
[0043] The mold is filled with the rubber or resin material and then cured or solidified. The curing or solidification method is not particularly limited and may be selected appropriately depending on the type of material. For example, when silicone rubber is used as the material, a method is employed in which the silicone rubber (main component) and a curing agent are mixed, the resulting mixture is filled into the mold, and then heated. The resulting cured product is released from the mold to obtain a molded product having numerous protrusions formed on its surface. When the mold of the present invention is used, the molded product obtained by curing or solidification can be easily released from the mold, and the molded product having numerous protrusions formed on its surface has high water repellency. Such molded products are used for a variety of purposes, such as gloves, cooking utensils, leisure goods, sporting goods, and automobiles. [Example]
[0044] The present invention will be explained in more detail below using examples.
[0045] Example 1 (Preparation of porous Ni plating solution) A porous Ni plating solution with a pH of 8.5 was prepared by adding 28 mass% ammonia water to an aqueous solution obtained by dissolving NiCl2·6H2O (0.1 mol / L) and (NH4)2SO4 (2.0 mol / L) in ion-exchanged water.
[0046] (Preparation of intermediate layer Cu plating solution) The intermediate layer Cu plating solution was prepared by adding H2SO4 (210 g / L), 36 mass% HCl (0.2 ml / 1 L of water), CuSO4·5H2O (150 g / L), and JCU additives "CU-BRITE21MU" (5 ml / L) and "STB" (0.5 ml / L) to ion-exchanged water.
[0047] (Preparation of surface layer Ni plating solution) The surface layer Ni plating solution was prepared by adding NiSO4·6H2O (240 g / L), NiCl2·6H2O (45 g / L), and H3BO3 (30 g / L) to ion-exchanged water.
[0048] (Pretreatment) A rectangular steel plate measuring 120 mm in length, 70 mm in width, and 3 mm in thickness was used as the substrate. The substrate was immersed in a 50°C aqueous solution containing an electrolytic degreaser "Pakuna THE-210" (50 g / L) manufactured by Yuken Industry Co., Ltd. and NaOH (3 g / L). The substrate was then used as a cathode, and a cathode current density of 5 A / dm 2 The substrate was degreased by passing an electric current through it for 60 seconds, then rinsed with running water and then with pure water. The degreased substrate was activated by immersing it for 30 seconds in a 50°C treatment solution obtained by adding activator "V-34C" manufactured by JCU Corporation (70 ml / 1 L of water) and 36 mass% hydrochloric acid (70 ml / 1 L of water) to ion-exchanged water, then rinsed with running water and then with pure water. The activated substrate was immersed for 60 seconds in a 20°C cleaning solution obtained by adding 36 mass% hydrochloric acid (100 ml / 1 L of water) to ion-exchanged water to remove the oxide film, and then rinsed with pure water.
[0049] (Formation of porous plating layer) The pretreated substrate was immersed in a porous Ni plating solution at 20°C. Then, the cathode current density was 15 A / dm 2 The porous Ni plating treatment was carried out at 80°C for 70 minutes, and then the substrate was washed with pure water. The porous Ni-plated substrate was degassed by immersing it in pure water at 80°C until no more bubbles were generated. The cross section of the porous plating layer was observed under an electron microscope, and its thickness was measured. Measurements were taken at three locations, and the average value was taken as the thickness of the porous plating layer. The results are shown in Table 1.
[0050] (Formation of intermediate plating layer) The substrate on which the porous plating layer was formed was immersed in an intermediate layer Cu plating solution at 20°C. Then, the plating solution was heated at a cathode current density of 2 A / dm 2 The Cu intermediate layer was plated at 80°C for 20 minutes, and then rinsed with pure water. The Cu intermediate layer-plated substrate was degassed by immersing it in pure water at 80°C until no more bubbles appeared. The thickness A (μm) of the intermediate plating layer was measured by gravimetric method using the following formula. The results are shown in Table 1. A = (10000 × B) / (C × D) B: Weight (g) of the deposit attached to the substrate by plating C: Plating area (cm 2 ) D: 8.94 g / cm 3 (Density of Cu at 20℃)
[0051] (Formation of surface plating layer) The substrate on which the intermediate plating layer was formed was immersed in a surface layer Ni plating solution at 60°C. Then, the cathode current density was 2 A / dm 2 The surface layer was Ni-plated for 5 minutes at 20°C, and then washed with pure water. The Ni-plated substrate was then dried by blowing air onto it. The thickness of the surface plating layer was defined as D, and the density of Ni at 20°C was 8.91 g / cm. 3 The results are shown in Table 1.
[0052] (Evaluation of multilayer plating film) (1) Surface observation The surface of the multilayer plating film on the resulting mold was photographed using a Keyence VHX-6000 optical microscope, and an optical microscope image was obtained. The obtained optical microscope image is shown in Figure 1.
[0053] (2) Hole diameter, hole depth, and hole spacing Several holes were selected from the optical microscope image of the surface of the obtained multilayer plating film, and the diameters of these holes were measured and calculated as the area-weighted average. If the holes were not circular, the equivalent circular diameter was used as the diameter. The hole depth was measured using an Olympus 3D measuring laser microscope "OLS5100". Measurements were taken at three locations, and the average value was used as the hole depth. The hole spacing was also measured using the same laser microscope. Measurements were taken at three locations, and the average value was used as the hole spacing. The results are shown in Table 1.
[0054] (Preparation of silicone rubber sheet) The multilayer plating film-formed surface of the resulting mold was sprayed with Ichinen Chemicals' "Lubricant Spray EX" mold release agent, and an aluminum upper mold with a recess measuring 20 mm wide, 60 mm long, and 1 mm deep was then secured in place with clips. Ten parts by weight of Shin-Etsu Chemical's "KE106" silicone rubber (base compound) and one part by weight of Shin-Etsu Chemical's "CAT-RG" curing agent were mixed and the mixture was filled into the cavity between the mold with the multilayer plating film and the upper mold. The mold filled with the mixture was placed in a vacuum chamber (pressure 0.06 MPa) for five minutes, then removed from the chamber and placed in air for another five minutes to remove any bubbles. The mold filled with the mixture was then heat-treated in a 100°C oven for 30 minutes. After removing the mold from the oven and cooling in air for five minutes, the upper mold was removed and the silicone rubber sheet was peeled off from the multilayer plating film. The mold releasability was evaluated according to the following criteria. The results are shown in Table 1. A The entire sheet was easy to peel off, and the multi-layer plating film was not attached to the peeled surface of the sheet. B The periphery of the sheet was a little difficult to peel off, but the multi-layer plating film was not attached to the peeled surface of the sheet. C The peripheral part of the sheet was difficult to peel off, but the multi-layer plating film was not attached to the peeled surface of the sheet. D The periphery of the sheet was difficult to peel off, and the other areas were also somewhat difficult to peel off. A microscope confirmed that a small amount of the multi-layer plating film was still attached to the peeled surface of the sheet. E The entire sheet was difficult to peel off, and it was visually confirmed that the multi-layer plating film was attached to the peeled surface of the sheet.
[0055] (Evaluation of silicone rubber sheets) Optical microscope images and laser microscope images of the obtained silicone rubber sheet surface (the surface peeled from the multilayer plating film) were obtained using a Keyence optical microscope "VHX-6000" and an Olympus 3D measuring laser microscope "OLS5100." The heights of the protrusions determined from the obtained optical microscope images, laser microscope images, and laser microscope images are shown in Figure 3 and Table 1. The condition of the obtained silicone rubber sheet surface (the surface peeled from the multilayer plating film) was evaluated according to the following criteria. A No foreign matter was found B: A slight adhesion of multi-layer plating film was confirmed under a microscope. C The adhesion of a multi-layer plating film was confirmed under a microscope. D Multi-layer plating film adhesion was visually confirmed
[0056] Water was dropped onto the resulting silicone rubber sheet, and the water repellency was evaluated visually according to the following criteria. A: Water dripped onto a silicone rubber sheet formed droplets and slid down when exposed to wind. B: Water dripped onto the part of the silicone rubber sheet where the multi-layer plating film was attached adhered, and was not removed even when blasted with air.
[0057] Using the same mold, the same method was used to produce silicone rubber sheets five more times. For the fifth time, a sheet was produced without applying a release agent. Laser microscope images of the resulting sheets and the height of the protrusions are shown in Figure 3 and Table 1.
[0058] (Evaluation of multi-layer plating film after peeling) Using the optical microscope, the surface of the multilayer plating film on the mold after five silicone rubber sheet production runs was photographed to obtain an optical microscope image. The optical microscope image obtained is shown in Figure 1. The condition of the multilayer plating film surface at this time was evaluated according to the following criteria. A No foreign matter was found B: A slight foreign object was detected C Foreign matter was found D Peeling of the plating layer and adhesion of the silicone rubber sheet were confirmed.
[0059] Examples 2 and 3 Except for changing the current application time during formation of the underlying plating layer to 15 minutes (Example 2) or 5 minutes (Example 3), molds were prepared and evaluated, and silicone rubber molded articles were prepared and evaluated using the obtained molds in the same manner as in Example 1. The results are shown in Table 1 and Figures 1 and 3.
[0060] Example 4 Except for not forming an underlying plating layer, a mold was prepared and evaluated, and a silicone rubber molded product was prepared and evaluated using the obtained mold in the same manner as in Example 1. The results are shown in Table 1 and Figures 1 and 3.
[0061] Example 5 (Preparation of surface layer Cr plating solution) A surface layer Cr plating solution was prepared by adding chromic anhydride (250 g / L) and H2SO4 (2.5 ml / L) to ion-exchanged water.
[0062] The same procedures as in Example 1 were carried out up to the "forming of a porous plating layer" step, except that the current application time for forming the porous plating layer was changed to 90 minutes. Then, the substrate on which the porous plating layer had been formed was immersed in a surface layer Cr plating solution at room temperature. Then, the cathode current density was 30 A / dm 2 The surface layer was Cr-plated for 3 minutes at 80°C, and then washed with pure water. The Cr-plated substrate was degassed by immersing it in 80°C pure water until no more bubbles appeared. The mold thus obtained was evaluated, and silicone rubber molded products were produced and evaluated using the mold. The results are shown in Table 1, Figures 2 and 4. The thickness of the surface plating layer was determined as D, where D is the density of Cr at 20°C, which is 7.19 g / cm. 3 The weight was measured by the gravimetric method in the same manner as in Example 1, except that the following was used. The results are shown in Table 1.
[0063] Example 6 The substrate was changed to a rectangular iron plate with a length of 67 mm, a width of 50 mm, and a thickness of 0.3 mm, and the cathode current density during porous Ni plating was changed to 20 A / dm 2The current application time was changed to 20 minutes, the porous Ni-plated substrate was immersed in pure water at room temperature and ultrasonically cleaned instead of being degassed by immersing it in pure water, and the cathode current density during the intermediate Cu plating treatment was changed to 3 A / dm 2 The current application time was changed to 8 minutes, the substrate with intermediate Cu plating treatment was immersed in pure water at room temperature and ultrasonically cleaned instead of being degassed by immersing it in pure water, and the cathode current density during surface Ni plating treatment was changed to 4 A / dm 2 Except for changing the energization time to 3 minutes, the mold was manufactured, the thickness of each plating layer was measured, and the multilayer plating film was evaluated in the same manner as in Example 1. The results are shown in Table 1 and Figures 2 and 4.
[0064] (Preparation of polypropylene sheets) The mold thus obtained was placed on a hot plate at 200°C with the surface on which the multilayer plating film was formed facing up. A rectangular polypropylene sheet measuring 40 mm in length, 20 mm in width, and 0.3 mm in thickness was placed on the mold and left for 2 minutes. A rectangular stainless steel plate measuring 67 mm in length, 100 mm in width, and 0.3 mm in thickness was pressed from above on the polypropylene sheet for approximately 10 seconds. After confirming that there were no air pockets between the mold and the polypropylene sheet (if any were found, pressing was continued until they disappeared), the mold with the polypropylene sheet adhered to it was removed from the hot plate and cooled in the air (room temperature). During cooling, a portion of the polypropylene sheet peeled off from the mold. After the mold was cooled to room temperature, the portion of the polypropylene sheet adhering to the mold was peeled off. The mold releasability at this time was evaluated using the same criteria as for the silicone rubber sheet. The peeled polypropylene sheet was evaluated in the same way as the silicone rubber sheet. The peeled multilayer plating film was also evaluated in the same way as in Example 1. The results are shown in Table 1.
[0065] Comparative Example 1 Except for not forming a surface plating layer or an intermediate plating layer, a mold was prepared and evaluated, and a silicone rubber molded product was prepared and evaluated using the obtained mold in the same manner as in Example 1. The results are shown in Table 1 and Figures 2 and 4.
[0066] [Table 1]
[0067] When the molds of Examples 1 to 3 and 6, in which a porous plating layer, an intermediate plating layer and a surface plating layer were formed, were used, the resulting silicone rubber sheet or polypropylene sheet exhibited good releasability. The thicker the intermediate plating layer, the easier it was to peel the molded product (silicone rubber sheet). When the mold of Example 1, which had the thickest intermediate plating layer, was used, peeling was extremely easy. When the mold of Example 3, in which the intermediate plating layer was the thinnest, was used, microscopic images confirmed that a small amount of multilayer plating film had adhered to the peeled sheet, and optical microscopic images confirmed that foreign matter had also adhered to the mold surface. When the molds of Examples 1, 2 and 6, in which the intermediate plating layer was thick, were used, no adhesion of the multilayer plating film to the silicone rubber sheet or polypropylene sheet or foreign matter to the mold surface was confirmed.
[0068] When the mold of Example 4 or 5, on which a porous plating layer and a surface plating layer were formed, was used, the releasability of the resulting silicone rubber molded article was good, although it was inferior to the molds of Examples 1 to 3. When the mold of Example 4 was used, the microscope image confirmed that a small amount of the multilayer plating film had adhered to the sheet, and the microscope image also confirmed that foreign matter had adhered to the mold surface after peeling, and the amount of adhered matter was greater than when the mold of Example 3 was used.
[0069] On the other hand, when the mold of Comparative Example 1, on which only a porous plating layer was formed, was used, it was difficult to peel off the obtained silicone rubber, and it was confirmed that the porous plating film was adhered to the sheet. Furthermore, it was confirmed visually that the porous plating on the mold had peeled off, and a microscope image confirmed that the silicone rubber sheet was adhered to the surface of the mold.
[0070] When water was applied to the surface of the resulting silicone rubber or polypropylene sheet on which the protrusions were formed (the surface peeled from the multilayer plating film) and the water repellency was visually confirmed, the molded articles obtained using the molds of Examples 1 to 6 had good water repellency, whereas the molded article obtained using the mold of Comparative Example 1 had insufficient water repellency, with water remaining in the areas where the plating film was attached. Furthermore, no significant change in the height of the protrusions was observed even when molded articles were repeatedly produced using the molds of Examples 1 to 6. In particular, when the molds of Examples 1 and 6 were used, the molded articles could be easily peeled off without applying a release agent, and no deposits were observed on the sheet or mold. On the other hand, when the mold of Comparative Example 1 was used, the height of the protrusions significantly decreased with repeated production of the silicone rubber sheet, making it difficult to form the protrusions.
Claims
1. A mold in which a multilayer plating film having a large number of holes is formed on a base material made of a conductive metal, The multilayer plating film is formed by forming a porous plating layer mainly composed of Ni on the base material, and then forming a surface plating layer mainly composed of Ni, Co, W, Cr, Rh, Ru, Ir or Pd on the porous plating layer, The average diameter of holes formed in the multilayer plating film is 1 to 300 μm in terms of area weighted average value, and The mold, wherein the porous plating layer has a thickness of 1 to 500 μm, and the surface plating layer has a thickness of 0.01 to 150 μm.
2. The mold according to claim 1, wherein the multilayer plating film is formed by forming the porous plating layer mainly composed of Ni on the base material, forming an intermediate plating layer mainly composed of Cu, Sn, Zn, Co, Fe, Pd, Ni, Ir or Ru on the porous plating layer, and forming a surface plating layer mainly composed of Ni, Co, W, Cr, Rh, Ru, Ir or Pd on the intermediate plating layer, and the thickness of the intermediate plating layer is 0.01 to 150 μm.
3. A method for manufacturing a mold according to claim 1 or 2, comprising the steps of: a porous plating step of forming the porous plating layer in a plating solution containing Ni ions; and a surface plating step of forming the surface plating layer in a plating solution containing Ni ions, Co ions, W ions, Cr ions, Rh ions, Ru ions, Ir ions or Pd ions, The porous plating layer is subjected to a current of 10 A / dm in a solution containing Ni ions at 0.01 to 1 mol / L and having a pH of 6 or more. 2 The method for manufacturing a mold includes electroplating at a cathode current density of 100 to 1500 nm or more.
4. 3. A method for producing a molded article having a large number of protrusions formed on its surface, comprising filling the mold according to claim 1 or 2 with rubber or resin, curing or solidifying the rubber or resin, and then releasing the obtained molded article from the mold.
Citation Information
Patent Citations
Sheet material, glove, hand mold for manufacturing glove, and manufacturing method of glove