Improved separator for reinforced flooded battery, battery, and related method

A microporous separator with reduced torsion and shish-kebab morphology, using high oil absorption silica and ultra-high molecular weight polyethylene, addresses the high internal resistance issue in lead-acid batteries, enhancing CCA and extending battery life.

JP2024153741AInactive Publication Date: 2024-10-29DARAMIC LLC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024118624
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-04-08
Filing Date
2024-07-24
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lead-acid batteries face challenges in achieving high cold cranking amps (CCA) due to high internal resistance, which can be addressed by developing improved battery separators with reduced electrical resistance and increased porosity.

Method used

The development of a microporous separator with reduced torsion, increased porosity, and a shish-kebab morphology, incorporating high oil absorption silica and ultra-high molecular weight polyethylene, along with performance-enhancing additives, to enhance ion transport and reduce electrical resistance.

Benefits of technology

The improved separator leads to a significant reduction in electrical resistance, increasing CCA by up to 30% and extending battery life, while maintaining mechanical strength and reducing water loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153741000022
    Figure 2024153741000022
  • Figure 2024153741000023
    Figure 2024153741000023
  • Figure 2024153741000024
    Figure 2024153741000024
Patent Text Reader

Abstract

To provide a new battery separator that reduces internal resistance and increases CCA in a reinforced flooded battery.SOLUTION: A separator for a lead acid battery including a polyolefin microporous membrane, the polyolefin microporous membrane includes polyethylene, preferably ultra-high molecular weight polyethylene, a particulate filler, and a treatment plasticizer, the particulate filler is present in an amount of 40% or more by weight, the polyethylene includes a shish-kebab formed polymer including a plurality of extended chain crystals (shish formation) and a plurality of folded chain crystals (kebab formation), the average repeat or period of the kebab formation is between 1 nm and 150 nm, preferably less than 120 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 319,959, filed April 8, 2016.

[0002] According to at least selected embodiments, the present disclosure or invention is directed to new or improved separators, battery separators, enhanced flooded battery separators, batteries, cells, and / or methods of making and / or using such separators, battery separators, enhanced flooded battery separators, cells, batteries, systems, methods and / or vehicles using the same. According to at least some embodiments, the present disclosure or invention is directed to new or improved battery separators, flooded lead acid battery separators, or enhanced flooded lead acid battery separators for "SLI" (starting, lighting, ignition) batteries, flooded batteries for deep cycle applications, and "EFB" (enhanced flooded batteries), and / or improved methods of making and / or using such improved separators, cells, batteries, systems, vehicles, or any combination thereof. According to at least some embodiments, the present disclosure or invention is directed to improved separators for enhanced flooded batteries and / or improved methods of making and / or using batteries having such improved separators. According to at least selected embodiments, the present disclosure or invention is directed to separators, and in particular separators for enhanced flooded batteries having reduced electrical resistance and / or improved CCA (cold cranking amps). Further disclosed herein are methods, systems, and battery separators for providing extended battery life, reduced water loss, reduced internal resistance, increased wettability, reduced acid stratification, improved acid diffusion, improved CCA, improved uniformity, or combinations thereof, in at least enhanced flooded batteries.According to at least certain embodiments, the present disclosure or invention is directed to an improved separator for reinforced flooded batteries, the separator comprising a performance enhancing additive or coating, increased porosity, increased void volume, comprising amorphous silica, high oil absorption silica, high silanol group silica, silica with an OH to Si ratio of 21:100 to 35:100, reduced electrical resistance, comprising a polyolefin microporous membrane comprising a shish-kebab structure or morphology, comprising a particulate filler such as ultra-high molecular weight polyethylene in an amount of 40% or more by weight of the membrane and polymer, having a shish-kebab formation with extended chain crystals (shish formation) and folded chain crystals (kebab formation), the average repeat period of the kebab formation is between 1 nm and 150 nm, reduced sheet thickness, reduced twist, etc. [Background technology]

[0003] To meet the expanding power needs of idle start-stop applications, enhanced flooded batteries ("EFB") and absorbent glassmat ("AGM") batteries have been developed. EFB systems have an architecture similar to that of traditional flooded lead-acid batteries, with the positive and / or negative electrodes surrounded by a microporous separator and immersed in a liquid electrolyte. AGM systems, on the other hand, do not contain free liquid electrolyte. Instead, the electrolyte is absorbed into a glass fiber mat, which is layered on top of the electrodes. Historically, AGM systems have been associated with increased discharge power, improved cycle life, and increased CCA compared to flooded battery systems. However, AGM systems are expensive to manufacture. The EFB system has a significantly higher charge / discharge ratio and is highly sensitive to overcharging. This makes the EFB system still attractive as a mobile and / or stationary power option in some markets and applications. Applications for such power sources and energy storage are varied and include, for example, flat-plate batteries, tubular batteries, vehicle SLI, and hybrid electric vehicle ISS applications; deep cycle applications; batteries for golf cars or golf carts and e-rickshaws; batteries operating in a partial state of charge ("PSOC"); inverter batteries; and storage batteries for renewable energy sources.

[0004] An EFB system may include one or more battery separators that separate the positive electrode from the negative electrode in a lead-acid battery cell. Battery separators can have two main functions. First, the battery separator must physically hold the positive electrode away from the negative electrode to prevent electrical current from flowing between the two electrodes. Second, the battery separator must allow ion diffusion between the positive and negative electrodes with as little resistance as possible to generate electrical current. Although battery separators can be made from many different materials, these two opposing functions are well served by battery separators composed of porous nonconductors. In this structure, the pores contribute to ion diffusion between the electrodes, and the nonconducting polymer network prevents electronic shorting. Summary of the Invention [Problem to be solved by the invention]

[0005] EFB batteries with increased discharge rate and CCA (cold cranking amperes (amps)) could replace AGM batteries. CCA is known to be correlated to the internal resistance of the battery. Therefore, lowering the internal resistance of a reinforced flooded battery would be expected to increase the CCA rating. Thus, there is a need for new battery separators and / or battery technologies that address and overcome the issues encountered in current lead acid battery systems, particularly those that reduce the internal resistance and increase the CCA in reinforced flooded batteries. [Means for solving the problem]

[0006] According to at least selected embodiments, the present disclosure or invention may address the above problems or needs. According to at least some objectives, the present disclosure or invention may provide improved separators and / or batteries that overcome the above-mentioned problems, for example, by providing an enhanced flooded battery with reduced internal electrical resistance and increased CCA.

[0007] According to at least selected embodiments, the present disclosure or invention may address the above problems or needs and / or provide new or improved separators and / or reinforced flooded batteries. According to at least selected embodiments, the present disclosure or invention is directed to new or improved separators, battery separators, reinforced flooded battery separators, batteries, cells, and / or methods of making and / or using such separators, battery separators, reinforced flooded battery separators, cells, and / or batteries. In accordance with at least some embodiments, the present disclosure or invention is directed to new or improved battery separators, flooded lead acid batteries, or enhanced flooded battery separators, and / or improved methods of making and / or using such improved separators, cells, batteries, systems, and the like, for high power demand batteries, such as automotive applications, idle start stop ("ISS") batteries, uninterrupted power supply ("UPS"), or valve regulated lead acid ("VRLA") batteries, and / or batteries with high CCA demands. In accordance with at least some embodiments, the present disclosure or invention is directed to improved separators for enhanced flooded batteries, and / or improved methods of using batteries having such improved separators. Further disclosed herein is at least one embodiment of a novel or improved battery separator, flooded lead acid battery, or enhanced flooded battery separator, and / or improved methods of making and / or using such improved separators, cells, batteries, systems, and the like. In accordance with at least certain embodiments, the present disclosure or invention is directed to improved separators for reinforced flooded batteries, which have reduced electrical resistance, include performance enhancing additives or coatings, include improved fillers, increase porosity, reduce twisting, reduce thickness, reduce oil content, increase wettability, increase acid diffusion, etc.

[0008] According to at least one embodiment, a microporous separator is provided with reduced tortuosity. Tortuosity refers to the degree of curvature / rotation over the length of the pores. Thus, a microporous separator with reduced tortuosity shortens the path that ions travel through the separator, thereby reducing electrical resistance. Microporous separators according to such embodiments can have reduced thickness, increased pore size, increased pore interconnection, and / or increased hole opening.

[0009] According to at least some selected embodiments, microporous separators with increased porosity or different pore structures with insignificant porosity from known separators and / or reduced thickness are provided. Microporous separators with increased porosity, increased void volume, reduced tortuosity, and / or reduced thickness allow ions to pass through more quickly, thus reducing electrical resistance. Such reduced thickness results in a reduced overall weight of the battery separator, which in turn reduces the weight of the reinforced flooded battery in which the separator is used, which in turn allows for a reduced overall weight of the vehicle in which the reinforced flooded battery is used. Alternatively, such reduced thickness can provide more space for positive active material ("PAM") or negative active material ("NAM") in the reinforced flooded battery in which the separator is used.

[0010] In accordance with at least some selected embodiments, a microporous separator is provided that has increased wettability (in water or acid) that allows easier access for electrolyte ionic species, resulting in easier passage through the separator and reduced electrical resistance.

[0011] In accordance with at least one embodiment, a microporous separator is provided that has reduced final oil content, which also facilitates reduced ER (electrical resistance) in an enhanced flooded battery or system.

[0012] The separator may include an improved filler with increased friability, which may increase the porosity, pore size, internal pore surface area, wettability, and / or surface area of ​​the separator. In some embodiments, the improved filler has higher structural morphology and / or smaller particle size and / or a different amount of silanol groups than previously known fillers, and / or is more hydroxylated than previously known fillers. The improved filler may absorb more oil during separator formation and / or allow for greater amounts of process oil to be incorporated without shrinking or compressing as the oil is removed after extrusion. The filler may also reduce what is called the hydration sphere of electrolyte ions, enhancing ion transport through the membrane, again reducing the overall electrical resistance or ER of the battery, such as an enhanced flooded battery or system.

[0013] The filler or fillers may include various species (e.g., polar species such as metals) that increase ionic diffusion and facilitate the flow of electrolytes and ions through the separator. When the paratators are used in flooded batteries, such as enhanced flooded batteries, they cause a reduction in the overall electrical resistance.

[0014] The microporous separator further includes a new and improved pore morphology and / or a new and improved fiber morphology such that when the separator is used in a flooded lead acid battery, the separator contributes to a significant reduction in electrical resistance in the flooded lead acid battery. Such improved pore morphology and / or fiber morphology results in a separator in which the pores and / or fibers approximate a shish kebab (or shish kebab) type morphology. Another way to describe the new and improved pore shapes and structures is a textured fiber morphology in which there are silica nodes or nodes of silica in a kebab type formation on the polymer fibers (sometimes referred to as shish) in the battery separator. Furthermore, in some embodiments, the silica and pore structure of a separator according to the present invention can be described as a skeletal or vertebral or spinal structure, with the silica nodes on the polymer kebabs along the polymer fibers looking like vertebrae or discs ("kebabs") and sometimes oriented approximately perpendicular to an elongated central projection or fiber (extended chain polymer crystal) ("shishi") approximating a spine shape.

[0015] In some examples, improved batteries including improved separators having improved pore morphology and / or fiber morphology exhibit a 20% reduction in electrical resistance ("ER"), in some examples a 25% reduction, in some examples a 30% reduction, and in some examples greater than a 30% reduction (which can reduce the battery internal resistance), while such separators balance and maintain other important desirable mechanical properties of lead acid battery separators. Additionally, in some embodiments, the separators described herein have novel and / or improved pore geometries that allow more electrolyte to flow through and / or fill the pores and / or voids than known separators.

[0016] The present disclosure further provides improved enhanced flooded lead-acid batteries including one or more improved battery separators for enhanced flooded batteries. The separators combine the desirable features of reduced acid stratification, reduced voltage drop (or increased voltage drop durability) and increased CCA for the battery. In some examples, the CCA increase is greater than 8%, or greater than 9%, or in some embodiments, greater than 10%, or greater than 15%. Such improved separators result in enhanced flooded batteries whose performance is comparable to or better than that of AGM batteries. Such low electrical resistance separators can also be processed to result in enhanced flooded lead-acid batteries with reduced water loss.

[0017] The separator may include one or more performance enhancing additives, such as surfactants, along with other additives or chemicals, residual oils, and fillers, which may inhibit oxidation of the separator and / or further facilitate ion transport through the membrane, thereby contributing to the overall reduced electrical resistance of the enhanced flooded batteries described herein.

[0018] The separator for the lead acid battery described herein may include a polyolefin microporous membrane, which includes a polymer such as polyethylene, such as ultra-high molecular weight polyethylene, a particulate filler, and a processing plasticizer (optionally with one or more additional additives or chemicals). The polyolefin microporous membrane may include a particulate filler in an amount of 40% or more by weight of the membrane. The ultra-high molecular weight polyethylene may also include a shish-kebab-formed polymer, which includes a plurality of extended chain crystals (shish formation) and a plurality of folded chain crystals (kebab formation). The average repetition or period of the kebab formation is 1 nm to 150 nm (at least in the rib-side portion of the separator), preferably 10 nm to 120 nm, and more preferably 20 nm to less than 100 nm.

[0019] The average repetition or period of kebab formation is calculated according to the following rules: After metal deposition, the surface of the polyolefin microporous membrane is observed using a scanning electron microscope ("SEM"), and then an image of the surface is taken, for example, at a magnification of 30,000 or 50,000 times and an accelerating voltage of 1.0 kV. Show at least three regions in which the shish-kebab formation extends continuously for a length of at least 0.5 μm or more within the same visual area of ​​the SEM image. Then calculate the kebab periodicity of each shown region. The kebab period is determined by calculating the average of the repetition periods by Fourier transformation of the density profile (contrast profile) obtained by projecting the shish-kebab formation perpendicular to the shish formation in each of the indicated regions. Analyze the images using common analysis tools, for example MATLAB® (R2013a). Among the spectral profiles obtained after the Fourier transformation, the spectrum detected in the short wavelength region is considered as noise. Such noise is mainly caused by deformation of the contrast profile. The contrast profile obtained with the separator according to the invention is expected to generate a square wave (not a sine wave). Furthermore, if the contrast profile is a square wave, the profile after the Fourier transformation will be a sine function, so that in addition to the main peak indicating the true kebab period, multiple peaks will be generated in the short wavelength region. Such peaks in the short wavelength region can be detected as noise.

[0020] In some embodiments, the separators for the lead acid batteries described herein include a filler selected from the group consisting of silica, precipitated silica, fused silica, and precipitated amorphous silica. 29 The molar ratio of OH groups to Si groups in the filler as measured by Si-NMR is in the range of 21:100 to 35:100, in some embodiments 23:100 to 31:100, in some embodiments 25:100 to 29:100, and in some preferred embodiments 27:100 or greater.

[0021] The silanol groups change the silica structure from a crystalline structure to an amorphous structure because the relatively rigid covalent bond network of Si-O partially disappears. Amorphous silicas such as Si(-O-Si)2(-OH)2 and Si(-O-Si)3(-OH) have many distortions, which can act as various oil absorption points. Thus, if the amount of silanol groups (Si-OH) of the silica increases, the oil absorption will be higher. Furthermore, the separators described herein may have increased hydrophilicity and / or increased void volume and / or some agglomerates surrounded by large voids when they contain silicas with a higher amount of silanol groups and / or hydroxyl groups than silicas used with known lead acid battery separators. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 includes a diagram of the pore size distribution of one embodiment of a low ER separator of the present invention compared to a conventional separator. [Diagram 2] Included is an illustration of the oxidative stability of one embodiment of the present invention (sometimes referred to as the "EFS" (Enhanced Flooded Separator™) product) compared to conventional separators. In a battery overcharge test, after 1000 hours, the separator according to the present invention is less brittle and therefore exhibits higher elongation than the control separator. [Diagram 3] Included are plots of electrical resistance data for separators prepared with various silica fillers, each of which has a different specific oil absorption. In some embodiments of the present invention, the improved separator is formed using a silica having a specific oil absorption value of about 175-350 ml / 100 g, in some embodiments about 200-350 ml / 100 g, in some embodiments about 250-350 ml / 100 g, and in some other embodiments about 260-320 ml / 100 g, although other oil absorption values ​​are possible. [Figure 4] A plot of electrical resistance data for separators prepared with various process oils is included, each with a different aniline point. [Diagram 5]1 includes a plot of acid stratification (%) versus Hg porosity (%) for separators according to the present invention. [Figure 6] Includes a plot of ER boiling versus backweb thickness. [Figure 7] FIG. 7 includes an SEM image of one embodiment of a separator of the present invention at 50,000 times magnification. [Figure 8A] Figure 8A is an SEM image of the same separator at 10,000x magnification. In the SEM, a shish-kebab type morphology or textured fiber type structure is observed, with some cavities or pores left by the pores and silica structure. The polymer webbing is significantly reduced (in some cases, there is almost no polymer webbing) and the thick fibers or threads of hydrophobic polymer are significantly reduced (in some cases, there are few or no thick fibers or threads of hydrophobic polymer). [Figure 8B] FIG. 8B is an SEM image of the same separator at 10,000x magnification. [Figure 9A] 9A-9C include plots of pore size distribution for separator embodiments: Figure 9A is for a control separator; [Figure 9B] 9B includes a diagram of the pore size distribution of the separator embodiment. FIG. 9B is of a low ER separator with desirable mechanical properties according to one embodiment of the present invention. FIG. 9B can also be considered as part of FIG. [Figure 10] 10 includes a comparison of various pore size measurements of a separator according to the present invention with a conventional separator. In FIG. 10, the difference in bubble flow rate is significant because it measures the porosity of the separator and its ability to functionally transport ions through the separator. While the average and minimum pore sizes are not significantly different, the maximum pore size is larger for the separator according to the present invention, and the bubble flow rate is significantly higher for the separator according to the present invention. [Figure 11A] 4A-4C are porometry data and diagrams of liquid flow through a separator according to one embodiment of the present invention; [Figure 11B] FIG. 11B shows liquid flow through a control separator compared to FIG. 11A. [Figure 12A] Includes two SEMs at two different magnifications of a control separator made by Daramic, LLC. In these SEMs, relatively thick fibers or threads of hydrophobic polymer are observed. [Figure 12B] Includes two SEMs at two different magnifications of a control separator made by Daramic, LLC. In these SEMs, relatively thick fibers or threads of hydrophobic polymer are observed. [Figure 13A] Two SEMs at two different magnifications of another control separator made by Daramic, LLC are included. In these SEMs, areas that appear to be polymer networks can be observed. [Figure 13B] Two SEMs at two different magnifications of another control separator made by Daramic, LLC are included. In these SEMs, areas that appear to be polymer networks can be observed. [Figure 14A] 1 includes an SEM of a separator formed according to one embodiment of the present invention, where one or more shish-kebab polymers are observed to form. [Figure 14B] We show how the Fourier transform of the contrast profile (lower spectrum in FIG. 14B) helps determine the repetition or periodicity of the separator's shish kebab formation (see the shish kebab formation in the upper part of FIG. 14B). [Figure 15A] 1 includes an SEM of the inventive separator of Example 1. [Figure 15B] FIG. 15B includes a graph of Welch power spectral density estimation showing the results of FTIR spectral testing performed on the three shish kebab regions (numbered 1, 2, and 3) shown and marked in FIG. 15A. [Figure 15C] FIG. 15B includes a graph of Welch power spectral density estimation showing the results of FTIR spectral testing performed on the three shish kebab regions (numbered 1, 2, and 3) shown and marked in FIG. 15A. [Figure 15D]15A includes graphs of Welch power spectral density estimates showing the results of FTIR spectral testing performed on the three shish kebab regions (numbered 1, 2, and 3) shown and marked in Figure 15A. The x-axis of the graphs in Figures 15B through 15D is normalized frequency (xπ radians / sample) and the y-axis of these graphs is power / frequency (dB / radians / sample). [Figure 16A] 15A-15D, but showing a separator according to the present invention according to a second embodiment. [Figure 16B] 15A-15D, but showing a separator according to the present invention according to a second embodiment. [Figure 16C] 15A-15D, but showing a separator according to the present invention according to a second embodiment. [Figure 16D] 15A-15D, but showing a separator according to the present invention according to a second embodiment. [Figure 17A] 15A-15D, but showing a separator according to the present invention according to a third embodiment. [Figure 17B] 15A-15D, but showing a separator according to the present invention according to a third embodiment. [Figure 17C] 15A-15D, but showing a separator according to the present invention according to a third embodiment. [Figure 17D] 15A-15D, but showing a separator according to the present invention according to a third embodiment. [Figure 18A] 15A-15D, but showing a separator according to the present invention according to Example 4. FIG. [Figure 18B] 15A-15D, but showing a separator according to the present invention according to Example 4. FIG. [Figure 18C] 15A-15D, but showing a separator according to the present invention according to Example 4. FIG. [Figure 18D] 15A-15D, but showing a separator according to the present invention according to Example 4. FIG. [Figure 19A] 15A-15D, but showing a separator according to the present invention according to Example 5. FIG. [Figure 19B] 15A-15D, but showing a separator according to the present invention according to Example 5. FIG. [Figure 19C] 15A-15D, but showing a separator according to the present invention according to Example 5. FIG. [Figure 19D] 15A-15D, but showing a separator according to the present invention according to Example 5. FIG. [Figure 20A] 15A to 15D, but showing the separator of Comparative Example 1 (CE1). [Figure 20B] 15A to 15D, but showing the separator of Comparative Example 1 (CE1). [Figure 20C] 15A to 15D, but showing the separator of Comparative Example 1 (CE1). [Figure 20D] 15A to 15D, but showing the separator of Comparative Example 1 (CE1). [Figure 21A] 15A and 15B, but showing the separator of Comparative Example 2. [Figure 21B] 15A and 15B, but showing the separator of Comparative Example 2. [Figure 22] 1 is an SEM of the separator of Comparative Example 3. [Diagram 23] 29Si-NMR spectra of Comparative Example 4 and Example 1 are included. [Figure 24] 23 includes deconvolution of the component peaks of the spectra of FIG. 23 to determine the Q2:Q3:Q4 ratios in the CE4 and Example 1 separator samples, respectively. [Diagram 25] 1 shows the tip used to pierce the test separator. [Figure 26A] FIG. 1 is a schematic representation of an extension test sample. [Figure 26B] 1 shows a sample holder for extension testing. [Figure 27] 1 shows a nuclear magnetic resonance ("NMR") tube in which a separator sample is immersed in DO. [Figure 28] Diffusion coefficients at -10°C and Δ=20 ms for H2SO4 solution only, a reference separator, an embodiment of the invention separator, and an AGM separator are shown. [Figure 29] The pore size distribution of an embodiment of the invention is shown in comparison to a commercially available separator. [Diagram 30] 1 shows the pore size distribution of a separator according to an embodiment of the invention. [Diagram 31] 1 is a chart showing the dispersion of a new silica filler in an embodiment of the invention separator and a standard silica in a commercially available separator. [Diagram 32] 1 shows standard silica sizes and silica sizes used in embodiments of the present invention. [Diagram 33] The size of the novel silica before and after ultrasonic treatment is shown. [Diagram 34] The silica size before and after sonication is shown, showing the particle size distribution of the novel silica and the standard silica before sonication, after 30 seconds of sonication, and after 60 seconds of sonication. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] composition The separator of the present invention is preferably a porous membrane made of natural or synthetic materials such as polyolefin, polyethylene, polypropylene, phenolic resin, PVC, rubber, synthetic wood pulp (SWP), glass fiber, synthetic fiber, cellulose fiber, or combinations thereof, and more preferably a microporous membrane made of one or more thermoplastic polymers. The thermoplastic polymer can in principle include all acid-resistant thermoplastic materials suitable for use in lead-acid batteries. Suitable thermoplastic polymers include polyvinyl and polyolefins. Polyvinyl includes, for example, polyvinyl chloride (PVC). Polyolefins include, for example, polyethylene, such as ultrahigh molecular weight polyethylene (UHMWPE), and polypropylene. One suitable embodiment may include UHMWPE and a filler. In general, suitable separators can be made by mixing the filler, the thermoplastic polymer, and the processing plasticizer in an extruder. The processing plasticizer can be a process oil, such as petroleum, paraffin-based mineral oil, mineral oil, and any combination thereof.

[0024] The microporous separator is preferably made of a polyolefin, such as polypropylene, ethylene-butene copolymers, and preferably polyethylene, more preferably high molecular weight polyethylene, i.e. polyethylene with a molecular weight of at least 600,000, more preferably ultra-high molecular weight polyethylene, i.e. polyethylene with a molecular weight of at least 1,000,000, in particular 4,000,000, most preferably 5 to 8,000,000 (measured by viscosity measurements and calculated by Margolie's equation) and having a standard load melt index of approximately zero (as specified in ASTM D 1238 (condition E) using a standard load of 2,160 g). The viscosity number is greater than or equal to 600 ml / g, preferably greater than or equal to 1,000 ml / g, more preferably greater than or equal to 2,000 ml / g, and most preferably greater than or equal to 3,000 ml / g (determined in a solution of 0.02 g of polyolefin in 100 g of decalin at 130° C.).

[0025] According to at least one embodiment, the separator is comprised of ultra-high molecular weight polyethylene (UHMWPE) mixed with process oil and fillers. According to at least one other embodiment, the separator is comprised of ultra-high molecular weight polyethylene (UHMWPE) mixed with process oil, additives, and fillers.

[0026] According to some selected embodiments, the separator can be prepared by combining about 5-15% polymer, in some instances about 10% polymer, about 10-60% filler, in some instances about 30% filler, and about 30-80% process oil, in some instances about 60% process oil, by weight. In other embodiments, the filler content is reduced and the oil content is increased, for example, greater than about 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, or 70% by weight. The filler:polymer (by weight) ratio can be, for example, about 2:1, 2.5:1, 3:1, 3.5:1, 4.0:1, 4.5:1, 5.0:1, 5.5:1, or 6:1 (or between about these specified ranges). The ratio of filler:polymer (by weight) can be from about 1.5:1 to about 6:1, in some instances from about 2:1 to 6:1, from about 2:1 to 5:1, from about 2:1 to 4:1, and in some instances from about 2:1 to about 3:1.

[0027] Additive Incorporation and Backweb Thickness The mixture may also contain small amounts of other additives or chemicals common in the separator art, such as surfactants, wetting agents, colorants, antistatic additives, antioxidants, and the like, and any combination thereof. The mixture may be extruded into a flat sheet form or into a sheet having ribs or other protrusions on one or both sides. After the separator is extruded, it may be further compressed using a mechanical press or a calender stack or rolls. The press or calender may be engraved to impart ribs, grooves, sawtooth, serrated ribs, embossments, and the like to the microporous separator.

[0028] According to some selected embodiments, the separator has a backweb thickness of less than about 150 μm, 140 μm, 130 μm, 120 μm, 110 μm, 100 μm, 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, or 40 μm. In some selected embodiments, the backweb thickness is about 100-500 μm, about 150-400 μm, about 150-350 μm, about 150-300 μm, or about 175-300 μm, or about 200-300 μm. In some embodiments, the backweb thickness is about 250 μm. In other embodiments, the backweb thickness is about 200 μm. In yet other embodiments, the backweb thickness is about 400 μm. In some selected embodiments, the separator backweb thickness is about 200±35 μm, 200-250 μm, 50-150 μm, 75-150 μm, 75-125 μm, 75-100 μm, 100-125 μm, or 50-100 μm.

[0029] rib In some embodiments, the separator can have ribs on at least one surface. The ribs can facilitate processing during folding and cutting steps, reduce acid stratification, and / or promote acid mixing and increase acid diffusion throughout the battery system. In accordance with at least another object of the present invention, a porous membrane is provided having cross-ribs. Cross-ribs are ribs that extend in a direction other than the vertical edges of the separator. In some cases, the cross-ribs are perpendicular to or extend in a direction other than the direction in which the main ribs of the separator extend. In some embodiments, the separator can have cross-ribs that extend in a direction other than the direction in which the main ribs of the separator extend. The transverse ribs are present on the separator even if the separator does not include main ribs. In some embodiments, the main ribs are disposed on one side of the microporous membrane separator and the transverse ribs (sometimes referred to as negative transverse ribs) are disposed on another side of the microporous membrane separator. In some embodiments of the invention, the main ribs or major ribs have a height in the range of about 5 μm to about 1.5 mm. In some embodiments of the invention, the rib height of the transverse ribs can be at least 0.005 mm, 0.01 mm, 0.025 mm, 0.05 mm, 0.075 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, or 1.0 mm. The height of the separator's lateral ribs can be 0.005-1.0 mm, 0.01-0.5 mm, 0.025 mm-0.5 mm, 0.05 mm-0.5 mm, 0.075 mm-0.5 mm, 0.1-0.5 mm, 0.2-0.4 mm, 0.3-0.5 mm, 0.4-0.5 mm.

[0030] filling material The separator can contain a filler with high structural morphology. Exemplary fillers can include dry fine silica, precipitated silica, amorphous silica, very friable silica, alumina, talc, fish meal, fish bone meal, and the like, and any combination thereof. In some preferred embodiments, the filler is one or more silicas. High structural morphology refers to an increased surface area. The filler can have a large surface area, for example a surface area of ​​100 m2.2 / g, 110m 2 / g, 120m 2 / g, 130m 2 / g, 140m 2 / g, 150m 2 / g, 160m 2 / g, 170m 2 / g, 180m 2 / g, 190m 2 / g, 200m 2 / g, 210m 2 / g, 220m 2 / g, 230m 2 / g, 240m 2 / g, or 250m 2 In some embodiments, the surface area of ​​the filler (e.g., silica) is 100 to 300 m 2 / g, 125-275m 2 / g, 150-250m 2 / g, or preferably 170 to 220 m 2 / g. Surface area can be assessed using TriStar3000™ for multi-point BET nitrogen surface area. High structural morphology allows fillers to retain more oil during the manufacturing process. For example, high structural morphology fillers can have high levels of oil absorption, such as about 150ml / 100g, 175ml / 100g, 200ml / 100g, 225ml / 100g, 250ml / 100g, 275ml / 100g, 300ml / 100g, 325ml / 100g, or 350ml / 100g. In some embodiments, the filler (e.g., silica) may have an oil absorption of 200-500 ml / 100 g, 200-400 ml / 100 g, 225-375 ml / 100 g, 225-350 ml / 100 g, 225-325 ml / 100 g, preferably 250-300 ml / 100 g. In some examples, a silica filler with an oil absorption of 266 ml / 100 g is used. Such a silica filler has a moisture content of 5.1% and a BET surface area of ​​178 m 2 / g, average particle size is 23 μm, 230 mesh sieve residue is 0.1%, and bulk density is 135 g / L.

[0031] Silica, having a relatively high level of oil absorption and a relatively high level of affinity for mineral oil, is desirably dispersible in a mixture of polyolefin (such as polyethylene) and mineral oil when forming a lead acid battery separator of the type shown herein. In the past, some separators have suffered from poor dispersibility due to silica agglomeration when large amounts of silica are used to make such separators or membranes. In at least some of the separators of the present invention shown and described herein, the polyolefin, such as polyethylene, forms a shish kebab structure as the molten polyolefin cools, since there are few silica agglomerates or clumps that inhibit the molecular motion of the polyolefin. This all contributes to improved ion permeability in the separator membrane that is produced. The formation of a shish kebab structure or morphology means that mechanical strength is maintained and thus improved, while producing a separator with a low overall ER.

[0032] In some selected embodiments, the filler has an average particle size of 25 μm or less, and in some examples, 22 μm, 20 μm, 18 μm, 15 μm, or 15 μm or less. In some examples, the filler particles (such as silica) have an average particle size of 15-25 μm. The particle size of the silica filler contributes to the oil absorption of the silica and / or the surface area of ​​the silica filler.

[0033] In some preferred embodiments, the silica used to make the separator of the present invention has an increased amount or number of surface silanol groups (surface hydroxyl groups) compared to silica fillers previously used to make lead acid battery separators. For example, silica fillers that may be used with some preferred embodiments herein may be silica fillers that have at least 10%, at least 15%, at least 20%, at least 25%, at least 30%, or at least 35% more silanol and / or hydroxyl surface groups than known silica fillers used to make known polyolefin lead acid battery separators.

[0034] The ratio of silanol groups (Si-OH) to elemental silicon (Si), (Si-OH) / Si, can be measured, for example, as follows.

[0035] 1. Freeze-grind a polyolefin microporous membrane (some inventive membranes contain various oil-absorbing silicas according to the invention) and subject the powdered sample to solid-state nuclear magnetic resonance spectroscopy ( 29 Prepare for 100 s NMR (Si-NMR).

[0036] 2. For powder samples 29 Perform Si-NMR and observe the spectrum containing Si spectrum intensity directly bonded to hydroxyl groups (spectra: Q2 and Q3) and Si spectrum intensity directly bonded to oxygen atoms (spectra: Q4). The molecular structure of each NMR peak spectrum can be expressed as follows: ·Q2: (SiO)2-Si*-(OH)2: has two hydroxyl groups Q3: (SiO)3-Si*-(OH): has one hydroxyl group Q4: (SiO)4-Si*: All Si bonds are SiO Here, Si* is identified as an element by NMR observation.

[0037] 3. Observation 29 The conditions for Si-NMR were as follows: ·Equipment: Bruker BioSpin Abance 500 ·Resonance frequency: 99.36MHz Sample size: 250mg NMR tube: diameter 7m Observation method: DD / MAS Pulse width: 45 degrees Repeat time: 100 seconds Scans: 800 Magic angle rotation: 5,000Hz Chemical shift reference: Silicone rubber (-22.43 ppm) (external reference)

[0038] 4. Numerically separate the spectrum peaks and calculate the area ratio of each peak belonging to Q2, Q3, and Q4. Then, based on these ratios, calculate the molar ratio of hydroxyl groups (-OH) directly bonded to Si. The conditions for numerical peak separation are as follows: ·Compatible area: -80~-130ppm Initial peak top: -93 ppm in Q2, -101 ppm in Q3, -111 ppm in Q4 Initial half-width: 400Hz for Q2, 350Hz for Q3, 450Hz for Q4 Gaussian function ratio: Initial 80%, during fitting 70-100%

[0039] 5. The peak area ratios (sum of 100) of Q2, Q3, and Q4 are calculated based on each peak obtained by fitting. The NMR peak areas correspond to the number of molecules of each silicate bond structure (so that in the Q4 NMR peak, there are four Si-O-Si bonds in the silicate structure; in the Q3 NMR peak, there are three Si-O-Si bonds and one Si-OH bond in the silicate structure; in the Q2 NMR peak, there are two Si-O-Si bonds and two Si-OH bonds in the silicate structure). Therefore, the number of hydroxyl groups (-OH) of Q2, Q3, and Q4, respectively, is multiplied by 2, 1, and 0. These three results are summed. The sum indicates the molar ratio of hydroxyl groups (-OH) directly bonded to Si.

[0040] In selected embodiments, the use of the fillers described above allows for a higher percentage of process oil to be used during the extrusion step. Higher initial oil absorption results in higher porosity or higher void volume, since the porous structure of the separator is formed in part by oil removal after extrusion. Although the process oil is an integral part of the extrusion step, the oil is a non-conductive element of the separator. Residual oil in the separator protects the separator from oxidation if it comes into contact with the positive electrode. In the manufacture of conventional separators, the exact amount of oil in the processing step can be controlled. Generally speaking, conventional separators are manufactured with 50-70% process oil by weight, in some embodiments 55-65%, in some embodiments 60-65%, and in some embodiments about 62% by weight. It is known that reducing the oil below about 59% can result in burning due to increased friction against the extruder components. However, increasing the oil significantly above the prescribed amount can result in shrinkage during the drying stage, leading to dimensional instability. Previous attempts to increase the oil content have resulted in pore shrinkage or condensation during oil removal, but in separators prepared as disclosed herein, minimal, if any, shrinkage and condensation is observed during oil removal. Thus, porosity can be increased without compromising pore size and dimensional stability, thereby reducing electrical resistance.

[0041] In some selected embodiments, the use of the fillers described above allows for a reduction in the final oil concentration in the finished separator. Since oil is a non-conductor, a reduction in the oil content can increase the ionic conductivity of the separator and help reduce the ER of the separator. Thus, separators with reduced final oil content can have high efficiency. In some selected embodiments, separators are provided with a final process oil content of less than 20% (by weight), for example, about 14% to 20%, and in some specific embodiments, less than 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, or 5%.

[0042] Friability In some selected embodiments, the filler can be alumina, talc, silica, or a combination thereof. In some embodiments, the filler can be precipitated silica, and in some embodiments, the precipitated silica is amorphous silica. In some embodiments, it is preferred to use silica aggregates and / or agglomerates that allow fine dispersion of the filler throughout the separator to reduce tortuosity and electrical resistance. In some preferred embodiments, the filler (e.g., silica) is characterized by a high level of friability. Good friability improves the dispersion of the filler throughout the polymer during extrusion of the microporous membrane, thus increasing the porosity and therefore the overall ionic conductivity through the separator.

[0043] Friability is the tendency of silica particles or materials (aggregates or clumps) to break down into smaller, more dispersible particles, It can be measured as the ability, tendency, or propensity to break into pieces or elements. As shown on the left side of Figure 34, the new silica is more friable (broken into smaller pieces after 30 and 60 seconds of sonication) than standard silica. For example, the new silica had a 50% volume particle size of 24.90um at 0 seconds of sonication, 5.17um at 30 seconds, and 0.49um at 60 seconds. Thus, the size (diameter) of the 50% volume silica particles was reduced by more than 50% at 30 seconds of sonication and by more than 75% at 60 seconds. Thus, one suitable definition of "high friability" is that the average size (diameter) of silica particles is reduced by at least 50% at 30 seconds of sonication (or in the treatment of a resin-silica mixture to form a membrane) and that the average size (diameter) is reduced by at least 75% at 60 seconds of sonication. In at least some embodiments, it may be preferred to use more friable silica, and moreover, it may be preferred to use silica that is friable and multi-modal, such as bi-modal or tri-modal in friability. Referring to FIG. 34, the standard silica appears monomodal in friability or particle size distribution, while the novel silica appears more friable and bimodal (2 peaks) at 30 seconds of sonication and trimodal (3 peaks) at 60 seconds of sonication. Such a friable multimodal particle size silica or silicas can provide improved membrane and separator properties.

[0044] The use of fillers having one or more of the above characteristics allows for the production of separators with higher final porosity. The separators disclosed herein can have a final porosity of 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, or 70%. Porosity can be measured by gas absorption. Porosity can be measured by BS-TE-2060.

[0045] In some selected embodiments, the microporous separator can have a higher percentage of larger pores while maintaining an average pore size of about 1 μm, 0.9 μm, 0.8 μm, 0.7 μm, 0.6 μm, 0.5 μm, or 0.1 μm or less.

[0046] According to at least one embodiment, the separator is comprised of a polyethylene, such as ultra-high molecular weight polyethylene ("UHMWPE"), mixed with a process oil and a filler, as well as any desired additives. According to at least one other embodiment, the separator is comprised of an ultra-high molecular weight polyethylene ("UHMWPE"), mixed with a process oil and talc. According to at least one other embodiment, the separator is comprised of an UHMWPE, mixed with a process oil and silica. The silica may be, for example, a precipitated silica, such as an amorphous precipitated silica. The additives may be applied to the separator by one or more of the techniques described above.

[0047] In addition to reduced electrical resistance and increased CCA, the preferred separators are designed to provide other benefits. For assembly, the separators pass easily through processing equipment and are therefore efficiently manufactured. To prevent short circuits during high speed assembly and later in life, the separators have superior puncture strength and oxidation resistance compared to standard PE separators. Combined with reduced electrical resistance and increased CCA, battery manufacturers may see improved sustained electrical performance in batteries using these new separators.

[0048] Electrical resistance In some select embodiments, the disclosed separators exhibit reduced electrical resistance, e.g., electrical resistance of about 200 mΩ·cm 2 , 180mΩ·cm 2 , 160mΩ·cm 2 , 140mΩ·cm 2 , 120mΩ·cm 2 , 100mΩ·cm 2 , 80mΩ·cm 2 , 60mΩ·cm2 , 50mΩ·cm 2 , 40mΩ·cm 2 , 30mΩ·cm 2 ,also is 20 mΩ cm 2 In various embodiments, the separators described herein exhibit an ER reduction of 20% or more compared to known separators of the same thickness, e.g., 60 mΩ·cm 2 Thus, a separator of the same thickness according to the present invention would have an ER of about 48 mΩ·cm. 2 has an ER value of less than

[0049] To test a sample separator for ER test evaluation according to the present invention, it must first be prepared. To do this, the sample separator is preferably immersed in a demineralized water bath, then the water is boiled and the separator is removed after 10 minutes in the boiling demineralized water bath. After removal, the separator is shaken to remove excess water and then placed in a sulfuric acid bath at 27°C ± 1°C and with a specific gravity of 1.280. The separator is allowed to soak in the sulfuric acid bath for 20 minutes. At this point the separator is ready to be tested for electrical resistance.

[0050] stab resistance In some selected embodiments, the exemplary separator can be characterized by an increased puncture resistance, such as about 9N or more, 9.5N or more, 10N or more, 10.5N or more, 11N or more, 11.5N or more, 12N or more, 12.5N or more, 13N or more, 13.5N or more, 14N or more, 14.5N or more, 15N or more, 15.5N or more, 16N or more, 16.5N or more, 17N or more, 17.5N or more, 18N or more, 18.5N or more, 19N or more, 19.5N or more, or 20N or more. In some embodiments, the exemplary separator can be preferably defined by a puncture resistance of about 9N to 20N or more, or more preferably about 12N to 20N or more.

[0051] Puncture resistance can be measured as the force required to pierce a porous membrane with a tip 100 as generally shown in Figure 25. The piercing base on which the porous membrane is supported as the tip 100 pierces the membrane can be roughly described as a base with a linear hole of 6.5 mm diameter and 10 mm deep. The tip travel limit can be approximately 4 mm to 8 mm below the piercing base surface. The piercing tip 100 moves linearly into the membrane at a speed of approximately 5 mm / s.

[0052] additives The separator may include one or more performance enhancing additives, such as surfactants, wetting agents, colorants, antistatic additives, antioxidants, and the like, and any combination thereof. The performance enhancing additive may preferably be a surfactant. Some suitable surfactants are non-ionic, while other suitable surfactants are anionic. The use of these particular suitable surfactants in conjunction with the separator of the present invention described herein can provide a further improved separator that, when used in a lead-acid battery, can provide the lead-acid battery with reduced water loss. Suitable surfactants include surfactants such as alkyl sulfates; alkylaryl sulfonates; alkylphenol-alkylene oxide adducts; soaps; alkyl-naphthalene-sulfonates; one or more sulfosuccinates, such as anionic sulfosuccinates; dialkyl esters of sulfosuccinate salts; quaternary amines; block copolymers of ethylene oxide and propylene oxide; and mono- and di-alkyl phosphate ester salts. The additives can be non-ionic surfactants such as polyol fatty acid esters, polyethoxylated esters, polyethoxylated alcohols, alkyl polysaccharides such as alkyl polyglycosides and blends thereof, amine ethoxylates, sorbitan fatty acid ester ethoxylates, organosilicon based surfactants, ethylene vinyl acetate terpolymers, ethoxylated alkylaryl phosphate esters, and sucrose fatty acid esters.

[0053] The battery separator can be provided with one or more additives, one or more chemicals, and / or one or more fillers in a variety of ways. The one or more additives can be applied to the separator, for example, once the separator is complete (e.g., after extraction of the plasticizer (e.g., process oil)). and / or can be added to the mixture used to finally extrude the separator. According to some preferred embodiments, the additive or a solution of the additive is applied to the surface of the separator. This variant is particularly suitable for applying additives that are not heat stable and that dissolve in the solvent used in the subsequent extraction. Particularly suitable as solvents for the additives according to the invention are low molecular weight alcohols such as methanol and ethanol, as well as mixtures of these alcohols with water. The application can be on the side of the separator facing the negative electrode, on the side facing the positive electrode, or on both sides. The application can also be carried out during the extraction of the pore former in the solvent bath.

[0054] Some embodiments of the separator according to the present invention do not incorporate additives such as non-ionic or anionic surfactants. In other embodiments, the additive (non-ionic or anionic surfactant) is present in an amount of at least 0.5 g / m 2 , 1.0g / m 2 , 1.5g / m 2 , 2.0g / m 2 , 2.5g / m 2 , 3.0g / m 2 , 3.5g / m 2 , 4.0g / m 2 , 4.5g / m 2 , 5.0g / m 2 , 5.5g / m 2 , 6.0g / m 2 , 6.5g / m 2 , 7.0g / m 2 , 7.5g / m 2 , 8.0g / m 2 , 8.5g / m 2 , 9.0g / m 2 , 9.5g / m 2 , or 10.0 g / m 2The additive may be present in a density of 0.5 to 10 g / m 2 , 1.0~10.0g / m 2 , 1.5~10.0g / m 2 , 2.0~10.0g / m 2 , 2.5~10.0g / m 2 , 3.0~10.0g / m 2 , 3.5~10.0g / m 2 , 4.0~10.0g / m 2 , 4.5~10.0g / m 2 , 5.0~10.0g / m 2 , 5.5~10.0g / m 2 , 6.0~10.0g / m 2 , 6.5~10.0g / m 2 , 7.0~10.0g / m 2 , 7.5~10.0g / m 2 , 5.0~10.5g / m 2 , 5.0~11.0g / m 2 , 5.0~12.0g / m 2 , or 5.0 to 15.0 g / m 2 The density of the separator may be 0.1 to 1.0.

[0055] Application can also be performed by immersing the battery separator in the additive or in a solution of the additive (solvent bath addition) and then optionally removing the solvent, for example by drying. In this way, application of the additive can be combined with an extraction, which is often applied, for example, during separator production. Other suitable methods are spraying the additive onto the surface of the separator, or roller or curtain coating the additive onto the surface of the separator.

[0056] Another suitable option is to mix one or more additives into the mixture of thermoplastic polymer, optionally filler, and other chemicals or additives used in producing the battery separator, and then form the homogenous mixture containing the additive into a web-shaped material.

[0057] In some embodiments, the exemplary separator may include one or more performance enhancing additives, which may be surfactants, wetting agents, colorants, antistatic additives, UV protection additives, antioxidants, and the like, and any combination thereof.

[0058] Some suitable surfactants are nonionic, while other suitable surfactants are anionic. The additive can be a single surfactant or a mixture of two or more surfactants, such as two or more anionic surfactants, two or more nonionic surfactants, or a mixture of at least one ionic surfactant and at least one nonionic surfactant. The suitable surfactant selected can have an HLB value of less than 6, and preferably less than 3. The use of these particular suitable surfactants in combination with the separator of the present invention described herein can provide a further improved separator that, when used in a lead-acid battery, can provide the lead-acid battery with reduced water loss, reduced antimony poisoning, improved cycling, reduced float current, reduced floating potential, and the like, or any combination thereof. Suitable surfactants include alkyl sulfates; alkylaryl sulfonates; alkylphenol-alkylene oxide adducts; soaps; alkyl-naphthalene-sulfates; and alkyl-phenyl ... The additives include surfactants such as sulfonate salts; one or more sulfosuccinates, such as anionic sulfosuccinates; dialkyl esters of sulfosuccinate salts; amino compounds (primary, secondary, or tertiary amines; quaternary amines; block copolymers of ethylene oxide and propylene oxide; various polyethylene oxides; and mono- and di-alkyl phosphate ester salts. The additives may include non-ionic surfactants such as polyol fatty acid esters, polyethoxylate esters, polyethoxylate alcohols, alkyl polysaccharides such as alkyl polyglycosides and blends thereof, amine ethoxylates, sorbitan fatty acid ester ethoxylates, organosilicon-based surfactants, ethylene vinyl acetate terpolymers, ethoxylated alkylaryl phosphate esters, and sucrose fatty acid esters.

[0059] In some embodiments described herein, the separator of the present invention is added with lesser amounts of anionic or ionic surfactants, or little or no surfactants. In such cases, the ER of the separator of the present invention may be slightly higher than that of the separator of the present invention that contains more anionic or nonionic surfactants. However, the combination of the lowered ER relative to known separators combined with the desirable feature of reduced total organic carbon (due to the reduced amount of surfactant) can produce the desired inventive separator according to such embodiments.

[0060] In some embodiments, the additive can be represented by a compound of formula (I).

[0061]

number

[0062] ·R is a non-aromatic hydrocarbon radical having 10 to 4200 carbon atoms, preferably 13 to 4200 carbon atoms, which can be interrupted by an oxygen atom. ·R 1 is H, -(CH2) k COOM X+ 1 / X , or -(CH2) k -SO3M X+ 1 / X and preferably H, where k=1 or 2. M is an alkali metal or alkaline earth metal ion, H + , or NH4 + Here, all of the variables M are simultaneously H + does not have the meaning of n=0 or 1. m = 0 or an integer between 10 and 1400. x=1 or 2.

[0063] The ratio of oxygen atoms to carbon atoms in the compound according to formula (I) is in the range of 1:1.5 to 1:30, and m and n cannot simultaneously be 0. However, preferably, only one of the variables n and m is different from 0.

[0064] By non-aromatic hydrocarbon radicals is meant radicals which do not contain aromatic groups or which themselves represent 1. The hydrocarbon radicals may be interrupted by oxygen atoms, i.e. they may contain one or more ether groups.

[0065] R is preferably a linear or branched aliphatic hydrocarbon radical which may be interrupted by an oxygen atom. Saturated non-bridged hydrocarbon radicals are especially highly preferred.

[0066] The use of compounds of formula (I) in the formation of battery separators can effectively protect such separators against oxidative breakdown.

[0067] Preferred is a battery separator comprising a compound according to formula (I), wherein: R has 10 to 180 carbon atoms, preferably 12 to 75 carbon atoms, and particularly preferably 14 to 4 0, which may be interrupted by 1 to 60, preferably 1 to 20, very preferably 1 to 8 oxygen atoms. Particularly preferably, this is a hydrocarbon radical of the formula R 2 -[(OC2H4) p (OC3H6) q ]-, where: ·R 2 is an alkyl radical having 10 to 30, preferably 12 to 25, particularly preferably 14 to 20 carbon atoms. P is an integer of 0 to 30, preferably 0 to 10, and particularly preferably 0 to 4. q is an integer of 0 to 30, preferably 0 to 10, and particularly preferably 0 to 4. Compounds in which the sum of p and q is 0 to 10, particularly 0 to 4, are particularly preferred. ·n=1. ·m=0.

[0068] formula R 2 -[(OC2H4) p (OC3H6) q It should be understood that ]- also includes compounds in which the order of the groups in the brackets is different from the order shown. For example, compounds in which the (OC2H4) and (OC3H6) groups are interchanged to form the radical in the brackets are suitable according to the invention.

[0069] R 2 However, additives which are linear or branched alkyl radicals having 10 to 20, preferably 14 to 18, carbon atoms have proven to be particularly advantageous. OC2H4 preferably represents OCH2CH2 and OC3H6 represents OCH(CH3)2 and / or OCH2CH2CH3.

[0070] As suitable additives, it can be mentioned in particular alcohols (p=q=0, m=0), particularly preferred primary alcohols, fatty alcohol ethoxylates (p=1-4, q=0), fatty alcohol propoxylates (p=0, q=1-4) and fatty alcohol alkoxylates (p=1-2, q=1-4) ethoxylates of primary alcohols. Fatty alcohol alkoxylates are obtainable, for example, by reaction of the corresponding alcohols with ethylene oxide or propylene oxide.

[0071] Additives of the type m=0, which are insoluble or only partially soluble in water and sulfuric acid, have proven to be particularly advantageous.

[0072] Also suitable are additives containing a compound according to formula (I) wherein ·R is an alkane radical having 20 to 4200, preferably 50 to 750, particularly preferably 80 to 225, carbon atoms. M is an alkali metal or alkaline earth metal ion, H + , or NH4 + In particular, Li + , Na + , and K + , or H +where all of the variables M are simultaneously H + does not have the meaning of ·n=0. m is an integer between 10 and 1400. x=1 or 2.

[0073] In some embodiments, suitable additives include, in particular, polyacrylic acid, polymethacrylic acid, and acrylic acid-methacrylic acid copolymers, in which the acid groups are at least partially neutralized, for example, preferably 40%, particularly preferably 80%. This percentage refers to the number of acid groups. Highly preferred is poly(meth)acrylic acid, which is present entirely in the form of a salt. Suitable salts include Li, Na, K, Rb, Be, Mg, Ca, Sr, Zn, and ammonia (NR4, where R is a hydrogen or carbon functional group). Poly(meth)acrylic acid may include polyacrylic acid, polymethacrylic acid, and acrylic acid-methacrylic acid copolymers. Poly(meth)acrylic acid is preferred, in particular with an average molar mass M w is 1,000 to 100,000 g / mol, particularly preferably 1,000 to 15,000 g / mol, The molecular weight of poly(meth)acrylic acid polymers and copolymers can be determined by measuring the viscosity of a 1% aqueous solution of the polymer neutralized with sodium hydroxide solution (Fikentscher's constant).

[0074] Also suitable are copolymers of (meth)acrylic acid, in particular those which, in addition to (meth)acrylic acid, contain ethylene, maleic acid, methyl acrylate, ethyl acrylate, butyl acrylate and / or ethylhexyl acrylate as comonomers. Preference is given to copolymers which contain at least 40% by weight, preferably at least 80% by weight, of (meth)acrylic acid monomers. This proportion is based on the acidic form of the monomer or polymer.

[0075] Alkali metal and alkaline earth metal hydroxides, such as potassium hydroxide, especially sodium hydroxide, are particularly suitable for neutralizing polyacrylic acid polymers and copolymers. Additionally, coatings and / or additives for reinforcing the separator may include, for example, metal alkoxides, where the metal may be, by way of example only (and not intended to be limiting), Zn, Na, or Al, and, by way of example only, sodium ethoxide.

[0076] The microporous polyolefin can be provided with one or more additives in various ways. The additives can be applied to the polyolefin, for example once it is finished (for example after extraction), or can be added to the mixture used to produce the polyolefin. According to a preferred embodiment, the additive or a solution of the additive is applied to the surface of the polyolefin. This variant is particularly suitable for applying non-thermally stable additives and additives that dissolve in the solvent used in the subsequent extraction. Particularly suitable as solvents for the additives according to the invention are low molecular weight alcohols, such as methanol and ethanol, as well as mixtures of these alcohols with water. The application can be carried out on the side of the separator facing the negative electrode, on the side facing the positive electrode, or on both sides.

[0077] In some embodiments, the microporous polyolefin porous membrane may include a coating on one or both sides of such layer. Such coatings may include surfactants or other materials. In some embodiments, the coating may include one or more materials described, for example, in U.S. Patent Publication No. 2012 / 0094183, which is incorporated herein by reference. Such coatings may extend battery life while inhibiting grid corrosion and prevent dryout and / or water loss, for example by reducing the overcharge voltage of the battery system.

[0078] diffusion In some selected embodiments, the exemplary separator may be defined as having a high diffusivity. Diffusivity is measured as the rate at which ions can pass through the separator, and thus may describe the ion flux through the separator. The more porous the separator, the higher the diffusion coefficient is expected to be. Pulsed Field Gradient Spin Echo ("PFGSE") may be used to analyze DO diffusion. To determine the diffusion coefficient, a separator sample without oil extraction is pre-soaked in DO. The separator sample is stacked in a nuclear magnetic resonance ("NMR") tube immersed in DO, as generally shown in FIG. 27. The NMR tube is placed under vacuum to remove air bubbles, and the diffusion coefficient (through the separator sample) in the vertical direction is monitored.

[0079] Diffusion can be calculated using the Stejskal formula as follows:

[0080]

number

[0081] E is the NMR signal peak intensity, γ is the magnetic spin ratio (depending on the nuclide), g is the magnetic field gradient, δ is the application time of the magnetic field gradient. Furthermore, the following holds:

[0082]

number

[0083] D e is the diffusion coefficient of the molecules inside the separator, D0 is the diffusion coefficient of the molecule in the solution, ε is the porosity, τ is a measure of pore tortuosity.

[0084] Table 1 below shows various diffusion coefficient values ​​at Δ=20 ms and at −10° C. and 30° C. for a control separator, an embodiment of the invention, and four commercially available separators.

[0085] [Table 1]

[0086] FIG. 28 shows the diffusion coefficients at −10° C. and Δ=20 ms for H2SO4 solution alone, a reference separator, a separator according to an embodiment of the present invention, and an AGM separator.

[0087] Figure 29 shows the pore size distribution of an embodiment of the present invention compared to commercial separator #1, showing that the average pore size of the embodiment of the present invention is 120 nm, while the average pore size of the commercial separator is only 109 nm.

[0088] Figure 30 shows the pore size distribution of the separator of the present invention. Figure 31 shows a chart showing the distribution of the new silica filler in the separator of the present invention and the standard silica in the commercial separator #1. The box plot shows the distribution between the first quartile (Q1) and the third quartile (Q3). In this chart, the lower the value, the better the silica distribution.

[0089] Fragility In some select embodiments, the exemplary separators may utilize more brittle silica than those used in commercially available separators. The more brittle silica is believed to increase the dispersion of the silica within the separator, allowing more oil to penetrate during the formation of the separator and less oil to remain in the separator after the oil is extracted. Good pore distribution is obtained with a smaller primary silica particle size. Reducing the primary silica particle size leads to increased particle aggregation, which is believed to increase oil absorption. This leads to a smaller average pore size and an increased pore volume, along with a low and narrow particle size distribution. In a believed preferred embodiment, the silica modulus is high (SiO2 / Na2O) and the sodium silicate concentration is increased during silica processing.

[0090] Figure 32 shows the size of standard silica and the size of silica used in the embodiment of the present invention. As can be seen, the novel silica has a smaller particle size. One way to determine the friability of silica is to subject it to ultrasonic frequencies (above 20 kHz). Figure 33 shows the size of silica before and after ultrasonic treatment, and Figure 34 shows the particle size distribution of novel silica and standard silica before ultrasonic treatment, after 30 seconds of ultrasonic treatment, and after 60 seconds of ultrasonic treatment.

[0091] Exemplary separators according to the present disclosure also exhibit high shrinkage values ​​in H2SO4. Table 2 below shows these values.

[0092] [Table 2]

[0093] Working Example The following examples further illustrate at least selected separator embodiments of the present invention.

[0094] In some embodiments, the following precipitated silicas can be used to obtain a separator according to the present invention:

[0095] Median particle size 20.48 μm, mean particle size 24.87 μm (measured using a Coulter LS230)

[0096] In preparing the separator, the silica samples shown in Table 3 below were used having the following characteristics:

[0097] [Table 3]

[0098] The polyethylene separator made using the above silica had the following properties shown in Tables 4 and 5 below.

[0099] [Table 4]

[0100] [Table 5]

[0101] Additionally, in another embodiment, the following silica fillers shown in Table 6 below were used in the separators shown in Table 7 below.

[0102] [Table 6]

[0103] [Table 7]

[0104] Another embodiment In the following set of examples, inventive reinforced liquid separators were made according to various embodiments of the present invention and tested against a control separator, with the results shown in Table 8 below.

[0105] [Table 8]

[0106] The results in Table 8 above show that the ER of the separator of Example A was nearly 20% lower than that of the control Separator A. Similarly, the ER of the separator of Example B was more than 20% lower than that of the control Separator A. These desirable low ER results occurred even though the porosity percentages of Separators A and B of the present invention were within the porosity tolerance (60% ± 7.5%) for such separators. Thus, the novel and unexpected pore structure of the separator contributed to the reduced ER combined with the porosity percentages of the separators that were consistent with (but not significantly higher than) the porosity of known separators.

[0107] Additional Examples Several separators were made according to the present invention. The separators were compared to comparative separators. The separators of the present invention were imaged by SEM to show shish kebab formation.

[0108] Example 1 In Example 1, a reinforced liquid separator with a backweb thickness of 250 μm was made in accordance with the present invention using UHMWPE, silica, and oil. The silica used was a high oil absorption silica. An SEM was taken of the low ER separator of the present invention. See Figure 15A.

[0109] In the SEM of FIG. 15A, i.e., the SEM of the separator of Example 1, three shish kebab regions numbered 1, 2, and 3, respectively, were identified. The three shish kebab regions were then An FTIR spectral profile was obtained for each of the three shish kebab regions (numbered 1, 2, and 3) of the SEM of FIG. 15A of the separator of Example 1, revealing the following peak position information and periodicity or repetition of the shish kebab formation or morphology, as shown in Table 9 below.

[0110] [Table 9]

[0111] Finally, an average repeat or period of the shish kebab morphology or structure of 63 nm was obtained.

[0112] Example 2 Further, in Example 2, a reinforced liquid separator with a backweb thickness of 200 μm was fabricated in accordance with the present invention using UHMWPE, silica, and oil, similar to Example 1 above. The silica used was a high oil absorption silica. SEM of the low ER separator of the present invention was taken. See Figure 16A.

[0113] In the SEM of FIG. 16A, the SEM of the separator of Example 2, three shish kebab regions were identified, numbered 1, 2, and 3, respectively. FTIR spectral profiles were then obtained for each of the three shish kebab regions. See FIG. 16B through FIG. 16D. The FTIR spectra obtained for each of the three shish kebab regions (numbered 1, 2, and 3) of the SEM of FIG. 16A of the separator of Example 2 revealed the following peak position information and periodicity or repetition of the shish kebab formation or morphology, as shown in Table 10 below.

[0114] [Table 10]

[0115] Finally, an average repeat or period of the shish kebab morphology or structure of 63 nm was obtained.

[0116] Example 3 In Example 3, a reinforced liquid separator with a backweb thickness of 250 μm was made in accordance with the present invention using UHMWPE, silica, and oil as in Example 1 above. The silica used was a high oil absorption silica. An SEM was taken of the low ER separator of the present invention. See Figure 17A.

[0117] In the SEM of FIG. 17A, the SEM of the separator of Example 3, three shish kebab regions were identified, numbered 1, 2, and 3, respectively. FTIR spectral profiles were then obtained for each of the three shish kebab regions. See FIG. 17B through FIG. 17D. The FTIR spectra obtained for each of the three shish kebab regions (numbered 1, 2, and 3) of the SEM of FIG. 17A of the separator of Example 3 revealed the following peak position information and periodicity or repetition of the shish kebab formation or morphology, as shown in Table 11 below.

[0118] [Table 11]

[0119] Finally, an average repeat or period of the shish kebab morphology or structure of 74 nm was obtained.

[0120] Example 4 In Example 4, a reinforced liquid separator with a backweb thickness of 250 μm was made in accordance with the present invention using UHMWPE, silica, and oil as in Example 1 above. The silica used was a high oil absorption silica (a different high oil absorption silica than the silica used in Examples 1-3 above. Each of the high oil absorption silicas used to make the separators of Examples 1-5 ranged from about 230 to about 280 ml / 100 g). An SEM was taken of the low ER separator of the present invention. See FIG. 18A.

[0121] In the SEM of FIG. 18A, the SEM of the separator of Example 4, three shish kebab regions were identified, numbered 1, 2, and 3, respectively. FTIR spectral profiles were then obtained for each of the three shish kebab regions. See FIG. 18B through FIG. 18D. The FTIR spectra obtained for each of the three shish kebab regions (numbered 1, 2, and 3) of the SEM of FIG. 18A of the separator of Example 4 revealed the following peak position information and periodicity or repetition of the shish kebab formation or morphology, as shown in Table 12 below.

[0122] [Table 12]

[0123] Finally, an average repeat or period of the shish kebab morphology or structure of 55 nm was obtained.

[0124] Example 5 In this Example 5, a reinforced liquid separator with a backweb thickness of 250 μm was made in accordance with the present invention using UHMWPE, silica, and oil as in Example 1 above. The silica used was a high oil absorption silica (a high oil absorption silica different from the silica used in Examples 1-3 above and Example 4 above). An SEM was taken of the low ER separator of the present invention. See Figure 19A.

[0125] In the SEM of FIG. 19A, the SEM of the separator of Example 5, three shish kebab regions were identified, numbered 1, 2, and 3, respectively. FTIR spectral profiles were then obtained for each of the three shish kebab regions. See FIG. 19B through FIG. 19D. The FTIR spectra obtained for each of the three shish kebab regions (numbered 1, 2, and 3) of the SEM of FIG. 19A of the separator of Example 5 revealed the following peak position information and periodicity or repetition of the shish kebab formation or morphology, as shown in Table 13 below.

[0126] [Table 13]

[0127] Finally, an average repeat or period of the shish kebab morphology or structure of 61 nm was obtained.

[0128] Comparative Example 1 A comparative polyethylene lead acid battery separator was obtained with a backweb thickness of 250 μm. The SEM of the separator of Comparative Example 1 was taken. See FIG. 20A.

[0129] In the SEM of FIG. 20A, i.e., the SEM of the separator of Comparative Example 1, three regions numbered 1, 2, and 3, respectively, were identified. FTIR spectral profiles of each of these three regions were then obtained. See FIG. 20B through FIG. 20D. The FTIR spectra obtained in each of the three numbered regions (numbered 1, 2, and 3) of the SEM of FIG. 20A of the separator of Comparative Example 1 revealed the following peak position information and period or repeat information regarding the crystal structure and / or morphology of these three regions, as shown in Table 14 below.

[0130] [Table 14]

[0131] Finally, an average repeat or period of the crystal structure or morphology of the identified regions was obtained of 170 nm.

[0132] Comparative Example 2 Another comparative polyethylene lead acid battery separator was obtained with a backweb thickness of 250 μm. SEM of the separator of Comparative Example 2 was taken. See FIG. 21A.

[0133] In the SEM of FIG. 21A, i.e., the SEM of the separator of Comparative Example 2, an area of ​​the separator SEM image numbered 1 was identified. An FTIR spectral profile of this area was then obtained. See FIG. 21B. The FTIR spectrum obtained in the area (numbered 1) of the SEM of FIG. 21A of the separator of Comparative Example 2 revealed the following peak position information and period or repeat information regarding the crystal structure and / or morphology of this area, as shown in Table 15 below:

[0134] [Table 15]

[0135] Thus, the average repeat or period of the crystal structure or morphology of the identified regions was 212 nm.

[0136] Comparative Example 3 Yet another comparative polyethylene lead acid battery separator was obtained, which was commercially available from Daramic, LLC. The separator had a backweb thickness of 250 μm. This separator was made similarly to the separators described in Examples 1-5 above, except that the silica used to make this separator did not have a high oil absorption value.

[0137] SEM was taken of the separator of Comparative Example 3. See Figure 22. Observing Figure 22, there was no continuous shish-kebab formation extending at least 0.5 μm in length in this SEM image of the polyolefin microporous membrane. Therefore, no areas were marked in this SEM and no further analysis was performed.

[0138] Table 16 below compares the results obtained for the periodicity or repetition of the shish kebab region in Examples 1-5 with the results obtained in Comparative Examples 1-3.

[0139] [Table 16]

[0140] In Examples 1 to 5, the average repetition or period of the shish-kebab formation and / or crystal structure and / or morphology was 1 nm to 150 nm, preferably 10 nm to 120 nm, more preferably 20 nm to 100 nm. This type of structure was not observed in the separators of Comparative Examples 1 to 3.

[0141] Table 17 below provides additional properties and characteristics of the separators of Examples 1-2 and 4-5 (whereas Table 3 above includes the properties of the separator of Example 3).

[0142] [Table 17]

[0143] Solid-state NMR examples The two separator samples are described in detail above. 29 The ratio of silanol groups (Si-OH) to elemental silicon (Si), (Si-OH) / Si, was measured using Si solid-state NMR techniques. A sample of the separator of Example 1 and a sample of a comparative separator were prepared for this NMR testing. The comparative separator was Comparative Example 4, a polyethylene separator available from Daramic, LLC, having a backweb thickness of 250 μm, made with the same type of polyethylene polymer and silica as the separator described above as Comparative Example 3.

[0144] For each sample 29 Si-NMR spectra were obtained. These spectra are included as Figure 23. The Q2 signal was observed at approximately -93 ppm, the Q3 signal was observed at approximately -103 ppm, and the Q4 signal was observed at approximately -111 ppm. Each component was deconvoluted as shown in Figure 24, and the information from Figure 24 was used to calculate the molecular ratio of Q2:Q3:Q4. The results are shown in Table 18 below.

[0145] [Table 18]

[0146] In the results shown above, the OH / Si ratio of the separator of Example 1 is 35% higher than that of the separator of Comparative Example 4. This means that the additional hydroxyl groups and / or silanol groups present in the silica of the separator of the present invention may contribute to the improved characteristics of the separator of the present invention, such as desirable pore structure and / or morphology and low ER.

[0147] According to at least selected embodiments, the separator may include any of the following: performance enhancing additives or coatings, increased porosity, increased pore volume, amorphous silica, high oil absorption silica, fillers or silica with increased friability, increased ion diffusion, high silanol group silica, silica with an OH to Si ratio of 21:100 to 35:100, reduced electrical resistance, shish kebab structure or morphology, membrane The membrane may include or exhibit a polyolefin microporous membrane comprising a particulate filler in an amount of 40% or more by weight, an ultra-high molecular weight polyethylene having a shish-kebab formation with extended chain crystals (shish formation) and folded chain crystals (kebab formation), an average repeat period of the kebab formations from 1 nm to 150 nm, reduced sheet thickness, reduced twist, etc., or a combination thereof. Such inventive separators are particularly suitable for Enhanced Flooded Batteries (EFBs) that are constructed for higher performance and reliability than conventional flooded batteries, support at least some start-stop functionality with enhanced starting power, meet the ever increasing electrical demands of many vehicles, provide a long lifespan of recovery from deep discharges, power electrical loads during engine off periods, allow a higher number of starts per trip, and further have better cycling capability, charge acceptance, and / or ability to operate at low and / or partial states of charge than conventional lead acid batteries, have tightly packed components, have better battery vibration resistance, reliable starting performance, superior cycling capability, improved cycling of batteries operating at low and / or partial states of charge, and / or longer life, etc.

[0148] According to at least selected embodiments, aspects, or objectives, disclosed or provided herein are new or improved separators, battery separators, reinforced flooded battery separators, batteries, cells, and / or methods of making and / or using such separators, battery separators, reinforced flooded battery separators, cells, and / or batteries. According to at least some embodiments, the present disclosure or invention is directed to new or improved battery separators for reinforced flooded batteries. Additionally, disclosed herein are methods, systems, and battery separators for extending battery life, reducing internal electrical resistance, increasing CCA, and / or improving uniformity in at least reinforced flooded batteries. According to at least certain embodiments, the present disclosure or invention is directed to improved separators for reinforced flooded batteries, which include performance enhancing additives or coatings, improved fillers, reduce twisting, increase wettability, reduce oil content, reduce thickness, reduce electrical resistance, and / or increase porosity, and further, the use of such separators in batteries reduces battery water loss, reduces battery acid stratification, reduces battery voltage drop, and / or increases battery CCA.According to at least certain embodiments, the separators provided include performance enhancing additives or coatings, increased porosity, increased void volume, amorphous silica, high oil absorption silica, fillers or silica with increased friability, increased ion diffusion, increased silanol groups, silica with OH to Si ratios of 21:100 to 35:100, silica with OH to Si ratios of at least 27:100, reduced electrical resistance, shish kebab structure or morphology, polyolefin microporous membranes with particulate fillers in an amount of 40% or more by weight of the membrane, extended chain crystals (shish formation) and folding. The separator includes ultra-high molecular weight polyethylene having a shish kebab formation with extended chain crystals (kebab formation), the average repeat period of the kebab formation is 1 nm to 150 nm, the average repeat period of the kebab formation is less than 150 nm, the average repeat period of the kebab formation is less than 120 nm, the average repeat period of the kebab formation is less than 100 nm, the ribbed side has a shish kebab formation with extended chain crystals (shishi formation) and folded chain crystals (kebab formation), the average repeat period of the kebab formation is 1 nm to less than 150 nm, the sheet thickness is reduced, twisting is reduced, etc. The separator is particularly suitable for reinforced flooded batteries and the like.

[0149] The invention may be embodied in other forms without departing from its spirit or essential attributes and, therefore, reference should be made to the appended claims, rather than the preceding specification, as indicating the scope of the invention.

[0150] The foregoing written descriptions of structures and methods have been presented for illustrative purposes only. The examples are used to disclose exemplary embodiments, including the best mode, and also to enable any person skilled in the art to practice the invention, including making and using any devices or systems, and performing any incorporated methods. These implementations are not intended to be limiting unless otherwise specified. The examples are not intended to be exhaustive or to limit the invention to the precise steps and / or forms disclosed, and many modifications and variations are possible in light of the above teachings. The features described herein may be combined in any combination. The steps of the methods described herein may be performed in any order that is physically possible. The patentable scope of the invention is defined by the appended claims, and may include other examples that occur to those skilled in the art. Such other examples are intended to be within the scope of the claims if they have structural elements that do not differ from the literal language of the claims, or if they include equivalent structural elements that differ insubstantially from the literal language of the claims.

[0151] The compositions and methods of the appended claims are not limited in scope by the specific compositions and methods described herein, which are intended as illustrations of a few aspects of the claims. Any compositions and methods that are functionally equivalent are intended to be within the scope of the claims. Various modifications of the compositions and methods in addition to those shown and described herein are intended to be within the scope of the appended claims. Furthermore, although only some representative compositions and method steps disclosed herein have been specifically described, other combinations of compositions and method steps are also intended to be within the scope of the appended claims, even if not specifically mentioned. Thus, although combinations of steps, elements, components, or elements may be explicitly mentioned herein or below, other combinations of steps, elements, components, and elements are included even if not explicitly stated.

[0152] As used in the specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. As used herein, ranges may be expressed as "about" or "approximately" from one particular value and / or to "about" or "approximately" another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values ​​are expressed as approximations, by use of the antecedent "about," it will be understood that the particular value forms another embodiment. It will further be understood that the endpoints of each range are significant both in relation to the other endpoint and independently of the other endpoint. "Optional" or "optionally" means that the subsequently described event or circumstance may or may not occur, and that the description includes instances when said event or circumstance occurs and instances when said event or circumstance does not occur.

[0153] Throughout the description and claims of this specification, the word "comprise" and variations of this word, such as "comprising" and "comprises," mean "including, but not limited to," and are not intended to exclude, for example, other additives, components, integers, or steps. The terms "consisting essentially of" and "consisting of" may be used in place of "comprising" and "including" to provide and disclose more specific embodiments of the invention. "Exemplary" means "an example of" and is not intended to convey an indication of a preferred or ideal embodiment. "Such as" is not used in a limiting sense, but is used for descriptive or exemplary purposes.

[0154] Except where noted, all numbers expressing geometric shapes, dimensions, and the like used in the specification and claims should, at the very least, be construed in light of the number of significant digits and ordinary rounding approaches but should not be construed as an attempt to limit the application of the doctrine of equivalents to the scope of the claims.

[0155] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the disclosed invention belongs. All publications referred to herein and the materials cited therein are specifically incorporated by reference.

[0156] Moreover, the invention illustratively disclosed herein may be practiced as appropriate in the absence of any element not specifically disclosed herein.

Claims

1. A separator for a lead acid battery comprising a polyolefin microporous membrane, the polyolefin microporous membrane comprising: a polyethylene, preferably ultra-high molecular weight polyethylene, a particulate filler, and a treatment plasticizer; said particulate filler being present in an amount of 40% or greater by weight; The polyethylene comprises a shish-kebab-formed polymer comprising a plurality of extended chain crystals (shish formation) and a plurality of folded chain crystals (kebab formation), the average repeat or period of the kebab formation being between 1 nm and 150 nm, preferably less than 120 nm.

2. 2. The separator for a lead acid battery according to claim 1, wherein the average repetition or period of the kebab formations is defined by taking an image of the surface of the polyolefin microporous membrane by SEM, showing at least three rectangular areas in the SEM image where the shish-kebab formations extend continuously for a length of at least 0.5 μm or more, and identifying the repetition or period by calculating the average of the repetition period by Fourier transformation of the contrast profile projected perpendicularly to the length direction of each of the shown rectangular areas.

3. the filler is selected from the group consisting of silica, precipitated silica, fused silica, and precipitated amorphous silica; 29 2. The separator for lead acid batteries according to claim 1, wherein the molar ratio of OH groups to Si groups in the filler measured by Si-NMR is in the range of 21:100 to 35:100, preferably 27:100 or more.

4. 10. The separator for a lead acid battery according to claim 1, wherein the processing plasticizer is selected from the group consisting of process oil, paraffin-based oil, and mineral oil.

5. 10. The separator for a lead acid battery of claim 1, wherein silica is present in said kebab formation of polymer.

6. A new or improved reinforced flooded battery separator comprising at least one microporous thermoplastic sheet, said separator having a resistance of at least 200 mΩ cm at least in a reinforced flooded battery. 2 a separator having at least one of electrical resistance less than 100%, improved battery life, reduced internal resistance, increased CCM (cold cranking amps), and / or improved uniformity, having performance enhancing additives or coatings, improved fillers, reduced kinking, increased wettability, reduced final oil content, reduced thickness, reduced electrical resistance, and / or increased porosity and / or void volume.

7. The microporous thermoplastic sheet is a) average pore size of 1 μm or less; b) 75 mΩ cm 2 Less than 70 mΩ cm 2 Less than 65 mΩ cm 2 Less than 60 mΩ cm 2 Less than or equal to 55 mΩ cm 2 Less than or equal to 50 mΩ cm 2 Less than or equal to 45 mΩ cm 2 Less than or equal to 40 mΩ cm 2 Less than or equal to 35 mΩ cm 2 Electrical resistance of less than or equal to c) an electrical resistance that is more than 20% less than the electrical resistance of known separators for flooded lead-acid batteries; d) a porosity greater than 50%; e) a final oil content of about 10 to 20% by weight, in some embodiments about 14 to 20% by weight; and f) ribs, serrated ribs, embossed ribs, and / or negative transverse ribs; 7. The separator of claim 6, characterized by one of:

8. The separator of claim 1 further comprising a filler having a high structural morphology.

9. The filler is a) an average particle size of 5 μm or less; b) At least 100 m 2 / g surface area, and c) an oil absorption rate of at least 150 ml / 100 g; 9. The separator according to claim 1, characterized by one of the following:

10. 10. The separator of claim 1, wherein the filler and thermoplastic polymer are present in a weight ratio of from 1.5:1 to 6:

1.

11. The separator of claim 1 , wherein the filler comprises precipitated silica.

12. 10. The separator of claim 1, wherein the particulate filler is friable such that after 30 seconds of sonication, the median silica particle size is about 5 microns or less.

13. 10. The separator of claim 1, wherein the particulate filler is friable such that after 60 seconds of sonication, the median silica particle size is about 0.5 μm or less.

14. 10. The separator of claim 1 comprising an average pore size of at least about 120 nm.

15. At least about 1.6·10 at −5°C -10 Diffusion coefficient of, and Approximately 40 mΩ・cm 2 10. The separator of claim 1 comprising an electrical resistance of:

16. At least about 8.8-10 at 30°C -10 Diffusion coefficient of, and Approximately 40 mΩ・cm 2 10. The separator of claim 1 comprising an electrical resistance of:

17. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; The particulate filler is friable such that after 30 seconds of ultrasonic treatment the silica median particle size is about 5.2 μm or less.

18. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; The particulate filler is friable such that after 60 seconds of ultrasonic treatment the silica median particle size is about 0.5 μm or less.

19. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; The particulate filler is friable such that after 60 seconds of ultrasonic treatment the silica median particle size is about 0.5 μm or less.

20. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; At least about 1.6·10 at −5°C -10 and the diffusion coefficient of Approximately 40 mΩ・cm 2 The electrical resistance and 23. A separator for a lead acid battery, comprising:

21. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; At least about 8.8-10 at 30°C -10 and the diffusion coefficient of Approximately 40 mΩ・cm 2 The electrical resistance and 23. A separator for a lead acid battery, comprising:

22. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; At least about 1.6·10 at −5°C -10 and the diffusion coefficient of wherein the particulate filler is friable such that after 30 seconds of ultrasonic treatment the silica median particle size is about 5 μm or less.

23. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; At least about 8.8-10 at 30°C -10 and the diffusion coefficient of wherein the particulate filler is friable such that after 60 seconds of ultrasonic treatment the silica median particle size is about 0.5 μm or less.

24. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; At least about 1.6·10 at −5°C -10 and the diffusion coefficient of an average pore size of at least about 120 nm; 23. A separator for a lead acid battery, comprising:

25. a polyolefin microporous membrane comprising polyethylene, a particulate filler, and a treatment plasticizer; At least about 8.8-10 at 30°C -10 and the diffusion coefficient of an average pore size of at least about 120 nm; 23. A separator for a lead acid battery, comprising:

26. 26. The separator of any one of claims 1 to 25, wherein the separator comprises one or more of a surfactant, a coating, a wetting agent, a colorant, an antistatic additive, an antioxidant, a chemical to inhibit oxidation, and combinations thereof.

27. 27. The separator of claim 26, wherein the separator comprises at least one surfactant, such surfactant being a non-ionic surfactant, an anionic surfactant, or a combination thereof.

28. 28. A method for reducing the internal resistance in a lead acid battery, preferably a reinforced flooded battery, comprising providing a separator according to any one of claims 1 to 27.

29. 29. A new or improved lead acid battery, preferably a reinforced flooded battery, comprising the separator of any one of claims 1 to 28.

30. 30. A new or improved vehicle comprising a battery or enhanced flooded battery according to claims 1 to 29.

31. Improved separators as shown and described herein for flooded lead acid batteries, preferably reinforced flooded lead acid batteries, exhibiting reduced electrical resistance (ER) in the battery compared to known separators for flooded lead acid batteries, having a shish kebab structure as defined herein, and exhibiting reduced acid stratification in the battery compared to known separators, reduced voltage drop in the battery compared to known separators, increased CCA (cold cranking amps) in the battery compared to known separators, reduced current in the battery compared to known separators, and reduced current in the battery compared to known separators in the flooded lead acid batteries, preferably reinforced flooded lead acid batteries. The improved separator exhibits at least one of water loss in a battery, increased charge acceptance in the battery compared to the known separators, and / or improved overall battery performance, battery life, and / or battery cycling compared to batteries employing the known separators.

32. 32. An improved battery separator for a flooded lead acid battery, or an improved flooded lead acid battery, or an improved vehicle including an improved flooded lead acid battery, according to any one or more of claims 1 to 31, wherein the improved battery separator or battery or vehicle approaches, matches or exceeds the performance of an AGM battery separator, and / or an AGM battery, and / or a vehicle including an AGM battery and an AGM battery separator.

33. New or improved separators, battery separators, enhanced flooded battery separators, batteries, cells, and / or methods of making and / or using such separators, battery separators, flow redox separators, cells, and / or batteries; new or improved enhanced flooded battery separators for enhanced flooded batteries; improved separators for enhanced flooded batteries, and / or improved methods of using such batteries having such improved separators; methods for reducing internal resistance, extending battery life, reducing water loss, reducing internal resistance, increasing wettability, reducing acid stratification, improving acid diffusion, improving CCA (cold cranking amps), and / or improving uniformity. Methods, systems, and battery separators, separators comprising or exhibiting performance enhancing additives or coatings, increased porosity, increased void volume, amorphous silica, high oil absorption silica, high silanol group silica, silica with an OH to Si ratio of 21:100 to 35:100, reduced electrical resistance, shish kebab structure or morphology, polyolefin microporous membranes comprising particulate fillers in an amount of 40% or more by weight of the membrane, ultra high molecular weight polyethylene having shish kebab formation with extended chain crystals (shish formation) and folded chain crystals (kebab formation), average repeat period of kebab formation of 1 nm to 150 nm, reduced sheet thickness, reduced twist, and the like, separators particularly suitable for reinforced flooded batteries and the like as shown or described herein.

Citation Information

Patent Citations

  • PE separator plate for lead acid battery and preparation method thereof

    CN102244219A

  • Lead-acid battery separator with improved electrical and mechanical properties

    JP2004523088A

  • Separator for storage battery, and its manufacturing method

    JP2005268006A

  • Microporous material and manufacturing method thereof

    JP2008523211A

  • Improved lead-acid battery separator, battery and related method

    JP2013541162A