Detection method

The film forming apparatus uses infrared spectroscopy to analyze film formation on substrates with complex patterns, addressing the challenge of detecting film quality on sidewalls and bottoms of recesses, enhancing film quality and productivity by adjusting process parameters based on differential data analysis.

JP2024152915AActive Publication Date: 2024-10-25TOKYO ELECTRON LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024139952
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-10-25
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

Existing methods fail to accurately detect the state of films formed on substrates with complex patterns, particularly in nanoscale recesses, due to differences between monitor substrates and actual substrates used in semiconductor manufacturing, leading to deteriorated film quality on sidewalls and bottoms of recesses.

Method used

A film forming apparatus using infrared spectroscopy to measure and analyze the state of films on substrates with patterns by comparing pre- and post-film formation data, enabling detection of chemical bonds and film quality through Fourier Transform Infrared Spectroscopy (FT-IR) and extracting differential data to adjust process parameters.

Benefits of technology

Enables precise detection of film quality on substrates with complex patterns, allowing for improved film formation by adjusting process parameters to enhance nitridation and uniformity, thereby improving film quality and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152915000001_ABST
    Figure 2024152915000001_ABST
Patent Text Reader

Abstract

To detect a status of a film during film deposition.SOLUTION: A detection method for detecting a status of a film during film deposition, includes the steps of: preparing a substrate in a chamber; depositing a film on the substrate by repeating a plurality of steps including an adsorption step of depositing a film on the substrate by ALD (Atomic Layer Deposition), wherein the ALD supplies a raw material gas into the chamber to be adsorbed to the substrate, and a reaction step of supplying a reaction gas into the chamber and making it react with the raw material gas to form a film on the substrate, and acquiring measurement data by irradiating the substrate with infrared light in each step; and extracting a difference in the measurement data between before and after each step.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to detection methods. [Background technology]

[0002] Patent Document 1 discloses a technology in which a film-formation substrate and a monitor substrate are placed on top of each other to form a film, the thin film formed on the monitor substrate is analyzed by infrared spectroscopy, and the quality of the film formed on the film-formation substrate is optimized based on the analytical values. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-56010 Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a technique for detecting the state of a film during film formation. [Means for solving the problem]

[0005] A detection method according to one aspect of the present disclosure is a detection method for detecting the state of a film during film formation, the detection method including a step of preparing a substrate in a chamber and a step of forming a film on the substrate by ALD (Atomic Layer Deposition), in which a film is formed on the substrate by repeating a plurality of steps including an adsorption step of supplying a source gas into the chamber and causing it to be adsorbed onto the substrate, and a reaction step of supplying a reactive gas into the chamber and reacting it with the source gas to form a film on the substrate, and in each step, a step of acquiring measurement data by irradiating the substrate with infrared light, and a step of extracting a difference in the measurement data before and after each step. Effect of the Invention

[0006] According to the present disclosure, the state of a film during film formation can be detected. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a film forming apparatus according to an embodiment. [Diagram 2] FIG. 2 is a diagram for explaining film formation by plasma according to the embodiment. [Figure 3A] FIG. 3A is a diagram illustrating the analysis by TEM-EDX. [Figure 3B] FIG. 3B is a diagram illustrating the analysis by TEM-EDX. [Figure 4] FIG. 4 is a diagram illustrating a conventional FT-IR analysis. [Diagram 5] FIG. 5 is a diagram illustrating the flow of the film forming method according to the embodiment. [Figure 6] FIG. 6 is a diagram illustrating difference data according to the embodiment. [Figure 7] FIG. 7 is a diagram illustrating an example of a plasma ALD process according to the embodiment. [Figure 8A] FIG. 8A is a diagram showing an example of a substrate on which a SiN film is formed according to the embodiment. [Figure 8B] FIG. 8B is a diagram showing an example of a silicon substrate on which a SiN film is formed according to a comparative example. [Figure 9] FIG. 9 is a diagram showing an example of absorbance for each wave number of infrared light. [Figure 10A] FIG. 10A is a diagram showing an example of absorbance for each wave number of infrared light. [Figure 10B] FIG. 10B is a diagram showing an example of absorbance for each wave number of infrared light. [Figure 10C] FIG. 10C is a diagram showing an example of absorbance for each wave number of infrared light. [Figure 11] FIG. 11 is a schematic configuration diagram showing another example of the film forming apparatus according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the detection method disclosed in the present application will be described in detail with reference to the drawings. Note that the detection method disclosed is not limited to the embodiment.

[0009] In the manufacture of semiconductor devices, a film is formed on a substrate such as a semiconductor wafer on which a pattern including recesses is formed by a film forming apparatus. The film forming apparatus places the substrate in a chamber (processing vessel) that is kept at a predetermined vacuum level, supplies a film forming source gas into the chamber, and generates plasma to form a film on the substrate. Known film forming techniques include plasma CVD (Chemical Vapor Deposition) and plasma ALD (Atomic Layer Deposition).

[0010] However, as patterns formed on substrates become finer, film quality on the sidewalls and bottoms of recesses in the patterns tends to deteriorate when films are formed using plasma. Therefore, in addition to the actual substrates on which semiconductor devices are manufactured, films are formed on flat monitor substrates, and the films formed on the monitor substrates are analyzed by infrared spectroscopy to infer the state of the films formed on the actual substrates.

[0011] However, the state of the film formed on the actual substrate and the monitor substrate differs, and even if the film formed on the monitor substrate is analyzed by infrared spectroscopy, the state of the film formed on the actual substrate cannot be determined.

[0012] Therefore, a technology for detecting the state of a film formed on a substrate on which a pattern including recesses is formed is desired.

[0013] [Embodiment] [Configuration of deposition equipment] Next, an embodiment will be described. First, a film forming apparatus 100 according to an embodiment will be described. FIG. 1 is a schematic cross-sectional view showing an example of a schematic configuration of the film forming apparatus 100 according to an embodiment. In one embodiment, the film forming apparatus 100 is an apparatus that forms a film on a substrate W. The film forming apparatus 100 shown in FIG. 1 has a chamber 1 that is airtight and electrically grounded. This chamber 1 is cylindrical and made of, for example, aluminum, nickel, or the like having an anodized coating formed on its surface. A mounting table 2 is provided in the chamber 1.

[0014] The mounting table 2 is formed of a metal such as aluminum or nickel. A substrate W such as a semiconductor wafer is placed on the upper surface of the mounting table 2. The mounting table 2 horizontally supports the placed substrate W. The lower surface of the mounting table 2 is electrically connected to a support member 4 formed of a conductive material. The mounting table 2 is supported by the support member 4. The support member 4 is supported by the bottom surface of the chamber 1. The lower end of the support member 4 is electrically connected to the bottom surface of the chamber 1 and is grounded via the chamber 1. The lower end of the support member 4 may be electrically connected to the bottom surface of the chamber 1 via a circuit adjusted to reduce the impedance between the mounting table 2 and the ground potential.

[0015] The mounting table 2 has a built-in heater 5, and the heater 5 can heat the substrate W mounted on the mounting table 2 to a predetermined temperature. The mounting table 2 may have a flow path (not shown) formed therein for circulating a coolant, and a coolant whose temperature is controlled by a chiller unit provided outside the chamber 1 may be circulated and supplied within the flow path. The mounting table 2 may control the substrate W to a predetermined temperature by heating with the heater 5 and cooling with the coolant supplied from the chiller unit. Note that the heater 5 may not be installed, and the temperature of the mounting table 2 may be controlled only by the coolant supplied from the chiller unit.

[0016] An electrode may be embedded in the mounting table 2. A DC voltage is supplied to this electrode, which generates an electrostatic force that causes the mounting table 2 to attract the substrate W placed on its upper surface. The mounting table 2 is also provided with lifting pins (not shown) for transferring the substrate W between the mounting table 2 and a transfer mechanism (not shown) provided outside the chamber 1.

[0017] A showerhead 16 formed in a substantially disk shape is provided above the mounting table 2 on the inner surface of the chamber 1. The showerhead 16 is supported on the upper part of the mounting table 2 via an insulating member 45 such as ceramics. This electrically insulates the chamber 1 from the showerhead 16. The showerhead 16 is made of a conductive metal such as nickel.

[0018] The shower head 16 has a top plate member 16a and a shower plate 16b. The top plate member 16a is provided so as to close the inside of the chamber 1 from above. The shower plate 16b is provided below the top plate member 16a so as to face the mounting table 2. A gas diffusion space 16c is formed in the top plate member 16a. The top plate member 16a and the shower plate 16b have a large number of gas discharge holes 16d formed in a dispersed manner and opening toward the gas diffusion space 16c.

[0019] The top plate member 16a is formed with a gas inlet 16e for introducing various gases into the gas diffusion space 16c. The gas inlet 16e is connected to a gas supply path 15a. The gas supply path 15a is connected to a gas supply unit 15.

[0020] The gas supply unit 15 has gas supply lines connected to the gas supply sources of various gases used in film formation. Each gas supply line branches appropriately according to the film formation process, and is provided with control devices for controlling the flow rate of the gas, such as valves such as an opening / closing valve and a flow rate controller such as a mass flow controller. The gas supply unit 15 can control the flow rate of various gases by controlling the control devices, such as the opening / closing valve and the flow rate controller, provided on each gas supply line.

[0021] The gas supply unit 15 supplies various gases used in film formation to the gas supply path 15a. For example, the gas supply unit 15 supplies a raw material gas for film formation to the gas supply path 15a. The gas supply unit 15 also supplies a purge gas and a reactive gas that reacts with the raw material gas to the gas supply path 15a. The gas supplied to the gas supply path 15a is diffused in the gas diffusion space 16c and discharged from each gas discharge hole 16d.

[0022] The space surrounded by the lower surface of the shower plate 16b and the upper surface of the mounting table 2 forms a processing space where a film formation process is performed. The shower plate 16b is paired with the mounting table 2, which is grounded via the support member 4 and the chamber 1, and is configured as an electrode plate for forming a capacitively coupled plasma (CCP) in the processing space. The shower head 16 is connected to a high-frequency power source 10 via a matching device 11, and the above-mentioned CCP is formed by supplying high-frequency power (RF power) to a gas supplied from the high-frequency power source 10 to the processing space 40 via the shower head 16. Note that the high-frequency power source 10 may be connected to the mounting table 2 instead of being connected to the shower head 16, and the shower head 16 may be grounded. In this embodiment, the parts that perform film formation, such as the shower head 16, the gas supply unit 15, and the high-frequency power source 10, correspond to the film formation unit of the present disclosure.

[0023] An exhaust port 71 is formed at the bottom of the chamber 1, and an exhaust device 73 is connected to this exhaust port 71 via an exhaust pipe 72. The exhaust device 73 has a vacuum pump and a pressure adjustment valve, and by operating this vacuum pump and pressure adjustment valve, the inside of the chamber 1 can be reduced in pressure and adjusted to a predetermined vacuum level.

[0024] The side wall of the chamber 1 is provided with windows 80a and 80b at positions facing each other across the mounting table 2. The windows 80a and 80b are fitted with a member having transparency to infrared light, such as quartz, and are sealed. An irradiation unit 81 that irradiates infrared light is provided outside the window 80a. A detection unit 82 that can detect infrared light is provided outside the window 80b. The positions of the window 80a and the irradiation unit 81 are adjusted so that the infrared light irradiated from the irradiation unit 81 is irradiated to the substrate W through the window 80a. The positions of the window 80b and the detection unit 82 are adjusted so that the infrared light reflected by the substrate W is incident on the detection unit 82 through the window 80b. A loading / unloading port (not shown) for loading and unloading the substrate W is provided on a side wall of the chamber 1 different from the windows 80a and 80b. A gate valve for opening and closing the loading / unloading port is provided at the loading / unloading port.

[0025] The irradiation unit 81 is disposed so that the irradiated infrared light strikes a predetermined region near the center of the substrate W through the window 80a. For example, the irradiation unit 81 irradiates an area of ​​the substrate W within a range of about 1 to 10 mm with the infrared light. The detection unit 82 is disposed so that the infrared light reflected from the predetermined region of the substrate W enters through the window 80b.

[0026] The film forming apparatus 100 according to this embodiment uses infrared spectroscopy (IR) to determine the absorbance for each wave number of the infrared light reflected by the substrate W, thereby detecting the state of the film formed on the substrate W. Specifically, the film forming apparatus 100 uses Fourier transform infrared spectroscopy (FT-IR) to determine the absorbance for each wave number of the reflected infrared light, thereby detecting the substance contained in the film formed on the substrate W.

[0027] The irradiation unit 81 incorporates a light source that emits infrared light, and optical elements such as mirrors and lenses, and is capable of irradiating interfered infrared light. For example, the irradiation unit 81 splits the intermediate portion of the optical path of the infrared light generated by the light source until it is emitted to the outside into two optical paths using a half mirror or the like, and varies the optical path length of one with respect to the optical path length of the other to change the optical path difference and cause interference, thereby irradiating infrared light of various interference waves with different optical path differences. Note that the irradiation unit 81 may be provided with a plurality of light sources, and the infrared light of each light source may be controlled by optical elements to be capable of irradiating infrared light of various interference waves with different optical path differences.

[0028] The detection unit 82 detects the signal intensities of infrared light of various interference waves reflected by the substrate W. In this embodiment, the parts that perform infrared spectroscopy measurement, such as the irradiation unit 81 and the detection unit 82, correspond to the measurement unit of the present disclosure.

[0029] The operation of the film forming apparatus 100 configured as above is generally controlled by a control unit 60. To the control unit 60, a user interface 61 and a storage unit 62 are connected.

[0030] The user interface 61 is composed of an operation unit such as a keyboard through which a process manager inputs commands to manage the film forming apparatus 100, and a display unit such as a display that visualizes and displays the operating status of the film forming apparatus 100. The user interface 61 accepts various operations. For example, the user interface 61 accepts a predetermined operation to instruct the start of plasma processing.

[0031] The storage unit 62 stores programs (software) for implementing various processes executed in the film forming apparatus 100 under the control of the control unit 60, and data such as processing conditions and process parameters. The programs and data may be stored in a computer-readable computer recording medium (e.g., a hard disk, a CD, a flexible disk, a semiconductor memory, etc.). Alternatively, the programs and data may be transmitted from other devices at any time via, for example, a dedicated line and used online.

[0032] The control unit 60 is, for example, a computer including a processor, a memory, etc. The control unit 60 reads out a program and data from the storage unit 62 based on an instruction from a user interface 61, etc., and controls each unit of the film forming apparatus 100 to execute the process of a film forming method described later.

[0033] The control unit 60 is connected to the irradiation unit 81 and the detection unit 82 via an interface (not shown) that inputs and outputs data, and inputs and outputs various information. The control unit 60 controls the irradiation unit 81 and the detection unit 82. For example, the irradiation unit 81 irradiates various interference waves with different optical path differences based on control information from the control unit 60. In addition, the control unit 60 receives information on the signal intensity of infrared light detected by the detection unit 82.

[0034] Incidentally, semiconductor devices are becoming finer, and patterns formed on a substrate W also have complex nanoscale shapes. In film formation using plasma, the film quality of the sidewalls and bottoms of recesses included in a nanoscale fine pattern is likely to deteriorate. FIG. 2 is a diagram for explaining film formation using plasma according to an embodiment. FIG. 2 shows a substrate W. A pattern 90 including nanoscale recesses 90a is formed on the substrate W. In film formation using plasma, ions and radicals have difficulty reaching the sidewalls and bottoms of the recesses 90a, and the film quality of the sidewalls and bottoms of the recesses 90a is likely to deteriorate. In order to improve the film quality, it is necessary to analyze the composition of the film on the sidewalls and bottoms of the recesses 90a.

[0035] Techniques for analyzing the deposited film include, for example, energy dispersive X-ray spectroscopy such as TEM-EDX, and infrared spectroscopy such as Fourier transform infrared spectroscopy (FT-IR).

[0036] 3A and 3B are diagrams for explaining analysis by TEM-EDX. FIG. 3A shows a schematic diagram of a pattern 90 having a recess 90a on which a SiN film 91 is formed by plasma ALD. The SiN film 91 on the bottom 90b (Bottom), sidewall 90c (Side) and top surface 90d (Top) of the recess 90a was analyzed by TEM-EDX. FIG. 3B shows an example of the results of analysis of the SiN film 91 on the bottom 90b (Bottom), sidewall 90c (Side) and top surface 90d (Top) by TEM-EDX. The elemental composition of the SiN film 91 can be known by TEM-EDX.

[0037] FIG. 3B shows the ratios of N (nitrogen), O (oxygen), and Si (silicon) at the bottom 90b (Bottom), side wall 90c (Side), and top surface 90d (Top). The ratio of N is higher at the top surface 90d than at the bottom 90b and side wall 90c. The ratio of O is higher at the top surface 90d, side wall 90c, and bottom 90b in that order. The ratio of Si is lower at the top surface 90d than at the bottom 90b and side wall 90c. This result shows that there are differences in elemental composition at the bottom 90b, side wall 90c, and top surface 90d, and therefore more detailed analysis is required. However, although TEM-EDX can detect elements, it cannot detect chemical bonds. For example, it is not clear whether N is bonded to O or Si. Furthermore, light atoms such as H (hydrogen) cannot be detected by analysis using TEM-EDX.

[0038] FIG. 4 is a diagram for explaining a conventional FT-IR analysis. Conventionally, in FT-IR analysis, a film is formed on a flat monitor substrate, separate from the actual substrate W on which a semiconductor device is manufactured, and infrared light is irradiated onto the monitor substrate, and the light transmitted through or reflected by the monitor substrate is analyzed to infer the state of the film formed on the actual substrate W. FIG. 4 shows a schematic diagram of a state in which a SiN film 96 is formed on a flat silicon substrate 95 for monitoring by plasma ALD. In FIG. 4, infrared light is irradiated onto the silicon substrate 95, and the light transmitted through the silicon substrate 95 is detected by a detector to perform FT-IR analysis. In the FT-IR analysis, information on chemical bonds is obtained. In addition, in the FT-IR analysis, the vibration of hydrogen atoms can be observed, and light atoms such as hydrogen can be detected. For example, in the SiN film 96, the molecules vibrate when infrared light is absorbed, and thus chemical bonds such as SiN, SiO, SiH, and NH can be detected by FT-IR analysis.

[0039] However, the state of the film formed on the actual substrate W used to manufacture the semiconductor device differs from that of the silicon substrate 95 used for monitoring, and even if the SiN film 96 formed on the silicon substrate 95 is analyzed by infrared spectroscopy, the state of the SiN film 91 formed on the substrate W cannot be determined.

[0040] Therefore, in the film forming apparatus 100 according to the embodiment, the control unit 60 controls each unit to perform the process of the following film forming method, and the composition of the film formed on the substrate W is analyzed.

[0041] 5 is a diagram illustrating the flow of the film forming method according to the embodiment. First, a substrate on which a pattern including recesses is formed before film formation is measured by infrared spectroscopy (step S10). For example, a substrate W on which a film is to be formed and on which a pattern 90 including recesses 90a is formed on its surface is placed on a mounting table 2. In the film forming apparatus 100, a control unit 60 controls an irradiation unit 81 to irradiate infrared light from the irradiation unit 81 to the substrate W before film formation, and the infrared light reflected by the substrate W is detected by a detection unit 82, and an FT-IR analysis is performed in the control unit 60.

[0042] Next, a film is formed on the substrate using plasma, such as plasma CVD or plasma ALD (step S11). For example, the control unit 60 controls the gas supply unit 15 and the high-frequency power supply 10 to form a SiN film 91 on the surface of the substrate W by plasma ALD.

[0043] Next, the substrate after the film formation is measured by infrared spectroscopy (step S12). For example, in the film formation apparatus 100, the control unit 60 controls the irradiation unit 81 to irradiate the substrate W with infrared light after the film formation, and the infrared light reflected by the substrate W is detected by the detection unit 82, and the control unit 60 performs FT-IR analysis.

[0044] Next, differential data between the measurement data measured in step S10 and the measurement data measured in step S12 is extracted (step S13). For example, the control unit 60 extracts differential data between the measurement data after film formation and the measurement data before film formation. FIG. 6 is a diagram for explaining differential data according to an embodiment. In FIG. 6, a substrate W on which a pattern 90 including a recess 90a is formed is shown as "before film formation". Also, a substrate W on which a SiN film 91 is formed on the pattern 90 is shown as "after film formation". By extracting the difference between the measurement data before film formation from the measurement data after film formation, a signal of the SiN film 91 can be extracted as differential data.

[0045] Next, based on the extracted difference data, the state of the film formed on the substrate W is displayed (step S14). For example, the control unit 60 detects chemical bonds contained in the SiN film 91 based on the difference data, and displays the detected chemical bonds on the user interface 61.

[0046] Furthermore, the control unit 60 controls the process parameters for film formation based on the extracted difference data (step S15). For example, the control unit 60 detects chemical bonds contained in the SiN film 91 based on the difference data, and controls the process parameters in accordance with the detected chemical bonds.

[0047] Here, an example of a specific detection result will be described. A SiN film 91 was formed on a substrate W on which a pattern 90 including a recess 90a was formed by plasma ALD using a film forming method according to an embodiment. FIG. 7 is a diagram showing an example of a plasma ALD process according to an embodiment. In the plasma ALD, first, DCS (DiChloroSilane: SiH2Cl2) gas is supplied to adsorb a precursor to the substrate W, and then the DCS gas is purged. Next, while supplying H2 gas, high frequency power of 13 MHz is supplied to generate plasma and perform modification. Next, while supplying NH3 gas, high frequency power of 13 MHz is supplied to generate plasma and perform nitridation. In the plasma ALD, a SiN film of a desired thickness is formed by repeating each of these steps.

[0048] 8A is a diagram showing an example of a substrate W on which a SiN film 91 according to an embodiment is formed. The substrate W has a pattern 90 including a recess 90a formed in single crystal silicon (c-Si). The pattern 90 has an aspect ratio of the depth to the diameter of the recess 90a of 8. The SiN film 91 is formed on the pattern 90 of the substrate W.

[0049] The control unit 60 extracted difference data between the measurement data of the FT-IR analysis before the film formation and the measurement data of the FT-IR analysis after the film formation. For example, the control unit 60 obtains the absorbance of infrared light for each wave number of infrared light from the measurement data before the film formation and the measurement data after the film formation. Then, the control unit 60 subtracts the absorbance of infrared light before the film formation from the absorbance of infrared light after the film formation for each wave number to extract the absorbance of infrared light by the SiN film 91 for each wave number as difference data.

[0050] As a comparative example, a SiN film was formed on a flat silicon substrate by plasma ALD using the film forming method according to the embodiment. FIG. 8B is a diagram showing an example of a silicon substrate 95 on which a SiN film 96 according to the comparative example is formed. The silicon substrate 95 is a silicon wafer with a flat upper surface, and a SiN film 96 is formed on the upper surface. Similarly, for the comparative example, the control unit 60 extracted difference data between the measurement data of the FT-IR analysis before the film formation and the measurement data of the FT-IR analysis after the film formation. For example, the control unit 60 obtains the absorbance of infrared light for each wave number of infrared light from the measurement data before the film formation and the measurement data after the film formation. Then, the control unit 60 subtracts the absorbance of infrared light before the film formation from the absorbance of infrared light after the film formation for each wave number, thereby extracting the absorbance of infrared light by the SiN film 96 for each wave number as difference data.

[0051] FIG. 9 is a diagram showing an example of absorbance for each wave number of infrared light. The horizontal axis of FIG. 9 is the wave number of infrared light. The vertical axis is the absorbance of infrared light. FIG. 9 shows a waveform L1 indicating the absorbance for each wave number of a SiN film 91 formed on a pattern 90 of a substrate W. Also, as a comparative example, a waveform L2 indicating the absorbance for each wave number of a SiN film 96 formed on a flat silicon substrate 95 is shown. The shorter the wavelength of infrared light, the larger the wave number. Also, the wave number of the infrared light absorbed differs depending on the substance. Therefore, FT-IR analysis can identify what substance is contained from the wave number of infrared light. Also, FT-IR analysis can estimate the content of the substance from the absorbance for each wave number. Also, FT-IR analysis can estimate the deposition (film thickness) of the film formed from the absorbance for each wave number.

[0052] 8A and 8B, the SiN film 91 is formed also on the side walls and bottom of the recess 90a of the pattern 90, and therefore has a larger volume than the SiN film 96 on the flat silicon substrate 95. For this reason, the waveform L1 of the SiN film 91 has a higher absorbance than the waveform L2 of the SiN film 96. The waveform L1 can detect weaker signals than the waveform L2, and therefore the waveform L1 can detect even trace amounts of substances.

[0053] In the SiN film 91, the higher the aspect ratio of the recess 90a of the pattern 90, the larger the volume of SiN on the sidewall of the recess 90a. Therefore, the higher the aspect ratio of the recess 90a, the more the component of the sidewall of the recess 90a becomes dominant in the waveform L1. In other words, the higher the aspect ratio of the recess 90a, the more the waveform L1 represents the state of the sidewall of the recess 90a.

[0054] 10A to 10C are diagrams showing an example of absorbance for each wave number of infrared light. The horizontal axis of FIG. 10A to 10C is the wave number of infrared light. The vertical axis is the absorbance of infrared light normalized by the area of ​​the SiN film. FIG. 10A to 10C show a waveform L1 showing the absorbance for each wave number of a SiN film 91 formed on a pattern 90 of a substrate W, and a waveform L2 showing the absorbance for each wave number of a SiN film 96 formed on a flat silicon substrate 95 as a comparative example. FIG. 10A to 10C also show the positions of the wave numbers of infrared light absorbed for each compound and chemical bond. As shown by the waveforms L1 and L2, the SiN film 91 formed on the pattern 90 and the SiN film 96 formed on the silicon substrate 95 have different states. For example, as shown in FIG. 10A, the absorbance of the waveform L2 is greater than that of the waveform L1 at the position of Si-N. On the other hand, the waveform L1 has a higher absorbance at the positions of Si-N, Si-O, and NH than the waveform L2. Therefore, the SiN film 91 formed on the pattern 90 contains Si-O and NH in addition to Si-N. Also, as shown in FIG. 10B, the waveform L2 has a lower absorbance at the position of NH2. On the other hand, the waveform L2 has a higher absorbance at the position of NH2. Therefore, the SiN film 91 formed on the pattern 90 also contains NH2. Also, as shown in FIG. 10C, the waveform L1 has a higher absorbance at the position of NH than the waveform L2. Therefore, the SiN film 91 formed on the pattern 90 contains a lot of NH. In this way, the state of the formed SiN film 91 and the SiN film 96 is different between the substrate W on which the pattern 90 is formed and the flat silicon substrate 95. For example, in the case of FIGS. 10A to 10C, the SiN film 91 contains a lot of NH, SiO, and NH2. This causes a deterioration in the Wet Etching Rate (WER). The reason why NH, SiO, and NH2 are present in the SiN film 91 is that ions and radicals do not sufficiently reach the side walls of the recesses 90a, resulting in insufficient nitriding. In this way, the state of the SiN film 91, such as the substances and chemical bonds contained in the SiN film 91, can be obtained from the difference data. For example, NH x , SiH x , SiO, and other substances that affect the film quality of the SiN film 91 can be detected.

[0055] The control unit 60 displays the state of the SiN film 91 formed on the substrate W based on the difference data. For example, the control unit 60 displays a waveform L1 indicating the absorbance of the SiN film 91 for each wave number on the user interface 61 as shown in FIG. 9 and FIGS. 10A to 10C. Also, for example, the control unit 60 identifies substances and chemical bonds contained in the SiN film 91 from the absorbance at the position of the wave number of infrared light absorbed by each substance and chemical bond, and displays the identified substances and chemical bonds on the user interface 61. The control unit 60 may estimate the film thickness of the formed SiN film 91 from the absorbance for each wave number, and display the estimated film thickness on the user interface 61.

[0056] Furthermore, the control unit 60 detects chemical bonds contained in the SiN film 91 based on the difference data, and controls the process parameters according to the detected chemical bonds. For example, when the SiN film 91 is insufficiently nitrided as shown in FIGS. 10A to 10C, the control unit 60 controls the process parameters for film formation so as to promote nitridation. For example, the control unit 60 controls the process parameters so as to increase the flow rate of NH3 gas supplied in nitridation and lengthen the nitridation time. This allows the film formation apparatus 100 to promote nitridation in subsequent film formation, improving the film quality of the SiN film 91 formed on the pattern 90.

[0057] In this embodiment, the FT-IR analysis is performed before and after the formation of the SiN film 91, but the present invention is not limited to this. FT-IR analysis may be performed before and after a specific process of the plasma ALD to obtain measurement data, and differential data may be extracted for the specific process. For example, FT-IR analysis may be performed before and after the precursor adsorption process, modification process, and nitridation process of the plasma ALD shown in FIG. 7 to obtain measurement data and extract differential data. In addition, FT-IR analysis may be performed at all times during each process, and the difference between the data before each process and the real-time data may be monitored in real time. This allows the states of the adsorption process, modification process, and nitridation process to be detected in real time from the differential data of the adsorption process, modification process, and nitridation process. For example, the degree of adsorption of the precursor in the adsorption process can be detected, and it can be detected in real time whether a desired amount of precursor is adsorbed. In addition, the degree of modification in the modification process can be detected, and it can be detected in real time whether a desired modification is performed. Moreover, in the nitriding step, the degree of nitriding can be detected, and it can be detected in real time whether the desired plasma nitriding is being performed. The control unit 60 controls the process parameters based on the difference data. For example, in the adsorption step, the modification step, and the nitriding step, when the adsorption, modification, or nitriding is insufficient as a result of detecting the state of adsorption, modification, or nitriding from the difference data, the control unit 60 controls the process parameters so as to perform the insufficient step. This makes it possible to suppress the insufficiency of adsorption, modification, or nitriding, and improve the film quality of the SiN film 91 to be formed. Also, when the process is performed for an unnecessarily long time, the process time can be shortened, and the productivity can be increased. Also, for example, the FT-IR analysis may be performed before or after each step of the plasma ALD shown in FIG. 7 to obtain measurement data, and the difference data from the measurement data of the previous step may be extracted to obtain the difference data of each step. This makes it possible to detect the state of each step in real time from the difference data of each step.

[0058] Thus, the film forming method according to the embodiment includes a first measurement step (step S10), a film forming step (step S11), a second measurement step (step S12), and an extraction step (step S13). The first measurement step measures the substrate W on which the pattern 90 including the recesses 90a is formed by infrared spectroscopy. The film forming step forms a film on the substrate W after the first measurement step. This film forming step may include a modification step. The film forming step may also be a modification step. The second measurement step measures the substrate W on which the film forming step is formed by infrared spectroscopy. The extraction step extracts difference data between the measurement data of the first measurement step and the measurement data of the second measurement step. In this way, the film forming method according to the embodiment can detect the state of the film formed on the substrate W on which the pattern 90 including the recesses 90a is formed.

[0059] In addition, the extraction step obtains the infrared light absorbance for each wave number of the infrared light from the measurement data before the film formation in the first measurement step and the measurement data after the film formation in the second measurement step. In the extraction step, the infrared light absorbance for each wave number by the film is extracted as difference data by subtracting the infrared light absorbance before the film formation from the infrared light absorbance after the film formation for each wave number. In this way, the film formation method according to the embodiment can detect the state of the film formed on the substrate W from the infrared light absorbance for each wave number extracted as difference data.

[0060] Moreover, the film forming method according to the embodiment includes a display step (step S14) of displaying the state of the film formed on the substrate W in the film forming step based on the difference data extracted in the extraction step. In this way, the film forming method according to the embodiment can present the state of the film actually formed on the substrate W to the process manager.

[0061] Moreover, the film forming method according to the embodiment includes a control step (step S15) of controlling process parameters of the film forming step based on the difference data extracted by the extraction step. As a result, the film forming method according to the embodiment can adjust the process parameters according to the state of the film actually formed on the substrate W, and can improve the film quality of the film formed on the substrate W in the subsequent film formation.

[0062] Although the embodiments have been described above, the disclosed embodiments should be considered to be illustrative and not restrictive in all respects. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the claims.

[0063] For example, in the above embodiment, the case where infrared light is reflected near the center of the substrate W to detect the state of the film near the center of the substrate W has been described, but the present invention is not limited to this. For example, an optical element such as a mirror or lens that reflects infrared light may be provided in the chamber 1, and the optical element may irradiate a plurality of locations such as near the center and near the periphery of the substrate W with the infrared light, and the infrared light reflected at each location may be detected to detect the state of the film at each of the plurality of locations of the substrate W. For example, FT-IR analysis is performed at a plurality of locations in the surface of the substrate W before and after film formation to obtain measurement data. The control unit 60 extracts difference data between the measurement data after film formation and the measurement data before film formation for each of the plurality of locations. The control unit 60 controls the process parameters based on the extracted difference data at the plurality of locations. For example, when the SiN film 91 is insufficiently nitrided at any location, the control unit 60 controls the process parameters of the film formation so as to promote nitridation. The control unit 60 may estimate the film thickness at a plurality of locations of the substrate W based on the difference data at the plurality of locations to detect the distribution of the film thickness. The control unit 60 may control the process parameters so as to obtain a predetermined film quality while uniformizing the film thickness distribution. For example, when the film thickness distribution of the SiN film 91 is non-uniform and the SiN film 91 is insufficiently nitrided at some points, the control unit 60 controls the film formation process parameters so as to uniformize the SiN film 91 and promote nitridation.

[0064] In the above embodiment, the case where the process parameters of the film formation are controlled from the difference data of one substrate W has been described as an example, but the present invention is not limited to this. The process parameters of the film formation process may be controlled based on the difference data of multiple substrates W, based on the comparison of the difference data between the substrates W. For example, when the film formation apparatus 100 forms a film on multiple substrates W, the state of the film formed may change due to changes over time. The control unit 60 changes the process parameters of the film formation process so as to suppress the change in the state of the film based on the comparison of the difference data between the substrates W. For example, when the SiN film 91 is not sufficiently nitrided, the control unit 60 controls the process parameters of the film formation so as to promote nitridation. This makes it possible to suppress the change in the state of the film formed on the multiple substrates W.

[0065] In the above embodiment, the case where the process parameters of the film formation are controlled from the difference data of one substrate W has been described as an example, but the present invention is not limited thereto. The condition of the film formation apparatus 100 changes over time, and the state of the film formed may change even if the film is formed under the same film formation conditions (recipe). Therefore, the film formation apparatus 100 may form a film under the same film formation conditions periodically, such as every few days or at a predetermined timing, perform FT-IR analysis before and after the film formation, and diagnose the condition of the film formation apparatus 100 from the result of the FT-IR analysis. For example, the film formation apparatus 100 forms a film on the substrate W under the same film formation conditions periodically. The control unit 60 diagnoses the condition of the film formation apparatus 100 based on a comparison of the difference data between the substrates W from the difference data of the multiple substrates W formed under the same film formation conditions. As a result, the film formation apparatus 100 can detect a change in the condition from a change in the state of the film formed under the same film formation conditions.

[0066] In the above embodiment, the film forming apparatus of the present disclosure has been described as a single-chamber type film forming apparatus 100 having one chamber, but the present disclosure is not limited thereto. The film forming apparatus of the present disclosure may be a multi-chamber type film forming apparatus having multiple chambers.

[0067] Fig. 11 is a schematic diagram showing another example of the film formation apparatus 200 according to the embodiment. As shown in Fig. 11, the film formation apparatus 200 is a multi-chamber type film formation apparatus having four chambers 201 to 204. In the film formation apparatus 200, plasma ALD is performed in each of the four chambers 201 to 204.

[0068] The chambers 201 to 204 are connected to the four walls of a vacuum transfer chamber 301, which has a heptagonal planar shape, via gate valves G. The inside of the vacuum transfer chamber 301 is evacuated by a vacuum pump and maintained at a predetermined vacuum level. Three load lock chambers 302 are connected to the other three walls of the vacuum transfer chamber 301 via gate valves G1. An atmospheric transfer chamber 303 is provided on the opposite side of the load lock chamber 302 from the vacuum transfer chamber 301. The three load lock chambers 302 are connected to the atmospheric transfer chamber 303 via gate valves G2. The load lock chambers 302 control the pressure between atmospheric pressure and vacuum when transferring the substrate W between the atmospheric transfer chamber 303 and the vacuum transfer chamber 301.

[0069] Three carrier attachment ports 305 for attaching carriers (FOUPs or the like) C that accommodate substrates W are provided on the wall of the atmospheric transfer chamber 303 opposite to the wall on which the load lock chamber 302 is attached. In addition, an alignment chamber 304 for aligning the substrates W is provided on the side wall of the atmospheric transfer chamber 303. A downflow of clean air is formed within the atmospheric transfer chamber 303.

[0070] A transfer mechanism 306 is provided in the vacuum transfer chamber 301. The transfer mechanism 306 transfers a substrate W to and from the chambers 201 to 204 and the load lock chamber 302. The transfer mechanism 306 has two transfer arms 307a and 307b that are independently movable.

[0071] A transfer mechanism 308 is provided in the atmospheric transfer chamber 303. The transfer mechanism 308 transfers the substrate W to the carrier C, the load lock chamber 302, and the alignment chamber 304.

[0072] The film forming apparatus 200 includes a control unit 310. The operation of the film forming apparatus 200 is generally controlled by the control unit 310.

[0073] In the film formation apparatus 200 configured as above, a measurement unit for measuring the substrate W by infrared spectroscopy may be provided in a chamber other than the chambers 201 to 204. For example, the film formation apparatus 200 provides a measurement unit for measuring the substrate W by infrared spectroscopy in the vacuum transfer chamber 301 or any of the load lock chambers 302. For example, in the measurement unit, an irradiation unit for irradiating infrared light and a detection unit for detecting infrared light are arranged in a vertical direction. When performing FT-IR analysis, the film formation apparatus 200 places the substrate W in the measurement unit by the transfer mechanism 306. In the measurement unit, the irradiation unit irradiates the substrate W with infrared light, and the detection unit detects the infrared light transmitted through the substrate W.

[0074] The control unit 310 measures the substrate W before film formation using the measurement unit. The control unit 310 forms a film on the substrate W using any one of the chambers 201 to 204. The control unit 310 measures the substrate W after film formation using the measurement unit. The control unit 310 extracts difference data between measurement data by the measurement unit before film formation and measurement data by the measurement unit after film formation. This makes it possible to detect the state of a film formed on the substrate W on which a pattern including recesses is formed, even in the film formation apparatus 200.

[0075] As described above, an example of detecting the state of a film by applying the technology of the present disclosure in a film formation process has been described, but the present disclosure is not limited to this. The process of detecting the state of a film is not limited to a film formation process, and may be, for example, any process related to a semiconductor manufacturing process for manufacturing a semiconductor device, such as an etching process or a resist process, or may be a plurality of processes including a combination of any process. In addition, from the viewpoint of any process related to a semiconductor manufacturing process and / or a plurality of processes including a combination thereof, the technology of the present disclosure may be applied as a diagnosis or monitoring within or between processes by applying the technology of the present disclosure before and after any process or a plurality of processes. For example, the technology of the present disclosure may be applied to various triggers (particles, intra-surface / inter-surface distribution, etc.) related to the productivity (operation rate, yield, etc.) of semiconductor manufacturing. In addition, as described above, the film formation apparatus of the present disclosure has been disclosed as an example of a single chamber or a multi-chamber type film formation apparatus having a plurality of chambers, but is not limited to this. For example, the film formation apparatus may be a batch type film formation apparatus capable of processing a plurality of substrates at once, or a carousel type semi-batch type film formation apparatus.

[0076] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be construed as limiting. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0077] W substrate 1. Chamber 2. Placement table 10 High frequency power supply 15 Gas supply section 16. Shower Head 60 Control section 61 User Interface 62 Storage section 80a Window 80b Window 81 Irradiation unit 82 Detection unit 90 Patterns 90a Recess 91 SiN film 95 Silicon Substrate 96 SiN film 100 Film deposition equipment 200 Film deposition equipment 201~204 Chamber

Claims

1. A method for detecting a state of a film during film formation, comprising the steps of: Providing a substrate in a chamber; a process of forming a film on the substrate by atomic layer deposition (ALD), the process repeating a plurality of steps including an adsorption step of supplying a source gas into the chamber and adsorbing the source gas on the substrate, and a reaction step of supplying a reactive gas into the chamber and reacting the reactive gas with the source gas to form a film on the substrate, and acquiring measurement data by irradiating the substrate with infrared light in each step; Extracting a difference between the measurement data before and after each step; The detection method comprising:

2. The ALD includes a modifying step, In the extracting step, a difference in measurement data before and after the modifying step is extracted. The detection method according to claim 1 .

3. In the extracting step, the absorbance of infrared light is calculated for each wave number of infrared light from the measurement data before and after each step, and the absorbance of infrared light for each wave number is subtracted to extract the absorbance of infrared light for each wave number as difference data. The detection method according to claim 1 or 2.

4. The method further includes a step of displaying a state of each step based on the difference data extracted by the extracting step. The detection method according to any one of claims 1 to 3.

5. The method further comprises a step of controlling a parameter of each step based on the difference data extracted by the extracting step. The detection method according to any one of claims 1 to 4.

6. The controlling step obtains a film thickness distribution and a film quality of the film formed on the substrate from the extracted difference data, and controls process parameters so as to achieve a predetermined film quality while uniformizing the film thickness distribution. The detection method according to claim 5.

7. The step of forming the film includes periodically forming a film on a substrate under the same film forming conditions; The method further includes a step of diagnosing the condition of an apparatus for performing the step of depositing the film based on a comparison of difference data between substrates from difference data of a plurality of substrates on which films are deposited under the same deposition conditions. The detection method according to any one of claims 1 to 6.

8. The source gas is a silicon-containing gas. The detection method according to any one of claims 1 to 7.

9. The reaction gas is a nitrogen-containing gas. The detection method according to any one of claims 1 to 8.

10. The step of modifying the surface of the substrate is carried out by using plasma of hydrogen gas. The detection method according to claim 2.

11. The infrared light irradiated onto the substrate is an interference wave of infrared light having different optical path differences. The detection method according to any one of claims 1 to 10.

12. The substrate is formed with a pattern including a recess; The film is deposited according to a pattern including recesses. The detection method according to any one of claims 1 to 11.

13. The film is a SiN film. The detection method according to any one of claims 1 to 12.

14. In each step of the film forming process, infrared light is irradiated onto the substrate from an irradiation unit provided on one side wall of the chamber, and the reflected infrared light is detected by a detection unit provided on the other side wall of the chamber, thereby acquiring the measurement data. The detection method according to any one of claims 1 to 13.

15. an optical element for reflecting infrared light is provided within the chamber; The infrared light irradiated from the irradiating unit is reflected by an optical element and irradiated onto the substrate. The detection method according to claim 14.

16. The optical elements are provided at a plurality of locations including the center of the substrate and the periphery of the substrate in the chamber. The detection method according to claim 15.

Citation Information

Patent Citations

  • Method and device for forming deposited film

    JP1991010082A

  • Method of evaluating film, method of measuring temperature, and method of manufacturing semiconductor device

    JP2003158160A

  • Plasma processing apparatus and plasma control method

    JP2018107202A

  • Film forming method and film forming apparatus of silicon nitride film

    JP2018198288A

  • Thin film forming method

    JP1998056010A