Optical member and lens unit
The method of using a silicate monomer and oligomer in a specific ratio forms a functional film with enhanced hardness and hydrophilicity, addressing the hardness issues of existing films and maintaining optical performance.
Patent Information
- Application Number
- JP2024115072
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-06-30
AI Technical Summary
Existing functional films formed using inorganic hydrophilic coating liquids lack sufficient hardness, leading to susceptibility to scratches when wiped to remove dirt.
A method for manufacturing an optical member with a functional film that includes a coating liquid containing a silicate monomer and a silicate oligomer, with a specific ratio of silicate oligomer between 3.5 mol% and 28.0 mol%, enhancing both hydrophilicity and hardness.
The functional film achieves excellent hydrophilicity and hardness, resisting scratches during wiping, thus maintaining optical performance by preventing water droplet formation and improving durability.
Smart Images

Figure 2024153699000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an optical member and an optical member. [Background technology]
[0002] The optical member includes, for example, a light-transmitting member and a functional film that covers the surface of the light-transmitting member. The functional film has, for example, hydrophilic properties.
[0003] An inorganic hydrophilic coating liquid is known that contains (a) an aqueous solution containing an amorphous silicate compound obtained by hydrolyzing and condensing a tetrafunctional silicon compound having a purity of 99.0% by mass or more in an aqueous medium at room temperature or higher and 170° C. or lower in the presence of a basic compound, (b) water, and (c) optionally 30% by mass or less of an alcohol, a ketone, a surfactant, or a combination of two or more of these (for example, Patent Document 1). This inorganic hydrophilic coating liquid has a concentration of solids derived from the aqueous solution containing the amorphous silicate compound of 0.01% by mass or more and 2.0% by mass or less. This inorganic hydrophilic coating liquid has a pH of 5 to 8. This inorganic hydrophilic coating liquid can be used to form the above-mentioned functional film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2013 / 001975 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the functional film formed from the inorganic hydrophilic coating liquid described in Patent Document 1 tends to have insufficient hardness.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide an optical member provided with a functional film that is excellent in hydrophilicity and hardness. [Means for solving the problem]
[0007] An exemplary method for manufacturing an optical member according to the present invention is a method for manufacturing an optical member including a light-transmitting member and a functional film covering the light-transmitting member, and includes a functional film forming step of forming the functional film by applying a coating liquid for forming a functional film to the light-transmitting member. The coating liquid for forming a functional film contains photocatalyst particles, a binder raw material, and a solvent. The binder raw material contains a silicate monomer and a silicate oligomer. The ratio of the amount of substance of the silicate oligomer to the total amount of substance of the silicate monomer and the silicate oligomer is 3.5 mol% or more and 28.0 mol% or less.
[0008] An exemplary optical member of the present invention is formed by the above-described method for manufacturing an optical member. Effect of the Invention
[0009] Illustratively, the present invention can provide an optical member having a functional film that is excellent in hydrophilicity and hardness. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram of an optical member formed by an example of a method for producing an optical member according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of an optical member formed by Variation 1 of the method for producing an optical member according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a graph showing the relationship between the proportion (α) of silicate oligomer and the contact angle for the functional films formed in the examples. [Figure 4] FIG. 4 is a graph showing the relationship between the silicate oligomer ratio (α) and the indentation hardness for the functional films formed in the examples. [Diagram 5] FIG. 5 is a graph showing the relationship between the proportion (α) of silicate oligomer and the gel fraction for the sample films formed in the examples. [Figure 6]FIG. 6 is a photograph showing the results of the wiping test carried out in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and the description will not be repeated. The dimensions of each member in the drawings are not necessarily the same as the dimensions of the actual member.
[0012] In this specification, "thickness" means average thickness. "Anti-reflection film thickness" is measured by a scanning electron microscope (e.g., "JSM-7900F" manufactured by JEOL Ltd.). "Functional film thickness" is measured by a contact type film thickness meter (e.g., "DekTakXT-S" manufactured by Bruker).
[0013] <Method of manufacturing optical members> The method for manufacturing an optical member according to a first embodiment of the present invention is a method for manufacturing an optical member including a light-transmitting member and a functional film covering the light-transmitting member, and includes a functional film forming step of forming a functional film by applying a functional film forming coating liquid to the light-transmitting member. The functional film forming coating liquid contains photocatalyst particles, a binder raw material, and a solvent. The binder raw material contains a silicate monomer and a silicate oligomer. The ratio of the substance amount of the silicate oligomer to the total substance amount of the silicate monomer and the silicate oligomer (hereinafter, sometimes referred to as the silicate oligomer ratio (α)) is 3.5 mol% or more and 28.0 mol% or less.
[0014] The optical member formed by the manufacturing method for an optical member according to this embodiment is suitable as an optical member for use in, for example, an optical unit including one or more optical members (particularly, an optical unit used outdoors). The above-mentioned optical member is particularly suitable as an optical member (hereinafter, sometimes referred to as a first optical member) located closest to the object among one or more lenses included in the optical unit. When used as a first optical member, the above-mentioned optical member is usually used with the surface on the functional film side facing the object side. Specifically, the above-mentioned optical member is suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle.
[0015] The optical member includes a functional film. The functional film is a hydrophilic film having photocatalytic activity. Even if water adheres to the functional film of the optical member, the adhered water spreads thinly on the functional film, so that water droplets are unlikely to form. Therefore, the optical member can suppress the deterioration of optical performance due to the adhesion of water droplets. Here, the known functional film is formed, for example, using a known functional film forming coating liquid containing photocatalyst particles and a silicate oligomer. The known functional film formed by the known functional film forming coating liquid contains photocatalyst particles and a binder. The binder contains a silicate cured product. Both the photocatalyst particles and the silicate cured product have excellent hydrophilicity. The known functional film can exhibit excellent hydrophilicity by containing the photocatalyst particles and the silicate cured product. On the other hand, the known functional film tends to have insufficient hardness. Therefore, the known functional film tends to be easily scratched when the surface is wiped to remove dirt (e.g., mud and dust) attached to the surface.
[0016] The present inventors have found that a functional film having excellent hardness can be formed by using a functional film-forming coating liquid containing a silicate monomer and a silicate oligomer and having a certain or higher ratio (α) of the silicate oligomer. This phenomenon is believed to be due to the fact that the addition of both the silicate monomer and the silicate oligomer to the functional film-forming coating liquid allows the silicate to be cured (for example, hydrolysis and condensation) efficiently. On the other hand, the present inventors have found that when the ratio (α) of the silicate oligomer in the functional film-forming coating liquid is set to a certain level or higher, the hydrophilicity of the formed functional film is reduced. This phenomenon is believed to occur for the following reasons. First, in the formation of the functional film, the silicate monomer and silicate oligomer contained in the functional film-forming coating liquid are not completely cured and remain partially unreacted. Therefore, when the ratio (α) of the silicate oligomer in the functional film-forming coating liquid is increased, the amount of silicate oligomer remaining in the functional film also increases. Here, the silicate oligomer has a lower hydrophilicity than the silicate monomer. Thus, the functional film formed by the functional film forming coating liquid having a certain or higher ratio (α) of the silicate oligomer contains a relatively large amount of the silicate oligomer, and therefore has a low hydrophilicity. The present invention is based on the above findings. That is, in the manufacturing method of the optical member according to the present embodiment, a functional film forming coating liquid containing a silicate monomer and a silicate oligomer and having a ratio (α) of the silicate oligomer of 3.5 mol % or more is used, so that a functional film having excellent hardness can be formed. In addition, in the manufacturing method of the optical member according to the present embodiment, the functional film forming coating liquid has a ratio (α) of the silicate oligomer of 28.0 mol % or less, so that a functional film having excellent hydrophilicity can be formed. This functional film has excellent hardness, so that it is difficult to cause scratches even when the surface is wiped (excellent wipe resistance).
[0017] The method for producing an optical member according to this embodiment will be further described below with reference to the drawings. Fig. 1 is a schematic diagram of an optical member 1 formed by an example of the method for producing an optical member according to this embodiment. The optical member 1 includes a light-transmitting member 2 and a functional film 3 that covers the light-transmitting member 2.
[0018] [Translucent member] The light-transmitting member 2 has a base material 2a and an anti-reflection film 2b that covers the base material 2a. However, as shown in Modification 1 described later, the light-transmitting member of the optical member formed by the manufacturing method for an optical member according to this embodiment may be composed of a single member. The light-transmitting member 2 has light-transmitting properties. In other words, the light-transmitting member 2 transmits light. The light-transmitting member 2 may be transparent or translucent.
[0019] The shape of the light-transmitting member 2 is, for example, lenticular. When the shape of the light-transmitting member 2 is lenticular, the surface of the light-transmitting member 2 on the anti-reflection film 2b side is, for example, convex. When the shape of the light-transmitting member 2 is lenticular, the radius of curvature of the lens surface of the light-transmitting member 2 is preferably 10 mm or more and 15 mm or less. When the radius of curvature of the light-transmitting member 2 is less than 10 mm, it tends to be difficult to adjust the thickness of the functional film 3. When the radius of curvature of the light-transmitting member 2 is more than 15 mm, it tends to be difficult to provide the optical member 1 with a desired angle of view.
[0020] (base material) The substrate 2a contains, for example, glass or resin as a main component.
[0021] (Anti-reflective film) The anti-reflection film 2b suppresses reflection of light. Specifically, the optical member 1 includes the anti-reflection film 2b, thereby suppressing reflection of light that attempts to enter the light-transmitting member 2 from the functional film 3 at the light-transmitting member 2.
[0022] The anti-reflection film 2b may have a single layer structure or a multi-layer structure. The anti-reflection film 2b contains, for example, a metal or a metal oxide. The anti-reflection film 2b is, for example, a vapor deposition film or a sputtering film.
[0023] The thickness of the antireflection film 2b is preferably 200 nm or more and 400 nm or less. If the thickness of the antireflection film 2b is less than 200 nm, a sufficient antireflection effect tends not to be obtained. If the thickness of the antireflection film 2b is more than 400 nm, the productivity of the optical member 1 tends to decrease.
[0024] [Functional membrane] The functional film 3 covers the surface of the light-transmitting member 2 on the antireflection film 2b side. The functional film 3 contains photocatalytic particles and a binder. The functional film 3 has photocatalytic activity. Specifically, the functional film 3 has hydrophilicity. The static contact angle of the functional film 3 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and even more preferably 10.0° or less.
[0025] The thickness of the functional film 3 is preferably 15 nm or more and 200 nm or less, and more preferably 20 nm or more and 180 nm or less. When the thickness of the functional film 3 is 15 nm or more, the hardness of the functional film 3 is further improved. When the thickness of the functional film 3 is 200 nm or less, the optical characteristics of the optical component 1 are improved.
[0026] (Photocatalyst particles) The photocatalyst particles include photocatalyst primary particles containing a photocatalyst. The photocatalyst particles may include photocatalyst secondary particles constituted by the photocatalyst primary particles. The photocatalyst particles may further contain components other than the photocatalyst as long as they contain a photocatalyst. Examples of the components other than the photocatalyst include components having an electron capture effect. Examples of the components having an electron capture effect include gold, silver, copper, platinum, palladium, iron, nickel, cobalt, zinc, and copper oxide. The content ratio of the photocatalyst in the photocatalyst particles is preferably 90% by mass or more, more preferably 99% by mass or more, and even more preferably 100% by mass.
[0027] Examples of photocatalysts contained in the photocatalyst particles include titanium oxide, strontium titanate, zinc oxide, silicon carbide, gallium phosphate, cadmium sulfide, cadmium selenide, and molybdenum trisulfide. The photocatalyst particles preferably contain titanium oxide. When the photocatalyst particles contain titanium oxide, the photocatalytic activity of the functional film 3 is further improved.
[0028] Examples of titanium oxide include anatase type titanium oxide, rutile type titanium oxide, and brookite type titanium oxide. From the viewpoint of photocatalytic activity, anatase type titanium oxide is preferable.
[0029] The average particle size of the photocatalyst particles is preferably 1 nm to 20 nm, more preferably 5 nm to 15 nm. When the average particle size of the photocatalyst particles is 1 nm to 20 nm, the light transmittance of the optical member 1 is improved.
[0030] (Binder) The binder contains a silicate cured material, which is produced by a curing reaction (for example, a hydrolysis condensation reaction) of a silicate monomer and a silicate oligomer.
[0031] [Method of manufacturing optical components] A method for manufacturing the optical member 1 will be described. The method for manufacturing the optical member 1 includes an anti-reflection film forming step of obtaining a light-transmitting member 2 by forming an anti-reflection film 2b on a base material 2a, and a functional film forming step of forming a functional film 3 by applying a functional film forming coating liquid to the light-transmitting member 2 (specifically, on the surface on the anti-reflection film 2b side). However, a commercially available light-transmitting member 2 may be used in the method for manufacturing the optical member 1. In this case, the anti-reflection film forming step may be omitted.
[0032] [Anti-reflection film formation process] In this step, the method for forming the anti-reflection film 2b is not particularly limited, and any known anti-reflection film forming method (for example, sputtering method and vapor deposition method) can be used.
[0033] [Functional film formation process] The functional film forming coating liquid used in this step contains photocatalyst particles, a binder raw material, and a solvent. The functional film forming coating liquid may further contain other components. The binder raw material contains a silicate monomer and a silicate oligomer.
[0034] The binder raw material may contain only the silicate monomer and the silicate oligomer, or may contain other components (e.g., silica). The total content of the silicate monomer and the silicate oligomer in the binder is preferably 80% by mass or more, more preferably 99% by mass or more, and even more preferably 100% by mass.
[0035] The silicate monomer is a silicate compound that does not have a siloxane bond (Si-O-Si) in the molecule. The silicate oligomer is a silicate compound that has one or more (e.g., 2 to 6) siloxane bonds in the molecule.
[0036] The molecular weight of the silicate monomer is preferably 120 or more and 210 or less. By setting the molecular weight of the silicate monomer to 120 or more and 210 or less, the hardness of the functional film 3 is further improved. In addition, the molecular weight of the silicate oligomer is preferably 200 or more and 1000 or less, and more preferably 600 or more and 850 or less. By setting the molecular weight of the silicate oligomer to 200 or more and 1000 or less, the hardness of the functional film 3 is further improved. In addition, when the binder contains multiple silicate monomers, the molecular weight of the silicate monomer means the number average molecular weight. Similarly, when the binder contains multiple silicate oligomers, the molecular weight of the silicate oligomer means the number average molecular weight.
[0037] The silicate monomer preferably contains a compound represented by the following general formula (1) (hereinafter, may be referred to as compound (1)). The silicate oligomer preferably contains a compound represented by the following general formula (2) (hereinafter, may be referred to as compound (2)). When the silicate monomer contains compound (1) and the silicate oligomer contains compound (2), the hardness and hydrophilicity of the functional film 3 are further improved. Si(OR1)n(OH)(4-n) (1) SimO(m-1)(OR2)(2m+2) (2)
[0038] In general formula (1), R1 represents an organic group having 1 to 8 carbon atoms. n represents an integer of 1 to 4. In general formula (2), R2 represents an alkyl group having 1 to 4 carbon atoms. m represents an integer of 2 to 6.
[0039] In the general formula (1), when n is an integer of 2 or more, multiple R1 may be the same or different, but preferably are the same. In the general formula (2), multiple R2 may be the same or different, but preferably are the same. Hereinafter, the details of compound (1) and compound (2) will be described.
[0040] (Compound (1)) In the general formula (1), examples of the organic group having 1 to 8 carbon atoms represented by R1 include an alkyl group having 1 to 4 carbon atoms and an alkoxysilyl group having 1 to 8 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group. Examples of the alkoxysilyl group having 1 to 8 carbon atoms include a trimethoxysilyl group and a triethoxysilyl group. Examples of the organic group having 1 to 8 carbon atoms represented by R1 include an alkyl group having 1 to 4 carbon atoms, and a methyl group or an ethyl group is more preferable.
[0041] The compound (1) is preferably a compound represented by the following general formula (1') (hereinafter, sometimes referred to as an ethyl silicate monomer): n in the following general formula (1') has the same meaning as n in the general formula (1). Si(OC2H5)n(OH)(4-n)···(1')
[0042] The silicate monomer may contain a mixture of two or more kinds of compound (1). In this case, in the mixture of compounds (1), the average value of n in general formula (1) is preferably 2.0 or more and 4.0 or less, more preferably 3.0 or more and 4.0 or less.
[0043] The calculation method of the average value of n in general formula (1) will be explained with an example. It is assumed that the mixture of compounds (1) contains equimolar amounts of compound (1) in general formula (1) where n is 1, compound (1) where n is 2, compound (1) where n is 3, and compound (1) where n is 4. In this case, the mixture of compounds (1) has an average value of n in general formula (1) of 2.5.
[0044] (Compound (2)) In the general formula (2), examples of the alkyl group having 1 to 4 carbon atoms represented by R2 include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group. The alkyl group having 1 to 4 carbon atoms represented by R2 is preferably a methyl group or an ethyl group.
[0045] The compound (2) is preferably a compound represented by the following general formula (2') (hereinafter, sometimes referred to as ethylsilicate oligomer): m in the following general formula (2') has the same meaning as m in the general formula (2). SimO(m-1)(OC2H5)(2m+2)...(2')
[0046] The silicate oligomer may contain a mixture of two or more kinds of compound (2). In this case, in the mixture of compounds (2), the average value of m in the general formula (2) is preferably 4.0 or more and 6.0 or less, more preferably 4.5 or more and 5.5 or less.
[0047] A method for calculating the average value of m in general formula (2) will be described with an example. It is assumed that a mixture of compounds (2) contains equimolar amounts of compound (2) in which m in general formula (2) is 2, compound (2) in which m is 3, compound (2) in which m is 4, compound (2) in which m is 5, and compound (2) in which m is 6. In this case, the mixture of compounds (2) has an average value of m in general formula (2) of 4.0.
[0048] The silicate oligomer ratio (α) is 3.5 mol% or more and 28.0 mol% or less, preferably 5.0 mol% or more and 28.0 mol% or less, and more preferably 10.0 mol% or more and 20.0 mol% or less. When the silicate oligomer ratio (α) is 3.5 mol% or more, the functional film 3 exhibits excellent hardness. When the silicate oligomer ratio (α) is 28.0 mol% or less, the functional film 3 exhibits excellent hydrophilicity.
[0049] The solvent of the functional film-forming coating liquid is preferably an aqueous solvent. The aqueous solvent contains water and additives added as necessary. Examples of the additives include organic acids, alcohol compounds, and ammonia. The content of the additives in the aqueous solvent is preferably more than 0% by mass and 20% by mass or less. Examples of the organic acids include formic acid, acetic acid, propionic acid, succinic acid, citric acid, and malic acid. Examples of the alcohol compounds include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, and butanol.
[0050] The coating method of the functional film-forming coating liquid is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, and a combination of these (e.g., dip spin coating). Examples of the wet process include spin coating, dip coating, and dip spin coating.
[0051] When the functional film-forming coating liquid is applied by spin coating or dip spin coating, the rotation speed is preferably 500 rpm or more and 10,000 rpm or less.
[0052] The solid content concentration of the photocatalyst particles in the functional film-forming coating liquid is preferably 1.0% by mass to 15.0% by mass, more preferably 2.0% by mass to 6.0% by mass. The solid content concentration of the binder raw material in the functional film-forming coating liquid is preferably 85.0% by mass to 99.0% by mass, more preferably 94.0% by mass to 98.0% by mass. The solid content concentration of the functional film-forming coating liquid is preferably 0.1% by mass to 10.0% by mass, more preferably 0.2% by mass to 1.0% by mass.
[0053] In this step, before applying the functional film-forming coating liquid, a surface treatment may be performed on the surface of the light-transmitting member 2 on the anti-reflection film 2b side. Examples of the surface treatment include plasma treatment, electron beam treatment, corona treatment, and flame treatment. Examples of the plasma treatment include high-frequency discharge plasma treatment and atmospheric pressure glow discharge plasma treatment. These surface treatments may be used in combination.
[0054] In this process, it is preferable to carry out a heat treatment after the application of the functional film-forming coating liquid. The heat treatment promotes the removal of volatile components in the functional film-forming coating liquid and the curing reaction. The heating conditions can be, for example, a treatment temperature of 60°C or higher and 200°C or lower, and a treatment time of 10 minutes or higher and 10 hours or lower.
[0055] <Variation 1> Next, an optical member 11 formed by an example of a manufacturing method for an optical member according to this embodiment will be described with reference to Fig. 2. The optical member 11 in Fig. 2 is a first modified example of the optical member 1 in Fig. 1. The optical member 11 includes a light-transmitting member 12 and a functional film 13 that covers the light-transmitting member 12.
[0056] The manufacturing method of the optical member 11 in Fig. 2 differs from the manufacturing method of the optical member 1 in Fig. 1 only in that the light-transmitting member 12 is a single member. Therefore, the description overlapping with the manufacturing method of the optical member 1 will be omitted. The light-transmitting member 12 is a member corresponding to the base material 2a of the optical member in Fig. 1. Since the optical member 11 does not include an anti-reflection film 2b, it can be manufactured at a lower cost than the optical member 1 in Fig. 1.
[0057] [Other variations] The method for manufacturing an optical member according to the present embodiment has been described above with reference to the drawings. However, the method for manufacturing an optical member according to the present embodiment is not limited to the method for manufacturing the optical member 1 in FIG. 1 and the method for manufacturing the optical member 11 in FIG.
[0058] The optical member formed by the optical member according to the present embodiment may further include other components in addition to the light-transmitting member and the functional film. The functional film preferably has a single-layer structure, but may have a multi-layer structure. The functional films preferably cover the entire surface of the light-transmitting member, but do not necessarily have to cover the entire surface.
[0059] <Second embodiment: Optical member> The optical member according to the second embodiment of the present invention is formed by the method for manufacturing an optical member according to the first embodiment described above. Details of the optical member formed by the method for manufacturing an optical member according to the first embodiment have been described above, so duplicated descriptions will be omitted. EXAMPLES
[0060] <Optical component manufacturing A> The optical members of Examples 1 to 4 and Comparative Examples 1 to 3 were manufactured by the following method. In manufacturing each optical member, a first coating liquid and a second coating liquid were prepared as functional film-forming coating liquids. The first coating liquid and the second coating liquid are described in detail below.
[0061] (First coating liquid) An ethyl silicate monomer ("Tetraethyl orthosilicate (TEOS)" manufactured by Tama Chemicals Co., Ltd., purity: 99.9% by mass or more), a photocatalyst dispersion liquid containing anatase-type titanium oxide particles ("Sagancoat (registered trademark) TO-85" manufactured by Japan Photocatalyst Center Co., Ltd., solid content concentration: 0.85% by mass, solvent: water), and water were mixed to the following composition to prepare a first coating liquid. The first coating liquid contained a silicate monomer (solid content equivalent concentration: 96% by mass), titanium oxide particles as photocatalyst particles (solid content equivalent concentration: 4% by mass), and a solvent (water) (solid content concentration: 0.45% by mass). The ethyl silicate monomer had an average value of n in the general formula (1) of about 4.0. The number average molecular weight of the ethyl silicate monomer contained in the first coating liquid was about 208. The average particle size of the titanium oxide particles contained in the first coating liquid was 10 nm.
[0062] (Second coating liquid) As the second coating liquid, a solution containing an ethyl silicate oligomer and a solvent ("Ethyl Silicate 40" manufactured by Colcoat Co., Ltd., solid content concentration: 0.34 mass%, solvent: ethanol) was prepared. The ethyl silicate oligomer contained in the second coating liquid was a mixture of multiple types of ethyl silicate oligomers having different values of m in general formula (2). The ethyl silicate oligomer contained in the second coating liquid had an average value of m in general formula (2) of 5.0. The number average molecular weight of the ethyl silicate oligomer contained in the second coating liquid was 745.2.
[0063] [Example 1] The optical member of Example 1 was manufactured by the following method. First, a lens ("TAFD-5G" manufactured by HOYA Corporation, composition: glass, diameter 12.9 mm) was prepared as a substrate. One surface of this lens was concave (radius of curvature 3 mm), and the other surface was convex (radius of curvature 12 mm). Next, an anti-reflection film was formed on the convex surface of the lens. The anti-reflection film included a SiO2 layer, a TiO2 layer, and a Ta2O5 layer. The total thickness of the anti-reflection film was about 300 nm. This resulted in a light-transmitting member including a substrate and an anti-reflection film. Next, a surface treatment (30 seconds) was performed on the surface of the light-transmitting member facing the anti-reflection film. As the surface treatment, a plasma treatment was performed using a plasma surface modification device.
[0064] Next, 8.1 g of the first coating liquid and 1.9 g of the second coating liquid were mixed. The resulting mixture was used as a coating liquid for forming a functional film. In the coating liquid for forming a functional film, the ratio of the amount of silicate oligomer (8.6×10-6 mol) to the total amount of silicate monomer and silicate oligomer (1.8×10-4 mol) was 4.9 mol%.
[0065] The above-mentioned functional film-forming coating solution was applied by spin coating onto the anti-reflection film of the translucent member after the plasma treatment. A spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.) was used for the spin coating. Coating conditions were a rotation speed of 8000 rpm and a rotation time of 30 seconds. After coating, a heat treatment was performed at 120°C for 30 minutes. This formed a functional film on the translucent member. As a result, an optical member of Example 1 was obtained in which a base material, an anti-reflection film, and a functional film were laminated in this order.
[0066] The thickness of the functional film of the optical member of Example 1 was measured using a contact film thickness measuring device ("DekTakXT-S" manufactured by Bruker). The thickness of the functional film of the optical member of Example 1 was 20 nm.
[0067] [Examples 2 to 4 and Comparative Examples 1 to 3] Except for the following changes, the optical members of Examples 2 to 4 and Comparative Examples 1 to 3 were manufactured by the same method as the manufacturing method of the optical member of Example 1. In the manufacture of the optical members of Examples 2 to 4 and Comparative Examples 1 to 3, in preparing the coating liquid for forming a functional film, the first coating liquid and the second coating liquid were mixed in the ratio shown in the following Table 1. In the manufacture of the optical member of Comparative Example 1, the first coating liquid was used as it is as the coating liquid for forming a functional film.
[0068] <Evaluation of hydrophilicity of functional membrane> For the optical members of Examples 1 to 4 and Comparative Examples 1 to 3, the static contact angle (hereinafter sometimes simply referred to as "contact angle") of the functional film with pure water was measured. The contact angle was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). The measurement environment was a temperature of 23°C ± 3°C and a relative humidity of 50% ± 10%. The measurement results are shown in Table 1 below. In this example, the contact angle of the functional film can be determined to be good if it is 15° or less.
[0069] FIG. 3 is a graph showing the relationship between the proportion (α) of silicate oligomer in the functional film and the contact angle for each optical member.
[0070] In Table 1 below, "First coating liquid [mass %]" and "Second coating liquid [mass %]" respectively indicate the mass proportions of the first coating liquid and the second coating liquid used in preparing the functional film-forming coating liquid. "Ratio (α) [mol %]" indicates the ratio (α) of silicate oligomer in the functional film. The same explanation applies to Tables 2 and 3 described below.
[0071] [Table 1]
[0072] As shown in Table 1 and Fig. 3, the proportion (α) of silicate oligomer in the functional film of the optical members of Comparative Example 1 and Examples 1 to 4 was 28.0 mol% or less. The contact angle of the functional film of the optical members of Comparative Example 1 and Examples 1 to 4 was good. On the other hand, the proportion (α) of silicate oligomer in the functional film of the optical members of Comparative Examples 2 and 3 exceeded 28.0 mol%. The contact angle of the functional film of the optical members of Comparative Examples 2 and 3 was not good.
[0073] <Optical component manufacturing B> The optical members of the above-mentioned Examples 1 to 4 and Comparative Examples 1 to 3 were produced again.
[0074] <Evaluation of functional film hardness> The hardness of the functional films of the optical members of Examples 1 to 4 and Comparative Examples 1 to 3 was measured. More specifically, a nanoindenter ("ENT-NEXUS" manufactured by Elionix Co., Ltd.) was used to perform a nanoindentation (ultra-microindentation hardness) test in accordance with "ISO 14577-1" on the functional film of each optical member. In the nanoindentation test, the indentation depth was 50 nm. The measured hardness of the functional film of each optical member is shown in Table 2 below. In this example, the indentation hardness of the functional film can be determined to be good if it is 1000 N / mm2 or more.
[0075] FIG. 4 is a graph showing the relationship between the proportion (α) of silicate oligomer in the functional film and the indentation hardness for each optical member.
[0076] [Table 2]
[0077] As shown in Table 2 and FIG. 4, the optical members of Examples 1 to 4 had a ratio (α) of silicate oligomer in the functional film of 3.5 mol % or more and 28.0 mol % or less. The optical members of Examples 1 to 4 had good hardness of the functional film. On the other hand, the optical member of Comparative Example 1 had a ratio (α) of silicate oligomer in the functional film of less than 3.5 mol %. The optical member of Comparative Example 1 had a poor hardness of the functional film. The optical members of Comparative Examples 2 and 3 had a ratio (α) of silicate oligomer in the functional film of more than 28.0 mol %. The optical members of Comparative Examples 2 and 3 had good hardness of the functional film, but as described above, it is determined that the contact angle of the functional film was not good.
[0078] From the above results, it is judged that when the proportion (α) of silicate oligomer in the functional film of the optical member is 3.5 mol % or more, the functional film has both good hydrophilicity and good hardness.
[0079] <Evaluation of gel fraction of binder> The relationship between the ratio (α) of silicate oligomer in the binder raw material and the hardening speed of the binder raw material was examined by the following method. First, a sample coating liquid was prepared that contained binder raw materials (silicate monomer and silicate oligomer) and did not contain photocatalyst particles. Five types of sample coating liquids with different ratios (α) of silicate oligomer were prepared as the sample coating liquid. A sample film was formed using each sample coating liquid, and the gel fraction of the binder in the formed sample film was measured. Here, it is determined that the faster the hardening speed of the binder raw material contained in the sample coating liquid, the higher the gel fraction of the binder in the formed sample film. Therefore, the gel fraction of the binder in the sample film was used as an index for estimating the hardening speed of the binder raw material contained in the sample coating liquid. Then, it was examined how the hardening speed (gel fraction) of the binder raw material changes when the ratio (α) of silicate oligomer in the binder raw material is increased or decreased. In this study, the binder raw material was cured under mild conditions in order to make it easier to estimate the curing speed of the binder raw material. The results are shown in Table 3 below.
[0080] First, an ethyl silicate monomer ("Tetraethyl orthosilicate (TEOS)" manufactured by Tama Chemicals Co., Ltd., purity: 99.9% by mass or more) and water were mixed to the following composition to prepare a first' coating liquid. The first' coating liquid contained a silicate monomer and a solvent (water) (solid concentration: 0.45% by mass).
[0081] Next, the first coating liquid' and the above-mentioned second coating liquid were mixed in the ratios shown in Table 3 below to prepare sample coating liquids A to E.
[0082] Next, the sample coating solutions A to E to be evaluated were applied by spin coating onto the plasma-treated glass substrate. A spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.) was used for the spin coating. The coating conditions were a rotation speed of 8000 rpm and a rotation time of 30 seconds. After coating, the substrate was left to stand at room temperature (23°C) for 130 hours. Thus, a sample film was formed on the glass substrate. The thickness of the sample film was measured using a contact film thickness measuring device ("DekTakXT-S" manufactured by Bruker). The thickness of the sample film was 20 nm.
[0083] Next, the mass (mass A) of the glass substrate on which the sample film was formed was measured. The value obtained by subtracting the mass of the glass substrate from mass A was defined as the "mass of the binder". Next, the glass substrate on which the sample film was formed was immersed in toluene at 23°C for 24 hours. After the immersion treatment, the glass substrate on which the sample film was formed was thoroughly washed and dried, and then its mass (mass B) was measured. The value obtained by subtracting the mass of the glass substrate from mass B was defined as the "mass of the gel content". The gel content of the binder was calculated based on the following formula: Gel fraction [mass%] = 100 × mass of gel fraction [g] / mass of binder [g]
[0084] FIG. 5 is a graph showing the relationship between the proportion (α) of silicate oligomers and the gel fraction for each sample film.
[0085] [Table 3]
[0086] As shown in Table 3 and FIG. 5, the gel fraction increased as the silicate oligomer ratio (α) was increased in the formation of the sample film. In particular, when the silicate oligomer ratio (α) was increased from 0.0 mass% to 3.9 mass%, the gel fraction increased rapidly. From the above, it is determined that the curing speed of the binder raw material can be improved by setting the silicate oligomer ratio (α) to 3.5 mass% or more. And, in the functional film forming coating liquid containing photocatalyst particles, it is determined that the curing speed of the binder raw material can be improved by setting the silicate oligomer ratio (α) to 3.5 mass% or more, as in the sample coating liquid not containing photocatalyst particles. In the above-mentioned Examples 1 to 4, it is determined that the excellent hardness of the functional film of the optical member was due to the efficient curing of the binder raw material of the functional film forming coating liquid.
[0087] The sample film is formed by curing the sample coating liquid under mild conditions. Therefore, the gel fraction of the sample film is relatively low, less than 60% by mass. On the other hand, the functional film of the optical member of each Example and Comparative Example is formed by curing the functional film-forming coating liquid at high temperature. Therefore, the gel fraction of the functional film of the optical member of each Example and Comparative Example is estimated to be close to 100% by mass.
[0088] <Evaluation of wipe resistance of functional film> The optical members of Example 3 and Comparative Example 1 described above were manufactured again. A wiping test was carried out on the functional film of each optical member. In detail, the surface of the functional film of each optical member was photographed with a laser microscope (OLS5000 manufactured by Olympus Corporation) (photographing magnification: 20 times). Next, the surface of the functional film of each optical member was lightly rubbed back and forth 10 times using a paper wiper (K-Dry (registered trademark) manufactured by Nippon Paper Crecia Co., Ltd.). After the wiping test, the surface of the functional film of each optical member was photographed with the above-mentioned laser microscope.
[0089] Figure 6 shows laser microscope photographs of the surface of the functional film of each optical component taken during the wipe test. "A1", "A2", "B1" and "B2" in Figure 6 are as follows. "A1", "A2", "B1" and "B2" in Figure 6 are all at full magnification. "S" in Figure 6 indicates scratches that occurred on the surface of the functional film. A1: Comparative Example 1 (before wiping test) A2: Comparative Example 1 (after wiping test) B1: Example 3 (before wiping test) B2: Example 3 (after wiping test)
[0090] 6, the wipe test did not cause any scratches on the surface of the functional film of the optical member of Example 3. On the other hand, the wipe test caused scratches on the surface of the functional film of the optical member of Comparative Example 1.
[0091] From the above, it is determined that when the proportion (α) of silicate oligomer in the functional film of the optical component is 3.5 mol % or more and 28.0 mol % or less, the wiping resistance of the functional film is improved. [Industrial Applicability]
[0092] The present invention is suitable for providing an optical member for a sensor or imaging device. [Explanation of symbols]
[0093] 1,11 Optical components 2,12 Translucent material 2a Base material 2b Anti-reflection coating 3,13 Functional membrane
Claims
1. A method for manufacturing an optical member including a light-transmitting member and a functional film that covers the light-transmitting member, the method comprising the steps of: a functional film forming step of forming the functional film by applying a functional film forming coating liquid to the light-transmitting member, The functional film-forming coating liquid contains photocatalyst particles, a binder raw material, and a solvent, The binder raw material includes a silicate monomer and a silicate oligomer, A method for producing an optical member, wherein a ratio of the amount of substance of the silicate oligomer to the total amount of substance of the silicate monomer and the silicate oligomer is 3.5 mol % or more and 28.0 mol % or less.
2. The silicate monomer includes a compound represented by the following general formula (1): The method for producing an optical member according to claim 1 , wherein the silicate oligomer contains a compound represented by the following general formula (2): Si(OR1)n(OH)(4-n)...(1) SimO(m-1)(OR2)(2m+2)...(2) (In the general formula (1), R represents an organic group having 1 to 8 carbon atoms, and n represents an integer of 1 to 4, In the general formula (2), R2 represents an alkyl group having 1 to 4 carbon atoms, and m represents an integer of 2 to 6.
3. The molecular weight of the silicate monomer is 120 or more and 210 or less, The method for producing an optical member according to claim 1 or 2, wherein the silicate oligomer has a molecular weight of 200 or more and 1,000 or less.
4. An optical member formed by the method for producing an optical member according to any one of claims 1 to 3.
Citation Information
Patent Citations
Polysiloxane / titanium sol photocatalytic composite film and preparation method thereof
CN104194011A
Photocatalytic hydrophilic member
JP1998315374A
Method for forming coating film, coating film produced thereby, antireflection film and photocatalytic film
JP2003327911A
Active energy ray-curable coating composition and method for forming protective film
JP2005325199A
Laminate having high barrier properties
JP2007168085A