Invisible fingerprint coatings and process for forming the same

Plasma-activated alkylsilane and OH-POSS coatings on substrates achieve invisible fingerprints by balancing hydrophobicity and hydrophilicity, addressing the limitations of existing coatings in visibility and durability.

JP2024153731APending Publication Date: 2024-10-29NBD NANOTECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024118289
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-05-24
Filing Date
2024-07-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing coatings fail to effectively render fingerprints invisible on surfaces while maintaining optical clarity and mechanical durability, with anti-fingerprint coatings either making fingerprints more visible or not preventing their formation, and invisible fingerprint coatings lacking suitable hydrophobicity and hydrophilicity.

Method used

A method involving plasma activation of substrates with inert gases followed by application of alkylsilane and hydroxyl-terminated polyhedral oligomeric silsesquioxane (OH-POSS) in solvents with aqueous acids or bases to create coatings with tailored hydrophobic and hydrophilic properties, achieving a water contact angle of 70-90 degrees and diiodomethane contact angle of 30-40 degrees.

Benefits of technology

The coatings provide optical transparency, mechanical durability, and self-healing properties, effectively rendering fingerprints invisible by spreading oil and allowing water droplets to bead up and evaporate, while maintaining surface cleanliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153731000001_ABST
    Figure 2024153731000001_ABST
Patent Text Reader

Abstract

To provide a fingerprint-resistant substrate having a coating layer to render fingerprints invisible or nearly invisible.SOLUTION: A fingerprint-resistant substrate comprises, on a surface of the substrate, a formulation for a fingerprint-resistant coating containing POSS and an alkylsilane of the formula (RA)3SiRB, where each RA is independently -O(C1-C6 alkyl), -O(C2-C6 alkenyl) or -O(C2-C6 alkynyl), and RB is C11 alkyl substituted with halogen, where the alkylsilane is free of fluoro. The fingerprint-resistant surface has a delta E of less than 2, where the delta E is calculated by a specific method for a surface of a fingerprint-resistant substrate with a fingerprint prepared under specific conditions.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Patent Application No. 62 / 676,052, filed May 24, 2018, the disclosure of which is incorporated by reference in its entirety.

[0002] Field DETAILED DESCRIPTION The present disclosure, in an exemplary embodiment, relates to a coating composition for coating a substrate to make fingerprints invisible or nearly invisible. [Background technology]

[0003] Humans naturally produce sebum (from sebaceous glands) and other oils on their faces and fingertips. Humans may deposit such oils on the display screen of a mobile phone (or other object), such as glass (or screen protectors, usually polymers or plastics), glass ceramics, metal oxides, plexiglass, or similar materials or surfaces. Often such oils are visible and may degrade the quality of the image viewed on such devices, as well as cause a decrease in the aesthetic appearance of the screen (along with dirt, dust, etc.). Fingerprint Invisibility ("IFP") coatings are generally oleophilic coatings that make the oil invisible or nearly invisible by spreading it along the screen surface. The oil may match the refractive index of the screen material, e.g., glass, resulting in light passing through and making it appear as though there is no fingerprint. Fingerprints may still be present, but they cannot be seen (at least without probing the surface). Coatings and coating materials that exhibit IFP properties may need to be hydrophobic enough to allow water to bead up and evaporate. If the coating is too hydrophilic, fingerprints may be visible, however, if the coating is too hydrophobic, the surface may not exhibit the proper properties.

[0004] In contrast, "anti-fingerprint" ("AFP") coatings are oleophobic coatings that resist wetting and can make any fingerprints that do form more easily cleaned, but do not prevent fingerprints from forming or reduce the noticeableness of any fingerprints that do form. IFP coatings function in a different manner than AFP coatings.

[0005] It is desirable to have a coating that can provide optical clarity, mechanical durability, and fingerprint invisibility. Summary of the Invention

[0006] The following presents a simplified summary to provide a basic understanding of some aspects of various invention embodiments. This summary is not an extensive overview of the invention. It is not intended to identify key or critical elements of the invention or to delineate the scope of the invention. The following summary merely presents some concepts of the invention in a simplified form as a prelude to the more detailed description below.

[0007] The present disclosure relates in an exemplary embodiment to compositions and formulations for providing an IFP coating. The present disclosure also relates to a method for forming a hydrophobic and oleophilic coating on a substrate, such as, but not limited to, a substrate made of a glass material, a ceramic, or a metal oxide surface.

[0008] In one exemplary embodiment, a method for forming a fingerprint resistant coating on a substrate includes the steps of: (a) reacting an inert gas, N 2 , O 2 and a mixture of at least two of said gases; and (b) a second deposition step in which a formulation for an anti-fingerprint coating comprising an alkylsilane, a POSS, or a mixture thereof is deposited.

[0009] In another exemplary embodiment, a formulation for an anti-fingerprint coating includes an alkylsilane, a POSS, or a mixture thereof, prepared in either a protic or aprotic solvent, and further includes either an aqueous base or an aqueous acid.

[0010] In another exemplary embodiment, a substrate obtained by the above method is disclosed, wherein the coating comprises a coating over the primer first layer, the coating comprising a mixture of alkylsilanes in either aqueous acid or aqueous base, a hydrophilic OH-POSS, or a mixture thereof.

[0011] In another exemplary embodiment, a composition for providing a fingerprint-invisible coating is disclosed that includes an alkylsilane, a POSS, or a mixture thereof, and has a water contact angle in the range of 70-90 degrees and a diiodomethane contact angle in the range of 30-40 degrees.

[0012] In another exemplary embodiment, a fingerprint-free coating material is disclosed comprising at least one alkylsilane material, a hydroxylated POSS, or a mixture thereof, wherein the coating material has a water contact angle in the range of 75-85 degrees and a diiodomethane contact angle in the range of 30-40 degrees.

[0013] Other features will become apparent from a reading of the following detailed description of certain exemplary embodiments, when taken in conjunction with the appended claims. [Brief description of the drawings]

[0014] The drawings disclose the following exemplary embodiments or test results.

[0015] [Figure 1] Figure 1A is a photograph of a fingerprint placed between two pieces of Gorilla Tempered Glass showing two substrates: the substrate on the left was coated according to Example 1, and the substrate on the right was uncoated.

[0016] FIG. 1B is a detailed view of the photograph of FIG. 1A.

[0017] [Diagram 2] FIG. 2 is a chart showing the chemical resistance of a substrate coated according to Example 5 before and after rubbing with isopropyl alcohol.

[0018] [Diagram 3] FIG. 3 is a graph showing mechanical wear test results of substrates coated according to Example 3 using water and diiodomethane oil. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The fingerprint-resistant substrate according to the present disclosure may include a surface coated with a fingerprint-resistant coating. Illustratively, the fingerprint-resistant substrate may be formed by a method including applying a fingerprint-resistant coating formulation to the surface of the substrate. In some embodiments, the fingerprint-resistant coating formulation includes an alkylsilane, a POSS, or a mixture thereof. As described herein, the fingerprint-resistant surface may have a delta E value of less than about 2 to provide the surface with abrasion resistance.

[0020] In an exemplary embodiment, the substrate may be a glass screen, such as those used in electronic displays, including, but not limited to, cell phone screens, computer monitors, television screens, touch screens, home appliances, heads-up displays, eyewear (e.g., eyeglasses and sunglasses), masks (e.g., welding masks), interior wall paints, and the like. In an exemplary embodiment, the substrate may also be used in the appliance and cosmetic finishing fields, such as decorative panels for appliances, particularly household appliances (refrigerator doors, oven doors, display cases, and the like). The substrate may be made of glass (or screen protectors, typically polymeric plastics), glass ceramics, metal oxides, plexiglass, or other materials. In some embodiments, the substrate comprises a glass, a glass ceramic, a metal oxide, or a plastic.

[0021] In this disclosure, the term "non-visible" should be understood to include not being visible, not visible, barely visible, or not noticeable (e.g., not visible unless the surface is closely inspected). "Non-visible" should be understood to some extent to depend on the refraction of light and also on the direction from which the surface is viewed. From one angle, a fingerprint may not be visible, but may be discernible from another. The term "wettability" refers to the propensity by which polar or non-polar liquids adhere to a substrate and form undesirable films, and further refers to the tendency of the substrate to retain any kind of dirt, stains, fingerprints, insects, etc.

[0022] In some embodiments, the presence of liquids, which may include oils, may be important in electronic displays, especially to reduce the visibility of fingerprints on the surface. The wetting properties of a substrate can be classified as hydrophobic / oleophobic and hydrophilic / oleophilic. A hydrophobic / oleophobic substrate means a substrate that repels oils (including organic liquids) and water. Typically, the contact angle of an omniphobic surface is greater than about 60 degrees for hexadecane and greater than about 90 degrees for water on a flat surface. A hydrophilic / oleophilic substrate means that oil and water are attracted to the surface. Thus, the liquid spreads easily across the surface and has a low contact angle (less than about 50 degrees).

[0023] In one approach to obtain a fingerprint-invisible coating, the water and oil contact angles may be optimized so that the resulting liquid spreads across the surface and matches the refractive index of the liquid on the surface derived from the glass substrate. In such a case, light will pass through the fingerprint, resulting in the visible effect of a fingerprint that is invisible. To obtain this contact angle, it has been demonstrated that a surface with hydrophobic and oleophilic properties is desirable. In one approach to optimizing the effect, it has been found that the water contact angle may be in the range of about 70-90 degrees or about 70-85 degrees, and the diiodomethane contact angle may be in the range of about 20-40 degrees or about 25-40 degrees.

[0024] A feature of some compositions disclosed herein is the use of hydrophobic alkylsilanes, OH-POSS, or mixtures thereof. The alkylsilanes provide hydrophobicity, but by themselves may have a water contact angle of about 110 degrees, which is too hydrophobic. Therefore, in some embodiments, additives are required to reduce both the water and diiodomethane contact angles, but the additives must provide wettability and IFP properties when incorporated into the coating, and also be able to form a coating with the alkylsilane. Therefore, existing additives were likely not suitable. In some exemplary embodiments disclosed herein, OH-POSS is used as an additive because it is hydrophilic.

[0025] There are several advantages of incorporating the fingerprint invisibility coating described herein on a substrate, such as a glass substrate. Such coatings can allow water droplets to slide off vertical or inclined surfaces and be easily washed off. The oleophilic surface of such coatings can allow fingerprint oils to spread across the surface, resulting in a liquid film instead of oil piling up. In an exemplary embodiment, a combination of hydrophobicity and oleophilicity tailored to a specific contact angle of at least about 70 degrees or at least about 80 degrees with water and less than about 40 degrees with diiodomethane can maximize light transmission or fingerprint invisibility. Such coatings can demonstrate self-healing properties with floating hydrophilic additives based on the hydrophobic coating, thereby reducing degradation over time.

[0026] Agents known to impart fingerprint-invisible properties that can be used in the form of a coating layer on glazing (substrate) include, but are not limited to, alkylsilanes in acidic or alkaline solutions, hydroxyl-terminated T8 POSS nanoparticles, or mixtures thereof. As described herein, the coating layer can be obtained by applying a solution containing alkylsilane materials and OH-POSS in an aqueous or non-aqueous acidic or basic solvent to the surface of the substrate.

[0027] In some embodiments, the alkylsilane is difunctional. Exemplary difunctional alkylsilanes include haloalkylsilanes, bisalkylsilanes, bisalkoxysilanes, aminoalkylsilanes, hydroxyalkylsilanes, and phosphatealkylsilanes.

[0028] Exemplary bisalkylsilanes include bistriethoxyoctylsilane and bis(trimethoxysilyl) 4-oxa-8-azundecan-6-ol.

[0029] Exemplary haloalkylsilanes include chloroundecylsilane and chlorohexylsilane.

[0030] Exemplary aminoalkylsilanes include aminoundecylsilane, N-2-aminoethyl-11-aminoundecyltriethoxysilane, and N-6-aminohexylaminomethyltriethoxysilane.

[0031] Exemplary hydroxyalkylsilanes include OH-decyltriethoxysilane.

[0032] Exemplary phosphate alkyl silanes include phosphate undecyltriethoxysilane.

[0033] A "self-healing" material is one that has the ability to repair damage caused by mechanical use over time. Hydroxyl T8-POSS is a nanoparticle-based structure whose ends are hydrophilic and oleophilic, which reduces the water repellency of the alkylsilane. The nanoparticles formed by the exemplary methods disclosed herein can be distributed nearly uniformly in a polymer matrix. These nanoparticles float to the surface of the polymer matrix when damaged, and exhibit self-healing capabilities.

[0034] As described herein, in some embodiments, the fingerprint resistant substrate comprises a substrate including a surface and a fingerprint resistant coating on the surface. Illustratively, the fingerprint resistant surface can have a delta E of less than 2.

[0035] Illustratively, the substrate may be made of glass, polymer, glass ceramic, metal oxide, plexiglas, or other materials.

[0036] The Delta E of the fingerprint resistant surface is the measured difference between clean or unused glass and glass with fingerprints, as described in the Examples. Illustratively, the lower the Delta E, the less visible the fingerprints are on the surface. The Delta E can also be measured after wiping the surface to determine how well the fingerprints have been removed. In some embodiments, the Delta E of the fingerprint resistant surface may be less than about 3, less than about 2, less than about 1, less than about 0.8, or less than about 0.5. In some embodiments, the Delta E of the fingerprint resistant surface is about 0.05, about 0.1, about 0.2, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1, about 1.1, about 1.2, about 1.3, about 1.4, about 1.5, about 1.6, about 1.7, about 1.8, about 1.9, about 2, about 2.2, about 2.5, or about 3. In a first set of ranges, the Delta E of the fingerprint resistant surface ranges from about 0.1 to about 2, from about 0.1 to about 1.5, from about 0.1 to about 1, from about 0.2 to about 1, from about 0.3 to about 1, or from about 0.4 to about 0.9. In a second set of ranges, the Delta E can be from about 0.05 to about 1.2, from about 0.05 to about 0.9, from about 0.05 to about 0.8, or from about 0.05 to about 0.5.

[0037] In some embodiments, the fingerprint resistant surface is resistant to diiodomethane (CH), as measured according to the Examples. 2 I 2 ) in a range of about 20° to about 60°, about 50° to about 45°, about 40° to about 35°, or about 30°. In some embodiments, the initial oil angle of the fingerprint resistant surface is about 20°, about 21°, about 22°, about 23°, about 24°, about 25°, about 26°, about 27°, about 28°, about 29°, about 30°, about 31°, about 32°, about 33°, about 34°, about 35°, about 37°, about 40°, about 45°, about 50°, about 55°, or about 60°. In some embodiments, the initial oil angle of the fingerprint resistant surface may range from about 20° to about 60°, about 20° to about 50°, about 20° to about 40°, about 20° to about 35°, or about 20° to about 30°.

[0038] In some embodiments, the fingerprint resistant surface has an initial water angle as measured according to the examples. In some embodiments, the initial water angle is greater than about 60°, greater than about 65°, greater than about 75°, greater than about 80°, greater than about 90°, or greater than about 100°. In some embodiments, the initial water angle of the fingerprint resistant surface is about 60°, about 65°, about 70°, about 75°, about 76°, about 77°, about 78°, about 79°, about 80°, about 81°, about 82°, about 83°, about 84°, about 85°, about 86°, about 87°, about 88°, about 89°, about 90°, about 95°, about 100°, about 105°, about 110°, or about 115°. In some embodiments, the initial water angle of the fingerprint resistant surface may range from about 60° to about 115°, from about 60° to about 110°, from about 70° to about 110°, from about 70° to about 95°, from about 70° to about 90°, or from about 75° to about 95°.

[0039] In some embodiments, the fingerprint-resistant surface has a particular abrasion resistance as measured by the water angle after a certain number of cycles, as described in the Examples. Exemplarily, the fingerprint-resistant surface may have a particular water angle after enduring about 1,500 cycles, about 3,000 cycles, or about 4,500 cycles, as described in the Examples. Exemplarily, the water angle after abrasion may be greater than about 40°, greater than about 50°, greater than about 55°, or greater than about 60°. In some embodiments, the water angle of the fingerprint-resistant surface after abrasion is about 40°, about 50°, about 55°, about 60°, about 65°, about 70°, about 75°, about 80°, or about 85° after about 1,500 cycles, about 3,000 cycles, or about 4,500 cycles. In some embodiments, the water angle of the fingerprint resistant surface after abrasion may range from about 40° to about 85°, about 50° to about 85°, about 50° to about 80°, or about 60° to about 80° after about 1,500 cycles, about 3,000 cycles, or about 4,500 cycles.

[0040] In exemplary embodiments, the fingerprint resistant surface has a particular coefficient of friction. In some embodiments, the coefficient of friction is less than about 0.2 or less than about 0.15. In some embodiments, the coefficient of friction is about 0.08, about 0.09, about 0.1, about 0.11, about 0.12, about 0.13, about 0.14, or about 0.15. In some embodiments, the coefficient of friction is in the range of about 0.08 to about 0.15 or about 0.09 to about 0.13.

[0041] In some embodiments, the fingerprint resistant surface is formed by applying a fingerprint resistant coating formulation onto a substrate. In some embodiments, the fingerprint resistant coating formulation comprises an alkyl silane, a POSS, or a mixture thereof. In some embodiments, the formulation comprises a solvent.

[0042] In some embodiments, the alkylsilane is an alkylsilane of the formula: (R A ) 3 SiR B and In the formula, each R A are independent, -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 alkynyl, and R B is C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 alkynyl, where -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, -OC 2 ~C 6 Alkynyl, C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C2 ~C 20 Each hydrogen atom in an alkynyl may be independently selected from deuterium, halogen, -OH, -CN, -OR ... 1 , -CO 2 H, -C(O)OR 1 , -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C 6 Alkyl, -S(O)NH(C 1 ~C 6 alkyl), -S(O) 2 NH(C 1 ~C 6 alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl) 2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl) 3 and where -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 C 1~ C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl, and 1 are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl. A Ha-OC 1 ~C6 In some embodiments, R B is C 10 ~C 20 Alkyl, C 10 ~C 20 Alkenyl, or C 10 ~C 20 alkynyl, where C 10 ~C 20 Alkyl, C 10 ~C 20 Alkenyl, or C 10 ~C 20 Each hydrogen atom in the alkynyl is optionally replaced with halo. B is halo-substituted n-octyltriethoxysilane or halo-substituted C 1 ~C 6 Not alkyl.

[0043] In some embodiments, R B is C 1 ~C 20 Alkyl, C 6 ~C 20 Alkyl, or C 10 ~C 20 alkyl, where C 1 ~C 20 Alkyl, C 6 ~C 20 Alkyl, or C 10 ~C 20 Each hydrogen atom in the alkyl is optionally substituted. In some embodiments, each hydrogen atom is independently optionally substituted with halogen, -OH, -CN, -OR 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO3 H 2 where R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6 is alkyl. Exemplarily, the halogen may be chloro, bromo, or iodo. In some embodiments, the alkylsilane contains a halogen but does not contain a fluoro. In some embodiments, the alkylsilane does not contain a PEG group.

[0044] In some embodiments, the alkylsilane may be at a specific concentration in the formulation for the anti-fingerprint coating. In some embodiments, the alkylsilane is present at a concentration of about 1 g / l to about 6 g / l, about 1 g / l to about 5 g / l, about 2 g / l to about 5 g / l, or about 3 g / l to about 5 g / l. In some embodiments, the alkylsilane may be present at a concentration of about 1 g / l, about 2 g / l, about 3 g / l, about 3.25 g / l, about 3.5 g / l, about 3.75 g / l, about 4 g / l, about 4.25 g / l, about 4.5 g / l, about 5 g / l, about 5.5 g / l, or about 6 g / l.

[0045] In some embodiments, the alkyl silane is selected from the group consisting of (chloroundecyl)(triethoxy)silane, (chloroundecyl)(trimethoxy)silane, (chlorohexyl)(triethoxy)silane, (chlorohexyl)(trimethoxy)silane, 11-(2-methoxyethoxy)undecyltrimethoxysilane, (aminoundecyl)(triethoxy)silane, (aminoundecyl)(trimethoxy)silane, (hydroxydecyl)(triethoxy)silane, (hydroxydecyl)(trimethoxy)silane, (11-undecylinic acid)(triethoxy)silane, (hydroxyheptyl)(triethoxy)silane, (hydroxyundecyl)(triethoxy)silane, and (11-phosphoundecyl)(triethoxy)silane.

[0046] In some embodiments, the POSS is a POSS of the formula: [ka] and In the formula, R is -C 1 ~C 6 Alkyl, -A E -OB F -C G -OD H , or -O-Si(C 1 ~C 6 Alkyl) 3 where A is C 1 ~C 6 alkyl and B is -C 1 ~C 6 alkyl-O-, C is C 1 ~C 6 alkyl and D is C 1 ~C 6 is alkyl, O is oxygen, E, G, and H are each at least 1, F is an integer from 5 to 12, -C 1 ~C 6 Each hydrogen atom in an alkyl group may be independently selected from deuterium, halogen, -OH, -CN, -OR, -N-C, -N-O ... 2 , -OC 1 ~C 6 Alkyl, -NH 2 , -NH(C 1 ~C 6 alkyl), -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -OPO 3 H and R 2 are independently deuterium, C 2 ~C 6Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 In some embodiments, R is -A E -OB F -C G -OD H or -O-Si(C 1 ~C 6 Alkyl) 3 In some embodiments, R is -A E -OB F -C G -OD H In some embodiments, R is -(CH 2 ) 3 O(CH 2 CH 2 O) 9 CH 2 CH 2 OCH 3 In some embodiments, R is -O-Si(CH 2 ) 2 CH 2 CH 2 CH 2 Exemplary POSS can be made according to Example 1 of US Patent Application Publication No. 2017 / 0349785 or purchased from Sigma Aldrich under CAS number 288290-32-4. In some embodiments, R is C 1 ~C 6 Alkyl or -O-Si-(C 1 ~C 6 Alkyl) 3 and at least one C 1 ~C 6 The alkyl is substituted with at least one hydroxy.

[0047] In some embodiments, the POSS may be present in a specific concentration in the formulation for the anti-fingerprint coating. In some embodiments, the POSS is present in a concentration of about 10 mg / l to about 1 g / l, about 10 mg / l to about 800 mg / l, about 20 mg / l to about 800 mg / l, about 50 mg / l to about 500 mg / l, or about 50 mg / l to about 250 mg / l. In some embodiments, the POSS may be present in a concentration of about 10 mg / l, about 50 mg / l, about 75 mg / l, about 100 mg / l, about 125 mg / l, about 150 mg / l, about 200 mg / l, about 300 mg / l, about 400 mg / l, about 500 mg / l, about 600 mg / l, about 700 mg / l, about 800 mg / l, or about 1 g / l.

[0048] In some embodiments, the composition comprises a siloxane. In some embodiments, the alkoxysilane is a trialkoxysilylsiloxane. In some embodiments, the dialkylsiloxane is a vinyl terminated dialkylsiloxane represented by the formula (R C O) 3 is formed by contacting a compound of SiH, where R C is an alkyl group. In some embodiments, the siloxane is an alkyl siloxane. In some embodiments, the alkoxy siloxane is an alkoxy polydimethyl siloxane. In some embodiments, the alkoxy siloxane is a trialkoxy silyl polydimethyl siloxane. In some embodiments, the siloxane, such as a trialkoxy silyl polydimethyl siloxane, has a molecular weight of at least about 2,000 Da, at least about 3,000 Da, or at least about 4,000 Da. In some embodiments, the siloxane, such as a trialkoxy silyl polydimethyl siloxane, has a molecular weight of less than about 8,000 Da, less than about 6,000 Da, or less than about 5,500 Da.

[0049] In some embodiments, the siloxane, such as trialkoxysilyl polydimethylsiloxane, may be at a specific concentration in the formulation for the fingerprint resistant coating. In some embodiments, the siloxane, such as trialkoxysilyl polydimethylsiloxane, may be present at a concentration of about 0.01 mg / l to about 5 mg / l, about 0.1 mg / l to about 3 mg / l, or about 0.2 mg / l to about 2 mg / l. In some embodiments, the siloxane, such as trialkoxysilyl polydimethylsiloxane, may be present at a concentration of about 0.01 mg / l, about 0.1 mg / l, about 0.2 mg / l, about 0.3 mg / l, about 0.4 mg / l, about 0.5 mg / l, about 0.6 mg / l, about 0.7 mg / l, about 1 mg / l, about 2 mg / l, about 3 mg / l, about 4 mg / l, or about 5 mg / l. In some embodiments, the siloxane, such as trialkoxysilylpolydimethylsiloxane, is present at about 0.375 mg / L.

[0050] In some embodiments, the composition comprises a weight ratio of alkylsilane to siloxane. In some embodiments, the weight ratio is at least about 5:1 or at least 25:1 alkylsilane:siloxane. In some embodiments, the weight ratio is about 5:1 to about 50:1, about 5:1 to about 40:1, or about 5:1 to about 20:1 alkylsilane:siloxane. In some embodiments, the ratio is about 10:1 alkylsilane:siloxane. These exemplary ratios apply equally when the siloxane is a trialkoxysilyl polydimethylsiloxane.

[0051] In some embodiments, the fingerprint resistant coating formulation comprises a solvent. In some embodiments, the solvent comprises water, an alcohol, or a mixture thereof. In some embodiments, the alcohol is C 1 ~C 6 alkyl-OH, In some embodiments, the solvent is methanol, ethanol, propanol, butanol, pentanol, hexanol, or a combination thereof.

[0052] In some embodiments, the solvent is present at an acidic pH. In some embodiments, the solvent is present at a pH of about 1 to about 7. In some embodiments, the pH is about 1, about 2, about 3, about 4, about 5, about 6, or about 7. In some embodiments, the pH is about 1 to about 6, about 2 to about 6, or about 2 to about 5. Illustratively, the solvent can be acidified using an acid. In some embodiments, the acid is nitric acid, although other acids capable of obtaining the desired pH can be used.

[0053] As an illustration, the fingerprint resistant surface formulation can be applied to a substrate to form a fingerprint resistant surface by a specific method. In some embodiments, the method for forming a fingerprint resistant coating on a substrate comprises an applying step. In some embodiments, the method comprises a curing step. In some embodiments, the method comprises an applying step and a curing step.

[0054] In some embodiments, the applying step may be performed by dipping the surface of the substrate into the fingerprint resistant coating formulation, wiping with the formulation, or spraying the surface of the substrate with the formulation.

[0055] In some embodiments, the applying step is performed by dipping the surface of the substrate into the fingerprint resistant coating formulation, wiping with the formulation, spraying the surface of the substrate with the formulation, chemical vapor deposition (CVD), or physical vapor deposition (PVD).

[0056] In some embodiments, a method for forming an anti-fingerprint coating on a substrate includes applying an anti-fingerprint coating formulation to a surface of the substrate by PVD. Illustratively, the applying step can be performed by thermal evaporation. In some embodiments, the method includes curing the formulation on the surface of the substrate. In some embodiments, the method includes cleaning the surface of the substrate. In some embodiments, the cleaning step is performed before the applying step. In some embodiments, the formulation is in the form of a pellet. In some embodiments, the method includes forming a pellet of the formulation. In some exemplary embodiments, forming the pellet includes contacting steel wool or copper foam with a hydrolysate.

[0057] Illustratively, the curing step can be performed at elevated temperatures or at room temperature. In some embodiments, the curing step is performed at room temperature. In some embodiments, the curing step is performed at at least about 70° C., at least about 80° C., at least about 90° C., or at least about 100° C.

[0058] In some embodiments, the curing step is carried out for a period of time to allow the formulation to harden, which may depend on the temperature used in the curing step. In some embodiments, the curing step is carried out overnight. In some embodiments, the curing step is carried out for at least about 5 minutes, at least about 10 minutes, or at least about 30 minutes. In some embodiments, the curing step is carried out for about 10 minutes, about 1 hour, about 2 hours, about 3 hours, about 4 hours, or about 6 hours. In some embodiments, the curing step is carried out at a temperature of about 120° C. for about 10 minutes. In some embodiments, the curing step is carried out at a temperature of about 80° C. for about 1 hour. In some embodiments, the curing step is carried out at room temperature overnight.

[0059] In some embodiments, the method further comprises the step of: 2 , O 2 and activating the surface of the substrate by exposing the surface to a plasma of at least one gas selected from the group consisting of a mixture of at least two of the aforementioned gases.

[0060] One of the more significant challenges with optically transparent substrates and coatings is mechanical abrasion, which degrades, wears off, or reduces the thickness, transparency, or effectiveness of the coating. Abrasion occurs to a greater or lesser extent during handling of the substrate by the user, for example, rubbing with a cloth to remove fingerprints or smudges. This is required periodically to restore sufficient visibility, especially through transparent substrates. Degradation can also occur due to exposure to ultraviolet light, heat, cold, chemicals, salt or other corrosive substances, dirt, other abrasives, or other environmental elements, conditions, or materials.

[0061] Such self-healing and abrasion resistance capabilities typically enable the substrate to more effectively meet the specifications currently imposed by the electronics industry in terms of abrasion resistance, violet UV resistance, and salt resistance.

[0062] In an exemplary embodiment, a suitable coating may have a water contact angle between 70 and 90 degrees or between 75 and 85 degrees. In an exemplary embodiment, a suitable coating may have a diiodomethane contact angle between 30 and 40 degrees.

[0063] According to one exemplary embodiment, an exemplary method for providing a coating on a substrate, such as a substrate formed of a glass material, a ceramic, or a metal oxide, is disclosed, the method comprising the steps of:

[0064] First, the substrate is heated with an inert gas of the Ar or He type, N 2 Gas, O 2 Gas, or H 2The substrate surface is activated by exposing it to a plasma of O gas, or a mixture of two or more of the foregoing. According to one exemplary embodiment, this activation step is performed using a plasma of H 2 This is done by exposing the substrate to a plasma of a gas mixture that includes O. The activation step increases the hydroxyl density on the surface of the substrate, thereby increasing the attachment density of the SAM.

[0065] Secondly, a hydrophobic coating is formed comprising at least one alkyl monolayer and T8 hydroxyl polyhedral oligomeric silsesquioxane (hydroxyl-POSS). In an exemplary embodiment, the alkyl monolayer is either an alkylsilane (AS) or an alkylthiol (AT). In another exemplary embodiment, the alkyl monolayer comprises a bifunctional silane. This is then mixed with a protic or aprotic solvent comprising either an aqueous base or an aqueous acid.

[0066] Third, an optional hydrophobic coating is deposited onto the substrate.

[0067] Fourth, formulations for fingerprint resistant coatings containing alkylsilanes, POSS, or mixtures thereof are prepared in either protic or aprotic solvents with either aqueous bases or aqueous acids.

[0068] Typically, the anti-fingerprint coating formulation is deposited by immersion, spraying, and thermal CVD (chemical vapor deposition) under conditions that allow for an RMS (root mean square) surface roughness between 5 and 100 nm to be obtained. In an exemplary embodiment, an RMS (root mean square) surface roughness between 5 and 10 nm can be obtained.

[0069] The glazed substrate thus obtained is optically transparent, resistant to mechanical abrasion and other mechanical impacts, and self-healing. In this disclosure, "optically transparent" means optically neutral with respect to the substrate (e.g., glass), i.e., the transmission or haze of the pretreated glass is not substantially altered.

[0070] According to one exemplary method, the step of depositing the coating is carried out using a solution obtained from a mixture of an alkylsilane (AS) of the formula, a hydroxyl-terminated T8 polyhedral oligomeric silsesquioxane, and either an aqueous acid or an aqueous base. In some embodiments, the alkylsilane is an alkylsilane of the formula: H 3 C-(CH 2 ) n -Si(X) 3-p (R) p and wherein n=0 to 15, preferably n=3 to 5, or n=10 to 20, and wherein p=0, or 2, or p=0 or 1, and in yet another exemplary embodiment, p=0. In some embodiments, R is an alkyl group or a hydrogen atom, and X is a hydrolyzable group, such as, but not limited to, a halide group or an alkoxy group. In some embodiments, the POSS has the following structure: [ka] having Here, R is OH-(CH 2 ) n , n=0 to 5, preferably n=1.

[0071] A feature of the exemplary embodiment of the composition of the present disclosure is to balance the relative amounts of alkyl silane and the OH-POSS. Conventional alkyl silanes would provide a material that is too hydrophobic and oleophobic to function adequately as a fingerprint-invisible coating. Pure glass is both hydrophilic and oleophobic (WCA of about 30 degrees, and diiodomethane CA of about 40-45 degrees). In terms of substitution on the POSS structure, generally, the more hydroxylation present, the more hydrophilic the structure. It is important to have the appropriate level of hydroxylation, avoiding too high or too low a WCA, which would result in insufficient properties to provide fingerprint-invisible functionality. Too much OH-POSS would make the material hydrophilic and not exhibit the desired properties. Too little OH-POSS would make the material too hydrophobic / oleophobic to function. Thus, wettability must be tailored for a particular OH-POSS composition and intended use (e.g., substrate) to adequately provide fingerprint-invisible properties. The coated surfaces with water contact angles in the range of 75-85 degrees and diiodomethane contact angles in the range of 30-40 degrees exhibited excellent non-visible properties.

[0072] In alternative exemplary embodiments, other non-fluorinated hydrophobic materials may be used in place of OH-POSS, including, but not limited to, other hydrophilic POSS materials such as PEGylated-POSS, amine-substituted POSS, carboxylic acid-substituted POSS, etc.

[0073] In another exemplary embodiment, a coating made according to the methods disclosed herein had a water contact angle of 80 degrees and a diiodomethane contact angle of 30 degrees, and exhibited excellent fingerprint non-visible properties.

[0074] The present disclosure also relates to omniphobic coatings that include or are formed by the substrates described herein, particularly for use as glazing for various media surfaces or buildings.

[0075] An aqueous acid or base may be required to aid in the nucleophilic reaction of the alkylsilane. In an exemplary embodiment, the acid may have a pH in the range of 1-3. In an exemplary embodiment, the acid may be a composition, such as, but not limited to, ascorbic acid, citric acid, salicylic acid, acetic acid, hydrochloric acid, oxalic acid, phosphoric acid, sulfuric acid, and the like. In an exemplary embodiment, the base may have a pH in the range of 11-14. In an exemplary embodiment, the base may be a composition, such as, but not limited to, ammonium hydroxide, sodium bicarbonate, sodium carbonate, sodium hydroxide, potassium hydroxide, and the like. Deprotonation of OH occurs on the surface of the substrate (e.g., glass) to produce O - Therefore, low pH acids or high pH bases as mentioned above are used, and this O - is a more reactive nucleophile than OH and therefore increases the binding density of SAMs bearing leaving groups.

[0076] According to an exemplary embodiment, the formulation for the anti-fingerprint coating comprising an alkylsilane, an OH-POSS, or a mixture thereof, and an aqueous base, as described herein above, may be deposited by any suitable deposition technique known to one of skill in the art.

[0077] The present disclosure also provides a glass, ceramic or metal oxide substrate with a fingerprint invisible coating that can be obtained by a method according to one of the above exemplary embodiments, the coating comprising an alkylsilane and an OH-POSS material in an aqueous base or acid, i.e. consisting essentially or exclusively of a fingerprint invisible layer, the surface of which has a surface roughness of more than 5 nm and which is impregnated with a rare gas of the Ar or He type, N 2 Gas or O 2The substrate is activated by treatment with a plasma of a gas selected from the group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 112, 124, 130, 140, 142, 150, 162, 170, 183, 195, 196, 197, 198, 199, 200, 211, 220, 230, 240,

[0078] In an exemplary embodiment, the substrate is H 2 O, Ar, He and N 2 and at least one gas selected from the group consisting of:

[0079] In an exemplary embodiment, the thickness of the non-visible fingerprint layer is between 10 and 500 nm, and in another exemplary embodiment, the thickness of the non-visible fingerprint layer is between 20 and 100 nm.

[0080] In an exemplary embodiment, the omniphobic layer has an RMS roughness of less than 10 nm. In another exemplary embodiment, the omniphobic layer has an RMS roughness of between 5 and 10 nm.

[0081] A feature of the coating materials disclosed in the exemplary embodiments is their ability to form a coating on a surface having a water contact angle of between 70-90 degrees or 75-85 degrees and a diiodomethane contact angle of between 30-40 degrees.

[0082] In some embodiments, the contacting step further comprises an alkoxysiloxane. In some embodiments, the alkoxysilane is a trialkoxysilylsiloxane. In some embodiments, the dialkylsiloxane is a vinyl terminated dialkylsiloxane represented by the formula (R C O) 3 is formed by contacting a compound of SiH, where R Cis an alkyl group. In some embodiments, the siloxane is an alkyl siloxane. In some embodiments, the alkoxy siloxane is an alkoxy polydimethyl siloxane. In some embodiments, the alkoxy siloxane is a trialkoxysilyl polydimethyl siloxane.

[0083] In exemplary embodiments, the trialkoxysilyl siloxane is formed by reacting a trialkoxysilane with a commercially available siloxane in the presence of a catalyst. Exemplary siloxanes include polydimethylsiloxane available from Gelest. In some embodiments, the catalyst is a platinum catalyst.

[0084] Although only a few exemplary embodiments have been described in detail above, those skilled in the art will readily appreciate that many modifications are possible in the exemplary embodiments without substantially departing from the novel teachings and advantages. The following numbered clauses include contemplated, non-limiting embodiments:

[0085] Clause 1. 1. A fingerprint resistant substrate comprising:

[0086] 1. A method for producing a fingerprint resistant coating comprising the steps of: applying a fingerprint resistant coating formulation to a surface of a substrate;

[0087] The resulting fingerprint resistant surface has a Delta E of less than 2.

[0088] Clause 2. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the fingerprint resistant surface has an initial oil angle of less than about 40° and an initial water angle of greater than about 65°.

[0089] Clause 3. The formulation for the anti-fingerprint coating comprises an alkylsilane of the formula: (R A ) 3 SiR B Including,

[0090] In the formula, each R A are independent, -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 is alkynyl,

[0091] R B is C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 alkynyl, where -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, -OC 2 ~C 6 Alkynyl, C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 Each hydrogen atom in an alkynyl may be independently selected from deuterium, halogen, -OH, -CN, -OR ... 1 , -CO 2 H, -C(O)OR 1 , -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C 6 Alkyl, -S(O)NH(C 1 ~C6 alkyl), -S(O) 2 NH(C 1 ~C 6 alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl) 2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl) 3 and where -N(H)C 1 ~C6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 C 1 ~C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl, and

[0092] R 1 are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6 The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein each hydrogen atom in the alkyl is optionally replaced with a hydroxyl.

[0093] Clause 4. R A Ha-OC 1 ~C 6 The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the alkyl group is an alkyl.

[0094] Clause 5. R B is C 6 ~C 20 Alkyl or C 10 ~C 20 The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the alkyl group is an alkyl group.

[0095] Clause 6. R B is C 6 ~C 20 Alkyl or C 10 ~C 20 Alkyl, C6 ~C 20 Alkyl or C 10 ~C 20 Each hydrogen atom in an alkyl group may be independently selected from halogen, -OH, -CN, -OR, -N, -N- ... 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -PO 3 H 2 is replaced by R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6 The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the alkyl group is an alkyl group.

[0096] Clause 7. 20. The fingerprint resistant substrate of any one of the preceding clauses or combinations thereof, wherein the alkyl silane is selected from the group consisting of (chloroundecyl)(triethoxy)silane, (chloroundecyl)(trimethoxy)silane, (chlorohexyl)(triethoxy)silane, (chlorohexyl)(trimethoxy)silane, 11-(2-methoxyethoxy)undecyltrimethoxysilane, (aminoundecyl)(triethoxy)silane, (aminoundecyl)(trimethoxy)silane, (hydroxydecyl)(triethoxy)silane, (hydroxydecyl)(trimethoxy)silane, (11-undecylinic acid)(triethoxy)silane, (hydroxyheptyl)(triethoxy)silane, (hydroxyundecyl)(triethoxy)silane, and (11-phosphoundecyl)(triethoxy)silane.

[0097] Clause 8. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein said alkyl silane is fluoro-free.

[0098] Clause 9. The formulation for the anti-fingerprint coating has the following formula: [ka] Including,

[0099] In the formula, R is -C 1 ~C 6 Alkyl, -A E -OB F -C G -OD H , or -O-Si(C 1 ~C 6 Alkyl) 3 where A is C 1 ~C 6 alkyl and B is -C 1 ~C 6 alkyl-O-, C is C 1 ~C 6 alkyl and D is C 1 ~C 6 is alkyl, O is oxygen, E, G, and H are each at least 1, F is an integer from 5 to 12, -C 1 ~C 6 Each hydrogen atom in an alkyl group may be independently selected from deuterium, halogen, -OH, -CN, -OR, -N-C, -N-O ... 2 , -OC 1 ~C 6 Alkyl, -NH 2 , -NH(C 1 ~C 6 alkyl), -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C1 ~C 6 Alkyl) 2 , or -OPO 3 is substituted with H, and

[0100] R 2 are independently deuterium, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the alkyl group is an alkyl group.

[0101] Clause 10. R is -A E -OB F -C G -OD H or -O-Si(C 1 ~C 6 Alkyl) 3 2. The fingerprint resistant substrate of claim 1, wherein the substrate is a

[0102] Clause 11. R is -A E -OB F -C G -OD H 2. The fingerprint resistant substrate of claim 1, wherein the substrate is a

[0103] Clause 12. R is -(CH 2 ) 3 O(CH 2 CH 2 O) 9 CH 2 CH 2 OCH 3 2. The fingerprint resistant substrate of claim 1, wherein the substrate is a

[0104] Clause 13. 2. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the fingerprint resistant substrate has a coefficient of friction of less than about 0.2.

[0105] Clause 14. 2. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the fingerprint resistant substrate has a coefficient of friction of less than about 0.13.

[0106] Clause 15. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the substrate comprises at least one material selected from the group consisting of glass, metal oxides, and acrylic polymers.

[0107] Article 16. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the fingerprint resistant substrate has an initial oil angle of at least about less than 50°.

[0108] Clause 17. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the fingerprint resistant substrate has an initial oil angle of at least less than about 45°.

[0109] Article 18. 2. The fingerprint resistant substrate of any one of the preceding clauses or combinations of clauses, wherein the fingerprint resistant substrate has an initial oil angle of less than about 35°.

[0110] Article 19. The fingerprint resistant substrate of any one of the preceding clauses or combination of clauses, wherein the fingerprint resistant substrate has an initial water angle of greater than about 65°.

[0111] Clause 20. The fingerprint-resistant substrate of any one of the preceding clauses or a combination of clauses, wherein the fingerprint-resistant substrate has an initial water angle of about 70° to about 90°.

[0112] Article 21. The fingerprint resistant substrate of any one of the preceding clauses or combination of clauses, wherein the fingerprint resistant substrate is substantially free of fluoride.

[0113] Clause 22. The fingerprint resistant substrate of any one of the preceding clauses or combination of clauses, wherein the Delta E is less than about 0.7.

[0114] Clause 23. A formulation for an anti-fingerprint coating, said formulation comprising:

[0115] Alkylsilanes,

[0116] POSS, and

[0117] solvent A formulation comprising:

[0118] Clause 24. The alkylsilane may be an alkylsilane of the formula: (R A ) 3 SiR B and

[0119] In the formula, each R A are independent, -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 is alkynyl,

[0120] R B is C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 alkynyl, where -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, -OC 2 ~C 6 Alkynyl, C 1 ~C 20 Alkyl, C 2~C 20 Alkenyl, or C 2 ~C 20 Each hydrogen atom in an alkynyl may be independently selected from deuterium, halogen, -OH, -CN, -OR ... 1 , -CO 2 H, -C(O)OR 1 , -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C 6 Alkyl, -S(O)NH(C 1 ~C 6 alkyl), -S(O) 2 NH(C 1 ~C 6 alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl) 2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl) 3 and where -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 C 1 ~C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl, and

[0121] R 1 are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6The compound of clause 23, wherein each hydrogen atom in the alkyl is optionally replaced with a hydroxyl.

[0122] Clause 25. R A Ha-OC 1 ~C 6 A combination of any one or any combination of clauses 23-24, wherein:

[0123] Article 26. R B is C 6 ~C 20 Alkyl or C 10 ~C 20 A combination of any one or any combination of clauses 23 to 25, wherein:

[0124] Article 27. R B is C 6 ~C 20 Alkyl or C 10 ~C 20 Alkyl, C 6 ~C 20 Alkyl or C 10 ~C 20 Each hydrogen atom in an alkyl group may be independently selected from halogen, -OH, -CN, -OR, -N, -N- ... 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -PO 3 H 2 is replaced by R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6A combination of any one or any combination of clauses 23 to 26, wherein:

[0125] Article 28. 28. The formulation of any one or any combination of clauses 23-27, wherein the alkyl silane is selected from the group consisting of (chloroundecyl)(triethoxy)silane, (chloroundecyl)(trimethoxy)silane, (chlorohexyl)(triethoxy)silane, (chlorohexyl)(trimethoxy)silane, 11-(2-methoxyethoxy)undecyltrimethoxysilane, (aminoundecyl)(triethoxy)silane, (aminoundecyl)(trimethoxy)silane, (hydroxydecyl)(triethoxy)silane, (hydroxydecyl)(trimethoxy)silane, (11-undecylinic acid)(triethoxy)silane, (hydroxyheptyl)(triethoxy)silane, (hydroxyundecyl)(triethoxy)silane, and (11-phosphoundecyl)(triethoxy)silane.

[0126] Article 29. The POSS has the formula: [ka] and

[0127] In the formula, R is -C 1 ~C 6 Alkyl, -A E -OB F -C G -OD H , or -O-Si(C 1 ~C 6 Alkyl) 3 where A is C 1 ~C 6 alkyl and B is -C 1 ~C 6 alkyl-O-, C is C 1 ~C 6 alkyl and D is C 1 ~C 6is alkyl, O is oxygen, E, G, and H are each at least 1, F is an integer from 5 to 12, -C 1 ~C 6 Each hydrogen atom in an alkyl group may be independently selected from deuterium, halogen, -OH, -CN, -OR, -N-C, -N-O ... 2 , -OC 1 ~C 6 Alkyl, -NH 2 , -NH(C 1 ~C 6 alkyl), -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -OPO 3 is substituted with H, and

[0128] R 2 are independently deuterium, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 A combination of any one or any combination of clauses 23 to 28, wherein:

[0129] Clause 30. R is -A E -OB F -C G -OD H or -O-Si(C 1 ~C 6 Alkyl) 3A combination of any one or any combination of clauses 23 to 29.

[0130] Article 31. R is -A E -OB F -C G -OD H A combination of any one or any combination of clauses 23 to 30.

[0131] Clause 32. R is -(CH 2 ) 3 O(CH 2 CH 2 O) 9 CH 2 CH 2 OCH 3 A combination of any one or any combination of clauses 23 to 31.

[0132] Clause 33. 33. The formulation of any one or any combination of clauses 23-32, wherein the alkylsilane is present in a concentration of about 1 g / L to about 6 g / L.

[0133] Clause 34. 35. The formulation of any one or any combination of clauses 23-34, wherein the concentration of the alkylsilane is from about 2 g / l to about 5 g / l.

[0134] Clause 35. The formulation of any one or any combination of clauses 23-34, wherein said POSS is present in a concentration of about 50 mg / l to about 500 mg / l.

[0135] Article 36. 36. The formulation of any one or any combination of clauses 23-35, wherein the concentration of said POSS is from about 50 mg / l to about 250 mg / l.

[0136] Clause 37. 37. The formulation of any one or any combination of clauses 23-36, wherein the solvent comprises water, alcohol, or a mixture thereof.

[0137] Article 38. 38. The formulation of any one or any combination of clauses 23-37, wherein said solvent is present at a pH of about 1 to 7.

[0138] Article 39. 39. The formulation of any one or any combination of clauses 23-38, wherein the formulation comprises PDMS.

[0139] Article 40. 40. The formulation of any one or any combination of clauses 23-39, wherein the PDMS is terminated with a trialkoxysilane.

[0140] Article 41. 41. The formulation of any one or any combination of clauses 23-40, wherein said PDMS has a molecular weight of less than about 10,000 Da.

[0141] Article 42. 42. The formulation of any one or any combination of clauses 23-41, wherein the molecular weight of said PDMS is at least 2,000 Da.

[0142] Article 43. 1. A method for forming an resistant fingerprint coating on a substrate, the method comprising:

[0143] applying a fingerprint-resistant coating formulation to a surface of the substrate; and

[0144] curing the fingerprint resistant coating formulation on a surface of the substrate to form a fingerprint resistant coating.

[0145] Clause 44. The formulation for the anti-fingerprint coating comprises an alkylsilane of the formula: (R A )3 SiR B Including,

[0146] In the formula, each R A are independent, -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 is alkynyl,

[0147] R B is C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 alkynyl, where -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, -OC 2 ~C 6 Alkynyl, C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 Each hydrogen atom in an alkynyl may be independently selected from deuterium, halogen, -OH, -CN, -OR ... 1 , -CO 2 H, -C(O)OR 1 , -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C6 Alkyl, -S(O)NH(C 1 ~C 6 alkyl), -S(O) 2 NH(C 1 ~C 6 alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl) 2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl)3 and where -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 C 1 ~C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl, and

[0148] R 1 are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6 The method of clause 43, wherein each hydrogen atom in the alkyl is optionally replaced with a hydroxyl.

[0149] Article 45. 45. The method of any one or combination of clauses 43-44, wherein the anti-fingerprint coating has an initial oil angle of less than about 50°.

[0150] Article 46. 46. ​​The method of any one or any combination of clauses 43-45, wherein the anti-fingerprint coating has an initial oil angle of less than about 45°.

[0151] Article 47. 47. The method of any one or any combination of clauses 43-46, wherein the anti-fingerprint coating has an initial water angle of greater than about 65°.

[0152] Article 48. 48. The method of any one or any combination of clauses 43-47, wherein the anti-fingerprint coating has an initial water angle of about 70° to about 90°.

[0153] Article 49. The method includes the step of: 2 , O 2 49. The method of any one or any combination of clauses 43-48, comprising activating the surface of the substrate by exposing the surface to a plasma of at least one gas selected from the group consisting of:

[0154] Article 50. 50. The method of any one or any combination of clauses 43-49, wherein the applying step is performed by dipping the surface of the substrate into the fingerprint resistant coating formulation, wiping with the formulation, or spraying the formulation onto the surface of the substrate.

[0155] Article 51. 51. The method of any one or any combination of clauses 43-50, wherein the anti-fingerprint coating has a coefficient of friction of less than about 0.2.

[0156] Article 52. 53. The method of any one or any combination of clauses 43-52, wherein the anti-fingerprint coating has a coefficient of friction of less than about 0.13.

[0157] Article 53. R B is halo-substituted n-octyltriethoxysilane or halo-substituted C 1 ~C 6 A substrate, formulation, or method of any of the preceding clauses or a combination of any of the preceding clauses that is not alkyl.

[0158] Article 54. R B is C 1 ~C 20 Alkyl, C 6 ~C20 Alkyl, or C 10 ~C 20 alkyl, where C 1 ~C 20 Alkyl, C 6 ~C 20 Alkyl, or C 10 ~C 20 The substrate, formulation, or method of any of the preceding clauses or any combination of the preceding clauses, wherein each hydrogen atom in the alkyl is optionally substituted. In some embodiments, each hydrogen atom is independently optionally substituted with a halogen, -OH, -CN, -OR 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 where R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6 It is an alkyl.

[0159] Article 55. The substrate, formulation, or method of any of the preceding clauses or any combination of the preceding clauses, wherein the alkylsilane comprises a halogen but does not comprise a fluoro, the alkylsilane does not comprise a PEG group, or both.

[0160] Article 56. The POSS has the formula: [ka] and

[0161] In the formula, R is C 1 ~C 6 Alkyl or -O-Si-(C 1 ~C 6 Alkyl) 3 and at least one C 1 ~C 6 The substrate, formulation, or method of any of the preceding clauses or any combination of the preceding clauses, wherein the alkyl is substituted with at least one hydroxy.

[0162] Article 57. The substrate, formulation, or method of any of the preceding clauses or any combination of the preceding clauses, wherein POSS is not present in said formulation for the fingerprint resistant coating.

[0163] Article 58. A formulation for an anti-fingerprint coating, said formulation comprising an alkylsilane and PDMS.

[0164] Article 59. 59. The formulation of clause 58, wherein the PDMS is terminated with a trialkoxysilane.

[0165] Article 60. 59. The formulation of any one or combination of clauses 58-59, wherein said PDMS has a molecular weight of less than about 10,000 Da.

[0166] Article 61. 61. The formulation of any one or any combination of clauses 58-60, wherein the molecular weight of said PDMS is at least 2,000 Da.

[0167] Article 62. The alkylsilane may be an alkylsilane of the formula: (R A ) 3 SiR B and

[0168] In the formula, each R A are independent, -OC1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 is alkynyl,

[0169] R B is C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 alkynyl, where -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, -OC 2 ~C 6 Alkynyl, C 1 ~C 20 Alkyl, C 2 ~C 20 Alkenyl, or C 2 ~C 20 Each hydrogen atom in an alkynyl may be independently selected from deuterium, halogen, -OH, -CN, -OR ... 1 , -CO 2 H, -C(O)OR 1 , -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C 6 Alkyl, -S(O)NH(C 1 ~C 6 alkyl), -S(O) 2 NH(C 1 ~C 6alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl) 2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl) 3 and where -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC1 ~C 6 Alkyl) 3 C 1 ~C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl, and

[0170] R 1 are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6 A combination of any one or any combination of clauses 58-61, wherein each hydrogen atom in the alkyl is optionally replaced with a hydroxyl.

[0171] Article 63. R B is C 6 ~C 20 Alkyl or C 10 ~C 20 Alkyl, C 6 ~C 20 Alkyl or C 10 ~C 20 Each hydrogen atom in an alkyl group may be independently selected from halogen, -OH, -CN, -OR, -N, -N- ... 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -PO 3 H2 is replaced by R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6 A combination of any one or any combination of clauses 58 to 63, wherein: In addition, the following non-limiting embodiments are provided. 1. 1. A fingerprint resistant substrate comprising: The surface of the substrate is provided with a formulation for an anti-fingerprint coating comprising an alkylsilane of the following formula: (R A ) 3 SiR B In the formula, each R A are independent, -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 is alkynyl, R B is C 11 is alkyl, wherein the surface of the fingerprint resistant substrate has a Delta E of less than 2; The Delta E is calculated based on colorimeter measurements of L, A and B values ​​of a virgin fingerprint resistant substrate and a fingerprinted fingerprint resistant substrate. 2. 2. The fingerprint-resistant substrate according to claim 1, wherein the surface of the fingerprint-resistant substrate has an initial oil angle of less than about 40° and an initial water angle of more than about 65°. 3. Said-OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, -OC 2 ~C 6 Alkynyl or C 11 Each hydrogen atom in an alkyl group may be independently selected from deuterium, halogen, -OH, -CN, -OR, -N-C, -N-O ... 1 , -CO 2 H, -C(O)OR 1, -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C 6 Alkyl, -S(O)NH(C 1 ~C 6 alkyl), -S(O) 2 NH(C 1 ~C 6 alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl) 2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl) 3 and where -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 C 1 ~C 6 Each hydrogen atom in the alkyl is optionally replaced with a hydroxyl, and R 1 are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6 3. The fingerprint resistant substrate according to claim 2, wherein each hydrogen atom in the alkyl is optionally replaced with a hydroxyl. 4. R A Ha-OC 1 ~C 6 4. The fingerprint-resistant substrate according to claim 3, wherein the alkyl group is an alkyl group. 5. Said C 11Each hydrogen atom in an alkyl group may be independently selected from halogen, -OH, -CN, -OR, -N, -N- ... 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -PO 3 H 2 is replaced by R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6 4. The fingerprint-resistant substrate according to claim 3, wherein the alkyl group is an alkyl group. 6. 6. The fingerprint-resistant substrate according to claim 5, wherein the alkyl silane is selected from the group consisting of (chloroundecyl)(triethoxy)silane, (chloroundecyl)(trimethoxy)silane, 11-(2-methoxyethoxy)undecyltrimethoxysilane, (aminoundecyl)(triethoxy)silane, (aminoundecyl)(trimethoxy)silane, (11-undecylinic acid)(triethoxy)silane, (hydroxyundecyl)(triethoxy)silane, and (11-phosphoundecyl)(triethoxy)silane. 7. 2. The fingerprint-resistant substrate according to claim 1, wherein the alkylsilane does not contain fluoro. 8. The formulation for the anti-fingerprint coating comprises a POSS compound of the formula as defined in clause 9. Including, In the formula, R is -C 1 ~C 6 Alkyl, -A E -OB F -C G -OD H , or -O-Si(C 1 ~C 6 Alkyl)3 where A is C 1 ~C 6 alkyl and B is -C 1 ~C 6 alkyl-O-, C is C 1 ~C 6 alkyl and D is C 1 ~C 6 is alkyl, O is oxygen, E, G, and H are each at least 1, F is an integer from 5 to 12, -C 1 ~C 6 Each hydrogen atom in an alkyl group may be independently selected from deuterium, halogen, -OH, -CN, -OR, -N-C, -N-O ... 2 , -OC 1 ~C 6 Alkyl, -NH 2 , -NH(C 1 ~C 6 alkyl), -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -OPO 3 is substituted with H, and R 2 are independently deuterium, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 2. The fingerprint-resistant substrate according to claim 1, wherein the alkyl group is an alkyl group. 9. R is -A E -OB F -C G -ODH or -O-Si(C 1 ~C 6 Alkyl) 3 9. The fingerprint-resistant substrate according to 8 above, 10. R is -A E -OB F -C G -OD H 9. The fingerprint-resistant substrate according to 8 above, 11. R is -(CH 2 ) 3 O(CH 2 CH 2 O) 9 CH 2 CH 2 OCH 3 11. The fingerprint-resistant substrate according to claim 10, 12. 2. The fingerprint-resistant substrate according to claim 1, wherein the substrate comprises at least one material selected from the group consisting of glass, metal oxides, and acrylic polymers. 13. 2. The fingerprint-resistant substrate according to claim 1, wherein the fingerprint-resistant substrate has an initial oil angle of at least about 50°. 14. 2. The fingerprint-resistant substrate according to claim 1, wherein the fingerprint-resistant substrate has an initial oil angle of at least about less than 45°. 15. 2. The fingerprint-resistant substrate according to claim 1, wherein the fingerprint-resistant substrate has an initial oil angle of at least about 35°. 16. 2. The fingerprint-resistant substrate according to claim 1, wherein the fingerprint-resistant substrate has an initial water angle of greater than about 65°. 17. 2. The fingerprint-resistant substrate according to 1 above, wherein the fingerprint-resistant substrate has an initial water angle of about 70° to about 90°. 18. 2. The fingerprint-resistant substrate according to claim 1, wherein the fingerprint-resistant substrate is substantially free of fluoride. 19. 2. The fingerprint resistant substrate according to claim 1, wherein the Delta E is less than about 0.7. 20. 1. A fingerprint resistant substrate comprising: A surface of a substrate is provided with a formulation for a fingerprint resistant coating; The formulation for the anti-fingerprint coating comprises an alkyl silane, the alkylsilane is selected from the group consisting of (chloroundecyl)(triethoxy)silane, (chloroundecyl)(trimethoxy)silane, (chlorohexyl)(triethoxy)silane, (chlorohexyl)(trimethoxy)silane, 11-(2-methoxyethoxy)undecyltrimethoxysilane, (aminoundecyl)(triethoxy)silane, (aminoundecyl)(trimethoxy)silane, (hydroxydecyl)(triethoxy)silane, (hydroxydecyl)(trimethoxy)silane, (11-undecylinic acid)(triethoxy)silane, (hydroxyheptyl)(triethoxy)silane, (hydroxyundecyl)(triethoxy)silane, and (11-phosphoundecyl)(triethoxy)silane; wherein the surface of the fingerprint resistant substrate has a Delta E of less than 2; The Delta E is calculated based on colorimeter measurements of L, A and B values ​​of a virgin fingerprint resistant substrate and a fingerprinted fingerprint resistant substrate. Further non-limiting embodiments are given below. A-1. 1. A fingerprint resistant substrate comprising: The surface of the substrate is provided with a formulation for an anti-fingerprint coating comprising an alkylsilane of the following formula: (R A ) 3 SiR B In the formula, each R A are independent, -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 Alkenyl, or -OC 2 ~C 6 is alkynyl, R B is halogen-substituted C 11 is alkyl, The alkylsilane does not contain fluoro. wherein the surface of the fingerprint resistant substrate has a Delta E of less than 2; The Delta E is calculated using a colorimeter and a black background based on the L, A and B values ​​of a virgin fingerprint resistant substrate and a fingerprinted fingerprint resistant substrate prepared by an operator wiping the operator's nose or forehead with all four fingers of their dominant hand 2-3 times and then immediately tapping the fingerprint resistant substrate with all four fingers with moderate pressure 10 times to obtain 40 fingerprints on the surface of the fingerprinted fingerprint resistant substrate. A-2. The fingerprint-resistant substrate according to A-1, wherein the surface of the fingerprint-resistant substrate has an initial oil angle using diiodomethane of less than 40° and an initial water angle of more than 65°. A-3. Each R A are independently deuterium, halogen, -OH, -CN, -OR 1 , -CO 2 H, -C(O)OR 1 , -C(O)OC 1 ~C 20 -PO 3 H 2 , -C(O)NH 2 , -C(O)NH(C 1 ~C 6 alkyl), -C(O)N(C 1 ~C 6 Alkyl) 2 , -SC 1 ~C 6 Alkyl, -S(O)C 1 ~C 6 Alkyl, -S(O) 2 C 1 ~C 6 Alkyl, -S(O)NH(C 1 ~C 6 alkyl), -S(O) 2 NH(C 1 ~C 6 alkyl), -S(O)N(C 1 ~C 6 Alkyl) 2 , -S(O) 2 N(C 1 ~C 6 Alkyl)2 , -NH 2 , -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(H)C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(R 1 ) C 1 ~C 6 Alkyl-N(R 1 ) C 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 , -N(H)C 1 ~C 6 Alkyl-N(H)C 1 ~C 6 Alkyl-NH 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , -PO 3 H 2 , or -Si(-OC 1 ~C 6 Alkyl) 3 and where -N(H)C 1 ~C 6 Alkyl-OC 1 ~C 6 Alkyl-Si(-OC 1 ~C 6 Alkyl) 3 C 1 ~C 6 The alkyl is substituted with a hydroxyl, and R 1are independently deuterium, C 1 ~C 6 Alkyl, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 alkyl, where C 1 ~C 6 The fingerprint resistant substrate according to A-1, wherein the alkyl is substituted with a hydroxyl. A-4. R A Ha-OC 1 ~C 6 The fingerprint-resistant substrate according to A-1, wherein the alkyl group is an alkyl group. A-5. R B are independently halogen, -OH, -CN, -OR 1 , -CO 2 H, -NH 2 , -NH(C 1 ~C 6 alkyl), -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -PO 3 H 2 is replaced by R 1 are independently deuterium or -C 1 ~C 6 Alkyl-OC 1 ~C 6 The fingerprint-resistant substrate according to A-1, wherein the alkyl group is an alkyl group. A-6. The fingerprint-resistant substrate according to A-1, wherein the alkylsilane is selected from the group consisting of (chloroundecyl)(triethoxy)silane and (chloroundecyl)(trimethoxy)silane. A-7. The formulation for the anti-fingerprint coating has the following formula: [ka] Including, In the formula, R is -C 1 ~C 6 Alkyl, -A E -OB F -C G -OD H , or -O-Si(C 1 ~C 6 Alkyl) 3 where A is C 1 ~C 6 alkyl and B is -C 1 ~C 6 alkyl-O-, C is C 1 ~C 6 alkyl and D is C 1 ~C 6 A-1, wherein A is alkyl, O is oxygen, E, G, and H are each at least 1, and F is an integer from 5 to 12. A-8. Said-C 1 ~C 6 Alkyl is independently selected from deuterium, halogen, -OH, -CN, -OR 2 , -OC 1 ~C 6 Alkyl, -NH 2 , -NH(C 1 ~C 6 alkyl), -NH(C 1 ~C 6 alkyl), -N(H)C 1 ~C 6 Alkyl-NH 2 , -N(C 1 ~C 6 Alkyl) 2 , -P(C 1 ~C 6 Alkyl) 2 , -P(O)(C 1 ~C 6 Alkyl) 2 , or -OPO 3 is substituted with H, and R 2are independently deuterium, C 2 ~C 6 Alkenyl, C 2 ~C 6 Alkynyl, C 3 ~C 6 Cycloalkyl, or -C 1 ~C 6 Alkyl-OC 1 ~C 6 The fingerprint-resistant substrate according to A-7, wherein the alkyl group is an alkyl group. A-9. R is -A E -OB F -C G -OD H or -O-Si(C 1 ~C 6 Alkyl) 3 The fingerprint-resistant substrate according to A-7, A-10. R is -A E -OB F -C G -OD H The fingerprint-resistant substrate according to A-7, A-11. R is -(CH 2 ) 3 O(CH 2 CH 2 O) 9 CH 2 CH 2 OCH 3 The fingerprint-resistant substrate according to A-10, A-12. The fingerprint-resistant substrate according to A-1, wherein the substrate comprises at least one material selected from the group consisting of glass, metal oxide, and acrylic polymer. A-13. The fingerprint-resistant substrate according to A-1, wherein the fingerprint-resistant substrate has an initial oil angle using diiodomethane of at least less than 50°. A-14. The fingerprint-resistant substrate according to A-1, wherein the fingerprint-resistant substrate has an initial oil angle using diiodomethane of at least less than 45°. A-15. The fingerprint-resistant substrate according to A-1, wherein the fingerprint-resistant substrate has an initial oil angle using diiodomethane of at least less than 35°. A-16. The fingerprint-resistant substrate according to A-1, wherein the fingerprint-resistant substrate has an initial water angle of more than 65°. A-17. The fingerprint-resistant substrate according to A-1, wherein the fingerprint-resistant substrate has an initial water angle of 70° to about 90°. A-18. The fingerprint-resistant substrate according to A-1, wherein the fingerprint-resistant substrate is substantially free of fluoride. A-19. The fingerprint-resistant substrate according to A-1, wherein the Delta E is less than 0.7. A-20. 1. A fingerprint resistant substrate comprising: A surface of a substrate is provided with a formulation for a fingerprint resistant coating; The formulation for the anti-fingerprint coating comprises an alkyl silane, the alkylsilane is selected from the group consisting of (chloroundecyl)(triethoxy)silane, (chloroundecyl)(trimethoxy)silane, (chlorohexyl)(triethoxy)silane, (chlorohexyl)(trimethoxy)silane, 11-(2-methoxyethoxy)undecyltrimethoxysilane, (aminoundecyl)(triethoxy)silane, (aminoundecyl)(trimethoxy)silane, (hydroxydecyl)(triethoxy)silane, (hydroxydecyl)(trimethoxy)silane, (11-undecylinic acid)(triethoxy)silane, (hydroxyheptyl)(triethoxy)silane, (hydroxyundecyl)(triethoxy)silane, and (11-phosphoundecyl)(triethoxy)silane; wherein the surface of the fingerprint resistant substrate has a Delta E of less than 2; The Delta E is calculated using a colorimeter and a black background based on the L, A and B values ​​of a virgin fingerprint resistant substrate and a fingerprinted fingerprint resistant substrate, the fingerprinted fingerprint resistant substrate being prepared by an operator wiping the operator's nose or forehead with all four fingers of their dominant hand 2-3 times, and then immediately tapping the fingerprint resistant substrate with all four fingers with moderate pressure 10 times, thereby applying 40 fingerprints to the surface of the fingerprinted fingerprint resistant substrate. Anti-fingerprint substrate. EXAMPLES

[0172] The following examples are presented for illustrative purposes only. Parts and percentages shown in such examples are by weight unless otherwise stated. OH-POSS was purchased from Sigma Aldrich.

[0173] Example 1

[0174] Activation plasma conditions:

[0175] According to an exemplary embodiment, the substrate was treated with an activated gas in the form of a plasma. This step can be carried out in a variety of vacuum or atmospheric chambers. For example, a parallel plate RF reactor can be used. The treatment results in a chemical modification of the substrate, but no physical changes such as morphology. The gases used are preferably Ar, He, N 2 , or O 2 , or a mixture of two or more of these gases. Typically, the pressure used was adjusted between 50 and 500 mTorr, the power between 10 and 200 W, and the activation time was about 1 minute to about 5 minutes, usually less than 1 minute.

[0176] Example 2

[0177] Testing and Analysis

[0178] For the tests, the control had no surface treatment and the test specimen had a fingerprint-invisible coating on a plasma-activated glass specimen. The test specimens prepared as described above were evaluated according to the following test methods.

[0179] Initial contact angle measurements were performed using water and diiodomethane, which provide a reference index for the omniphobicity of the grafted substrates.

[0180] The transmittance test was measured as a percentage of light irradiance according to ASTM D1003.

[0181] The grafted coating was subjected to ASTM D4060 at a translation speed of 50 cycles / min and a rotation speed of 6 rpm for a 1.5 cm 2 Abrasion resistance was obtained by measuring the residual contact angle of water on the specimen after it had been abraded using an abrasive disk of CS10 hardness with a load of 250 g on an area of ​​1000 mm. If the contact angle remains above 80° after 1500 cycles, the specimen is satisfactory in the test.

[0182] Chemical resistance tests were performed at room temperature in strong acid (pH 2) and base (sodium hydroxide, pH 11) environments. Specimens are considered satisfactory in the test if the water contact angle remains above 90 degrees after 8 hours.

[0183] Example 3

[0184] contact angle measurement

[0185] The fingerprint non-visible coating was estimated by contact angle measurements with various fluids such as water and diiodomethane. The results obtained for the test specimens prepared according to the above procedure are shown in Table 1 below.

[0186] [Table 1]

[0187] Table 2 below shows the contact angle measurements for alkylsilanes (AS) without the OH-POSS coating.

[0188] [Table 2]

[0189] Example 4

[0190] Fingerprint resistant and invisible

[0191] Fingerprint characteristics were measured by placing the fingerprint between two substrates, coated (left) and uncoated (right), in each of the photographs in Figure 1A and B of a fingerprint placed between two pieces of Gorilla® tempered glass. The coated substrate on the left had no fingerprint, while the uncoated substrate on the right has a clear fingerprint smudge.

[0192] Example 5

[0193] Chemical resistance

[0194] Generally, hydrophobic coatings are vulnerable to hydrolysis after exposure to harsh solvent conditions, resulting in coating failure. The purpose of this test was to measure the chemical resistance of a substrate with a fingerprint-free coating formed according to an exemplary method of the present disclosure. The test consisted of rubbing the sample 10 times with a cloth soaked in isopropanol alcohol (IPA). As can be seen in the chart of FIG. 2, the test results of the chemical resistance test before and after IPA rubbing showed that the water contact angle and diiodomethane contact angle of the coating were not affected by solvent exposure.

[0195] Example 6

[0196] Abrasion resistance

[0197] The abrasion resistance of the resulting omniphobic substrate was measured according to ASTM D4060: 1.5 cm at a translation speed of 50 cycles / min and a rotation speed of 6 rpm. 2 Tests were performed on the specimens using an abrasive disk of CS-10 hardness with a load of 250 g on the area of ​​1500 cycles. If the water contact angle remained above 70 degrees after 1500 cycles, the specimens were considered satisfactory in said test. The tests were performed for 1,500, 3,000 or 4,500 cycles. As shown in Figure 3, which illustrates the results of the mechanical abrasion (ASTM D4060 Taber) test, 500 g weight load (CS-10 wheel) for 1,500 cycles, it can be seen that the abrasion resistance of the specimens was sufficient and there was no slight deterioration in the water contact angle.

[0198] A 500 g weight was placed on a CS-10 hardness abrasive disc. The abrasion resistance of the specimen showed slight degradation. After 1,500 cycles, the water contact angle exceeded the cut-off limits for water and diiodomethane (70° and 30°).

[0199] Example 7

[0200] Triethoxyundecylinic acid silane synthesis [ka]

[0201] Undecylenic acid (1.0 g, 5.4 mmol, 1 equiv.) and triethoxysilane (1.07 g, 6.5 mmol, 1.2 equiv.) in 3 ml of anhydrous toluene were placed in a 25 ml round bottom flask equipped with a stir bar. The reaction mixture was purged under argon for 30 minutes. 0.01 ml of Pt(dvs) (~2% Pt in xylene, available from Aldrich) was added dropwise to the reaction mixture. The reaction mixture was slowly heated to 80°C and left stirring at 80°C overnight. Toluene and excess triethoxysilane were evaporated on a rotary evaporator. The resulting organic oil was filtered through Celite refined oil. Yield: 1.1 g. % yield: 58%.

[0202] Example 8

[0203] Triethoxyundecylhydroxysilane Synthesis [ka]

[0204] 10-Undecen-1-ol (10 g, 0.059 mol, 1 eq.) and triethoxysilane (11.6 g, 0.07 mol, 1.2 eq.) in 30 ml of anhydrous toluene were placed in a 100 ml round bottom flask equipped with a stir bar. The reaction mixture was purged under argon for 30 minutes. 0.1 ml of Pt(dvs) (~2% Pt in xylene, available from Aldrich) was added dropwise to the reaction mixture. The reaction mixture was slowly heated to 80°C and left stirring at 80°C overnight. Toluene and excess triethoxysilane were evaporated on a rotary evaporator. The resulting organic oil was filtered through celite to give a brown oil. Yield: 6.8 g. % yield: 34%.

[0205] Example 9

[0206] Triethoxyhexylhydroxysilane Synthesis [ka]

[0207] 5-Hexen-1-ol (5 g, 0.05 mol, 1 eq.) and triethoxysilane (9.84 g, 0.06 mol, 1.2 eq.) in 15 ml of anhydrous toluene were placed in a 100 ml round bottom flask equipped with a stir bar. The reaction mixture was purged under argon for 30 minutes. 0.05 ml of Pt(dvs) (~2% Pt in xylene, available from Aldrich) was added dropwise to the reaction mixture. The reaction mixture was slowly heated to 80°C and left stirring at 80°C overnight. Toluene and excess triethoxysilane were evaporated on a rotary evaporator. The resulting organic oil was filtered through Celite to give a colorless oil which turned into a shiny solid over time. Yield: 6.15 g. % Yield: 44%.

[0208] Example 10

[0209] Phosphonoundecyltriethoxysilane Synthesis [ka]

[0210] 11-Phosphonoundecyl acrylate (0.75 g, 2.45 mmol, 1 equiv.) and triethoxysilane (0.48 g, 2.9 mmol, 1.2 equiv.) in 2 ml of anhydrous toluene were placed in a 25 ml round bottom flask equipped with a stir bar. The reaction mixture was purged under argon for 30 minutes. 5 μl of Pt(dvs) (approximately 2% Pt in xylene, available from Aldrich) was added dropwise to the reaction mixture. The reaction mixture was slowly heated to 80° C. and left stirring at 80° C. overnight. Toluene and excess triethoxysilane were evaporated on a rotary evaporator. The resulting organic oil was filtered through Celite to give a colorless oil. Yield: 0.6 g. % yield: 52%.

[0211] Example 11

[0212] compound

[0213] A formulation for the anti-fingerprint coating was prepared by mixing alkylsilanes and POSS in a solvent, as described in Table 3 below. The OH-POSS was prepared as described in Example 1 of US Patent Application Publication No. 2017 / 0349785, which is incorporated by reference in its entirety, or purchased from Sigma Aldrich (catalog number 594180). The solvent was 20% ethanol, 70% water, and 10% aqueous 5M NH 4 The formulation was a mixture of 11-aminoundecyltriethoxysilane (CAS#120876315) and 11-aminoundecyltrimethoxysilane (CAS#17948-05-9) listed was purchased from Gelest. The chlorohexyltrimethoxysilane (CAS#1145666-63-2) listed was purchased from Gelest. The N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane (CAS#121772-92-7) listed was purchased from Gelest. The 11-aminoundecyltriethoxysilane (CAS#116821-45-5) listed was purchased from Gelest. The listed PEG silane (CAS#1384163-86-3) was purchased from Gelest and the listed hydroxydecyltriethoxysilane was prepared according to Example 12. The listed N-(6-aminohexyl)aminomethyltriethoxysilane (CAS#15129-36-9) was purchased from Gelest.

[0214] The formulation was sprayed onto the corona / plasma treated surface until the surface was thoroughly wetted. Excess formulation was wiped off. The treated surface was cured in an oven at 120° C. for approximately 10 minutes. Initial oil angle was determined as described in Example 2 above. Abrasion resistance was measured according to Example 6. Abrasion resistance results are shown in Table 4.

[0215] [Table 3]

[0216] [Table 4]

[0217] Example 12

[0218] Abrasion resistance

[0219] Coating formulations were prepared by mixing silane and POSS in a solvent as described in Example 11 above. The silane was chloroundecyltriethoxysilane (CAS#120876315) purchased from Gelest. Mono-OH POSS was prepared according to Example 1 of US Patent Application Publication No. 2017 / 0349785, which is incorporated herein by reference in its entirety. The Mono-PEG POSS (CAS#1838163-04-4) was purchased from Hybrid Plastics. Sigma OH-POSS (CAS#288290-32-4) was purchased from Sigma Aldrich.

[0220] [Table 5]

[0221] Example 13

[0222] Delta E

[0223] To measure fingerprint performance, the LAB value of unused glass on a black background is measured using a Konica Minolta colorimeter, ideally using a black card stock or a black OLED display. The operator is then asked to wipe the nose or forehead, which are the oiliest parts of the body, with all four fingers of their dominant hand 2-3 times. They then immediately tap the glass with all four fingers with moderate pressure 10 times. This results in 40 fingerprints on the surface. They then measure the LAB value using the colorimeter and use those values ​​to calculate a Delta E based on the unused glass and the glass with the fingerprints. The lower the Delta E, the less visible the fingerprints will be. The operator then takes a piece of jeans material, ideally a standardized LEVIS 401 jeans material, and wipes the glass along the same area twice to wipe off those fingerprints. The operator then calculates the Delta E compared to unused glass to measure the cleanability of the coating. The closer the value is to 0, the less visible the fingerprints will be.

[0224] The test was performed on surfaces prepared as described in Example 12. The results are shown in Table 6.

[0225] [Table 6]

[0226] Example 14

[0227] Synthesis of PDMS-TEOS

[0228] Monovinyl-terminated PDMS(5k) (10 g, 0.002 mol, 1 eq.; available from Gelest) and triethoxysilane (0.5 g, 0.003 mol, 1.5 eq.) were dissolved in 5 ml of anhydrous toluene and purged under Ar for 30 min. 0.1 mL of Pt(dvs) (~2% Pt in xylene, available from Aldrich) was added to the reaction mixture and brought to 90°C. The reaction mixture was stirred at 90°C for ~60 h. The reaction mixture was cooled to room temperature and then directly filtered through celite. Yield: 7.9 g.

[0229] Example 15

[0230] Synthesis of PDMS-TEOS

[0231] 3-Isocyanatopropyltriethoxysilane (0.197 g, 0.8 mmol, 2 eq., available from Gelest) was combined with PDMS bisamino (1 g, 0.4 mmol, 1 eq., available from Sigma Aldrich, CAS number 106214-84-0). The resulting mixture was stirred for up to 4 h. Yield 1.1 g.

[0232] Example 16

[0233] compound

[0234] OH-POSS (final concentration 100 mg / mL) was combined with chloroundecylsilane (final concentration 3.75 mg / mL) in ethanol and PDMS-TEOS (final concentration 0.375 mg / mL) from Example 15. The resulting solution was applied to the surface as described above.

[0235] The coefficient of friction of the coated surfaces was measured using an MDX-02 coefficient of friction tester. The coefficient of friction of the surface coated with the formulation containing PDMS-TEOS was measured to be about 0.116. The coefficient of friction of the surface coated with the formulation without PDMS-TEOS was measured to be about 0.168.

[0236] Although the methods, apparatus and systems have been described in connection with specific embodiments, the scope thereof is not intended to be limited to the particular embodiments described, as the embodiments herein are intended in all respects to be illustrative and not restrictive.

[0237] Unless otherwise expressly stated, it is in no way intended that any method described herein be construed as requiring that its steps be performed in a particular order. Thus, unless a method claim actually recites the order in which its steps are to be followed, or the claim or specification specifically states that the steps are limited to a particular order, no order is intended to be inferred in any respect.

[0238] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0239] Ranges may be expressed herein as from "about" one particular value, and / or to "about" another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values ​​are expressed as approximations, it will be understood that by use of "about" the antecedent, the particular value forms another embodiment. It will be further understood that the endpoints of each of the ranges are both significant in relation to the other endpoint, and independent of the other endpoint.

[0240] "Optional" or "optionally" means that the subsequently described event or circumstance may or may not occur, and the description includes instances where said event or circumstance occurs and instances where it does not occur.

[0241] Throughout the description and claims of this specification, the word "comprise" and variations of said word such as "comprising" and "comprises" mean "including, but not limited to," and are not intended to exclude, for example, other additives, ingredients, integers, or steps. "Exemplary" means "one example of" and is not intended to convey an indication of a preferred or ideal embodiment. "For example" or "specifically" are used for purposes of illustration rather than limitation.

[0242] Components that can be used to implement the disclosed methods, devices and systems are disclosed. These and other components are disclosed herein, and when combinations, subsets, interactions, groups, etc. of these components are disclosed, specific references to each of the various individual and collective combinations and permutations of these are not explicitly disclosed, but each is specifically considered and described herein for all methods, devices and systems. This applies to all aspects of this application, including, but not limited to, the steps of the disclosed methods. Thus, when there are a variety of additional steps that can be implemented, it is understood that each of these additional steps can be implemented in any particular embodiment or combination of embodiments of the disclosed methods.

[0243] It should further be noted that any patents, applications and publications mentioned herein are incorporated by reference in their entirety.

[0244] Although only a few exemplary embodiments have been described in detail above, those skilled in the art will readily appreciate that many modifications are possible in the exemplary embodiments without substantially departing from the novel teachings and advantages thereof, and all such modifications are therefore intended to be included within the scope of the present disclosure, as defined in the following claims.

Claims

[Claim 1] 1. A fingerprint resistant substrate comprising: The surface of the substrate is provided with a formulation for an anti-fingerprint coating comprising POSS and an alkylsilane of the following formula: (R A ) 3 SiR B In the formula, each R A are independently -OC 1 ~C 6 Alkyl, -OC 2 ~C 6 alkenyl, or -OC 2 ~C 6 is alkynyl, R B is halogen-substituted C 11 is alkyl, The alkylsilane does not contain fluoro. wherein the surface of the fingerprint resistant substrate has a Delta E of less than 2; The Delta E is calculated using a colorimeter and a black background based on the L, A and B values ​​of a virgin fingerprint resistant substrate and a fingerprinted fingerprint resistant substrate prepared by an operator applying 40 fingerprints to the surface of the fingerprinted fingerprint resistant substrate by wiping the operator's nose or forehead with all four fingers of their dominant hand 2-3 times and then immediately tapping the fingerprint resistant substrate 10 times with all four fingers using moderate pressure.