Blank mask and method of fabricating the same
Patent Information
- Application Number
- JP2024066246
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-16
AI Technical Summary
【0030】 実施例によるブランクマスクの製造方法は、洗浄段階における厚さ変化を最小化する。また、実施例によるブランクマスクの製造方法は、洗浄段階における透過率変化を最小化することができる。実施例によるブランクマスクの製造方法は、上記洗浄段階における光学密度変化を最小化することができる。実施例によるブランクマスクの製造方法は、上記洗浄段階における反射率変化を最小化することができる。
Smart Images

Figure 2024153599000001_ABST
Abstract
Description
[Technical field]
[0001] The embodiment relates to a blank mask and a method for manufacturing the same. [Background technology]
[0002] The increasing integration of semiconductor devices and other devices requires finer circuit patterns, which further emphasizes the importance of lithography, a technology for developing circuit patterns on the surface of a wafer using a photomask.
[0003] In order to develop fine circuit patterns, the exposure light source used in the exposure process must have a shorter wavelength. In recent years, the exposure light source used is the ArF excimer laser (wavelength 193 nm).
[0004] Meanwhile, photomasks include binary masks and phase shift masks.
[0005] A binary mask has a configuration in which a light-shielding layer pattern is formed on a light-transmitting substrate. In the binary mask, on the surface on which the pattern is formed, a transparent portion not including a light-shielding layer transmits the exposure light, and a light-shielding portion including a light-shielding layer blocks the exposure light, thereby exposing the pattern on a resist film on the surface of the wafer. However, as the pattern becomes finer, a binary mask may cause problems in developing fine patterns due to diffraction of light occurring at the edge of the transparent portion during the exposure process.
[0006] Phase shift masks include Levenson type, outrigger type, and half-tone type. Among them, the half-tone type phase shift mask has a configuration in which a pattern formed of a semi-transmitting film is formed on a light-transmitting substrate 10. In the half-tone type phase shift mask, on the surface on which the pattern is formed, the transmissive portion not including the semi-transmitting layer transmits the exposure light, and the semi-transmitting portion including the semi-transmitting layer transmits the attenuated exposure light. The attenuated exposure light has a phase difference compared to the exposure light that has passed through the transmissive portion. As a result, the diffracted light generated at the edge of the transmissive portion is offset by the exposure light that has passed through the semi-transmitting portion, and the phase shift mask can form a more elaborate and fine pattern on the surface of the wafer. [Prior art documents] [Patent documents]
[0007] The relevant prior art documents are as follows: [Patent Document 1] Korean Patent Publication No. 10-2012-0057488 [Patent Document 2] Korean Patent Publication No. 10-2014-0130420 Summary of the Invention [Problem to be solved by the invention]
[0008] The embodiments provide a blank mask and a manufacturing method thereof that can provide a photomask having fewer defects, improved number of uses, and high precision. [Means for solving the problem]
[0009] A manufacturing method of a blank mask according to an embodiment includes a step of forming a light-shielding film on a light-transmitting substrate and a step of cleaning the light-shielding film with a cleaning solution, and a thickness change of the light-shielding film during the cleaning step may be less than 15 nm.
[0010] In one embodiment, the method for manufacturing a blank mask may further include forming a phase shifting film on the light-transmitting substrate, and the light-shielding film may be formed on the phase shifting film.
[0011] In the method for manufacturing a blank mask according to an embodiment, the content of halogen ions on the entire surface of the blank mask is 0.1 ng / cm 2 The nitrogen ion content is less than 3ng / cm 2 The sulfur ion content is less than 0.1ng / cm 2 It may be less than.
[0012] In the method for manufacturing a blank mask according to an embodiment, the halogen ions may include chloride-based ions, the nitrogen-based ions may include nitrite ions, nitrate ions, and ammonia ions, and the sulfur-based ions may include sulfate ions.
[0013] In the method for manufacturing a blank mask according to an embodiment, the cleaning liquid may include carbonated water.
[0014] In the method for manufacturing a blank mask according to an embodiment, a change in transmittance of the light-shielding film during the cleaning step may be less than 0.05%.
[0015] In the method for manufacturing a blank mask according to an embodiment, the change in optical density of the light-shielding film during the cleaning step may be less than 0.07.
[0016] In the method for manufacturing a blank mask according to an embodiment, a change in reflectance of the light-shielding film during the cleaning step may be less than 0.5%.
[0017] In the method for manufacturing a blank mask according to an embodiment, a change in thickness of the light-shielding film in the cleaning step may be 0.3 nm to 3 nm.
[0018] In one embodiment of the method for manufacturing a blank mask, the light-shielding film includes a first light-shielding layer disposed on the light-transmitting substrate, and a second light-shielding layer disposed on the first light-shielding layer, and the second light-shielding layer may include nitrogen elements at a content of 20 atomic % to 40 atomic %, chromium elements at a content of 30 atomic % to 50 atomic %, and oxygen elements at a content of 20 atomic % to 40 atomic %.
[0019] In the method for manufacturing a blank mask according to an embodiment, the first light-shielding layer may contain nitrogen element with a content of 10 atomic % to 30 atomic %, chromium element with a content of 60 atomic % to 90 atomic %, and oxygen element with a content of 0.5 atomic % to 10 atomic %.
[0020] In the method for manufacturing a blank mask according to an embodiment, the second light-shielding layer may contain carbon element at a content of less than 5 atom %.
[0021] The blank mask according to the embodiment includes a light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate, and the halogen ion content on the entire surface is 0.05 ng / cm 2 The nitrogen ion content is less than 2ng / cm 2 The sulfur ion content is less than 0.1ng / cm 2 It may be less than.
[0022] In the blank mask according to one embodiment, the thickness change of the light-shielding film measured by the following measurement method may be less than 15 nm.
[0023] [Measurement method] The light-shielding film was immersed in carbonated water having a carbon dioxide concentration of 2000 mg / l for 10 minutes, and the thickness change of the light-shielding film was the difference between the thickness of the light-shielding film before immersion and the thickness of the light-shielding film after immersion.
[0024] In a blank mask according to one embodiment, a change in transmittance of the light-shielding film is less than 0.05%, a change in optical density of the light-shielding film is less than 0.07, a change in reflectance of the light-shielding film is less than 0.5%, the change in transmittance is a difference between the transmittance of the light-shielding film before immersion and the transmittance of the light-shielding film after immersion, the change in optical density is a difference between the optical density of the light-shielding film before immersion and the optical density of the light-shielding film after immersion, and the change in reflectance may be a difference between the reflectance of the light-shielding film before immersion and the reflectance of the light-shielding film after immersion.
[0025] In the blank mask according to one embodiment, the light-shielding film includes a first light-shielding layer disposed on the light-transmitting substrate, and a second light-shielding layer disposed on the first light-shielding layer, and the second light-shielding layer may include nitrogen elements at a content of 20 atomic % to 40 atomic %, chromium elements at a content of 30 atomic % to 50 atomic %, and oxygen elements at a content of 20 atomic % to 40 atomic %.
[0026] In the blank mask according to an embodiment, the first light-shielding layer may contain nitrogen element with a content of 10 atomic % to 30 atomic %, chromium element with a content of 60 atomic % to 90 atomic %, and oxygen element with a content of 0.5 atomic % to 10 atomic %.
[0027] In the blank mask according to one embodiment, the thickness change of the light-shielding film may be 0.3 nm to 3 nm.
[0028] In the blank mask according to one embodiment, the thickness variation of the light-shielding film may be 0.1 nm to 1 nm.
[0029] The photomask according to the embodiment includes a light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate, and the halogen ion content on the entire surface is 0.05 ng / cm 2 The nitrogen ion content is less than 2ng / cm 2 The sulfur ion content is less than 0.1ng / cm 2 It may be less than. Effect of the Invention
[0030] The blank mask manufacturing method according to the embodiment can minimize thickness variation during the cleaning step. Also, the blank mask manufacturing method according to the embodiment can minimize transmittance variation during the cleaning step. The blank mask manufacturing method according to the embodiment can minimize optical density variation during the cleaning step. The blank mask manufacturing method according to the embodiment can minimize reflectance variation during the cleaning step.
[0031] Thus, in the method for manufacturing a blank mask according to the embodiment, the ion concentration at the surface may be low.The concentrations of halogen ions, nitrogen-based ions, and sulfur-based ions at the surface of the blank mask according to the embodiment may be low.
[0032] In the method for manufacturing a blank mask according to the embodiment, the cleaning solution may include carbonated water, thereby minimizing the thickness change, the transmittance change, the optical density change, and the reflectance change during the cleaning step, and reducing the concentrations of the halogen ions, the nitrogen ions, and the sulfur-based ions. [Brief description of the drawings]
[0033] [Figure 1] 1 is a cross-sectional view showing one cross section of a blank mask according to an embodiment. [Diagram 2] FIG. 11 is a cross-sectional view showing one section of a blank mask according to another embodiment. [Diagram 3] 13 is a cross-sectional view showing one cross section of a blank mask according to still another embodiment. FIG. [Figure 4] 1 is a cross-sectional view showing one cross section of a photomask according to an embodiment; [Diagram 5] 11A to 11C are diagrams illustrating a process of cleaning a blank mask according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings, in which: FIG. 1 is a block diagram of a method for manufacturing a semiconductor device according to an embodiment of the present invention;
[0035] As used herein, terms of degree such as "about," "substantially," and the like are used to mean a value at or near that value when the tolerances of manufacturing and materials inherent in the referred meaning are given, and are used to prevent unscrupulous infringers from unfairly exploiting the contents of the disclosure in which precise or absolute values are referred to for the understanding of embodiments.
[0036] Throughout this specification, the term "combinations thereof" contained in a Markush form phrase means a mixture or combination of one or more selected from the group of components set forth in the Markush form phrase, including one or more selected from the group of components set forth above.
[0037] Throughout this specification, the phrase "A and / or B" means "A, B, or A and B."
[0038] Throughout this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from one another, unless otherwise specified.
[0039] In this specification, the term "B is located on A" means that B is located on A, or B is located on A with another layer therebetween, or B may be located thereon, and is not to be interpreted as being limited to B being located in contact with the surface of A.
[0040] In this specification, the singular expression is to be construed as including the singular or plural as the context requires, unless otherwise specified.
[0041] Fig. 1 is a cross-sectional view showing one cross section of a blank mask according to one embodiment. Fig. 2 is a cross-sectional view showing one cross section of a blank mask according to another embodiment. Fig. 3 is a cross-sectional view showing one cross section of a blank mask according to yet another embodiment. Fig. 4 is a cross-sectional view showing one cross section of a photomask according to one embodiment. Fig. 5 is a view showing a process of cleaning a blank mask according to an embodiment.
[0042] The blank mask 100 according to the embodiment includes a light-transmitting substrate 10 and a light-shielding film 20 located on the light-transmitting substrate 10 .
[0043] The light-transmitting substrate 10 may have light transmittance to the exposure light. The light-transmitting substrate 10 may have a transmittance of more than about 85% to the exposure light having a wavelength of about 193 nm. The transmittance of the light-transmitting substrate 20 may be more than about 87%. The transmittance of the light-transmitting substrate 10 may be less than 99.99%. The light-transmitting substrate 10 may include a synthetic quartz substrate. In such a case, the light-transmitting substrate 10 can suppress attenuation of the transmitted light.
[0044] The light-transmitting substrate 10 has surface characteristics such as appropriate flatness and appropriate illuminance, and therefore can suppress distortion of the transmitted light.
[0045] The light-shielding film 20 may be disposed on the top side of the light-transmitting substrate 10 .
[0046] The light-shielding film 20 can at least selectively block exposure light incident on the bottom side of the light-transmitting substrate 10 .
[0047] In addition, as shown in FIG. 2, when a phase shifting film 30 or the like is disposed between the light-transmitting substrate 10 and the light-shielding film 20, the light-shielding film 20 can be used as an etching mask in a process of etching the phase shifting film 30 or the like according to a pattern shape.
[0048] The light-shielding film 20 may contain at least one of a transition metal, oxygen, and nitrogen.
[0049] The light-shielding film 20 may include chromium, oxygen, nitrogen, and carbon. The elemental contents of the entire light-shielding film 20 may be different in the thickness direction. When the light-shielding film 20 is a multi-layered film, the elemental contents of the entire light-shielding film 20 may be different for each layer.
[0050] The light-shielding film 20 may contain chromium at a content of about 44 atom % to about 60 atom %.The light-shielding film 20 may contain chromium at a content of about 47 atom % to about 57 atom %.
[0051] The light-shielding film 20 may contain carbon at a content of about 5 atom % to about 30 atom %.The light-shielding film 20 may contain carbon at a content of about 7 atom % to about 25 atom %.
[0052] The light-shielding film 20 may contain nitrogen at a content of about 3 atom % to about 20 atom %. The light-shielding film 20 may contain nitrogen at a content of about 5 atom % to about 15 atom %. The light-shielding film 20 may contain oxygen at a content of about 20 atom % to about 45 atom %. The light-shielding film 20 may contain oxygen at a content of about 25 atom % to about 40 atom %.
[0053] The upper portion of the light-shielding film 20 may contain nitrogen elements at a content of about 6 atom % to about 16 atom %, chromium elements at a content of about 26 atom % to about 46 atom %, oxygen elements at a content of about 37 atom % to about 47 atom %, and carbon elements at a content of about 4 atom % to about 14 atom %.
[0054] The upper portion of the light-shielding film 20 may contain nitrogen element at a content of about 16 atom % to about 26 atom %, chromium element at a content of about 28 atom % to about 40 atom %, oxygen element at a content of about 27 atom % to about 37 atom %, and carbon element at a content of about 3 atom % to about 13 atom %.
[0055] The upper portion of the light-shielding film 20 may contain nitrogen element at a content of about 18 atom % to about 27 atom %, chromium element at a content of about 35 atom % to about 41 atom %, oxygen element at a content of about 31 atom % to about 41 atom %, and carbon element at a content of about 1 atom % to about 4 atom %.
[0056] The upper portion of the light-shielding film 20 can be defined as a depth of 1 / 8 based on the total thickness of the light-shielding film 20 from the upper surface of the light-shielding film 20. In other words, when the total thickness of the light-shielding film 20 is 8, the upper portion of the light-shielding film 20 means a depth of 1 from the upper surface of the light-shielding film 20.
[0057] The nitrogen element content in the upper part of the light-shielding film 20 may gradually increase. The nitrogen element content in the upper part of the light-shielding film 20 may gradually increase from anywhere in a range of about 15 atom % to about 25 atom %. In this case, the difference between the minimum and maximum values of the nitrogen element content in the upper part of the light-shielding film 20 may be about 3 atom % to about 8 atom %.
[0058] The chromium element content in the upper part of the light-shielding film 20 may gradually increase. The chromium element content in the upper part of the light-shielding film 20 may gradually increase from anywhere in a range of about 30 atom % to about 40 atom %. In this case, the difference between the minimum and maximum values of the chromium element content in the upper part of the light-shielding film 20 may be about 3 atom % to about 8 atom %.
[0059] The carbon element content in the upper portion of the light-shielding film 20 may be gradually decreased. The carbon element content in the upper portion of the light-shielding film 20 may be gradually decreased from any one of about 1 atom % to about 7 atom %. In this case, the difference between the minimum and maximum values of the carbon element content in the upper portion of the light-shielding film 20 may be about 0.5 atom % to about 5 atom %.
[0060] The oxygen element content in the upper part of the light-shielding film 20 may be gradually decreased. The oxygen element content in the upper part of the light-shielding film 20 may be gradually decreased from anywhere in a range of about 35 atom% to about 45 atom%. In this case, the difference between the minimum and maximum value of the oxygen element content in the upper part of the light-shielding film 20 may be about 4 atom% to about 14 atom%.
[0061] In this case, the light-shielding film 20 can have sufficient light-extinguishing properties.
[0062] As shown in FIG. 3, the light-shielding film 20 may include a first light-shielding layer 21 and a second light-shielding layer 22 disposed on the first light-shielding layer 21.
[0063] The second light-shielding layer 22 includes a transition metal. The second light-shielding layer 22 may also include at least one of oxygen, nitrogen, and carbon. The second light-shielding layer 22 may include a transition metal content of about 50 atom % to about 80 atom %. The second light-shielding layer 22 may include a transition metal content of about 55 atom % to about 75 atom %. The second light-shielding layer 22 may include a transition metal content of about 60 atom % to about 70 atom %.
[0064] The content of the element corresponding to at least one of oxygen, nitrogen, and carbon in the second light-shielding layer 22 may be about 10 atom % to about 35 atom %. The content of the element corresponding to at least one of oxygen, nitrogen, and carbon in the second light-shielding layer 22 may be about 15 atom % to about 25 atom %.
[0065] The second light-shielding layer 22 may contain nitrogen at a content of about 5 atom % to about 20 atom %.The second light-shielding layer 22 may contain nitrogen at a content of about 7 atom % to about 13 atom %.
[0066] The second light-shielding layer 22 may contain oxygen at a content of about 5 atom % to about 20 atom %.The second light-shielding layer 22 may contain oxygen at a content of about 7 atom % to about 13 atom %.
[0067] The second light-shielding layer 22 may contain carbon at a content of about 2 atom % to about 10 atom %.The second light-shielding layer 22 may contain nitrogen at a content of about 37 atom % to about 8 atom %.
[0068] The second light-shielding layer 22 may contain any of nitrogen, oxygen, and carbon.
[0069] In such a case, the light-shielding film 20 may form a laminate with the phase shift film 30 to help substantially block the exposure light.
[0070] The first light-shielding layer 21 may contain a transition metal. The first light-shielding layer 21 may contain oxygen and nitrogen. The first light-shielding layer 21 may contain a transition metal at 30 atom % or more and 60 atom % or less. The light-shielding layer 21 may contain a transition metal at 35 atom % or more and 55 atom % or less. The first light-shielding layer 21 may contain a transition metal at 40 atom % or more and 50 atom % or less.
[0071] The sum of the oxygen content and the nitrogen content of the first light-shielding layer 21 may be 40 atom % or more and 70 atom % or less. The sum of the oxygen content and the nitrogen content of the first light-shielding layer 21 may be 45 atom % or more and 65 atom % or less. The sum of the oxygen content and the nitrogen content of the first light-shielding layer 21 may be 50 atom % or more and 60 atom % or less.
[0072] The first light-shielding layer 21 may contain oxygen at 20 atom % or more and 40 atom % or less. The first light-shielding layer 21 may contain oxygen at 23 atom % or more and 33 atom % or less. The first light-shielding layer 21 may contain oxygen at 25 atom % or more and 30 atom % or less.
[0073] The first light-shielding layer 21 may contain nitrogen at 5 atomic % or more and 20 atomic % or less. The first light-shielding layer 21 may contain nitrogen at 7 atomic % or more and 17 atomic % or less. The first light-shielding layer 21 may contain nitrogen at 10 atomic % or more and 15 atomic % or less.
[0074] In this case, the first light-shielding layer 21 can help the light-shielding film 20 to have excellent extinction properties.
[0075] The transition metal may include at least one of Cr, Ta, Ti, and Hf. The transition metal may be Cr.
[0076] The second light-shielding layer may contain nitrogen element at a content of about 20 atomic % to about 40 atomic %, chromium element at a content of about 30 atomic % to about 50 atomic %, and oxygen element at a content of about 20 atomic % to about 40 atomic %. The second light-shielding layer may further contain carbon element at a content of less than 5 atomic %.
[0077] The second light-shielding layer may contain nitrogen at a content of about 24 atom% to about 34 atom%, chromium at a content of about 35 atom% to about 45 atom%, and oxygen at a content of about 26 atom% to about 36 atom%, and may further contain carbon at a content of less than 3 atom%.
[0078] The second light-shielding layer may contain nitrogen element at a content of about 6 atom % to about 16 atom %, chromium element at a content of about 26 atom % to about 46 atom %, oxygen element at a content of about 37 atom % to about 47 atom %, and carbon element at a content of about 4 atom % to about 14 atom %.
[0079] The second light-shielding layer may contain nitrogen element at a content of about 16 atom % to about 26 atom %, chromium element at a content of about 28 atom % to about 40 atom %, oxygen element at a content of about 27 atom % to about 37 atom %, and carbon element at a content of about 3 atom % to about 13 atom %.
[0080] The first light-shielding layer may contain nitrogen element at a content of about 10 atom% to about 30 atom%, chromium element at a content of about 60 atom% to about 90 atom%, and oxygen element at a content of about 0.5 atom% to about 5 atom%. The first light-shielding layer may also contain carbon element at a content of less than 5 atom%.
[0081] The composition of the light-shielding film can be measured by X-ray Photoelectron Spectroscopy (XPS).
[0082] For example, a blank mask according to the embodiment is processed to a size of 15 mm in width and 15 mm in length to prepare a specimen. The specimen is then placed in a Thermo Scientific K-Alpha model, and a region of 4 mm in width and 2 mm in length located in the center of the specimen is etched with argon gas. During the etching time for each layer, the vacuum level in the measurement equipment is maintained at 1.0×10 -8 The pressure was 1000 psi, the X-ray source was a Monochromator Al Kα (1486.6 eV), the anode power was 72 W, the anode voltage was 12 kV, and the voltage of the argon ion beam was 1 kV.
[0083] Furthermore, in the etching time of the light-shielding film, the composition data from about 0 seconds to about 30 seconds is inaccurate data, and therefore can be excluded from the composition of the light-shielding film.
[0084] The first light-shielding layer 21 may have a thickness of about 250 Å to about 650 Å. The first light-shielding layer 21 may have a thickness of about 350 Å to about 600 Å. The first light-shielding layer 21 may have a thickness of about 400 Å to about 550 Å. In this case, the first light-shielding layer 21 may help the light-shielding film 20 to effectively block exposure light.
[0085] The second light-shielding layer 22 may have a thickness of about 30 Å to about 200 Å. The second light-shielding layer 22 may have a thickness of about 30 Å to about 100 Å. The second light-shielding layer 22 may have a thickness of about 40 Å to about 80 Å. In this case, the second light-shielding layer 22 may improve the extinction characteristic of the light-shielding film 20, and may help to more precisely control the surface profile of the side of the light-shielding pattern film 25 formed when the light-shielding film 20 is patterned.
[0086] A ratio of a thickness of the second light-shielding layer 22 to a thickness of the first light-shielding layer 21 may be about 0.05 to about 0.3. A ratio of a thickness of the second light-shielding layer 22 to a thickness of the first light-shielding layer 21 may be about 0.07 to about 0.25. A ratio of a thickness of the second light-shielding layer 22 to a thickness of the first light-shielding layer 21 may be about 0.1 to about 0.2.
[0087] In such a case, the light-shielding film 20 has sufficient extinction properties, and the surface profile of the side surface of the light-shielding pattern film 25 formed during patterning of the light-shielding film 20 can be controlled more precisely.
[0088] The second light-shielding layer 22 may have a transition metal content greater than that of the first light-shielding layer 21 .
[0089] In order to more precisely control the surface profile of the side of the light-shielding pattern film 25 formed by patterning the light-shielding film 20 and to ensure that the surface reflectance of the light-shielding film 20 to the inspection light in defect inspection has a value suitable for inspection, the second light-shielding layer 22 is required to have a larger transition metal content than the first light-shielding layer 31.
[0090] However, in this case, recovery, recrystallization, and grain growth may occur in the transition metal contained in the second light-shielding layer 22 during heat treatment of the formed light-shielding film 20. If grain growth occurs in the second light-shielding layer 22 containing a high content of transition metal, the surface illuminance characteristics of the light-shielding film 20 may fluctuate excessively due to overgrown transition metal particles. This may cause an increase in the number of false defects detected when the surface of the light-shielding film 20 is inspected for defects with high sensitivity.
[0091] The light-shielding film 20 may have a transmittance of about 1% to about 2% for light with a wavelength of 193 nm. The light-shielding film 20 may have a transmittance of about 1.3% to about 2% for light with a wavelength of 193 nm. The light-shielding film 20 may have a transmittance of about 1.4% to about 2% for light with a wavelength of 193 nm.
[0092] The light-shielding film 20 may have an optical density of about 1.8 to about 3. The light-shielding film 20 may have an optical density of about 1.9 to about 3.
[0093] In such a case, the thin film including the light-shielding film 20 can effectively suppress the transmission of the exposure light.
[0094] As shown in FIG. 3, the blank mask 100 according to the embodiment may further include a phase shift film 30 .
[0095] The phase shift film 30 may be disposed between the light-transmitting substrate 10 and the light-shielding film 20. The phase shift film 30 may be a thin film that attenuates the intensity of the transmitted exposure light, adjusts the phase difference, and substantially suppresses diffracted light generated at the edge of a pattern.
[0096] The phase shift film 30 may have a phase difference of about 170° to about 190° with respect to light having a wavelength of 193 nm. The phase shift film 40 may have a phase difference of about 175° to about 185° with respect to light having a wavelength of 193 nm.
[0097] The phase shift film 30 may have a transmittance of about 3% to about 10% for light with a wavelength of 193 nm. The phase shift film 30 may have a transmittance of about 4% to about 8% for light with a wavelength of 193 nm. In such a case, the resolution of the photomask 200 including the phase shift film 30 may be improved.
[0098] The phase shifter film 30 may contain a transition metal and silicon. The phase shifter film 30 may contain a transition metal, silicon, oxygen, and nitrogen. The transition metal may be molybdenum.
[0099] A hard mask (not shown) may be positioned on the light-shielding film 20. The hard mask may function as an etching mask film when etching the pattern of the light-shielding film 20. The hard mask may contain silicon, nitrogen, and oxygen.
[0100] As shown in FIG. 4, the photomask 200 according to the embodiment includes the light-transmitting substrate 10 and a light-shielding pattern film 25 disposed on the light-transmitting substrate 10 .
[0101] The light-shielding pattern film 25 contains at least one of a transition metal, oxygen, and nitrogen.
[0102] The light-shielding pattern film 25 may be formed by patterning the light-shielding film 20 of the blank mask 100 described above.
[0103] Descriptions of the properties, composition, structure, etc. of the light-shielding pattern film 25 overlap with the description of the light-shielding film 20 of the blank mask 100, and therefore will be omitted.
[0104] The manufacturing method of the blank mask 100 according to the embodiment includes forming the light-shielding film 20 on the light-transmitting film. The light-shielding film 20 may be formed by a sputtering process.
[0105] The method may include a preparation step of providing a light-transmitting substrate and a sputtering target in a sputtering chamber such that the distance between the light-transmitting substrate and the sputtering target is 260 mm or more and 300 mm or less.
[0106] The manufacturing method of the blank mask 100 according to the embodiment may include a deposition step of depositing the light-shielding film 20 by injecting an atmospheric gas into a sputtering chamber, applying power to the sputtering target, and rotating the light-transmitting substrate at 25 rpm or more.
[0107] The deposition step may include a first light-shielding layer deposition process of depositing a first light-shielding layer on a light-transmitting substrate, and a second light-shielding layer deposition process of depositing a second light-shielding layer on the first light-shielding layer.
[0108] After the sputtering process, a heat treatment process may be performed.
[0109] The heat treatment step can be performed at a temperature of about 200°C to about 400°C.
[0110] The heat treatment step may be performed for about 5 minutes to about 30 minutes.
[0111] Also, the method for manufacturing the blank mask 100 according to the embodiment may further include a step of freezing the light-shielding film 20 that has been subjected to the heat treatment process.
[0112] The sputtering target can be selected in consideration of the composition of the light-shielding film 20 to be formed. The sputtering target can be one target containing a transition metal. The sputtering target can be two or more targets including one target containing a transition metal. The target containing a transition metal may contain 90 atom% or more of the transition metal. The target containing a transition metal may contain 95 atom% or more of the transition metal. The target containing a transition metal may contain 99 atom% of the transition metal.
[0113] The transition metal may include at least one of Cr, Ta, Ti, and Hf. The transition metal may include Cr.
[0114] In the deposition step, the rotation speed of the light-transmitting substrate may be 25 rpm or more. The rotation speed may be 30 rpm or more. The rotation speed may be 100 rpm or less. In such a case, the variation in thickness of the light-shielding film 20 in the in-plane direction to be deposited may be effectively reduced. In addition, the surface illuminance characteristics of each sector within the surface of the light-shielding film 20 may be adjusted to within a range already set in the embodiment.
[0115] The atmospheric gas may include an inert gas, a reactive gas, and a sputtering gas. The inert gas is a gas that does not contain elements that constitute the deposited thin film. The reactive gas is a gas that contains elements that constitute the deposited thin film.
[0116] The sputtering gas is a gas that is ionized in a plasma atmosphere and collides with a target. The inert gas may include helium.
[0117] The reactive gas may include a gas containing a nitrogen element. The gas containing a nitrogen element may be, for example, N2, NO, NO2, N2O, N2O3, N2O4, or N2O5. The reactive gas may include a gas containing an oxygen element.
[0118] The gas containing oxygen may be O2, for example. The reactive gas may include a gas containing nitrogen and a gas containing oxygen. The reactive gas may include a gas containing both nitrogen and oxygen. The gas containing both nitrogen and oxygen may be NO, NO2, N2O, N2O3, N2O4, or N2O5, for example.
[0119] The reactive gas containing carbon and oxygen may also be CO2.
[0120] The sputtering gas may be Ar gas.
[0121] The power source for applying power to the sputtering target may be a DC power source or an RF power source.
[0122] In the process of forming the first light-shielding layer 21, the power applied to the sputtering target can be about 1.5 kW to about 2.5 kW. In the process of forming the first light-shielding layer 21, the power applied to the sputtering target can be about 1.6 kW to about 2 kW.
[0123] In the process of forming the first light-shielding layer 21, the ratio of the flow rate of the reactive gas to the flow rate of the inert gas in the atmospheric gas may be about 1.5 to about 3. The ratio of the flow rates may be about 1.8 to about 2.7. The ratio of the flow rates may be about 2 to about 2.5.
[0124] The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be about 1.5 to about 4. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be about 2 to about 3. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be about 2.2 to about 2.7.
[0125] In this case, the first light-shielding layer 21 can help the light-shielding film 20 to have sufficient extinction properties. Also, the etching speed of the first light-shielding layer 21 can be improved to help the surface profile of the side of the light-shielding pattern film 25 formed by patterning the light-shielding film 20 to have a shape close to perpendicular to the light-transmitting substrate 10.
[0126] The deposition time of the first light-shielding layer 21 may be about 200 seconds to about 300 seconds. The deposition time of the first light-shielding layer 21 may be about 210 seconds to about 240 seconds. In this case, the first light-shielding layer 21 may help the light-shielding film 20 to have sufficient extinction properties.
[0127] In the process of forming the second light-shielding layer 22, the power applied to the sputtering target can be about 1 kW to about 2 kW. In the process of forming the second light-shielding layer 22, the power applied to the sputtering target can be about 1.2 kW to about 1.7 kW.
[0128] In the process of forming the second light-shielding layer 22, the ratio of the flow rate of the reactive gas to the flow rate of the inert gas in the atmospheric gas may be about 0.3 to about 0.8. The ratio of the flow rates may be about 0.4 to about 0.6.
[0129] In the process of forming the second light-shielding layer 22, the ratio of the oxygen content to the nitrogen content contained in the reactive gas may be less than about 0.3. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be less than about 0.1. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be more than 0.001. Since the second light-shielding layer 22 is formed as described above, the light-shielding film 20 may have stable quenching properties.
[0130] The deposition time of the second light-shielding layer 22 may be about 10 seconds to about 30 seconds. The deposition time of the second light-shielding layer 22 may be about 15 seconds to about 25 seconds. In such a case, the second light-shielding layer 22 can suppress the transmission of the exposure light.
[0131] In the heat treatment step, a plurality of regions on the surface of the light-shielding film 20 may be heat-treated at temperatures independently controlled. Specifically, a heater may be provided for each region on the surface of the light-shielding film 20. The heater for each region may be provided on the light-transmitting substrate side.
[0132] The temperature of the heaters for each zone can be controlled independently within a range of about 200°C to 400°C.
[0133] The blank mask 100 may be cooled within 2 minutes after the heat treatment, which may effectively prevent the growth of crystal grains of transition metal particles due to residual heat in the light-shielding film 20.
[0134] In the above cooling step, pins having a preset length are provided at each corner of the cooling plate, and the blank mask 100 is placed on the pins so that the substrate faces the cooling plate, thereby controlling the cooling rate of the blank mask 100 according to the embodiment.
[0135] In the cooling step, the cooling temperature applied to the cooling plate may be about 10° C. to about 30° C. The cooling temperature may be about 15° C. to about 25° C.
[0136] In the cooling step, the distance between the blank mask 100 according to the embodiment and the cooling plate may be about 0.01 mm to about 30 mm. The distance may be 0.05 mm or more and 5 mm or less. The distance may be 0.1 mm or more and 2 mm or less.
[0137] The cooling step can be carried out for about 1 minute to about 10 minutes. The cooling step can be carried out for about 3 minutes to about 7 minutes.
[0138] Thereafter, the cooled light-shielding film 20 can be washed. The washing step may include an ultraviolet ray irradiation step and / or a rinsing step.
[0139] The ultraviolet ray irradiation step may include a step of irradiating the light-shielding film 20 with ultraviolet rays.
[0140] The ultraviolet light used in the ultraviolet light irradiation step may be vacuum ultraviolet light.The ultraviolet light used in the ultraviolet light irradiation step may be ultraviolet light having a peak wavelength band of about 100 nm to about 190 nm.
[0141] The ultraviolet irradiation step can be carried out at room temperature and at a relative humidity of about 30% to about 60%.The ultraviolet irradiation step can be carried out at room temperature and at a relative humidity of about 40% to about 50%.
[0142] In the ultraviolet ray irradiation step, the output of the ultraviolet ray irradiated onto the light-shielding film 20 is about 5 mW / cm 2 ~about 100mW / cm 2 In the ultraviolet ray irradiation step, the output of the ultraviolet ray irradiated onto the light-shielding film 20 may be about 10 mW / cm. 2 ~about 70mW / cm 2 may be also possible.
[0143] In the ultraviolet irradiation step, the time for irradiating the light-shielding film 20 with the ultraviolet light may be about 10 seconds to about 10 minutes. In the ultraviolet irradiation step, the time for irradiating the light-shielding film 20 with the ultraviolet light may be about 10 seconds to about 5 minutes. In the ultraviolet irradiation step, the time for irradiating the light-shielding film 20 with the ultraviolet light may be about 1 minute to about 10 minutes. In the ultraviolet irradiation step, the time for irradiating the light-shielding film 20 with the ultraviolet light may be about 10 seconds to about 1 minute.
[0144] In the ultraviolet ray irradiation step, nitrogen gas (N2) or oxygen gas (O2) can be used as the atmospheric gas.
[0145] The rinsing process includes treating the light-shielding film 20 with a cleaning solution. The cleaning solution may include at least one of deionized water, hydrogen water, ozone water, and carbonated water. The cleaning solution may include the carbonated water.
[0146] The carbonated water may have a carbon dioxide concentration of about 500 mg / l to about 5000 mg / l.The carbonated water may have a carbon dioxide concentration of about 1000 mg / l to about 3000 mg / l.
[0147] The ozone concentration in the ozone water may be about 50 mg / l to about 2000 mg / l.The ozone concentration in the ozone water may be about 100 mg / l to about 1000 mg / l.
[0148] The hydrogen concentration in the hydrogen water may be about 0.1 mg / l to about 10 mg / l.The hydrogen concentration in the hydrogen water may be about 0.5 mg / l to about 5 mg / l.
[0149] The cleaning solution treatment step may include a step of immersing the blank mask 100 according to the embodiment in the cleaning solution. The cleaning solution treatment step may include a step of spraying the cleaning solution on the light-shielding film 20 to cause the cleaning solution to flow.
[0150] In the cleaning solution treatment step, the process time may be from about 1 minute to about 10 minutes.In the cleaning solution treatment step, the process time may be from about 2 minutes to about 7 minutes.
[0151] Thereafter, in the cleaning solution treatment step, the light-shielding film 20 may be irradiated with ultraviolet light. That is, the rinsing process and the ultraviolet light irradiation process may be performed simultaneously. The rinsing process may be performed after the ultraviolet light irradiation process. During the rinsing process, the light-shielding film 20 may be irradiated with ultraviolet light in a manner similar to the ultraviolet light irradiation process.
[0152] After the above rinsing process is performed, the blank mask 100 according to the embodiment can be dried.
[0153] 6, the thickness of the light-shielding film 20 may change in the cleaning process. That is, in the cleaning process, a part of the light-shielding film 20 may be removed, and the thickness of the light-shielding film 20 may decrease. In the cleaning process, the thickness change (ΔT) of the light-shielding film 20 may be the difference between the thickness before the cleaning process and the thickness after the cleaning process.
[0154] In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 15 nm. In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 5 nm. In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 4 nm. In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 3 nm. In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 2.5 nm. In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 2 nm. In the cleaning process, the thickness change of the light-shielding film 20 may be less than about 1.5 nm.
[0155] In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.3 nm to about 3 nm, or about 0.1 nm to about 1 nm.
[0156] In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.1 nm to about 5 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.2 nm to about 5 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.3 nm to about 5 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.1 nm to about 3 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.2 nm to about 3 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 0.3 nm to about 3 nm.
[0157] In the cleaning step, the thickness change of the light-shielding film 20 may be about 3 nm to about 15 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 3 nm to about 8 nm. In the cleaning step, the thickness change of the light-shielding film 20 may be about 5 nm to about 15 nm.
[0158] In the cleaning step, the thickness of the light-shielding film 20 in the film-forming step can be determined by taking into consideration the change in thickness of the light-shielding film 20.
[0159] In the cleaning step, the thickness change of the light-shielding film 20 may be a thickness change of the second light-shielding layer 22.
[0160] In the cleaning step, the thickness change of the light-shielding film 20 has an appropriate range as described above, and therefore the optical properties of the light-shielding film 20 can change in an appropriate range.
[0161] In the cleaning process, the thickness change of the light-shielding film 20 is the same as described above, so that the change in the optical properties of the light-shielding film 20 can be minimized.
[0162] In the cleaning process, a change in transmittance of the light-shielding film 20 may occur. The change in transmittance of the light-shielding film 20 may be a difference between the transmittance before the cleaning process and the transmittance after the cleaning process. The transmittance of the light-shielding film 20 can be measured by light in a wavelength band of about 193 nm.
[0163] In the cleaning process, the change in transmittance of the light-shielding film 20 may be less than about 0.03%. In the cleaning process, the change in transmittance of the light-shielding film 20 may be less than about 0.02%. In the cleaning process, the change in transmittance of the light-shielding film 20 may be less than about 0.01%. In the cleaning process, the change in transmittance of the light-shielding film 20 may be less than about 0.007%. In the cleaning process, the change in transmittance of the light-shielding film 20 may be less than about 0.005%. In the cleaning process, the change in transmittance of the light-shielding film 20 may be less than about 0.003%.
[0164] In the cleaning step, the change in transmittance of the light-shielding film 20 may be about 0.005% to about 0.02%.
[0165] In the cleaning process, the minimum change in transmittance of the light-shielding film 20 may be about 0.00001%.
[0166] In the cleaning process, the change in transmittance of the light-shielding film 20 is the same as described above, so that the light-shielding film 20 can reduce deviation in transmittance at different positions, thereby providing a precise photomask using the blank mask 100 according to the embodiment.
[0167] During the cleaning process, a change in optical density may occur in the light-shielding film 20. The change in optical density of the light-shielding film 20 may be a difference between the optical density before the cleaning process and the optical density after the cleaning process. The optical density may be measured by an optical density meter such as a Linshang LS117.
[0168] In the cleaning process, the optical density change of the light-shielding film 20 may be less than about 0.1. In the cleaning process, the optical density change of the light-shielding film 20 may be less than about 0.07. In the cleaning process, the optical density change of the light-shielding film 20 may be less than about 0.05. In the cleaning process, the optical density change of the light-shielding film 20 may be less than about 0.03. In the cleaning process, the optical density change of the light-shielding film 20 may be less than about 0.02.
[0169] In the cleaning step, the change in optical density of the light-shielding film 20 may be about 0.01 to about 0.08.
[0170] In the cleaning process, the change in optical density of the light-shielding film 20 is the same as described above, so that the light-shielding film 20 can reduce the deviation in optical density at each position, thereby providing a precise photomask using the blank mask 100 according to the embodiment.
[0171] In the cleaning process, a change in reflectance of the light-shielding film 20 may occur. The change in reflectance of the light-shielding film 20 may be a difference between the reflectance before the cleaning process and the reflectance after the cleaning process. The reflectance can be measured by light in a wavelength band of about 193 nm.
[0172] In the cleaning process, the change in reflectance of the light-shielding film 20 may be less than about 0.5%. In the cleaning process, the change in reflectance of the light-shielding film 20 may be less than about 0.4%. In the cleaning process, the change in reflectance of the light-shielding film 20 may be less than about 0.3%. In the cleaning process, the change in reflectance of the light-shielding film 20 may be less than about 0.2%.
[0173] In the cleaning process, the minimum change in reflectance of the light-shielding film 20 may be about 0.01%.
[0174] In the cleaning process, the change in reflectance of the light-shielding film 20 is the same as described above, so that the light-shielding film 20 can reduce deviation in reflectance at different positions, thereby providing a precise photomask using the blank mask 100 according to the embodiment.
[0175] The blank mask 100 according to the embodiment may have a low ion concentration at the surface.
[0176] The halogen ion content on the entire surface of the blank mask 100 according to the embodiment is 0.15 ng / cm 2 The halogen ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.10 ng / cm 2 The halogen ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.07 ng / cm 2 The halogen ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.05 ng / cm 2 It may be less than.
[0177] The halogen ions may include chloride ions.
[0178] The nitrogen-based ion content on the entire surface of the blank mask 100 according to the embodiment is 3 ng / cm 2The nitrogen-based ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 2.5 ng / cm 2 The nitrogen-based ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 2 ng / cm 2 The nitrogen-based ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 1.8 ng / cm 2 The nitrogen-based ion content on the entire surface of the blank mask 100 according to the embodiment may be less than 1.5 ng / cm 2 It may be less than.
[0179] The nitrogen-based ions may include nitrite ions, nitrate ions, and ammonia ions.
[0180] The content of sulfur-based ions on the entire surface of the blank mask 100 according to the embodiment is about 0.2 ng / cm 2 The content of sulfur-based ions on the entire surface of the blank mask 100 according to the embodiment may be about 0.17 ng / cm 2 The content of sulfur-based ions on the entire surface of the blank mask 100 according to the embodiment may be about 0.1 ng / cm 2 The content of sulfur-based ions on the entire surface of the blank mask 100 according to the embodiment may be about 0.07 ng / cm 2 It may be less than.
[0181] The sulfur-based ions may include sulfate ions.
[0182] In addition, the acetate content on the entire surface of the blank mask 100 according to the embodiment is 0.02 ng / cm 2 The content of oxalic acid on the entire surface of the blank mask 100 according to the embodiment may be less than 0.02 ng / cm 2 The sodium content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.02 ng / cm 2The potassium content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.02 ng / cm 2 The magnesium content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.02 ng / cm 2 The calcium content on the entire surface of the blank mask 100 according to the embodiment may be less than 0.02 ng / cm 2 It may be less than.
[0183] As described above, the blank mask 100 according to the embodiment has a low surface ion concentration, which makes it possible to suppress defects and provide a photomask of improved quality.
[0184] The surface ion concentration of the blank mask 100 according to the embodiment can be measured by ion chromatography. The blank mask 100 according to the embodiment is immersed in deionized water for a sufficient time to dissolve ions, and the content of the dissolved ions can be measured.
[0185] In the blank mask 100 according to the embodiment, the thickness change of the light-shielding film 20 measured by the following measurement method may be less than about 2 nm.
[0186] [Measurement method] The light-shielding film 20 is immersed in carbonated water having a carbon dioxide concentration of about 2000 mg / l for about 10 minutes, and the thickness change of the light-shielding film 20 is the difference between the thickness of the light-shielding film 20 before and after immersion.
[0187] The thickness change may be less than about 20 nm. The thickness change may be less than about 15 nm. The thickness change may be less than about 10 nm. The thickness change may be less than about 7 nm. The thickness change may be less than about 5 nm. The thickness change may be less than about 4 nm. The thickness change may be less than about 3 nm. The thickness change may be less than about 2.5 nm. The thickness change may be less than about 2 nm. The thickness change may be less than about 1.55 nm.
[0188] The thickness change may be from about 0.1 nm to about 10 nm. The thickness change may be from about 0.1 nm to about 7 nm. The thickness change may be from about 0.1 nm to about 5 nm. The thickness change may be from about 0.1 nm to about 4 nm. The thickness change may be from about 0.1 nm to about 3 nm. The thickness change may be from about 0.1 nm to about 2.5 nm. The thickness change may be from about 0.1 nm to about 2 nm. The thickness change may be from about 0.1 nm to about 1.55 nm.
[0189] The thickness change may be from 0.3 nm to 3 nm, or from 0.1 nm to 1 nm.
[0190] The thickness change may be from about 3 nm to about 15 nm.The thickness change may be from about 3 nm to about 8 nm.The thickness change may be from about 7 nm to about 15 nm.
[0191] The thickness change may be a thickness change of the second light-shielding layer 22 .
[0192] Moreover, the blank mask 100 according to the embodiment may have a transmittance change. The transmittance change can be derived by the measurement method. The transmittance change is the difference between the transmittance of the light-shielding film 20 before the immersion and the transmittance of the light-shielding film 20 after the immersion.
[0193] The transmission change may be less than about 0.3%. The transmission change may be less than about 0.2%. The transmission change may be less than about 0.1%. The transmission change may be less than about 0.05%. The minimum transmission change may be about 0.00001%.
[0194] The transmittance change may be from about 0.003% to about 0.02%.
[0195] Moreover, the blank mask 100 according to the embodiment may have an optical density variation, which can be derived by the measurement method.
[0196] The optical density change may be less than 0.1. The optical density change may be less than 0.08. The optical density change may be less than 0.07. The optical density change may be less than 0.05. The optical density change may be less than 0.03. The optical density change may be less than 0.02. The minimum optical density change may be about 0.0001.
[0197] The change in optical density may be between 0.01 and 0.07.The change in optical density may be between 0.01 and 0.04.The change in optical density may be between 0.03 and 0.07.
[0198] Moreover, the blank mask 100 according to the embodiment may have a reflectance change, which can be derived by the measurement method.
[0199] The reflectance change may be less than about 0.3%. The reflectance change may be less than about 0.2%. The reflectance change may be less than about 0.1%. The reflectance change may be less than about 0.08%. The reflectance change may be less than about 0.05%. The minimum reflectance change may be about 0.0001%.
[0200] As described above, the blank mask 100 according to the embodiment has low changes in thickness, transmittance, optical density, and reflectance after immersion in carbonated water, and thus the blank mask 100 according to the embodiment can minimize changes in optical properties during a cleaning process in the photomask manufacturing process.
[0201] The method for manufacturing a semiconductor device according to the embodiment includes a preparation step of arranging a light source, a photomask 200, and a semiconductor wafer coated with a resist film, an exposure step of selectively transmitting and emitting light incident from the light source through the photomask 200 onto the semiconductor wafer, and a development step of developing a pattern on the semiconductor wafer.
[0202] The photomask 200 includes a light-transmitting substrate 10 and a light-shielding pattern film 35 disposed on the light-transmitting substrate 10 .
[0203] The light-shielding pattern film 25 contains at least one of a transition metal, oxygen, nitrogen, and carbon.
[0204] In the preparation step, the light source is a device capable of generating short-wavelength exposure light. The exposure light may be light having a wavelength of 200 nm or less. The exposure light may be ArF light having a wavelength of 193 nm.
[0205] A lens may be further disposed between the photomask 200 and the semiconductor wafer. The lens serves to reduce the shape of the circuit pattern on the photomask 200 and transfer it onto the semiconductor wafer. The lens is not limited as long as it is generally applicable to the ArF semiconductor wafer exposure process. As an example, the lens may be a lens made of calcium fluoride (CaF2).
[0206] In the exposure step, the exposure light can be selectively transmitted onto the semiconductor wafer through the photomask 200. In this case, chemical modification can occur in the portion of the resist film on which the exposure light is incident.
[0207] In the above-mentioned developing step, the semiconductor wafer after the exposure step can be treated with a developing solution to develop a pattern on the semiconductor wafer. If the applied resist film is a positive resist, the part of the resist film on which the exposure light is incident can be dissolved by the developing solution. If the applied resist film is a negative resist, the part of the resist film on which the exposure light is not incident can be dissolved by the developing solution. The resist film is formed into a resist pattern by treatment with the developing solution. A pattern can be formed on the semiconductor wafer using the resist pattern as a mask.
[0208] The description of the photomask 200 is omitted since it overlaps with the above description.
[0209] Specific examples will be described in more detail below.
[0210] Example 1 A light-transmitting substrate made of quartz, 6 inches wide, 6 inches long, and 0.25 inches thick, was placed in the chamber of a DC sputtering device. A chromium target was placed in the chamber so that the T / S distance was 200 mm and the angle between the substrate and the target was 45 degrees. The temperature of the chamber was increased to about 400°C.
[0211] Then, an atmospheric gas mixture of 21 volume percent Ar, 11 volume percent N2, 32 volume percent CO2, and 36 volume percent He was introduced into the chamber, the power applied to the sputtering target was set to 1.85 kW, the substrate rotation speed was set to 30 rpm, and a sputtering process was performed for 250 seconds to form a first light-shielding layer.
[0212] After completing the deposition of the first light-shielding layer, an atmospheric gas mixture of 57% by volume of Ar, 33% by volume of N2, and 10% by volume of CO2 was introduced into the chamber on the first light-shielding layer, the power applied to the sputtering target was set to 1.5 kW, the substrate rotation speed was set to 30 rpm, and a sputtering process was performed for 45 seconds to produce a blank mask specimen on which a second light-shielding layer was deposited.
[0213] The specimen on which the second light-shielding layer was formed was placed in a heat treatment chamber, and a heater temperature was set to about 300° C., and heat treatment was performed for about 15 minutes.
[0214] A cooling plate with a cooling temperature of 23°C was installed on the substrate side of the heat-treated specimen. Then, a cooling gas was injected through a nozzle at a flow rate of 50 sccm to perform a cooling process for 5 minutes. Helium was used as the cooling gas.
[0215] Then, a vacuum ultraviolet ray having a wavelength band of about 185 nm is applied to the upper surface of the light-shielding film at about 40 mW / cm 2 The irradiation was performed in a chamber to which a vacuum pressure was applied for about 1 minute at an intensity of 100 nm.
[0216] After that, carbonated water (carbonate concentration: 2000 mg / l) was poured onto the light-shielding film that had been subjected to the ultraviolet ray process. At the same time, the vacuum ultraviolet ray was also irradiated onto the light-shielding film under the same conditions as above. The rinsing process using the carbonated water was carried out for about 1 minute.
[0217] Thereafter, a cleaning solution of about 1:1 mixture of carbonated water and hydrogen water (hydrogen concentration, 1.6 mg / l) was flowed onto the light-shielding film for about 30 seconds to perform a surface cleaning process.
[0218] The blank mask according to the embodiment was then dried.
[0219] Examples 2 to 4 and Comparative Example 1 The film forming conditions and cleaning conditions for the second light-shielding layer were as shown in the following Tables 1 and 2, and the other steps were the same as those in Example 1. The ozone concentration in the ozone water was about 200 mg / l.
[0220] Examples 5 to 8 A light-transmitting substrate made of quartz, 6 inches wide, 6 inches long, and 0.25 inches thick, was placed in the chamber of a DC sputtering device. A chromium target was placed in the chamber so that the T / S distance was 200 mm and the angle between the substrate and the target was 45 degrees. The temperature of the chamber was increased to about 400°C.
[0221] Then, an atmospheric gas mixture of 57% by volume of Ar and 43% by volume of N2 was introduced into the chamber, the power applied to the sputtering target was set to 1.35 kW, the substrate rotation speed was set to 30 rpm, and the sputtering process was carried out for 430 seconds to form a first light-shielding layer.
[0222] After completing the deposition of the first light-shielding layer, an atmospheric gas mixture of 15 volume % Ar, 72 volume % N2, and 13 volume % O2 was introduced into the chamber on the first light-shielding layer, the power applied to the sputtering target was set to 1.85 kW, the substrate rotation speed was set to 30 rpm, and a sputtering process was performed for 210 seconds to produce a blank mask specimen on which a second light-shielding layer was deposited.
[0223] After the light-shielding layer was formed, the heat treatment step, cooling step, and cleaning step were performed in the same manner as in Example 1.
[0224] In Examples 6 to 8, the deposition conditions and cleaning conditions for the second light-shielding layer were as shown in Tables 1 and 2 below, and other steps were performed as in Example 5. In Examples 7 and 8, helium gas was applied at approximately 34 volume % and approximately 32 volume %, respectively.
[0225] Example 9 A light-transmitting substrate made of quartz, 6 inches wide, 6 inches long, and 0.25 inches thick, was placed in the chamber of a DC sputtering device. A chromium target was placed in the chamber so that the T / S distance was 200 mm and the angle between the substrate and the target was 45 degrees. The temperature of the chamber was increased to about 400°C.
[0226] The chamber was filled with argon gas and nitrogen gas in a volume ratio of about 15:35. Then, a one-stage sputtering process was carried out for about 30 seconds at a power of about 1.4 kW while maintaining the ratio of argon gas and nitrogen gas inside the chamber.
[0227] Thereafter, the sputtering power was increased from about 1.4 kW to about 1.8 kW, and a two-stage sputtering process was performed for about 80 seconds while argon gas, nitrogen gas, and carbon dioxide were flowed into the chamber in a volume ratio of 2:2:1.
[0228] Then, three sputtering steps were performed for about 100 seconds. In the three sputtering steps, the volume ratios of the gases introduced into the chamber were adjusted so that the volume ratio of the argon gas, helium gas, nitrogen gas, oxygen gas, and carbon dioxide in the chamber gradually changed from about 2:2:0:0:1 to about 2:2:4:4:1. During the three sputtering steps, the sputtering power was continuously lowered from about 1.8 kW to about 1.4 kW.
[0229] Then, four sputtering steps were performed for about 60 seconds. During the four sputtering steps, the sputtering power was maintained at about 1.4 kW. In addition, in the four sputtering steps, the volume ratio of the gases introduced into the chamber was adjusted so that the volume ratio of the argon gas, helium gas, nitrogen gas, oxygen gas, and carbon dioxide in the chamber gradually changed from about 2:2:4:4:1 to 2:2:2:5:1.
[0230] After the light-shielding layer was formed, the heat treatment step, cooling step, and cleaning step were performed in the same manner as in Example 1.
[0231] [Table 1]
[0232] [Table 2]
[0233] Evaluation example 1. Surface ion concentration The blank masks manufactured in the examples and comparative examples were placed in a clean bag, and about 100 ml of deionized water was poured into the clean bag. Then, the clean bag containing the blank masks manufactured in the examples and comparative examples was left at a temperature of about 90° C. for about 120 minutes. Then, the concentration of ions dissolved from the blank masks manufactured in the examples and comparative examples was analyzed using an ion chromatography device (Dionex ICS-2100 from Thermo Scientific), and the concentration of the dissolved ions relative to the surface area of the blank mask was shown in Table 3 below. Fluorine, acetate, formate, oxalate, sodium, potassium, magnesium, and calcium were not detected.
[0234] 2. Measurement of thickness change, transmittance change, optical density change, and reflectance change The thickness change, the transmittance change, the optical density change, and the reflectance change of the light-shielding film before and after cleaning were measured and are shown in Table 4 below.
[0235] The blank masks manufactured in the examples and comparative examples were immersed in carbonated water having a carbon dioxide concentration of about 2000 mg / l for about 10 minutes.
[0236] The thickness change, transmittance change, optical density change, and reflectance change of the light-shielding film before and after the immersion were measured and are shown in Table 5 below.
[0237] The thickness, transmittance, optical density, and reflectance of the light-shielding film were measured at 23 points and derived as average values.
[0238] The thickness, transmittance, optical density and reflectance of the light-shielding film are measured by Nanoview's MG-PRO.
[0239] The transmittance and reflectance are measured for light in the wavelength range of about 193 nm.
[0240] 3. Composition of the light-shielding layer The composition of the light-shielding layer is measured by X-ray Photolectron Spectroscopy (XPS).
[0241] The blank masks manufactured in the examples and comparative examples were processed to a size of 15 mm in width and 15 mm in length to prepare specimens. The specimens were then placed in a Thermo Scientific K-Alpha model, and an area of 4 mm in width and 2 mm in length located in the center of the specimen was etched with argon gas. The degree of vacuum in the measurement equipment during each layer etching time was 1.0×10 -8 The pressure was 700 nm, the X-ray source was a Monochromator Al Kα (1486.6 eV), the anode power was 72 W, the anode voltage was 12 kV, and the voltage of the argon ion beam was 1 kV.
[0242] The composition of the second light-shielding layer during the etching time from about 30 seconds to about 80 seconds was measured using the above measuring equipment as shown in Table 6 below.
[0243] In addition, the light-shielding film in Example 9 was etched for a period of time ranging from about 30 seconds to about 84 seconds, and the composition of the upper portion of the light-shielding layer was measured using the above-mentioned measuring equipment as shown in Table 7 below.
[0244] [Table 3]
[0245] [Table 4]
[0246] [Table 5]
[0247] [Table 6]
[0248] [Table 7]
[0249] As shown in Tables 3 to 7, the blank masks according to the examples have a low surface ion concentration, and have low thickness variation, transmittance variation, optical density variation, and reflectance variation. [Explanation of symbols]
[0250] 100 Blank Mask 10 Light-transparent substrate 20 Light-shielding film 21 1st light shielding layer 22 Second light shielding layer 25 Light-shielding pattern film 30 Phase inversion film 200 Photomasks
Claims
1. forming a light-shielding film on a light-transmitting substrate; cleaning the light-shielding film with a cleaning solution; Including, The thickness change of the light-shielding film during the cleaning step is less than 15 nm. A method for manufacturing a blank mask.
2. The method further includes forming a phase shift film on the light-transmitting substrate, The light-shielding film is formed on the phase shift film. A method for producing the blank mask according to claim 1 .
3. The halogen ion content on the entire surface is 0.1 ng / cm 2 The nitrogen-based ion content is less than 3 ng / cm 2 The sulfur-based ion content is less than 0.1 ng / cm 2 is less than A method for producing the blank mask according to claim 1 .
4. The halogen ions include chloride ions, the nitrogen ions include nitrite ions, nitrate ions, and ammonia ions, and the sulfur ions include sulfate ions. The method for producing the blank mask according to claim 3 .
5. The cleaning solution includes carbonated water. A method for producing the blank mask according to claim 1 .
6. The change in transmittance of the light-shielding film during the cleaning step is less than 0.05%. The method for producing the blank mask according to claim 5 .
7. The change in optical density of the light-shielding film during the cleaning step is less than 0.
07. The method for producing the blank mask according to claim 6 .
8. The change in reflectance of the light-shielding film during the cleaning step is less than 0.5%. The method for producing the blank mask according to claim 7 .
9. The thickness change of the light-shielding film in the cleaning step is 0.3 nm to 3 nm. A method for producing the blank mask according to claim 1 .
10. The light-shielding film is A first light-shielding layer disposed on the light-transmitting substrate; A second light-shielding layer disposed on the first light-shielding layer; Including, The second light-shielding layer includes a nitrogen element having a content of 20 atom% to 40 atom%, a chromium element having a content of 30 atom% to 50 atom%, and an oxygen element having a content of 20 atom% to 40 atom%, The method for producing the blank mask according to claim 9 .
11. The first light-shielding layer includes a nitrogen element having a content of 10 atom% to 30 atom%, a chromium element having a content of 60 atom% to 90 atom%, and an oxygen element having a content of 0.5 atom% to 10 atom%, The method for producing the blank mask according to claim 10 .
12. The second light-shielding layer contains carbon element in an amount of less than 5 atom %. The method for producing the blank mask according to claim 10 .
13. A light-transmitting substrate; a light-shielding film disposed on the light-transmitting substrate; Including, The halogen ion content on the entire surface is 0.05 ng / cm 2 The nitrogen-based ion content is less than 2 ng / cm 2 The sulfur-based ion content is less than 0.1 ng / cm 2 is less than Blank mask.
14. The thickness change of the light-shielding film measured by the following measurement method is less than 15 nm. The blank mask of claim 13. [Measurement method] The light-shielding film was immersed in carbonated water having a carbon dioxide concentration of 2000 mg / l for 10 minutes, and the thickness change of the light-shielding film was the difference between the thickness of the light-shielding film before immersion and the thickness of the light-shielding film after immersion.
Citation Information
Patent Citations
Blank mask and photo mask using the blank mask
JP2017027006A
Reflective photomask blank and reflective photomask
JP2022185356A
Method of cleaning substrate for blank mask, substrate for blank mask, and blank mask including the same
JP2023029232A
Preparation method of laminate and laminate for optical use
KR102495224B1
Method for manufacturing photomask blank and photomask blank and photomask
KR1020120057488A