Composite member and method for manufacturing the same, and beverage container and method for manufacturing the same
The composite member manufacturing method ensures a strong, inseparable bond between silicone rubber and polypropylene components in beverage container stoppers, addressing separability issues and enhancing durability and security.
Patent Information
- Application Number
- JP2024139115
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-05-29
AI Technical Summary
Existing beverage container stopper members with silicone rubber and polypropylene components face issues with separability, leading to potential leakage, dirt accumulation, and theft of the rubber component, due to inadequate bonding strength between these materials.
A method for manufacturing a composite member involving a silicone rubber molded body and a polypropylene molded body, utilizing surface modification, primer application, and insert molding to achieve a peel strength of 3.0 N/mm or more, ensuring inseparable bonding of the inner stopper packing and base material.
The solution provides a strong, inseparable bond between silicone rubber and polypropylene components, preventing leakage, dirt accumulation, and theft, while maintaining the benefits of both materials' properties, such as low water absorption and chemical resistance.
Smart Images

Figure 2024152878000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite member and a manufacturing method thereof, and a beverage container and a manufacturing method thereof. [Background technology]
[0002] Patent Document 1 describes an inner plug of a plug member that closes the opening of a food or beverage container, the inner plug of the plug member comprising: an inner plug rubber that fits tightly against the inner circumference of the opening; a rubber receiver into which the inner plug rubber is fitted; and a restraining portion that is formed integrally with the rubber receiver and restrains the inner plug rubber so that it cannot be separated from the rubber receiver. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-007296 A Summary of the Invention [Problem to be solved by the invention]
[0004] Meanwhile, the inventors of the present invention have conducted extensive research into a technical means for adhering the silicone rubber surface of the inner plug gasket and the polypropylene surface of the inner plug base material in a case where a silicone rubber molded body is used as the inner plug gasket and a polypropylene molded body is used as the inner plug base material supporting the inner plug gasket, in relation to a inner plug member for a beverage container.
[0005] The present invention has been made in consideration of the above-mentioned problems, and one of its objects is to provide a composite member comprising a silicone rubber molded body and a polypropylene molded body bonded to each other and a method for manufacturing the same, as well as a beverage container and a method for manufacturing the same. [Means for solving the problem]
[0006] According to one embodiment of the present invention for solving the above problems, a method for producing a composite member including a first member and a second member includes a bonding step of bonding a silicone rubber surface of the first member, which is a silicone rubber molded body, to a polypropylene surface of the second member, which is a polypropylene molded body. According to the present invention, there is provided a method for producing a composite member including a silicone rubber molded body and a polypropylene molded body bonded to each other.
[0007] The method may further include a surface modification step of performing a surface modification treatment on the polypropylene surface of the second member, and a primer application step of applying a primer to the polypropylene surface of the second member that has been subjected to the surface modification treatment, and the bonding step may bond the silicone rubber surface of the first member to the polypropylene surface of the second member that has been coated with the primer. The bonding step may also bond the silicone rubber surface of the first member to the polypropylene surface of the second member by insert molding. The bonding step may also bond the silicone rubber surface to the polypropylene surface with a peel strength of 3.0 N / mm or more measured by a method conforming to JIS K6256-2.
[0008] In addition, in the above method, the composite member may be an inner plug member of a beverage container including an insulated double container, the first member may include an inner plug gasket that is in close contact with the inner surface of the upper opening of the insulated double container, and the second member may include an inner plug base material that supports the inner plug gasket.
[0009] According to one embodiment of the present invention for solving the above problems, a composite member includes a first member which is a silicone rubber molded body and a second member which is a polypropylene molded body, and the silicone rubber surface of the first member is bonded to the polypropylene surface of the second member. According to the present invention, there is provided a composite member including a silicone rubber molded body and a polypropylene molded body bonded to each other.
[0010] In the composite member, the silicone rubber surface of the first member and the polypropylene surface of the second member may be bonded via a primer-derived component. In this case, the second member may have a modified polypropylene surface. The composite member may be an insert molding. In the composite member, the silicone rubber surface and the polypropylene surface may be bonded with a peel strength of 3.0 N / mm or more as measured by a method in accordance with JIS K6256-2.
[0011] The composite member may also be an inner plug member of a beverage container including an insulated double container, the first member including an inner plug gasket that is in close contact with the inner surface of the upper opening of the insulated double container, and the second member including an inner plug base material that supports the inner plug gasket.
[0012] According to an embodiment of the present invention for solving the above problem, a beverage container includes an insulated double container and the inner plug member. According to the present invention, there is provided a beverage container provided with an inner plug member including an inner plug packing and an inner plug base material bonded to each other.
[0013] According to an embodiment of the present invention for solving the above problems, a method for manufacturing a beverage container includes a step of attaching the inner plug member to an insulated double container. According to the present invention, a method for manufacturing a beverage container provided with an inner plug member including an inner plug packing and an inner plug base material bonded to each other is provided.
[0014] The method for manufacturing a beverage container may further include a step of manufacturing the inner plug member by the method for manufacturing an inner plug member. Effect of the Invention
[0015] According to the present invention, there are provided a composite member including a silicone rubber molded body and a polypropylene molded body bonded to each other and a method for producing the same, as well as a beverage container and a method for producing the same. [Brief description of the drawings]
[0016] [Figure 1] 1 is a cross-sectional view of an example of a beverage container according to an embodiment of the present invention. [Diagram 2] 2 is a perspective cross-sectional view of the stopper of the beverage container shown in FIG. 1. [Figure 3A] 2 is an explanatory view showing a surface modification step included in an example of a method for producing the inside plug member shown in FIG. 1. FIG. [Figure 3B] 2 is an explanatory view showing a primer coating step included in the example of a method for producing the inside plug member shown in FIG. 1. FIG. [Figure 3C] 2 is an explanatory view showing a bonding step included in an example of a manufacturing method of the inside plug member shown in FIG. [Figure 3D] 3B is a cross-sectional view of one example of an inner plug member produced by a method for producing an inner plug member including the steps shown in FIGS. 3A to 3C. FIG. [Figure 4] 4 is a cross-sectional view of a portion of another example of a beverage container according to an embodiment of the present invention. FIG. [Figure 5A] 5 is an explanatory view showing a surface modification step included in the example of a method for producing the inside plug member shown in FIG. 4. [Figure 5B] 5 is an explanatory view showing a primer coating step included in the example of a method for producing the inside plug member shown in FIG. 4. FIG. [Figure 5C] 5 is an explanatory view showing a bonding step included in the example of a manufacturing method of the inside plug member shown in FIG. 4. [Figure 5D] 5A to 5C. FIG. 5C is a cross-sectional view of one example of an inner plug member produced by a method for producing an inner plug member including the steps shown in FIGS. 5A to 5C. [Figure 6] FIG. 11 is an explanatory diagram showing the results of measuring the peel strength of a test piece in Example 2 according to the present embodiment by a method conforming to JIS K6256-2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of the present invention will be described below, however, the present invention is not limited to this embodiment.
[0018] One aspect of the method according to the present embodiment is a method for producing a composite member including a first member and a second member, and includes a bonding step of bonding a silicone rubber surface of the first member, which is a silicone rubber molded body, to a polypropylene surface of the second member, which is a polypropylene molded body.
[0019] Moreover, the composite member according to this embodiment includes a first member which is a silicone rubber molded body and a second member which is a polypropylene molded body, and the silicone rubber surface of the first member is bonded to the polypropylene surface of the second member.
[0020] The composite member of the present invention is not particularly limited as long as it includes a first member and a second member bonded to each other, but in this specification, an example will be mainly described in which the composite member is an inner plug member of a beverage container including an insulated double container, the first member including an inner plug gasket that is in close contact with the inner surface of the upper opening of the insulated double container, and the second member including an inner plug base material that supports the inner plug gasket.
[0021] Fig. 1 shows a cross section of an example of a beverage container 1 including an inner plug member 21. In the example shown in Fig. 1, the beverage container 1 includes an insulated double container 10 and a plug 20 that covers an upper opening 11 of the insulated double container 10 in an openable and closable manner, and the plug 20 includes an inner plug member 21.
[0022] Fig. 2 shows a perspective cross-sectional view of the stopper 20 of the beverage container 1 shown in Fig. 1. Figs. 3A, 3B, and 3C show main steps included in an example of a method for producing the inner stopper member 21 shown in Fig. 1, and Fig. 3D shows the inner stopper member 21 produced by this method.
[0023] Fig. 4 shows a cross section of a part of another example of the beverage container 1. Figs. 5A, 5B, and 5C show main steps included in an example of a method for manufacturing the inner plug member 21 shown in Fig. 4, and Fig. 5D shows the inner plug member 21 manufactured by that method.
[0024] In this specification and drawings, the same or similar components are described with the same reference numerals. In this specification, the direction along the axis A (FIGS. 1 and 4) of the beverage container 1 is referred to as the "axial direction", the direction from the bottom surface 12 of the insulated double container 10 toward the upper opening 11 in the axial direction is referred to as the "upward direction", and the opposite direction is referred to as the "downward direction". In addition, the direction perpendicular to the axis A of the beverage container 1 is referred to as the "radial direction", and in the radial direction, the direction from the center of the insulated double container 10 toward the outside is referred to as the "radial outward direction", and the opposite direction is referred to as the "radial inward direction".
[0025] First, a description will be given of a manufacturing method of the inner plug member 21. The inner plug member 21 is a composite member including an inner plug gasket (first member) 30 that is in close contact with the inner peripheral surface 11a of the upper opening 11 of the thermally insulated double container 10 of the beverage container 1, and an inner plug base material (second member) 40 that supports the inner plug gasket 30.
[0026] The inside plug gasket 30 is a silicone rubber molded body, and has a silicone rubber surface (hereinafter referred to as the “rubber surface”) 31. The inside plug base material 40 is a polypropylene molded body, and has a polypropylene surface (hereinafter referred to as the “PP surface”) 41.
[0027] The manufacturing method of the inside plug member 21 includes a bonding step of bonding the rubber surface 31 of the inside plug packing 30 and the PP surface 41 of the inside plug substrate 40. In the bonding step, the rubber surface 31 of the inside plug packing 30 and the PP surface 41 of the inside plug substrate 40 are bonded to each other with such adhesive strength that the rubber surface 31 of the inside plug packing 30 and the PP surface 41 of the inside plug substrate 40 are inseparable during normal use of the inside plug member 21.
[0028] Specifically, in the bonding process, it is preferable that the rubber surface 31 of the inner plug gasket 30 and the PP surface 41 of the inner plug substrate 40 are bonded together with a peel strength (hereinafter simply referred to as "peel strength") of 3.0 N / mm or more, as measured by a method in accordance with JIS K6256-2 "Vulcanized rubber and thermoplastic rubber -- Determination of adhesion -- Part 2: 90° peel strength from rigid plate."
[0029] In this case, the adhesive strength between the rubber surface 31 and the PP surface 41 achieved in the adhesion step is not particularly limited as long as the peel strength is in the range of 3.0 N / mm or more, but the peel strength is, for example, preferably 4.0 N / mm or more, more preferably 5.0 N / mm or more, even more preferably 5.5 N / mm or more, and particularly preferably 6.0 N / mm or more. Since there is no particular problem caused by a high peel strength between the rubber surface 31 and the PP surface 41, the upper limit of the peel strength is not particularly limited.
[0030] The peel strength (N / mm) is calculated by dividing the maximum peel force (N) measured by a method conforming to JIS K6256-2 by the width of the test piece (25 mm). The maximum peel force (N) is the maximum force (N) required for peeling measured by a method conforming to JIS K6256-2. The maximum peel force is calculated as the arithmetic average value of the measured values obtained for four samples.
[0031] In the bonding step, the method for bonding the rubber surface 31 of the inside plug gasket 30 and the PP surface 41 of the inside plug substrate 40 is not particularly limited as long as it achieves the desired adhesive strength (for example, an adhesive strength having a peel strength equal to or greater than the above-mentioned specified value), but it is preferable that the manufacturing method for the inside plug member 21 further includes a surface modification step of subjecting the PP surface 41 of the inside plug substrate 40 to a surface modification treatment, and a primer application step of applying a primer to the PP surface 41 of the inside plug substrate 40 that has been subjected to the surface modification treatment, and that in the bonding step, the rubber surface 31 of the inside plug gasket 30 is bonded to the PP surface 41 of the inside plug substrate 40 to which the primer has been applied.
[0032] In the surface modification step, a surface modification treatment is applied to the PP surface 41 of the preformed plug substrate 40, thereby introducing reactive functional groups having the property of chemically reacting with the primer to form a chemical bond (e.g., a covalent bond) into the PP surface 41 (FIGS. 3A and 5A). The surface modification treatment is not particularly limited as long as it is a treatment that introduces reactive functional groups into the PP surface 41 of the plug substrate 40, but is preferably one or more treatments selected from the group consisting of plasma discharge treatment, corona discharge treatment, flame treatment, itro treatment, and ultraviolet irradiation treatment.
[0033] The reactive functional group introduced into the PP surface 41 of the plug substrate 40 may be, for example, a polar functional group, preferably a polar functional group containing an oxygen atom, and particularly preferably one or more selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), and a carbonyl group (-C(=O)-). In the surface modification step, the portion of the PP surface 41 of the plug substrate 40 that comes into contact with the rubber surface 31 of the plug packing 30 is subjected to a surface modification treatment to introduce a reactive functional group.
[0034] In the primer application step, a primer is applied to the surface-modified PP surface 41 of the inside plug substrate 40 (FIGS. 3B and 5B). The primer is not particularly limited as long as it has a reactive functional group capable of forming a chemical bond (e.g., a covalent bond) with the silicone rubber constituting the rubber surface 31 of the inside plug packing 30, and a reactive functional group capable of forming a chemical bond (e.g., a covalent bond) with the reactive functional group on the modified PP surface 41 of the inside plug substrate 40.
[0035] The reactive functional group of the primer can be, for example, an alkoxy group, but is not particularly limited as long as it is one or more types of reactive functional groups that form chemical bonds with the silicone rubber and the modified PP surface 41 as described above.
[0036] The method for applying the primer to the PP surface 41 of the inside plug member 40 is not particularly limited, but is preferably one or more selected from the group consisting of spray application, brush application, printing, and dipping. In the primer application step, the primer is applied to a part or all of the portion of the modified PP surface 41 of the inside plug substrate 40 that comes into contact with the rubber surface 31 of the inside plug packing 30.
[0037] In the bonding step, the rubber surface 31 of the inside plug packing 30 is bonded to the PP surface 41 of the inside plug substrate 40 to which a primer has been applied in the primer application step (FIGS. 3C and 5C). The method for bonding the rubber surface 31 of the inside plug packing 30 to the PP surface 41 of the inside plug substrate 40 is not particularly limited as long as it is a method for bonding the rubber surface 31 and the PP surface 41 via a primer, but in the bonding step, it is preferable to bond the rubber surface 31 of the inside plug packing 30 to the PP surface 41 of the inside plug substrate 40 by insert molding.
[0038] In insert molding, as shown in Figs. 3C and 5C, inside a heated mold 100, a center plug gasket 30 is molded from a silicone rubber raw material composition M on a PP surface 41 of a center plug substrate 40.
[0039] That is, under heating, a silicone rubber raw material composition M (specifically, an amorphous composition containing a silicone rubber raw material and a vulcanizing agent (e.g., an organic peroxide)) is pressed between a PP surface 41 (specifically, the modified PP surface 41 coated with a primer) of a stopper substrate 40 fixed to a part (lower mold 101) of an insert molding mold 100 and another part (upper mold 102) of the mold 100.
[0040] As a result, within the heated mold 100, the vulcanization of the silicone rubber is caused to proceed on the PP surface 41 of the stopper substrate 40 to form the stopper gasket 30, and the PP surface 41 and the rubber surface 31 of the stopper gasket 30 are bonded together via a primer.
[0041] Specifically, the modified polypropylene that constitutes the PP surface 41 of the inner plug substrate 40 and the primer form a chemical bond (e.g., a covalent bond) through a chemical reaction, and the primer and the silicone rubber that constitutes the rubber surface 31 of the inner plug gasket 30 form a chemical bond (e.g., a covalent bond) through a chemical reaction, thereby firmly adhering the PP surface 41 and the rubber surface 31.
[0042] The heating temperature in the insert molding is not particularly limited as long as it is within a range in which the vulcanization of the silicone rubber progresses, the chemical bond formation reaction between the primer and the rubber surface 31 and the PP surface 41 progresses, and the plug substrate 40 is not thermally deformed to such an extent that its function is impaired.
[0043] The heating temperature is determined, for example, as a range in which the temperature range suitable for the vulcanization reaction by the vulcanizing agent contained in the silicone rubber raw material composition M overlaps the temperature range suitable for the chemical bond formation reaction by the primer, and the heat resistance temperature range of the polypropylene constituting the inside plug substrate 40. Specifically, the heating temperature is preferably a temperature at which the vulcanization reaction by the vulcanizing agent proceeds sufficiently depending on the type of vulcanizing agent used (for example, the recommended temperature for that vulcanizing agent).
[0044] The time for which the mold 100 is held at the above-mentioned heating temperature during insert molding is not particularly limited as long as it is within the range in which the insert molded body, that is, the plug member 21, is obtained. For example, depending on the type of vulcanizing agent used, a time for which the vulcanization reaction by the vulcanizing agent proceeds sufficiently (for example, the recommended time for that vulcanizing agent) is preferably used.
[0045] The manufacturing method of the inner plug member 21 may further include a secondary vulcanization step of performing secondary vulcanization of the inner plug member 21 obtained in the adhesion step. That is, when the inner plug member 21 is molded by insert molding, the inner plug member 21 removed from the mold 100 is held under heating to perform secondary vulcanization.
[0046] The heating temperature of the inner plug member 21 in the secondary vulcanization step is not particularly limited as long as it is within a range in which the effect of the secondary vulcanization can be obtained, but is preferably, for example, the recommended temperature of the vulcanizing agent. The time for which the inner plug member 21 is held at the heating temperature in the secondary vulcanization step is not particularly limited as long as it is within a range in which the effect of the secondary vulcanization can be obtained, but is preferably, for example, the recommended time of the vulcanizing agent.
[0047] Next, the inner plug member 21 and the beverage container 1 according to this embodiment will be described. The beverage container 1 includes an insulated double container 10. The insulated double container 10 includes an inner container 13 and an outer container 14, and an insulated space 15 is formed between the inner container 13 and the outer container 14.
[0048] Although there is no particular limitation on the materials constituting the inner container 13 and the outer container 14, the inner container 13 and the outer container 14 are preferably made of, for example, metal or glass, respectively. In the example shown in Figures 1 and 4, the inner container 13 and the outer container 14 of the double insulated container 10 are both made of stainless steel.
[0049] The inner container 13 and the outer container 14 are connected so as to form a sealed space therebetween. In the example shown in Fig. 1 and Fig. 4, the upper end of the inner container 13 and the upper end of the outer container 14 are connected by welding, and a heat-insulating space 15, which is a depressurized sealed space, is formed between the inner container 13 and the outer container 14. The heat-insulating double container 10 obtained in this manner is a so-called vacuum heat-insulating container.
[0050] The beverage container 1 includes an inner plug member 21. That is, in the example shown in Figures 1, 2 and 4, the beverage container 1 includes a plug 20 that covers the upper opening 11 of the insulated double container 10 in an openable and closable manner, and the plug 20 includes the inner plug member 21 and a cover member 22 that supports the inner plug member 21.
[0051] The cover member 22 is manufactured separately from the inner plug member 21, and the inner plug member 21 is attached to the cover member 22. The cover member 22 includes a canopy portion 22a disposed above the upper opening 11 of the insulating double container 10, and a cylindrical portion 22b covering the outer peripheral surface 11b of the upper opening 11.
[0052] The cover member 22 is attached to the insulated double container 10 by engaging an inner peripheral surface 22c of the cylindrical portion 22b with an outer peripheral surface 11b of the upper opening 11 of the insulated double container 10. Specifically, in the example shown in Fig. 1 and Fig. 4, the inner peripheral surface 22c of the cylindrical portion 22b of the cover member 22 and the outer peripheral surface 11b of the upper opening 11 of the insulated double container 10 are screwed together.
[0053] The cover member 22 may house the inside plug member 21. That is, in the example shown in Fig. 1, Fig. 2 and Fig. 4, the cover member 22 is formed in a bottomed tubular shape including a canopy portion 22a and a tubular portion 22b, and the inside plug member 21 is housed in a space surrounded by the canopy portion 22a and the tubular portion 22b.
[0054] The inner plug member 21 includes an inner plug gasket 30 which is a silicone rubber molded body, and an inner plug base material 40 which is a polypropylene molded body. In this embodiment, the inner plug member 21 is composed of the inner plug gasket 30 and the inner plug base material 40.
[0055] The inner plug member 21 is disposed in the beverage container 1 such that the inner plug gasket 30 thereof is in close contact with the inner circumferential surface 11a of the upper opening 11 of the thermally insulated double container 10. Specifically, a portion of the outer circumferential surface 32 of the inner plug gasket 30 (more specifically, the lower end of the outer circumferential surface 32) is in close contact with the inner circumferential surface 11a of the upper opening 11 of the thermally insulated double container 10.
[0056] In the beverage container 1, the inner stopper gasket 30 is in close contact with the inner surface 11a of the upper opening 11 of the insulated double container 10, effectively preventing the beverage in the insulated double container 10 from leaking between the inner stopper gasket 30 and the inner surface 11a.
[0057] As shown in Figures 1, 2 and 4, the stopper gasket 30 of this embodiment has a base 33 supported from above by a stopper substrate 40, and a cylindrical extension portion 34 extending downward from the radially outer end of the base 33, and the outer peripheral surface 34b of the extension portion 34 (part of the outer peripheral surface 32 of the stopper gasket 30) is in close contact with the inner peripheral surface 11a of the upper opening 11 of the insulated double container 10.
[0058] In addition, in the example shown in Figures 1 and 4, the inner plug gasket 30 is in close contact with a portion (reduced diameter portion) of the inner surface 11a of the insulated double container 10 that protrudes radially inward so as to reduce the inner diameter of the insulated double container 10.
[0059] When the inner plug gasket 30 is in close contact with the inner peripheral surface 11a of the upper opening 11 of the thermally insulated double container 10, the lower surface 35 of the inner plug gasket 30 is exposed within the upper opening 11. Specifically, in the example shown in Figs. 1 and 4, the lower surface 35 of the inner plug gasket 30 and the inner peripheral surface 34a of the extension portion 34 are exposed within the upper opening 11 of the thermally insulated double container 10.
[0060] Here, one of the characteristics of inside plug member 21 according to the present invention is that inside plug packing 30 and inside plug base material 40 are bonded together so as to be inseparable during normal use of beverage container 1.
[0061] In other words, for example, when a user of the beverage container 1 attempts to separate the inner plug gasket 30 and the inner plug base material 40 in order to clean the inner plug member 21, the inner plug gasket 30 and the inner plug base material 40 are firmly bonded to each other to such an extent that the user can recognize that the inner plug gasket 30 and the inner plug base material 40 cannot be separated.
[0062] In this regard, conventionally, in the inner plug member of a beverage container including a thermally insulated double container, a resin inner plug base material and a rubber inner plug packing are separably fitted together. This was to enable a user of the beverage container 1 to separate the inner plug packing and the inner plug base material and wash these components separately when washing the inner plug member.
[0063] However, for example, it is inevitable that a gap will form between the separable inner plug gasket and the inner plug base material, and as a result of using the beverage container, dirt may accumulate in the gap.
[0064] In addition, for example, if a user forgets to attach the inner plug gasket to the inner plug base material after separating and cleaning the inner plug gasket from the inner plug base material, the beverage container will be used without the inner plug gasket, and as a result, the beverage may leak from the upper opening of the insulated double container. In addition, for example, when beverage containers are displayed and sold, the inner plug gasket of the beverage container may be removed from the inner plug base material and stolen. In contrast, in the inner plug member 21 according to the present invention, the inner plug gasket 30 and the inner plug base material 40 are bonded inseparably, so that the above problem is effectively avoided.
[0065] Another characteristic feature of the inside plug member 21 according to the present invention is that a silicone rubber molded body is used as the inside plug packing 30 and a polypropylene molded body is used as the inside plug base material 40 .
[0066] Silicone rubber is an excellent material for forming the inner plug gasket 30 compared to other rubber materials in that it has low water absorption, maintains sufficient elasticity even at high and low temperatures, and has sufficient chemical resistance.
[0067] Furthermore, polypropylene is superior as a material for forming the inside plug base material 40 compared to other resins such as ABS resin, nylon, and polycarbonate in that it has low water absorption, sufficient strength and chemical resistance, and is inexpensive.
[0068] The inventors of the present invention therefore conducted extensive research into technical means for inseparably bonding silicone rubber and polypropylene, which had previously been thought to be difficult to bond firmly, and have now completed the present invention.
[0069] Specifically, in the inside plug member 21 according to the present invention, the rubber surface 31 of the inside plug packing 30 and the PP surface 41 of the inside plug substrate 40 are preferably bonded with a peel strength of 3.0 N / mm or more. In this case, the adhesive strength between the rubber surface 31 of the inside plug packing 30 and the PP surface 41 of the inside plug substrate 40 is not particularly limited as long as the peel strength is in the range of 3.0 N / mm or more, but the peel strength is preferably, for example, 4.0 N / mm or more, more preferably 5.0 N / mm or more, even more preferably 5.5 N / mm or more, and particularly preferably 6.0 N / mm or more. Since there is no particular problem due to a large peel strength relating to the adhesion between the rubber surface 31 of the inside plug packing 30 and the PP surface 41 of the inside plug substrate 40, the upper limit of the peel strength is not particularly limited.
[0070] In addition, the inner plug member 21 may be fixed to the cover member 22 in an inseparable manner (for example, by forced fitting with resin). In this case, for example, when a user of the beverage container 1 attempts to separate the inner plug member 21 and the cover member 22 in order to wash the plug 20, the inner plug member 21 and the cover member 22 are firmly fixed to each other to an extent that the user can recognize that the inner plug member 21 and the cover member 22 cannot be separated.
[0071] When inside plug member 21 is manufactured using a primer as described above, rubber surface 31 of inside plug packing 30 and PP surface 41 of inside plug substrate 40 are bonded via a component derived from the primer.
[0072] In other words, in this case, a chemical bond (e.g., a covalent bond) is formed between the silicone rubber that constitutes the rubber surface 31 of the stopper gasket 30 and the primer-derived component, and a chemical bond (e.g., a covalent bond) is also formed between the primer-derived component and the polypropylene that constitutes the PP surface 41 of the stopper substrate 40.
[0073] The primer-derived component is a chemical structure corresponding to a portion of the primer molecule remaining between rubber surface 31 and PP surface 41 as a result of chemical bonds being formed by a chemical reaction between the primer and the silicone rubber that constitutes rubber surface 31 of inner plug gasket 30 and the modified polypropylene that constitutes PP surface 41 of inner plug substrate 40 (more specifically, reactive functional groups introduced into PP surface 41 by the surface modification treatment) (for example, the chemical structure of a portion of the primer molecule that does not change by the chemical reaction that forms the above-mentioned chemical bonds).
[0074] Specifically, for example, when alkoxysilane is used as a primer, a chemical structure corresponding to a part of the alkoxysilane molecule is contained between the rubber surface 31 of the inside plug gasket 30 and the PP surface 41 of the inside plug substrate 40.
[0075] The inside plug substrate 40 may have a modified PP surface 41. In other words, when the PP surface 41 of the inside plug substrate 40 is subjected to a surface modification treatment during the manufacturing process of the inside plug member 21, the inside plug substrate 40 included in the manufactured inside plug member 21 has the modified PP surface 41.
[0076] The modified PP surface 41 of the stopper substrate 40 contains, for example, a reactive functional group-derived component introduced by the surface modification treatment in addition to the above-mentioned primer-derived component. The reactive functional group-derived component is a chemical structure corresponding to a part of the reactive functional group remaining on the PP surface 41 as a result of the reactive functional group on the PP surface 41 of the stopper substrate 40 and the primer forming a chemical bond by chemical reaction.
[0077] Also, for example, reactive functional groups that are not consumed in the chemical reaction with the primer may remain on PP surface 41 of inside plug substrate 40 that is bonded to rubber surface 31 of inside plug packing 30.
[0078] Furthermore, for example, if reactive functional groups are introduced by surface modification treatment into the portion of the PP surface 41 of the plug substrate 40 that is not adhered to the rubber surface 31 of the plug gasket 30 during the manufacturing process of the plug member 21, the plug substrate 40 may have a modified PP surface 41 (the PP surface 41 into which the reactive functional groups have been introduced) that is not adhered to the rubber surface 31.
[0079] The reactive functional group contained in the PP surface 41 of the inside plug substrate 40 may be, for example, a polar functional group, preferably a polar functional group containing an oxygen atom, and particularly preferably one or more selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), and a carbonyl group (-C(=O)-). The PP surface 41 that has been subjected to the surface modification treatment has higher hydrophilicity than the PP surface 41 that has not been subjected to the surface modification treatment.
[0080] The inner plug member 21 is preferably an insert-molded body. That is, the inner plug member 21 is preferably manufactured by insert molding as described above (FIGS. 3C and 5C).
[0081] In the inside plug member 21, the inside plug base material 40 preferably has a flange portion 42 that extends downward and penetrates into the inside plug packing 30. That is, in the examples shown in Figures 1, 2, and 4, the inside plug base portion 40 has a cylindrical flange portion 42 that extends downward.
[0082] As a result of the flange portion 42 of the inside plug substrate 40 penetrating into the inside of the inside plug gasket 30, the inside plug gasket 30 (specifically, the base portion 33) covers the flange portion 42. In other words, the surface of the flange portion 42 of the inside plug substrate 40 is part of the PP surface 41, and is adhered to the rubber surface 31 of the inside plug gasket 30. For this reason, by the inside plug substrate 40 having the flange portion 42, the adhesion area between the PP surface 41 of the inside plug substrate 40 and the rubber surface 31 of the inside plug gasket 30 is effectively increased.
[0083] Moreover, it is preferable that the flange portion 42 has a tapered shape in which the radial thickness increases from its lower end (tip) toward the upper side (see, for example, FIG. 2). By forming the flange portion 42 in such a tapered shape, a primer can be easily and reliably applied to the surfaces of the flange portion 42 (the lower end face, the radially outer side surface, and the radially inner side surface), and the adhesive strength between the inside plug substrate 40 and the inside plug packing 30 can be effectively increased.
[0084] The inner plug base material 40 may not have a flange portion that extends radially (for example, radially outward) and penetrates the inner plug gasket 30. That is, in a conventional inner plug member in which the inner plug gasket and the inner plug base material are separable, a flange portion that extends radially and penetrates the inner plug gasket has been provided on the inner plug base material to prevent the inner plug gasket from axially detaching from the inner plug base material when the inside of the insulating double container is cooled and reduced pressure.
[0085] However, in the inside plug member 21 according to the present invention, the inside plug packing 30 and the inside plug base material 40 are inseparably bonded together, so that there is no need to provide the conventional flange portion extending in the radial direction.
[0086] Furthermore, for example, in insert molding, not only the silicone rubber raw material composition M but also the center plug substrate 40 is pressed in the vertical direction under heat (FIGS. 3C and 5C), so if the center plug substrate 40 has a flange portion extending in the radial direction, the flange portion may be deformed by the insert molding. For this reason, the center plug substrate 40 may have a flange portion extending in the radial direction, but preferably has a flange portion 42 extending downward.
[0087] The plug substrate 40 may have a bridge portion 44 that extends in the radial direction and is sandwiched by the plug gasket 30 from above and below (see Figs. 2 and 3D). That is, in the insert molding, the silicone rubber raw material composition M penetrates into gaps (not shown) formed above and below the bridge portion 44 of the plug substrate 40 and hardens, so that in the obtained plug member 21, the bridge portion 44 is embedded in the plug gasket 30. By the plug substrate 40 having the bridge portion 44, the adhesive area between the plug substrate 40 and the plug gasket 30 in the plug member 21 is increased, effectively increasing the adhesive strength, and effectively preventing the plug gasket 30 from detaching from the plug substrate 40 in the axial direction.
[0088] The inside plug substrate 40 may have a bank portion 43 that extends downward and covers a part (specifically, the upper end portion of the outer circumferential surface 32) of the inside plug packing 30 (specifically, the base portion 33). In this case, the lower surface 43a of the bank portion 43 may not be covered by the inside plug packing 30. The bank portion 43 of the inside plug substrate 40 serves to hold back the silicone rubber raw material composition M so that the silicone rubber raw material composition M does not protrude radially outward during, for example, insert molding.
[0089] The inside plug packing 30 may have an annular protrusion 36 that protrudes radially outward in an annular shape on the outer circumferential surface 32. It is preferable that the annular protrusion 36 does not protrude radially outward beyond the outer circumferential surface 34b of the extension portion 34. In other words, it is preferable that the radially outer end (protruding tip) of the annular protrusion 36 is located radially inward beyond the outer circumferential surface 34b of the extension portion 34. The annular protrusion 36 of the inside plug packing 30 is formed by the silicone rubber raw material composition M slightly protruding radially outward at the boundary surface between the lower mold 101 and the upper mold 102 during the insert molding shown in Figures 3C and 5C.
[0090] In the beverage container 1, the inner plug member 21 may be a member capable of blocking the entire radial cross-section of the upper opening 11 of the insulated double container 10, or it may be a member capable of blocking only a portion of the radial cross-section of the upper opening 11.
[0091] 1, the inner plug member 21 closes the entire radial cross section of the upper opening 11 of the thermally insulated double container 10. Specifically, the base 33 of the inner plug packing 30 has a central portion 37 that covers the radial central portion of the upper opening 11 of the thermally insulated double container 10, and is in close contact with the inner circumferential surface a of the upper opening 11, thereby closing the entire radial cross section of the upper opening 11.
[0092] In this way, the inside plug gasket 30 having the central portion 37 covers the entire PP surface 41 below the inside plug base material 40. As a result, the adhesive area between the inside plug gasket 30 and the inside plug base material 40 is increased, and the adhesive strength is effectively increased, compared to when the inside plug gasket 30 does not have the central portion 37.
[0093] 4, the inner plug member 21 closes only a portion of the radial cross section of the upper opening 11 of the thermally insulated double container 10. Specifically, a communication hole 23 that axially penetrates the inner plug packing 30 and the inner plug base material 40 is formed in the radial central portion of the inner plug member 21. Therefore, the inner plug member 21 closes only the radial outer periphery of the upper opening 11 of the thermally insulated double container 10, and does not close the radial central portion of the upper opening 11.
[0094] In the beverage container 1, the plug 20 may be attached to the insulating double container 10 in its entirety so as to be openable and closable, or may be attached to the insulating double container 10 in its entirety so as to be openable and closable.
[0095] 1, the stopper 20 is attached to the insulated double container 10 in an openable and closable manner. Specifically, in this example, by removing the entire stopper 20 from the insulated double container 10, the upper opening 11 of the insulated double container 10 is connected to the outside, and the beverage container 1 is in an open state. With the beverage container 1 in an open state, a user can pour the beverage contained in the insulated double container 10 through the upper opening 11 of the insulated double container 10.
[0096] 4, the plug 20 is attached to the insulated double container 10 so that a portion of the plug 20 can be opened and closed. Specifically, in this example, the canopy portion 22a of the cover member 22 of the plug 20 is attached to the cylindrical portion 22b via the hinge portion 22d so as to be rotatable.
[0097] Then, with the cylindrical portion 22b of the cover member 22 attached to the outer peripheral surface 11b of the upper opening 11 of the double insulated container 10 and the inner stopper member 21 attached to the cylindrical portion 22b (with the inner stopper gasket 30 in close contact with the inner peripheral surface 11a of the upper opening 11), by rotating the canopy portion 22a of the cover member 22, the upper opening 11 of the insulated double container 10 is connected to the outside via the communication hole 23 of the inner stopper member 21, and the beverage container 1 is in an open state.
[0098] When the beverage container 1 is in an open state, a user can pour out the beverage contained in the insulated double container 10 through the upper opening 11 of the insulated double container 10 and the communication hole 23 of the inner plug member 21.
[0099] In the beverage container 1, the inner plug gasket 30 may be disposed within the upper opening 11 of the thermally insulated double container 10, as shown in Figures 1 and 4. Specifically, in this case, the inner plug gasket 30 is disposed entirely below the upper end 11c of the upper opening 11 of the thermally insulated double container 10 (more specifically, the upper end of the thermally insulated double container). In addition, a portion of the inner plug base material 40 may also be disposed within the upper opening 11 of the thermally insulated double container 10.
[0100] Another aspect of the method according to the present embodiment is a method for manufacturing a beverage container 1, which includes an attachment step of attaching an inner plug member 21 to the insulated double container 10. In the attachment step, the inner plug member 21 is attached to the insulated double container 10 such that the inner plug gasket 30 of the inner plug member 21 is in close contact with the inner circumferential surface 11a of the upper opening 11 of the insulated double container 10.
[0101] When manufacturing a beverage container 1 having a stopper 20 including an inner stopper member 21, the stopper 20 is attached to the insulated double container 10 so that the inner stopper gasket 30 is in close contact with the inner surface 11a of the upper opening 11 of the insulated double container 10.
[0102] The method for manufacturing the beverage container 1 may further include a step of manufacturing the inner plug member 21 by the above-mentioned method for manufacturing the inner plug member 21. In this case, the method for manufacturing the beverage container 1 includes the above-mentioned bonding step. The method for manufacturing the beverage container 1 may further include the above-mentioned surface modification step and primer application step. That is, the method for manufacturing the beverage container 1 may include the surface modification step, primer application step, bonding step, and attachment step.
[0103] Next, a specific example according to this embodiment will be described. EXAMPLES
[0104] [Example 1] The inside plug member 21 and beverage container 1 shown in Figures 1 and 2 were manufactured. First, the inside plug base material 40 was molded by injection molding of polypropylene. Next, as shown in Figure 3A, a surface modification treatment was applied to the PP surface 41 of the inside plug base material 40. Furthermore, as shown in Figure 3B, a primer was applied to the PP surface 41 of the inside plug base material 40 that had been subjected to the surface modification treatment.
[0105] Then, insert molding was performed as shown in Fig. 3C. That is, a silicone rubber raw material composition M containing a silicone rubber raw material and a vulcanizing agent was pressed between the heated lower mold 101 and upper mold 102 onto the primer-coated PP surface 41 of the inside plug substrate 40 fixed to the lower mold 101, and the temperature and time were maintained within a range where the vulcanization was sufficiently advanced and the polypropylene could withstand the heat.
[0106] In this way, as shown in Fig. 3D, a center plug member 21 was obtained as an insert molded body composed of a center plug packing 30, which was a silicone rubber molded body, and a center plug base material 40, which was a polypropylene molded body. Then, the center plug member 21 was removed from the mold 100 and placed in an oven equipped with an exhaust mechanism, and secondary vulcanization was carried out by maintaining it at a temperature and for a time at which vulcanization sufficiently proceeded.
[0107] In the manufactured inner plug member 21, the inner plug packing 30 and the inner plug base material 40 were firmly bonded, and it was practically impossible to separate them by pulling them by hand. Then, the inner plug member 21 was attached to a separately manufactured cover member 22 to manufacture the plug 20 as shown in Fig. 2. Furthermore, the plug 20 was attached to a separately manufactured insulated double container 10 to manufacture the beverage container 1 as shown in Fig. 1.
[0108] [Example 2] In Example 2-1, the peel strength between a silicone rubber test piece and a polypropylene test piece in an insert molding composed of the silicone rubber test piece and the polypropylene test piece was evaluated by a method in accordance with JIS K6256-2.
[0109] First, a polypropylene test piece was molded by injection molding of polypropylene. Next, one surface of the polypropylene test piece was subjected to a surface modification treatment. Furthermore, a primer was applied to the surface of the polypropylene test piece that had been subjected to the surface modification treatment.
[0110] A silicone rubber raw material composition containing a silicone rubber raw material and a vulcanizing agent was then placed on the primer-coated surface of the polypropylene test piece fixed to the lower mold, and the resulting mixture was pressed between the heated lower and upper molds. The temperature and time were maintained at a range where vulcanization had progressed sufficiently and where the polypropylene could withstand the heat, thereby performing insert molding.
[0111] In this way, an insert molded article was obtained that was composed of a silicone rubber test piece, which was a silicone rubber molded article, and a polypropylene test piece, which was a polypropylene molded article. The insert molded article was then removed from the mold and placed in an oven equipped with an exhaust mechanism, and held at a temperature and for a time at which vulcanization was sufficiently advanced, thereby carrying out secondary vulcanization.
[0112] Then, using a commercially available test device (a precision universal testing machine Autograph equipped with a rubber adhesion tester type 2 (90 degrees) as a test jig, manufactured by Shimadzu Corporation), a 90° peel test was performed between the silicone rubber test piece and the polypropylene test piece in the insert molding, and the test force (N) relative to the displacement (mm) was measured and recorded. The peel strength (N / mm) was calculated by dividing the maximum peel force (N) measured in the peel test by the width of the test piece (25 mm).
[0113] In Example 2-2, a composite test piece was obtained by bonding a silicone rubber test piece and a polypropylene test piece with an adhesive, and the peel strength between the silicone rubber test piece and the polypropylene test piece was evaluated using a method in accordance with JIS K6256-2.
[0114] First, a polypropylene test piece was molded in the same manner as in Example 2-1 above. Next, a primer included with a commercially available adhesive for plastics (Aron Alpha, Toa Gosei Co., Ltd.) that can be used for polypropylene and polyethylene was applied to one surface of the polypropylene test piece. Meanwhile, a silicone rubber test piece was molded by compression molding the same silicone rubber raw material composition as that used in Example 2-1 above.
[0115] Next, the primer-coated surface of the polypropylene test piece was bonded to one surface of the silicone rubber test piece using the commercially available adhesive (Aron Alpha, Toa Gosei Co., Ltd.) The peel strength between the silicone rubber test piece and the polypropylene test piece in the composite test piece was then evaluated in the same manner as in Example 2-1 above.
[0116] In Example 2-3, the peel strength between the silicone rubber test piece and the polypropylene test piece in the composite test piece was evaluated in the same manner as in Example 2-2 above, except that no primer was applied to the surface of the polypropylene test piece, and a commercially available adhesive that can also be used on polypropylene and polyethylene (Scotch (registered trademark), Ultra-Strong Adhesive Premier Gold Super Multi-Purpose, 3M Japan Ltd.) was used as the adhesive.
[0117] In Example 2-4, the peel strength between the silicone rubber test piece and the polycarbonate test piece in the insert molded body was evaluated in the same manner as in Example 2-1 above, except that a polycarbonate test piece obtained by injection molding of polycarbonate was used instead of the polypropylene test piece.
[0118] The maximum peel force (N) and peel strength (N / mm) measured in each of Examples 2-1, 2-2, 2-3, and 2-4 are shown in Figure 6. The maximum peel force shown in Figure 6 is the arithmetic average of the four maximum peel forces measured using four test pieces in each example.
[0119] As shown in Figure 6, the peel strengths of Examples 2-2 and 2-3, which used an adhesive, were 1.5 N / mm and 0.8 N / mm, respectively, while the peel strengths of Examples 2-1 and 2-4, which used insert molding, were 6.2 N / mm and 5.4 N / mm, respectively. In other words, the peel strength achieved by insert molding was significantly greater than that achieved by using an adhesive.
[0120] Moreover, the peel strength achieved in Example 2-1 using the polypropylene test piece was greater than the peel strength achieved in Example 2-4 using the polycarbonate test piece. That is, in Example 2-1, by using polypropylene suitable for the inner plug member 21 of the beverage container 1, a higher adhesive strength was achieved than when polycarbonate was used. [Explanation of symbols]
[0121] 1 beverage container, 10 insulated double container, 11 upper opening, 11a inner peripheral surface, 11b outer peripheral surface, 11c upper end, 12 bottom surface, 13 inner container, 14 outer container, 15 insulated space, 20 stopper, 21 middle stopper member, 22 cover member, 22a top portion, 22b cylindrical portion, 22c inner peripheral surface, 22d hinge portion, 23 communication hole, 30 middle stopper packing, 31 silicone rubber surface (rubber surface), 32 outer peripheral surface, 33 base portion, 34 extension portion, 34a inner peripheral surface, 34b outer peripheral surface, 35 lower surface, 36 annular protrusion portion, 37 center portion, 40 middle stopper base material, 41 polypropylene surface (PP surface), 42 flange portion, 43 bank portion, 43a lower surface, 44 bridge portion, 100 Mold, 101 lower mold, 102 upper mold, A axis, M silicone rubber raw material composition.
Claims
1. A method for manufacturing a composite member including a first member and a second member, comprising: A method for producing a composite member, comprising: a bonding step of bonding a silicone rubber surface of the first member, which is a silicone rubber molded body, to a polypropylene surface of the second member, which is a polypropylene molded body.
2. a surface modification step of performing a surface modification treatment on the polypropylene surface of the second member; A primer application step of applying a primer to the polypropylene surface on which the surface modification treatment of the second member has been performed; Further comprising: In the bonding step, the silicone rubber surface of the first member and the polypropylene surface to which the primer is applied of the second member are bonded to each other. A method for producing the composite member according to claim 1.
3. In the bonding step, the silicone rubber surface of the first member and the polypropylene surface of the second member are bonded to each other by insert molding. A method for producing the composite member according to claim 1 or 2.
4. In the bonding step, the silicone rubber surface and the polypropylene surface are bonded to each other with a peel strength of 3.0 N / mm or more as measured by a method in accordance with JIS K6256-2. A method for producing the composite member according to any one of claims 1 to 3.
5. The composite member is An inner plug member for a beverage container including a thermally insulated double container, The first member includes an inner plug gasket that is in close contact with the inner circumferential surface of the upper opening of the insulating double container, The second member includes a plug base material supporting the plug packing. A method for producing the composite member according to any one of claims 1 to 4.
6. A first member which is a silicone rubber molded body; A second member which is a polypropylene molded body; Including, A composite member, wherein a silicone rubber surface of the first member and a polypropylene surface of the second member are bonded to each other.
7. the silicone rubber surface of the first member and the polypropylene surface of the second member are bonded to each other via a component derived from a primer; The composite member according to claim 6.
8. The second member has a modified polypropylene surface. The composite member according to claim 7.
9. The composite member is an insert molding. A composite member according to any one of claims 6 to 8.
10. the silicone rubber surface and the polypropylene surface are bonded with a peel strength of 3.0 N / mm or more as measured by a method in accordance with JIS K6256-2; A composite member according to any one of claims 6 to 9.
11. The composite member is An inner plug member for a beverage container including a thermally insulated double container, The first member includes an inner plug gasket that is in close contact with the inner circumferential surface of the upper opening of the insulating double container, The second member includes a plug base material supporting the plug packing. A composite member according to any one of claims 6 to 10.
12. A thermally insulated double container, The inside plug member according to claim 11 , 2. A beverage container comprising:
13. The method includes the step of attaching the inner plug member according to claim 11 to an insulating double container. A method for manufacturing beverage containers.
14. The method of claim 5 further comprising the step of manufacturing the plug member. A method for manufacturing a beverage container according to claim 13.
Citation Information
Patent Citations
Plug body for liquid container
JP1996071005A
Highly airtight container with lid
JP2007204075A
Cap with gasket
JP2013169978A
Inside plug of plug member
JP2016007296A
Cap unit and container with cap
JP2018144840A
Cited By
Functional film and method for manufacturing the same
US12305037B2