Intravascular blood pump with corrosion-resistant permanent magnet

A composite coating with a metal layer, metal oxide layer, bifunctional linker, and poly(p-xylylene) polymer layer addresses the corrosion issue of neodymium iron boron magnets in intravascular blood pumps, enhancing their durability and performance.

JP2024153702AActive Publication Date: 2024-10-29ABIOMED EUROPE GMBH
View PDF 26 Cites 0 Cited by

Patent Information

Application Number
JP2024115481
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-11-02
Filing Date
2024-07-19
Publication Date
2024-10-29
Estimated Expiration
2037-10-25

AI Technical Summary

Technical Problem

Neodymium iron boron magnets used in intravascular blood pumps are prone to corrosion due to their interaction with atmospheric oxygen and moisture, leading to a reduction in magnetic properties and potential structural failure.

Method used

A composite coating comprising a metal layer, a metal oxide layer, a bifunctional linker layer, and a poly(p-xylylene) polymer layer is applied to the magnet surface, providing corrosion resistance while maintaining magnetic performance.

Benefits of technology

The composite coating effectively protects the magnets from corrosion, ensuring long-term reliability and performance of intravascular blood pumps by preventing coating delamination and maintaining magnetic integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153702000004
    Figure 2024153702000004
  • Figure 2024153702000005
    Figure 2024153702000005
  • Figure 2024153702000006
    Figure 2024153702000006
Patent Text Reader

Abstract

To provide a corrosion resistant permanent magnet, a method of manufacturing the corrosion resistant permanent magnet, and an intravascular blood pump including the magnet.SOLUTION: A magnet according to the present disclosure includes a magnet body, and a composite coating provided on and covering the surface of the magnet body. The composite coating includes (a) a metal layer on the magnet body, (b) optionally a metal oxide layer on the surface of the metal layer opposite the magnet body, (c) a linker layer on the top of the metal layer or the metal oxide layer, and (d) a layer formed of poly(2-chloro-p-xylylene) over the linker layer. The magnet body is a rare earth metal / iron / boron permanent magnet. The metal of the metal layer is selected from aluminum, titanium, tantalum, niobium, zirconium, and alloys thereof, and the linker forming the linker layer is alkoxysilane.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to corrosion protection for permanent magnets. In particular, the present invention relates to a protection material that provides corrosion resistance to magnets. The present invention relates to a permanent magnet having a coating and a method for producing a corrosion-resistant permanent magnet. The present invention also relates to an intravascular blood pump equipped with the corrosion-resistant permanent magnet of the present invention. While any type of permanent magnet is applicable, rare earth permanent magnets are preferred, with neodymium iron boron magnets being preferred. NdFeB permanent magnets are particularly suitable. [Background technology]

[0002] Intravascular blood pumps support the flow of blood within a patient's blood vessels. They are used, for example, to The catheter is then inserted percutaneously into the femoral artery and passed through the body's vascular system to its intended location, e.g., to the ventricle of the heart. This is derived from the following.

[0003] A blood pump typically includes a pump case having a blood inlet and a blood outlet. In order to allow blood to flow from the blood inlet to the blood outlet, a rotating shaft is rotated around the inside of the pump case. An impeller or rotor is rotatably supported within the housing, and the impeller is provided with a rotor for transporting blood. One or more blades are provided.

[0004] An exemplary blood pump is depicted in FIG. 1. FIG. 1 illustrates an exemplary intravascular blood pump 10. FIG. 1 is a schematic longitudinal cross-sectional view of a blood pump. The blood pump has a motor section 11 and a pump section 12. These are arranged coaxially one behind the other, resulting in a rod-shaped structure. The pump section is extended by a flexible suction hose (not shown). The hose has an opening at its end and / or in its side wall for the inflow of blood to the pump. The end of the blood pump 10 opposite the suction hose is connected to a catheter 14. Optionally, it can be combined with a guide wire to steer the blood pump to the desired location. I am fooled.

[0005] The exemplary intravascular blood pump shown in FIG. 1 includes a motor section 11 rigidly connected to each other. and a pump section 12. The motor section 11 has an elongated housing 20 in which The electric motor 21 is housed in the rotor and the stator. The rotor is the moving part of the electromagnetic circuit of the motor. One of the motors has an electrically conductive winding and the other has a permanent magnet. The current flowing through the windings creates an electromagnetic field that interacts with the magnetic field of the permanent magnets, causing the rotor to rotate. In the exemplary blood pump 10 of FIG. , in the usual way, with numerous circumferentially distributed windings, as well as a longitudinal magnetic return path 2 8, which is rigidly connected to the motor housing. The stator 24 is The rotor 1 is made of permanent magnets connected to the rotor shaft 25 and magnetized in the active direction. The motor shaft 25 extends the entire length of the motor housing 20. , protruding away from it. There is an impeller 34 there, which The pump has blades 32 or pump blades projecting from the tubular pump housing. The pump housing 32 rotates inside the motor housing 20. is connected to

[0006] The proximal end of the motor housing 20 has a flexible casing 24 hermetically attached thereto. catheter 14. In this disclosure, "proximal" and "distal" refer to the intravascular blood pump. The position of the catheter 14 relative to the inserting physician is shown. That is, the distal end is the impeller side. An electric cable 23 for supplying power to and controlling the electric motor 21 extends through the An additional purge fluid line 29 extends through the catheter 14. The purge fluid (schematically depicted by the thick arrows) passes through the proximal end wall 22 of the motor housing 20. The purge fluid (shown in FIG. 1) is supplied to the interior of the motor housing 20 through a purge fluid line 29, The air flows through the gap 26 between the rotor 1 and the stator 24 and reaches the end face 30 at the far end of the motor housing. The purge pressure prevents blood from entering the motor housing. To prevent this, the blood pressure is chosen to be higher than the blood pressure. The pressure of the gas fluid is between 300 and 1400 mmHg at the motor where the pressure is generated.

[0007] A good purge fluid is water with a viscosity of η = 0.75 mPa s at 37°C. ) and, in particular, fluids with a viscosity higher than 1.2 mPa s at 37 °C. A purge fluid with a certain degree of viscosity. For example, 5% to 40% glucose in water. A solution can be used for injection, although saline is also suitable.

[0008] When the impeller 34 rotates, blood (schematically depicted by white arrows) flows through the pump house. The air is sucked in through the end surface suction opening 37 of the pump housing 32 and flows axially through the inside of the pump housing 32. Through the outlet opening 38 of the pump housing 32, the blood is conveyed backward to the pump section 12. The pump part is conveyed in the reverse direction. Alternatively, the motor housing 20 may be moved in the opposite direction, in which case blood is drawn along the motor housing 20. The object is then sucked in and comes out through opening 37.

[0009] The motor shaft 25 is connected to the motor housing at the proximal end on the one hand and to the motor housing at the proximal end on the other hand. At the far end of the housing, it is mounted in radial bearings 27 and 31. Additionally, the motor shaft 25 is also axially mounted in an axial bearing 40. If a fluid pump is used to pump blood in the reverse direction as well, or only in the reverse direction, For example, the corresponding axial bearing 40 is also / only at the proximal end of the motor housing 20. The method is provided in accordance with the present invention.

[0010] The blood pumps described above are merely examples, and the present invention may also be applied to blood pumps equipped with electric motors, i.e. It is emphasized that it is also applicable to different blood pumps which require permanent magnets.

[0011] Intravascular blood pumps must meet a number of requirements. The smallest pumps currently in use are Despite its small outer diameter of approximately 4 mm, the pump is capable of delivering high flow rates through the human blood circulation. Therefore, a tiny pump must be a high-performance engine.

[0012] Additionally, implantable blood pumps are capable of dissipating blood pressure, such as the blood being pumped and the surrounding tissue. The pump must not have any detrimental effects on the biological environment. They should be biocompatible, i.e. they should not cause any damage to the human body or its components. The equipment should not contain or produce any potentially harmful substances or significant heat.

[0013] In addition, pump replacement is a burden for the patient. Considering his, and of course the economy, From economic considerations, the intravascular blood pump should have a long service life, preferably 180 days or longer. It should have a useful life.

[0014] The materials and design of the intravascular blood pump must be appropriately selected and specifically designed to meet these various requirements. The metric must be adapted to meet these requirements.

[0015] Importantly, the appropriate permanent magnet for the electric motor must be selected. In terms of efficiency and long life of the pump, the magnets must have a high magnetic field, i.e. high residual magnetic field, demagnetization It should have high resistance to magnetic fields, i.e., high coercive force, and high saturation magnetization. rare earth permanent magnets, in particular those having neodymium as the rare earth metal, and in particular neodymium ferromagnets Boron (NdFeB) permanent magnets are the magnets of choice. Other rare earth iron boron permanent magnets may also be used.

[0016] The stronger the magnet, the smaller it can be while still producing sufficient rotational force. Thus, the more powerful the magnets are, the smaller the electric motor can be. eB permanent magnets are the most powerful permanent magnets currently available. They are It appears to be ideal for use in a pump.

[0017] The magnetic properties of rare earth metal-based magnets, e.g. NdFeB magnets, depend on the specific alloy composition, microstructure, It is well known that the magnetization depends on the magnetization and manufacturing technique used. They are available as lamella-bonded magnets and as sintered magnets. Sintered magnets have the following magnetic properties: They are made by mixing raw materials, forming an alloy, and grinding them into a powder. The material is prepared by pressing and sintering it. During or after preparation, the material is magnetized. To achieve this, an external magnetic field is applied. The most well-studied magnets are Nd2Fe 14 B crystals are especially neo It is a fine crystalline sintered material in which the gymnosilicate is surrounded by a thin layer of rich material. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] US Patent Application Publication No. 2003 / 041920 Summary of the Invention [Problem to be solved by the invention]

[0019] Neodymium iron boron magnets make them particularly suitable for use in the electric motors of intravascular blood pumps. It has magnetic properties that make it suitable for use in industrial applications, but it also has serious shortcomings. Commercially available NdFeB magnets, which are made of Zn, Fe, and Boron, and in particular sintered Sintered NdFeB magnets with highly active Nd-rich phases at the grain boundaries are Magnets are always subject to corrosion. Magnets, for example, have voids, especially (but not only) at their grain boundaries. It can be corroded by atmospheric oxygen and moisture. Corrosion results in a severe loss of magnetic properties. If corrosion progresses while the magnet is in use, the performance of the blood pump in which the magnet is used may be affected. This phenomenon occurs because the neodymium iron boron magnet acts as a sponge for corrosion products. This tendency is exacerbated by the tendency of the magnet to break down and cause fine particles to fall off the magnet's surface. This can lead to the magnet eventually breaking into pieces.

[0020] Unfortunately, the tendency to corrode is a common property of all rare earth metals. Rare earth metal based permanent magnets are prone to corrosion, as discussed above for NdFeB magnets. For magnets currently available, the rule of thumb is It can be said that the stronger the magnet, the greater its tendency to corrode.

[0021] In an intravascular blood pump, the magnets are placed in a corrosive environment, i.e. between the rotor and the stator. It must operate in a flowing purging liquid (see Figure 1). The difluids are typically aqueous fluids and may be chloride-containing fluids. It is highly corrosive to rare earth metal based magnets, but also to water and oxygen dissolved in water. It also causes severe corrosion in a very short period of time, only a few hours.

[0022] Apparently, rare earth metal based magnets such as neodymium iron boron magnets for intravascular blood pumps The permanent magnets in the magnets need to be protected against corrosion.

[0023] A variety of products that protect neodymium iron boron magnets and other rare earth metal based magnets from corrosion. For example, corrosion resistance can be achieved by coating the magnet with a protective coating. This can be improved by

[0024] Typical coatings are nickel coatings and epoxy resin based coatings. For blood pumps in particular, titanium coating and parylene (Paryle However, these coatings also have drawbacks. Biocompatible metals and organic resins such as titanium and parylene, respectively, were selected. However, the metal coating must be relatively thick to provide adequate protection. As a result, there is a problem of the magnets and windings in the electric motor of the blood pump. The gap must be relatively large. A large gap is detrimental to the performance of the electric motor. A large gap requires a larger motor current and has a strong negative effect on the The motor current creates unwanted heat that can cause damage to blood and tissue.

[0025] Furthermore, organic materials such as parylene have a thermal expansion coefficient that differs significantly from that of magnets. Therefore, temperature fluctuations during use of the magnet often cause cracks and This can result in flaking and / or peeling.

[0026] Currently, biocompatible coatings for permanent magnets, e.g. neodymium iron boron magnets, None are known that meet all the requirements for use in an intravascular blood pump. Such a coating must have good corrosion resistance of its own and be thin but dense. must not develop cracks or other defects during use, and the magnets must Of course, the coating must be biocompatible and adhere reliably and intimately to the skin. and the entire magnet, or at least the magnets that are exposed to a corrosive environment during use, A portion of the magnet must be coated with a uniform thickness. Many magnets have porous surfaces and This is a particularly high requirement since the shape of the tube includes edges. Permanent magnets, such as rare earth metal based magnets, e.g. neodymium, for use in liquid pumps. Iron boron magnets are items that cannot be easily coated with a uniform thickness. It is. [Means for solving the problem]

[0027] The present invention provides a solution to the problems discussed above.

[0028] The present invention provides a method for preventing magnetic flux loss during use in an intravascular blood pump over an extended period of time. To provide a coating for a permanent magnet that reliably protects the stone from corrosion.

[0029] The subject of the present invention is a corrosion-resistant permanent magnet having the characteristics defined in independent claim 1, A method for producing a corrosion-resistant permanent magnet having the features defined in independent claim 21 and a method for producing a corrosion-resistant permanent magnet having the features defined in independent claim 30 The present invention relates to an intravascular blood pump having the following features: It is disclosed in the claims.

[0030] A magnet is considered to be corrosion-resistant within the meaning of the present invention if it passes the tests described in the experimental part. It is.

[0031] According to the invention, a strong permanent magnet completely surrounds the magnet body or the magnet is The magnet body surface exposed to the fluid when operating in an intravascular blood pump is covered with a The coating is adapted to prevent, during use in an intravascular blood pump, It provides the magnet with corrosion resistance. The preferred magnet body is a sintered alloy consisting primarily of neodymium, iron, and boron. As mentioned above, it is a magnet made of fine tetragonal magnetic Nd2Fe 14 B crystal and its crystal The NdFeB alloy has a neodymium-rich nonmagnetic phase surrounding the NdFeB alloy. 2Fe 14The B crystals have an average crystal size in the range of 1 to 80 μm. The Murich phase constitutes 1% to 50% of the magnet body by volume. These magnets are commercially They are readily available in the market because of their high magnetic properties and because they are particularly strong. Since it has a high magnetic flux density, it is preferable. For reasons explained above, applications in intravascular blood pumps require particularly powerful magnets. In principle, the corrosion resistant coating of the present invention can be applied to any object requiring protection against corrosion. It can be applied to different materials, for example, different rare earth iron boron magnetic materials or any other magnetic materials. This can be done.

[0032] The coating of the present invention is a composite material provided on the surface of the magnet body, i.e., the actual magnetic material. Composite coatings consist of a metallic layer on the surface of the magnet body, optionally and a metal oxide layer on the exposed surface of the metal layer, poly(2-chloro-p-oxy) A layer formed from poly(2-chloro-p-xylylene), and a metal layer or a metal oxide layer and a poly(2-chloro-p-xylylene) A linker layer is provided between the polymer layer and the polymerizable polymer (polymerizable polymer layer).

[0033] Rare earth metal based magnets purchased from suppliers typically have a phosphate coating. This phosphate coating is then protected by a phosphate coating prior to the application of the metal layer, e.g. However, the phosphate coating may be removed by washing with an acid. on the magnet body without detrimentally interfering with the coating or coating process. Preferably, the phosphate coating is not removed. Not removing the However, it is recommended to clean the magnet prior to application of the metal layer to avoid introducing impurities into the magnet. Cleaning is preferably carried out by washing the magnet with an organic solvent, e.g. alcohol. Particularly suitable cleaning agents are isopropanol, and a mixture of isopropanol and ethanol. After washing with organic solvents, the magnets were It is dried, for example, in a vacuum or in a stream of air.

[0034] After cleaning and drying, a metal layer is applied to the surface of the magnet body. The metal for use in the present invention is not particularly limited. The term "metal" as used herein includes metal alloys. Suitable for forming the metal layer are dense The material may be any metal (metal alloy) that is capable of forming a layer thereon and is biocompatible. The method of applying the metal layer to the substrate is not particularly limited. Dry methods such as chemical vapor deposition, in particular ion vapor deposition, plasma coating, and atomic layer deposition; as well as wet methods such as galvanic deposition (ion plating). Although plasma deposition and ion deposition are very fast and cost effective methods, wet deposition is more It is known to result in metal layers having good quality, i.e. metal layers having enhanced density. However, layers deposited by ion deposition or other dry methods have shown excellent long-term It has long-term stability.

[0035] The preferred metal for forming the metal layer is aluminum. The deposition of the compound can be carried out by methods conventional in the art, for example, by using aluminum chloride and 1-ethyl-3-methyl- This can be done without ionic liquids by using a mixture with ethyl imidazolium chloride. The aluminum is preferably pure, e.g., at least 99% pure. and particularly preferably has a purity of at least 99.9%.

[0036] Aluminum forms a protective oxide layer when exposed to air. This naturally formed The (native) oxide layer is only a few nanometers thin and is intimately connected to the underlying metal. Other metals that form a native oxide layer are also suitable. Exemplary metals are , titanium, tantalum, niobium, zirconium, and two or more of these metals The above alloys include, for example, aluminum alloys and niobium-titanium alloys. The layer forms naturally upon exposure to air by oxidation of the metal coated on the magnet body. or artificially, for example by anodization. The layers are only a few nanometers thick, for example 2 to 5 nanometers. It also works well without an oxide layer, and biocompatible metals without an oxide layer can be effectively used. Such metals and metal alloys are, for example, the noble metals, such as platinum and gold.

[0037] The thickness of the metal layers and the combined metal / metal oxide layers is preferably small, i.e., about A thickness of 20 μm or less is particularly preferred. A thickness of 10 μm or less is particularly preferred.

[0038] To enhance the corrosion protection provided by the metal layer or metal / metal oxide layer, Or a metal / metal oxide layer is combined with a poly(p-xylylene) polymer layer. The silylene polymer layer is known by the trade name Parylene. Parylene reacts with surfaces that contain hydroxyl groups. It is known that this method can form pinhole-free coatings at low layer thicknesses. In addition, they have a low dielectric constant (about 3), which is beneficial in implantable blood pumps. Composite coatings comprising a metal or metal / metal oxide layer and a parylene layer are biocompatible. However, the incorporation of parylene into metal or metal / metal oxide layers also provides corrosion protection. The adhesion of the layer is not strong enough for the operating environment of an intravascular blood pump. The parylene layer is acceptable The metal layer or metal oxide layer begins to peel off in a short time. The layer or metal / metal oxide layer cannot adequately protect the magnet body, and this causes the magnet body to The body begins to decay.

[0039] According to the present invention, this scenario is prevented by a combination of two measures: the provision of an interface layer linking the metal or metal oxide layer with the parylene layer, and The use of parylene compounds.

[0040] The compound forming the interfacial layer, ie the linker compound, must be bifunctional. Bifunctionality means that the linker compound has two types of functional groups or groups with different functionalities (reactivities). A functional group or molecular moiety is, for example, a metal layer or a metal oxide layer. By reacting with the surface hydroxyl groups of the functional layer, the functional group is bonded to the metal layer or metal oxide layer, and the functional group of the other layer is bonded to the metal layer or metal oxide layer. The groups or molecular moieties bond to the parylene, thereby forming a bond between the metal or metal oxide layer and the organic parylene. The link may be a covalent bond or other bond, such as a van der Waals bond. It can be provided by Waals forces.

[0041] A functional group or molecular moiety that bonds with a metal or metal oxide and a functional group or molecular moiety that bonds with the parylene layer Linkers having a molecular moiety are known. Exemplary linkers include silane compounds. Substances, mercaptans, phosphines (phosphorus hydroxides), disulfides, and thiols. Mention may be made of silanes bearing silane, phosphine or disulfide groups. Depending on the metal, different Preferred are linker compounds which are

[0042] Aluminum, titanium, tantalum, niobium, zirconium, and oxides of these metals In the latter case, the linkers to the metal and metal oxide layers are preferably methoxysilanes and Alkoxysilanes such as ethoxysilane, e.g., having the formula (H3CO)3Si-R The silanes (R is, for example, methacrylate, alkylamine, phenylamine, or epoxy) For attachment to parylene, the linker is preferably acryloyl. The silyl part of the linker and the (meth)acryloyloxy functional group are The length of the carbon chain between the yloxy moiety is typically 1 to 16 carbon atoms (methyl , ethyl, propyl, butyl, pentyl, ...). The hydrocarbon chain is typically saturated. However, they may also contain one or more unsaturated bonds. Particularly suitable linkers are Silquest The compound is 3-(trimethoxysilyl)propyl methacrylate (A-174) from Other silane coupling agents such as G-170 (vinyl functional silane coupling agent) from Silquest Lanthanide compounds are also suitable. In addition, bis-trimethoxysilyl or bis-triethoxysilyl A silyl-containing linker, such as bis(trimethoxysilylethyl)benzene, is used. obtain.

[0043] Particularly for titanium, zirconium, and platinum, hybrids such as trihydrosilane are used. Linkers with lid functional groups work well. 10-Undecenylsilane and n-O Particular mention may be made of octadecylsilane. The silanes are preferably reacted from the gas phase or aprotic In addition, the above-mentioned acryloyloxy group-containing acryloyloxy group is added at room temperature from a solution. Alkoxysilane, and bis-trimethoxysilyl or bis-triethoxysilyl functional groups Compounds having the formula:

[0044] Suitable linkers for linking the parylene layer to the gold layer are typically mercaptans, phosphatides, Sulfides or disulfides, preferably having 10 to 16 carbon atoms. longer hydrocarbon groups such as alkyl- or dialkyl-disulfides with alkyl groups Has a chain.

[0045] Such alkyl groups form dense and well-ordered layers on the surface of metals or metal oxides. However, alkyl groups having only 1 to 9 carbon atoms can also be used.

[0046] Equally suitable for gold layers are thiol, phosphine or disulfide groups. A particularly preferred example is 3-(2-pyridylethyl)thiopropyl silane linker. Trimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, 2- (Diphenylphosphino)ethyltriethoxysilane, Bis(2-methacryloyl)oxy diethyl disulfide, and dihexadecyl disulfide.

[0047] The bifunctional linker is preferably applied by a plasma coating process or by a plasma By plasma-free physical vapor deposition or by the addition of aprotic or aryl groups to the bifunctional linker compounds. The metal or metal oxide surface is coated with an alcoholic or aqueous solution. The silane compound is applied to the metal or metal oxide surface in a plasma chamber. The ions are oriented substantially parallel to the metal oxide surface and are bonded to the surface via oxygen atoms. This results in a glassy layer with Si-O-Si-O chains. The organic residues are on the opposite side of the surface. Physical vapor deposition and wet application are also suitable for bonding with parylene. The resulting interface layer has a structure but does not have a glassy appearance.

[0048] Plasma deposition results in a dense layer with acceptable adhesion to parylene. The physical vapor deposition produced a layer that adhered better to the parylene than the plasma deposited layer and was less dense. Wet application results in a disordered network with a high degree of cross-linking and high percent These layers also have a high degree of silicon-bonded oxygen. Therefore, wet application is particularly preferred.

[0049] Alternatively, plasma deposition and (plasma-free) physical vapor deposition or wet deposition processes can be combined. That is, a glassy interface layer is first formed by plasma deposition. This is followed by physical vapor deposition or wet application of a second linker layer, thereby forming a composite linker. In such a composite linker layer, the silicon atoms of the glassy layer The second layer is covalently linked to the oxygen atom of the first layer, and the second layer is (methacrylate, alkyl acrylate, Organic residues (such as amines, or epoxyacrylics) are bonded covalently or, for example, to phenols. Available for bonding with Parylene in different ways, such as by der Waals forces It is.

[0050] The interface layer typically has a thickness in the range of 20 to 150 nm, preferably 50 to 100 nm. Yes.

[0051] Finally, a parylene layer, i.e., a poly(p-xylylene) polymer layer, is formed on top of the interfacial layer. The poly(p-xylylene) polymer layer has the following structural formula: [ka] where n is the degree of polymerization.

[0052] The precursor of the poly(p-xylylene) compound is [2.2]paracyclo[p-xylylene] having the following structure: I'm a fan. [ka]

[0053] Precursors of dimeric compounds such as Parylene N, Parylene C, Parylene D, and Parylene F Parylene N is available on the market. X and R1 to R4 are all hydrogen. In Parylene C, one of R1 to R4 is chlorine while the other residues R and X are hydrogen. In Parylene D, two of the residues R1 to R4 are chlorine, while all other residues are In Parylene F, residue X is fluorine while residues R1-R4 are hydrogen. Parylene layers are typically used as a moisture barrier and a dielectric barrier. .

[0054] At high temperatures in a vacuum (above about 500°C, depending on the particular parylene), the dimers split. The monomer is polymerized to form the corresponding p-xylylene radical. On the one hand, the methacrylate group is used to form a methacrylic polymer. Alternatively, they may simply attach to the hydrophobic sites of the interfacial layer.

[0055] According to the present invention, Parylene C, in which one of R1 to R4 is chlorine, is used as the cation exchange layer of the above-mentioned composite layer. When applied as a barrier layer, it makes the magnetic material corrosion resistant in the environments encountered in intravascular blood pumps. It has been found that the Parylene C layer is preferably applied by plasma deposition, The thickness is preferably in the range of 5 to 20 μm, and more preferably 10 to 16 μm.

[0056] When Parylene C is applied directly onto the surface of the magnetic material, the protective Parylene C layer cladding Crack formation and delamination as well as corrosion of the magnetic material are observed within a few days. When applied onto a metal layer or a metal / metal oxide layer, it is possible to obtain a membrane that can be tolerated in the environment of an intravascular blood pump. Corrosion of the magnetic material due to spalling is observed within an unacceptably short period of time. Parylene compounds other than Parylene C are not compatible with adhesion promoters, i.e., Silane. When applied over the interface layer of a base, it does not provide sufficient corrosion protection.

[0057] The composite coating of the present invention adheres well to the magnet body and is made up of inorganic and organic constituents. Since the structure is made of both inorganic and organic materials, it is effective for both inorganic and organic materials. In addition, the glassy interfacial layer also has barrier properties.

[0058] In a particularly preferred embodiment of the invention, the corrosion protection of the magnetic material is achieved by covering the magnet body with a uniform thickness. By specially adapting the shape of the magnet body to allow the formation of a coating that For this purpose, the magnet body has no sharp edges and is Preferably, the magnet body has a rod-like shape. and extending longitudinally inwardly to receive a motor shaft of an intravascular blood pump. The magnet body has a channel through which the magnet passes and the front faces of both sides of the magnet body are chamfered towards the channel. The channels do not need to be coated with a composite coating because the intravascular blood In a pump, the channel receives the motor shaft and is fixed to it. Of course, as a safety measure, the channel may be coated in some way.

[0059] The magnet body may be a single piece or may consist of several segments. In this case, each segment is provided with a coating of the present invention that completely surrounds it. or at least surrounding the exposed surface thereof. It has a sharp edge.

[0060] The invention will be further explained with reference to the accompanying drawings. [Brief description of the drawings]

[0061] [Figure 1] 1 is a schematic longitudinal cross-sectional view of an exemplary embodiment of an intravascular blood pump; [Figure 2a] FIG. 2 is a schematic diagram of an exemplary single-piece magnet in accordance with the present invention. [Figure 2b] FIG. 2b is a partial cross-sectional view showing a detail of the magnet depicted in FIG. 2a. [Diagram 3] FIG. 2 is a schematic top view of an exemplary segmented magnet in accordance with the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0062] The drawings are not to scale. They are not intended to limit the invention in any way. It should not be regarded as a thing.

[0063] The intravascular blood pump 10 depicted in FIG. 1 has been described above. This pump is generally The pump shown in FIG. In this invention, the magnet is rod-shaped and both front faces are flat and parallel to each other. Composite coatings according to the present invention have been shown to be resistant to corrosion over extended time periods as depicted in FIG. However, in the present invention, the magnet body having a sharp edge can be effectively protected. In this case, it is preferable to use a magnet body having a shape as illustrated in FIG. 2 and FIG. Each individual layer of the composite coating is completely coated onto each previously applied composite coating layer. It is extended.

[0064] FIG. 2a shows a rod-shaped rod having holes or channels extending longitudinally therethrough. The magnet 1 in the intravascular blood pump 10 as depicted in FIG. During use, the channel receives the motor shaft 25. The front faces 4 on either side of the magnet The magnet 1 is exposed to the fluid flowing through the gap 26. On the outer surface 2 exposed to the outside and on the tapered front surface 4, a composite coating according to the invention is applied. The inner surface 3 adjacent to the motor shaft 25 is coated An edge 5 at the transition between the outer surface 2 and the front surface 4, and The edge 6 at the transition between the front surface 4 and the inner surface 3 is coated. "N" is soft and promotes the formation of a better adherent and uniform coating. and "S" represent the north and south poles of a magnet.

[0065] FIG. 2b is a partial cross-sectional view taken along the dashed line in FIG. 2a. Fig. 2b clearly shows the soft edges 5, 6.

[0066] FIG. 3 shows a segmented magnet 7. The magnet depicted in FIG. 3 has four segments. The segments 8 face each other and are marked "N" in the top view of FIG. As shown, the segments 8' also face each other and have the same magnetic polarity. As a result, they have the same magnetic polarity, as indicated by "S" in the top view of Figure 3. Adjacent segments 8, 8' have opposite magnetic polarities.

[0067] The segments 8, 8' are arranged on the inner surface, the outer surface, and the inner surface of the magnet. The side surfaces, the front surfaces on both sides, the edges at the transition between the outer surface and the front surface, and the front and inner The front surface has an edge at the transition between the front surface and the side surface. is designated 4', and the edges are designated 5' and 6', respectively. In addition, segments 8 and 8' are In the drawing it has sides 9, 9' separated by a gap. Of course, magnets are used. When the magnet is in contact with the magnet, the sides 9, 9' contact each other. Although they may be completely covered by the composite coating of the present invention, they are in contact with each other. The side surfaces 9, 9' that are not exposed to the outside, as well as the side surfaces 10, 11' that are not exposed because they are in contact with the motor shaft The inner surfaces of all segments do not need to be coated. The edges are soft edges.

[0068] Table 1 shows the results of corrosion tests of niobium iron boron magnets with different coatings. Identical cylindrical non-magnetized NdFe with a length of 12 mm and a diameter of 2.8 mm. 14 B 12 sintered magnets , coated as shown below, and dissolved in water containing 0.9% by weight of sodium chloride at 60°C. The test specimens were inspected daily for up to 60 days, after which They were inspected once a week. Corrosion of the magnetic material can result in the coating lifting or deformation. Thus, the formation of coating lift or bulges on the surface of the test specimen is a sign of the magnetic material The formation of bulges of 0.1 mm in height and the lifting of the coating indicate the chipping of the magnet. It was stipulated that this indicates a defect.

[0069] The test samples were prepared in the following manner: All samples: Unmagnetized neodymium iron boron magnet bodies (as purchased, phosphate passivated) The coated plate (without coating) was washed with isopropanol and then dried in a stream of air. After the coating is applied, the coated magnet is magnetized in a magnetic field. Magnetizing the magnet body prior to application of the composite coating of the present invention has been subject to Not suitable. The coating thickness is approximately 7 μm for the aluminum layer and 10 μm for the silane layer. for the SiO2 layer, about 100 nm, and for the Parylene layer, about 10 μm, where applicable. Ta.

[0070] Samples 1 and 2: Dry magnet bodies coated with aluminum by ion deposition. Exposure to air causes an aluminum oxide layer to form (a natural aluminum oxide layer). Then Parylene C was applied on top of it.

[0071] Samples 3 and 4: Dry magnet bodies coated with aluminum by ion deposition. Exposure to air causes the natural aluminum oxide layer to dissolve into the exposed aluminum layer. A further coating was not applied.

[0072] Sample 5: A dried magnet body was coated with aluminum by ion deposition. Upon exposure to air, a layer of natural aluminum oxide was formed. (Toxylyl)propyl methacrylate (Silane A-174) is plasma coated Then, Parylene F was applied by plasma coating.

[0073] Samples 6 and 7: Dry magnet bodies coated with aluminum by ion deposition. Upon exposure to air, a layer of native aluminum oxide was formed. Alcoholic solution containing A-174 (water / ethanol; acetic acid to obtain a pH of about 5-6; After about 5 minutes of reaction time (approximately 1% silane concentration) the alcohol was evaporated. , Parylene C was applied by plasma coating.

[0074] Sample 8: A dried magnet body was coated with aluminum by ion deposition. Upon exposure to air, a natural aluminum oxide layer was formed. Silane A-1 was then 74 was applied by plasma coating, followed by Parylene C. Granted by Ng.

[0075] Ion deposition for samples 1 to 8 was performed at approximately 10 -3 In argon gas at about 100 mbar It was performed at a voltage of 0 volts and a current of 1500 amps DC. Typically, it is about 400-1 000 volts and approximately 500 to 1500 DC amps are suitable.

[0076] Samples 9 and 10: Dry magnet bodies were spray-coated with ethylene and Coated with chlorotrifluoroethylene copolymer. Coated magnet The was subjected to baking and then cooled.

[0077] Samples 11 and 12: Dried magnet body spray-coated with polyphenylene sulfide resin. The plate was then coated with 100% cellulose acetate and baked at 135° C. for 30 minutes.

[0078] [Table 1] Coated Nd2Fe 14 B magnet in 0.9% NaCl solution at 60℃ Test results If the coating lifts or buckles, reaching 0.1mm, the magnet will be rejected. A magnet passes the test if the time to failure is at least 6 months (1 month = 30 days). If the magnet passes the test, i.e. the time to failure is at least 180 days, the magnet is Stones are corrosion resistant in the context of the present invention.

[0079] Samples 9, 10, 11, and 12 were directly applied to the neodymium iron boron magnet body. Each has a resin coating according to the state of the art, but is heated to 60°C with sodium chloride. It failed in less than 3 days in the thorium solution. Samples 1-5, which had a layer of silicium, survived for a longer time. Samples without any protective layer and protected from corrosion by an aluminum / aluminum oxide layer 3 and 4 failed in less than one month. When applied directly onto the aluminum layer, i.e., without the silane-based interfacial layer (sample The same results were obtained for samples 1 and 2. In addition, the aluminum oxide layer and the parylene layer There is a silane-based interface layer between the two layers, but the parylene layer is not made of Parylene C (see test The same results were obtained with sample 5).

[0080] Sample 8 has essentially the same coating composition as Sample 5, and is a composite coating. The individual layers of coating were applied in the same manner. However, in sample 8, the coating Parylene C was used instead of Parylene F in Model 5. Amazingly, this slight improvement However, sample 5 had already failed in less than a month, while sample 8 had failed in 6 This resulted in no failure even after a month.

[0081] The coating composition of samples 6 and 7 is the same as that of sample 8. However, in samples 6 and 7, a wet process was used to apply the interface layer. In sample 8, the interface layer was applied by plasma coating. As a result, samples 6 and 7 were not affected when testing was stopped after one year. Sample 8 was left in a corrosive environment for 12 months and still showed no signs of corrosion. did not survive.

[0082] The above test results were obtained from the metal layer, the linker layer, and the poly(2-chloro-p-xylylene). A neodymium iron boron permanent magnet having a composite coating with an outer layer formed from It has excellent corrosion resistance even under harsh conditions and can be advantageously used in intravascular blood pumps. gives a clear result.

[0083] The test results also show that the method of application of the linker layer affects corrosion resistance. Particularly good corrosion resistance was achieved when the linker layer was applied by a wet process.

[0084] To achieve optimum corrosion resistance, the composite coating of the present invention is applied to a non-magnetized magnet body. It is preferred to apply the coating to the magnet only after the magnet has been applied and magnetize the magnet only after the coating has been applied.

[0085] Samples 6, 7, and 8 met both of the above conditions. The unmagnetized magnet body was Coated with the composite coating of the present invention, magnetized after application of the complete composite coating. As a result, samples 6, 7, and 8 were dissolved in 0.9 wt% NaCl solution. Even after at least 180 days at 60°C, the coating shows no lifting and 0. The thickness was less than 1 mm. Therefore, samples 6, 7, and 8 are corrosion-resistant magnets. .

Claims

1. A magnet body, a composite coating disposed on and covering a surface of the magnet body; wherein the composite coating comprises: (a) a metal layer on the magnet body; (b) optionally, a metal oxide layer on the surface of the metal layer opposite the magnet body; and, (c) a linker layer on the metal layer or the metal oxide layer; and (d) a layer formed of poly(2-chloro-p-xylylene) on the linker layer; and Equipped with The magnet body is a rare earth metal-iron-boron permanent magnet, If the metal of the metal layer is aluminum, titanium, tantalum, niobium, zirconium, and a mixture of two or more of aluminum, titanium, tantalum, niobium, and zirconium. Selected from gold, The linker forming the linker layer is selected from alkoxysilanes. Permanent magnet.

2. The magnet of claim 1 , wherein the magnet body is a sintered magnet body.

3. 3. The magnet of claim 1 or 2, wherein the rare earth metal is neodymium.

4. The magnet body is made of Nd 2 Fe 14 B crystal and the Nd 2 Fe 14 Neodymium surrounding B crystal and a neodymium iron boron material, 2 Fe 14 4. The magnet of claim 3 which is richer in neodymium than B crystals.

5. The magnet body according to claims 1 to 4, wherein the magnet body is rod-shaped and all edges are rounded. The magnet according to any one of the preceding claims.

6. The silane is a trimetanyl silane having an acryloyloxy or methacryloyloxy functional group. triethoxysilane and triethoxysilane, or bis-trimethoxysilyl functional groups The magnet according to any one of claims 1 to 5, wherein the linker is selected from the group consisting of

7. The metal of the metal layer is aluminum, titanium, tantalum, niobium, zirconium, and An alloy of two or more of aluminum, titanium, tantalum, niobium, and zirconium and the surface of the metal layer opposite to the magnet body is selected from the group consisting of the metal or metal alloy.

7. The method according to claim 1, further comprising the step of: The magnet according to claim 1.

8. All layers of the composite coating extend completely over all surfaces of the magnet body. The magnet according to any one of claims 1 to 7.

9. The thickness of the metal layer or the total thickness of the metal layer and the metal oxide layer is 5 μm to 20 μm. The magnet according to any one of claims 1 to 8, wherein the magnet has a molecular weight in the range of m.

10. The metal layer is covered by an oxide layer, the oxide layer having a thickness in the range of 2 nm to 5 nm. The magnet according to any one of claims 1 to 8, comprising only one of the above-mentioned components.

11. 11. The method according to claim 1, wherein the thickness of the linker layer is in the range of 20 nm to 150 nm. or a magnet as described in any one of the preceding claims.

12. The thickness of the layer formed from poly(2-chloro-p-xylylene) is 5 μm to 20 μm. The magnet according to any one of claims 1 to 11, wherein the range is

13. 13. The method according to claim 1, wherein the thickness of the composite coating is less than 50 μm. Magnet as described.

14. Providing an unmagnetized magnet body; forming a metal layer on a surface of the magnet body; A step of forming a linker layer on the metal layer or the metal oxide layer formed on the metal layer. Tep and forming a layer of poly(2-chloro-p-xylylene) over the linker layer; 、 magnetizing the magnet body; Inclusive of The magnet body is a rare earth metal-iron-boron permanent magnet, If the metal of the metal layer is aluminum, titanium, tantalum, niobium, zirconium, and a mixture of two or more of aluminum, titanium, tantalum, niobium, and zirconium. Selected from gold, The linker forming the linker layer is selected from alkoxysilanes. A method for manufacturing a permanent magnet.

15. The magnet body is a magnet body as defined in any one of claims 1 to 5. The method according to claim 14.

16. The metal layer is applied by ion deposition or plasma deposition or atomic layer deposition.

16. The method of claim 14 or 15, wherein the compound is formed by:

17. The metal layer is formed by applying metal by galvanic deposition from an ionic liquid.

16. The method of claim 14 or 15, wherein the

18. A metal oxide layer is formed on the metal layer by oxidizing the metal or alloy. The method according to any one of claims 14 to 17.

19. The linker layer is formed by physical vapor deposition using or without plasma. Phosphorus can be deposited by physical vapor deposition, or by a wet process, or by a combination of both. The method according to any one of claims 14 to 18, wherein the surface is formed by applying a curing agent.

20. 20. The method of claim 19, wherein the linker is a linker as defined in claim 6. 。

21. The poly(2-chloro-p-xylylene) layer is The method according to any one of claims 14 to 20, wherein the layer is formed by plasma deposition of a compound.

22. Claim 14. The layer has a thickness as defined in any one of claims 9 to 13.

22. The method according to any one of claims 1 to 21.

23. An intravascular blood pump comprising an electric motor, the electric motor being any one of claims 1 to 13.

2. An intravascular blood pump comprising a magnet as defined in any one of claims 1 to 11.

Citation Information

Patent Citations

  • Excellent corrosion-resisting permanent magnet and manufacture thereof

    JP1990208904A

  • Metal foil with adhesion acceleration layer

    JP1995170064A

  • R-fe-b permanent magnet having electric insulating film excellent in adhesion and its manufacture

    JP1997289108A

  • Method for coating with organic material

    JP1998070114A

  • Piezoelectric ceramic element and protection method for its electrode

    JP1998290138A