Semiconductor device
By using polycrystalline In-M-Zn oxide powders to form a sputtering target for oxide semiconductor films with a homologous structure, the issues of low crystallinity and defects are addressed, resulting in improved electrical stability and reliability of semiconductor devices.
Patent Information
- Application Number
- JP2024129840
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2013-02-28
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Oxide semiconductor films used in transistors often have low crystallinity, leading to defects such as oxygen vacancies and dangling bonds, which result in changes in electrical characteristics and increased fluctuations in threshold voltage due to differences in crystallinity between stacked films and the presence of defects and hydrogen, affecting the reliability and stability of the transistors.
The use of polycrystalline In-M-Zn oxide powders, where M is aluminum, titanium, gallium, yttrium, zirconium, lanthanum, cesium, neodymium, or hafnium, is mixed with zinc oxide to form a sputtering target, which is then processed to create an oxide semiconductor film with a homologous structure and high crystallinity, reducing defects and improving electrical characteristics.
This method allows for the formation of an oxide semiconductor film with reduced defects, enhancing the electrical performance and reliability of semiconductor devices by stabilizing the threshold voltage and reducing fluctuations in electrical characteristics.
Smart Images

Figure 2024152760000001_ABST
Abstract
Description
[Technical field]
[0001] Method for manufacturing sputtering target, method for forming oxide film, and transistor do. [Background technology]
[0002] It is used in many flat panel displays, such as liquid crystal displays and light-emitting displays. The transistors used are amorphous silicon and single crystal silicon formed on a glass substrate. The silicon semiconductor is made of silicon semiconductor such as polycrystalline silicon or polysilicon. Transistors using semiconductors are also used in integrated circuits (ICs).
[0003] In recent years, metal oxides that exhibit semiconducting properties have been used in transistors instead of silicon semiconductors. In this specification, the term "oxide" refers to a metal oxide that exhibits semiconductor properties. Let us call them semiconductors.
[0004] For example, as an oxide semiconductor, InGaO3(ZnO) having a homologous phase m (m: Natural numbers) are known (see Non-Patent Documents 1 and 2).
[0005] In addition, Patent Document 1 describes a homologous compound InMO3(ZnO) m (M=In, Fe, Transparent thin-film field-effect transistor using Ga, Al, m = an integer of 1 or more and less than 50 The data is disclosed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-103957 A [Non-patent literature]
[0007] [Non-Patent Document 1] M. Nakamura, N. Kimizuka, and T. Mohri, “The Phase Relations in the In2O3-Ga2ZnO4-ZnO System at 1350℃”, J. Solid State Chem., 1991, Vol.93, p.298-315 [Non-Patent Document 2] Masaki Nakamura, Noboru Kimizuka, Takahiko Mouri, Mitsumasa Isobe, "Synthesis and crystal structure of homologous phase, InFeO3(ZnO)m (m: natural number) and its isomorphic compounds", Solid State Physics, 1993, Vol.28, No.5, pp.317-327 Summary of the Invention [Problem to be solved by the invention]
[0008] However, when the crystallinity of an oxide semiconductor film is low, oxygen vacancies and dung may occur in the oxide semiconductor film. It is prone to contain defects such as ring bonds.
[0009] In addition, when oxide semiconductor films are stacked using sputtering targets having different compositions, When the crystallinity of each oxide semiconductor film is different, the boundary between the stacked oxide semiconductor films may be Defects will occur on the surface.
[0010] The oxide semiconductor film is filled with hydrogen and other elements due to defects in the film or due to bonds between the defects and hydrogen or the like. This may cause a rear to occur, which may change the electrical characteristics of the oxide semiconductor film. This leads to poor electrical characteristics of the transistor, and also to deterioration over time and stress testing (e.g., BT( Bias-Temperature stress tests, optical BT stress tests, etc. This causes an increase in the amount of variation in the electrical characteristics of a transistor, typically the threshold voltage. .
[0011] In view of the above, one embodiment of the present invention provides a semiconductor device capable of forming an oxide semiconductor film with few defects. It is an object of the present invention to provide a method for producing a sputtering target. An object of one embodiment is to form an oxide semiconductor film with a small amount of defects. One embodiment of the present invention is a semiconductor device including an oxide semiconductor film, which is characterized in that the electrical characteristics of the semiconductor device are improved. Another object of one embodiment of the present invention is to provide a semiconductor device including an oxide semiconductor film. It is an object of the present invention to improve the reliability of the device. It is not necessary to solve all of these problems. [Means for solving the problem]
[0012] One aspect of the present invention is indium oxide, metal oxide (the metal is aluminum, titanium, gallium, etc. Sodium, yttrium, zirconium, lanthanum, cesium, neodymium, or hafnium In-M-Zn oxide (M is Aluminum, titanium, gallium, yttrium, zirconium, lanthanum, cesium, Neodymium or hafnium) powder to form polycrystalline In-M-Zn oxide powder and oxide mixing the mixture with zinc powder to form a mixture, molding the mixture to form a compact, and firing the compact. The present invention relates to a method for producing a sputtering target.
[0013] In the above sputtering target, M (M is aluminum, titanium, gallium) Sodium, yttrium, zirconium, lanthanum, cesium, neodymium, or hafnium The zinc composition is greater than that of the other metals.
[0014] In addition, the polycrystalline In-M-Zn oxide powder used to manufacture the sputtering target is It is a morogus compound.
[0015] In addition, one embodiment of the present invention is a method for manufacturing a semiconductor device using indium, M (M is aluminum, titanium, gallium, yttrium, zirconium, lanthanum, cesium, neodymium, or hafnium), and A sputtering target having a zinc content greater than M is used. By the annealing method, In-M-Zn oxide (M is aluminum, titanium, gallium, and yttrium) was depositing a thin film of Cr, Ti, H, Zr, Lanthanum, Cesium, Neodymium, or Hafnium A method for forming an oxide film.
[0016] In-M-Zn oxide (where M is aluminum, titanium, gallium, or yttrium) , zirconium, lanthanum, cesium, neodymium, or hafnium) have a homologous structure It has a structure.
[0017] In-M-Zn oxide (where M is aluminum, titanium, gallium, or yttrium) , zirconium, lanthanum, cesium, neodymium, or hafnium) are Z for M The atomic ratio of n is greater than 0.5.
[0018] In addition, one aspect of the present invention is the above-mentioned In-M-Zn oxide (M is aluminum, titanium, Gallium, yttrium, zirconium, lanthanum, cesium, neodymium, or hafnium A transistor having a gate insulating layer. Effect of the Invention
[0019] According to one embodiment of the present invention, a spatula capable of forming an oxide semiconductor film with few defects can be provided. According to one aspect of the present invention, a method for manufacturing a targeting target can be provided. In this way, an oxide semiconductor film with fewer defects can be formed. As a result, electrical characteristics of a semiconductor device including an oxide semiconductor film can be improved. According to one embodiment of the present invention, a semiconductor device including an oxide semiconductor film can be provided with high reliability. It is possible to improve the performance. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a diagram illustrating the crystal structure of a homologous compound. [Diagram 2] 1A to 1C are diagrams illustrating a manufacturing process of a sputtering target. [Diagram 3] 1A to 1C are diagrams illustrating a manufacturing process of a sputtering target. [Figure 4] Schematic diagrams illustrating a method for producing an oxide. [Diagram 5] FIG. 1 is a schematic diagram illustrating an oxide. [Figure 6] FIG. 2 is a schematic diagram illustrating sputtered particles. [Figure 7] FIG. 2 is a diagram illustrating the crystal structure of a homologous compound. [Figure 8] Schematic diagrams illustrating a method for producing an oxide. [Figure 9] FIG. 1 is a schematic diagram illustrating an oxide. [Figure 10] FIG. 1 shows nanobeam electron diffraction patterns of CAAC-OS and nc-OS. [Figure 11] FIG. 1 is a diagram illustrating the process of zinc oxide crystal growth. [Figure 12] FIG. 1 is a diagram illustrating the process of zinc oxide crystal growth. [Figure 13] FIG. 1 is a diagram illustrating the process of zinc oxide crystal growth. [Figure 14] Schematic diagrams illustrating a method for producing an oxide. [Figure 15]FIG. 1 is a schematic diagram illustrating an oxide. [Figure 16] Schematic diagrams illustrating a method for producing an oxide. [Figure 17] Schematic diagrams illustrating a method for producing an oxide. [Figure 18] Schematic diagrams illustrating a method for producing an oxide. [Figure 19] FIG. [Figure 20] FIG. [Figure 21] FIG. 2 is a diagram for explaining plasma discharge in a sputtering method using a DC power source and an AC power source. [Figure 22] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a transistor. [Diagram 23] FIG. 1 is a cross-sectional view illustrating one embodiment of a transistor. [Figure 24] FIG. 1 is a cross-sectional view illustrating one embodiment of a transistor. [Diagram 25] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a transistor. [Figure 26] FIG. 1 is a cross-sectional view illustrating one embodiment of a transistor. [Figure 27] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a transistor. [Figure 28] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a transistor. [Figure 29] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a transistor. [Diagram 30] 1A to 1C are cross-sectional views illustrating one mode of a method for manufacturing a transistor. [Diagram 31] 1A to 1C are cross-sectional views illustrating one mode of a method for manufacturing a transistor. [Diagram 32] FIG. 2 is a diagram showing the atomic ratio of an In--Ga--Zn oxide film obtained from the results of XPS analysis. [Diagram 33] X-ray diffraction measurement results of In-Ga-Zn oxide film. [Diagram 34] X-ray diffraction measurement results of In-Ga-Zn oxide film. [Diagram 35]X-ray diffraction measurement results of In-Ga-Zn oxide film. [Diagram 36] Ternary phase diagram of a sputtering target and an In-Ga-Zn oxide film. [Figure 37] Cross-sectional images of sample 2 and sample 3 observed by TEM. [Figure 38] Cross-sectional image observed by HAADF-STEM. [Figure 39] Band diagram of In-Ga-Zn oxide film. [Diagram 40] Band diagram of In-Ga-Zn oxide film. [Diagram 41] TEM cross-sectional images of Samples 11 to 13. [Diagram 42] TEM cross-sectional images of Samples 11 to 13. [Diagram 43] Cross-sectional images of sample 12 and sample 13 observed by TEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and the embodiments and aspects of the present invention may be modified without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various modifications may be made to the embodiments and details of the present invention. However, the present invention should not be construed as being limited to the description of the following embodiments and examples. In the following embodiments and examples, the same parts or parts having similar functions are In the case of parts, the same reference numerals or the same hatch patterns are used in common among different drawings, and the repetition The explanation of the repetition will be omitted.
[0022] In each figure described in this specification, the size, thickness, or area of each component is indicated by the following formula: The figures may be exaggerated for clarity and are not necessarily limited to scale. stomach.
[0023] In addition, the terms "first," "second," "third," etc., used in this specification are used interchangeably to avoid confusion of components. The number is added for convenience and is not intended to be a numerical limit. The terms can be replaced with "second" or "third" as appropriate for explanation.
[0024] The function of the "source" and "drain" is to change the direction of the current during circuit operation. For this reason, in this specification, the terms "sauce" and "dressing" are used interchangeably. The terms "in" and "in" may be used interchangeably.
[0025] Voltage is the potential difference between two points, and potential is the electrostatic field at a certain point. This refers to the electrostatic energy (electrical potential energy) possessed by a unit charge in a particle. Generally, the potential difference between a potential at a certain point and a reference potential (for example, ground potential) This is simply called potential or voltage, and potential and voltage are often used synonymously. Therefore, in this specification, unless otherwise specified, potential may be read as voltage. In this specification, voltage may be read as potential.
[0026] In this specification, when an etching process is performed after a photolithography process, After the etching process, the mask formed in the photolithography process is removed. .
[0027] (Embodiment 1) In this embodiment, a method for producing a sputtering target will be described.
[0028] <Homologous compounds and homologous structures> First, InMO3(ZnO) m(M is Al, Ti, Ga, Y, Zr, La, Cs, This section describes the homologous compounds represented by InM O3(ZnO) m The crystal structure of the homologous compound represented by - layer and (FeZn m )O m+1 1+ LuFeO3(Z nO) m When m is an odd number, it has the space group R-3m, and when m is an even number, it has the space group R-3m. The InMO3(ZnO) has the space group P63 / mmc. m (m=1) In this case, it is also called YbFe2O4 type. This type of crystal structure is called a homologous structure. In the present specification, the crystal structure is based on the hexagonal representation.
[0029] Next, InMO3(ZnO) m A representative example is InGaO3(ZnO) m Using Explain the crystal structure of molybdenum compounds. InGaO3(ZnO) m In m=1 (i.e. The crystal structure of InGaO3(ZnO)1) is shown in Figure 1(A), where m=2 (i.e., InGa The crystal structure of InGaO3(ZnO)2 is shown in Figure 1(B), where m=3 (i.e., InGaO3(Z The crystal structure of nO)3) is shown in Figure 1(C).
[0030] As shown in Figure 1, InMO3(ZnO) m The homologous compound represented by the formula The crystal structure has a plurality of repeating units u1 to u3 stacked together. Between the O2 layers, a layer having gallium atoms or / and zinc atoms and oxygen atoms (Zn O, GaO, and (Ga,Zn)O have a crystal structure with (m + 1) layers provided. Thus, such a structure is called a homologous structure. In addition, m even outside the homologous compound represented by InMO3(ZnO), it is possible to have a homologous structure.
[0031] <CAAC-OS film> Next, CAAC-OS (C Axis Aligned Crystalline O xide Semiconductor) will be described. Here, only the crystal structure of CAAC -OS will be described, and the details of CAAC-OS will be described in Embodiment 2.
[0032] CAAC-OS is an oxide semiconductor having CAAC (C Axis Aligned Crystal).
[0033] CAAC-OS may have, for example, a plurality of crystal parts, and in the plurality of crystal parts, the c-axes may be aligned in a direction parallel to the normal vector of the formation surface or the upper surface. Also, CAAC -OS may, for example, when analyzed by the out-of-plane method using an X-ray diffraction (XRD: X-Ray Diffraction) apparatus, show peaks identified as c-axis orientation, for example, peaks identified as plane orientation (00x). Also, CAAC-OS may, for example, have spots (bright spots) observed in an electron diffraction pattern. Also, CAAC-O S may, for example, have the directions of the a-axis and b-axis not aligned in different crystal parts.
[0034] The CAAC-OS film is observed by TEM from a direction substantially parallel to the sample surface (cross-sectional TEM observation). When the metal atoms are observed, it can be confirmed that they are arranged in layers in the crystal part. Each layer of the CAAC-OS film is formed on a surface on which the film is to be formed (also called a surface on which the film is to be formed) or on a concave surface on the upper surface. The shape reflects a convexity, and is aligned parallel to the surface on which the CAAC-OS film is formed or the upper surface.
[0035] On the other hand, the CAAC-OS film was observed by TEM from a direction roughly perpendicular to the sample surface (plane T EM observation reveals that metal atoms are arranged in triangular or hexagonal shapes in the crystals. However, no regularity was observed in the arrangement of metal atoms between different crystal regions. do not have.
[0036] In this specification, when simply referring to vertical, it means 80° or more and 100° or less, or 85° or less. The range of angles between 95° and 10° is also included. This also includes ranges of 10° or -5° to 5°.
[0037] In addition, in CAAC-OS, gallium atoms and / or zinc atoms are interposed between the InO2 layers. It has one or more layers containing ZnO, GaO, (Ga,Zn)O and oxygen atoms. In this case, it becomes a homologous structure.
[0038] <First method for producing sputtering target> Next, we developed a method for forming a homologous In-Ga-Zn oxide film using a spatula. The manufacturing method of the printing target will be described with reference to FIG. A method for manufacturing a sputtering target capable of depositing a CAAC-OS film having a structure This method will be explained with reference to FIG.
[0039] As shown in FIG. 2, in step S101, a raw material for In-Ga-Zn oxide is Indium oxide powder, gallium oxide powder, and zinc oxide powder are prepared, milled, and mixed. Indium oxide powder, gallium oxide powder, and zinc oxide powder are mixed together to form a mixture. stands for powders with a purity of 99.9%, 99.99%, or 99.999% or higher, respectively. As a result, the concentration of impurities in an oxide semiconductor film to be formed later can be reduced. Therefore, a transistor with excellent electrical characteristics can be manufactured.
[0040] Alternatively, as a raw material for In-Ga-Zn oxide, steps S111 to S114 in FIG. 3 described later may be used. Using the polycrystalline In-Ga-Zn oxide powder and zinc oxide powder prepared in step S113, Alternatively, the raw material of In-Ga-Zn oxide may be The polycrystalline In-Ga-Zn oxide powder and Ga-Zn n-oxide powder can be used.
[0041] The atomic ratio of Zn to Ga in the mixture is Ga <Znとなるように、In-Ga- Prepare Zn oxide raw material. For example, In:Ga:Zn=1:3:4, In:Ga:Z n=1:3:5, In:Ga:Zn=1:3:6, In:Ga:Zn=1:3:7, In :Ga:Zn=1:3:8, In:Ga:Zn=1:3:9, In:Ga:Zn=1:3 :10, In:Ga:Zn=1:4:5, In:Ga:Zn=1:4:6, In:Ga: Zn=1:4:7, In:Ga:Zn=1:4:8, In:Ga:Zn=1:4:9, I n:Ga:Zn=1:4:10, In:Ga:Zn=1:5:6, In:Ga:Zn=1 :5:7, In:Ga:Zn=1:5:8, In:Ga:Zn=1:5:9, In:Ga :Zn=1:5:10, In:Ga:Zn=1:6:7, In:Ga:Zn=1:6:8 , In:Ga:Zn=1:6:9, In:Ga:Zn=1:6:10 The raw material for the -Ga-Zn oxide powder is prepared. As a result, the homologous It is possible to manufacture a sputtering target containing In-Ga-Zn oxide with a lattice structure. do.
[0042] For grinding and mixing the raw materials of In-Ga-Zn oxide, ball mills, bead mills, roll mills, etc. are used. A mixer grinder such as a grinding mill, a jet mill, or an ultrasonic device can be used. By doing so, the raw material of In-Ga-Zn oxide is crushed to a specified particle size and mixed. It is possible.
[0043] The average particle size of the crushed In-Ga-Zn oxide raw material is 0.01μm to 3.0μm. It is preferable that the thickness is equal to or less than 0.1 μm or equal to or less than 2.0 μm.
[0044] Next, in step S102, the mixture is molded to form a molded body.
[0045] Methods for forming the compact include die molding and cold isostatic pressing. In the treatment, polyvinyl alcohol, methyl cellulose, polywax, olein, etc. A molding aid such as an acid may be used.
[0046] In step S101, the raw material of In-Ga-Zn oxide is mixed with water, a dispersing agent, and a binder. The mixture is mixed with the binder to form a slurry, and in step S102, the slurry is poured into a mold. The mold may be dried by sucking water from the bottom of the mold. The process involves natural drying followed by heat treatment at temperatures between 300 and 700°C to produce a compact. The moisture contained in the
[0047] Next, in step S103, the compact is sintered to form a sintered body.
[0048] In the firing process in step S103, the temperature is 1200° C. or more and 1600° C. or less. The mixture is heated to 1300°C or more and 1500°C or less. It is possible to form crystalline In-Ga-Zn oxide. In this case, the atomic ratio of Zn to Ga is Ga <Znとなる。
[0049] After this, the sintered body is heated in a reducing atmosphere such as hydrogen, methane, carbon monoxide, or nitrogen, rare gas, etc. As a result, the variation in resistance of the sintered body is reduced. It is possible.
[0050] In addition, step S102 (molding step) and step S103 (firing step) are performed simultaneously. In this way, a sputtering target can be manufactured. Examples of the methods include hot pressing and hot isostatic firing.
[0051] Next, in step S104, the sintered body is processed to manufacture a sputtering target. do.
[0052] In step S104, the sintered body is cut and processed to attach a backing plate, etc. The sintered body is cut and then mirror-finished to a surface roughness (Ra) of 5 μm. The mirror finish is mechanical polishing, chemical polishing, CM There are P etc.
[0053] Through the above steps, a sputtering target can be manufactured. The sputtering target produced by the method has an atomic ratio of Zn to Ga of Ga. <Znと By using such a sputtering target, It is possible to form an In-Ga-Zn oxide film with a homologous structure. and an In-Ga-Zn oxide film that is a CAAC-OS can be formed. .
[0054] <Second method for producing sputtering target> Here, InGaO3(ZnO) m It is possible to form a film of a homologous compound represented by the formula: A method for producing a sputtering target capable of producing a large amount of In is described with reference to FIG. GaO3(ZnO) m and forming a CAAC-OS film. A method for producing a sputtering target capable of forming a thin film will be described with reference to FIG. do.
[0055] As shown in FIG. 3, first, an In-Ga-Zn oxide powder is prepared.
[0056] In step S111, indium oxide, which is the raw material for the In-Ga-Zn oxide powder, is The powder, gallium oxide powder, and zinc oxide powder are mixed in an amount to form a mixture. The indium oxide powder, gallium oxide powder, and zinc oxide powder each have a purity of 9. Use powder with a purity of 9.9%, 99.99%, or 99.999% or higher. As a result, It is possible to reduce the concentration of impurities in an oxide semiconductor film that is formed later. It is possible to fabricate a transistor having the above electrical characteristics.
[0057] In the mixture, the atomic ratio of the metal elements is In:Ga:Zn=1:1:m (m is a natural number). The amounts of indium oxide powder, gallium oxide powder, and zinc oxide powder are adjusted so that As a result, in the firing process of step S112, InGaO3(Z nO) m A sputtering target containing an In-Ga-Zn oxide with a homologous structure represented by A get can be manufactured.
[0058] Next, in step S112, the mixture is sintered to obtain polycrystalline In-Ga-Zn oxide. Form.
[0059] The firing step can be performed in the same manner as the firing step shown in step S103 of FIG. This process allows the formation of polycrystalline In-Ga-Zn oxide. n-Ga-Zn oxide is InGaO3(ZnO) m There are homologous compounds represented by Representative examples are InGaZnO4, InGaZn2O5, InGaZn3O6, and InGaZ Examples include In4O7, InGaZn5O8, etc.
[0060] Next, in step S113, the polycrystalline In-Ga-Zn oxide is crushed to obtain polycrystalline Form In-Ga-Zn oxide powder.
[0061] The polycrystalline In-Ga-Zn oxide was ground using a ball mill, a bead mill, a roll mill, or a die mill. The grinding is carried out using a grinding method such as a mill or ultrasonic device.
[0062] The average particle size of the crushed polycrystalline In-Ga-Zn oxide powder is 0.01 μm or more and 3.0 It is preferable that the thickness is 0.1 μm or less, or 0.1 μm or more and 2.0 μm or less.
[0063] In addition, when the average particle size of the crushed polycrystalline In-Ga-Zn oxide powder is 3.0 μm or more, In this case, it is preferable to carry out the crushing step shown in step S113 again.
[0064] Next, the manufacturing process of the sputtering target will be described.
[0065] In step S114, the polycrystalline In-Ga-Zn oxide powder and the zinc oxide powder are mixed. In this mixing step, polycrystalline In-Ga-Zn The oxide powder and zinc oxide powder may be pulverized separately to improve the uniformity of the particle size of the powder.
[0066] Here, the polycrystalline In-, which is a homologous compound obtained in step S113, is The Ga-Zn oxide powder and the zinc oxide powder are mixed to form a mixture. The atomic ratio of Zn to Ga is (m+0.05) or more and (m+0.5) or less. Polycrystalline In-Ga-Zn oxide powder and zinc oxide powder are prepared. For example, In:Ga: Zn=1:1:1.05, In:Ga:Zn=1:1:2.05, In:Ga:Zn=1 Polycrystalline In-Ga-Zn oxide powder and zinc oxide powder were mixed at a ratio of 1:3.05. As a result, in the subsequent firing process in step S116, InGaO3(ZnO) m The sputtering reaction has a higher number of zinc atoms than the gallium atoms contained in the homologous compound represented by the formula: It is possible to manufacture a target.
[0067] Next, in step S115, the mixture is molded to form a molded body.
[0068] As a method of molding the mixture to form a molded body, it can be performed in the same manner as the molding process shown in step S102 of FIG. 2. This can be done in the same manner as the process shown in step S102 of FIG. 2.
[0069] Also, in step S114, water, a dispersant, and a binder are mixed with the polycrystalline In-Ga-Zn oxide powder and zinc oxide powder to form a slurry. In step S115, the slurry is poured into a mold, water is sucked from the bottom surface of the mold, and a drying process is performed, whereby a molded body may be formed. The drying process can remove the moisture contained in the molded body by performing natural drying and then performing a heat treatment at 300°C or higher and 700°C or lower. This can remove the moisture contained in the molded body by performing natural drying and then performing a heat treatment at 300°C or higher and 700°C or lower.
[0070] Next, in step S116, the molded body is sintered to form a sintered body.
[0071] In the firing process in step S116, the mixture is heated at 800°C or higher and 1600°C or lower, or 1300 °C or higher and 1500°C or lower. By this process, polycrystalline In- Ga-Zn oxide can be formed as a sintered body. In the polycrystalline In-Ga-Zn oxide, the atomic ratio of Zn to Ga is Ga < Zn. The polycrystalline In-Ga-Zn oxide is a mixed crystal of a homologous compound represented by In GaO3(ZnO) and ZnO. m It is a mixed crystal of a homologous compound represented by InGaO3(ZnO) and ZnO.
[0072] After that, the sintered body may be heat-treated in a reducing atmosphere such as hydrogen, methane, carbon monoxide, or an inert gas atmosphere such as nitrogen or a noble gas. As a result, the variation in the resistance of the sintered body can be reduced. This can reduce the variation in the resistance of the sintered body. This can reduce the variation in the resistance of the sintered body.
[0073] In addition, step S115 (molding step) and step S116 (firing step) are performed simultaneously. Such a molding method can be used to form a sintered body. Hot isostatic firing, etc.
[0074] Next, in step S117, the sintered body is processed to manufacture a sputtering target. do.
[0075] In step S117, the processing step shown in step S104 in FIG. 2 is appropriately used. It is possible.
[0076] Through the above steps, a sputtering target can be manufactured. The sputtering target produced is InGaO3(ZnO) m The homology represented by It is a mixed crystal of gas compounds and ZnO, and the ratio of Z to Ga in the sputtering target is The atomic ratio of n is (m+0.05) or more and (m+0.5) or less. The homologous compound In-Ga- Furthermore, a Zn oxide film can be formed. It is possible to form an In-Ga-Zn oxide film, which is an AC-OS.
[0077] (Embodiment 2) In this embodiment, an oxidation process using the sputtering target manufactured in the first embodiment is performed. The method for forming the In-M-Zn Representative examples of oxides (where M is Al, Ti, Ga, Y, Zr, La, Cs, Nd, or Hf) The following description will be given using In-Ga-Zn oxide.
[0078] 4, 8, 14, 16, 17, and 18 are diagrams showing sputtering in a film formation chamber of a film formation apparatus. In addition, in the present embodiment, a film forming chamber of the film forming apparatus is simply The details will be described in the third embodiment.
[0079] <Heated deposition (deposition temperature: 150℃ or higher, but less than 600℃)> As shown in FIG. 4A, a substrate stage 12 and a substrate holder 13 are disposed in a film forming chamber 11 of a film forming apparatus. The sputtering target 13 manufactured in the manner described above is provided facing the substrate. A substrate 121 is placed on the substrate 12 .
[0080] In the film-forming chamber 11, which has been depressurized, an inert gas such as argon or a sputtering gas such as oxygen is introduced. A voltage is applied to the sputtering target 13 to generate plasma 17. The sputtering gas is ionized in the plasma 17, generating ions 15. When the ions 15 collide with the ring target 13, the ions 15 are contained in the sputtering target 13. The interatomic bonds between the particles are broken, and the particles are peeled off from the sputtering target 13. Therefore, ions, sputtering particles, electrons, etc. exist in the plasma 17. The particles peeled off from the sputtering target are called sputtered particles.
[0081] The ions 15 may be, for example, positive oxygen ions. By using the ion beam, for example, plasma damage during film formation can be reduced. By using oxygen positive ions as the ions 15, for example, the ions 15 can be sputtered. The crystallinity of the sputtering target 13 when colliding with the surface of the target 13 In addition, the use of oxygen cations as the ions 15 can suppress the deterioration or amorphization. For example, when ions 15 collide with the surface of the sputtering target 13, In some cases, the crystallinity of the deposition target 13 can be improved. For example, the positive charge of rare gases (helium, neon, argon, krypton, xenon, etc.) Ions may also be used.
[0082] Sputtering particles include zinc particles, oxygen particles, zinc oxide particles, and In-Ga-Zn. The sputtering target produced in the first embodiment has a higher content of Ga than that of Ga oxide particles. For this reason, in this embodiment, zinc particles, After oxygen particles or zinc oxide particles are preferentially peeled off, zinc particles, oxygen particles, zinc oxide particles This will be explained using a model in which In-Ga-Zn oxide particles peel off.
[0083] First, zinc particles 123a and oxygen particles 123b are sputtered as sputtering particles. The zinc particles 123a and the oxygen particles 123b are then peeled off from the plating target 13. By moving onto the substrate 121, the hexagonal crystal grains 123c formed of zinc oxide are formed on the substrate. is formed.
[0084] FIG. 5(A) shows a model of the top surface shape of a hexagonal crystal grain 123c formed of zinc oxide. As shown in Figure 5(A), the hexagonal crystal grain 123c formed in zinc oxide is composed of Zn atoms. The electron and O atoms are bonded in a hexagonal shape.
[0085] As described later in the section "Crystal Growth Mechanism of Zinc Oxide," zinc oxide grows parallel to the ab plane. Since the crystal growth is fast, when the substrate temperature is between 150°C and 600°C, the film is formed of zinc oxide. The hexagonal crystal grains 123c are aligned in a direction parallel to the surface of the substrate 121, that is, in a direction parallel to the cross section of the zinc oxide film. As a result, the crystal grows laterally on the surface of the hexagonal crystal, as shown in FIG. A zinc film 125 is formed. That is, the hexagonal zinc oxide film 125 has a single crystal region. The hexagonal zinc oxide film 125 may include regions that are not single crystal regions.
[0086] FIG. 5B shows a model of the top surface shape of a region 126 of a hexagonal zinc oxide film 125. FIG. 5C shows a model of the cross-sectional shape of region 126. As shown in FIG. 5B, the hexagonal oxide In the zinc film 125, Zn atoms and O atoms are bonded in a hexagonal shape. The bonds between n and O atoms extend across the ab plane.
[0087] Next, sputtering particles are ejected from the sputtering target. As the puttering particles, In-Ga-Zn oxide particles peeled off, as shown in Figure 4(C). On the hexagonal zinc oxide film 125, In-Ga-Zn oxide particles 127 are deposited, and In-Ga A film 129 having Zn oxide particles is formed. Zinc particles, oxygen particles, and zinc oxide particles were also peeled off as coating particles, but these are omitted here. do.
[0088] The In-Ga-Zn oxide particles 127 have crystallinity and are typically single crystals. In some cases, the In-Ga-Zn oxide particles 127 are polycrystalline.
[0089] Here, the shape of the In-Ga-Zn oxide particles 127 will be described with reference to FIG. As shown in FIG. 6A, the In-Ga-Zn oxide particle 127 has an aspect ratio of Unlike the quartz crystals, they are flat or plate-like, with the width longer than the length. In the n-Ga-Zn oxide particle 127, the side parallel to the c-axis corresponds to the width in the cross section. In the In-Ga-Zn oxide grain 127, this corresponds to a side parallel to the axis intersecting the c-axis. As shown in Figure 6(A), there are two parallel hexagons (regular hexagons) with all interior angles of 120°. Alternatively, as shown in FIG. 6(C), it is preferable that all of the interior angles are 6. It is preferable that the lens has two parallel faces 127s of a 0° triangle (equilateral triangle). The In-Ga-Zn oxide particles 127 can be called pellets. For example, the surface 127s is parallel to the ab plane of the crystal. The direction perpendicular to the direction of the crystal is the c-axis direction. The thickness is 100 nm or less, 1 nm or more but 30 nm or less, or 1 nm or more but 10 nm or less.
[0090] The In-Ga-Zn oxide particles 127 are positively or negatively charged. In the case of the In-Ga-Zn oxide particles 127a, some of the oxygen atoms in the particles 127a are charged by the ion collision. Alternatively, by being exposed to plasma, one of the oxygen atoms of the In-Ga-Zn oxide particles 127a may be FIG. 6B shows a negatively charged In-Ga-Zn oxide particle 127a. As shown in FIG. 6B, the In-Ga-Zn oxide particles 127a Some of the oxygen in the In-Ga-Zn oxide particles may be negatively charged. Oxygen ions may bond to 27a.
[0091] Here, as an example of the crystal contained in the sputtering target, InGaO3(Zn O) m The crystal structure of a homologous compound represented by m=1 (m is a natural number) is called the ab plane. The figure is shown from a parallel perspective (see FIG. 7(A)). In FIG. 7(A), the area surrounded by the dashed line An enlarged view of this portion is shown in FIG.
[0092] For example, in the crystals contained in the sputtering target, the gallium oxide shown in FIG. A first layer having gallium atoms or / and zinc atoms and oxygen atoms, and a second layer having gallium atoms or and / or a second layer having zinc atoms and oxygen atoms, This is because the oxygen atoms in the first layer and the oxygen atoms in the second layer are close to each other. This is due to the fact that oxygen atoms, for example, carry a negative charge. Therefore, if oxygen atoms are close to each other, the bond between the layers may be weakened. The chemical bonds in the first layer and the second layer are bonded to the bonds between the first layer and the second layer. The chemical bonds in the first and second layers are much larger than those in the first layer, and a cleavage plane forms between the first and second layers. Thus, the cleavage plane may be parallel to the ab plane.
[0093] In addition, the crystal structure shown in Fig. 7 has gold atoms arranged in equilateral triangles and equilateral hexagons when viewed perpendicular to the ab plane. Therefore, the sputtering process contains crystals with the crystal structure shown in Figure 7. When the target is used, the In-Ga-Zn oxide particles 127 have an interior angle of 120°. There is a high probability that the shape will have regular hexagonal faces or equilateral triangular faces with internal angles of 60°. It is thought that.
[0094] Here, the In-Ga-Zn oxide formed by peeling off on the cleavage plane shown in FIG. Representative examples of the crystal structure of the particle 127 are shown in FIG. 5(D) and FIG. 5(E).
[0095] The In-Ga-Zn oxide particles 127a shown in FIG. 5(D) are composed of gallium atoms and / or The first layer, which has zinc and oxygen atoms (denoted as (Ga,Zn)O), is an oxide layer. A layer of indium (InO2) and a layer of gallium or / and zinc and oxygen atoms. The first layer (indicated as (Ga,Zn)O) is bonded to the second layer (indicated as (Ga,Zn)O).
[0096] Also, the In-Ga-Zn oxide particle 127b shown in FIG. 5(E) is a gallium atom or and a first layer having zinc atoms and oxygen atoms (denoted as (Ga,Zn)O); A second layer having gallium atoms and / or zinc atoms and oxygen atoms ((Ga,Zn )O.) and an indium oxide layer (InO2) and gallium atoms or / and zinc A third layer, which has gallium atoms and oxygen atoms (denoted as (Ga,Zn)O), and / or a fourth layer having zinc atoms and oxygen atoms (denoted as (Ga,Zn)O). ) are bonded in sequence to form a five-layer structure.
[0097] When the hexagonal zinc oxide film 125 is formed on the substrate 121, the hexagonal zinc oxide film 1 In-Ga-Zn oxide particles 127 are deposited in the direction of 25. Since the hexagonal zinc oxide film 125 is heated, the energy from the heat treatment causes the The c-axis of the In-Ga-Zn oxide particles 127 was aligned parallel to the c-axis of the In-Ga-Zn oxide particles 127 by sputtering. The In-Ga-Zn oxide particles 127 peeled off from the target 13 are hexagonal zinc oxide. After being moved or rotated in the vicinity of the film 125 , it is deposited on the hexagonal zinc oxide film 125 .
[0098] At this time, the a-axis and b-axis directions of the In-Ga-Zn oxide particles already deposited are aligned. Similarly, the In-Ga-Zn oxide particles 127 may rotate and bond on the ab plane. As a result, the a-axis and b-axis directions of adjacent In-Ga-Zn oxide grains are aligned. As a result, single crystal regions are formed in the film 129 having In-Ga-Zn oxide particles. A film 12 having In-Ga-Zn oxide particles is formed on the entire surface of the cubic zinc oxide film 125. The crystal orientation of the In-Ga-Zn oxide particles is aligned, and the film 129 having the In-Ga-Zn oxide particles becomes a single crystal region. Alternatively, in the film 129 having In-Ga-Zn oxide particles, single crystal Multiple regions are formed, and the direction of the c-axis of the In-Ga-Zn oxide grains in each region is Only the a-axis and b-axis may be aligned, but not aligned.
[0099] FIG. 5(F) shows the zinc oxide film and the In-Ga-Z A model of the cross-sectional shape near the interface of the film 129 having n oxide particles is shown in FIG. As shown in the figure, the Zn of the hexagonal zinc oxide film and the film 129 having In-Ga-Zn oxide particles are A layer having gallium atoms or / and zinc atoms and oxygen atoms ((Ga, Zn)O.) is bonded to the oxygen.
[0100] Since the hexagonal zinc oxide film 125 has high crystallinity, the hexagonal zinc oxide film 125 is used as a seed crystal. By doing so, it is possible to improve the crystallinity of the film 129 having In-Ga-Zn oxide particles. It is.
[0101] Next, in the same manner as in FIG. 4(A), as shown in FIG. 8(A), zinc particles 123a and oxygen particles 123b peels off from the sputtering target and deposits on the In-Ga-Zn oxide particles 127. , whereby hexagonal crystal grains 123c made of zinc oxide are formed on the substrate. .
[0102] Since zinc oxide crystals grow quickly in the direction parallel to the ab plane, the oxide The hexagonal crystal grains 123c formed of zinc chloride are oriented in a direction parallel to the surface of the substrate 121, i.e., in the direction of the oxide. The zinc oxide film is crystallized laterally in the cross section to form a hexagonal zinc oxide film 131. (See FIG. 8B.) That is, the hexagonal zinc oxide film 131 has single crystal regions.
[0103] After this, sputtering particles are released from the sputtering target, as in Figure 4(C). As shown in FIG. 8(C), an In-Ga-Zn oxide film is formed on the hexagonal zinc oxide film 131. In-Ga-Zn oxide particles 133 are deposited. Zn oxide particles are deposited.
[0104] The process of forming the hexagonal zinc oxide film 131 shown in FIG. 8(B) and the process of forming the In By repeating the process of depositing Ga-Zn oxide particles 133, a highly crystalline oxide film is obtained. A film can be formed.
[0105] Formed by a sputtering method using the sputtering target of the first embodiment The atomic ratio of Ga to In in In-Ga-Zn oxide (Ga / In), and the Z ratio The atomic ratio of n (Zn / In) is smaller than the atomic ratio contained in the sputtering target. In addition, in the In-Ga-Zn oxide film, the atomic ratio of Zn to Ga (Zn / Ga) is 0.5 or more.
[0106] In addition, the In-Ga-Zn oxide particles are deposited in the hexagonal zinc oxide film along the c-axis direction. Therefore, the oxide film obtained by this process has a c-axis that is aligned with the normal vector of the surface on which it is formed or the surface The CAAC-OS film is aligned parallel to the normal vector of the
[0107] In addition, the crystal structure of the oxide film obtained by the film formation process shown in Figs. 4 and 8 will be described with reference to Fig. 9. The oxide film obtained by the film formation process shown in FIG. 4 and FIG. 8 is composed of two indium oxide layers (I nO2), a layer having gallium atoms or / and zinc atoms and oxygen atoms is placed between the Since multiple layers of In-Ga-Zn oxide particles having the above properties are stacked, it has a homologous structure. .
[0108] As shown in FIG. 9A, the oxide film obtained by the film forming process of FIG. 4 and FIG. 8 is a first oxide film. Indium layer (InO2) and gallium atoms or / and zinc atoms and oxygen atoms A layer having a thickness of 100 nm (denoted as (Ga,Zn)O) and a second indium oxide layer (InO2). The structure is made up of three layers bonded in order. That is, between the indium oxide layers, gallium atoms or and / or one layer having zinc atoms and oxygen atoms.
[0109] As shown in FIG. 9B, the oxide film obtained by the film forming process shown in FIG. 4 and FIG. Indium oxide layer (InO2) and gallium atoms and / or zinc atoms and oxygen The first layer has gallium atoms (denoted as (Ga,Zn)O) and the second layer has gallium atoms or / and zinc atoms (denoted as (Ga,Zn)O). A second layer having lead and oxygen atoms (denoted as (Ga,Zn)O) and a second oxide layer The structure is made up of four layers, one of which is an indium oxide (InO2) and the other is an indium oxide (InO3). Between the two layers, two layers having gallium atoms or / and zinc atoms and oxygen atoms are provided. It is being done.
[0110] As shown in FIG. 9C, the oxide film obtained by the film forming process shown in FIGS. Indium oxide layer (InO2) and gallium atoms and / or zinc atoms and oxygen The first layer has atoms (denoted as (Ga,Zn)O), the second layer has zinc oxide (ZnO), and the third layer has gallium (Ga,Zn)O. The second layer, which has aluminum atoms and / or zinc atoms and oxygen atoms ((Ga,Zn)O The structure is made up of five layers, one of which is a first layer of indium oxide (InO2) and the other is a second layer of indium oxide (InO2). That is, between the indium oxide layers, gallium atoms and / or zinc atoms and oxide Two layers having atomic elements and a zinc oxide film are provided.
[0111] In addition, a layer having a plurality of gallium atoms and / or zinc atoms and oxygen atoms ((G The structure of the repeating unit having a zinc oxide film between the ZnO layers is shown in Figure 8(C). As shown, the In-Ga-Zn oxide particles 127, the hexagonal zinc oxide film 131, and the In -Ga-Zn oxide particles 133 are formed in the region where they are stacked.
[0112] In this embodiment, the steps of forming the hexagonal zinc oxide film 131 shown in FIG. 8(B) and FIG. Although the process of depositing the In-Ga-Zn oxide particles 133 shown in FIG. In this case, in the step of FIG. 8(B), In-Ga-Zn oxide is In some cases, the hexagonal zinc oxide film 131 is formed not only on the top surface of the solid particle but also on the side surface.
[0113] By the above process, a CAAC-OS film can be formed. In addition, the In-Ga-Zn oxide film can be formed. In place of Ga, Al, Ti, Y, Zr, La, Cs, Nd, or Hf may be used as appropriate. By using In-M-Zn oxide (M is Al, Ti, Y, Zr, La, Cs, Nd In this model, a crystal layer of SiO2 or Hf can be formed on the substrate 121. Instead of the grains 123c being formed, the In-Ga-Zn oxide grains 127 shown in FIG. 5(a), or In-Ga-Zn oxide particles 127b shown in FIG. 5(E) are formed on the substrate 121. The model allows the deposition of CAAC-OS films. It is possible to form an In-Ga-Zn oxide film.
[0114] Here, the formed CAAC-OS will be described in detail.
[0115] The CAAC-OS film is one of the oxide semiconductor films that has multiple crystal parts aligned along the c-axis. .
[0116] The CAAC-OS film was observed under a transmission electron microscope (TEM). When observed using a quartz crystal microscope, clear boundaries between crystal parts were observed, i.e. It is difficult to confirm the grain boundary. It can be said that the AC-OS film is less susceptible to the decrease in electron mobility caused by grain boundaries.
[0117] Cross-sectional and planar TEM observations revealed that the crystals in the CAAC-OS film had an orientation. It can be seen that...
[0118] Most of the crystals in the CAAC-OS film are cubic with a side length of less than 100 nm. The size is small enough to fit inside the body. Therefore, the crystal part in the CAAC-OS film has a side length of 10 This includes sizes that fit within a cube of less than 3 nm, 5 nm, or 5 nm. However, multiple crystals in the CAAC-OS film are connected to form a single large crystal domain. For example, in a planar TEM image, 2 More than 5μm 2 More than or equal to 1000μm 2 In some cases, crystal regions having more than this amount may be observed.
[0119] For example, the CAAC-OS has a plurality of crystal parts, and the c-axes of the crystal parts are aligned in the crystal parts. They may be aligned in a direction parallel to the normal vector of the forming plane or the normal vector of the surface. Therefore, CAAC-OS can be characterized by, for example, X-ray diffraction (XRD). When the out-of-plane analysis was performed using a fusion apparatus, the c-axis orientation was In some cases, a peak identified to the crystal plane orientation (00x), for example, a peak identified to the crystal plane orientation (00x), may appear.
[0120] In the CAAC-OS film, the orientation of the a-axis and b-axis is irregular between different crystal regions. The c-axis has a c-axis orientation, and the c-axis is parallel to the normal vector of the surface to be formed or the upper surface. Therefore, it is clear that the layers of metal atoms arranged in layers, as confirmed by cross-sectional TEM observation, are is a plane parallel to the ab plane of the crystal.
[0121] The crystalline part is formed when the CAAC-OS film is formed or after a crystallization process such as a heat treatment. As described above, the c-axis of the crystal is aligned to the surface on which the CAAC-OS film is to be formed. Orientation is parallel to the normal vector of the top surface. When the shape is changed by etching, the c-axis of the crystal is aligned with the CAAC-OS film. It may not be parallel to the face or top surface normal vector.
[0122] In addition, the distribution of the c-axis oriented crystal parts in the CAAC-OS film may not be uniform. For example, the crystals in the CAAC-OS film grow from the top surface of the CAAC-OS film. Therefore, when the crystal is formed, the region near the top surface has more c-axis oriented crystals than the region near the surface on which the crystal is formed. In addition, when impurities are added to the CAAC-OS film, the proportion of impurities may increase. The region where the material was added changed in quality, and regions with different proportions of c-axis oriented crystals were formed. It may also be possible.
[0123] In addition, for example, in the electron diffraction pattern of CAAC-OS, spots (bright spots) are observed. In addition, the probe diameter is close to or smaller than the size of the crystal part (for example, 1 nm or more). Electron beam diffraction using an electron beam of 30 nm or less is also called nanobeam electron beam diffraction.
[0124] FIG. 10(A) shows an example of a nanobeam electron diffraction pattern of a sample having a CAAC-OS. Here, the sample was cut in a direction perpendicular to the CAAC-OS surface, and the thickness was 4 mm. The electron beam diameter is 1 nmφ. The incident light is perpendicular to the cut surface of the sample. It can be seen that spots are observed in the electron beam diffraction pattern.
[0125] The CAAC-OS film is an oxide semiconductor film with a low concentration of impurities. The oxide semiconductor film is preferably made of silicon or a transition metal element other than the main component of the oxide semiconductor film. The elements that bond to oxygen stronger than the metal elements that form the oxide semiconductor film, such as Zn, By removing oxygen from the oxide semiconductor film, the atomic arrangement of the oxide semiconductor film is disturbed, and the crystallinity is reduced. In addition, heavy metals such as iron and nickel, argon, and carbon dioxide are Since the diameter (or molecular radius) of the ions is large, when the ions are contained inside the oxide semiconductor film, the oxide semiconductor film The impurities contained in the oxide semiconductor film are disturbed, which causes a decrease in crystallinity. Pure materials may act as carrier traps or carrier generation sources.
[0126] The CAAC-OS film is an oxide semiconductor film with a low density of defect states. Oxygen vacancies in semiconductor films act as carrier traps and trap hydrogen. This can become a carrier generation source.
[0127] The low impurity concentration and low defect level density (low oxygen vacancies) are called high purity intrinsic or The term "high-purity intrinsic" refers to a substantially high-purity intrinsic oxide semiconductor. Since the film has a small carrier generation source, the carrier density can be reduced. The transistor using the oxide semiconductor film has electrical characteristics (noise) in which the threshold voltage is negative. It is also called "marine". It is rare for it to become "high purity genuine" or "substantially high purity". The intrinsic oxide semiconductor film has few carrier traps. Transistors using the film have little fluctuation in electrical characteristics and are highly reliable. Note that it takes a certain time for charges trapped in the carrier traps in the oxide semiconductor film to be released. The time is long and the charge may behave as if it were a fixed charge. In addition, a transistor using an oxide semiconductor film having a high density of defect states has unstable electrical characteristics. There may be cases where this occurs.
[0128] In addition, transistors using CAAC-OS that are high purity intrinsic or substantially high purity intrinsic are The electrical characteristics of this capacitor change little when exposed to visible or ultraviolet light.
[0129] <Crystal growth mechanism of zinc oxide> Here, the crystal growth mechanism of the zinc oxide film 125 shown in FIG. 4(B) will be described with reference to FIGS. 3 will be used to explain.
[0130] The atomic motion during heat treatment was examined using classical molecular dynamics. So the force acting on atoms can be expressed by defining an empirical potential that characterizes the interactions between atoms. Here, we apply the laws of classical mechanics to each atom and estimate its motion according to Newton's law. The motion (time evolution) of each atom was verified by solving the equations numerically. As an empirical potential, the Born-Mayer-Huggins potential was used.
[0131] As shown in FIG. 11, amorphous zinc oxide (hereinafter referred to as a-ZnO) has a width of 1 nm. Single crystal zinc oxide (hereinafter referred to as c-ZnO) is arranged at equal intervals as crystal nuclei 180. The model was created with the density of a-ZnO and c-ZnO set at 5.5 g / cm 3 It was decided. The vertical direction was defined as the c-axis direction.
[0132] Next, in the model of Fig. 11, c-ZnO is fixed and the 3D periodic boundary condition is set at 70 Classical molecular dynamics at 0℃ for 100psec (time step width 0.2fsec x 500,000 steps) The results of the mathematical calculations are shown in Figs. 12 and 13.
[0133] 12(A), 12(B), and 12(C) are for 20 psec, 40 psec, and The change in atomic configuration over 60 psec is shown in Figure 13(A) and Figure 13(B). The changes in atomic configuration after 80psec and 100psec are shown. In each figure, the distance and direction of crystal growth are indicated by the length and direction of the arrow.
[0134] The crystal growth rates in the vertical direction (c-axis
[0001] ) and the horizontal direction perpendicular to it are shown in Table 1. .
[0135] [Table 1]
[0136] In FIG. 12, the arrows 182, 186, and 190 in the vertical direction (c-axis direction) are Arrows 184a, 184b, 188a, 188b, 192a, 1 The longer length of 92b indicates that lateral crystal growth is predominant. ) shows that crystal growth is terminated between adjacent crystal nuclei.
[0137] In FIG. 13, the crystalline regions formed on the surface are used as seeds, as indicated by arrows 194 and 196. As can be seen, the crystal grows in the vertical direction (c-axis direction).
[0138] In addition, from Table 1, it is clear that the crystal growth is greater in the horizontal direction perpendicular to the vertical direction (c-axis
[0001] ) than in the vertical direction. From these results, it can be seen that the growth rate of ZnO is about 4.9 times faster than that of the surface (a Crystal growth proceeds in a direction parallel to the ab plane. At this time, crystal growth proceeds in the lateral direction on the ab plane. Next, the single crystal region formed on the surface (ab plane) is used as a seed to grow the surface ( Crystal growth proceeds along the c-axis, which is perpendicular to the ab plane. Thus, after the crystals grow preferentially in the direction parallel to the surface (ab plane), The crystal grows along the c-axis, which is perpendicular to the surface (epitaxial growth, or axial growth). This process (also called bulk growth) results in the formation of single crystal regions.
[0139] <Heated deposition (deposition temperature: 600°C or higher, but below the substrate distortion point)> Next, a film formation method different from that shown in FIGS. 4 to 9 will be described with reference to FIGS. The film formation method shown in FIGS. 14 to 16 has a higher film formation temperature than the film formation method shown in FIGS. Zinc oxide is easily evaporated at temperatures of 600° C. or higher in a reduced pressure atmosphere. The oxide film formed by the film forming method shown in FIG. 9 and the film forming method shown in FIG. The crystal structure is different.
[0140] As shown in FIG. 14(A), similarly to FIG. 4(A), the sputtering target 13 is The ions 15 collide with the sputtering target 13, causing sputtering particles to be ejected from the sputtering target 13. Therefore, in the plasma 17, there are ions, sputtering particles, electrons, etc.
[0141] Sputtering particles include zinc particles, oxygen particles, zinc oxide particles, and In-Ga-Zn. The sputtering target produced in the first embodiment is made of Z rather than Ga. For this reason, in this embodiment, zinc particles, oxide, etc. are extracted from the sputtering target 13. After the elementary particles or zinc oxide particles are preferentially peeled off, the zinc particles, oxygen particles, zinc oxide particles This will be explained using a model in which In-Ga-Zn oxide particles peel off.
[0142] First, zinc particles 143a and oxygen particles 143b are sputtered. Next, the zinc particles 143a and the oxygen particles 143b are peeled off from the pulverizing target 13. As a result, the hexagonal crystal grains 143c formed of zinc oxide move onto the substrate 141. is formed on top.
[0143] In this case, since the substrate temperature is 600° C. or higher, the direction is parallel to the surface of the substrate 141. As a result, the crystal grows laterally on the ab plane, and a hexagonal In other words, the hexagonal zinc oxide film 145 has a single crystal region. Unlike the film formation process shown in FIG. 4(B), a part of the zinc oxide evaporates. The hexagonal zinc oxide film 145 is separated.
[0144] FIG. 15 shows a model of the top surface shape of the hexagonal zinc oxide film 145. As shown in FIG. In the hexagonal zinc oxide film 145, Zn atoms and O atoms are bonded in a hexagonal shape. The hexagonal bonds between Zn and O atoms are spread across the ab plane.
[0145] Next, sputtering particles are ejected from the sputtering target. As the puttering particles, In-Ga-Zn oxide particles peeled off, as shown in Figure 14(C). In-Ga-Zn oxide particles 147 are deposited on the hexagonal zinc oxide film 145, A film 149 having In-Ga-Zn oxide particles is formed. has the same structure as the In-Ga-Zn oxide particles 127. Although zinc particles and oxygen particles were also peeled off as sputtering particles, their description is omitted here. .
[0146] Here, the hexagonal zinc oxide film 145 formed on the substrate 141 is separate. Therefore, the hexagonal zinc oxide film 145 does not cover the entire surface of the substrate 141. In-Ga-Zn oxide particles 147 are deposited in the same crystal orientation as the zinc oxide film 145. Specifically, the c-axis of the hexagonal zinc oxide film 145 and the c-axis of the In-Ga-Zn oxide grains 147 The In-Ga- After the Zn oxide particles 147 move or rotate in the vicinity of the hexagonal zinc oxide film 145, the hexagonal The zinc oxide film 145 is deposited on the crystalline zinc oxide film 145 .
[0147] On the other hand, in the region where the hexagonal zinc oxide film 145 is not formed, In-Ga-Z The crystal orientation of the n oxide particles 147 is random.
[0148] Next, in the same manner as in FIG. 14(A), zinc particles 143a and oxygen are mixed together as shown in FIG. 16(A). Particles 143b peel off from the sputtering target, and In-Ga-Zn oxide particles 14 Zinc particles 143a and oxygen particles 143b reach and adhere to the surface of the substrate 7. As a result, as shown in FIG. As shown in FIG. 1B, a hexagonal zinc oxide film 151 is formed.
[0149] After this, as in FIG. 14(B), sputtering particles are released from the sputtering target. As shown in FIG. 16(C), the In-Ga-Zn oxide is formed on the hexagonal zinc oxide film 151. On the In-Ga-Zn oxide particles 153, another In-Ga a-Zn oxide particles are deposited.
[0150] The process of forming the hexagonal zinc oxide film 151 shown in FIG. 16(B) and the process of forming the hexagonal zinc oxide film 152 shown in FIG. 16(C) By repeating the process of depositing In-Ga-Zn oxide particles 153, highly crystalline oxide A film can be formed.
[0151] Formed by a sputtering method using the sputtering target of the first embodiment The atomic ratio of Ga to In in In-Ga-Zn oxide (Ga / In), and the Z ratio The atomic ratio of n (Zn / In) is smaller than the atomic ratio contained in the sputtering target. In addition, in the In-Ga-Zn oxide film, the atomic ratio of Zn to Ga (Zn / Ga) is 0.5 or more.
[0152] In addition, since the crystal orientation of the oxide film obtained in the film formation process of FIG. 14 to FIG. 16 is random, However, the sputtering grains that accumulate during the film formation process Each of the molecules has a homologous structure. The oxide film thus obtained contains a region having a homologous structure and has high crystallinity.
[0153] By the above steps, a polycrystalline In-Ga-Zn oxide film can be formed. In the In-Ga-Zn oxide, Ga may be replaced with Al, Ti, Y, or Zr. By using La, Cs, Nd, or Hf, polycrystalline In-M-Zn oxide ( M can be Al, Ti, Y, Zr, La, Cs, Nd, or Hf.
[0154] Here, the polycrystalline In-M-Zn oxide that is formed will be described. The In-M-Zn oxide having a crystal structure is hereinafter referred to as a polycrystalline oxide semiconductor. The body contains a plurality of grains.
[0155] In the polycrystalline oxide semiconductor film, crystal grains can be confirmed in the TEM image. The crystal grains contained in the crystalline oxide semiconductor film are, for example, 2 nm to 3 nm in a TEM image. 00 nm or less, 3 nm to 100 nm or 5 nm to 50 nm. In addition, in the case of a polycrystalline oxide semiconductor film, crystal grain boundaries cannot be confirmed in the TEM images. There may be cases where this occurs.
[0156] The polycrystalline oxide semiconductor film has, for example, a plurality of crystal grains. The crystal orientation may be different. When structural analysis is performed using this method, for example, a polycrystalline oxide semiconductor having InGaZnO4 crystals is obtained. In the out-of-plane analysis of the membrane, a peak was observed at 2θ near 31°, and a peak was observed at 2θ near 3 A peak near 6° or other peaks may appear.
[0157] A polycrystalline oxide semiconductor film has, for example, high crystallinity and therefore high electron mobility. Therefore, a transistor in which a polycrystalline oxide semiconductor film is used for a channel formation region may However, the polycrystalline oxide semiconductor film has impurities at the grain boundaries. In addition, the grain boundaries of the polycrystalline oxide semiconductor film may become defect states. In an oxide semiconductor film, crystal grain boundaries can become carrier traps or carrier generation sources. In the transistor in which a polycrystalline oxide semiconductor film is used for a channel formation region, Compared to transistors that use SiO2 in the channel formation region, the fluctuation in electrical characteristics is large and reliability is poor. In some cases, the transistor may be low.
[0158] <Room temperature film formation (film formation temperature: 20℃ or higher and 150℃ or lower)> Next, a film formation method different from that shown in FIGS. 4 to 9 will be described with reference to FIGS. The film formation methods shown in FIGS. 17 and 18 have a lower film formation temperature than the film formation methods shown in FIGS.
[0159] As shown in FIG. 17(A), similarly to FIG. 4(A), the sputtering target 13 is The ions 15 collide with the sputtering target 13, causing sputtering particles to be ejected from the sputtering target 13. Therefore, in the plasma 17, there are ions, sputtering particles, electrons, etc.
[0160] Sputtering particles include zinc particles, oxygen particles, zinc oxide particles, and In-Ga-Zn. The sputtering target produced in the first embodiment is made of Z rather than Ga. For this reason, in this embodiment, zinc particles, oxide, etc. are extracted from the sputtering target 13. After the elementary particles or zinc oxide particles are preferentially peeled off, the zinc particles, oxygen particles, zinc oxide, and This will be explained using a model in which In-Ga-Zn oxide particles peel off.
[0161] First, zinc particles 163a and oxygen particles 163b are sputtered as sputtering particles. The zinc particles 163a and the oxygen particles 163b are peeled off from the plating target 13 and deposited on the substrate 161. 3b arrives, and a zinc oxide film 165 is formed on the substrate 161 as shown in FIG. 17(B). do.
[0162] In this case, since the substrate temperature is 20° C. or more and 150° C. or less, the zinc oxide film 165 Low crystallinity.
[0163] Next, sputtering particles are ejected from the sputtering target. As the puttering particles, In-Ga-Zn oxide particles peeled off, as shown in Figure 17(C). In-Ga-Zn oxide particles 167 are deposited on the zinc oxide film 165, and the In-Ga-Zn A film 169 having oxide particles is formed. The In-Ga-Zn oxide particles 167 are In The structure of the -Ga-Zn oxide particles 127 is the same as that of the -Ga-Zn oxide particles 127. Zinc particles and oxygen particles are also peeled off as tarring particles, but they are omitted here.
[0164] In this case, since the zinc oxide film 165 has low crystallinity, the In deposited on the zinc oxide film 165 The crystal orientation of the -Ga-Zn oxide grains 167 is random.
[0165] After that, as shown in FIG. 18(A), zinc particles 163a and oxygen particles 163b are spat out. The In-Ga-Zn oxide particles 167 are peeled off from the pulverizing target and the zinc particles 16 As a result, a zinc oxide film with low crystallinity is formed. In addition, a separate sputtering process is performed simultaneously with the zinc particles 163a and the oxygen particles 163b. The particles are deposited on the In-Ga-Zn oxide particles 167 or on the zinc oxide film with low crystallinity. As a result, as shown in FIG. 18(B), a zinc oxide film 169a having low crystallinity and an In-G a-Zn oxide particles 169b are mixed in.
[0166] As shown in FIG. 18(A), zinc particles 163a and an oxide are formed on an In-Ga-Zn oxide particle 167. The process in which the elementary particles 163b arrive and adhere to the substrate 163b and the In-Ga-Zn oxide shown in FIG. By repeating the process of depositing particles 169b, a microcrystalline In-Ga-Zn oxide film is formed. A film can be formed.
[0167] Formed by a sputtering method using the sputtering target of the first embodiment The atomic ratio of Ga to In in In-Ga-Zn oxide (Ga / In), and the Z ratio The atomic ratio of n (Zn / In) is smaller than the atomic ratio contained in the sputtering target. In addition, in the In-Ga-Zn oxide film, the atomic ratio of Zn to Ga (Zn / Ga) is 0.5 or more.
[0168] The crystal orientation of the oxide film obtained in the film formation process of FIGS. 17 and 18 is random. Furthermore, since the film formation temperature is lower than that of the oxide film obtained by the film formation process shown in FIGS. However, the sputtering particles that accumulate during the film formation process have homologous structures. The oxide film has a higher crystallinity than an oxide film having an amorphous structure.
[0169] Through the above steps, an In-Ga-Zn oxide film having a microcrystalline structure can be formed. In the In-Ga-Zn oxide, Ga may be replaced with Al, Ti, Y, or Zr. By using La, Cs, Nd, or Hf, a microcrystalline In-M-Zn oxide ( M can be Al, Ti, Y, Zr, La, Cs, Nd, or Hf.
[0170] The crystal structure of the formed oxide film having a microcrystalline structure will be described below. Hereinafter, the In-M-Zn oxide having a microcrystalline structure will be referred to as a microcrystalline oxide semiconductor.
[0171] In the microcrystalline oxide semiconductor film, it is difficult to clearly identify the crystal parts in the TEM image. The crystal parts included in the microcrystalline oxide semiconductor film may have a size of, for example, 1 nm or more and 100 nm or less. The size is often less than nm, or between 1 nm and 10 nm. Nanocrystals (nc: nanocrystals) are microcrystals with a diameter of 10 nm or less, or between 1 nm and 3 nm. The oxide semiconductor film having crystal was The nc-OS film is also called the nc-OS film. For example, it may be difficult to clearly identify grain boundaries in TEM images.
[0172] The nc-OS film is a microscopic region (e.g., a region of 1 nm to 10 nm, especially a region of 1 nm or less). The nc-OS film has a periodic atomic arrangement in the region of 3 nm or less. There is no regularity in the crystal orientation between the crystals. Therefore, no orientation is observed throughout the film. Depending on the analysis method, the nc-OS film may be indistinguishable from an amorphous oxide semiconductor film. For example, an XRD device that uses X-rays with a diameter larger than that of the crystal part is used for the nc-OS film. When the structure was analyzed using the out-of-plane method, peaks indicating crystal planes were In addition, for the nc-OS film, the probe diameter is larger than the crystalline part. Electron beam diffraction pattern (selected area electron beam diffraction) using an electron beam (e.g., 50 nmφ or more) ) produces a halo-like diffraction pattern. For the -OS film, the probe diameter is close to or smaller than the size of the crystal part (e.g., 1 nm When electron diffraction is performed using an electron beam with a diameter of 30 nm or more, spots are observed. Nanobeam electron diffraction of the nc-OS film revealed multiple spots in the ring-shaped region. may be observed.
[0173] Figure 10(B) shows the results of nanobeam electron spectroscopy at different measurement points on a sample with an nc-OS film. 1 is an example of a X-ray diffraction pattern. Here, the sample is aligned in a direction perpendicular to the surface on which the nc-OS film is formed. The specimen is cut into thin slices with a thickness of 10 nm or less. An electron beam of 1 nm is incident from a direction perpendicular to the cut surface of the sample. From Fig. 10(B), nc When nanobeam electron diffraction is performed on a sample with an -OS film, a diffraction pattern showing the crystal planes is obtained. However, it was found that no specific crystal plane orientation was observed.
[0174] The nc-OS film is an oxide semiconductor film that has higher order than an amorphous oxide semiconductor film. Therefore, the nc-OS film has a lower density of defect states than the amorphous oxide semiconductor film. The nc-OS film has no regularity in the crystal orientation between different crystal parts. , the defect density is higher than that of the CAAC-OS film.
[0175] Therefore, the nc-OS film may have a higher carrier density than the CAAC-OS film. An oxide semiconductor film having a high carrier density may have high electron mobility. A transistor using an nc-OS film for the channel formation region has high field-effect mobility. In addition, the nc-OS film has a higher density of defect states than the CAAC-OS film. Therefore, the nc-OS film is used as the channel formation region. The transistors used in the channel formation region are transistors using a CAAC-OS film. Compared to conventional transistors, the fluctuation in electrical characteristics is large, and the transistors may become less reliable. However, the nc-OS film can be formed even if it contains a relatively large amount of impurities. It is easier to form than the AAC-OS film, and can be used preferably in some applications. Therefore, it is possible to manufacture a semiconductor device having a transistor using an nc-OS film with high productivity. It can be made.
[0176] (Embodiment 3) In this embodiment, a film forming apparatus for forming an oxide film with high crystallinity is as follows: This will be explained with reference to FIG. 19 and FIG. 20.
[0177] First, let us consider the structure of a film formation device that minimizes the amount of impurities mixed into the film during film formation. Let's explain using 0.
[0178] FIG. 19 is a schematic top view of a single-wafer multi-chamber film forming apparatus 4000. The deposition apparatus 4000 includes a cassette port 4101 for accommodating a substrate and a substrate alignment device. and an atmosphere-side substrate supply chamber 4001 having an alignment port 4102 for performing the alignment. The substrate supply chamber 4001 is connected to the atmospheric substrate transfer chamber 4002, which transfers the substrate, and the substrate transfer chamber 4003 is connected to the atmospheric substrate transfer chamber 4002. A load lock chamber in which the pressure inside the chamber is switched from atmospheric pressure to reduced pressure or from reduced pressure to atmospheric pressure. 4003a, the substrate is removed, and the pressure in the chamber is reduced to atmospheric pressure or vice versa. The unload lock chamber 4003b is switched to a reduced pressure state, and the transfer chamber 4003 is used for transferring substrates in a vacuum. 004, a substrate heating chamber 4005 for heating the substrate, and a sputtering target is disposed in the chamber. The film forming chambers 4006a, 4006b, and 4006c are provided for film formation.
[0179] As shown in FIG. 19, the cassette port 4101 is provided in a plurality of positions (three in FIG. 19). ) may be included.
[0180] The atmospheric substrate transfer chamber 4002 includes a load lock chamber 4003a and an unload lock The load lock chamber 4003a and the unload lock chamber 4003b are connected to each other. The transfer chamber 4004 is connected to a substrate heating chamber 4005 and a film forming chamber 400. Connect to 6a, 4006b, and 4006c.
[0181] A gate valve 4104 is provided at the connection between the chambers, and the atmosphere side substrate supply chamber 4 Except for the atmospheric side substrate transfer chamber 4001 and the atmospheric side substrate transfer chamber 4002, each chamber can be independently maintained in a vacuum state. In addition, the atmospheric side substrate transfer chamber 4002 and the transfer chamber 4004 are connected to a substrate transfer robot 41. 03 and capable of transporting glass substrates.
[0182] The film forming apparatus 4000 can transport the substrate between processes without exposing it to the atmosphere. This can prevent impurities from being adsorbed on the substrate. The number of lock chambers, unload lock chambers and substrate heating chambers is not limited to the above, and may vary depending on the installation space. An optimal number can be set appropriately according to the process conditions.
[0183] Next, a cross section of the film forming apparatus 4000 shown in FIG. 19, which corresponds to the dashed line B1-B2, is shown in FIG. show.
[0184] In addition, examples of heating mechanisms that can be used in the substrate heating chamber 4005 include resistance heating. Alternatively, the heating mechanism may be a mechanism that uses a medium such as a heated gas to heat the device. The heating mechanism may be a device that heats the device by thermal conduction or thermal radiation. For example, GRTA (G as Rapid Thermal Anneal), LRTA(Lamp Rapid Thermal Anneal (RTA) eal) can be used. LRTA can be used with halogen lamps, metal halide lamps, Xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure mercury lamp The object to be treated is heated by radiating light (electromagnetic waves) emitted from lamps such as the following: Heat treatment is performed using high-temperature gas, preferably an inert gas.
[0185] The transfer chamber 4004 includes a substrate transfer robot 4103. The third has a plurality of movable parts and an arm for holding a substrate, and can transport the substrate to each chamber. The transfer chamber 4004 is connected to a vacuum pump 4200 and a cryopump 4200 via a valve. With this configuration, the transfer chamber 4004 is connected to the air Uses Vacuum Pump 4200 for pressures ranging from low to medium vacuum (0.1 to several hundred Pa). The vacuum is evacuated by switching the valve to change from medium vacuum to high vacuum or ultra-high vacuum (0.1 Pa to 1 ×10 -7 The pressure is evacuated to 100MPa (Pa) using a cryopump 4201.
[0186] In addition, for example, two or more cryopumps 4201 are connected in parallel to the transfer chamber 4004. With this configuration, even if one cryopump is in regeneration, Even if the amount of the cryopump is increased, the remaining cryopump can still be used to pump the remaining cryopumps. Cryopump refers to the process of releasing molecules (or atoms) stored in the cryopump. If the Lyopump accumulates too many molecules (or atoms), its pumping capacity will decrease. Regeneration occurs periodically.
[0187] FIG. 20 is a cross-sectional view of the film forming chamber 4006b, the transfer chamber 4004, and the load lock chamber 4003a. The load lock chamber 4003a includes a substrate transfer stage 4111.
[0188] Here, the details of the film formation chamber will be described with reference to FIG. A film forming chamber, a plasma processing chamber, etc. can be appropriately used. The deposition chamber corresponds to the deposition chamber described in the second embodiment. In the film formation chamber shown in the second embodiment, the sputtering target and the substrate are placed horizontally. In the deposition chamber shown in this embodiment, the sputtering target and The board is illustrated as being vertically oriented.
[0189] The film forming chamber 4006b shown in FIG. 20 includes a sputtering target 4106 and an adhesion prevention plate 41 4107 and a substrate stage 4108. The substrate stage 4108 supports the substrate 410. The substrate 4109 is equipped with a substrate holding mechanism and a back heater for heating the substrate 4109 from the back side. It's fine.
[0190] A direct current (DC) power supply is used to apply voltage to the sputtering target. It is preferable to use a radio frequency (RF) power source or an alternating current (AC) power source. However, in the sputtering method using an RF power source, it is difficult to generate uniform plasma over a large area. Therefore, sputtering using an RF power source is not suitable for forming a large-area substrate. In addition, DC power is more advantageous than AC power for the following reasons: C power may be preferred.
[0191] In the sputtering method using a DC power source, for example, as shown in FIG. A DC voltage is applied between the target and the substrate. The potential difference between the sputtering target and the substrate during the sputtering was kept constant as shown in FIG. Thus, the sputtering method using a DC power supply can maintain a continuous plasma discharge. It can be held.
[0192] On the other hand, in the sputtering method using an AC power source, for example, as shown in FIG. In the adjacent sputtering targets, the cathode and the anode are For example, in the period A shown in FIG. 21(B2), the sputtering The get (1) acts as the cathode and the sputtering target (2) acts as the anode. In addition, for example, in the period B shown in FIG. 21(B2), the sputtering The target (1) acts as the anode and the sputtering target (2) acts as the cathode. Period A and Period B together can last, for example, 20 microseconds to 50 microseconds. In this way, the sputtering method using an AC power source has two periods, period A and period B. Plasma discharge occurs while alternating between these.
[0193] During film formation, the substrate stage 4108 is held approximately perpendicular to the floor. When the product is delivered, it is held in a roughly horizontal position relative to the floor. The position indicated by is the position where the substrate stage 4108 is held when the substrate is delivered. By adopting such a structure, dust or particles that may be mixed in during film formation are prevented from adhering to the substrate 4109. However, the probability of the substrate stage 41 being moved can be reduced more than when the substrate stage 41 is held horizontally. If 08 is held vertically (90°) to the floor, there is a risk that the board 4109 may fall. Therefore, it is preferable that the substrate stage 4108 has an angle of 80° or more and less than 90°.
[0194] The adhesion prevention plate 4107 is formed by sputtering the metal from the sputtering target 4106. This can prevent the accumulation of particles in unnecessary areas. It is desirable to process the surface so that the sputtered particles do not peel off. For example, To increase the resistance, blasting treatment may be performed, or the surface of the adhesion prevention plate 4107 may be made uneven.
[0195] The deposition chamber 4006b is connected to a mass flow controller 4302 via a gas heating mechanism 4302. 300, and the gas heating mechanism 4302 is precisely controlled via the mass flow controller 4300. The gas is introduced into the deposition chamber 4006b by a gas heating mechanism 4302. The gas can be heated to 40°C or higher and 400°C or lower, or 50°C or higher and 200°C or lower. The gas heating mechanism 4302, the mass flow controller 4300, and the refiner 43 Although the number of gas types is equal to the number of gas types, only one gas type is shown for simplicity. The dew point of the gas introduced is -80℃ or less, -100℃ or less, or -120℃ or less. Gases such as oxygen gas, nitrogen gas, and rare gases (argon gas) can be used. (such as a sachet, etc.) are used.
[0196] The film-forming chamber 4006b is connected to a turbo molecular pump 4202 and a vacuum pump 4203 via a valve. It is connected to P4200.
[0197] Further, the film formation chamber 4006b is provided with a cryotrap 4110.
[0198] The Cryotrap 4110 is designed to adsorb molecules (or atoms) with relatively high melting points, such as water. The turbo molecular pump 4202 is a mechanism that can pump large molecules (or atoms). It is highly productive because it stably exhausts hydrogen and other gases and requires little maintenance. Therefore, in order to improve the pumping capacity for water, etc., a cryotrap is The cryotrap 4110 is connected to the deposition chamber 4006b. The temperature of the refrigerator is set to 100K or less, or 80K or less. Also, the cryotrap 4 When 110 has multiple refrigerators, changing the temperature of each refrigerator can improve efficiency of exhaust. For example, the temperature of the first stage refrigerator is set to 100K or less, and the second stage refrigerator is set to 100K or less. The temperature of the first refrigerator should be set to 20K or less.
[0199] The method of exhausting the film forming chamber 4006b is not limited to this, and may be the same as that of the transfer chamber 4004. The pumping method may be the same as that of a cryopump and a vacuum pump. Of course, the exhaust method for the transfer chamber 4004 is the same as that for the film forming chamber 4006b (a turbo molecular pump, etc.). The same structure as that of the vacuum pump (exhaust method) may be used.
[0200] In addition, the back pressure ( It is preferable that the total pressure and the partial pressure of each gas molecule (atom) are as follows. The back pressure of the film-forming chamber 4006b and the partial pressure of each gas molecule (atom) are mixed into the film to be formed. It is necessary to be careful because there is a possibility that
[0201] The back pressure (total pressure) of each of the above mentioned chambers is 1×10 -4 Pa or less, or 3×10 -5 Pa or less , or 1 × 10 -5 The mass-to-charge ratio (m / z) of each of the above-mentioned chambers is 18. The partial pressure of the gas molecules (atoms) is 3×10 -5 Pa or less, or 1×10 -5 Pa or less or 3×10 -6 In addition, the gas molecules having m / z of 28 in each of the above-mentioned chambers ( The partial pressure of the atom is 3×10 -5 Pa or less, or 1×10 -5 Pa or less, or 3×10 -6 In addition, the partial pressure of the gas molecules (atoms) with m / z of 44 in each of the above-mentioned chambers is is 3 x 10 -5 Pa or less, or 1×10 -5 Pa or less, or 3×10 -6 Pa or less It is.
[0202] The total and partial pressures in the vacuum chamber can be measured using a mass spectrometer. For example, the quadrupole mass spectrometer (also called Q-mass) manufactured by ULVAC, Inc. lee CGM-051 can be used.
[0203] The above-mentioned transfer chamber 4004, substrate heating chamber 4005, and film forming chamber 4006b are It is desirable to have a configuration with little leakage or internal leakage.
[0204] For example, the above-mentioned transfer chamber 4004, the substrate heating chamber 4005, and the film forming chamber 4006b The crate is 3×10 -6 Pa·m 3 / s or less, or 1×10 -6 Pa·m 3 / s or less In addition, the leak rate of a gas molecule (atom) with m / z of 18 is 1×10 -7 Pa m 3 / s or less, or 3×10 -8 Pa·m 3 / s or less. Also, the m / z is 28. The leak rate of a gas molecule (atom) is 1×10 -5 Pa·m 3 / s or less, or 1×1 0 -6 Pa·m 3 / s or less. Also, the leak of gas molecules (atoms) with m / z of 44 The rate is 3x10 -6 Pa·m 3 / s or less, or 1×10 -6 Pa·m 3 / s or less do.
[0205] The leak rate was calculated from the total and partial pressures measured using the mass spectrometer mentioned above. It can be derived from
[0206] By forming an oxide film using the above film forming apparatus, the inclusion of impurities in the oxide film is suppressed. Can be controlled.
[0207] (Embodiment 4) In this embodiment, a semiconductor device according to one embodiment of the present invention and a manufacturing method thereof will be described with reference to drawings. Please refer to the following for explanation.
[0208] In a transistor including an oxide semiconductor film, An example of such defects is oxygen vacancies. The threshold voltage of a transistor using a thin film is easily shifted in the negative direction. This is because charges are generated due to oxygen vacancies in the oxide semiconductor film. When a transistor has normally-on characteristics, Various problems such as malfunctions becoming more likely or power consumption increasing when not in operation In addition, the electrical characteristics of transistors, typically There is a problem in that the amount of variation in the threshold voltage increases.
[0209] One of the causes of oxygen vacancies is damage that occurs during the manufacturing process of a transistor. For example, an insulating film or a conductive film is formed on an oxide semiconductor film by plasma CVD or sputtering. When forming an oxide semiconductor film, the oxide semiconductor film may be damaged depending on the forming conditions. There are times when this happens.
[0210] One of the causes of oxygen vacancies is oxygen desorption from an oxide semiconductor film due to heat treatment. For example, in order to remove impurities such as hydrogen and water contained in the oxide semiconductor film, However, when heat treatment is performed in a state where the oxide semiconductor film is exposed, the oxide Oxygen is released from the semiconductor film, forming oxygen vacancies.
[0211] In addition to oxygen deficiencies, impurities such as silicon and carbon, which are constituent elements of the insulating film, can also cause damage to the transistor. Therefore, the impurities may be mixed into the oxide semiconductor film, which may cause poor electrical characteristics of the transistor. As a result, the resistance of the oxide semiconductor film is reduced, and the oxide semiconductor film is easily deteriorated due to deterioration over time or in a stress test. This leads to a problem that the amount of variation in the electrical characteristics of the transistor, typically the threshold voltage, increases. There is.
[0212] In view of the above, in this embodiment, a semiconductor device including a transistor having an oxide semiconductor film is In the above, oxygen vacancies in the oxide semiconductor film, which is a channel region, and impurities in the oxide semiconductor film One of the objectives is to reduce the concentration of substances.
[0213] On the other hand, display devices on the market are becoming larger, with screen sizes of 60 inches or more diagonally. There is a trend toward larger screen sizes, with development also taking into account screen sizes of 120 inches or more. For this reason, the glass substrates used in display devices are large, 8th generation or higher. However, when using a large-area substrate, high-temperature processing, e.g., 450 Heating at temperatures above 30°C requires large, expensive heating equipment, which increases production costs. In addition, high temperature processing can cause warping and shrinkage of the substrate, resulting in a lower yield. is reduced.
[0214] Therefore, in this embodiment, the number of heat treatment steps is small and a large-area substrate can be used. Another object of the present invention is to manufacture a semiconductor device by using heat treatment at low temperature.
[0215] 22A to 22C are top views and The transistor 250 shown in FIG. 22 is a channel etch type transistor. FIG. 22A is a top view of the transistor 250, and FIG. FIG. 22(C) is a cross-sectional view taken along the dashed line C- in FIG. 22(A). 22(A) is a cross-sectional view of the substrate 211 and the transistor D for clarity. Some of the components of the capacitor 250 (for example, the gate insulating film 217), the oxide insulating film 223, the oxide 224, nitride insulating film 225, etc.) are omitted.
[0216] The transistor 250 shown in FIG. 22B and FIG. 22C is provided on a substrate 211. The gate electrode 215 is formed on the substrate 211. A gate insulating film 217 and an oxide semiconductor layer overlapping the gate electrode 215 via the gate insulating film 217 are formed. The semiconductor device includes a conductive film 218 and a pair of electrodes 221 and 222 in contact with the oxide semiconductor film 218 . Further, on the gate insulating film 217, the oxide semiconductor film 218, and the pair of electrodes 221 and 222, The insulating film 223 is a protection film including an oxide insulating film 224, and a nitride insulating film 225. A protective membrane 226 is formed.
[0217] The transistor 250 described in this embodiment includes an oxide semiconductor film 218. In addition, part of the oxide semiconductor film 218 functions as a channel region. The oxide insulating film 223 is formed in contact with the insulating film 218. An oxide insulating film 224 is formed so as to cover the insulating film 223.
[0218] The oxide semiconductor film 218 is typically an In-M-Zn oxide (wherein M is Al, Ti, Ga , Y, Zr, La, Cs, Nd, or Hf).
[0219] Metal elements of sputtering targets used to deposit In-M-Zn oxide films The atomic ratio preferably satisfies In≧M and Zn≧M. The atomic ratio of the target metal elements is In:M:Zn=1:1:1, In:M:Zn= 3:1:2 is preferred.
[0220] When the oxide semiconductor film 218 is an In-M-Zn oxide film, the sum of In and M is 10 When the atomic percentage of In and M is 0, the atomic percentage of In and M is also is In 25 atomic % or more, M is less than 75 atomic %, or In is 34 atomic % or more. omic% or more, and M less than 66 atomic%.
[0221] The oxide semiconductor film 218 has an energy gap of 2 eV or more, or 2.5 eV or more. In this way, the energy gap of the oxide semiconductor is wide. This allows the off-state current of the transistor 250 to be reduced.
[0222] The thickness of the oxide semiconductor film 218 is 3 nm to 200 nm, or nm or less, or between 3 nm and 50 nm.
[0223] The oxide semiconductor film 218 was formed using the sputtering target described in Embodiment 1. It is preferable to form a Zn-Zn alloy having an atomic ratio of In:M:Zn=1:1:1.05 or more. A sputtering target having a refractive index of 1.5 or less can be used. In the oxide semiconductor film 218 formed using the sputtering target, The atomic ratio of M and the atomic ratio of Zn to In are compared with those of the sputtering target. and becomes smaller.
[0224] The In-Ga-Zn oxide film formed using such a sputtering target has the following properties: It has a homologous structure.
[0225] As the oxide semiconductor film 218, an oxide semiconductor film with low carrier density is used. For example, The oxide semiconductor film 218 has a carrier density of 1×1017 pieces / cm 3 Less than or equal to 1×1 0 15 pieces / cm 3 or less, or 1×10 13 pieces / cm 3 or less, or 1×10 11 pcs / c m 3 The following oxide semiconductor film is used.
[0226] In addition, the semiconductor characteristics and electrical characteristics (field effect) of the required transistors are not limited to these. It is sufficient to use a material with an appropriate composition according to the required properties (e.g., the resultant mobility, threshold voltage, etc.). In order to obtain semiconductor characteristics of a transistor, the carrier density and impurity of the oxide semiconductor film 218 are controlled. The concentration of metals, defect density, atomic ratio of metal elements to oxygen, interatomic distance, density, etc. are appropriately adjusted. It is preferable.
[0227] Note that the oxide semiconductor film 218 is an oxide semiconductor having a low impurity concentration and a low density of defect states. By using a conductive film, it is possible to fabricate a transistor with even better electrical characteristics. In addition, the highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor film is preferably an off-type oxide semiconductor film. The current is extremely small, and the channel width is 1×10 6 μm and the channel length L is 10 μm. However, the voltage between the source and drain electrodes (drain voltage) is in the range of 1V to 10V. The off-state current is below the measurement limit of the semiconductor parameter analyzer, that is, 1×10 - 13 Therefore, the oxide semiconductor film has a channel region of 0.1 μm or less. The transistor in which this is formed has small fluctuations in electrical characteristics and is highly reliable. There may be cases where this occurs.
[0228] Hydrogen contained in the oxide semiconductor film reacts with oxygen that is bonded to metal atoms to form water. Oxygen vacancies are formed in the lattice from which oxygen has been removed (or in the portion from which oxygen has been removed). When hydrogen enters the gap, electrons, which act as carriers, can be generated. When it bonds with oxygen, which bonds with metal atoms, it can generate electrons, which act as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen has normally-on characteristics. It is easy to become.
[0229] For this reason, it is preferable that the amount of hydrogen in the oxide semiconductor film 218 be reduced as much as possible. Specifically, the oxide semiconductor film 218 was analyzed by secondary ion mass spectrometry (SIMS). Hydrogen concentration obtained by ondary ion mass spectrometry 5 × 10 19 atoms / cm 3 or less, or 1×10 19 atoms / cm 3 below , 5×10 18 atoms / cm 3 or less, or 1×10 18 atoms / cm 3 below, or 5×10 17 atoms / cm 3 or less, or 1×10 16 atoms / cm 3 Below Below.
[0230] The oxide semiconductor film 218 contains silicon or carbon, which is one of the Group 14 elements. As a result, oxygen vacancies increase in the oxide semiconductor film 218, causing the oxide semiconductor film 218 to become n-type. The concentrations of silicon and carbon in the nitride semiconductor film 218 (obtained by secondary ion mass spectrometry) The concentration of 18 atoms / cm3 or less, or 2×10 17 atoms / c m 3 The following applies.
[0231] In addition, in the oxide semiconductor film 218, an alkali metal ion was obtained by secondary ion mass spectrometry. The concentration of metal or alkaline earth metal is 1×10 18 atoms / cm 3 Less than or equal to 2 ×10 16 atoms / cm 3 The alkali metals and alkaline earth metals are oxidized When they combine with semiconductors, they can generate carriers, increasing the off-state current of transistors. For this reason, the alkali metal or alkaline earth metal of the oxide semiconductor film 218 may be It is preferable to reduce the concentration of metalloids.
[0232] When the oxide semiconductor film 218 contains nitrogen, electrons serving as carriers are generated, and The carrier density increases and it becomes easier to make the material n-type. Therefore, the transistor having the oxide semiconductor film tends to be normally on. In this case, it is preferable that the nitrogen content is reduced as much as possible. For example, in the case of secondary ion mass spectrometry, The nitrogen concentration obtained is 5×10 18 atoms / cm 3 It is preferable to do the following: .
[0233] The oxide semiconductor film 218 is formed according to the film formation model described in Embodiment 2. The oxide semiconductor film 218 may have a non-single crystal structure. CAAC-OS (C Axis Aligned Crystalline O xide semiconductor), polycrystalline structure, microcrystalline structure, and amorphous structure Among non-single crystal structures, the amorphous structure has the highest density of defect states, and CAAC-OS has Therefore, the oxide semiconductor film 218 is a CAAC-OS film. is preferred.
[0234] Note that the oxide semiconductor film 218 may have an amorphous structure, a microcrystalline structure, or a polycrystalline structure. A mixed film having two or more of the following regions may be used: a region of a CAAC-OS structure, a region of a single crystal structure, and a region of a crystalline structure. The mixed film may have, for example, an amorphous structure region, a microcrystalline structure region, a polycrystalline structure region, a CA In the case of a single-layer structure having two or more regions of either AC-OS or single crystal structure In addition, the mixed film may have an amorphous structure region, a microcrystalline structure region, a polycrystalline structure region, etc. A laminated structure of two or more of the following regions: a CAAC-OS region, a single crystal structure region, There may be cases where this is the case.
[0235] In the transistor 250 described in this embodiment, The oxide insulating film 223 is formed as shown in FIG. A velum 224 is formed.
[0236] The oxide insulating film 223 is an oxygen-permeable oxide insulating film. 3 is a graph showing the effect of preventing damage to the oxide semiconductor film 218 when forming the oxide insulating film 224 to be formed later. It also functions as a pressure relief film.
[0237] The oxide insulating film 223 has a thickness of 5 nm to 150 nm, or A silicon oxide film, a silicon oxynitride film, or the like having a thickness of 0 nm or less can be used. In the specification, a silicon oxynitride film is a film having a composition in which the oxygen content is higher than that of nitrogen. A silicon nitride oxide film is a film that contains more nitrogen than oxygen. This refers to a thin membrane.
[0238] The oxide insulating film 223 preferably has few defects. The signal at g = 2.001 originating from the silicon dangling bond is The density is 3×10 17 spins / cm 3 This is because the oxide insulating If the insulating film 223 contains a large number of defects, oxygen will bind to the defects, resulting in an oxide insulating film. This is because the amount of oxygen permeating through the film 223 decreases.
[0239] In addition, the number of defects at the interface between the oxide insulating film 223 and the oxide semiconductor film 218 is small. Typically, the oxide semiconductor film 218 is found to have a defect-derived morphology by ESR measurement. The spin density of the signal appearing at g=1.93 is 1×10 17 spins / cm 3 Further details are below. is preferably below the lower limit of detection.
[0240] An oxide insulating film 224 is formed in contact with the oxide insulating film 223. The film 224 is formed by using an oxide insulating film containing more oxygen than the oxygen that satisfies the stoichiometric composition. The oxide insulating film containing more oxygen than the stoichiometric composition is heated. A part of oxygen is released. Oxides containing more oxygen than the stoichiometric composition. The insulating film had a loss of oxygen of 1.0×10 in terms of oxygen atoms as determined by TDS analysis. 18 at oms / cm 3 or more than 3.0×1020 atoms / cm 3 More than 100% oxide insulation It is a membrane.
[0241] The oxide insulating film 224 has a thickness of 30 nm or more and 500 nm or less, or Silicon oxide, silicon oxynitride, etc., having a thickness of 400 nm or less can be used.
[0242] The oxide insulating film 224 preferably has few defects. The signal at g = 2.001 originating from the silicon dangling bond is The density is 1.5×10 18 spins / cm 3 Less than or even 1×10 18 spins / c m 3 Note that the oxide insulating film 224 has a thickness smaller than that of the oxide insulating film 223. Since the oxide insulating film 223 is located farther away from the oxide semiconductor film 218, the defect density is lower than that of the oxide insulating film 223. More is better.
[0243] Other configuration details of transistor 250 are described below.
[0244] There is no particular restriction on the material of the substrate 211, but it should be strong enough to withstand the subsequent heat treatment. For example, glass substrates, ceramic substrates, quartz substrates, and sa A fire substrate or the like may be used as the substrate 211. Also, silicon, silicon carbide, etc. Single crystal semiconductor substrates, polycrystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium, It is also possible to use SOI substrates, etc., and semiconductor elements are provided on these substrates. The substrate 211 may be a glass substrate. Combined, 6th generation (1500mm x 1850mm), 7th generation (1870mm x 2200mm ), 8th generation (2200mm x 2400mm), 9th generation (2400mm x 2800mm ), 10th generation (2950mm x 3400mm) and other large area substrates, A display device can be fabricated.
[0245] In addition, a flexible substrate is used as the substrate 211, and the transistor 25 is directly formed on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 211 and the transistor 250. The release layer is preferably removed from the substrate 211 after a semiconductor device is partially or entirely completed thereon. The transistor 250 can be separated and used for transfer to another substrate. It can also be transferred to substrates with poor thermal properties or flexible substrates.
[0246] The gate electrode 215 may be made of any of a variety of materials including aluminum, chromium, copper, tantalum, titanium, molybdenum, and tantalum. or an alloy containing the above-mentioned metal elements, The alloy may be formed by combining the above metal elements. The metal element may be selected from one or more of the following: The electrode 215 may have a single-layer structure or a laminated structure of two or more layers. A single-layer structure of an aluminum film containing titanium, a two-layer structure of a titanium film laminated on an aluminum film, and a titanium nitride structure. A two-layer structure in which a titanium film is laminated on a tungsten film, and a two-layer structure in which a tungsten film is laminated on a titanium nitride film A two-layer structure in which a tungsten film is laminated on a tantalum nitride film or a tungsten nitride film. The structure is a titanium film, an aluminum film is laminated on the titanium film, and a titanium film is laminated on top of that. There are also three-layer structures that can be formed using aluminum, titanium, tantalum, tungsten, Combination of one or more elements selected from molybdenum, chromium, neodymium, and scandium Alternatively, an alloy film or a nitride film may be used.
[0247] The gate electrode 215 may be made of indium tin oxide or indium containing tungsten oxide. Oxide, indium zinc oxide with tungsten oxide, indium oxide with titanium oxide Indium tin oxide, indium zinc oxide, silicon oxide, etc. A light-transmitting conductive material such as doped indium tin oxide can also be used. Alternatively, the conductive material having light-transmitting properties and the metal element may be laminated together.
[0248] The gate insulating film 217 is made of, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, Silicon nitride, aluminum oxide, hafnium oxide, gallium oxide or Ga-Zn-based gold Metal oxides or the like may be used, and the layer may be a laminate or a single layer.
[0249] The gate insulating film 217 is made of hafnium silicate (HfSiO x ), nitrogen is added Added hafnium silicate (HfSi x O y N z ), hafnium aluminium doped with nitrogen Luminate (HfAl x O y N z ), hafnium oxide, yttrium oxide and other high The use of -k materials can reduce gate leakage of transistors.
[0250] The thickness of the gate insulating film 217 is 5 nm or more and 400 nm or less, or 10 nm or more and 300 It is preferable to set the thickness to 50 nm or less, or 50 nm to 250 nm.
[0251] The pair of electrodes 221 and 222 are made of a conductive material such as aluminum, titanium, chromium, or nickel. Kel, copper, yttrium, zirconium, molybdenum, silver, tantalum, or tungsten A single metal consisting of arsenic or an alloy consisting mainly of this metal is used in a single-layer structure or a multilayer structure. For example, a single-layer structure of an aluminum film containing silicon, a titanium film on an aluminum film, A two-layer structure in which a titanium film is laminated on a tungsten film, a two-layer structure in which a copper-magnesium film is laminated on a tungsten film, A two-layer structure in which a copper film is laminated on a titanium-aluminum alloy film, a titanium film or a titanium nitride film, An aluminum film or a copper film is laminated on the titanium film or the titanium nitride film, and further A three-layer structure in which a titanium film or titanium nitride film is formed on top of the molybdenum film or molybdenum nitride film A molybdenum film and an aluminum film or A three-layer structure in which a copper film is laminated and a molybdenum film or molybdenum nitride film is further formed on top of the copper film. It should be noted that transparent conductive materials containing indium oxide, tin oxide, or zinc oxide may also be used. good.
[0252] Further, oxygen, hydrogen, water, an alkali metal, an alkaline earth metal, or the like may be added to the oxide insulating film 224. By providing the nitride insulating film 225 having a blocking effect such as 8 to the outside and hydrogen, water, etc. to enter the oxide semiconductor film 218 from the outside. The nitride insulating film can be made of silicon nitride, silicon oxynitride, aluminum nitride, etc. Aluminum, aluminum oxide, etc. In addition, oxygen, hydrogen, water, alkali metals, aluminum Instead of a nitride insulating film with a blocking effect of potassium earth metals, etc., oxygen, hydrogen, water, etc. An oxide insulating film having a blocking effect against oxygen, hydrogen, water, etc. may be provided. Examples of the oxide insulating film having a blocking effect include aluminum oxide, aluminum oxynitride, and oxide. Gallium oxide, gallium oxynitride, yttrium oxide, yttrium oxynitride, hafnium oxide Examples include hafnium oxide and hafnium nitride.
[0253] Next, a method for manufacturing the transistor 250 shown in FIG. 22 will be described with reference to FIG. .
[0254] As shown in FIG. 23(A), a gate electrode 215 is formed on a substrate 211. A gate insulating film 217 is formed on the substrate 15 .
[0255] Here, a glass substrate is used as the substrate 211.
[0256] The method of forming the gate electrode 215 will be described below. First, the sputtering method, the CVD method, A conductive film is formed by a deposition method or the like, and a mask is formed on the conductive film by a photolithography process. Next, a part of the conductive film is etched using the mask to form a gate electrode 215. After that, the mask is removed.
[0257] The gate electrode 215 may be formed by electrolytic plating, printing, inkjet printing, or the like instead of the above-mentioned method. It may be formed by a jet method or the like.
[0258] Here, a tungsten film having a thickness of 100 nm is formed by sputtering. A mask is formed by a photolithography process, and a tungsten film is formed using the mask. A gate electrode 215 is formed by dry etching.
[0259] The gate insulating film 217 is formed by a sputtering method, a CVD method, a vapor deposition method, or the like.
[0260] In addition, when a gallium oxide film is formed as the gate insulating film 217, MOCVD (Me Al Organic Chemical Vapor Deposition (ACVD) method It can be formed by
[0261] Here, the gate insulating film 217 is a silicon nitride film having a thickness of 400 nm and a SiO 2 film having a thickness of 50 A silicon oxynitride film having a thickness of nm is formed by laminating the film using the plasma CVD method.
[0262] Next, as shown in FIG. 23B, an oxide semiconductor film 218 is formed on the gate insulating film 217. Complete.
[0263] A method for forming the oxide semiconductor film 218 will be described below. Then, an oxide semiconductor film that becomes the oxide semiconductor film 218 is formed. After a mask is formed by a photolithography process, a part of the oxide semiconductor film is By etching the portion, as shown in FIG. 23(B), Then, an oxide semiconductor film 218 is formed to be isolated from the gate electrode 215 so as to overlap with a part of the gate electrode 215. After that, the mask is removed.
[0264] The oxide semiconductor film that will become the oxide semiconductor film 218 later can be formed by a sputtering method, a coating method, a pulsation method, or the like. The thin film can be formed by using a laser deposition method, a laser ablation method, or the like.
[0265] Here, the film formation apparatus shown in the third embodiment has a sputtering chamber as a film formation chamber. The oxide semiconductor film is formed by a sputtering method using a deposition apparatus that can form an oxide semiconductor film. The sputtering target manufactured according to the first embodiment is placed in the sputtering chamber. It is being done.
[0266] The sputtering gas is a rare gas (typically argon), oxygen, or a mixture of a rare gas and oxygen. In the case of a mixture of rare gas and oxygen, the amount of oxygen gas is appropriately adjusted relative to the amount of rare gas. A higher ratio is preferred.
[0267] In order to obtain a highly pure intrinsic or substantially highly pure intrinsic oxide semiconductor film, Not only is it necessary to evacuate the inside of the chamber to a high vacuum, but it is also necessary to highly purify the sputtering gas. The oxygen and argon gases used for this purpose must have a dew point of -40°C or less, or -80°C or less. By using gas highly purified to below -100℃ or below -120℃, This makes it possible to prevent moisture and the like from being taken into the semiconductor film as much as possible.
[0268] Here, the atomic ratio of In:Ga:Zn is 1:1:1.05. A 35-nm-thick In-GaAs oxide semiconductor film was deposited by sputtering using a target. A-Zn oxide film is formed. Next, a mask is formed on the oxide semiconductor film, and the oxide semiconductor The oxide semiconductor film 218 is formed by selectively etching part of the film.
[0269] Next, as shown in FIG. 23(C), a pair of electrodes 221 and 222 are formed.
[0270] The method for forming the pair of electrodes 221 and 222 will be described below. First, the sputtering method, C A conductive film is formed by a VD method, a vapor deposition method, or the like. Next, a photolithography process is performed on the conductive film. Next, the conductive film is etched using the mask to form a pair of electrodes 22. 1, 222 are formed. After this, the mask is removed.
[0271] Here, a tungsten film having a thickness of 50 nm, an aluminum film having a thickness of 400 nm, and a A titanium film having a thickness of 100 nm is then laminated on the titanium film by sputtering. A mask is formed by a photolithography process, and a tungsten film and an aluminum film are formed by using the mask. The aluminum film and the titanium film are dry etched to form a pair of electrodes 221 and 222. do.
[0272] Next, as shown in FIG. 23D, the oxide semiconductor film 218 and the pair of electrodes 221 and 22 The oxide insulating film 223 is formed over the oxide insulating film 223. Form 24.
[0273] The oxide insulating film 223 is made of a silicon oxide film placed in a processing chamber of a plasma CVD apparatus that has been evacuated to a vacuum. The substrate is maintained at a temperature of 280°C to 400°C, and a source gas is introduced into the processing chamber. The pressure in the chamber must be between 20 Pa and 250 Pa, or between 100 Pa and 250 Pa. Depending on the conditions for supplying high frequency power to an electrode provided in the processing chamber, the oxide insulating film 223 is A silicon oxide film or a silicon oxynitride film can be formed by using the above-mentioned method.
[0274] The source gas for the oxide insulating film 223 is a deposition gas containing silicon and an oxidizing gas. Representative examples of deposition gases containing silicon include silane and disilane. , trisilane, fluorinated silane, etc. Oxidizing gases include oxygen, ozone, dinitrogen monoxide, etc. Examples include nitrogen dioxide and nitrogen oxide.
[0275] By using the above conditions, an oxide insulating film that transmits oxygen is formed as the oxide insulating film 223. By providing the oxide insulating film 223, the oxide insulating film 223 can be formed later. In the process of forming the insulating film 224, damage to the oxide semiconductor film 218 can be reduced. As a result, the amount of oxygen vacancies in the oxide semiconductor film can be reduced.
[0276] Under the above film formation conditions, by setting the substrate temperature to the above temperature, the bonding strength of silicon and oxygen As a result, the oxide insulating film 223 becomes oxygen-permeable, dense, and hard. A thin oxide insulating film, typically etched with 0.5% by weight hydrofluoric acid at 25°C. A silicon oxide film or silicon oxynitride film having a deposition rate of 10 nm / min or less, or 8 nm / min or less. A silicon film can be formed.
[0277] Here, the oxide insulating film 223 is formed by using silane at a flow rate of 30 sccm and SiO2 at a flow rate of 4000 s. The source gas was nitrous oxide (N2O) at 1.0 ccm, the pressure in the processing chamber was 200 Pa, and the substrate temperature was 220° C. A 27.12 MHz high-frequency power source was used to supply 150 W of high-frequency power to the parallel plate electrodes. A silicon oxynitride film with a thickness of 50 nm is formed by the plasma CVD method using the above conditions. In this way, a silicon oxynitride film through which oxygen is transmitted can be formed.
[0278] The oxide insulating film 224 is made of a silicon oxide film placed in a processing chamber of a plasma CVD apparatus that has been evacuated to a vacuum. The substrate is then held at a temperature between 180°C and 280°C, or between 200°C and 240°C, and processed. A raw material gas is introduced into the chamber to set the pressure in the processing chamber at 100 Pa or more and 250 Pa or less, or The pressure is between 100 Pa and 200 Pa, and the pressure applied to the electrodes in the treatment chamber is 0.17 W / cm 2 Below Upper 0.5W / cm 2 or less than 0.25W / cm2 More than 0.35W / cm 2 Below high frequency Depending on the conditions for supplying the wave power, a silicon oxide film or a silicon oxynitride film is formed.
[0279] The source gas for the oxide insulating film 224 is a deposition gas containing silicon and an oxidizing gas. Representative examples of deposition gases containing silicon include silane and disilane. , trisilane, fluorinated silane, etc. Oxidizing gases include oxygen, ozone, dinitrogen monoxide, etc. Examples include nitrogen dioxide and nitrogen oxide.
[0280] Here, the oxide insulating film 224 is formed by using silane at a flow rate of 200 sccm and The source gas was dinitrogen monoxide at a flow rate of 100 sccm. The pressure in the processing chamber was set to 200 Pa, and the substrate temperature was set to 220 ℃, and a 27.12MHz high-frequency power source was used to apply 1500W of high-frequency power to parallel plate electrodes. A silicon oxynitride film having a thickness of 400 nm is formed by plasma CVD using a gas supplied to the substrate. The plasma CVD device has an electrode area of 6000 cm 2 Parallel plate plasma CV D equipment, and the power supplied is converted to power per unit area (power density) of 0.25 W / cm 2 It is.
[0281] Next, a heat treatment is performed. The temperature of the heat treatment is typically 250° C. or higher but not higher than the substrate distortion point. or 300°C or higher and 550°C or lower, or 350°C or higher and 510°C or lower.
[0282] The heat treatment can be performed using an electric furnace, an RTA device, or the like. Therefore, heat treatment can be performed at a temperature above the distortion point of the substrate for a short period of time. The processing time can be reduced.
[0283] Heat treatment is carried out in nitrogen, oxygen, or ultra-dry air (water content less than 20 ppm, or less than 1 ppm) or less than 10 ppb of air), or an atmosphere of rare gas (argon, helium, etc.) In addition, if the nitrogen, oxygen, ultra-dry air, or rare gas contains hydrogen, water, etc. It is preferable that this not be the case.
[0284] The heat treatment apparatus used in the heat treatment is the substrate heating chamber 400 shown in the third embodiment. The heating mechanism provided in 5 can be used appropriately.
[0285] By this heat treatment, part of oxygen contained in the oxide insulating film 224 is oxidized to the oxide semiconductor film 21 8, the amount of oxygen vacancies in the oxide semiconductor film 218 can be further reduced. do.
[0286] When the oxide insulating film 223 and the oxide insulating film 224 contain water, hydrogen, or the like, A nitride insulating film 225 having a function of blocking elements is formed later, and a heat treatment is performed. Water, hydrogen, and the like contained in the oxide insulating film 223 and the oxide insulating film 224 are absorbed by the oxide semiconductor The oxide semiconductor film 218 is then moved to the oxide semiconductor film 218, causing defects in the oxide semiconductor film 218. Water, hydrogen, and the like contained in the oxide insulating film 223 and the oxide insulating film 224 are released by heat. This reduces the variation in the electrical characteristics of the transistor 250 and also reduces the threshold. Therefore, fluctuations in the low voltage can be suppressed.
[0287] Note that the oxide insulating film 224 is formed over the oxide insulating film 223 under heating. Since oxygen can be transferred to the oxide semiconductor film 218, the heat treatment is not required. It would be good.
[0288] Here, heat treatment is performed in a nitrogen and oxygen atmosphere at 350° C. for 1 hour.
[0289] Next, a nitride insulating film 225 is formed by sputtering, CVD or the like.
[0290] When the nitride insulating film 225 is formed by the plasma CVD method, The substrate placed in the evacuated processing chamber is heated to 300°C to 400°C or 320°C. A temperature of 370° C. or higher is preferable because a dense nitride insulating film can be formed by the temperature control.
[0291] Here, silane at a flow rate of 50 sccm and 5000 The source gases were nitrogen at a flow rate of 100 sccm and ammonia at a flow rate of 100 sccm. The pressure in the processing chamber was The pressure was set at 100 Pa, the substrate temperature was set at 350°C, and a 27.12 MHz high frequency power source was used for 1000 A 50 nm thick nitride film was formed by plasma CVD using a 1000 MHz high frequency power supply to parallel plate electrodes. A silicon film is formed. The plasma CVD device has an electrode area of 6000 cm. 2 It is flat This is a horizontal and flat type plasma CVD device, and the supplied power is expressed as power per unit area (power density ) is converted to 1.7 × 10 -1 W / cm 2 It is.
[0292] Through the above steps, the oxide insulating film 223, the oxide insulating film 224, and the nitride insulating film 22 5, a protective film 226 can be formed.
[0293] Next, a heat treatment may be performed. The temperature of the heat treatment is typically 300° C. or higher and 40° C. or lower. The temperature must be below 0℃, or between 320℃ and 370℃.
[0294] Through the above steps, the transistor 250 can be manufactured.
[0295] From the above, it is possible to provide a semiconductor device including an oxide semiconductor film, in which the amount of defects is reduced. In addition, the electrical characteristics of a semiconductor device including an oxide semiconductor film can be improved. The above semiconductor device can be obtained.
[0296] <Modification 1, Regarding the Undercoat Insulating Film> In the transistor 250 shown in this embodiment, the substrate 211 and the gate A base insulating film can be provided between the gate electrode 215. The base insulating film can be made of an oxide. Silicon, silicon oxynitride, silicon nitride, silicon nitride oxide, gallium oxide, gallium oxide Examples include fluorine oxide, yttrium oxide, aluminum oxide, and aluminum oxynitride. The materials for the base insulating film are silicon nitride, gallium oxide, hafnium oxide, and yttrium oxide. By using lithium, aluminum oxide, etc., impurities, typically alkali, are removed from the substrate 211. Diffusion of lithium metals, water, hydrogen, and the like into the oxide semiconductor film 218 can be suppressed.
[0297] The base insulating film can be formed by a sputtering method, a CVD method, or the like.
[0298] <Modification 2: Gate insulating film> In the transistor 250 described in this embodiment, the gate insulating film 217 may be formed as needed. can be a laminated structure.
[0299] The gate insulating film 217 is a nitride insulating film and an oxide insulating film, which are arranged in this order from the gate electrode 215 side. The nitride insulating film may be provided on the gate electrode 215 side. As a result, impurities from the gate electrode 215, typically hydrogen, nitrogen, alkali metals, or This can prevent the alkaline earth metal and the like from moving to the oxide semiconductor film 218.
[0300] In addition, by providing an oxide insulating film on the oxide semiconductor film 218 side, The defect state density at the interface between the oxide semiconductor film 218 and the oxide semiconductor film 219 can be reduced. As a result, a transistor with little deterioration in electrical characteristics can be obtained. Like the oxide insulating film 224, the oxide insulating film 224 contains more oxygen than the stoichiometric composition. When the oxide insulating film is used, a gate insulating film 217 is formed at the interface between the gate insulating film 217 and the oxide semiconductor film 218. This is more preferable since it is possible to further reduce the defect state density in the semiconductor layer.
[0301] The gate insulating film 217 is made of a nitride insulating film with few defects and a high hydrogen blocking property. A laminated structure in which a thin nitride insulating film and an oxide insulating film are laminated in this order from the gate electrode 215 side. By providing a nitride insulating film with few defects as the gate insulating film 217, As a result, the dielectric strength of the gate insulating film 217 can be improved. By providing a nitride insulating film with high adhesion, the gate electrode 215 and the nitride insulating film with few defects can be formed. Hydrogen from the film can be prevented from transferring to the oxide semiconductor film 218.
[0302] The gate insulating film 217 is made of a nitride insulating film having a high impurity blocking property and a gate insulating film having a high defect blocking property. a nitride insulating film having a low hydrogen blocking property, a nitride insulating film having a high hydrogen blocking property, and an oxide insulating film, The gate insulating film 21 may have a laminated structure in which the gate insulating film 21 is laminated in order from the gate electrode 215 side. 7, a nitride insulating film having high impurity blocking properties is provided, Impurities from 5, typically hydrogen, nitrogen, alkali metals, alkaline earth metals, etc. The transfer to the oxide semiconductor film 218 can be prevented.
[0303] <Modification 3: Pair of Electrodes> As a pair of electrodes 221 and 222 provided in the transistor 250 shown in this embodiment, , tungsten, titanium, aluminum, copper, molybdenum, chromium, or tantalum alone It is preferable to use a conductive material that easily bonds with oxygen, such as an alloy. The oxygen contained in the semiconductor film 218 is bonded to the conductive material contained in the pair of electrodes 221 and 222. As a result, oxygen vacancy regions are formed in the oxide semiconductor film 218. In the case where a part of the constituent elements of the conductive material forming the pair of electrodes 221 and 222 is mixed into the film 218, As a result, in the oxide semiconductor film 218, a pair of Low resistance regions 220a and 220b are formed in the vicinity of the regions in contact with the electrodes 221 and 222. The low resistance regions 220a and 220b are in contact with a pair of electrodes 221 and 222, and are formed on the gate insulating film. 217 and a pair of electrodes 221 and 222. Since the oxide semiconductor film 218 has high electrical conductivity, the contact resistance between the oxide semiconductor film 218 and the pair of electrodes 221 and 222 is It is possible to reduce the on-state current of the transistor and increase the on-state current of the transistor.
[0304] <Modification 4: Oxide Semiconductor Film> In the method for manufacturing the transistor 250 described in this embodiment, After forming the oxide semiconductor film 2, the oxide semiconductor film 218 is exposed to plasma generated in an oxygen atmosphere to be oxidized. Oxygen can be supplied to the semiconductor film 218. The oxidizing atmosphere can be oxygen, ozone, In the plasma treatment, the substrate is subjected to the treatment with nitrous oxide or nitrogen dioxide. The oxide semiconductor film 218 is exposed to plasma generated without applying a bias to the 211 side. As a result, it is possible to prevent damage to the oxide semiconductor film 218 and to supply oxygen. Therefore, the amount of oxygen vacancies in the oxide semiconductor film 218 can be reduced. In addition, impurities remaining on the surface of the oxide semiconductor film 218 due to the etching treatment, such as For example, halogens such as fluorine and chlorine can be removed.
[0305] The configuration and method described in this embodiment may be applied to other embodiments and their modifications, as well as The present invention can be used in appropriate combination with the configurations and methods shown in the embodiments.
[0306] (Embodiment 5) In this embodiment, the number of defects in the oxide semiconductor film is further reduced compared to that in Embodiment 4. A semiconductor device having a transistor capable of implementing the above-mentioned method will be described with reference to the drawings. The transistor described in this embodiment has a structure similar to that of the transistor in Embodiment 4, in which an oxide semiconductor film and an oxide The difference is that it has a multilayer film having an oxide in contact with a nitride semiconductor film.
[0307] FIG. 25 illustrates a top view and a cross-sectional view of a transistor 260 included in the semiconductor device. FIG. 25(A) is a top view of a transistor 260, and FIG. 25(B) is a top view of a transistor 260 shown in FIG. FIG. 25(C) is a cross-sectional view taken along dashed line CD in FIG. 25(A). In addition, in FIG. 25(A), for the sake of clarity, the configuration of the substrate 211 and the transistor 260 is shown. A part of the element (for example, the gate insulating film 217), the oxide insulating film 223, and the oxide insulating film 224 , the nitride insulating film 225 and the like are omitted.
[0308] The transistor 260 shown in FIG. 25A to FIG. 25C has a gate insulating film 217 interposed therebetween. The multilayer film 220 overlaps the gate electrode 215, and the pair of electrodes 22 contact the multilayer film 220. The gate insulating film 217, the multilayer film 220, and the pair of electrodes 22 An oxide insulating film 223, an oxide insulating film 224, and a nitride insulating film 225 are formed over the first and second insulating films 222. A protective film 226 made of the above is formed.
[0309] In the transistor 260 described in this embodiment, the multilayer film 220 includes an oxide semiconductor film 2 The multilayer film 220 has a two-layer structure. A part of the semiconductor film 218 functions as a channel region. The oxide insulating film 223 is formed on the insulating film 224. In other words, an insulating film 224 is formed between the oxide semiconductor film 218 and the oxide insulating film 223. An oxide film 219 is provided on the insulating layer 214 .
[0310] The oxide film 219 is an oxide film formed of one or more elements constituting the oxide semiconductor film 218. Note that the oxide film 219 is a oxide semiconductor film containing at least one of the elements constituting the oxide semiconductor film 218. Since the oxide semiconductor film 218 and the oxide film 219 are formed from the top, Therefore, the movement of carriers is not hindered at the interface, and the The field effect mobility of the transistor is increased.
[0311] The oxide film 219 is typically made of In-Ga oxide, In-Zn oxide, or In-MnO. n-oxide (M is Al, Ti, Ga, Y, Zr, La, Cs, Nd or Hf) and The energy of the bottom of the conduction band is closer to the vacuum level than that of the oxide semiconductor film 218. , the energy of the bottom of the conduction band of the oxide film 219 and the energy of the bottom of the conduction band of the oxide semiconductor film 218 The difference in energy between the 0.15 eV or more and 2 eV or less, 1 eV or less, 0.5 eV or less, or 0.4 eV or less That is, the electron affinity of the oxide film 219 and the electron affinity of the oxide semiconductor film 218 are The difference is 0.05 eV or more, 0.07 eV or more, 0.1 eV or more, or 0.15 eV or more. and 2 eV or less, 1 eV or less, 0.5 eV or less, or 0.4 eV or less.
[0312] The oxide film 219 contains In, which increases the carrier mobility (electron mobility). preferable.
[0313] The oxide film 219 is made of Al, Ti, Ga, Y, Zr, La, Cs, Nd or Hf. By having a higher atomic ratio than In, the following effects may be obtained: (1) Oxide film (2) To increase the energy gap of the oxide film 219. (3) The insulating layer 214 is shielded from impurities from the outside. (5) Al, Ti, Ga, Y, Zr, La, Cs, Nd, or Hf is an acid. Because they have strong bonding strength with metals, Al, Ti, Ga, Y, Zr, La, Cs, and N By having d or Hf in a higher atomic ratio than In, oxygen vacancies are less likely to occur.
[0314] The oxide film 219 is an In-M-Zn oxide film (wherein M is Al, Ti, Ga, Y, Zr, La, In the case of In-M-Zn oxide films, the sputtering agent used to deposit the In-M-Zn oxide film is The atomic ratio of the metal elements in the deposition target preferably satisfies M>In and Zn>M. The atomic ratio of the metal elements in such a sputtering target is In:Ga:Z. n=1:3:4, In:Ga:Zn=1:3:5, In:Ga:Zn=1:3:6, In :Ga:Zn=1:3:7, In:Ga:Zn=1:3:8, In:Ga:Zn=1:3 :9, In:Ga:Zn=1:3:10, In:Ga:Zn=1:4:5, In:Ga: Zn=1:4:6, In:Ga:Zn=1:4:7, In:Ga:Zn=1:4:8, I n:Ga:Zn=1:4:9, In:Ga:Zn=1:4:10, In:Ga:Zn=1 :5:6, In:Ga:Zn=1:5:7, In:Ga:Zn=1:5:8, In:Ga :Zn=1:5:9, In:Ga:Zn=1:5:10, In:Ga:Zn=1:6:7 , In:Ga:Zn=1:6:8, In:Ga:Zn=1:6:9, In:Ga:Zn= A ratio of 1:6:10 is preferred.
[0315] When the oxide film 219 is an In-M-Zn oxide film, the sum of In and M is 10 When the atomic percentage of In is 0, the atomic ratio of In to M is 50 atomic%. c% or less, M is 50 atomic% or more, or In is less than 25 atomic%, M is Must be 75 atomic% or more.
[0316] The oxide semiconductor film 218 and the oxide film 219 are In-M-Zn oxide films (M is A In the case of ZnO, Ti, Ga, Y, Zr, La, Cs, Nd or Hf, the oxide semiconductor film 21 In comparison with 8, the M (Al, Ti, Ga, Y, Zr, La, Cs) contained in the oxide film 219 is , Nd, or Hf) is present in the oxide semiconductor film 218. The atomic ratio is 1.5 times or more, 2 times or more, or 3 times or more higher than the above atoms. be.
[0317] The oxide semiconductor film 218 and the oxide film 219 are In-M-Zn oxide films (M is A In the case of ZnO, Ti, Ga, Y, Zr, La, Cs, Nd or Hf, the oxide film 219 is The atomic ratio of n:M:Zn is x1:y1:z1, and the oxide semiconductor film 218 is In:M:Zn =x2:y2:z2 [atomic ratio], then y1 / x1 is greater than y2 / x2, and is y1 / x1 is 1.5 times greater than y2 / x2. Or, y1 / x1 is y2 / x 2 or y1 / x1 is more than three times greater than y2 / x2. In the oxide semiconductor film, when y2 is equal to or greater than x2, This is preferable because it can provide stable electrical characteristics to the transistor. However, y2 must be three times larger than x2. If the temperature exceeds this value, the field-effect mobility of a transistor including the oxide semiconductor film decreases. To avoid this, it is preferable that y2 is less than three times x2.
[0318] The oxide semiconductor film 218 was formed by a process similar to that of the oxide semiconductor film described in Embodiment 4. It can be used appropriately.
[0319] In addition, the oxide film 219 was formed using the sputtering target shown in Embodiment 1. It is preferable to form a Zn-Zn alloy having an atomic ratio of In:M:Zn=1:3:(3.05 or less than 10), or the atomic ratio of In:M:Zn=1 :6: (6.05 or more and 10 or less) can be used. In addition, the oxide film 219 formed using such a sputtering target contains The atomic ratios of M / In and Zn / In are determined based on the atomic ratios contained in the sputtering target. In addition, in the In-Ga-Zn oxide film, the ratio of the number of Zn atoms to M (Z n / M) is 0.5 or more.
[0320] By using such a sputtering target, a homologous structure It is possible to form an In-Ga-Zn oxide film having a CAAC-OS structure. .
[0321] The oxide film 219 is a semiconductor film used for forming the oxide insulating film 224 later. As a result, the oxide semiconductor film 218 also functions as a damage reducing film. Furthermore, by forming the oxide film 219, the amount of oxygen vacancies can be reduced. The insulating film to be formed over the oxide semiconductor film 218, for example, the oxide insulating film, is formed of the oxide semiconductor film 218. Therefore, the inclusion of these elements in the compound semiconductor film 218 can be suppressed.
[0322] The thickness of the oxide film 219 is set to 3 nm or more and 100 nm or less, or 3 nm or more and 50 nm or less. do.
[0323] Similarly to the oxide semiconductor film 218, the oxide film 219 may have a non-single crystal structure, for example. The non-single crystal structure may be, for example, the CAAC-OS shown in Embodiment 2, the polycrystalline structure, and the microcrystalline structure. Among non-single crystal structures, the amorphous structure has the lowest density of defect levels. The CAAC-OS has the highest defect density, and the CAAC-OS has the lowest defect density. Preferably it is AC-OS.
[0324] Note that the oxide semiconductor film 218 and the oxide film 219 are amorphous and microcrystalline regions, respectively. Two or more of the following: a crystal structure region, a polycrystalline structure region, a CAAC-OS region, and a single crystal structure region The mixed film may have, for example, an amorphous structure region, a microcrystalline structure region, and Two or more of the following regions: a region of polycrystalline structure, a region of CAAC-OS, and a region of single crystal structure In some cases, the mixed film has a monolayer structure with regions of amorphous structure, finely crystalline structure, etc. Crystal structure region, polycrystalline structure region, CAAC-OS region, or single crystal structure region In some cases, the oxide semiconductor film 218 and the oxide semiconductor film 220 may have a stacked structure. The oxide film 219 may have a stacked structure of a microcrystalline structure and a CAAC-OS structure in that order. The oxide semiconductor film 218 has a stacked structure of a microcrystalline structure and a CAAC-OS structure, and the oxide film 21 9 may be CAAC-OS.
[0325] When the oxide semiconductor film 218 and the oxide film 219 are both CAAC-OS, It is possible to improve the crystallinity at the interface between the solid film 218 and the oxide film 219, which is preferable. .
[0326] In the multilayer film 220, the gate electrode 215 is overlapped and a pair of electrodes 221 and 222 are formed. The region sandwiched between 22 is called a channel formation region. The region where the carriers mainly flow is called the channel region. The oxide semiconductor film 218 provided between the pair of electrodes 221 is a channel region. , 222 is called the channel length.
[0327] Here, the oxide film 219 is provided between the oxide semiconductor film 218 and the oxide insulating film 223. For this reason, impurities and Even if a trap state is formed due to the defects, the trap state and the oxide semiconductor film 218 As a result, electrons flowing through the oxide semiconductor film 218 are transported to the trap states. It is difficult to be captured, and it is possible to increase the on-current of the transistor. In addition, when an electron is captured in a trap level, the electron is transported to the This results in a shift in the threshold voltage of the transistor. However, since there is a gap between the oxide semiconductor film 218 and the trap states, It is possible to reduce the capture of electrons in the trap level, and the fluctuation of the threshold voltage is reduced. It can be reduced.
[0328] In addition, the oxide film 219 can block impurities from the outside. It is possible to reduce the amount of impurities that move from the oxide semiconductor film 218 to the oxide semiconductor film 218. For these reasons, the oxide semiconductor film 218 is not easily formed with oxygen vacancies. It is possible to reduce the concentration of impurities and the amount of oxygen vacancies.
[0329] Note that the oxide semiconductor film 218 and the oxide film 219 are not simply stacked but are formed continuously. A continuous junction (here, a structure in which the energy at the bottom of the conduction band changes continuously between each film) In other words, trap centers and recombination centers are formed at the interfaces of each film. The stacked structure is designed so that there are no impurities that would form defect levels such as those shown in the figure. When impurities are present between the oxide semiconductor film 218 and the oxide film 219, The continuity of the energy band is lost, and carriers are trapped or recombined at the interface, It disappears.
[0330] In order to form continuous junctions, a multi-chamber equipped with a load lock chamber as shown in the third embodiment is used. Using a multi-layer film-forming device, each film can be stacked continuously without being exposed to the air. It is necessary.
[0331] As shown in FIG. 25D, a transistor 265 is formed on the gate insulating film 217. A multilayer film 234 overlapping the electrode 215 and a pair of electrodes 221 and 222 in contact with the multilayer film 234. and
[0332] The multilayer film 234 includes an oxide film 231, an oxide semiconductor film 218, and an oxide film 219. That is, the multilayer film 234 has a three-layer structure. It functions as:
[0333] In addition, the gate insulating film 217 and the oxide film 231 are in contact with each other. An oxide film 231 is provided between the oxide semiconductor film 218 and the oxide semiconductor film 218 .
[0334] The multilayer film 234 and the oxide insulating film 223 are in contact with each other. In other words, the oxide semiconductor film 218 is in contact with the oxide insulating film 223. An oxide film 219 is provided on the insulating layer 214 .
[0335] The oxide film 231 is formed using a material and a method similar to those of the oxide film 219 described in Embodiment 4. It can be used as appropriate.
[0336] The oxide film 231 is thinner than the oxide semiconductor film 218, so that the transistor It is possible to reduce the amount of variation in the threshold voltage.
[0337] The transistor described in this embodiment has a gate insulating film 217 and an oxide semiconductor film 218. The oxide film 231 is provided between the oxide semiconductor film 218 and the oxide insulating film 223. Since the oxide film 219 is provided between the oxide film 231 and the oxide semiconductor film 218 The concentration of silicon or carbon in the vicinity of the interface with the oxide semiconductor film 218 The concentration of carbon or the concentration of silicon in the vicinity of the interface between the oxide film 219 and the oxide semiconductor film 218 This can reduce the concentration of fluorine and carbon.
[0338] The transistor 265 having such a structure includes a multilayer film 2 including an oxide semiconductor film 218. 34 has very few defects, which makes it possible to improve the electrical characteristics of transistors Typically, it is possible to increase the on-current and improve the field effect mobility. Threshold voltage in the BT stress test and the light BT stress test, which are examples of stress tests The fluctuation is small and the reliability is high.
[0339] The configuration and method described in this embodiment may be applied to other embodiments and their modifications, as well as The present invention can be used in appropriate combination with the configurations and methods shown in the embodiments.
[0340] (Embodiment 6) In this embodiment, a transistor having a structure different from those in the fourth and fifth embodiments is described. 26. The transistor 280 described in this embodiment is a transistor including an oxide semiconductor It is characterized by having a plurality of gate electrodes opposed to each other via a film.
[0341] The transistor 280 shown in FIG. 26 has a gate electrode 215 provided on a substrate 211. In addition, a gate insulating film 217 formed on the substrate 211 and the gate electrode 215 and a gate An oxide semiconductor film 218 overlapping with the gate electrode 215 with the gate insulating film 217 interposed therebetween; A pair of electrodes 221 and 222 are in contact with the semiconductor film 218. 17, an oxide insulating film 22 is formed over the oxide semiconductor film 218 and the pair of electrodes 221 and 222. 3. A protective film 226 consisting of an oxide insulating film 224 and a nitride insulating film 225 is formed. In addition, a gate electrode 281 overlapping with the oxide semiconductor film 218 with a protective film 226 interposed therebetween is provided. do.
[0342] The gate electrode 281 can be formed in the same manner as the gate electrode 215 shown in the fourth embodiment. Cut.
[0343] The transistor 280 described in this embodiment has a gate electrode facing the gate insulating film 218 therebetween. The gate electrode 215 and the gate electrode 281 are By applying different potentials, the threshold voltage of the transistor 280 can be controlled. do.
[0344] In addition, by using the oxide semiconductor film 218 in which the amount of oxygen vacancies is reduced, It is possible to improve electrical characteristics. In addition, the fluctuation of the threshold voltage is small, and reliability is high. This results in a high-performance transistor.
[0345] The configuration and method described in this embodiment may be applied to other embodiments and their modifications, as well as The present invention can be used in appropriate combination with the configurations and methods shown in the embodiments.
[0346] (Embodiment 7) In this embodiment, a transistor having a structure different from those in the fourth to sixth embodiments will be described. This will be explained with reference to FIG.
[0347] In this embodiment, compared with Embodiments 4 to 6, defects in an oxide semiconductor film can be reduced. A semiconductor device having a transistor capable of further reducing the amount of The transistor described in this embodiment will be described in the following. In contrast, the back channel side of the oxide semiconductor film 218 is covered with a protective film. The difference is that it is not exposed to the plasma generated in the etching process for forming the poles.
[0348] FIG. 27 illustrates a top view and a cross-sectional view of a transistor 290 included in the semiconductor device. FIG. 27(A) is a top view of a transistor 290, and FIG. 27(B) is a top view of a transistor 290 shown in FIG. FIG. 27(C) is a cross-sectional view taken along dashed line CD in FIG. 27(A). In FIG. 27A, for the sake of clarity, the configuration of the substrate 211 and the transistor 290 is shown. A part of the element (for example, the gate insulating film 217), the oxide insulating film 223, and the oxide insulating film 224 , the nitride insulating film 225 and the like are omitted.
[0349] The transistor 290 shown in FIG. 27 has a gate electrode 215 provided on a substrate 211. In addition, a gate insulating film 217 formed on the substrate 211 and the gate electrode 215 and a gate The gate electrode 215 includes an oxide semiconductor film 218 overlapping with the gate electrode 215 with the gate insulating film 217 interposed therebetween. In addition, an oxide insulating film 223 and an oxide semiconductor film 218 are formed over the gate insulating film 217 and the oxide semiconductor film 218. A protective film 226 is formed by an insulating film 224 and a nitride insulating film 225. A pair of electrodes 22 are formed and connected to the oxide semiconductor film 218 through the openings in the protective film 226. 1b, 222b.
[0350] Next, a method for manufacturing the transistor 290 will be described.
[0351] As in the fourth embodiment, a gate electrode 215 is formed on a substrate 211. A gate insulating film 217 is formed on the gate electrode 215. Next, an oxide film is formed on the gate insulating film 217. A compound semiconductor film 218 is formed.
[0352] Next, in a manner similar to that of Embodiment 4, a second insulating film 216 was formed on the gate insulating film 217 and the oxide semiconductor film 218. After the oxide insulating film 223 is formed while heating at a temperature of 20° C. to 400° C., the oxide insulating film After the oxide insulating film 224 is formed, a nitride insulating film 225 is formed. Heat treatment is performed to supply part of oxygen contained in the oxide insulating film 224 to the oxide semiconductor film 218. Provide.
[0353] Next, the oxide insulating film 223, the oxide insulating film 224, and the nitride insulating film 225 were A part of the oxide semiconductor film 218 is etched to form an opening that exposes a part of the oxide semiconductor film 218. Thereafter, the pair of electrodes 221b and 222b in contact with the oxide semiconductor film 218 are It is formed in the same way.
[0354] In this embodiment, when the pair of electrodes 221b and 222b are etched, the oxide Since the semiconductor film 218 is covered with the protective film 226, a pair of electrodes 221b and 222b are formed. The oxide semiconductor film 218, particularly the back surface of the oxide semiconductor film 218, is etched to form a The channel region is not damaged. Furthermore, the oxide insulating film 224 has a stoichiometric composition. The oxide insulating film contains more oxygen than the oxygen that fills the gap. Part of the oxygen contained in the oxide semiconductor film 224 is transferred to the oxide semiconductor film 218. The amount of oxygen vacancies contained in the alloy can be reduced.
[0355] Through the above steps, defects in the oxide semiconductor film 218 can be reduced. , the reliability of the transistor 290 can be improved.
[0356] The configuration and method described in this embodiment may be applied to other embodiments and their modifications, as well as The present invention can be used in appropriate combination with the configurations and methods shown in the embodiments.
[0357] (Embodiment 8) In this embodiment, a transistor having a structure different from those in the fourth to seventh embodiments will be described. This will be explained with reference to FIG.
[0358] In this embodiment, compared with Embodiments 4 to 7, defects in an oxide semiconductor film can be reduced. A semiconductor device having a transistor capable of further reducing the amount of The transistor described in this embodiment is a transistor including an oxide semiconductor The back channel side of the conductor film 218 is covered with a protective film, and a pair of electrodes is formed. The point that the semiconductor device is not exposed to plasma generated during the etching process is different from that of the fourth to seventh embodiments. is different.
[0359] FIG. 28 illustrates a top view and a cross-sectional view of a transistor 295 included in the semiconductor device. The transistor 295 shown in FIG. 28A is a channel protection transistor. FIG. 28(B) is a top view of the transistor 295, and FIG. 28(B) is a top view of the transistor 295 between the dashed line AB in FIG. 28(A). 28(C) is a cross-sectional view taken along dashed line CD in FIG. 28A, for clarity, the substrate 211 and some of the components of the transistor 295 are shown. (For example, the gate insulating film 217, etc.) are omitted.
[0360] The transistor 295 shown in FIG. 28 has a gate electrode 215 provided on a substrate 211. In addition, a gate insulating film 217 formed on the substrate 211 and the gate electrode 215 and a gate The gate electrode 215 has an oxide semiconductor film 218 overlapping therewith with a gate insulating film 217 interposed therebetween. In addition, an oxide insulating film 223a and an oxide semiconductor film 218 are formed over the gate insulating film 217 and the oxide semiconductor film 218. A protective film 226a is formed by a nitride insulating film 224a and a nitride insulating film 225a. A pair of electrodes 2 formed on the insulating film 217, the oxide semiconductor film 218, and the protective film 226a. 21c, 222c.
[0361] Next, a method for manufacturing the transistor 295 will be described.
[0362] As in the fourth embodiment, a gate electrode 215 is formed on a substrate 211. A gate insulating film 217 is formed on the gate electrode 215. Next, an oxide film is formed on the gate insulating film 217. A compound semiconductor film 218 is formed.
[0363] Next, in a manner similar to that of Embodiment 4, a second insulating film 216 was formed on the gate insulating film 217 and the oxide semiconductor film 218. After the oxide insulating film 223 is formed while heating at a temperature of 20° C. to 400° C., the oxide insulating film After the oxide insulating film 224 is formed, a nitride insulating film 225 is formed. Heat treatment is performed to supply part of oxygen contained in the oxide insulating film 224 to the oxide semiconductor film 218. Provide.
[0364] Next, the oxide insulating film 223, the oxide insulating film 224, and the nitride insulating film 225 were The oxide insulating film 223a, the oxide insulating film 224a, and the nitride insulating film 225 are partially etched. A protective film 226a is formed from the film 225a.
[0365] Next, the pair of electrodes 221c and 222c in contact with the oxide semiconductor film 218 are formed by the method described in Embodiment 4. The same is formed as above.
[0366] In this embodiment, when the pair of electrodes 221c and 222c are etched, the oxide Since the semiconductor film 218 is covered with the protective film 226a, the pair of electrodes 221c and 222c The oxide semiconductor film 218 is not damaged by the etching. The oxide insulating film 224a is an oxide insulating film containing more oxygen than the oxygen required for the stoichiometric composition. Therefore, part of the oxygen contained in the oxide insulating film 224a is converted to the oxide semiconductor The amount of oxygen vacancies in the oxide semiconductor film 218 can be reduced by transferring the oxygen vacancies to the oxide semiconductor film 218. do.
[0367] In FIG. 28, a nitride insulating film 225a is formed as the protective film 226a. Alternatively, the oxide insulating film 223a and the oxide insulating film 224a may have a stacked-layer structure. In this case, after forming the pair of electrodes 221c and 222c, the nitride insulating film 225a is formed. As a result, it is possible to prevent hydrogen, water, and the like from entering the oxide semiconductor film 218 from the outside. can be done.
[0368] Through the above steps, defects in the oxide semiconductor film 218 can be reduced. , the reliability of the transistor 295 can be improved.
[0369] (Embodiment 9) In this embodiment, a top-gate transistor and a manufacturing method thereof will be described. do.
[0370] 29A to 29C are top views and 29A is a top view of the transistor 400, and FIG. FIG. 29(C) is a cross-sectional view taken along the dashed line AB in FIG. 29(A), and FIG. 29(C) is a cross-sectional view taken along the dashed line AB in FIG. 29A is a cross-sectional view taken along dashed lines CD. For clarity, in FIG. 29A, the substrate 401 and the acid The oxide insulating film 413, some of the components of the transistor 400 (for example, the oxide film 423, the Port insulating film 425), insulating film 427, insulating film 429, etc. are omitted.
[0371] The transistor 400 illustrated in FIG. 29 is formed on an oxide insulating film 413 provided over a substrate 401. an oxide semiconductor film 411 provided over the oxide film 409; A pair of electrodes 415 and 416 in contact with the conductive film 411, an oxide insulating film 413, an oxide semiconductor The oxide film 423 is in contact with the film 411 and the pair of electrodes 415 and 416. The gate insulating film 425 is in contact with the oxide semiconductor film 411 and overlaps the oxide semiconductor film 411 with the gate insulating film 425 interposed therebetween. Note that the oxide film 409, the oxide semiconductor film 411, and the oxide The oxide film 423 is called a multilayer film 424. The gate insulating film 425 and the gate electrode 421 are The gate insulating film 427 may cover the gate insulating film 427, and the insulating film 429 may cover the gate insulating film 427. A pair of electrodes is formed in the openings 433 and 434 of the insulating films 425, 427, and 429. There may be wires 431, 432 in contact with the poles 415, 416.
[0372] Each component of the transistor 400 will be described below.
[0373] As the substrate 401, the substrate 211 described in Embodiment 4 can be used as appropriate.
[0374] The oxide insulating film 413 serving as a base insulating film can be made of silicon oxide, silicon oxynitride, or the like. Silicon nitride, silicon oxide nitride, gallium oxide, hafnium oxide, yttrium oxide Examples of the oxide that serves as the base insulating film include aluminum oxide and aluminum oxynitride. The insulating film 413 may be made of silicon nitride, gallium oxide, hafnium oxide, or yttrium oxide. By using aluminum oxide or the like, impurities, typically aluminum, are removed from the substrate 401. The diffusion of potassium metal, water, hydrogen, and the like into the oxide semiconductor film can be suppressed.
[0375] The oxide insulating film 413 contains more oxygen than the stoichiometric composition. That is, the insulating film can be formed using an oxide insulating film in which part of oxygen is released by heating. In this way, the oxide insulating film 413 can be formed. The oxygen contained in the oxide semiconductor film 411 is moved to the oxide insulating film 413, whereby the oxide semiconductor film 411 is formed. In addition, the defect states at the interface of the oxide semiconductor film 409 can be reduced. By filling the oxygen vacancies, it is possible to further reduce the oxygen vacancies.
[0376] The oxide film 409 and the oxide film 423 constituting the multilayer film 424 are formed by the oxide film 409 and the oxide film 423 of the oxide film 424 shown in Embodiment 5. The oxide semiconductor film 411 can be made of any of the materials for the oxide semiconductor films 219 and 231. The material of the oxide semiconductor film 218 described in Embodiment 5 can be used as appropriate.
[0377] The thickness of the oxide semiconductor film 411 is 3 nm or more and 200 nm or less, or 3 nm or more and 100 nm or less, or between 3 nm and 50 nm.
[0378] The thickness of the oxide film 409 and the oxide film 423 is 0.3 nm or more and 200 nm or less, and 3 nm The thickness of the oxide film 409 is set to 100 nm or more, or 3 nm or more and 50 nm or less. The thickness of the oxide film 423 is preferably larger than that of the oxide semiconductor film 411. It is preferable that the thickness of the oxide semiconductor film be thinner than that of the oxide semiconductor film 411.
[0379] When the oxide film 409 is too thin, the interface between the oxide film 409 and the oxide semiconductor film 411 Electrons are trapped in the oxide film 4, which reduces the on-state current of the transistor. When the thickness of the oxide insulating film 413 is too thick, oxygen moves from the oxide semiconductor film 411 to the oxide insulating film 413. As a result, it becomes difficult to reduce the amount of oxygen vacancies in the oxide semiconductor film 411. For this reason, the thickness of the oxide film 409 is set to be thicker than that of the oxide semiconductor film 411 and to be 20 nm or more. The thickness of the oxide film 423 is preferably 200 nm or less. The oxide film 409 is made thicker than the oxide semiconductor film 411. This is preferable because it makes it possible to manufacture a transistor with a small variation in threshold voltage.
[0380] When the oxide film 423 is a semiconductor, a large number of electrons are induced in the oxide film 423 . The oxide film 423 in which electrons are induced shields the electric field of the gate electrode 421, and the oxide semiconductor film 4 The electric field applied to 11 is weakened, resulting in a decrease in the on-state current of the transistor. Therefore, the thickness of the oxide film 423 is set to be thinner than that of the oxide semiconductor film 411 and to be 0.3 nm or more. It is preferable to set the thickness to 10 nm or less.
[0381] The oxide films 409 and 423 and the oxide semiconductor film 411 were formed in the same manner as in the deposition model described in Embodiment 2. The oxide films 409 and 423 and the oxide semiconductor film 411 are formed using a non-single-crystal The non-single crystal structure may be, for example, the CAAC-OS shown in the second embodiment, or a polycrystalline structure. Among non-single crystal structures, the amorphous structure is the most The defect density of the oxide film 4 is high, and the defect density of the CAAC-OS is the lowest. The oxide semiconductor film 09, 423, and the oxide semiconductor film 411 are preferably CAAC-OS.
[0382] Note that the oxide films 409 and 423 and the oxide semiconductor film 411 each have an amorphous structure. region, microcrystalline region, polycrystalline region, CAAC-OS region, and single crystal region. The mixed film may have two or more kinds of materials. The mixed film may have, for example, an amorphous structure region, a microcrystalline structure region, The structure region, the polycrystalline structure region, the CAAC-OS region, and the single-crystalline structure region are either In some cases, the mixed film has a single layer structure with one or more regions of an amorphous structure. region, microcrystalline region, polycrystalline region, CAAC-OS region, and single crystal region. In some cases, the oxide film 409 and the oxide film 408 may have a laminated structure of two or more of these regions. The oxide semiconductor film 411 and the oxide film 423 are in the order of a microcrystalline structure, a CAAC-OS, and a CA Alternatively, the oxide film 409 may have a microcrystalline structure and a CAA structure. The oxide semiconductor film 411 and the oxide film 423 are stacked in a CAAC-OS layer. may be also possible.
[0383] The pair of electrodes 415 and 416 may be appropriately formed by using the pair of electrodes 221 and 222 shown in the fourth embodiment. There can be.
[0384] The gate insulating film 425 can be formed using the gate insulating film 217 described in Embodiment 4 as appropriate. Cut.
[0385] The gate electrode 421 can be formed using the gate electrode 215 described in Embodiment 4 as appropriate. .
[0386] The insulating films 427 and 429 are the oxide insulating film 223 and the oxide insulating film 222 described in Embodiment 4. Note that the insulating film 427 can be formed of a material other than SiO 2 as a blocking film for oxygen. Aluminum oxide film, hafnium oxide, yttrium oxide, etc. can be used. It is possible.
[0387] In addition, the side surfaces of the oxide film 423, the gate insulating film 425, and the gate electrode 421 are aligned substantially flush with each other. The insulating film 427 covers the surfaces of the pair of electrodes 415 and 416, the oxide film 423, and the gate electrode 425. When the multilayer film 4 is in contact with the gate insulating film 425 and the gate electrode 421, the multilayer film 4 Since the desorption of oxygen from 24 can be reduced, the variation in the electrical characteristics of the transistors can be reduced. At the same time, the fluctuation of the threshold voltage can be suppressed.
[0388] Note that although the insulating films 427 and 429 have a stacked structure here, they may have a single layer structure.
[0389] The wirings 431 and 432 can be made of the same material as the pair of electrodes 415 and 416. Cut.
[0390] In the transistor described in this embodiment, the oxide film 423 and the gate insulating film 425 are The oxide film 423 is characterized in that it is substantially aligned with the edge of the gate electrode 421. The gate insulating film 425 is formed by forming the gate electrode 421 in FIG. 31(A) and then by etching with an acid. By etching the oxide film 417 and the gate insulating film 419, the number of photomasks can be increased. Therefore, the oxide film 423 and the gate insulating film 425 can be formed without heating.
[0391] In the transistor 400, the etching residues generated during the formation of the gate electrode 421 are oxidized. Since the insulating film 423 and the gate insulating film 425 can be removed during the formation of the insulating film 423 and the gate insulating film 425, the It is possible to reduce the leakage current occurring between the port electrode 421 and the wirings 431 and 432. It is.
[0392] Next, a method for manufacturing the semiconductor device will be described with reference to FIGS.
[0393] As shown in FIG. 30(A), an oxide insulating film 403 is formed as a base insulating film on a substrate 401. An oxide film 405 and an oxide semiconductor film 407 are formed over the oxide insulating film 403.
[0394] Here, a glass substrate is used as the substrate 401 .
[0395] The oxide insulating film 403 can be formed by a sputtering method or a CVD method. do.
[0396] The oxide insulating film 403 was formed using a compound similar to the oxide insulating film 224 in Embodiment 4. When forming an oxide insulating film containing more oxygen than the stoichiometric composition, the CVD method is used. Alternatively, the insulating layer 11 may be formed by a CVD method or a sputtering method. After forming an oxide insulating film by the ring method, etc., ion implantation method, ion doping method, plasma Oxygen may be added to the oxide insulating film by a thermal treatment or the like.
[0397] Here, the oxide insulating film 403 is a 300-nm-thick oxide insulating film formed by a sputtering method. A recombinant membrane is used.
[0398] The oxide film 405 and the oxide semiconductor film 407 are formed by a sputtering method, a coating method, a pulse laser deposition method, or the like. The thin film can be formed by using a laser deposition method, a laser ablation method, or the like.
[0399] Here, the atomic ratio of the sputtering target is In:Ga:Zn=1:3:4. A 20 nm thick In-Ga- A Zn oxide film is formed.
[0400] Next, heat treatment is performed to change the oxide insulating film 403, the oxide film 405, and the oxide semiconductor film It is preferable that oxygen is transferred to the oxide film 405 and the oxide semiconductor film 407. It is preferable to remove impurities contained in 07.
[0401] The temperature of the heat treatment is typically 250° C. or higher and lower than the substrate distortion point, or 300° C. or higher and lower than 5 50°C or less, or furthermore, 350°C to 510°C.
[0402] The heat treatment can be performed using an electric furnace, an RTA device, or the like. Therefore, heat treatment can be performed at a temperature above the distortion point of the substrate for a short period of time. The processing time can be reduced.
[0403] Heat treatment is carried out in nitrogen, oxygen, or ultra-dry air (water content less than 20 ppm, or less than 1 ppm) or less than 10 ppb of air), or an atmosphere of rare gas (argon, helium, etc.) In addition, if the nitrogen, oxygen, ultra-dry air, or rare gas contains hydrogen, water, etc. It is preferable that this not be the case.
[0404] Here, the heat treatment is performed in a nitrogen atmosphere at 450°C for 1 hour, and then in an oxygen atmosphere. The mixture is then heat treated at 450° C. for 1 hour.
[0405] By this heat treatment, the oxide insulating film 403 which serves as a base insulating film and the oxide insulating film 404 to which oxygen has been added are A part of oxygen contained in the oxide semiconductor film 409 is transferred to the oxide semiconductor film 407, and the oxide semiconductor film 4 The amount of oxygen vacancies in the oxide film 409 is reduced by the heat treatment. This process reduces the oxygen content.
[0406] Through the above steps, oxygen vacancies in the oxide semiconductor film can be reduced.
[0407] The heat treatment may be performed in a later step rather than in the present step. In another heat treatment, part of oxygen contained in the oxide insulating film 403 is converted to an oxide semi-conductor. It may be moved to the conductive film 407. As a result, the number of heating steps can be reduced.
[0408] Next, a mask is formed over the oxide semiconductor film 407 by a photolithography process. Using the mask, the oxide film 409 and the oxide semiconductor film 407 are partly etched. As a result, the oxide film 409 and the oxide semiconductor film 411 were formed as shown in FIG. After that, the mask is removed. Note that in this etching process, the oxide insulating A portion of the film 403 may be etched. Here, a portion of the oxide film 403 is etched. The oxide insulating film 403 is referred to as an oxide insulating film 413.
[0409] Next, as shown in FIG. 30C, a pair of electrodes 415 and 41 Form 6.
[0410] The method for forming the pair of electrodes 415 and 416 will be described below. First, a sputtering method, C A conductive film is formed by a VD method, a vapor deposition method, or the like. Next, a photolithography process is performed on the conductive film. Next, the conductive film is etched using the mask to form a pair of electrodes 41. 5, 416 are formed. After this, the mask is removed.
[0411] Here, a titanium film having a thickness of 50 nm, an aluminum film having a thickness of 400 nm, and a A 0 nm thick titanium film is then laminated by sputtering. A mask is formed by a lithography process, and the titanium film, the aluminum film, The titanium film is then dry etched to form a pair of electrodes 415 and 416 .
[0412] After the pair of electrodes 415 and 416 are formed, the substrate is washed to remove etching residues. By this cleaning process, the pair of electrodes 415 and 416 can be shortened. This cleaning process uses TMAH (Tetramethylammonium hydroxide) Alkaline solutions such as dilute hydrofluoric acid, oxalic acid, This can be done using an acidic solution such as phosphoric acid.
[0413] Next, as shown in FIG. 30D, the oxide semiconductor film 411 and the pair of electrodes 415 and 41 An oxide film 417 is formed on the first insulating film 6, and a gate insulating film 419 is formed on the oxide film 417.
[0414] The oxide film 417 can be formed in the same manner as the oxide film 409. The film 419 can be formed by sputtering, CVD, or the like.
[0415] Here, the atomic ratio of the sputtering target is In:Ga:Zn=1:3:4. The oxide film 417 was formed by sputtering with In-Ga-Z Forms an n-oxide film.
[0416] Next, as shown in FIG. 31A, an oxide semiconductor film A gate electrode 421 is formed in the region overlapping with 411 .
[0417] The method of forming the gate electrode 421 will be described below. First, a sputtering method, a CVD method, A conductive film is formed by a deposition method or the like, and a mask is formed on the conductive film by a photolithography process. Next, a part of the conductive film is etched using the mask to form a gate electrode 421. After that, the mask is removed.
[0418] The gate electrode 421 may be formed by electrolytic plating, printing, inkjet printing, or the like instead of the above-mentioned method. It may be formed by a jet method or the like.
[0419] Here, a tantalum nitride film with a thickness of 15 nm and a tungsten film with a thickness of 135 nm are spat. Next, a mask is formed by a photolithography process. The tantalum nitride film and the tungsten film are then dry-etched using the mask to form a gate. A ground electrode 421 is formed.
[0420] Next, as shown in FIG. 31(B), the oxide film 417 is removed using the gate electrode 421 as a mask. The gate insulating film 419 is etched to form an oxide film 423 and a gate insulating film 425. Therefore, the oxide film 423 and the gate insulating film 424 can be formed without increasing the number of photomasks. In addition, the oxide film 423 and the gate insulating film 425 can be formed. The end portion substantially coincides with the end portion of the gate electrode 421 .
[0421] In addition, in the transistor 450, etching residues from the formation of the gate electrode 421 Since the oxide film 423 and the gate insulating film 425 can be removed during the process of forming the oxide film 423 and the gate insulating film 425, Therefore, a leakage current occurs between the gate electrode 421 and the wirings 431 and 432 to be formed later. It is possible to reduce
[0422] Next, as shown in FIG. 31C, the pair of electrodes 415 and 416 and the gate electrode 421 are An insulating film 427 and an insulating film 429 are stacked in this order on the insulating film 427. Next, heat treatment is performed. After openings are formed in the insulating film 427 and the insulating film 429, wirings 431 and 432 are formed.
[0423] The insulating film 427 and the insulating film 429 can be formed by a sputtering method, a CVD method, or the like. By using an oxygen blocking film as the insulating film 427, Since the desorption of oxygen from the multilayer film 424 can be reduced, the variation in the electrical characteristics of the transistors can be reduced. This can reduce the adhesion and suppress the fluctuation of the threshold voltage.
[0424] Here, the insulating film 427 is a 300 nm thick oxynitride film formed by plasma CVD. A silicon film is formed, and a 50 nm thick nitride silicon film is formed as an insulating film 429 by a sputtering method. Form a recombinant membrane.
[0425] The heat treatment is typically performed at a temperature of 150° C. or higher but below the substrate distortion point, or at a temperature of 250° C. or higher but not higher than 500° C. The temperature is set to 300° C. or higher and 450° C. or lower. Here, the nitrogen and oxygen atmosphere is used. Heat treatment is carried out at 350℃ for 1 hour.
[0426] The wirings 431 and 432 can be formed in the same manner as the pair of electrodes 415 and 416. Alternatively, it can be formed by a damascene method.
[0427] By the above process, the localized level density of the multilayer film including the oxide semiconductor film is low, and excellent electrical properties are obtained. It is also possible to manufacture transistors with the characteristics shown in Fig. 1. It is possible to manufacture a highly reliable transistor with little fluctuation in electrical characteristics.
[0428] The configuration and method described in this embodiment may be applied to other embodiments and their modifications, as well as The present invention can be used in appropriate combination with the configurations and methods shown in the embodiments.
[0429] (Embodiment 10) Various films such as the metal film, the oxide semiconductor film, and the inorganic insulating film disclosed in the above embodiments are For the CVD (Plasma Chemical Vapor Deposition) method However, it may be formed by other methods, for example, a thermal CVD method. As an example of the CVD method, MOCVD (Metal Organic Chemical Vapor Deposition) por Deposition method and ALD (Atomic Layer Deposition) method. tion) method may also be used.
[0430] Thermal CVD is a film formation method that does not use plasma, so defects can occur due to plasma damage. This has the advantage that no additional steps are required.
[0431] In the thermal CVD method, the source gas and the oxidizing agent are fed into the chamber at the same time, and the chamber is heated to atmospheric pressure. Alternatively, a film is formed by reacting the reactants near or on the substrate under reduced pressure and depositing the reactants on the substrate. You may go.
[0432] In addition, in the ALD method, the pressure inside the chamber is set at atmospheric pressure or reduced pressure, and the source gas for the reaction is The gases may be introduced into the chamber in sequence, and the film may be formed by repeating the gas introduction sequence. For example, by switching each switching valve (also called high-speed valve), two or more types of The above source gases are supplied to the chamber in order, and the first source gas is supplied to the chamber in order to prevent the mixture of the source gases. An inert gas (such as argon or nitrogen) is introduced simultaneously with or after the raw material gas. The second source gas is introduced. When an inert gas is introduced at the same time, the inert gas is It acts as a carrier gas, and even if an inert gas is introduced at the same time as the second source gas is introduced, In addition, the first source gas is discharged by evacuation instead of introducing an inert gas. After that, a second source gas may be introduced. The first source gas is adsorbed on the surface of the substrate to form a first layer. The first layer is deposited on the second layer by reacting with the second source gas introduced later. This process is repeated several times while controlling the gas introduction sequence until the desired thickness is reached. By doing so, a thin film with excellent step coverage can be formed. The thickness of the thin film is determined by the gas introduction. The thickness can be precisely adjusted by changing the number of times the sequence is repeated. This is suitable for producing miniature FETs.
[0433] Thermal CVD methods such as MOCVD and ALD have been disclosed in the embodiments described above. It is possible to form various films such as metal films, oxide semiconductor films, and inorganic insulating films. In the case of forming an nGaZnO film, trimethylindium, trimethylgallium, and Dimethyl zinc is used. The chemical formula for trimethyl indium is In(CH3)3. The chemical formula for trimethylgallium is Ga(CH3)3. The chemical formula for lead is Zn(CH3)2. Using triethylgallium (chemical formula Ga(C2H5)3) instead of methylgallium It is also possible to use diethylzinc (chemical formula Zn(C2H5)2) instead of dimethylzinc. It is also possible.
[0434] For example, when forming a hafnium oxide film using a film forming apparatus that uses ALD, the solvent and a liquid containing a hafnium precursor compound (hafnium alkoxide solution, typically tetra The raw material gas is vaporized with tetramethyl tert-butyl amide hafnium (TDMAH) as an oxidizing agent. Two types of gases are used: tetrakisdimethylamidohafnium (TDA) and ozone (O3). The chemical formula is Hf[N(CH3)2]4. Other material liquids include tetrakis(ethoxycarbonyl) (ethylmethylamido) hafnium.
[0435] For example, when forming an aluminum oxide film using an ALD deposition system, A liquid containing a catalyst and an aluminum precursor compound (e.g., trimethylaluminum (TMA)) is added. Two types of gases are used: vaporized source gas and H2O as an oxidizing agent. The chemical formula for aluminum is Al(CH3)3. Other liquid materials include Tris( Dimethylamido)aluminum, triisobutylaluminum, aluminum tris(2 ,2,6,6-tetramethyl-3,5-heptanedionate).
[0436] For example, when forming a silicon oxide film using a deposition system that uses ALD, Chlorodisilane is adsorbed onto the surface to be coated, the chlorine contained in the adsorbed matter is removed, and the oxidizing gas (O 2. Nitrous oxide (NO) radicals are supplied to react with the adsorbed material.
[0437] For example, when forming a tungsten film using an ALD deposition system, WF6 The initial tungsten film was formed by repeatedly introducing B2H6 gas and WF 6 gas and H2 gas are introduced simultaneously to form a tungsten film. Alternatively, SiH4 gas may be used.
[0438] For example, an oxide semiconductor film, such as In-Ga-Zn- When forming an O film, In(CH3)3 gas and O3 gas are introduced in sequence. Then, Ga(CH3)3 gas and O3 gas are introduced simultaneously to form a GaO layer. Then, Zn(CH3)2 and O3 gases are introduced simultaneously to form a ZnO layer. The order of these layers is not limited to this example. A mixed compound layer such as an O layer, an In-Zn-O layer, or a Ga-Zn-O layer may be formed. Instead of O3 gas, H2O gas obtained by bubbling with an inert gas such as Ar can be used. However, it is preferable to use O3 gas that does not contain H. In(CH3)3 gas is also used. Alternatively, In(C2H5)3 gas may be used. Ga(C2H5)3 gas may be used. Also, instead of In(CH3)3 gas, In( C2H5)3 gas may be used. Also, Zn(CH3)2 gas may be used.
[0439] The configuration and method described in this embodiment may be applied to other embodiments and their modifications, as well as The present invention can be used in appropriate combination with the configurations and methods shown in the embodiments. EXAMPLES
[0440] In this embodiment, a sputtering target having an In-Ga-Zn oxide was used. A film of In-Ga-Zn oxide was formed. The atomic ratio of the sputtering target and the film formed was and the crystal structure.
[0441] <Sample structure> First, a method for preparing the sample will be described.
[0442] In this example, a 100 nm thick In-Ga-Zn oxide film was formed on a quartz substrate. The materials were prepared.
[0443] Here, a sputtering target having In-Ga-Zn oxide is used, and the flow rate is A mixed gas of oxygen and argon (1:2) was supplied into the deposition chamber as a sputtering gas. The pressure in the chamber was controlled at 0.4 Pa, and 200 W of DC power was supplied to the In-Ga-Zn oxide. A nitride film was formed.
[0444] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a ZnO / GaAs ratio of 3:2. The sample was named Sample 1. The substrate temperature was set to 200°C.
[0445] In addition, the atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a composition ratio of 1:3:4. The sample was named Sample 2. The substrate temperature was set to 200°C.
[0446] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a composition ratio of 1:3:6. The sample was named Sample 3. The substrate temperature was set to 200°C.
[0447] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a ZnO / GaAs ratio of 6:2. The sample was named Sample 4. The substrate temperature was set to 200°C.
[0448] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a ZnO / GaAs ratio of 6:4. The sample was named Sample 5. The substrate temperature was set to 200°C.
[0449] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a composition ratio of 1:6:8. The sample was named Sample 6. The substrate temperature was set to 200°C.
[0450] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. A sputtering target with a ratio of Zn:Ga:Zn was used to form an In-Ga-Zn oxide film. The resulting sample was designated as Sample 7. The substrate temperature was set to 200°C.
[0451] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=0. In-Ga-Zn oxide films were formed using a sputtering target with a ZnO / GaAs ratio of 1:2:1. The sample was named Sample 8. The substrate temperature was set to 200°C.
[0452] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=3. In-Ga-Zn oxide films were formed using a sputtering target with a ZnO / GaAs ratio of 1:1. The sample was named Sample 9. The substrate temperature was set to 200°C.
[0453] The atomic ratio of metal elements contained in In-Ga-Zn oxide is In:Ga:Zn=1. In-Ga-Zn oxide films were formed using a sputtering target with a ZnO / GaAs ratio of 1:1. The sample was named Sample 10. The substrate temperature was set to 300°C.
[0454] <xps> Next, in Samples 1 to 10, the In-Ga-Zn oxide film and Samples 1 to 10 The atomic ratio of the metal elements contained in the sputtering target used to deposit the 0 film was measured using X-ray photoelectron spectroscopy. Spectroscopy (X-ray Photoelectron Spectroscopy:) Analysis Next, the atomic ratio of Ga to In and the atomic ratio of Zn to In were The numerical ratios are shown in FIG. 32. In FIG. 32, the numbers in parentheses indicate the spa The atomic ratio of In:Ga:Zn contained in the annealing target is shown.
[0455] From FIG. 32, the atomic ratio of Ga to In in the sputtering target and I The atomic ratio of Zn to n in the In-Ga-Zn oxide film is It can be seen that the atomic ratio of Ga to In and the atomic ratio of Zn to In are smaller.
[0456] <xrd> Next, the crystal structures of the In-Ga-Zn oxide films included in Samples 1 to 10 will be described. X-ray diffraction (XRD) measurements were performed. In the samples 10 to 10, the sputtering gas for forming the In-Ga-Zn oxide film was The flow rate of the mixed gas is oxygen:argon = 1:2, and the flow rate of the oxygen gas is oxygen only. A sample was prepared.
[0457] Next, the results of X-ray diffraction measurement of the formed In-Ga-Zn oxide film are shown in Figs. 33 to 35. Here, the X-ray diffraction measurement results of sample 1, sample 2, and sample 3 are shown as representative examples. The results are shown in Figs. 33 to 35. In the samples 1, 2, and 3, the sputtering The In-Ga-Zn oxide film deposited using only oxygen as the etching gas was measured.
[0458] In FIG. 33 to FIG. 35, (A) is an XRD scan obtained by using the out-of-plane method. The results of the spectrum measurement are shown, with the vertical axis representing the X-ray diffraction intensity (arbitrary units) and the horizontal axis representing the diffraction angle. (B) The XRD spectrum was measured using the in-plane method. The results are shown in the table. The vertical axis shows the X-ray diffraction intensity (arbitrary unit) and the horizontal axis shows the diffraction angle 2θ (deg .) is taken.
[0459] In FIG. 33 to FIG. 35, h indicates a homologous structure, and s indicates a spinel structure. In addition, ( ) indicates the plane orientation of the crystal structure.
[0460] In Sample 1 shown in FIG. 33, the In—Ga—Zn oxide film has a spinel structure. On the other hand, sample 2 shown in FIG. 34 has a spinel structure and a homologous structure. 3. The In-Ga-Zn oxide film has a homologous structure.
[0461] From Fig. 33 to Fig. 35, when a sputtering target with a larger Zn content than Ga was used, By forming the film using this method, it is possible to form an In-Ga-Zn oxide film with a homologous structure. be.
[0462] Next, based on the XPS measurement results shown in FIG. 32 and the X-ray diffraction measurement results shown in FIGS. 33 to 35, The In-Ga-Zn oxide film of each sample and the sputtering temperature used to prepare each sample are shown in Fig. A ternary phase diagram plotting the In, Ga, and Zn compositions of the get is shown in Figure 36. In the table, the numbers in parentheses indicate the composition of In, Ga, and Zn contained in the sputtering target. In addition, the amount of oxygen is not taken into consideration in Figure 36.
[0463] In Fig. 36, the diamond markers indicate the homologous structure, and the square markers indicate the spinel structure. The white markers indicate the composition of the sputtering target. The black markers are the In-Ga-Zn oxide films. Markers plotted according to film composition.
[0464] As shown in Fig. 36, the In-Ga-Zn oxide film formed is It can be seen that the composition is different from the original.
[0465] The dashed line L1 indicates the composition of the metal elements Ga:Zn=2:1. The dashed line L2 indicates the composition of the trivalent gold. Group ions (M 3+ ) and divalent metal ions (M 2+ ) has a composition of M 3+ :M 2 +=2:1 do.
[0466] In Fig. 36, in the region to the right of the dashed line L1, that is, in the region where the amount of Ga increases relative to Zn, It can be seen that a spinel-structured In-Ga-Zn oxide film is formed in the dotted line L. In the region to the left of 1, i.e., the region where the amount of Zn increases relative to Ga, the homologous structure It can be seen that an In-Ga-Zn oxide film is formed.
[0467] Next, the composition of In, Ga, and Zn in the In-Ga-Zn oxide films included in Samples 1 to 9 was The composition, atomic ratio of Zn to Ga (Zn / Ga), crystal structure, and the The composition of the sputtering target is shown in Table 2. The oxide film was formed using a deposition gas of 33 vol% oxygen (diluted with argon). The crystal structure of the film was measured using 33 vol% oxygen (diluted with argon) or The graph shows the measurement results for a film formed using 100 vol % oxygen as the film formation gas.
[0468] [Table 2]
[0469] From Table 2, the sputtering target with Zn more than Ga is The In-Ga-Zn oxide film formed using the In-Ga-Zn target has a homologous structure. It can be seen that...
[0470] In addition, from Table 2, the ratio of Zn to Ga in the formed In-Ga-Zn oxide film was It is found that films with a ratio (Zn / Ga) of greater than 0.5 have a homologous structure.
[0471] From the above, it was found that the film was formed using a sputtering target with a larger Zn content than Ga. By this, it is possible to form an In-Ga-Zn oxide film having a homologous structure.
[0472] <tem> Next, the atomic arrangement of the cross sections of Sample 2 and Sample 3 was observed using a transmission electron microscope. Observed using a TEM (Electron Ion Microscope) A cross-sectional observation image (bright field image) is shown in Figure 37. Here, the accelerating voltage was 300 kV and the magnification was 8. The vicinity of the surface of the In-Ga-Zn oxide film of each sample was observed at a magnification of 100,000 times. In FIG. 37, the values in parentheses indicate the amounts of In, Ga, and Zn contained in the sputtering target. Represents the composition.
[0473] FIG. 37(A) is a cross-sectional observation image of sample 2, and is a partially enlarged cross-sectional observation image of FIG. 37(A). FIG. 37(B) shows a cross-sectional observation image of sample 3. An enlarged cross-sectional image of a portion of the above is shown in FIG.
[0474] As shown in FIG. 37, in Sample 2 and Sample 3, the atomic arrangement is regular and parallel to the upper surface. From this, it was found that the In-Ga-Zn oxide formed in Sample 2 and Sample 3 It was found that the oxide film was a CAAC-OS film.
[0475] <haadf-stem> Next, the atomic arrangement of the cross sections of sample 2 and sample 3 was examined using a high-angle annular dark-field scanning transmission electron microscope ( HAADF-STEM:High-Angle Annular Dark Field Scanning Transmission Electron Microscope The cross-sectional image obtained by observation using an accelerating voltage of 200 The In-Ga-Zn oxide film on each sample was observed at a voltage of 100 kV and a magnification of 8 million times. Ta.
[0476] FIG. 38(A) is a cross-sectional observation image obtained by observing sample 2, and FIG. 38(B) is a cross-sectional observation image obtained by observing sample 2. 3 is a cross-sectional image obtained by observing the sample shown in FIG.
[0477] In HAADF-STEM images, contrast proportional to the square of the atomic number is obtained. Therefore, brighter dots indicate heavier atoms. The bright points indicated by the arrows are In, and the dark points between them are Ga or Zn. Since Zn and Zn have almost the same mass, it is difficult to distinguish them. No element is observed.
[0478] In FIG. 38(A), In, Ga, and Zn are arranged in parallel. In addition, two or three layers of Ga or Zn exist between the In shown by the arrows. .
[0479] In FIG. 38(B), In, Ga, and Zn are arranged in parallel. In addition, three or four layers of Ga or Zn exist between the In indicated by the arrows. .
[0480] As shown in FIG. 38, layers containing In are arranged periodically with multiple layers containing Ga or Zn between them. Therefore, the In-Ga-Zn oxide films of sample 2 and sample 3 have a homologous structure. In other words, the sputtering target with a larger Zn content than Ga content was used. By using this method, it is possible to form an In-Ga-Zn oxide film with a homologous structure. . EXAMPLES
[0481] In this example, sputtering targets having In-Ga-Zn oxides with different compositions were used. Using a quartz crystal, we formed stacked films of In-Ga-Zn oxides with different compositions. The band diagram and crystal structure are described below.
[0482] Here, samples 1 to 4, 6, 7, and 10 shown in Example 1 were used. In Samples 1 to 4, 6, 7, and 10, the substrate was silicon. A silicon wafer was used.
[0483] In addition, the In-Ga-Zn oxide film (thickness 20 mm) formed in sample 1 was placed on the silicon wafer. nm), the In-Ga-Zn oxide film (thickness 15 nm) formed on sample 10, and the In-Ga-Zn oxide film (thickness 15 nm) formed on sample 1 A sample was prepared by laminating a Zn-Ga-Zn oxide film (5 nm thick) on the substrate. This sample was named Sample 11.
[0484] In addition, the In-Ga-Zn oxide film (thickness 20 mm) formed in sample 2 was placed on the silicon wafer. nm), the In-Ga-Zn oxide film (thickness 15 nm) formed on sample 10, and the In-Ga-Zn oxide film (thickness 15 nm) formed on sample 2 A sample was prepared by laminating a 10 nm thick In-Ga-Zn oxide film on the substrate. This sample was designated as sample 12.
[0485] In addition, the In-Ga-Zn oxide film (thickness 20 mm) formed in sample 3 was placed on the silicon wafer. nm), the In-Ga-Zn oxide film (thickness 10 nm) formed on sample 10, and the In-Ga-Zn oxide film (thickness 10 nm) formed on sample 3 A sample was prepared by laminating a 15 nm thick In-Ga-Zn oxide film on the substrate. This sample was designated as sample 13.
[0486] <Band diagram> Next, the structures formed on Samples 1 to 4, 6, 7, and 10 prepared in Example 1 were The energy difference between the conduction band edge Ec and the valence band edge Ev of the In-Ga-Zn oxide film is That is, the energy gap Eg was measured using a spectroscopic ellipsometer. Ultraviolet Photoelectron Spectrometry (UPS) tron scopy) to obtain the energy difference between the vacuum level Evac and the top of the valence band Ev, That is, the ionization potential Ip was measured. Next, the ionization potential Ip and the energy By calculating the difference between the vacuum level Evac and the electric band edge Ec, The energy difference, i.e., the electron affinity χ, was calculated. The resulting band diagram is shown in FIG. As shown in.
[0487] As shown in FIG. 39, Samples 1 to 4, Sample 6, and Sample 7 are superior to Sample 10 in terms of the The electron affinity χ is small, and the energy difference is between 0.2 eV and 0.4 eV. .
[0488] Next, the band diagrams of Samples 12 and 13 will be described with reference to FIG. .
[0489] The ionization potential Ip and energy gap Eg of sample 12 were measured and obtained. The band diagram is shown in FIG. 40(A). The ionization potential Ip and ionization potential Ip of sample 13 are shown in FIG. The band diagram obtained by measuring the energy gap Eg is shown in FIG. In 40, the horizontal axis indicates the sputtering time, and the vertical axis indicates the valence band upper limit Ev and the vacuum level. The energy difference between Evac (Ev-Evac), the electric band edge Ec and the vacuum level Evac The energy difference (Ec-Evac) is shown.
[0490] Here, an In-Ga-Zn oxide film is sputtered from the surface with argon ions. The In-Ga-Zn The energy difference between the vacuum level Evac and the top of the valence band Ev of the oxide film, i.e., the ionization potential The electric charge Ip was measured and plotted. The energy difference between the lower end of the electric conduction band Ec and the upper end of the valence band Ev was also The energy difference, i.e., the energy gap Eg, was measured using a spectroscopic ellipsometer. By calculating the difference between the ionization potential Ip and the energy gap Eg, the vacuum level Ev The energy difference between ac and the bottom edge of the conduction band Ec, that is, the electron affinity χ, was calculated. Next, the valence band The upper end Ev and the lower end Ec of the conduction band are plotted.
[0491] As shown in FIG. 40A, the In-Ga-Zn oxide film formed on sample 2 and the In-Ga-Zn oxide film formed on sample 10 are The difference in energy between the conduction band minimum Ec and the In-Ga-Zn oxide film is 0.2 eV. In addition, the In-Ga-Zn oxide film formed in sample 2 was interposed between the In-Ga-Zn oxide films formed in sample 10. By providing the n-Ga-Zn oxide film, the In-Ga-Zn oxide formed on the sample 10 It can be seen that the membrane forms wells.
[0492] As shown in FIG. 40B, the In-Ga-Zn oxide film formed on sample 3 and the In-Ga-Zn oxide film formed on sample 10 are The difference in energy between the conduction band minimum Ec and the In-Ga-Zn oxide film is 0.2 eV. In addition, the In-Ga-Zn oxide film formed in sample 3 was interposed between the In-Ga-Zn oxide film formed in sample 10. By providing the n-Ga-Zn oxide film, the In-Ga-Zn oxide formed on the sample 10 It can be seen that the membrane forms wells.
[0493] <tem> Next, the atomic arrangement of the cross sections of Samples 11 to 13 was observed using a transmission electron microscope. Observation using a Transmission Electron Microscope (TEM) The cross-sectional observation images (bright field images) are shown in Figs. 41 to 43. Here, the accelerating voltage was 300 kV. The magnification was set to 2 million and 4 million times, and the In-Ga-Zn oxide film of each sample was was observed.
[0494] FIG. 41 shows cross-sectional observation images of Samples 11 to 13 at a magnification of 2,000,000 times. FIG. 43 is a cross-sectional observation image of Samples 11 to 13 at a magnification of 4,000,000 times. 41 to 43 are enlarged cross-sectional observation images. The Ga-Zn oxide films are designated S1, S2, and S3 in this order. indicates the vicinity of the interface between S1 and S2.
[0495] As shown in FIG. 41, in Samples 12 and 13, different sputtering targets were used. The crystallinity is uniform in the films S1 to S3 formed using the SiO2 solution.
[0496] As shown in FIG. 42, in sample 11, no crystallinity was confirmed in S1, and only crystallinity was confirmed in S2. On the other hand, in Samples 12 and 13, crystallinity was confirmed in S1 to S3. Crystallinity was confirmed.
[0497] As shown in FIG. 43, the In-Ga-Zn oxide films of Samples 12 and 13 have flat surfaces. In addition, the interface between S1 and S2 has a regular atomic arrangement. This indicates that the In formed in Samples 12 and 13 is a regular arrangement of atoms. It was found that S1 and S2 contained in the -Ga-Zn oxide film were CAAC-OS films. It is also clear that there is little crystal distortion at the interface between S1 and S2.
[0498] By using a sputtering target with a higher Zn content than Ga, It is possible to form an In-Ga-Zn oxide film with a logarithmic structure. The CAAC-OS film was formed using a sputtering target with a large n composition. It is also possible to deposit multiple films by using sputtering targets with different compositions. In the In-Ga-Zn oxide film with several layers stacked, the crystal structure is uniform throughout the film. and there is little crystal distortion at the interfaces of the layers.
[0499] Therefore, the In-Ga-Zn oxide film fabricated in this embodiment has a reduced defect amount. It is possible to reduce the fluctuation of electrical characteristics of semiconductor devices fabricated using In-Ga-Zn oxide films. It is possible to reduce the number of defects and improve the reliability.< / tem> < / tem> < / xrd> < / xps>
Claims
1. a gate electrode layer; a gate insulating layer having a region located above the gate electrode layer; a first oxide layer having a region overlying the gate insulating layer; a second oxide layer having a region overlying the first oxide layer; a first electrode layer and a second electrode layer having an area overlying the second oxide layer; an insulating layer having a region overlying the second oxide layer; the first oxide layer and the second oxide layer contain In, Ga, and Zn; an atomic ratio of Ga to In in the second oxide layer is greater than an atomic ratio of Ga to In in the first oxide layer; In a cross-sectional observation image obtained using a HAADF-STEM, the second oxide layer has an area in which a plurality of bright points and a plurality of dark points are arranged in parallel, a region of the first electrode that overlaps with the gate electrode has a region that does not overlap with the first oxide layer.
2. a gate electrode layer; a gate insulating layer having a region located above the gate electrode layer; a first oxide layer having a region overlying the gate insulating layer; a second oxide layer having a region overlying the first oxide layer; a first electrode layer and a second electrode layer having an area overlying the second oxide layer; an insulating layer having a region overlying the second oxide layer; the first oxide layer and the second oxide layer contain In, Ga, and Zn; an atomic ratio of Ga to In in the second oxide layer is greater than an atomic ratio of Ga to In in the first oxide layer; In a cross-sectional observation image obtained using a HAADF-STEM, the second oxide layer has a region in which a layer containing In and a layer containing Ga or Zn are arranged in parallel, a first oxide film having an end portion in contact with the first electrode or the second electrode in a region overlapping with the gate electrode when viewed in a cross section in a channel length direction;
3. In claim 1 or 2, a ratio of the number of Ga atoms to In atoms in the second oxide layer is 1.5 times or more a ratio of the number of Ga atoms to In atoms in the first oxide layer.
4. In claim 1 or 2, a ratio of the number of Ga atoms to In atoms in the second oxide layer is equal to or greater than twice the number of Ga atoms to In atoms in the first oxide layer.
5. In claim 1 or 2, a ratio of the number of Ga atoms to In atoms in the second oxide layer is three or more times a ratio of the number of Ga atoms to In atoms in the first oxide layer.
6. In any one of claims 1 to 5, the insulating layer has a laminated structure including an oxide insulating layer and a nitride insulating layer having a region located above the oxide insulating layer.
Citation Information
Patent Citations
Oxide semiconductor element having insulating layer, and display device using the same
JP2009141002A
Oxide semiconductor film and semiconductor device
JP2011100979A
Field sequential driving type display device
JP2011227477A
Thin film transistor and method of manufacturing the same, and device with thin film transistor
JP2012059860A
Optical detection circuit, input device, and input / output device
JP2012256829A