Multilayer electronic component

The multilayer ceramic capacitors with a core-shell structured dielectric layer and specific rare earth element distribution address reliability and capacitance issues, achieving enhanced performance in high-temperature and pressure environments.

JP2024153528APending Publication Date: 2024-10-29SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023127368
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2023-08-03
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face challenges in achieving high reliability, satisfying X7R or X7S characteristics, and improving MTTF under high temperature and pressure, while maintaining high capacitance.

Method used

The multilayer electronic component incorporates a dielectric layer with a core-shell structure of dielectric crystal grains containing rare earth elements, where the secondary phases of rare earth elements are distributed with specific ratios and sizes to enhance reliability and capacitance, and includes a specific composition of internal and external electrodes.

Benefits of technology

The solution enhances the reliability and capacitance of multilayer ceramic capacitors, meeting X7R or X7S characteristics and achieving a minimum MTTF of 150 hours under accelerated life testing conditions, with improved dielectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153528000001_ABST
    Figure 2024153528000001_ABST
Patent Text Reader

Abstract

To provide a multilayer electronic component having improved reliability, having improved MTTF with high-temperature / high-voltage accelerated life, and having improved capacitance.SOLUTION: A multilayer electronic component includes a body including a dielectric layer 111 and internal electrodes 121, 122, and an external electrode disposed on the body. The dielectric layer 111 includes a rare earth element, a secondary phase 141 of the rare earth element, and a dielectric grain. When an average thickness of the dielectric layer 111 is defined as td and a maximum size D of the dielectric layer of a secondary phase 141 of the rare earth element in a thickness direction is defined as D, the dielectric layer 111 includes two or more secondary phases 141 of a rare earth element satisfying D / td≤0.2. The dielectric grain includes a first dielectric grain having a core-shell structure including a core portion and a shell portion disposed on at least a portion of the core portion, and when a ratio of a number of moles of the rare earth element to a total number of moles of the entirety of elements other than an oxygen element is defined as RE, a shell portion of the first dielectric grain includes a region satisfying 1.5%≤RE≤3.0%.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multi-layered ceramic capacitors (MLCCs), which are one type of multi-layered electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones, and serve to charge and discharge electricity.

[0003] Such multilayer ceramic capacitors have the advantages of being small yet high capacitance and easy to mount, and can be used as components of various electronic devices. As various electronic devices such as computers and mobile devices become smaller and have higher output, there is an increasing demand for multilayer ceramic capacitors to be smaller and have higher capacitance.

[0004] As the market for MLCCs for electrical equipment as well as IT expands, the demand for products with high rated voltage and excellent reliability in the same capacity range is increasing. It is generally known that the smaller the crystal grain size and the more grain boundaries there are, the higher the reliability of the dielectric. The effects of fixed valence acceptors, transition metal elements that are variable valence acceptors, and rare earth elements in the additive elements of the MLCC dielectric composition on reliability are known, and conditions with good reliability are generally selected by optimizing the composition ratio of the dielectric additive elements including these. Over the 30 years since the industrialization of BME (Base Metal Electrode) MLCCs, work on optimizing the composition to improve reliability has been continuously carried out, and many such cases have already been reported as patents. Recently, it has been reported that even with the same dielectric composition, there are large differences in reliability depending on the microstructure, the distribution and solid solution degree of additive elements, and process conditions, and research on this issue is being actively conducted. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2001-006966 [Patent Document 2] Japanese Patent Publication No. 2011-162401 [Patent Document 3] Korean Patent Publication No. 10-2015-0121569 Summary of the Invention [Problem to be solved by the invention]

[0006] One of the problems to be solved by the present invention is to provide a multilayer electronic component with improved reliability.

[0007] One of the problems that the present invention aims to solve is to provide a multilayer electronic component that satisfies X7R or X7S characteristics.

[0008] One of the problems to be solved by the present invention is to provide a multilayer electronic component having an improved MTTF (high-temperature / high-pressure accelerated life).

[0009] One of the problems to be solved by the present invention is to provide a multilayer electronic component having improved capacitance.

[0010] However, some of the problems that the present invention aims to solve are not limited to the above content, and can be more easily understood in the process of describing specific embodiments of the present invention. [Means for solving the problem]

[0011] A multilayer electronic component according to an embodiment of the present invention includes a main body including a dielectric layer and an internal electrode, and an external electrode disposed on the main body, the dielectric layer including a rare earth element, a secondary phase of the rare earth element, and dielectric crystal grains, the dielectric layer including two or more secondary phases of the rare earth element satisfying D / td≦0.2 when an average thickness of the dielectric layer is defined as td and a maximum distance of the secondary phase of the rare earth element in the thickness direction of the dielectric layer is defined as D, the dielectric layer includes two or more secondary phases of the rare earth element satisfying D / td≦0.2, the dielectric crystal grains include first dielectric crystal grains having a core-shell structure including a core portion and a shell portion disposed on at least a part of the core portion, and the shell portion of the first dielectric crystal grains includes a region satisfying 1.5%≦RE≦3.0% when a ratio of the mole number of the rare earth element to the total mole number of all elements except oxygen is defined as RE. Effect of the Invention

[0012] One of the various effects of the present invention is to improve the reliability of the multilayer electronic component.

[0013] One of the various advantages of the present invention is that it satisfies the X7R or X7S characteristics of multilayer electronic components.

[0014] One of the various effects of the present invention is to improve the MTTF (high temperature / high pressure accelerated life) of multilayer electronic components.

[0015] One of the various advantages of the present invention is that it improves the capacitance of a multilayer electronic component.

[0016] However, the various and beneficial advantages and effects of the present invention are not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic perspective view of a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic exploded perspective view showing a laminated structure of internal electrodes. [Diagram 3] 2 is a schematic cross-sectional view taken along line II' of FIG. 1. [Figure 4] 2 is a schematic cross-sectional view taken along line II-II' in FIG. 1. [Diagram 5] 4 is a schematic diagram showing an enlarged view of region P in FIG. 3; [Figure 6] 3 is a schematic diagram showing the structure of a first dielectric crystal grain having a core-shell structure and the atomic percentage of a rare earth element by region contained therein. [Figure 7] 1 is a STEM / EDS image obtained by photographing and mapping a capacitance forming portion according to an embodiment of the present invention. [Figure 8] 1A is a STEM image of a first dielectric crystal grain having a core-shell structure according to an embodiment of the present invention, and FIG. 1B is a graph showing the RE content obtained by applying a line profile to a line AB drawn on the same first dielectric crystal grain. [Figure 9] 1A is a STEM image of a first dielectric crystal grain having a core-shell structure according to an embodiment of the present invention, and FIG. 1B is a graph showing the RE content by applying a line profile to a CD line drawn on the same first dielectric crystal grain. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be exaggerated for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0019] In order to clearly explain the present invention in the drawings, parts that are not relevant to the explanation are omitted, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited to those shown in the drawings. In addition, components having the same function within the same concept are described using the same reference numerals. Furthermore, throughout the specification, when a part is said to "include" a certain component, this does not mean that other components are excluded, but that the part may further include other components, unless otherwise specified.

[0020] In the drawings, the first direction can be defined as the stacking direction or thickness T direction, the second direction can be defined as the length L direction, and the third direction can be defined as the width W direction.

[0021] Multilayer Electronic Components FIG. 1 is a schematic perspective view of a multilayer electronic component according to one embodiment of the present invention, FIG. 2 is a schematic perspective view showing a laminated structure of an internal electrode, FIG. 3 is a schematic cross-sectional view taken along line I-I' in FIG. 1, FIG. 4 is a schematic cross-sectional view taken along line II-II' in FIG. 1, FIG. 5 is a schematic enlarged view of region P in FIG. 3, and FIG. 6 is a schematic view showing the structure of a first dielectric crystal grain having a core-shell structure and the atomic percentage of rare earth elements contained therein by region.

[0022] A multilayer electronic component according to an embodiment of the present invention will be described in detail below with reference to Figures 1 to 6. Although a multilayer ceramic capacitor will be described as an example of a multilayer electronic component, the present invention can also be applied to various electronic products that use a dielectric composition, such as inductors, piezoelectric elements, varistors, thermistors, and the like.

[0023] A laminated electronic component 100 according to an embodiment of the present invention includes a body 110 including a dielectric layer 111 and internal electrodes 121, 122, and external electrodes 131, 132 disposed on the body 110. The dielectric layer 111 includes a rare earth element, a secondary phase 141 of the rare earth element, and dielectric crystal grains. When an average thickness of the dielectric layer 111 is defined as td and a maximum distance of the secondary phase 141 of the rare earth element in the thickness direction of the dielectric layer is defined as D, the dielectric layer 111 includes two or more secondary phases 141 of the rare earth element satisfying D / td≦0.2. The dielectric crystal grains include first dielectric crystal grains 10 having a core-shell structure including a core portion 11 and a shell portion 12 disposed on at least a portion of the core portion 11. When a ratio of the mole number of the rare earth element to the total mole number of all elements except oxygen is defined as RE, the shell portion 12 of the first dielectric crystal grains can include a region satisfying 1.5%≦RE≦3.0%.

[0024] The body 110 may be formed by alternately stacking dielectric layers 111 and internal electrodes 121, 122.

[0025] More specifically, the body 110 may include a capacitance forming portion Ac that is disposed inside the body 110 and includes first internal electrodes 121 and second internal electrodes 122 that are alternately arranged to face each other with the dielectric layer 111 therebetween and form a capacitance.

[0026] Although there is no particular limitation on the specific shape of the body 110, as shown in the figure, the body 110 may have a hexahedral shape or a shape similar thereto. Due to shrinkage of the ceramic powder contained in the body 110 during the firing process, the body 110 may have a substantially hexahedral shape, although it is not a hexahedral shape with perfectly straight lines.

[0027] The main body 110 can have a first surface 1 and a second surface 2 that face each other in a first direction, a third surface 3 and a fourth surface 4 that are connected to the first and second surfaces 1 and 2 and face each other in a second direction, and a fifth surface 5 and a sixth surface 6 that are connected to the first to fourth surfaces 1, 2, 3, and 4 and face each other in a third direction.

[0028] The plurality of dielectric layers 111 forming the main body 110 are in a fired state, and the boundary between adjacent dielectric layers 111 can be integrated so as to be difficult to confirm without using a scanning electron microscope (SEM).

[0029] The raw material for forming the dielectric layer 111 is not limited as long as sufficient capacitance can be obtained. Generally, perovskite (ABO3)-based materials can be used. For example, barium titanate-based materials, lead composite perovskite-based materials, or strontium titanate-based materials can be used. As the barium titanate-based material, BaTiO3-based ceramic powder can be included. Examples of the ceramic powder include BaTiO3, (Ba 1-x Ca x )TiO3 (0 < x < 1), Ba(Ti 1-y Ca y )O3 (0 < y < 1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1), or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc.

[0030] In addition, as the raw material for forming the dielectric layer 111, various ceramic additives, organic solvents, binders, dispersants, etc. can be added as sub-components to powders such as barium titanate (BaTiO3) according to the object of the present invention.

[0031] The thickness td of the dielectric layer 111 does not need to be particularly limited.

[0032] However, in order to achieve a high capacity of the multilayer electronic component, the thickness td of the dielectric layer may be 5.0 μm or less, preferably 4.0 μm or less, and more preferably 3.0 μm or less. In addition, in order to more easily achieve a small size and high capacity of the multilayer electronic component, the thickness td of the dielectric layer may be 1.0 μm or less, preferably 0.6 μm or less, and more preferably 0.4 μm or less.

[0033] Here, the thickness td of the dielectric layer may refer to the thickness td of the dielectric layer disposed between the first and second internal electrodes 121 and 122.

[0034] Meanwhile, the thickness td of the dielectric layer may mean the distance in the first direction of the dielectric layer 111. In addition, the thickness td of the dielectric layer may mean the average thickness td of the dielectric layer, or may mean the average distance in the first direction of the dielectric layer 111.

[0035] The average distance in the first direction of the dielectric layer 111 may be measured by scanning an image of a cross-section in the first and second directions of the body 110 with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, the average distance in the first direction of one dielectric layer 111 may mean an average value calculated by measuring the distance in the first direction at 30 points equally spaced in the second direction in one dielectric layer 111. The 30 equally spaced points may be designated as the capacitance forming part Ac. Furthermore, if the measurement of such an average value is extended to 10 dielectric layers 111 and the average value is measured, the average distance in the first direction of the dielectric layer 111 may be further generalized.

[0036] Meanwhile, as the market for MLCCs for electrical equipment as well as IT use expands, the demand for products with high rated voltage and excellent reliability in the same capacity range is increasing. It is generally known that the smaller the grain size and the more grain boundaries there are, the higher the reliability of the dielectric. The effects of fixed valence acceptors, variable valence acceptors, transition metal elements, and rare earth elements, among the additive elements in the MLCC dielectric composition, on reliability are known, and conditions with good reliability are generally selected by optimizing the composition ratio of the dielectric additive elements including these. For more than 30 years since BME MLCC was industrialized, work on optimizing the composition to improve reliability has been continuously carried out, and many such cases have already been reported as patents. Recently, it has been reported that even with the same dielectric composition, there are large differences in reliability depending on the microstructure, the distribution and solid solution degree of additive elements, and process conditions, and research on this is being actively conducted.

[0037] The dielectric of current high capacitance BME MLCCs such as X5R, X7R, X8R, and Y5V is BaTiO3 base material or modified by partial solid solution of Ca, Zr, etc. (Ba 1-x Ca x )(Ti 1-y Ca y )O3, (Ba 1-x Ca x )(Ti 1- y Zr y )O3, Ba(Ti 1-y Zr yIt is based on a material in which a base material such as SiO3 is co-doped with fixed valence acceptor elements such as Mg and Al and rare earth elements acting as donors such as Y, Dy, Ho, and Er, and then sintered by further adding variable valence acceptor elements such as Mn, V, and Cr, extra Ba, and SiO2 or a sintering aid containing the same. In order to achieve normal capacitance and insulation characteristics of a high-capacity MLCC when sintered in a reducing atmosphere, it is necessary to suppress grain growth and achieve reduction resistance, and it is known that these two effects can be achieved by adding an appropriate amount of fixed valence acceptor such as Mg. However, when only a fixed valence acceptor such as Mg is added, the dielectric has poor withstand voltage characteristics and reliability, and by adding a transition metal element that is a variable valence acceptor such as Mn and V together with a rare earth element, the withstand voltage and reliability can be improved. Most of these elements are co-doped and dissolved in the shell region of the BaTiO3 matrix crystal grains to form a core-shell structure, realizing stable capacitance characteristics and reliability over temperature for MLCCs.

[0038] It is known that rare earth elements play a role in improving the accelerated life or reliability, and it has been observed that the more these elements are dissolved in the BaTiO3 lattice, the better the properties become. However, if too many rare earth elements are added, huge secondary phases with high rare earth element content, such as pyrochlore (e.g., Re2Ti2O7, where Re is Y, Dy, Ho, Yb, etc.) or RE2Si2O7, may be generated, which may significantly worsen the accelerated life.

[0039] However, according to the present invention, when the size of the secondary phase having a high content of rare earth elements is uniformly distributed at a specific size or less compared to the thickness of the dielectric layer, and at the same time, the content of rare earth elements contained in the shell portion of the main component barium titanate (BaTiO3) dielectric crystal grains has a specific distribution, it is possible to satisfy the X7R-TCC temperature characteristic, and it is possible to improve the dielectric capacitance and reliability.

[0040] Specifically, the target characteristic may be one of the following characteristics: dielectric constant≧2000, mean time to failure (MTTF) of 150 hours or more under accelerated test conditions of applying an electric field of 43 V / μm at a temperature of 150° C., RC value≧1000ΩF, and TCC characteristic of −15% or more and +15% or less in the temperature range of −55° C. to 125° C., and preferably, the target characteristic may be one of the following characteristics: dielectric constant≧2000, mean time to failure (MTTF) of 150 hours or more under accelerated test conditions of applying an electric field of 43 V / μm at a temperature of 150° C., RC value≧1000ΩF, and TCC characteristic of −15% or more and +15% or less in the temperature range of −55° C. to 125° C.

[0041] The dielectric layer 111 may include a rare earth element and a secondary phase 141 of the rare earth element. In this case, when the average thickness of the dielectric layer 111 is defined as td and the distance of the secondary phase 141 of the rare earth element in the thickness direction of the dielectric layer 111 is defined as D, the dielectric layer may include two or more secondary phases of the rare earth element satisfying D / td≦0.2.

[0042] Here, the ratio or percentage (%) of the number of moles of the rare earth element in the secondary phase 141 of the rare earth element to the number of moles of all elements except oxygen can be 30% or more.

[0043] In this case, the dielectric layer 111 can include two or more secondary phases of a rare earth element that satisfy the above D / td≦0.2 within a region of td μm×td μm.

[0044] There is no particular upper limit on the number of secondary phases of rare earth elements that satisfy D / td≦0.2 within the region of td μm×td μm, and when the thickness td of the dielectric layer is 5 μm or less, it is preferable that there are seven or fewer phases. When the thickness td of the dielectric layer is more than 5 μm, more than seven phases can be included.

[0045] Here, the region of td μm×td μm may refer to a rectangular region having an area obtained by multiplying the distance td μm in the thickness direction of the dielectric layer by the distance td μm in the direction perpendicular to the thickness direction of the dielectric layer, which may be the same distance as the average thickness td μm of the dielectric layer, and the area obtained by multiplying the distance td μm in the thickness direction of the dielectric layer by the distance td μm in the direction perpendicular to the thickness direction of the dielectric layer. For example, it may refer to a rectangular region having a distance of td μm in the first direction and a distance of td μm in the second direction based on cross-sections of the dielectric layer 111 in the first and second directions.

[0046] Also, D may refer to the maximum distance in the thickness direction of the dielectric layer of the rare earth element secondary phase 141. For example, D may refer to a value obtained by measuring the distance in the first direction between two arbitrary straight lines drawn in the second direction so as to include both end points in the first direction in the region of the rare earth element secondary phase 141 observed in the cross-sections in the first and second directions of the dielectric layer 111 through SEM, TEM, and STEM.

[0047] The type and content of elements contained in the rare earth secondary phase 141 can also be measured by calculating the average value of regions or points inside the rare earth secondary phase 141 through the SEM, TEM, and STEM EDS analysis modes.

[0048] On the other hand, the dielectric layer 111 includes two or more rare earth element secondary phases satisfying D / td≦0.2 in the tdμm×tdμm region, and does not mean that the dielectric layer 111 includes at least one region that includes two or more rare earth element secondary phases satisfying D / td≦0.2 in the tdμm×tdμm region, but does not mean that the dielectric layer 111 includes all of the above conditions. However, it is preferable that the dielectric layer 111 includes a plurality of tdμm×tdμm regions that include two or more rare earth element secondary phases that satisfy D / td≦0.2, and it is more preferable that the dielectric layer 111 includes at least two rare earth element secondary phases that satisfy D / td≦0.2 in the entire tdμm×tdμm region.

[0049] Since the dielectric layer 111 contains two or more secondary phases of a rare earth element satisfying D / td≦0.2, it can satisfy at least one of the following characteristics: a dielectric constant ≧2000, a mean failure life of 150 hours or more under accelerated test conditions of applying an electric field of 43 V / μm at a temperature of 150°C, an RC value ≧1000 ΩF, and a TCC characteristic of -15% or more and +15% or less in the temperature range of -55°C to 125°C.

[0050] The dielectric layer 111 may include dielectric crystal grains, and the dielectric crystal grains may include first dielectric crystal grains 10 having a core-shell structure including an inner core portion 11 and a shell portion 12 disposed on at least a portion of the core portion 11. However, the dielectric layer 111 is not particularly limited thereto, and may include second dielectric crystal grains not having a core-shell structure.

[0051] In this case, when the ratio of the mole number of the rare earth element to the total mole number of all elements except oxygen is defined as RE, the shell portion 12 of the first dielectric crystal grain may include a region that satisfies 1.5%≦RE≦3.0%. Here, all elements except oxygen may mean including the rare earth element.

[0052] As a more specific example of a method for measuring the content of each element contained in the shell part 12, in the case of a destructive method, the components inside the dielectric crystal grains at the center of the chip can be analyzed using TEM-EDS or STEM-EDS. First, an analysis sample is prepared by cutting a region including a dielectric layer in a cross section of a body where sintering is completed, using a focused ion beam (FIB) device. Then, the surface damage layer of the cut sample is removed using Ar ion milling, and then each component is mapped in an image obtained using (S)TEM-EDS to perform qualitative / quantitative analysis. In this case, the qualitative / quantitative analysis graph of each component can be expressed in terms of mass fraction (wt%), atomic percentage (at%), or molar fraction (mol%) of each element.

[0053] As another method, the chip is crushed to remove the internal electrodes, and then the dielectric layer portion is separated. The components of the dielectric layer thus separated can be analyzed using an apparatus such as an inductively coupled plasma optical emission spectrometer (ICP-OES) or an inductively coupled plasma mass spectrometer (ICP-MS).

[0054] For example, RE can be measured in the following manner. First, an arbitrary 2.5 μm×2.5 μm area of ​​the dielectric layer 111 is photographed at an acceleration voltage of 200 kV, HAADF mode, and magnification of 50,000 times using STEM equipment, and then an arbitrary 1 μm×1 μm area is subjected to EDS mapping analysis again. The resolution at this time is 512×512 pixels, and an image is formed by receiving a signal for 30 ms per pixel. Then, an arbitrary one dielectric crystal grain included in the 1 μm×1 μm area is selected, and a line profile is performed passing through the center. 200 points of data can be obtained from one line, and the intensity at each point corresponds to a signal obtained by repeating five times for 10 seconds. RE can be obtained by calculating the ratio or percentage (%) of the total mole number of rare earth elements to the total mole number of all elements except oxygen element (O) among the elements measured in the line profile.

[0055] The ratio or percentage (%) of the moles of rare earth elements relative to the total moles of all elements except oxygen may have substantially the same meaning as atomic percentage (at%), and all elements except oxygen may include rare earth elements. In a more detailed example, it may mean the percentage (%) value of [rare earth elements] / ([Ba]+[Ti]+[rare earth elements]+[Mg]+[Mn]+[V]+[Si]+[Ca]+[Zr]+···). Here, the square brackets ([ ]) may mean the atomic percentage (at%) of each element measured.

[0056] Furthermore, the fact that the shell portion 12 includes a region that satisfies 1.5%≦RE≦3.0% does not mean that all regions of the shell portion 12 should satisfy 1.5%≦RE≦3.0%, but rather that it is sufficient for the shell portion 12 to include a region that satisfies 1.5%≦RE≦3.0%.

[0057] On the other hand, when the length of the first dielectric crystal grain 10 is defined as G and the length of the region in the shell portion 12 of the first dielectric crystal grain that satisfies 1.5%≦RE≦3.0% is defined as d based on the straight line L passing through the center of the first dielectric crystal grain 10, it is possible to satisfy 2.5%≦d / G≦47.0%.

[0058] 6, as described above, since the shell portion 12 may surround at least a part of the core portion 11, the region satisfying 1.5%≦RE≦3.0% may be two or more regions based on the straight line L passing through the center of the first dielectric crystal grain 141, and the lengths of the two regions may be defined as d1, d2, etc. In this case, each region may satisfy 2.5%≦d1 / G≦47.0% and 2.5%≦d2 / G≦47.0%.

[0059] If d / G is less than 2.5%, the reliability may decrease, and if d / G exceeds 47.0%, the dielectric characteristics may decrease.

[0060] Here, the method of measuring d or G may be measured using a SEM, TEM, STEM device, etc., but is not limited thereto. For example, the first dielectric crystal grain 10 to be measured is selected using a STEM device, a straight line is drawn to pass through the center of the first dielectric crystal grain 10, and then calculation is performed using a program. Here, the straight line passing through the center may refer to the above-mentioned line profile.

[0061] The length G of the dielectric crystal grain 10 may be 170 nm or more and 400 nm or less, and the length d of the region in the shell portion 12 of the first dielectric crystal grain that satisfies 1.5%≦RE≦3.0% may be 10 nm or more and 80 nm or less.

[0062] If G is less than 170 nm, it is difficult to achieve the target dielectric properties, and if it exceeds 400 nm, it may be difficult to achieve a thin dielectric layer.

[0063] If d is less than 10 nm, the shell region is relatively small, which may result in reduced reliability, whereas if d is more than 80 nm, the shell region is relatively large, which may result in reduced dielectric properties.

[0064] Furthermore, according to one embodiment of the present invention, the dielectric layer 111 may include three or more first dielectric crystal grains 10 having a shell portion 12 including an area that satisfies 1.5%≦RE≦3.0% within an area of ​​1 μm×1 μm.

[0065] Here, the 1 μm×1 μm region may refer to a rectangular region having a size of 1 μm in the thickness direction of the dielectric layer and a size of 1 μm in a direction perpendicular to the thickness direction of the dielectric layer, for example, a rectangular region having a distance of 1 μm in the first direction and a distance of 1 μm in the second direction based on a cross-section in the first and second directions.

[0066] By including three or more first dielectric crystal grains 10 having a shell portion 12 including an area satisfying 1.5%≦RE≦3.0% within a 1 μm x 1 μm area of ​​the dielectric layer 111, it is possible to satisfy at least one of the following characteristics: a dielectric constant of ≧2000, a mean failure life of 150 hours or more under accelerated test conditions of applying an electric field of 43 V / μm at a temperature of 150°C, an RC value of ≧1000 ΩF, and a TCC characteristic of -15% or more and +15% or less in the temperature range of -55°C to 125°C.

[0067] In one embodiment of the present invention, the dielectric layer 111 may include a main component and a subcomponent including Ti, where the Ti may come from the main component (e.g., BaTiO3) and the subcomponent may come from an additive.

[0068] In the present invention, the dielectric composition is described based on including the main component and the subcomponent of the dielectric before firing, and the dielectric crystal grains are described based on including the contents of the main component and the subcomponent of the dielectric after firing, but the contents of each element described in the main component and the subcomponent of the dielectric can remain without significant error before and after firing.

[0069] In the present invention, the term "major component" may refer to a component that occupies a relatively large proportion compared to other components, and may refer to a component that occupies 50 at % or more based on the content of the entire composition or the entire dielectric layer.

[0070] In the present invention, the term "minor component" may refer to a component that occupies a relatively small proportion compared to the main component, and may refer to a component that occupies less than 50 at % based on the content of the entire composition or the entire dielectric layer.

[0071] Hereinafter, the minor components that may be included in the dielectric layer 111 will be described in detail. The minor components described in the present invention will be described based on the number of moles of the elements, and can be calculated by converting the amount of oxide or carbonate added as an additive before sintering. As described above, the content of elements before and after sintering may not have a large error value unless there are special circumstances, and the type and content of elements included in the dielectric layer 111 can be measured in a chip state after sintering using various measurement methods such as SEM-EDS, TEM-EDS, and STEM-EDS.

[0072] As a more specific example of a method for measuring the content of each element contained in the dielectric layer 111, in the case of a destructive method, the components inside the dielectric crystal grains at the center of the chip can be analyzed using TEM-EDS or STEM-EDS. First, an analysis sample is prepared by cutting a region including the dielectric layer in a cross section of the body after sintering using a focused ion beam (FIB) device. Then, the sliced ​​sample is subjected to Ar ion milling to remove a damaged layer on the surface, and then each component is mapped in an image obtained using (S)TEM-EDS to perform qualitative / quantitative analysis. In this case, the qualitative / quantitative analysis graph of each component can be expressed in terms of mass fraction (wt%), atomic percentage (at%), or molar fraction (mol%) of each element.

[0073] As another method, the chip is crushed to remove the internal electrodes, and then the dielectric layer portion is separated. The components of the dielectric layer thus separated can be analyzed using an apparatus such as an inductively coupled plasma optical emission spectrometer (ICP-OES) or an inductively coupled plasma mass spectrometer (ICP-MS).

[0074] a) First subcomponent According to an embodiment of the present invention, the subcomponents may include a first subcomponent including a variable valence acceptor element, and the variable valence acceptor element may include one or more of Mn, V, Cr, Fe, Co, Ni, Cu, Co, and Zn, and the content of the first subcomponent may be 0.2 mol to 1.4 mol per 100 mol of Ti.

[0075] The first subcomponent may be one or more of an oxide or carbonate of a variable valence acceptor element. When a plurality of first subcomponent elements are added, the total content of the first subcomponent elements may be defined as the content of the first subcomponent.

[0076] The variable valence acceptor element contained in the first minor component may play a role in lowering the firing temperature of a multilayer electronic device to which the dielectric composition is applied, and in improving the dielectric properties and high temperature accelerated life characteristics.

[0077] If the content of the first subcomponent is less than 0.2 moles per 100 moles of Ti, the high temperature accelerated life may be deteriorated, and if it exceeds 1.4 moles per 100 moles of Ti, the dielectric constant may be deteriorated.

[0078] b) Second subcomponent According to an embodiment of the present invention, the subcomponents may include a second subcomponent containing Mg, and the content of the second subcomponent may be 2.0 mol or less with respect to 100 mol of the Ti.

[0079] The second subcomponent may be one or more of an oxide and a carbonate of Mg.

[0080] The second auxiliary component Mg can play a role in imparting reduction resistance and increasing the RC value.

[0081] Here, the second subcomponent is not an essential component, and even if it is not added, the target properties can be achieved by appropriately adding other components.

[0082] However, if the content of the second subcomponent exceeds 2.0 moles per 100 moles of Ti, the TCC may not satisfy the X7R characteristics.

[0083] c) Third subcomponent According to an embodiment of the present invention, the subcomponents may include a third subcomponent including a rare earth element, and the rare earth element may include at least one of Y, Dy, Tb, Ho, Er, Gd, Ce, Nd, Sm, Tm, La, and Yb, and the content of the third subcomponent may be 2.5 moles or more and 8.0 moles or less with respect to 100 moles of Ti.

[0084] The third subcomponent may be one or more of an oxide and a carbonate of a rare earth element.

[0085] The rare earth element contained in the third subcomponent can play a role in improving the targeted high temperature accelerated life.

[0086] If the content of the third subcomponent is less than 2.5 mol or more than 8.0 mol per 100 mol of Ti, the room temperature dielectric constant or insulation resistance characteristics may be deteriorated.

[0087] d) Fourth subcomponent According to an embodiment of the present invention, the subcomponents may include a fourth subcomponent including at least one element of Ba and Ca, and the content of the fourth subcomponent may be 4.8 mol or less with respect to 100 mol of the Ti.

[0088] The fourth subcomponent may be at least one of an oxide and a carbonate of at least one element of Ba and Ca.

[0089] Meanwhile, since Ba and Ca can be used as the main components of the base material such as BaTiO3, (Ba, Ca)TiO3, etc., the contents of the minor components detected in the dielectric layer may be inaccurate, and the description will be based on the contents added to the dielectric composition before firing.

[0090] Here, the fourth subcomponent is not an essential component, and even if it is not added, the target properties can be achieved by appropriately adding other components.

[0091] If the content of the fourth subcomponent exceeds 4.8 moles per 100 moles of Ti, the room temperature dielectric constant and high temperature withstand voltage may decrease.

[0092] e) Fifth subcomponent According to an embodiment of the present invention, the subcomponents may include a fifth subcomponent containing Si. The content of the fifth subcomponent may be 1.0 mol or more and less than 4.0 mol relative to 100 mol of Ti, with a preferred lower limit of 1.5 mol or more, more preferably 1.65 mol or more, and a preferred upper limit of 3.5 mol or less, more preferably 3.0 mol or less.

[0093] The fifth subcomponent may be at least one of an oxide of Si, a carbonate of Si, and a glass containing Si.

[0094] If the content of the fifth subcomponent is less than 1.0 mole per 100 moles of Ti, the sintered density may be low and the high-temperature life characteristics may be deteriorated. If the content is 4.0 moles or more, the secondary phase may be excessively generated, and the room temperature dielectric constant and high-temperature life characteristics may be deteriorated.

[0095] In addition, when the fourth and fifth subcomponents are added simultaneously, the ratio of the content of the fourth subcomponent to the content of the fifth subcomponent based on 100 moles of Ti may be 1.60 or less.

[0096] If the ratio of the content of the fourth minor component to the content of the fifth minor component exceeds 1.60, the room temperature dielectric constant and the high temperature withstand voltage may decrease.

[0097] The internal electrodes 121 , 122 may then be stacked alternately with the dielectric layers 111 .

[0098] The internal electrodes 121, 122 may include a first internal electrode 121 and a second internal electrode 122, and the first and second internal electrodes 121, 122 may be alternately arranged to face each other with the dielectric layer 111 constituting the body 110 therebetween, and may be exposed to the third and fourth surfaces 3, 4 of the body 110, respectively. At this time, the first and second internal electrodes 121, 122 may be electrically isolated from each other by the dielectric layer 111 arranged therebetween.

[0099] More specifically, the first internal electrode 121 may be spaced apart from the fourth surface 4 and exposed through the third surface 3, and the second internal electrode 122 may be spaced apart from the third surface 3 and exposed through the fourth surface 4.

[0100] In this case, a first external electrode 131 may be arranged on the third surface 3 of the body 110 and connected to the first internal electrode 121, and a second external electrode 132 may be arranged on the fourth surface 4 of the body 110 and connected to the second internal electrode 122.

[0101] That is, the first internal electrode 121 may be connected to the first external electrode 131 but not to the second external electrode 132, and the second internal electrode 122 may be connected to the second external electrode 132 but not to the first external electrode 131.

[0102] Meanwhile, the body 110 may be formed by alternately stacking ceramic green sheets on which the first internal electrodes 121 are printed and ceramic green sheets on which the second internal electrodes 122 are printed, and then firing the stacked ceramic green sheets.

[0103] There is no particular limitation on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 can include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0104] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes, which contains at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, on a ceramic green sheet. The method for printing the conductive paste for internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.

[0105] On the other hand, the thickness te of the internal electrodes 121 and 122 does not need to be particularly limited.

[0106] However, in order to achieve a high capacity of the multilayer electronic component, the thickness te of the internal electrodes may be 1.0 μm or less, and in order to more easily achieve a small size and high capacity of the multilayer electronic component, the thickness te of the internal electrodes may be 0.6 μm or less, and more preferably 0.4 μm or less.

[0107] Here, the thickness te of the internal electrode can mean the distance in the first direction of the internal electrodes 121 and 122. Note that the thickness te of the internal electrode means the average thickness te of the internal electrode and can mean the average distance in the first direction of the internal electrodes 121 and 122.

[0108] The average distance in the first direction of the internal electrodes 121 and 122 can be measured by scanning an image of a cross-section in the first and second directions of the main body 110 with a scanning electron microscope (SEM) at a magnification of 10,000 times. More specifically, the average distance in the first direction of one internal electrode can be the average value calculated by measuring the distance in the first direction at 30 points that are equally spaced in the second direction within one internal electrode. The 30 equally spaced points can be specified in the capacitance forming portion Ac. Further, when such measurement of the average value is extended to 10 internal electrodes to measure the average value, the average distance in the first direction of the internal electrodes can be further generalized.

[0109] On the other hand, in one embodiment of the present invention, the average thickness td1 of at least one of the plurality of dielectric layers 111 and the average thickness te1 of at least one of the plurality of internal electrodes 121 and 122 can satisfy te1 < td1, and more preferably can satisfy te1 × 2 < td1.

[0110] In other words, the average thickness td1 of one dielectric layer may be larger than the average thickness te1 of any one of the first and second internal electrodes 121 and 122, and preferably, the average thickness td1 of one dielectric layer may be larger than twice the average thickness te1 of any one of the first and second internal electrodes 121 and 122.

[0111] Generally, for electronic components for high-voltage electrical equipment, the main issue is the reliability problem due to the decrease in the breakdown voltage (BDV) in a high-voltage environment.

[0112] Therefore, in order to prevent a drop in the breakdown voltage in a high-voltage environment, the average thickness td of the dielectric layer 111 is made larger than the average thickness te of the internal electrodes 121, 122, thereby increasing the thickness of the dielectric layer, which is the distance between the internal electrodes, and improving the breakdown voltage characteristics.

[0113] If the average thickness td of the dielectric layer 111 is less than or equal to the average thickness te of the internal electrodes 121, 122, the average thickness of the dielectric layer, which is the distance between the internal electrodes, is small, so that the breakdown voltage may decrease and a short circuit may occur between the internal electrodes.

[0114] In the high-voltage electronic component, the average thickness te of the internal electrodes may be 1 μm or less, and the average thickness td of the dielectric layers may be 3.0 μm or less, but are not necessarily limited to this.

[0115] Meanwhile, the body 110 may include cover portions 112 and 113 disposed on both end surfaces in the first direction of the capacitance forming portion Ac.

[0116] More specifically, it may include an upper cover part 112 disposed on an upper part of the capacitance forming part Ac in the first direction, and a lower cover part 113 disposed on a lower part of the capacitance forming part Ac in the first direction.

[0117] The upper cover part 112 and the lower cover part 113 may be formed by stacking a single dielectric layer 111 or two or more dielectric layers 111 in a first direction on the upper and lower surfaces of the capacitance forming part Ac, respectively, and may basically serve to prevent damage to the internal electrodes 121, 122 due to physical or chemical stress.

[0118] The upper cover part 112 and the lower cover part 113 do not include the internal electrodes 121, 122 and may include the same material as the dielectric layer 111. That is, the upper cover part 112 and the lower cover part 113 may include a ceramic material, for example, a barium titanate (BaTiO3)-based ceramic material.

[0119] On the other hand, the thickness tc of the covers 112 and 113 does not need to be particularly limited.

[0120] However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the thickness tc of the cover portion may be 100 μm or less, preferably 30 μm or less, and in the case of ultra-small products, more preferably 20 μm or less.

[0121] Here, the thickness tc of the cover portion may mean the distance in the first direction between the cover portions 112 and 113. In addition, the thickness tc of the cover portion may mean the average thickness tc of the cover portion, and may mean the average distance in the first direction between the cover portions 112 and 113.

[0122] The average distance in the first direction of the covers 112 and 113 may be measured by scanning an image of a cross-section in the first and second directions of the body 110 with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, it may mean an average value calculated by measuring the distance in the first direction at 30 points that are equally spaced in the second direction in an image obtained by scanning one cover.

[0123] In addition, the average distance in the first direction of the cover portion measured by the above-mentioned method may have substantially the same size as the average distance in the first direction of the cover portion based on the cross-sections in the first and third directions of the main body 110.

[0124] Meanwhile, the multilayer electronic component 100 may include side margin portions 114 and 115 disposed on both end surfaces of the body 110 in the third direction.

[0125] More specifically, the side margin portions 114 , 115 may include a first side margin portion 114 disposed on the fifth surface 5 of the body 110 and a second side margin portion 115 disposed on the sixth surface 6 of the body 110 .

[0126] As shown in the figure, the side margin portions 114, 115 may refer to the areas between the end surfaces in the third direction of the first and second internal electrodes 121, 122 and the boundary surface of the body 110 based on the cross-sections in the first and third directions of the body 110.

[0127] The side margin portions 114, 115 can also be formed by forming internal electrodes 121, 122 by applying a conductive paste to a ceramic green sheet applied to the capacitance forming portion Ac except for the areas where the side margin portions 114, 115 are to be formed, and then cutting the laminated internal electrodes 121, 122 so that they are exposed on the fifth and sixth surfaces 5, 6 of the main body 110 in order to suppress steps caused by the internal electrodes 121, 122, and then stacking a single dielectric layer 111 or two or more dielectric layers 111 in the third direction on both end surfaces in the third direction of the capacitance forming portion Ac.

[0128] The side margins 114 and 115 essentially serve to prevent damage to the internal electrodes 121 and 122 due to physical or chemical stress.

[0129] The first side margin portion 114 and the second side margin portion 115 do not include the internal electrodes 121, 122, and may include the same material as the dielectric layer 111. That is, the first side margin portion 114 and the second side margin portion 115 may include a ceramic material, for example, a barium titanate (BaTiO3)-based ceramic material.

[0130] On the other hand, the width wm of the first and second side margin portions 114, 115 does not need to be particularly limited.

[0131] However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component 100, the width wm of the side margin portion may be 100 μm or less, preferably 30 μm or less, and in the case of ultra-small products, more preferably 20 μm or less.

[0132] Here, the width wm of the side margin portion may mean the distance in the third direction between the side margin portions 114, 115. Note that the width wm of the side margin portion may mean the average width wm of the side margin portion, and may mean the average distance in the third direction between the side margin portions 114, 115.

[0133] The average distance in the third direction of the side margins 114, 115 may be measured by scanning an image of a cross-section in the first and third directions of the body 110 with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, it may mean an average value calculated by measuring the distance in the third direction at 10 points equally spaced in the first direction in an image obtained by scanning one side margin.

[0134] In one embodiment of the present invention, a structure is described in which the ceramic electronic component 100 has two external electrodes 131, 132; however, the number and shape of the external electrodes 131, 132 can be changed depending on the shape of the internal electrodes 121, 122 and other purposes.

[0135] The outer electrodes 131 and 132 may be disposed on the body 110 and connected to the inner electrodes 121 and 122 .

[0136] More specifically, the external electrodes 131, 132 may include first and second external electrodes 131, 132 disposed on the third and fourth surfaces 3, 4 of the body 110, respectively, and connected to the first and second internal electrodes 121, 122, respectively. That is, the first external electrode 131 may be disposed on the third surface 3 of the body and connected to the first internal electrode 121, and the second external electrode 132 may be disposed on the fourth surface 4 of the body and connected to the second internal electrode 122.

[0137] Meanwhile, the external electrodes 131, 132 may be formed using any material having electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical characteristics, structural stability, etc., and may further have a multi-layer structure.

[0138] For example, the external electrodes 131 and 132 may include electrode layers 131a, 132a, 131b, and 132b disposed on the body 110 and plating layers 131c and 132c disposed on the electrode layers 131a, 132a, 131b, and 132b.

[0139] As a more specific example of the electrode layers 131a, 132a, 131b, and 132b, the electrode layers 131a, 132a, 131b, and 132b may include the first electrode layers 131a, 132a which are fired electrodes including a first conductive metal and glass, and the second electrode layers 131b, 132b which are resin-based electrodes including a second conductive metal and resin.

[0140] Here, the first conductive metal may refer to a conductive metal included in the first electrode layers 131a and 132a, and the second conductive metal may refer to a conductive metal included in the second electrode layers 131b and 132b. In this case, the first conductive metal and the second conductive metal may be the same or different, and may include the same metal material, but are not limited thereto.

[0141] Furthermore, the electrode layers 131a, 132a, 131b, and 132b may be in a form in which a fired electrode and a resin-based electrode are successively formed on a main body.

[0142] The electrode layers 131a, 132a, 131b, and 132b may be formed by transferring a sheet containing a conductive metal onto the main body, or may be formed by transferring a sheet containing a conductive metal onto a fired electrode.

[0143] The conductive metal contained in the electrode layers 131a, 132a, 131b, and 132b may be a material having excellent electrical conductivity. For example, the conductive metal may include, but is not limited to, one or more selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0144] In one embodiment of the present invention, the electrode layers 131a, 132a, 131b, 132b may have a two-layer structure including a first electrode layer 131a, 132a and a second electrode layer 131b, 132b, whereby the external electrodes 131, 132 may include a first electrode layer 131a, 132a including a conductive metal and glass and a second electrode layer 131b, 132b disposed on the first electrode layer 131a, 132a and including a conductive metal and a resin.

[0145] The first electrode layers 131a and 132a contain glass, thereby improving the adhesion to the body 110, and the second electrode layers 131b and 132b contain resin, thereby improving the bending strength.

[0146] The conductive metal used for the first electrode layers 131a and 132a is not particularly limited as long as it can be electrically connected to the internal electrodes 121 and 122 to form capacitance, and may include, for example, at least one selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof. The first electrode layers 131a and 132a may be formed by applying a conductive paste prepared by adding glass frit to the conductive metal powder, and then firing the paste.

[0147] The conductive metal contained in the second electrode layers 131b and 132b may serve to electrically connect the second electrode layers 131a and 132a to the first electrode layers 131a and 132a.

[0148] The conductive metal contained in the second electrode layers 131b and 132b is not particularly limited as long as it is a material that can be electrically connected to the electrode layers 131a and 132a, and may include one or more selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0149] The conductive metal contained in the second electrode layers 131b and 132b may include one or more of spherical particles and flake particles. That is, the conductive metal may be composed of only flake particles, may be composed of only spherical particles, or may be a mixture of flake particles and spherical particles. Here, the spherical particles may include a shape that is not completely spherical, for example, a shape in which the length ratio of the major axis to the minor axis (major axis / minor axis) is 1.45 or less. The flake particles refer to particles having a flat and elongated shape, and are not particularly limited, but may be, for example, a shape in which the length ratio of the major axis to the minor axis (major axis / minor axis) is 1.95 or more. The lengths of the major axis and minor axis of the spherical particles and the flake particles can be measured from an image obtained by scanning a cross-section in the first and second directions cut at the center of the third direction of the ceramic electronic component with a scanning electron microscope (SEM).

[0150] The resin contained in the second electrode layers 131b and 132b can ensure bonding and absorb shock. The resin contained in the second electrode layers 131b and 132b is not particularly limited as long as it has bonding and shock absorbing properties and can be mixed with a conductive metal powder to produce a paste, and can include, for example, an epoxy resin.

[0151] In addition, the second electrode layers 131b and 132b may include a plurality of metal particles, an intermetallic compound, and a resin. By including the intermetallic compound, the electrical connectivity with the first electrode layers 131a and 132a may be further improved. The intermetallic compound may function to connect the plurality of metal particles to improve the electrical connectivity, and may function to surround the plurality of metal particles to connect them to each other.

[0152] At this time, the intermetallic compound may include a metal having a melting point lower than the curing temperature of the resin. That is, since the intermetallic compound includes a metal having a melting point lower than the curing temperature of the resin, the metal having a melting point lower than the curing temperature of the resin melts during the drying and curing process, and forms an intermetallic compound with a part of the metal particles to surround the metal particles. At this time, the intermetallic compound may include a low melting point metal of preferably 300° C. or less.

[0153] For example, it may contain Sn having a melting point of 213 to 220°C. During the drying and hardening process, Sn melts, and the molten Sn wets high melting point metal particles such as Ag, Ni, or Cu by capillary action and reacts with some of the Ag, Ni, or Cu metal particles to form intermetallic compounds such as Ag3Sn, Ni3Sn4, Cu6Sn5, and Cu3Sn. Ag, Ni, or Cu that is not involved in the reaction remains in the form of metal particles.

[0154] Thus, the metal particles may include one or more of Ag, Ni, and Cu, and the intermetallic compound may include one or more of Ag3Sn, Ni3Sn4, Cu6Sn5, and Cu3Sn.

[0155] The plating layers 131c and 132c can serve to improve mounting characteristics.

[0156] The type of plating layers 131c, 132c is not particularly limited, and may be a single layer plating layer 131c, 132c containing one or more of nickel (Ni), tin (Sn), palladium (Pd), and alloys thereof, or may be formed of multiple layers.

[0157] As a more specific example of the plating layers 131c, 132c, the plating layers 131c, 132c may be Ni plating layers or Sn plating layers, and may be in a form in which a Ni plating layer and a Sn plating layer are sequentially formed on the electrode layers 131a, 132a, 131b, 132b, or in a form in which a Sn plating layer, a Ni plating layer, and a Sn plating layer are sequentially formed. The plating layers 131c, 132c may also include a plurality of Ni plating layers and / or a plurality of Sn plating layers.

[0158] The size of the multilayer electronic component 100 does not need to be particularly limited.

[0159] To achieve high capacitance, the size may be 3216 (length x width: 3.2 mm x 1.6 mm) or less. To simultaneously achieve miniaturization and high capacitance, the thickness of the dielectric layers and internal electrodes must be reduced to increase the number of layers, so the size may be 1005 (length x width: 1.0 mm x 0.5 mm) or less.

[0160] The present invention will be described in more detail below with reference to examples. However, these examples are intended to aid in the specific understanding of the present invention, and the scope of the present invention is not limited to these examples.

[0161] (Example) BaTiO3 particles with an average particle size of 150 nm were used as the base material of the main component. Zirconia beads were used as a mixing / dispersing medium, and the raw powder containing the subcomponents corresponding to the composition specified in Tables 1, 3, and 5 and the main component BaTiO3 particles were mixed with an ethanol / toluene solvent and a dispersant and milled for 10 hours, and after mixing with a binder, milled for an additional 5 hours. The slurry thus produced was used to produce molded sheets with thicknesses of 7.0 μm and 10 μm using a sheet production molding machine. Nickel (Ni) internal electrodes were printed on the molded sheets. The upper and lower cover parts were produced by laminating 25 layers of cover sheets (thickness of 10 μm to 13 μm), and the 21 layers of printed sheets were pressed and laminated to produce a bar. The crimping bar was cut into chips of 3216 (length x width: 3.2mm x 1.6mm) size using a cutting machine. The MLCC chips of 3216 size that were completed were calcined, sintered in a reducing atmosphere of 0.1% H2 / 99.9% N2~0.5% H2 / 99.5% N2 (H2O / H2 / N2 atmosphere) at 1240~1280℃ for 2 hours, and then reoxidized in a N2 atmosphere at 1000℃ for 3 hours. Here, a hydrogen concentration of 0.1% corresponds to an electromotive force of 670mV in an 850℃ measurement environment using an oxygen partial pressure meter, and a hydrogen concentration of 0.5% corresponds to an electromotive force of 760mV. The sintered chips were subjected to a termination process using copper paste and electrode sintering to complete the external electrodes. As a result, a 3216 size MLCC chip was produced in which the dielectric layer had a thickness of approximately 2.0 μm after firing and the number of dielectric layers was 20.

[0162] The room temperature capacitance and dielectric loss of the MLCC chip were measured using an LCR meter under the conditions of 1 kHz and AC 0.5 V / μm. The dielectric constant of the MLCC chip dielectric was calculated from the capacitance, the thickness of the dielectric of the MLCC chip, the area of ​​the internal electrode, and the number of layers. The room temperature insulation resistance was measured after 60 seconds had elapsed with 10 samples taken and DC 10 V / μm applied. The change in capacitance due to temperature was measured in the temperature range of -55°C to 145°C. The accelerated life evaluation (HALT: Highly Accelerated Life Time Test) was performed by applying a voltage corresponding to an electric field of 43 V / μm at 150°C to 40 samples of each type, measuring the time until failure occurred, and calculating the mean time (MTTF: Mean Time to Failure). Tables 2, 4, and 6 show the characteristics of the prototype chips corresponding to the embodiments specified in Tables 1, 3, and 5.

[0163] FIG. 7 shows an example of a microstructure in which Ni and Dy components were mapped by STEM / EDS analysis of a dielectric material with a high accelerated life, where it was confirmed that the number of rare earth element secondary phases in any tdμm×tdμm region was two or more and D / td≦0.2 was satisfied, where T is the thickness of the dielectric layer and D is the size in the thickness direction of the dielectric layer of the secondary phase of the rare earth element containing 30% or more moles of rare earth element (excluding oxygen element).

[0164] The secondary phase of rare earth elements in the dielectric layer was confirmed by STEM / EDS analysis to confirm the components of the secondary phase of rare earth elements, and the rare earth element fraction (%) was limited to a ratio of the number of moles of one or more of the rare earth elements Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, Tb, Tm, and Gd to the total number of moles of all elements excluding oxygen, [rare earth elements] / ([Ba]+[Ti]+[rare earth elements]+[Mg]+[Mn]+[V]+[Si]+[Ca]+[Zr], etc.) being 30% or more.

[0165] Figures 8(a), 8(b) and 9(a) and 9(b) show measurements taken by detecting and measuring crystal grains having a thickness of 10nm to 80nm in the shell portion of dielectric crystal grains of BaTiO3, the main component, which has a core-shell structure, in which the rare earth element content of one or more of the rare earth elements Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, Tb, Tm, and Gd is in the range of 1.5% to 3.0% relative to all elements excluding oxygen.

[0166] The multilayer electronic component according to one embodiment of the present invention aims to produce a dielectric that can realize all of the following characteristics under firing conditions in a reducing atmosphere to which nickel (Ni) internal electrodes can be applied, such as X7R or X7S temperature-temperature capacitance (TCC) characteristics and high high-temperature reliability, and an MLCC using the dielectric. As criteria for determining characteristics for this purpose, preferred target characteristics are an example that can realize all of the following characteristics: dielectric constant ≧2000, mean failure life of 150 hours or more under accelerated test conditions of applying an electric field of 43 V / μm at a temperature of 150°C, RC value ≧1000ΩF, and TCC characteristics of -15% or more and +15% or less in the temperature range of -55°C to 125°C. Examples that achieve these characteristics are described below.

[0167] Depending on the type or content of the added subcomponent, at least one of the above characteristics can be satisfied. If all the listed characteristics are satisfied, the characteristic evaluation is marked with "O." If even one of the characteristics is not satisfied, it is marked with "X." In other words, even if it is marked with "X," it may be possible that at least one of the multiple characteristics is satisfied.

[0168] The content of each subcomponent is expressed as moles based on the additive, and means the number of moles of the content added to 100 moles of BaTiO3 matrix (or 100 moles of Ti). For example, in Example 1-1, 0.2 mol of MnO2 and 0.1 mol of V2O5, which are the first subcomponents, were added, which means that 0.2 mol of MnO2 was added to 100 mol of BaTiO3 and 0.1 mol of V2O5 was added to 100 mol of BaTiO3, and when converted based on the number of moles of the elements, Mn can be calculated as 0.2 mol and V as 0.2 mol, respectively. Hereinafter, RE2O3 or RE in the RE-rich phase may mean rare earth elements (RE), and does not need to be redefined in the present invention. Those skilled in the art will be able to distinguish between RE and rare earth elements (RE) redefined in the present invention.

[0169] [Table 1]

[0170] [Table 2]

[0171] Examples 1-1 to 1-7 in Table 1 show examples according to the type of rare earth element in the third subcomponent when the total of the variable valence elements (Mn, V) in the first subcomponent is 0.3 mol, the content of the Mg in the second subcomponent is 1.0 mol, the content of the rare earth RE2O3 in the third subcomponent is 2.5 mol (5.0 mol based on the Dy element), the content of Ba or Ca in the fourth subcomponent is 1.0 mol, and the content of SiO2 in the fifth subcomponent is 1.25 mol, relative to 100 mol of the BaTiO3 base material of the main component 150 nm. Examples 1-1 to 1-7 in Table 2 show the characteristics of prototype MLCC samples corresponding to these examples. When the third subcomponent is La and Yb (Examples 1-1 to 1-2), D / td is 0.2 or more, and the MTTF shows low characteristics of less than 150 hours. On the other hand, when the third subcomponent is Y, Dy, Tb, Ho, or Gd, a microstructure is realized in which D / td is 0.2 or less and the number of RE-rich secondary phases (RE-rich phase and RE-rich secondary phase mean secondary phases of rare earth elements, and the same applies below) is two or more in an arbitrary dielectric thickness region of td μm × td μm under the firing conditions, and at this time, the MTTF is significantly improved to 150 hours or more, and it can be confirmed that all of the target characteristics of the present invention, which are a dielectric constant of 2000 or more, an MTTF of 150 hours or more, an RC value of 1000 ΩF or more, and a TCC characteristic of -15% or more and +15% or less in the temperature range of -55°C to 125°C, are realized.

[0172] The size and distribution of the RE-rich secondary phase may vary depending on the type of rare earth element and the firing conditions, but when the rare earth element of the third subcomponent is Y, the hydrogen concentration of the firing atmosphere is as low as 0.1% and the EMF value at 850 ° C is as low as 670 mV, or the firing temperature is as high as 1280 ° C (Examples 2-1 and 2-2), D / td is 0.2 or more, and the MTTF is very low at less than 100 hours. On the other hand, when the rare earth element of the third subcomponent is Dy (Examples 2-3 and 2-4), even under firing conditions where D / td is 0.2 or more when the third subcomponent is Y, a microstructure in which D / td is 0.2 or less and the number of RE-rich secondary phases is two or more is realized in an arbitrary dielectric layer td μm × td μm region, and in this case, the MTTF is greatly improved to 150 hours or more, and all the target characteristics of the present invention are realized. Therefore, regardless of the type of the third subcomponent, when a microstructure in which D / td is 0.2 or less and the number of RE-rich secondary phases is two or more is realized in the region of the dielectric layer tdμm×tdμm, it can be confirmed that the MTTF is significantly improved to 150 hours or more.

[0173] In the above-mentioned Examples 1-1 to 2-4, when the content of rare earth elements in the shell part of the main component BaTiO3 crystal grains having a core-shell structure within an arbitrary 1 μm×1 μm region of the dielectric layer was confirmed from the samples that realized all the target characteristics of the present invention, it was confirmed that there existed crystal grains having a length of 10 nm to 80 nm in the region where the total ratio of one or more of the rare earth elements Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, Tb, Tm, and Gd to all elements except oxygen is 1.5 at % to 3.0 at %, and the number of such crystal grains was always 3 or more. This can be said to be the satisfying condition of the main crystal grains to obtain the target characteristics of the present invention.

[0174] Example 2-5 in Table 1 applies the same composition and firing conditions as Example 2-4, but the batch milling time is reduced to 1 / 4, and the additive dispersion state is poor. Example 2-5 in Table 2 shows its electrical characteristics. In this case, a microstructure in which D / td is 0.2 or less and the number of RE-rich secondary phases is two or more is realized in the tdμm×tdμm region of the dielectric layer, but the content and distribution of rare earth elements in the main crystal grains do not meet the above-mentioned main crystal grain satisfaction conditions, the MTTF is less than 150 hours, and the target characteristics are not realized. In addition, as in Example 1-2, even if the content and distribution of rare earth elements in the main crystal grains meet the above-mentioned main crystal grain satisfaction conditions, if a microstructure in which D / td is 0.2 or less and the number of RE-rich secondary phases is two or more is not realized in the tdμm×tdμm region of the dielectric layer, the target characteristics of the present invention cannot be realized.

[0175] Therefore, in order to realize the target characteristics of the present invention, when the size (length) in the thickness direction of the dielectric of the secondary phase in which the total content of one or more of the rare earth elements Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, Tb, Tm, and Gd is 30 at % or more, which is the condition for the secondary phase, is D, the number of the secondary phases in any td μm × td μm region is always two or more and D / td≦0.2 is satisfied, and further, the content of the rare earth elements in the shell part of the main component BaTiO3 crystal grains having a core-shell structure in any 1 μm × 1 μm region of the dielectric layer, which is the condition for the main crystal grains, is the rare earth elements Y, Dy, Ho, It can be seen that the target characteristics of the present invention are realized when a dielectric material having crystal grains with a length of a region in the range of 10 nm to 80 nm in which the total ratio of one or more of Er, Gd, Ce, Nd, Sm, Tb, Tm, and Gd falls within the range of 1.5% to 3.0% and the number of such crystal grains is three or more is simultaneously realized.

[0176] [Table 3]

[0177] [Table 4]

[0178] Examples 3-1 to 5-6 in Table 3 show examples with varying contents of the third, second, and first subcomponents for 100 mol of BaTiO3 matrix with a main component of 150 nm, and Table 4 shows the properties of the samples corresponding to these examples. When the content of Dy2O3, which is the third subcomponent, is relatively low at 1.0 mol or 2.0 at% in element ratio (Examples 3-1 to 3-2), the satisfactory condition of the main crystal grains of the present invention is not met, or even if the satisfactory condition of the main crystal grains is met, the RE-rich secondary phase does not exist, the high temperature TCC (125°C) characteristics are out of the standard, or the MTTF characteristics are low at less than 150 hours, which is the target value of the present invention, so the target characteristics are not achieved. In addition, when the Dy2O3 content is relatively high at 4.5 mol or 9.0 at% in element ratio (Examples 3-8 to 3-9), the rare earth content in the shell region of the main crystal grain exceeds 3.0 at%, which does not meet the conditions for the main crystal grain of the present invention, the dielectric constant becomes low at less than 2000, the size of the RE-rich secondary phase becomes excessively large, D / td becomes 0.2 or more in an arbitrary dielectric layer td μm × td μm region, the MTTF characteristic is less than 150 hours, and the target characteristic of the present invention is not realized. When the Dy2O3 content is in the range of 1.25 mol to 4.0 mol or the Dy element ratio is in the range of 2.5 at % to 8.00 at % (Examples 3-3 to 3-7), it is confirmed that both the main crystal grain satisfaction condition and the secondary phase condition of the present invention are satisfied, and at this time, it is possible to satisfy all the characteristics, namely, dielectric constant ≧ 2000, HALT MTTF ≧ 150 hours at 150 °C and DC 43 V / μm, RC value ≧ 1000 ΩF, and TCC characteristic in the temperature range of -55 °C to 125 °C is -15% or more and +15% or less.

[0179] In Examples 4-1 to 4-4, when Mg, the second subcomponent, is added, it has the effect of increasing the RC value, but when the amount is excessive, 3.0 mol or 3.0 at%, the MTTF characteristics are less than the target value of 100 hours of the present invention, and the characteristics are not realized. When the content of MgCO3, the second subcomponent, is in the range of 0 mol (not added) to 2.0 mol or 0 at% (not added) to 2.0 at% in terms of Mg element ratio (Examples 4-1 to 4-3), all the characteristics of the present invention can be realized. In Example 5-1 to Example 5-6, when the total content of transition metals Mn and V is too low at an element ratio of 0.1 at% (Example 5-1), the MTTF characteristic is less than the target value of the present invention, 100 hours, and the characteristic is not realized. When the total content of transition metals Mn and V is excessive at an element ratio of 2.0 at% (Example 5-4), the RC value is less than 1000 and the MTTF is less than 150 hours, and the target characteristic of the present invention cannot be satisfied. In Examples 5-5 to 5-6, Mn alone or V alone is added at an element ratio of 0.5 at%, and the target characteristic of the present invention can be realized in either case. Therefore, it can be said that the content of the first subcomponent for realizing the target characteristic of the present invention is 0.2 at% to 1.4 at% in element ratio.

[0180] [Table 5]

[0181] [Table 6]

[0182] Table 5 shows examples of the fourth and fifth subcomponents with respect to 100 mol of BaTiO3 matrix with a main component of 150 nm, and Table 6 shows the properties of the samples corresponding to these examples. When the content of the fifth subcomponent SiO2 is as low as 0.5 mol (Examples 6-1 to 6-3), there is a problem that the sintered density is low, and the room temperature dielectric constant and MTTF are low, regardless of the content of the fourth subcomponent. When the fourth subcomponent Ba is added in an appropriate amount for each SiO2 content, and the ratio of (Ba+Ca) / Si is 0.48 (Examples 7-2, 8-3, and 9-2), the effect of increasing the room temperature dielectric constant while satisfying all the properties of the present invention can be confirmed compared to the condition where the ratio is 0 (Examples 7-1, 8-1, and 9-1). However, under the condition that SiO2 is added excessively and the ratio of (Ba+Ca) / Si is 1.88 (Example 7-4, Example 8-5, Example 9-4), the room temperature dielectric constant is less than 2000 or the MTTF is less than 100 hours, and the target characteristics of the present invention cannot be met. From Example 6-1 to Example 9-4, it can be confirmed that the target characteristics of the present invention are realized when the ratio (Ba+Ca) / Si of the fourth and fifth subcomponents is in the range of 1.60 or less. Examples 10-1 to 10-2 show examples according to the change in the content of BaCO3 when the content of the fifth subcomponent SiO2 is excessive at 4.0 mol or 4.0 at% in element ratio, but in this case, it can be confirmed that even if the ratio (Ba+Ca) / Si of the fourth and fifth subcomponents is in the range of 1.60 or less, the room temperature dielectric constant and MTTF are lower than the target values ​​of the present invention, and the target characteristics cannot be realized. Therefore, to summarize the variation examples of the fourth and fifth subcomponents, when the content of the fourth subcomponent is in the range of 4.8 mol or 4.8 at% or less in element ratio, and the content of the fifth subcomponent, SiO2, is in the range of 0.8 mol to 3.0 mol or 0.8 at% to 3.0 at% in element ratio, and the ratio of the fourth and fifth subcomponents, (Ba+Ca) / Si, is in the range of 1.60 or less, the target characteristics of the present invention can be realized.

[0183] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above-described embodiment and the accompanying drawings, but is limited by the scope of the accompanying claims. Therefore, various substitutions, modifications and changes can be made by a person having ordinary knowledge in the art within the scope of the technical idea of ​​the present invention described in the claims, and these also belong to the scope of the present invention.

[0184] In addition, the expression "one embodiment" used in this specification does not mean the same embodiment, but is provided to emphasize and describe each unique feature that is different from the others. However, the above-mentioned one embodiment does not exclude being realized in combination with the features of another embodiment. For example, even if a matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description that is opposite or contradictory to the matter in the other embodiment.

[0185] The terms used in this specification are merely used to describe one embodiment and are not intended to limit the present invention. In this case, the singular expression includes the plural expression unless the context clearly indicates otherwise. [Explanation of symbols]

[0186] 10: First dielectric crystal grain 11: Core section 12: Shell part 100: Multilayer electronic components 110: Main unit 111: Dielectric layer 112, 113: Cover part 114, 115: Side margin 121, 122: Internal electrode 131, 132: External electrode 141:Secondary phases of rare earth elements

Claims

1. a body including a dielectric layer and an internal electrode; an external electrode disposed on the body; the dielectric layer includes a rare earth element, a secondary phase of the rare earth element, and dielectric grains; When an average thickness of the dielectric layer is defined as td and a maximum distance of the secondary phase of the rare earth element in the thickness direction of the dielectric layer is defined as D, the dielectric layer contains two or more secondary phases of the rare earth element satisfying D / td≦0.2; The dielectric crystal grains include first dielectric crystal grains having a core-shell structure including a core portion and a shell portion disposed on at least a portion of the core portion, and when the ratio of the number of moles of the rare earth element to the total number of moles of all elements excluding oxygen is defined as RE, the shell portion of the first dielectric crystal grains includes a region that satisfies 1.5%≦RE≦3.0%.

2. 2. The multilayer electronic component according to claim 1, wherein the dielectric layer includes a region including two or more secondary phases of a rare earth element that satisfy D / td≦0.2 within a region of td μm×td μm.

3. When the length of the first dielectric crystal grain is defined as G and the length of a region in the shell portion of the first dielectric crystal grain that satisfies 1.5%≦RE≦3.0% is defined as d based on a straight line L passing through the center of the first dielectric crystal grain, 2. The multilayer electronic component according to claim 1, wherein 2.5%≦d / G≦47.0% is satisfied.

4. 4. The multilayer electronic component according to claim 3, wherein said d is 10 nm or more and 80 nm or less.

5. 2. The multilayer electronic component according to claim 1, wherein the dielectric layer includes a region including three or more of the first dielectric crystal grains within a region of 1 μm×1 μm.

6. 2. The multilayer electronic component according to claim 1, wherein the ratio of the number of moles of the rare earth element in the secondary phase to the total number of moles of all elements except oxygen is 30% or more.

7. 2. The multilayer electronic component according to claim 1, wherein the dielectric layer comprises a main component containing Ti, and a subcomponent.

8. The subcomponent includes a first subcomponent including a variable valence acceptor element, The variable valence acceptor element includes at least one of Mn, V, Cr, Fe, Co, Ni, Cu, Co, and Zn; 8. The multilayer electronic component according to claim 7, wherein the content of the first subcomponent is 0.2 mol to 1.4 mol per 100 mol of Ti.

9. The subcomponents include a second subcomponent containing Mg, The multilayer electronic component according to claim 7 , wherein the content of the second subcomponent is 2.0 moles or less per 100 moles of Ti.

10. The subcomponents include a third subcomponent containing a rare earth element, The rare earth element includes at least one of Y, Dy, Tb, Ho, Er, Gd, Ce, Nd, Sm, Tm, La, and Yb; 8. The multilayer electronic component according to claim 7, wherein the content of the third subcomponent is 2.5 mol to 8.0 mol per 100 mol of Ti.

11. The subcomponents include a fourth subcomponent including at least one element of Ba and Ca, The multilayer electronic component according to claim 7 , wherein the content of the fourth subcomponent is 4.8 mol or less per 100 mol of Ti.

12. The subcomponents include a fifth subcomponent containing Si, The multilayer electronic component according to claim 7 , wherein the content of the fifth subcomponent is 1.0 mole or more and less than 4.0 moles per 100 moles of Ti.

13. The subcomponents include a fifth subcomponent containing Si, and the content of the fifth subcomponent is 1.0 mole or more and less than 4.0 moles per 100 moles of Ti, The multilayer electronic component according to claim 11 , wherein a ratio of a content of the fourth subcomponent to a content of the fifth subcomponent based on 100 moles of Ti is 1.60 or less.

14. the dielectric layer includes a plurality of dielectric layers; 2. The multilayer electronic component according to claim 1, wherein at least one of said plurality of dielectric layers has an average thickness of 3.0 μm or less.

15. The internal electrode includes a plurality of internal electrodes, 2. The multilayer electronic component according to claim 1, wherein an average thickness of at least one of the plurality of internal electrodes is 1.0 [mu]m or less.

16. The dielectric layer includes a plurality of dielectric layers, and the internal electrode includes a plurality of internal electrodes. When an average thickness of at least one of the plurality of dielectric layers is defined as td1 and an average thickness of at least one of the plurality of internal electrodes is defined as te1, 2. The multilayer electronic component according to claim 1, wherein te1×2<td1 is satisfied.

17. The dielectric layer includes a main component including Ti and first to sixth subcomponents, The first subcomponent includes a variable valence acceptor element including at least one of Mn, V, Cr, Fe, Co, Ni, Cu, Co, and Zn, and the content of the first subcomponent is 0.2 moles to 1.4 moles with respect to 100 moles of Ti; The second subcomponent includes Mg, and the content of the second subcomponent is 2.0 moles or less per 100 moles of Ti; The third subcomponent includes at least one rare earth element selected from the group consisting of Y, Dy, Tb, Ho, Er, Gd, Ce, Nd, Sm, Tm, La, and Yb, and the content of the third subcomponent is 2.5 moles or more and 8.0 moles or less with respect to 100 moles of Ti; The fourth subcomponent includes at least one element selected from Ba and Ca, and the content of the fourth subcomponent is 4.8 mol or less relative to 100 mol of Ti; 2 . The multilayer electronic component according to claim 1 , wherein the fifth minor component includes Si, and the content of the fifth minor component is 1.0 mole or more and less than 4.0 moles per 100 moles of Ti.

18. The dielectric layer includes a main component including Ti and first to sixth subcomponents, The first subcomponent includes a variable valence acceptor element including at least one of Mn, V, Cr, Fe, Co, Ni, Cu, Co, and Zn, and the content of the first subcomponent is 0.2 moles to 1.4 moles with respect to 100 moles of Ti; The second subcomponent includes Mg, and the content of the second subcomponent is 2.0 moles or less per 100 moles of Ti; The third subcomponent includes at least one rare earth element selected from the group consisting of Y, Dy, Tb, Ho, Er, Gd, Ce, Nd, Sm, Tm, La, and Yb, and the content of the third subcomponent is 2.5 moles or more and 8.0 moles or less with respect to 100 moles of Ti; The fourth subcomponent includes at least one element selected from Ba and Ca, and the content of the fourth subcomponent is 4.8 mol or less relative to 100 mol of Ti; 4. The multilayer electronic component according to claim 3, wherein the fifth minor component contains Si, and the content of the fifth minor component is 1.0 mole or more and less than 4.0 moles per 100 moles of Ti.

Citation Information

Patent Citations

  • Ceramic capacitor and its manufacture

    JP2001006966A

  • Dielectric ceramic and laminated ceramic capacitor

    JP2011162401A

  • Dielectric ceramic composition and multilayer ceramic capacitor comprising the same

    KR1020150121569A