Polar group-containing olefin copolymer
A multi-component polar group-containing olefin copolymer addresses the balance of transparency, rigidity, and toughness in ethylene-based ionomers by incorporating specific structural units, resulting in improved mechanical and thermal properties.
Patent Information
- Application Number
- JP2024123193
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-01-28
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-01-27
AI Technical Summary
Existing ethylene-based ionomers face challenges in achieving a balanced combination of transparency, rigidity, and toughness due to high crystallinity, which affects their mechanical strength and thermal properties.
A multi-component polar group-containing olefin copolymer is developed, incorporating structural units derived from ethylene or α-olefins, carboxyl group-containing units, and acrylic acid-derived units that do not undergo elimination reactions, allowing for improved tensile modulus, stress, elongation, impact strength, and crystallinity.
The copolymer achieves a better balance of physical properties, enhancing its suitability as a material for ionomers with improved transparency, rigidity, and toughness compared to conventional ethylene-based ionomers.
Smart Images

Figure 2024153808000021 
Figure 2024153808000022 
Figure 2024153808000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polar group-containing olefin copolymer, in particular a copolymer that can be used to prepare an ionomer and has an excellent balance of physical properties such as tensile modulus, tensile stress at break, tensile elongation at break, tensile impact strength, crystallinity, and phase angle, and a method for producing the same. [Background technology]
[0002] Ethylene-based ionomers are resins that use ethylene-unsaturated carboxylic acid copolymers as the base resin and are intermolecularly bonded with metal ions such as sodium and zinc. They are strong, elastic, flexible, abrasion-resistant, transparent, and other characteristics (Patent Document 1). Known commercially available ethylene-methacrylic acid copolymers include "Nucrel (registered trademark)" developed by Dupont, and ethylene-based ionomers include "Surlyn (registered trademark)", a sodium or zinc salt of ethylene-methacrylic acid copolymer also developed by Dupont.
[0003] As the ethylene-unsaturated carboxylic acid copolymer serving as the base resin of this conventionally known ethylene-based ionomer, specifically, an ethylene-unsaturated carboxylic acid copolymer obtained by polymerizing ethylene and a polar group-containing monomer such as (meth)acrylic acid by a high-pressure radical polymerization method is used (Patent Documents 2 to 4). However, the molecular structure of the ethylene-unsaturated carboxylic acid copolymer produced by the high-pressure radical polymerization method is a structure having many long-chain branches and short-chain branches irregularly, and has the disadvantage of being insufficient in terms of strength.
[0004] On the other hand, as another method for producing an ethylene-unsaturated carboxylic acid copolymer that serves as the base resin of an ethylene-based ionomer, a method has been reported in which a copolymer of ethylene and t-butyl acrylate is produced using a late transition metal catalyst (Patent Document 5), and the resulting polar group-containing olefin copolymer is modified by heat or acid treatment to form an ethylene-acrylic acid copolymer (Patent Document 6).
[0005] In addition, a method for producing an ethylene-unsaturated carboxylic acid copolymer, which serves as the base resin for a highly rigid ionomer, has also been reported in which ethylene-cyclic olefin copolymer (COC) is graft-modified with maleic anhydride (Patent Document 7). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] U.S. Pat. No. 3,264,272 [Patent Document 2] Japanese Patent Application Publication No. 47-23490 [Patent Document 3] Japanese Unexamined Patent Publication No. 11388 / 1983 [Patent Document 4] Japanese Patent Application Laid-Open No. 63-186710 [Patent Document 5] JP 2015-163691 A [Patent Document 6] JP 2016-79408 A [Patent Document 7] International Publication No. 2009 / 123138 Summary of the Invention [Problem to be solved by the invention]
[0007] Ionomers generally tend to have good moldability, compatibility with pigments, rigidity, transparency, and other physical properties. For example, they are advantageous as materials for packaging materials, and therefore methods for synthesizing copolymers for the production of ionomers have been researched. However, in the method described in Patent Document 6, since an α-olefin-unsaturated carboxylic acid copolymer produced using a transition metal catalyst is used as the base resin, ionomers with excellent thermal properties and mechanical strength are obtained, but the resulting polymer has a high degree of crystallinity, resulting in low transparency, which is a problem. In the ethylene-based ionomer using an ethylene-acrylic acid copolymer as the base resin described in the examples of Patent Document 6, the transparency can be controlled by the crystallinity. However, since there is a trade-off between crystallinity and rigidity, lowering the crystallinity in order to increase transparency results in a decrease in rigidity, and it is therefore difficult to balance transparency, rigidity, and toughness.
[0008] In the method described in Patent Document 7, since it is extremely difficult to produce an α-olefin-unsaturated carboxylic acid copolymer having a large amount of maleic anhydride by graft modification, there is a drawback that the acid content in the α-olefin-unsaturated carboxylic acid copolymer is low. In fact, the maleic anhydride content of the copolymer described in the examples of Patent Document 7 is about 0.7 to 1.4 wt% (0.5 to 1 mol%). Therefore, an ethylene-based ionomer having a graft-modified copolymer as a base resin has a drawback that the balance of rigidity, toughness, and transparency is insufficient because the copolymer has few polar sites. In addition, since there are few reaction sites with metal ions, it is considered that the toughness and elasticity expected of an ionomer are not fully expressed. Furthermore, since the base resin of the ethylene-based ionomer used in the examples of Patent Document 7 contains 21 to 35 mol% of cyclic olefin, there is a drawback that the glass transition point (Tg) is high and too hard.
[0009] Since ionomers generally inherit the properties of the α-olefin-unsaturated carboxylic acid copolymer (acid copolymer) that serves as the base resin, obtaining an acid copolymer with various excellent physical properties, or an olefin copolymer containing a polar group before modification, leads to obtaining an ionomer with various excellent physical properties. However, such a copolymer that has excellent physical properties in itself and can be used as an ionomer has not been obtained. Therefore, the object of the present invention is to provide an α-olefin-unsaturated carboxylic acid copolymer or a polar group-containing olefin copolymer that has an excellent balance of physical properties such as crystallinity, rigidity, and toughness. [Means for solving the problem]
[0010] In order to solve the above problems, the inventors conducted extensive research and discovered that by introducing into a polymer a structural unit derived from a polar group-containing olefin monomer that does not undergo an elimination reaction due to heat or acid, and forming a multi-component copolymer based on components having at least three types of properties, the balance of tensile modulus, tensile stress at break, tensile elongation at break, tensile impact strength, crystallinity and phase angle can be improved, resulting in the present invention.
[0011] That is, a first aspect of the present invention is a multi-component polar group-containing olefin copolymer, characterized by comprising a structural unit (A) derived from ethylene or an α-olefin, a structural unit (B) having a carboxy group or a structure that generates a carboxy group through an elimination reaction caused by heat or acid, and a structural unit (C) derived from acrylic acid that does not have a carboxy group and does not undergo an elimination reaction caused by heat under the same conditions as those in which the structural unit (B) undergoes an elimination reaction caused by heat or acid to generate a carboxy group. Effect of the Invention
[0012] The present invention can provide a copolymer having an improved balance of tensile modulus, tensile stress at break, tensile elongation at break, tensile impact strength, crystallinity, and phase angle. The multi-component polar group-containing olefin copolymer of the present invention is a useful material that can be used not only as a material itself but also for preparing an ionomer having better physical properties than conventional materials. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the balance between stiffness and toughness in the copolymers of Examples and Comparative Examples. [Diagram 2] FIG. 2 is a graph showing the balance between stiffness and strength in the copolymers of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] One aspect of the present invention is a multi-component polar group-containing olefin copolymer, characterized by comprising a structural unit (A) derived from ethylene or α-olefin, a structural unit (B) having a carboxy group or a structure that generates a carboxy group by thermal or acid elimination reaction, and a structural unit (C) derived from acrylic acid that does not have a carboxy group and does not undergo thermal elimination reaction under the same conditions as the thermal or acid elimination reaction that generates a carboxy group of the structural unit (B). The constituent monomers of the polymer, catalyst components, production method, etc. will be described in detail below.
[0015] In the following description, the term "polymerization" collectively refers to homopolymerization of one type of monomer and copolymerization of multiple types of monomers, and copolymerization may be referred to simply as "polymerization" in this specification. In addition, although the present invention relates to a polymer, the structure of a polymer itself cannot generally be uniquely determined by a chemical formula or the like. Therefore, in the description of a polymer in this specification, the polymer may be described using its production method, as necessary. In this specification, the term "~" indicating a range of values is used to mean that the values before and after it are included as the lower and upper limits. In addition, in this specification, a hydrocarbon group may be expressed using "R" or the like without a subscript as necessary. The hydrocarbon group includes general groups composed of carbon and hydrogen, such as linear or branched alkyl groups such as methyl, ethyl, and t-butyl, groups having unsaturated bonds such as vinyl, cyclic groups such as cyclopentyl, cyclohexyl, and norbornyl, and aromatic groups such as phenyl and naphthyl, but if any of these is specifically excluded in a particular context, this will be clearly stated. In addition, unless otherwise specified, a "hydrocarbon group" is a monovalent substituent such as an alkyl group or a phenyl group, but if it is clear from the context or if the valence is clearly stated, the valence of the hydrocarbon group follows that description.
[0016] (1) Structural unit (A) The structural unit (A) is at least one structural unit selected from the group consisting of structural units derived from ethylene and structural units derived from an α-olefin. Of the α-olefins according to the present disclosure, more preferred are those having the structural formula: CH 2 =CHR d (wherein R d is a hydrocarbon group having 1 to 18 carbon atoms, which may have a linear structure or may be branched.) More preferably, it is an α-olefin having 3 to 12 carbon atoms.
[0017] Specific examples of the monomer from which the structural unit (A) is derived include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, 4-methyl-1-pentene, and the like, and may be ethylene. The structural unit may be of one type or of multiple types.
[0018] Examples of the combination of the two types of structural units (A) include ethylene-propylene, ethylene-1-butene, ethylene-1-hexene, ethylene-1-octene, propylene-1-butene, propylene-1-hexene, and propylene-1-octene.
[0019] Examples of the combination of the three types of structural units (A) include ethylene-propylene-1-butene, ethylene-propylene-1-hexene, ethylene-propylene-1-octene, propylene-1-butene-hexene, and propylene-1-butene-1-octene.
[0020] In the present disclosure, the monomer from which the structural unit (A) is derived preferably essentially contains ethylene and may further contain, as necessary, one or more α-olefins having 3 to 20 carbon atoms. In this case, the proportion of ethylene contained in the monomer from which the structural unit (A) is derived may be 65 to 100 mol % or 70 to 100 mol % based on the total moles of the structural unit (A).
[0021] (2) Structural unit (B) The structural unit (B) is a structural unit derived from a monomer having a carboxy group or a structure that generates a carboxy group upon elimination reaction by heat or acid. Here, the carboxy group or the structure that generates a carboxy group upon elimination reaction by heat or acid is bonded to any part of the carbon atom that forms the main chain of the multi-component polar group-containing olefin copolymer of the present invention, other than the molecular chain terminal. Therefore, the monomer from which the structural unit (B) is derived is a monomer having a structure that serves as a polymerization reaction point, such as a carbon-carbon double bond, and a carboxy group bonded to a carbon atom of the structure, or a structure that generates a carboxy group upon elimination reaction by heat or acid. The structure that serves as the polymerization reaction point is preferably a carbon-carbon double bond, and a vinyl group (H 2 C=CH-) is more preferable. In the multi-component polar group-containing olefin copolymer of the present invention, the carboxy group of the structural unit (B) or the structure that generates a carboxy group by elimination reaction with heat or acid is located in the side chain of the copolymer.
[0022] The structural unit (B) includes a structure that generates a carboxyl group by an elimination reaction by heat or acid. The "elimination reaction" here is preferably a deprotection reaction of an ester. In this way, an α-olefin-unsaturated carboxylic acid copolymer that serves as a base resin for an ionomer can be obtained from the multi-component polar group-containing olefin copolymer of the present invention. From the above, there is no particular restriction on the reaction conditions used for deprotection of a general ester in order to obtain an α-olefin-unsaturated carboxylic acid copolymer. As the reaction conditions for the elimination reaction, heat or acid, generally adopted conditions and reagents can be adopted. The conditions such as temperature and reagents in the elimination reaction are well known to those skilled in the art, and can be adopted in appropriate combination with reference to the following examples. The reaction temperature when the multi-component polar group-containing olefin copolymer of the present invention is subjected to an elimination reaction by heat may be any temperature at which the structural unit (B) becomes a carboxylic acid, and if the heating temperature is too low, the ester is not converted to a carboxylic acid, and if the heating temperature is too high, decarbonylation and decomposition of the copolymer proceed. Therefore, the heating temperature of the present invention is preferably in the range of 80°C to 350°C, more preferably 100°C to 340°C, even more preferably 150°C to 330°C, and even more preferably 200°C to 320°C. The reaction time varies depending on the heating temperature, the reactivity of the structural unit (B), etc., but is usually 1 minute to 50 hours, more preferably 2 minutes to 30 hours, even more preferably 2 minutes to 10 hours, still more preferably 2 minutes to 3 hours, and particularly preferably 3 minutes to 2 hours. In the above steps, the reaction atmosphere is not particularly limited, but it is generally preferable to carry out the reaction under an inert gas flow. Examples of inert gases that can be used include nitrogen, argon, and carbon dioxide atmospheres, and a small amount of oxygen or air may be mixed in. A solvent can also be used as the reaction medium. As the solvent, any solvent that is inert under the conditions of this reaction can be used without particular limitation. When a solvent is used, the upper limit of the reaction temperature is preferably the boiling point of the solvent used. Toluene is preferably used because it has a boiling point within the range of the above-mentioned preferred reaction temperature. The reactor used in the above step is not particularly limited, and any method can be used as long as it can substantially uniformly stir the copolymer. A glass vessel or an autoclave (AC) equipped with a stirrer may be used, or any conventionally known kneading machine such as a Brabender plastograph, a single-screw or twin-screw extruder, a high-intensity screw-type kneader, a Banbury mixer, a kneader, or a roll may be used. As an additive for promoting the elimination reaction by heat, a conventionally known acid-base catalyst may be used. The acid-base catalyst is not particularly limited, but may be, for example, hydroxides of alkali metals or alkaline earth metals such as sodium hydroxide, potassium hydroxide, or lithium hydroxide, alkali metals such as sodium hydrogencarbonate or sodium carbonate, carbonates of alkaline earth metals, solid acids such as montmorillonite, inorganic acids such as hydrochloric acid, nitric acid, or sulfuric acid, or organic acids such as formic acid, acetic acid, benzoic acid, citric acid, paratoluenesulfonic acid, trifluoroacetic acid, or trifluoromethanesulfonic acid. From the viewpoints of reaction promotion effect, cost, equipment corrosivity, etc., sodium hydroxide, potassium hydroxide, sodium carbonate, or paratoluenesulfonic acid is preferred, and paratoluenesulfonic acid is more preferred.
[0023] When the multi-component polar group-containing olefin copolymer of the present invention is subjected to an elimination reaction with an acid, a conventionally known acid can be used. The acid catalyst is not particularly limited, but for example, a solid acid such as montmorillonite, an inorganic acid such as hydrochloric acid, nitric acid, and sulfuric acid, and an organic acid such as formic acid, acetic acid, benzoic acid, citric acid, paratoluenesulfonic acid, trifluoroacetic acid, and trifluoromethanesulfonic acid can be appropriately used. From the viewpoints of reaction promotion effect, cost, equipment corrosiveness, etc., paratoluenesulfonic acid is preferred, and paratoluenesulfonic acid is more preferred.
[0024] The temperature during the elimination reaction with an acid may be any temperature at which the ester becomes a carboxylic acid, and if the temperature is too low, the ester is not converted to a carboxylic acid, and if the temperature is too high, decarbonylation and decomposition of the copolymer proceed. Therefore, the heating temperature in the present invention is preferably in the range of 20°C to 250°C, more preferably 50°C to 200°C, even more preferably 60°C to 150°C, particularly preferably 70°C to 140°C, even more preferably 80°C to 130°C, and even more particularly preferably 90°C to 120°C.
[0025] The reaction time for the elimination reaction with an acid varies depending on the temperature, the reactivity of the ester group portion, etc., but is usually 1 minute to 50 hours, more preferably 2 minutes to 30 hours, even more preferably 2 minutes to 10 hours, still more preferably 2 minutes to 7 hours, and particularly preferably 3 minutes to 5 hours.
[0026] In the above steps, the reaction atmosphere is not particularly limited, but it is generally preferable to carry out the reaction under an inert gas flow. Examples of the inert gas include nitrogen, argon, and carbon dioxide. A small amount of oxygen or air may be mixed in.
[0027] The reactor used in the above step is not particularly limited, and any method can be used as long as it can substantially uniformly stir the copolymer. A glass vessel or an autoclave (AC) equipped with a stirrer may be used, or any conventionally known kneading machine such as a Brabender plastograph, a single-screw or twin-screw extruder, a high-intensity screw-type kneader, a Banbury mixer, a kneader, or a roll may be used.
[0028] A preferred embodiment of the structural unit (B) is at least one selected from the group consisting of structural units (b-1) derived from a polar group-containing olefin monomer represented by the following general formula (1) and structural units (b-2) derived from a polar group-containing olefin monomer represented by the following general formula (2). H 2 C=CH-T 1 (1) [In general formula (1), T 1 teeth, Carboxy group, an alkoxycarbonyl group having 2 to 20 carbon atoms substituted with one or more carboxy groups; a hydrocarbon group having 1 to 30 carbon atoms substituted with one or more carboxy groups; an alkoxy group having 1 to 20 carbon atoms substituted with one or more carboxy groups; an acyloxy group having 1 to 20 carbon atoms substituted with one or more carboxy groups; a substituted amino group having 1 to 12 carbon atoms substituted with one or more carboxy groups; Substituted silyl group having 1 to 18 carbon atoms and substituted with one or more carboxy groups It is.] In general formula (1), T 1 is a carboxyl group structure. H 2 C=CH-X-COOT 2 (2) [In general formula (2), T 2 teeth, t-butyl group, Allyl group Benzyl group -CR a R b -OR c (where R a is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and R b , R c are each a hydrocarbon group having 1 to 10 carbon atoms, and R b and R c are substituents selected from the group consisting of groups represented by the formula (I) and (II), which together may be a divalent hydrocarbon group having 1 to 8 carbon atoms, in which one or more methylene groups may be replaced by an ether group or an ester group, and each group may have a hydrocarbon substituent having 1 to 4 carbon atoms; X is a direct bond or -COO-R'- (wherein R' is a divalent hydrocarbon group having 1 to 30 carbon atoms). In general formula (2), T 2 is a structure which generates a carboxyl group by elimination reaction with heat or acid.
[0029] T other than the carboxy group in the monomer represented by the general formula (1) 1That is, the alkoxycarbonyl group having 2 to 20 carbon atoms, the hydrocarbon group having 1 to 30 carbon atoms, the alkoxy group having 1 to 20 carbon atoms, the acyloxy group having 1 to 20 carbon atoms, the substituted amino group having 1 to 12 carbon atoms, or the substituted silyl group having 1 to 18 carbon atoms, which are substituted with one or more carboxy groups, are not particularly limited in structure as long as they are substituted with one or more carboxy groups and satisfy the condition of the carbon number. The position where the carboxy group is substituted in the above structure is also not particularly limited. However, since there is a tendency for reaction with metal ions to occur easily when forming an ionomer, it is preferable that the terminal of the above structure is substituted with a carboxy group.
[0030] T 1 The carbon skeleton of the alkoxycarbonyl group, hydrocarbon group, alkoxy group, acyloxy group, substituted amino group, and substituted silyl group may have a branch, a ring, and / or an unsaturated bond. Here, the ring may be an aromatic ring. The carbon skeleton may be substituted with one or more halogens such as chlorine, fluorine, and bromine, a hydroxyl group, a silyl group, and an amino group, and may contain one or more groups having a heteroatom such as an ether bond (-O-), an ester bond, a carbonyl group (C=O), and an amino group. T 1 The lower limit of the number of carbon atoms in the alkoxycarbonyl group (-COOR) may be 2 or more, and the upper limit may be 20 or less, or may be 15 or less. T 1 The lower limit of the number of carbon atoms in the hydrocarbon group (R-) may be 1 or more, and the upper limit may be 30 or less, or may be 10 or less. T 1 The number of carbon atoms in the alkoxy group (RO-) in the above formula may be 1 or more, and may be 20 or less, or may be 10 or less. Here, R may be an aromatic ring. 1 The alkoxy group in the above formula also includes a phenol structure. T 1 With respect to the number of carbon atoms in the acyloxy group (RCOO-), the lower limit may be 2 or more, and the upper limit may be 20 or less, or may be 10 or less.
[0031] T 1 In the substituted amino group, the amino group (R 2 The carbon number of N-) may be 1 or more in total of two R, and may be 2 or more, and the upper limit may be 12 or less in total of two R, and may be 9 or less. For example, one of the two R may be an undecyl group (carbon number 11) and the other may be a methyl group (carbon number 1). In the amino group, the two types of R may each independently be a substituent having 1 to 6 carbon atoms, and the substituent may have the same carbon skeleton or may be different, and one of them may be a hydrogen atom. In addition, oxygen may be directly bonded to nitrogen to have a structure of hydroxylamine or a hydroxylamine derivative. In other words, the amino group may contain a hydroxyl group or an alkoxy group as R. Non-limiting examples of amino groups not substituted with carboxy groups include dimethylamino group, diethylamino group, di-n-propylamino group, cyclohexylamino group, dodecylamino group, N,O-dimethylhydroxylamino, etc.
[0032] T 1 In the substituted silyl group, the silyl group (R 3The carbon number of Si-) may be 1 or more in total of three R, and may be 3 or more, and the upper limit may be 18 or less in total of three R, and may be 12 or less. For example, one of the three R may be a hexadecyl group (carbon number 16), and the remaining two may be methyl groups (carbon number 1). In the substituted silyl group, the three R may each independently be a substituent having 1 to 6 carbon atoms, and the substituent may have the same carbon skeleton or may be different, and as long as at least one R has a substituent having 1 to 6 carbon atoms, the other R may be a hydrogen atom. In addition, the silyl group may have a structure in which oxygen is directly bonded to silicon to become a hydroxysilyl or alkoxysilyl group. In other words, the silyl group may contain a hydroxyl group or an alkoxy group as R. Non-limiting examples of silyl groups that are not substituted with a carboxy group include a trimethylsilyl group, a triethylsilyl group, a tri-n-propylsilyl group, a dimethylphenylsilyl group, a methyldiphenylsilyl group, and a triphenylsilyl group.
[0033] Non-limiting examples of preferred monomers from which the structural unit (b-1) is derived include the following compounds. Based on these examples and the above definitions, a person skilled in the art can determine the structure of the monomer from which the structural unit (b-1) is derived without being bound by the following examples. [ka] [ka]
[0034] One of the preferred embodiments of the structural unit (B) is the structural unit (b-2) derived from a polar group-containing olefin monomer represented by the general formula (2). 2 C=CH-X-COOT 2 where T 2 is a t-butyl group, an allyl group, a benzyl group, -CR a Rb -OR c (where R a , R b , R c is as defined above), and X is a direct bond or -COO-R'- (wherein R' is a divalent hydrocarbon group having 1 to 30 carbon atoms). That is, the structural unit (b-2) as one of the preferred embodiments is a structural unit (b-3) having a group T 2 is a monomer derived from acrylic acid, in which the above group T 2 A more preferred embodiment of the structural unit (B) is a monomer derived from acrylic acid substituted with T 2 t-butyl group, -CR a R b -OR c (where R a ~R c is as defined above), and X is a substituent that is a direct bond. 2 is a t-butyl group and X is a direct bond, that is, a structural unit derived from t-butyl acrylate.
[0035] T 2 The t-butyl, allyl, and benzyl groups in the above are functional groups used as protecting groups for esters. The t-butyl group can be removed under strong acid conditions, the allyl group in the presence of a Pd catalyst, and the benzyl group under ester hydrolysis conditions.
[0036] T 2 The group -CR a R b -OR c (R a ~R c (wherein R is as defined above) is used as an acetal-based ester protecting group, and can be deprotected under hydrolysis conditions. If R is a chemical species capable of protecting and deprotecting a carboxy group, a ~Rc There is no particular restriction on the structure of each. R is preferred because the protecting group reagents are easily available. a is a methyl group, or R b and R c In a preferred embodiment, these are combined to form a divalent hydrocarbon group having 1 to 8 carbon atoms in which one or more methylene groups may be replaced by an ether group or an ester group. T 2 In the group -CR a R b -OR c Examples of reagents known for forming the above (i.e., for introducing a protecting group for a carboxy group) include 3,4-dihydro-2H-pyran, 2,3-dihydrofuran, allyl alkyl ethers such as allyl ethyl ether and allyl isobutyl ether, and chloromethyl methyl ether.
[0037] X is a direct bond or a group represented by -COO-R'- (wherein R' is a divalent hydrocarbon group having 1 to 30 carbon atoms). R' in the -COO-R'- group is a divalent hydrocarbon group, and is not a methylene group (-CH 2 -), ethylene group (-CH 2 CH 2 -), propylene group (-CH 2 CH 2 CH 2 -), butylene group (-CH 2 CH 2 CH 2 CH 2 -), 1,4-phenylene groups (-C 6 H 4 -) and other arylene groups. R' is preferably a linear alkylene group. X is preferably a direct bond.
[0038] Non-limiting examples of preferred monomers from which the structural unit (b-2) is derived include t-butyl acrylate, allyl acrylate, and benzyl acrylate, as well as the following compounds: Based on these examples and the above definitions, a person skilled in the art would be able to determine the structure of the monomer from which the structural unit (b-2) is derived without being bound by the following examples. [ka]
[0039] (3) Structural unit (C) The structural unit (C) is a structural unit derived from an acrylic acid derivative that does not have a carboxy group and does not undergo an elimination reaction due to heat or acid under the same conditions as those in which the structural unit (B) undergoes an elimination reaction due to heat or acid to produce a carboxy group. Therefore, the monomer from which the structural unit (C) is derived is an acrylic acid ester (H 2 C=CHC(=O)OR), but unlike the structural unit (B), the R does not have a carboxyl group as a substituent and does not undergo an elimination reaction. As long as this condition is met, the chemical species of the monomer from which the structural unit (C) is derived is not particularly limited, and a person skilled in the art can appropriately select it based on the reactivity as a monomer and the physical properties to be imparted to the copolymer. In this specification, when the structural unit (C) is said to "not undergo an elimination reaction," it is used to mean that the structural unit (B) does not undergo an elimination reaction under the same conditions as the elimination reaction caused by heat or acid that generates a carboxyl group.
[0040] A preferred monomer from which the structural unit (C) is derived is a polar group-containing olefin monomer represented by the following general formula (3). H 2 C=CH-COOCHZ 1 Z 2 (3) [In general formula (3), Z 1 and Z 2 are each independently Hydrogen atom, Hydroxyl group, a hydrocarbon group having 1 to 10 carbon atoms substituted with a hydroxyl group; an alkyl group having 1 to 30 carbon atoms; a hydrocarbon group having 3 to 20 carbon atoms substituted with an alkoxycarbonyl group having 2 to 10 carbon atoms; a hydrocarbon group having 3 to 20 carbon atoms substituted with an acyloxy group having 2 to 10 carbon atoms; a hydrocarbon group having 2 to 20 carbon atoms substituted with a substituted amino group having 1 to 12 carbon atoms; a hydrocarbon group having 4 to 30 carbon atoms substituted with a substituted silyl group having 3 to 18 carbon atoms; an alkoxycarbonyl group having 2 to 20 carbon atoms; an acyloxy group having 2 to 10 carbon atoms; Amino group, a substituted amino group having 1 to 12 carbon atoms, a substituted silyl group having 3 to 18 carbon atoms; And a hydrocarbon group having 1 to 20 carbon atoms substituted with halogen. In addition, Z is a substituent selected from the group consisting of 1 and Z 2 may be bonded to each other to form a ring.
[0041] In general formula (3), the alkyl group, alkoxycarbonyl group, acyloxy group, substituted amino group, substituted silyl group, and hydrocarbon group may have the same carbon numbers as those explained above in relation to general formula (1). In the general formula (3), Z 1 or Z 2 When one of the groups is a hydroxyl group or an amino group, the other is preferably a hydrogen atom. Therefore, the substituent bonded to the oxygen atom derived from acrylic acid is preferably a methyl group, a hydroxymethyl group, a (substituted) aminomethyl group, a substituted silylmethyl group, or a group having at least two consecutive carbon atoms.
[0042] Non-limiting examples of monomers from which the preferred structural unit (C) is derived are listed below. These are just examples, and there is no limitation on the type of monomer from which the structural unit (C) is derived as long as it satisfies the above conditions. A person skilled in the art can determine the structure of the monomer based on these examples and the above definitions without being bound by the following examples. [ka] [ka]
[0043] (4) Multicomponent polar group-containing olefin copolymer As described above, the multi-component polar group-containing olefin copolymer of the present disclosure is characterized by comprising a structural unit (A) derived from ethylene or an α-olefin, a structural unit (B) having a carboxy group or a structure that generates a carboxy group through an elimination reaction caused by heat or acid, and a structural unit (C) derived from acrylic acid that does not have a carboxy group and does not undergo an elimination reaction caused by heat or acid under the same conditions as those in which the structural unit (B) undergoes an elimination reaction caused by heat or acid to generate a carboxy group.
[0044] The multi-component polar group-containing olefin copolymer of the present disclosure contains at least one type of each of the structural units (A), (B), and (C) described above, and contains a total of three or more types of monomer units. The structural units and the amounts of the structural units in the multi-component polar group-containing olefin copolymer according to the present disclosure will be described. A structure derived from one molecule of each of ethylene or α-olefin, a monomer having a carboxy group or a structure that generates a carboxy group upon elimination reaction by heat or acid, and an acrylic acid monomer that does not have a carboxy group and does not undergo elimination reaction by heat is defined as one structural unit in the multi-component polar group-containing olefin copolymer. The ratio of each structural unit in the multi-component polar group-containing olefin copolymer expressed in mol % is the structural unit amount.
[0045] Amount of structural units of ethylene or α-olefin (A): The structural unit amount of the structural unit (A) according to the present disclosure has a lower limit of 60.000 mol% or more, preferably 70.000 mol% or more, more preferably 80.000 mol% or more, even more preferably 85.000 mol% or more, even more preferably 87.000 mol% or more, and particularly preferably 91.400 mol% or more, and an upper limit selected from 97.999 mol% or less, preferably 97.990 mol% or less, more preferably 97.980 mol% or less, even more preferably 96.980 mol% or less, even more preferably 96.900 mol% or less, and particularly preferably 94.300 mol%. If the amount of structural units derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms is less than the above range, the toughness will be inferior, whereas if it is more than the above range, the crystallinity will be high and the transparency will tend to be poor.
[0046] Amount of structural units of monomer (B) having a carboxy group or a structure that generates a carboxy group upon elimination reaction by heat or acid: The structural unit amount of the structural unit (B) according to the present disclosure has a lower limit of 2.000 mol% or more, preferably 2.900 mol% or more, and an upper limit of 20.000 mol% or less, preferably 15.000 mol% or less, more preferably 10.000 mol% or less, even more preferably 8.000 mol%, and particularly preferably 6.100 mol% or less. If the structural unit amount derived from the olefin monomer is less than the above range, the adhesion to a different material having high polarity is insufficient, and if it is more than the above range, sufficient mechanical properties tend not to be obtained.
[0047] Amount of structural units of acrylic acid-derived monomer (C) which does not have a carboxy group and does not undergo an elimination reaction due to heat or acid under the same conditions as those in which the structural unit (B) undergoes an elimination reaction due to heat or acid to produce a carboxy group: The structural unit amount of the structural unit (C) according to the present disclosure has a lower limit of 0.001 mol% or more, preferably 0.010 mol% or more, more preferably 0.100 mol% or more, even more preferably 0.500 mol% or more, and most preferably 1.900 mol% or more, and an upper limit of 20.000 mol% or less, preferably 15.000 mol% or less, more preferably 10.000 mol% or less, even more preferably 7.000 mol% or less, and particularly preferably 4.800 mol% or less. If the structural unit amount derived from the olefin is less than the above range, the rigidity is insufficient, and if it is more than the above range, the rigidity and toughness tend to be unbalanced.
[0048] The total amount of the structural unit (A), the structural unit (B), and the structural unit (C) must be 100 mol %, but it is preferable to set the amount of the structural unit (A) so that the amounts of the structural units (B) and (C) are within the above ranges.
[0049] Method for measuring the amount of structural units of polar group-containing monomers in multicomponent polar group-containing olefin copolymers: The amount of structural units of the polar group in the multi-component polar group-containing olefin copolymer according to the present disclosure is 13 It can be determined using C-NMR spectroscopy. 13 The C-NMR spectrum is measured, for example, by the following method. 200-250 mg of sample was mixed with o-dichlorobenzene / deuterated bromide benzene (C 6 D 5 The mixture is placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a tetrahydrofuran (Br) solution (volume ratio) of 1.0 to 1.0 ml and hexamethyldisiloxane, a chemical shift standard substance, and then the tube is purged with nitrogen, sealed, heated to dissolve, and the resulting homogeneous solution is subjected to NMR measurement. NMR measurements are performed at 120°C using a Bruker Biospin AV400M NMR instrument equipped with a 10 mm diameter cryoprobe. 13C-NMR measurements are performed using the inverse gate decoupling method with a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation count of 512 or more. The chemical shift is set to 1.98 ppm for the methyl carbon peak of hexamethyldisiloxane, and the chemical shifts of peaks due to other carbons are based on this. Obtained 13 In C-NMR, the content of each comonomer in a copolymer can be analyzed by identifying signals specific to the substituents of the copolymer and comparing their intensities. The positions of the substituents and signals can be referred to publicly known materials, or can be independently identified depending on the sample. Such an analysis method is commonly known to those skilled in the art.
[0050] Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn): The weight average molecular weight (Mw) of the multi-component polar group-containing olefin copolymer according to the present disclosure is usually in the range of 1,000 to 2,000,000, preferably 10,000 to 1,500,000, more preferably 20,000 to 1,000,000, more preferably 31,000 to 800,000, and even more preferably 35,000 to 800,000. If Mw is less than 1,000, physical properties such as mechanical strength and impact resistance are insufficient, and if Mw exceeds 2,000,000, the melt viscosity becomes very high, which may make molding difficult.
[0051] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the multi-component polar group-containing olefin copolymer according to the present disclosure is preferably in the range of 1.5 to 4.0, more preferably 1.6 to 3.3, and even more preferably 1.7 to 3.0. If Mw / Mn is less than 1.5, various processabilities including moldability may become insufficient, and if it exceeds 4.0, mechanical properties may become poor. In the present disclosure, (Mw / Mn) may be expressed as a molecular weight distribution parameter.
[0052] The weight average molecular weight (Mw) in the present disclosure is determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) is determined by further determining the number average molecular weight (Mn) by gel permeation chromatography (GPC), and calculating the ratio of Mw to Mn, Mw / Mn.
[0053] An example of the GPC measurement method according to the present disclosure is also described in the Examples section, but it can be measured using a commercially available device and measurement conditions. The molecular weight is calculated by the standard polystyrene method, and the conversion from the retention volume to the molecular weight can be performed using a calibration curve of the standard polystyrene that has been prepared in advance. The standard polystyrene used is, for example, (F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000) brand, all manufactured by Tosoh Corporation. A calibration curve is created by injecting 0.2 mL of a solution in which each is dissolved in ODCB (containing 0.5 mg / mL BHT) so that the concentration is 0.5 mg / mL. The calibration curve uses a cubic equation obtained by approximating with the least squares method. The viscosity equation [η] = K × Mα used for conversion to molecular weight uses the following values. PS:K=1.38×10 -4 , α=0.7 PE:K = 3.92 x 10 -4 , α=0.733 PP:K = 1.03 x 10 -4 , α=0.78
[0054] Melting point (℃): In the multi-component polar group-containing olefin copolymer of the present disclosure, it is more preferable that the melting point (Tm, ° C.) observed by differential scanning calorimetry (DSC) and the total content [Y] (mol %) of the structural unit (B) and the structural unit (C) satisfy the following formula (I): 50 <Tm<-3.74×[Y]+130···(I) In addition to the total content [Y] (mol%) of the structural units (B) and (C) in the copolymer, the melting point of the copolymer has a large effect on the mechanical properties of the copolymer, and a copolymer with a lower melting point can exhibit better mechanical properties. However, for example, in the case of a binary copolymer of ethylene and (B) as (A), the melting point of the copolymer depends on the content of (B), and it is extremely difficult to make the melting point lower than −3.74 × [Y] + 130 (°C) (where [Y] is the content (mol %) of the structural unit (B)), and sufficient improvement in mechanical properties may not be expected. Therefore, when the melting point of the copolymer according to the present disclosure exceeds -3.74 x [Y] + 130 (°C), improvement in mechanical properties is not expected and sufficient mechanical properties may not be easily exhibited. Also, when the melting point is less than 50°C, it may be difficult to maintain the minimum heat resistance required for an ethylene copolymer.
[0055] The melting point can be determined, for example, using an "EXSTAR6000" manufactured by Seiko Electronics Co., Ltd., by measuring at an isothermal temperature of 40°C for 1 minute, heating from 40°C to 160°C at 10°C / min, isothermal temperature at 160°C for 10 minutes, cooling from 160°C to 10°C at 10°C / min, isothermal temperature at 10°C for 5 minutes, and then heating from 10°C to 160°C at 10°C / min.
[0056] The melting point Tm of the multi-component polar group-containing olefin copolymer according to the present disclosure more preferably satisfies the relationship of formula (I) above, but assuming polyethylene, the melting point is more preferably more than 50° C. and less than 130° C., particularly preferably 60° C. to 128° C., and most preferably 70° C. to 126° C. If it is lower than this range, the heat resistance is insufficient, and if it is higher than this range, the impact resistance may be poor.
[0057] Crystallinity (%): In the multi-component polar group-containing olefin copolymer of the present disclosure, the crystallinity observed by differential scanning calorimetry (DSC) is not particularly limited, but is preferably greater than 0% and not greater than 30%, more preferably greater than 0% and not greater than 25%, and most preferably greater than 5% and not greater than 25%. If the crystallinity is lower than this range, the toughness is insufficient, and if it is higher than this range, the transparency is poor. Note that the crystallinity is an index of transparency, and it can be determined that the lower the crystallinity, the better the transparency. The degree of crystallinity can be determined, for example, by using an "EXSTAR6000" manufactured by Seiko Electric Industries Co., Ltd., determining the heat of fusion from the area of the melting endothermic peak obtained when the temperature is raised from room temperature to 160°C, and dividing the heat of fusion by the heat of fusion of perfectly crystalline polyethylene (HDPE), which is 293 J / g.
[0058] Molecular structure of multi-component polar group-containing olefin copolymer: The multi-component polar group-containing olefin copolymer according to the present disclosure may be a random copolymer, a block copolymer, a graft copolymer, etc., of structural units (A), (B), and (C). Among these, a random copolymer capable of containing a large amount of polar groups may be used. The molecular chain terminal of the multi-component polar group-containing olefin copolymer according to the present disclosure may be any one of the structural units (A), (B) and (C).
[0059] The multi-component polar group-containing olefin copolymer according to the present disclosure may be produced in the presence of a transition metal catalyst in order to make its molecular structure linear. It is known that the molecular structure varies depending on the production method, such as polymerization by a high-pressure radical polymerization process or polymerization using a metal catalyst. The difference in molecular structure can be controlled by selecting the production method. For example, as described in JP 2010-150532 A, the molecular structure can be estimated from the complex modulus measured by a rotational rheometer.
[0060] · Absolute value of complex elastic modulus G * Phase angle δ at =0.1MPa In the multi-component polar group-containing olefin copolymer of the present disclosure, the absolute value of the complex modulus G measured by a rotational rheometer * The phase angle δ at pressure = 0.1 MPa may be 50 degrees to 75 degrees. More specifically, the absolute value of the complex modulus G measured by a rotational rheometer * = Phase angle δ at 0.1 MPa (G *= 0.1 MPa) is 50 degrees or higher, the molecular structure is a linear structure that contains either no long chain branches or a small amount of long chain branches that does not affect the mechanical strength. Absolute value of complex modulus G measured by a rotational rheometer * = Phase angle δ at 0.1 MPa (G * = 0.1 MPa) is lower than 50 degrees, which indicates that the molecular structure contains an excessive amount of long chain branches, and the mechanical strength tends to be inferior. Absolute value of complex modulus G measured by a rotational rheometer * The phase angle δ at G = 0.1 MPa is affected by both the molecular weight distribution and long chain branching, but it is an index of the amount of long chain branching only for those with Mw / Mn ≦ 4, more preferably Mw / Mn ≦ 3. The more long chain branching there is, the higher the δ(G * =0.1MPa) value is small. If Mw / Mn is 1.5 or more, the δ(G * =0.1MPa) value never exceeds 75 degrees.
[0061] The method for measuring the complex elastic modulus is as follows. The sample is placed in a 1.0 mm thick mold for hot pressing, preheated for 5 minutes in a hot press machine with a surface temperature of 180°C, and then the residual gas in the molten resin is degassed by repeatedly applying and depressurizing pressure, and then pressurized to 4.9 MPa and held for 5 minutes. The sample is then transferred to a press machine with a surface temperature of 25°C, and cooled by holding at a pressure of 4.9 MPa for 3 minutes to create a press plate made of the sample with a thickness of approximately 1.0 mm. The press plate made of the sample is processed into a circle with a diameter of 25 mm to use as a sample, and a Rheometrics ARES type rotational rheometer is used as a measuring device for dynamic viscoelastic properties to measure dynamic viscoelasticity under the following conditions in a nitrogen atmosphere. Plate: φ25mm parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2 ~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1 MPa). LogG in the measurement point * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG * The δ value at logG = 5.0 is calculated by linear interpolation. * <5, logG * Using the three largest values, we plot logG on a quadratic curve. * = 5.0.
[0062] Molecular structure of multi-component polar group-containing olefin copolymer: The multi-component polar group-containing olefin copolymer according to the present disclosure may be a random copolymer. An example of the molecular structure of a typical ternary polar group-containing olefin copolymer (1) is shown below. A random copolymer is a copolymer in which the probability of finding a structural unit (A) of ethylene or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) of a polar group-containing monomer, and a structural unit (C) of a nonpolar cyclic olefin at any position in a molecular chain, as shown in the molecular structure example (1) below, is independent of the type of the adjacent structural unit. In addition, the molecular chain terminal of the polar group-containing olefin copolymer may be a structural unit (A) of ethylene or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) of a polar group-containing monomer, or a structural unit (C) of a non-polar cyclic olefin. As shown below, in the molecular structure example (1) of the polar group-containing olefin copolymer, structural units (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms, structural units (B) of a polar group-containing monomer, and structural units (C) of a non-polar cyclic olefin form a random copolymer. [ka] For reference, an example of the molecular structure (2) of an olefin copolymer into which a polar group has been introduced by graft modification is also shown. A part of the olefin copolymer in which structural units (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms and structural units (C) of a non-polar cyclic olefin are copolymerized is graft modified with structural units (B) of a polar group-containing monomer. [ka]
[0063] Methyl branch In the polymer obtained by the polymerization reaction, the monomers are usually linked in a straight line to form a molecular chain that serves as the main chain. In the present invention, the olefin moieties (C=C) of the structural units (A), (B) and (C) are usually linked in a straight line to form a polyethylene chain. In this case, the saturated hydrocarbon chain when the structural unit (A) contains an α-olefin, the group T of the structural unit (B) 1 Ya-X 1 -COOT 2 The part represented by the structural unit (C) -COOCHZ 1 Z 2The moieties shown in the figure will exist as side chains of the polyethylene chain. However, in some cases, the olefin moieties do not form a linear molecular chain but branch. In this case, a structure in which methyl groups exist as side chains is generated, which is called a methyl branch. It is generally known that the number of branches in a polyethylene chain is inversely proportional to the melting point, and the melting point decreases as the number of branches increases, and does not depend on the branching group (Skupov, KM; Piche, L.; Claverie, JP Macromolecules 2008, 41, p. 2309-2310. Please refer to them as necessary). In other words, the more structural units (B) and (C) and methyl branches are contained in a copolymer, the lower the melting point of the copolymer, and the lower the heat resistance and strength of the copolymer. In addition, when the content of structural units (B) and (C) is the same, it is thought that the functionality due to polar groups will be expressed at the same level, and the fewer the methyl branches, the higher the melting point and the higher the heat resistance and strength of the copolymer. Copolymers produced by radical polymerization have a structure with many long-chain branches and short-chain branches irregularly, and have the disadvantage of being insufficient in terms of strength. In the present invention, the number of methyl branches is preferably 50 or less per 1,000 carbons, more preferably 5 or less per 1,000 carbons, even more preferably 3.0 or less, and particularly preferably 1.0 or less, with no particular lower limit, and the lower the better. A smaller number of methyl branches is preferable because it improves heat resistance and strength. The method for measuring the number of methyl branches in a polymer is as described below, and a method that can be normally performed by a person skilled in the art can be used.
[0064] (5) Production of multi-component polar group-containing olefin copolymers The multi-component polar group-containing olefin copolymer according to the present disclosure may be produced in the presence of a transition metal catalyst in order to make its molecular structure linear.
[0065] Polymerization catalyst The type of polymerization catalyst used in the production of the multi-component polar group-containing olefin copolymer according to the present disclosure is not particularly limited as long as it is capable of copolymerizing the monomers from which the structural units (A), (B), and (C) are derived. For example, a Group 5 to 11 transition metal compound having a chelating ligand can be mentioned. Specific examples of preferred transition metals include vanadium atom, niobium atom, tantalum atom, chromium atom, molybdenum atom, tungsten atom, manganese atom, iron atom, platinum atom, ruthenium atom, cobalt atom, rhodium atom, nickel atom, palladium atom, copper atom, etc. Among these, preferred are transition metals of Groups 8 to 11, more preferred are transition metals of Group 10, and particularly preferred are nickel (Ni) and palladium (Pd). These metals may be used alone or in combination. Chelating ligands have at least two atoms selected from the group consisting of P, N, O, and S, and include ligands that are bidentate or multidentate, and are electronically neutral or anionic. Exemplary structures are given in the review by Brookhart et al. (Chem. Rev., 2000, 100, 1169). Preferred examples of bidentate anionic P,O ligands include phosphorus sulfonates, phosphorus carboxylic acids, phosphorus phenols, and phosphorus enolates. Other examples of bidentate anionic N,O ligands include salicylaldiminates and pyridine carboxylic acids, and other examples include diimine ligands, diphenoxide ligands, and diamide ligands.
[0066] The structure of the metal complex obtained from the chelating ligand is represented by the following structural formula (A) and / or (B) in which an arylphosphine compound, an arylarsine compound, or an arylantimony compound, which may have a substituent, is coordinated.
[0067] [ka] [ka] In structural formulas (A) and (B), M represents a transition metal belonging to any one of Groups 5 to 11 of the periodic table of the elements, that is, various transition metals as described above. X 1 is oxygen, sulfur, -SO 3 - or -CO 2 - represents. Y 1 represents carbon or silicon. n represents an integer of 0 or 1. E 1 represents phosphorus, arsenic or antimony. R 1 represents hydrogen or a hydrocarbon group having 1 to 20 carbon atoms. R 2 represents a hydrocarbon group having 1 to 20 carbon atoms. R 3 and R 4 each independently represents hydrogen or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 5 each independently represents hydrogen, a halogen, or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 6 and R 7 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom, OR 2 , CO 2 R 2 , CO 2 M', C(O)N(R 1 ) 2 , C(O)R 2 , S.R. 2 , S.O. 2 R 2 , SOR 2 , O.S.O. 2 R 2 , P(O)(OR 2 ) 2-y (R 1 ) y , C.N., N.H.R. 2 , N(R 2 ) 2 , Si(OR 1 ) 3-x (R1 ) x , OSi(OR 1 ) 3-x (R 1 ) x , NO 2 , S.O. 3 M', PO 3 M' 2 , P(O)(OR 2 ) 2 M' represents an epoxy-containing group. M′ represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium; x represents an integer of 0 to 3; and y represents an integer of 0 to 2. In addition, R 6 and R 7 may be linked to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing a heteroatom selected from oxygen, nitrogen, and sulfur, in which case the ring has 5 to 8 members and may or may not have a substituent on the ring. L 1 represents a ligand coordinated to M. Also, R 3 and L 1 may be bonded to each other to form a ring. Here, the term "may contain heteroatoms" means that heteroatoms such as oxygen, nitrogen, and sulfur are present in the hydrocarbon carbon or methylene group (-CH 2 This means that the presence of a structure in which a hydrogen atom of a hydrocarbon is replaced by a hetero atom, such as an ether structure or a carbonyl group, is permitted.
[0068] The catalyst used in the preparation of the copolymer of the present invention is more preferably a transition metal complex represented by the following structural formula (C). [ka] In structural formula (C), M represents a transition metal belonging to any one of Groups 5 to 11 of the periodic table of the elements, that is, various transition metals as described above. X 1 is oxygen, sulfur, -SO 3- or -CO 2 - represents. Y 1 represents carbon or silicon. n represents an integer of 0 or 1. E 1 represents phosphorus, arsenic or antimony. R 3 and R 4 each independently represents hydrogen or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 5 each independently represents hydrogen, a halogen, or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 8 , R 9 , R 10 and R 11 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom, OR 2 , CO 2 R 2 , CO 2 M', C(O)N(R 1 ) 2 , C(O)R 2 , S.R. 2 , S.O. 2 R 2 , SOR 2 , O.S.O. 2 R 2 , P(O)(OR 2 ) 2-y (R 1 ) y , C.N., N.H.R. 2 , N(R 2 ) 2 , Si(OR 1 ) 3-x (R 1 ) x , OSi(OR 1 ) 3-x (R 1 ) x , NO 2 , S.O. 3 M', PO 3 M' 2 , P(O)(OR 2 ) 2 M' represents an epoxy-containing group. M′ represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium; x represents an integer of 0 to 3; and y represents an integer of 0 to 2. In addition, R 8 ~R 11 A plurality of groups appropriately selected from the above may be linked together to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing a heteroatom selected from oxygen, nitrogen, and sulfur. In this case, the number of ring members is 5 to 8, and the ring may or may not have a substituent. L 1 represents a ligand coordinated to M. Also, R 3 and L 1 may be bonded to each other to form a ring.
[0069] Here, typical catalysts of Group 5 to 11 transition metal compounds having a chelating ligand are known to be the so-called SHOP type and Drent type catalysts. The SHOP catalyst is a catalyst in which a phosphorus-based ligand having an aryl group which may have a substituent is coordinated to nickel metal (see, for example, WO2010-050256). Moreover, the Drent system is a catalyst in which a phosphorus-based ligand having an aryl group which may have a substituent is coordinated to a palladium metal (see, for example, JP-A-2010-202647).
[0070] ·Organometallic compounds: In the production of the multi-component polar group-containing olefin copolymer according to the present disclosure, the polymerization activity can be further increased by contacting a polar group-containing olefin monomer with a small amount of an organometallic compound, and then copolymerizing the monomers from which the structural units (A), (B), and (C) are derived in the presence of the transition metal catalyst. The organometallic compound is an organometallic compound containing a hydrocarbon group which may have a substituent, and can be represented by the following structural formula (H). R 30 nM 30 X 30 mn Structural formula (H) (In the formula, R 30represents a hydrocarbon group having 1 to 12 carbon atoms which may have a substituent, M 30 is a metal selected from the group consisting of groups 1, 2, 12 and 13 of the periodic table; X 30 represents a halogen atom or a hydrogen atom, and m represents M 30 The valence, n, is 1 to m.
[0071] Examples of the organometallic compound represented by the above structural formula (H) include alkylaluminums such as tri-n-butylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, and tri-n-decylaluminum, and alkylaluminum halides such as methylaluminum dichloride, ethylaluminum dichloride, dimethylaluminum chloride, diethylaluminum chloride, and diethylaluminum ethoxide, and preferably trialkylaluminums are selected. More preferably, a trialkylaluminum having a hydrocarbon group with 4 or more carbon atoms is selected, further preferably a trialkylaluminum having a hydrocarbon group with 6 or more carbon atoms is selected, and even more preferably, tri-n-hexylaluminum, tri-n-octylaluminum, or tri-n-decylaluminum is selected, with tri-n-octylaluminum being the most preferably used. The organometallic compound is used in a molar ratio of 10 to the polar group-containing olefin comonomer. -5 ~0.9, preferably 10 -4 ~0.2, more preferably 10 -4 From the viewpoints of polymerization activity and cost, it is preferable to contact the catalyst in an amount of 1 to 0.1.
[0072] Polymerization method for multi-component polar group-containing olefin copolymer: The polymerization method for the multi-component polar group-containing olefin copolymer according to the present disclosure is not limited. An example of the polymerization method is as will be made clear in the examples below. Examples of the polymerization method include slurry polymerization in which at least a part of the produced polymer is made into a slurry in a medium, bulk polymerization in which liquefied monomer itself is used as a medium, gas phase polymerization in vaporized monomer, or high pressure ionic polymerization in which at least a part of the produced polymer is dissolved in monomer liquefied at high temperature and pressure. The polymerization method may be any of batch polymerization, semi-batch polymerization, and continuous polymerization. Furthermore, the polymerization may be a living polymerization, or the polymerization may be carried out while simultaneously causing chain transfer. Furthermore, a so-called chain shuttling agent (CSA) may be used in combination to carry out a chain shuttling reaction or coordinate chain transfer polymerization (CCTP). Specific production processes and conditions are disclosed, for example, in JP-A-2010-260913 and JP-A-2010-202647. When the above-mentioned transition metal catalyst is used in the polymerization reaction, the catalyst is removed by a well-known method such as filtration or reprecipitation in the polymerization of the multi-component polar group-containing olefin copolymer, but the resulting copolymer may contain a trace amount of metal derived from the catalyst. The presence of such a metal element indicates that the copolymer was prepared by a transition metal catalyst, and one aspect of the present invention relates to a multi-component polar group-containing olefin copolymer characterized by containing a transition metal element of Group 10 of the periodic table, particularly nickel or palladium, used as a polymerization catalyst. The content can be measured by means such as ICP-OES. When a transition metal element is contained, its content is 20,000 μg / g or less, preferably 10,000 μg / g or less, more preferably 5,000 μg / g or less, particularly preferably 2,000 μg / g or less, and most preferably 1,000 μg / g or less. The metal content is inversely proportional to the polymerization activity, and decreases as the activity increases. In other words, as the activity increases, the metal content approaches zero.
[0073] (6) Additives The multi-component polar group-containing olefin copolymer according to the present disclosure may contain additives such as antioxidants, light stabilizers, ultraviolet absorbers, metal soaps, hydrochloric acid absorbers, lubricants, antistatic agents, antiblocking agents, colorants, pigments, crosslinking agents, foaming agents, nucleating agents, flame retardants, conductive materials, and fillers, within the scope of the present disclosure.
[0074] The multi-component polar group-containing olefin copolymer of the present invention is excellent in physical properties such as transparency and compatibility derived from each structural unit, and is useful as a material for packaging materials, etc. In addition, the multi-component polar group-containing olefin copolymer of the present invention can be used as a base resin for ionomers under general deprotection reaction conditions. By the deprotection reaction, a carboxy group can be generated from the structure of the structural unit (B) contained in the multi-component polar group-containing olefin copolymer, which generates a carboxy group by a thermal or acid elimination reaction. The conditions of temperature, reagents, reaction atmosphere and solvent, use of additives, reactor, etc. described above for the structural unit (B) can be adopted. The multi-component polar group-containing olefin copolymer of the present invention is also useful as a raw material for the base resin of ionomers. EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0076] [Evaluation method of copolymer] (1) Melting point Tm, heat of fusion ΔH, degree of crystallinity The melting point Tm of the produced olefin copolymer was determined by the following DSC measurement. Using an "EXSTAR6000" manufactured by Seiko Electronics Co., Ltd., the melting point Tm was determined by measurements at 40°C for 1 minute isothermal, heating from 40 to 160°C at 10°C / min, isothermal at 160°C for 10 minutes, cooling from 160 to 10°C at 10°C / min, isothermal at 10°C for 5 minutes, and then heating from 10 to 160°C at 10°C / min. The degree of crystallinity was calculated by calculating the heat of fusion ΔH from the area of the melting endothermic peak obtained when the temperature was raised from room temperature to 160°C, and dividing ΔH by the heat of fusion of perfectly crystalline polyethylene (HDPE), 293 J / g.
[0077] (2) Molecular weight distribution parameter Mw / Mn The molecular weight distribution parameter Mw / Mn of the produced olefin polymer was measured by GPC. Equipment: Alliance GPCV2000 manufactured by Japan Waters Detector: GPCV2000 built-in differential refractometer detector Sample preparation: 3 mg of sample and 3 mL of orthodichlorobenzene (containing 0.1 mg / mL 1,2,4-trimethylphenol) were weighed into a 4 mL vial, and the vial was sealed with a plastic screw cap and a Teflon (registered trademark) septum, after which dissolution was carried out for 2 hours using a Senshu Scientific SSC-9300 high-temperature shaker set at 150° C. After dissolution was complete, it was visually confirmed that there were no insoluble components. Column: Showa Denko Shodex HT-806M x 2 + Showa Denko Shodex HT-G x 1 Preparation of HT-G calibration curve: Four 4 mL glass bottles were prepared, and 0.2 mg of the monodisperse polystyrene standard samples or n-alkanes of the combinations (i) to (iv) below were weighed into each bottle, followed by weighing out 3 mL of ortho-dichlorobenzene (containing 0.1 mg / mL of 1,2,4-trimethylphenol). The bottles were then capped with plastic screw caps and Teflon (registered trademark) septa, and dissolved for 2 hours in a Senshu Scientific SSC-9300 high-temperature shaker set to 150°C. (i) Shodex S-1460, S-66.0, n-Eicosane (ii) Shodex S-1950, S-152, n-tetracontane (iii) Shodex S-3900, Shodex S-565, Shodex S-5.05 (iv)Shodex S-7500, Shodex S-1010, Shodex S-28.5 The vial containing the sample solution was placed in the device, and measurements were performed under the above-mentioned conditions. A chromatogram (a data set of retention time and differential refractometer detector response) was recorded at a sampling interval of 1 s. The retention time (peak apex) of each polystyrene standard sample was read from the obtained chromatogram and plotted against the logarithmic value of the molecular weight. Here, the molecular weights of n-eicosane and n-tetracontane were 600 and 1,200, respectively. The nonlinear least squares method was applied to this plot, and the obtained quartic curve was used as the calibration curve.
[0078] Calculation of molecular weight: Measurement was performed under the above-mentioned conditions, and the chromatogram was recorded at a sampling interval of 1 s. Using this chromatogram, the differential molecular weight distribution curve and average molecular weight values (Mn, Mw, and Mz) were calculated according to the method described in "Size Exclusion Chromatography" by Mori Sadao (Kyoritsu Shuppan), Chapter 4, pp. 51-60. However, in order to correct the molecular weight dependency of dn / dc, the height H from the baseline in the chromatogram was corrected using the following formula (H' = H after correction). Recording of the chromatogram (data acquisition) and calculation of the average molecular weight were performed using a program developed in-house (created with Microsoft Visual Basic 6.0) on a PC installed with Microsoft OS Windows (registered trademark) XP. H' = H / [1.032 + 189.2 / M(PE)] The molecular weight conversion from polystyrene to polyethylene was carried out using the following formula. M(PE) = 0.468 × M(PS) Measurement temperature: 145℃ Concentration: 20mg / 10mL Injection amount: 0.2ml Solvent: orthodichlorobenzene Flow rate: 1.0ml / min
[0079] (3) Comonomer Content The comonomer content of the produced olefin copolymer was determined by the following measurement. Measurement method for the amount of structural units of polar group-containing monomers in multi-component polar group-containing olefin copolymers: The amount of structural units of the polar group in the multi-component polar group-containing olefin copolymer according to the present invention is 13 It can be determined using C-NMR spectroscopy. 13 C-NMR spectra are measured by the following method. 1) 200-250 mg of sample was mixed with o-dichlorobenzene / deuterated bromide benzene (C 6 D 5 The mixture is placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a tetrahydrofuran (Br) solution (volume ratio) of 1.0 to 1.0 ml and hexamethyldisiloxane, a chemical shift standard substance, and then the tube is purged with nitrogen, sealed, heated to dissolve, and the resulting homogeneous solution is subjected to NMR measurement. The NMR measurements were performed using an AV400 NMR instrument (Bruker Japan) equipped with a 10 mmφ cryoprobe. 13 The C-NMR measurement conditions were a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation count of 512 or more, using the inverse gate decoupling method. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shifts of the C signals were based on this.
[0080] 4) Analysis method for comonomer content <e tba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 It is detected at 79.6 to 78.8 in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (E) 〕 Here, I (tBA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (tBA) ×7) / 2 <e tba nba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methylene signal of the butoxy group of nBA was detected at 64.1 to 63.4 ppm in the C-NMR spectrum and 79.6 to 78.8 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (nBA) +I (E) 〕 Total amount of nBA (mol%) = I (nBA) ×100 / 〔I (tBA) +I (nBA) +I (E) 〕 Here, I (tBA) , I (nBA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (nBA) =I 64.1~63.4 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (nBA) ×7-I (tBA) ×7) / 2 <e tba iba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methylene signal of the isobutoxy group of iBA is detected at 70.5 to 69.8 ppm, and the methyl signal of the isobutoxy group is detected at 19.5 to 18.9 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (iBA) +I (E) 〕 Total amount of iBA (mol%) = I (iBA) ×100 / 〔I (tBA) +I (iBA) +I (E) 〕 Here, I (tBA) , I (iBA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (iBA) =(I 70.5~69.8 +I 19.5~18.9 ) / 3 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (iBA) ×7-I (tBA) ×7) / 2 <e tba ma> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methyl carbon signal of the methoxy group of methyl acrylate (MA) was detected at 51.1 to 50.4 ppm in the C-NMR spectrum from 79.6 to 78.8 ppm. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (MA) +I (E) 〕 Total amount of MA (mol%) = I (MA) ×100 / 〔I (tBA) +I (MA) +I (E) 〕 Here, I (tBA) , I (MA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (MA) =I 51.1~50.4 / 2 I(E)=(I 180.0~135.0 +I 120.0~2.0 -I (MA) ×4-I (tBA) ×7) / 2 <e tba ea> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methyl carbon signal of the ethoxy group of ethyl acrylate (EA) was detected at 14.7 to 14.1 ppm, and the methylene carbon signal was detected at 60.0 to 59.3 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (EA) +I (E) 〕 Total amount of EA (mol%) = I (EA) ×100 / 〔I (tBA) +I (EA) +I (E) 〕 Here, I (tBA) , I (EA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (EA) =(I 14.7~14.1 +I 60.0~59.3 ) / 2 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (EA) ×5-I (tBA) ×7) / 2 <e tba c6> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methylene signal of 1-hexene was detected at 23.4 to 23.1 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (C6) +I (E) 〕 Total C6 content (mol%) = I (C6) ×100 / 〔I (tBA) +I (C6) +I (E) 〕 Here, I (tBA) , I (C6) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (C6) =I 23.4~23.1 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (C6) ×6-I (tBA) ×7) / 2 <e tba va> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The C-NMR spectrum shows signals at 79.6 to 78.8 ppm, and the vinyl acetate methyl signal at 20.9 to 20.2 ppm. Using these signal intensities, the amount of comonomer was calculated from the following formula: Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (VA) +I (E) 〕 Total amount of VA (mol%) = I (VA) ×100 / 〔I (tBA) +I (VA) +I (E) 〕 Here, I (tBA) , I (VA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (VA) =I 20.9~20.2 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (VA) ×4-I (tBA) ×7) / 2 <e tba mma> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The C-NMR spectrum shows a signal intensity of 79.6 to 78.8 ppm, and the methoxy signal of methyl methacrylate is detected at 52.5 to 49.5 ppm. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I (tBA) ×100 / 〔I (tBA) +I (MMA) +I (E) 〕 Total amount of MMA (mol%) = I (MMA) ×100 / 〔I (tBA) +I (MMA) +I (E) 〕 Here, I (tBA) , I (MMA) , I (E) are the quantities shown in the following formulas, respectively. I (tBA) =I 79.6~78.8 I (MMA) =I 52.5~49.5 I (E) =(I 180.0~135.0 +I 120.0~2.0 -I (MMA) ×5-I (tBA) ×7) / 2 In the following description, when the amount of each copolymer is indicated by "<0.1" including an inequality sign, this means that it is present as a structural unit in the copolymer, but the amount is less than 0.1 mol%, taking into account significant digits.
[0081] (4) Tensile test Using the resins of each Example and Comparative Example, a sheet having a thickness of 1 mm was prepared by the method described in JIS K7151 (1995) (cooling method A), and a tensile test was performed at a temperature of 23°C according to JIS K7161 (2014) using a small 5B type test piece described in JIS K7162 (1994) that was punched out of the sheet, to measure the tensile modulus, tensile stress at break, and tensile elongation at break. The test speed was 10 mm / min.
[0082] (5) Tensile impact strength test 1) How to prepare samples for tensile impact strength test The resins of each Example and Comparative Example were placed in a 1 mm thick mold for hot pressing, preheated for 5 minutes in a hot press machine with a surface temperature of 180 ° C., and then repeatedly pressurized and depressurized to melt the resin and degas the residual gas in the molten resin, and further pressurized at 4.9 MPa and held for 5 minutes. Then, under a pressure of 4.9 MPa, the mold was gradually cooled at a rate of 10 ° C. / min, and when the temperature had dropped to near room temperature, the molded plate was removed from the mold. The obtained molded plate was conditioned for 48 hours or more in an environment of a temperature of 23 ± 2 ° C. and a humidity of 50 ± 5 ° C. A test piece having the shape of ASTM D1822 Type-S was punched out from the press plate after conditioning to obtain a tensile impact strength test sample.
[0083] 2) Tensile impact strength test conditions The tensile impact strength was measured by using the resins of each Example and Comparative Example with reference to JIS K 7160-1996 Method B. The only difference from JIS K 7160-1996 was the shape of the test piece. As for other measurement conditions, the test was performed according to the method of JIS K 7160-1996, and the tensile impact strength was measured.
[0084] (6) Absolute value of complex elastic modulus G * = Phase angle δ at 0.1 MPa (G * =0.1MPa) The resin of each Example and Comparative Example was placed in a 1.0 mm thick mold for hot pressing, preheated for 5 minutes in a hot press machine with a surface temperature of 180°C, and then repeatedly pressurized and depressurized to remove residual gas in the molten resin. The mold was then pressurized at 4.9 MPa and held for 5 minutes. The mold was then transferred to a press machine with a surface temperature of 25°C and held at a pressure of 4.9 MPa for 3 minutes to cool the mold, producing a press plate made of a sample with a thickness of about 1.0 mm. The press plate made of the sample was processed into a circle with a diameter of 25 mm to form a sample, and a Rheometrics ARES type rotational rheometer was used as a measuring device for dynamic viscoelastic properties to measure dynamic viscoelasticity under the following conditions in a nitrogen atmosphere. Plate: φ25mm parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2 ~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1MPa). * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG * The δ value at logG = 5.0 was calculated by linear interpolation. * <5, logG * Using the three largest values, we plot logG on a quadratic curve. * The δ value at =5.0 was extrapolated.
[0085] (7) Change from ester structure to carboxylic acid structure by IR spectrum analysis The copolymer was melted at 180° C. for 3 minutes and compression molded to prepare a film having a thickness of about 50 μm. This film was analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer. Product name: FT / IR-6100_Manufactured by JASCO Corporation Measurement method: transmission method Detector: TGS Accumulation count: Auto (16~64 times) Resolution: 4.0cm -1 Measurement wavelength: 5000~500cm -1
[0086] (8) Number of methyl branches per 1,000 carbons To quantify the number of methyl branches, 13 C-NMR was used. 13 The C-NMR measurement conditions were a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation count of 512 or more, using the inverse gate decoupling method. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shift of the C signal was used as a reference, and the number of methyl branches was quantified by the integral ratio of the methyl group signals derived from the methyl branches. 13 The method for quantifying the number of methyl branches by C-NMR is known to those skilled in the art.
[0087] (9) Metal content in copolymer ICP-OES was used to quantify the metal content. Approximately 0.1 to 0.3 g of the sample was placed in a Kelder flask, and sulfuric acid was added and heated to perform wet decomposition. The decomposition liquid was transferred to a measuring flask. The volume was adjusted to a constant value, and the Ni in the solution was measured by ICP-OES. Product name: ICP-OES, Thermo Fisher Scientific, iCAP6500DUO
[0088] (10)Vp activity The productivity (Vp activity) of the produced olefin copolymer was calculated by the following formula. Productivity (Vp activity) = {yield of olefin copolymer produced (kg)} ÷ {amount of catalyst (mol) × polymerization time (h)}
[0089] [Metal complexes] The B-27DM / Ni complex was synthesized according to the synthesis example described in JP 2013-043871 A, and the ligand B-27DM represented by the following chemical formula was used. In addition, bis-1,5-cyclooctadiene nickel(0) (Ni(COD) 2 (called "COD"), B-27DM and Ni(COD) 2 A nickel complex was synthesized by reacting with 1:1 (molar ratio). In the formula, "Me" means a methyl group, "C 6 F 5 " represents a pentafluorophenyl group. [ka]
[0090] The B-423 / Ni catalyst used the ligand B-423, which is represented by the following chemical formula. Ni(acac)2 (51.4 mg) was weighed into a 50 ml eggplant flask and dissolved in toluene (10 ml) to prepare a 20 mM Ni(acac)2 toluene solution. The resulting solution was blue and transparent. The Ni(acac)2 toluene solution (10 ml) obtained here was added to an eggplant flask containing B-423 (111.7 mg) and stirred at room temperature for 1 minute to obtain a purple transparent solution. Here, the concentration of the reaction product was calculated assuming that B-423 and Ni(acac) reacted in a 1:1 ratio to form a nickel complex. In the formula, "Me" represents a methyl group and "iPr" represents an isopropyl group. [ka]
[0091] Examples and Comparative Examples Example 1 1) Preparation of ethylene / t-butyl acrylate (tBA) / n-butyl acrylate (nBA) terpolymer (E / tBA / nBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of tri-n-octylaluminum (TNOA), 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 4.3 ml (30 mmol) of a predetermined amount of n-butyl acrylate (nBA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 38 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / nBA resin 1. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 980 μg / g.
[0092] 2) Preparation of ethylene / acrylic acid (AA) / n-butyl acrylate (nBA) terpolymer (E / AA / nBA) by modification: In a 50 ml separable flask, 4 g of the resin 1, 0.08 g of paratoluenesulfonic acid monohydrate, and 18.5 ml of toluene were added and stirred at 105° C. for 4 hours. 18.5 ml of ion-exchanged water was added, stirred, and allowed to stand, and then the aqueous layer was extracted. Thereafter, the addition and extraction of ion-exchanged water was repeated until the pH of the extracted aqueous layer reached 5 or more. The solvent was removed from the remaining solution by distillation under reduced pressure, and the solution was dried until it reached a constant weight, yielding E / AA / nBA resin I. The results of the physical property measurements are shown in Table 3. In the IR spectrum of Resin I, the 1730 cm -1 The peak at around 850 cm due to the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The quantitative Ni analysis by ICP-OES was 960μg / g.
[0093] Example 2 1) Preparation of ethylene / t-butyl acrylate (tBA) / isobutyl acrylate (iBA) terpolymer (E / tBA / iBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 4.3 ml (30 mmol) of a predetermined amount of isobutyl acrylate (iBA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 45 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / iBA resin 2. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 1130 μg / g.
[0094] 2) Preparation of ethylene / acrylic acid (AA) / isobutyl acrylate (iBA) terpolymer (E / AA / iBA) by modification: Using the above-mentioned Resin 2, E / AA / iBA Resin II was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 3. In the IR spectrum of the above resin II, the 1730 cm -1 The peak at around 850 cm due to the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The nearby peaks were increasing. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 960μg / g.
[0095] Example 3 1) Preparation of ethylene / t-butyl acrylate (tBA) / methyl acrylate (MA) terpolymer (E / tBA / MA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 73 mg (0.20 mmol) of TNOA, 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 2.7 ml (30 mmol) of a predetermined amount of methyl acrylate (MA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 75 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / MA resin 3. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 960 μg / g.
[0096] 2) Preparation of ethylene / acrylic acid (AA) / methyl acrylate (MA) terpolymer (E / AA / MA) by modification: Using the resin 3, an E / AA / MA resin III was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 3. In the IR spectrum of the above resin III, the 1730 cm -1 The peak at around 850 cm due to the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The nearby peaks were increasing. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 950μg / g.
[0097] Example 4 1) Preparation of ethylene / t-butyl acrylate (tBA) / ethyl acrylate (EA) terpolymer (E / tBA / EA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 73 mg (0.20 mmol) of TNOA, 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 3.3 ml (30 mmol) of a predetermined amount of ethyl acrylate (EA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 49 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / EA resin 4. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 1,000 μg / g.
[0098] 2) Preparation of ethylene / acrylic acid (AA) / methyl acrylate (EA) terpolymer (E / AA / EA) by modification: Using the above-mentioned Resin 4, E / AA / EA Resin IV was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 3. In the IR spectrum of the above resin IV, the carbonyl group of the ester is at 1730 cm -1 The peak at around 850 cm due to the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The nearby peaks were increasing. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 930μg / g.
[0099] Comparative Example 1 1) Preparation of ethylene / t-butyl acrylate (tBA) / 1-hexene (C6) terpolymer (E / tBA / C6): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 3.8 ml (30 mmol) of a predetermined amount of 1-hexene (C6: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 22 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / C6 resin 5. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 770 μg / g.
[0100] 2) Preparation of ethylene / acrylic acid (AA) / 1-hexene (C6) terpolymer (E / AA / C6) by modification: Using the resin 5, E / AA / C6 resin V was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 3. In the IR spectrum of the resin V, the 1730 cm -1 The peak at 850 cm originates from the t-butyl group of the t-butyl ester. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around 10 ...
[0101] Comparative Example 2 1) Preparation of ethylene / t-butyl acrylate (tBA) / vinyl acetate (VA) terpolymer (E / tBA / VA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 2.8 ml (30 mmol) of a predetermined amount of vinyl acetate (VA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 52 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / VA resin 6. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 880 μg / g.
[0102] 2) Preparation of ethylene / acrylic acid (AA) / vinyl acetate (VA) terpolymer (E / AA / VA) by modification: Using the resin 6, an E / AA / VA resin VI was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 3. In the IR spectrum of the above resin VI, the 1730 cm -1 The peak at 850 cm originates from the t-butyl group of the t-butyl ester. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around 10 ...
[0103] Comparative Example 3 1) Preparation of ethylene / t-butyl acrylate (tBA) / methyl methacrylate (MMA) terpolymer (E / tBA / MMA): A 2.4-liter autoclave equipped with a stirring blade was charged with dry toluene (1.0 liter), 55 mg (0.15 mmol) of TNOA, 8.7 ml (60 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 3.2 ml (30 mmol) of a predetermined amount of methyl methacrylate (MMA: comonomer 2). The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.2 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 1.0 MPa. After the adjustment was completed, 10 ml (200 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 23 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and further dried under reduced pressure until a constant weight was reached to obtain E / tBA / MMA resin 7. The results are shown in Tables 1 and 2. The Ni quantitative analysis result by ICP-OES was 800 μg / g.
[0104] 2) Preparation of ethylene / acrylic acid (AA) / methyl methacrylate (MMA) terpolymer (E / AA / MMA) by modification: Using the resin 7, an E / AA / VA resin VII was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 3. In the IR spectrum of Resin VII, the 1730 cm -1 The peak at 850 cm originates from the t-butyl group of the t-butyl ester. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around 10 ...
[0105] Example 5 1) Preparation of ethylene / t-butyl acrylate (tBA) / n-butyl acrylate (nBA) terpolymer (E / tBA / nBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 29.1 ml (200 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 8.6 ml (60 mmol) of a predetermined amount of n-butyl acrylate (nBA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.3 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 3.3 MPa. After the adjustment was completed, 24 ml (480 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 92 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then filtered, washed, and recovered, and then dried under reduced pressure until it reached a constant weight, yielding E / tBA / nBA resin 8. The results are shown in Tables 4 and 6. The Ni quantitative analysis result by ICP-OES was 210 μg / g. In the tables, "no data" means that no measurement was performed.
[0106] 2) Preparation of ethylene / acrylic acid (AA) / n-butyl acrylate (nBA) terpolymer (E / AA / nBA) by modification: Using the resin 8, E / AA / nBA resin VIII was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the table, "no data" means that no measurements were performed. In the IR spectrum of the resin VIII, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 210 μg / g.
[0107] Example 6 1) Preparation of ethylene / t-butyl acrylate (tBA) / n-butyl acrylate (nBA) terpolymer (E / tBA / nBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 29.1 ml (200 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 11.4 ml (80 mmol) of a predetermined amount of n-butyl acrylate (nBA: comonomer 2) were charged. The temperature of the autoclave was raised to 80° C. with stirring, and nitrogen was fed until the pressure reached 0.3 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 3.3 MPa. After the adjustment was completed, 24 ml (480 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 180 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then recovered by filtration and washing, and further dried under reduced pressure until a constant weight was reached, yielding E / tBA / nBA resin 9. The results are shown in Tables 4 and 6. The Ni quantitative analysis result by ICP-OES was 210 μg / g.
[0108] 2) Preparation of ethylene / acrylic acid (AA) / n-butyl acrylate (AA) terpolymer (E / BA / nBA) by modification: Using the above-mentioned Resin 9, E / AA / nBA Resin IX was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin IX, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 210 μg / g.
[0109] Example 7 Preparation of ethylene / t-butyl acrylate (tBA) / n-butyl acrylate (nBA) terpolymer (E / tBA / nBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 29.1 ml (200 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 7.1 ml (50 mmol) of a predetermined amount of n-butyl acrylate (nBA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.3 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 3.3 MPa. After the adjustment was completed, 18 ml (360 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 88 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then recovered by filtration and washing, and further dried under reduced pressure until a constant weight was reached, yielding E / tBA / nBA resin 10. The results are shown in Tables 4 and 6. The Ni quantitative analysis result by ICP-OES was 164 μg / g.
[0110] 2) Preparation of ethylene / acrylic acid (AA) / n-butyl acrylate (nBA) terpolymer (E / BA / nBA) by modification: Using the resin 10, an E / AA / nBA resin X was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin X, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 160 μg / g.
[0111] Example 8 Preparation of ethylene / t-butyl acrylate (tBA) / isobutyl acrylate (iBA) terpolymer (E / tBA / iBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, a predetermined amount of 17.0 ml (115 mmol) of t-butyl acrylate (tBA: comonomer 1), and a predetermined amount of 14.0 ml (100 mmol) of isobutyl acrylate (iBA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.3 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 3.3 MPa. After the adjustment was completed, 24 ml (480 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 120 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then recovered by filtration and washing, and further dried under reduced pressure until a constant weight was reached, yielding E / tBA / iBA resin 11. The results are shown in Tables 4 and 6. The Ni quantitative analysis result by ICP-OES was 240 μg / g.
[0112] 2) Preparation of ethylene / acrylic acid (AA) / isobutyl acrylate (iBA) terpolymer (E / BA / iBA) by modification: Using the resin 11, E / AA / iBA resin XI was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin XI, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 230 μg / g.
[0113] Example 9 Preparation of ethylene / t-butyl acrylate (tBA) / isobutyl acrylate (iBA) terpolymer (E / tBA / iBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, a predetermined amount of 28.0 ml (190 mmol) of t-butyl acrylate (tBA: comonomer 1), and a predetermined amount of 3.0 ml (22 mmol) of isobutyl acrylate (iBA: comonomer 2) were charged. The temperature of the autoclave was raised to 90° C. with stirring, and nitrogen was fed until the pressure reached 0.3 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 3.3 MPa. After the adjustment was completed, 24 ml (480 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 55 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then recovered by filtration and washing, and further dried under reduced pressure until a constant weight was reached, yielding E / tBA / iBA resin 12. The results are shown in Tables 4 and 6. The Ni quantitative analysis result by ICP-OES was 200 μg / g.
[0114] 2) Preparation of ethylene / acrylic acid (AA) / isobutyl acrylate (iBA) terpolymer (E / BA / iBA) by modification: Using the resin 12, E / AA / iBA resin XII was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin XII, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The quantitative Ni analysis by ICP-OES was 190 μg / g.
[0115] Example 10 Preparation of ethylene / t-butyl acrylate (tBA) / isobutyl acrylate (iBA) terpolymer (E / tBA / iBA): Into a 2.4 L autoclave equipped with a stirring blade, dry toluene (1.0 L), 55 mg (0.15 mmol) of TNOA, 27.5 ml (189 mmol) of a predetermined amount of t-butyl acrylate (tBA: comonomer 1), and 1.0 ml (7 mmol) of a predetermined amount of isobutyl acrylate (iBA: comonomer 2) were charged. The temperature of the autoclave was raised to 100° C. with stirring, and nitrogen was fed until the pressure reached 0.3 MPa. Then, ethylene was fed into the autoclave to adjust the pressure to 3.3 MPa. After the adjustment was completed, 24 ml (480 μmol) of B-27DM / Ni catalyst was injected with nitrogen to initiate copolymerization. After polymerization for 29 minutes, the reaction was stopped by cooling and depressurizing. The reaction solution was poured into 1 liter of acetone to precipitate the polymer, which was then recovered by filtration and washing, and further dried under reduced pressure until a constant weight was reached, yielding E / tBA / iBA resin 13. The results are shown in Tables 4 and 6. The Ni quantitative analysis result by ICP-OES was 210 μg / g.
[0116] 2) Preparation of ethylene / acrylic acid (AA) / isobutyl acrylate (iBA) terpolymer (E / BA / iBA) by modification: Using the resin 13, an E / AA / iBA resin XIII was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin XIII, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the 1000 nm increased. This confirmed the decomposition of t-butyl ester and the generation of carboxylic acid. The Ni quantitative analysis result by ICP-OES was 210 μg / g.
[0117] Example 11 1) Preparation of ethylene / t-butyl acrylate (tBA) / isobutyl acrylate (iBA) terpolymer (E / tBA / iBA): Internal volume 1.6m 3 Into an autoclave equipped with a stirring blade, dry toluene (1000 L), 0.0375 kg (0.256 mol) of TNOA, and predetermined amounts of 4.4 kg (35 mol) of t-butyl acrylate (tBA: comonomer 1) and 1.6 kg (12 mol) of isobutyl acrylate (iBA: comonomer 2) were charged. The temperature of the autoclave was raised to 95° C. with stirring, and then ethylene was supplied to the autoclave to adjust the pressure to 0.8 MPa. After the adjustment, B-423 / Ni catalyst was fed (3 mmol / min) to carry out copolymerization. During the reaction, the temperature was kept at 95°C, ethylene was fed so as to maintain the pressure, and tBA and iBA were fed so as to obtain ethylene:tBA:iBA=92.0:5.4:2.6 (molar ratio). After polymerization for 515 minutes, the reaction was stopped to obtain E / tBA / iBA resin 14. The results are shown in Tables 5 and 7.
[0118] 2) Preparation of ethylene / acrylic acid (AA) / isobutyl acrylate terpolymer (E / AA / iBA) by modification: Using the resin 14, E / AA / iBA resin XIV was obtained in the same manner as in 2) of Example 1. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin XIV, the 1730 cm -1 The peak at around 850 cm originating from the t-butyl group of the t-butyl ester decreased. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around the carboxyl group increased, confirming the decomposition of t-butyl ester and the production of carboxylic acid.
[0119] Comparative Example 4 Comparative material: Ethylene / methacrylic acid copolymer (E / MAA) A polar group-containing olefin copolymer (manufactured by Mitsui DuPont Polychemicals Co., Ltd., brand: Nucrel N1560), which is a copolymer of ethylene and methacrylic acid and produced by a high-pressure radical process, was used as a comparative raw material. The results of the physical property measurements are shown in Table 8.
[0120] Comparative Example 5 Preparation of ethylene / t-butyl acrylate (tBA) copolymer (E / tBA): Internal volume 1.6m 3 Into an autoclave equipped with a stirring blade, dry toluene (1000 L), 50 g (0.14 mol) of TNOA, and a predetermined amount of 6.3 kg (49 mol) of t-butyl acrylate (tBA: comonomer 1) were charged. The temperature of the autoclave was raised to 100° C. with stirring, and then ethylene was supplied to the autoclave to adjust the pressure to 0.8 MPa. After the adjustment was completed, B-27DM / Ni catalyst (160 mmol) was fed to initiate copolymerization. During the reaction, the temperature was kept at 100°C, and B-27DM / Ni catalyst (160 mmol) was further fed in several portions. Ethylene was fed so as to maintain the pressure, and tBA was fed so as to give an ethylene:tBA ratio of 94.4:5.6 (molar ratio). After polymerization for 240 minutes, the reaction was stopped to obtain E / tBA resin 15. The results are shown in Tables 5 and 7.
[0121] 2) Preparation of ethylene / acrylic acid (AA) copolymer (E / AA): E / AA resin XV was obtained in the same manner as in 2) of Example 1 using resin 15. The results of the physical property measurements are shown in Table 8. In the IR spectrum of the resin XV, the 1730 cm -1 The peak at 850 cm originates from the t-butyl group of the t-butyl ester. -1 The peak at 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) has disappeared. -1 The peak around 1000 nm increased, confirming that the ester had been thermally decomposed.
[0122] Comparative Example 6 Ethylene / methacrylic acid / isobutyl acrylate copolymer (E / MAA / iBA): A polar group-containing olefin copolymer (methacrylic acid content = 4 wt%, isobutyl acrylate content = 16 wt%) produced by a high pressure radical process was used as a copolymer of ethylene, methacrylic acid and isobutyl acrylate (resin XVI). The results of physical property measurements are shown in Table 8.
[0123] [Table 1]
[0124] [Table 2]
[0125] [Table 3]
[0126] [Table 4]
[0127] [Table 5]
[0128] [Table 6]
[0129] [Table 7]
[0130] [Table 8]
[0131] From Table 2, it can be seen that resins 1 to 4, which are copolymers using acrylic acid ester as comonomer 2 in Examples 1 to 4, have significantly lower crystallinity and higher transparency under the same feeding conditions, compared to resins 5 to 7, which are copolymers using α-olefin, vinyl ester, and methyl methacrylate as comonomer 2 in Comparative Examples 1 to 3. If an attempt is made to achieve the same transparency as resins 1 to 4 by using α-olefin, vinyl ester, and methyl methacrylate as comonomer 2, a large amount of comonomer is required, which is relatively inferior in terms of economy to acrylic acid ester. From Table 3, it can be seen that Resins I to IV, which are acid copolymers made from Resins 1 to 4 in Examples 1 to 4, have a significantly lower degree of crystallinity and higher transparency than Resins V to VII, which are acid copolymers made from Resins 5 to 7 in Comparative Examples 1 to 3. This suggests that Resins 1 to 4 maintain high transparency even after being made into acid copolymers. In addition, Resins I to IV have a larger phase angle δ than Resins V to VII, and therefore are thought to exhibit superior mechanical strength. From the above, Resins I to IV have achieved improvements in not only mechanical strength but also transparency compared to known resins. In Table 8, compared with Comparative Example 4 produced by radical polymerization, Resins VIII to XII and XIV of the acid copolymer obtained from Examples 5 to 9 and 11 have high tensile elongation at break and tensile impact strength. Furthermore, Resins VIII, IX, X, XII and XIV also have high tensile stress at break. Furthermore, Resins IX and XIV have low crystallinity and high transparency. Furthermore, Resin XIII of the acid copolymer obtained from Example 10 has a tensile modulus that is extremely higher than that of Comparative Example 4, and is found to have a good balance of physical properties. Resins VIII to XIV have a larger phase angle than Comparative Example 4, and are considered to show good mechanical strength. From the above, Examples 5 to 11 have a relatively better balance of rigidity, toughness and transparency than Comparative Example 4. In Table 8, the acid copolymer resins VIII to XIV obtained from Examples 5 to 11 have higher tensile stress at break, tensile elongation at break, and tensile impact strength, lower crystallinity, and larger phase angle than the acid copolymer resin XV obtained from Comparative Example 5. From the above, Examples 5 to 11 have a relatively better balance of rigidity, toughness, and transparency than Comparative Example 5. In Table 8, compared with Resin XVI of Comparative Example 6 produced by radical polymerization, Resins VIII to XIV of the acid copolymers obtained from Examples 5 to 11 have high tensile modulus of elasticity and tensile stress at break, and a large phase angle. Furthermore, Resins VIII to XII have high tensile impact strength. And Resins VIII, IX, XI, and XIV have low crystallinity and good transparency. Therefore, Examples 5 to 11 have a relatively better balance of elasticity, rigidity, and transparency than Comparative Example 6.
[0132] The results of measuring the physical properties of the copolymers obtained in the Examples and Comparative Examples are summarized in Figures 1 and 2. According to these figures, the samples of the Comparative Examples are significantly inferior to the other samples in terms of stiffness, strength, and toughness, while the samples of the Examples show well-balanced values in all physical properties. In other words, it can be seen that the copolymers of the present invention have well-balanced physical properties and are easy to use.< / e> < / e> < / e> < / e> < / e> < / e> < / e> < / e>
Claims
1. A structural unit (A) derived from ethylene or an α-olefin, A structural unit (B) having a carboxy group or a structure that generates a carboxy group upon elimination reaction by heat or acid, and a structural unit (C) derived from acrylic acid which does not have a carboxy group and does not undergo an elimination reaction due to heat or acid under the same conditions as those under which the structural unit (B) undergoes an elimination reaction due to heat or acid to produce a carboxy group; A multi-component polar group-containing olefin copolymer comprising:
2. at least one structural unit (A) selected from the group consisting of structural units derived from ethylene and structural units derived from an α-olefin having 3 to 20 carbon atoms; At least one structural unit (B) selected from the group consisting of a structural unit (b-1) derived from a polar group-containing olefin monomer represented by general formula (1) and a structural unit (b-2) derived from a polar group-containing olefin monomer represented by general formula (2), A structural unit (C) derived from a polar group-containing olefin monomer represented by the following general formula (3), The multi-component polar group-containing olefin copolymer according to claim 1 , H 2 C=CH-T 1 ・・・(1) [In general formula (1), T 1 teeth, Carboxy group, an alkoxycarbonyl group having 2 to 20 carbon atoms substituted by one or more carboxy groups; A hydrocarbon group having 1 to 30 carbon atoms and substituted with one or more carboxy groups. an alkoxy group having 1 to 20 carbon atoms substituted by one or more carboxy groups; an acyloxy group having 1 to 20 carbon atoms substituted by one or more carboxy groups; a substituted amino group having 1 to 12 carbon atoms substituted with one or more carboxy groups; A substituted silyl group having 1 to 18 carbon atoms and substituted with one or more carboxy groups. It is.] H 2 C=CH-X-COOT 2 ・・・(2) [In general formula (2), T 2 teeth, t-butyl group, Allyl group Benzyl group -CR a R b -O-R c (Here, R a is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, R b , R c are each a hydrocarbon group having 1 to 10 carbon atoms, R b and R c may be taken together to represent a divalent hydrocarbon group having 1 to 8 carbon atoms in which one or more methylene groups may be replaced by an ether group or an ester group, and each group may have a hydrocarbon substituent having 1 to 4 carbon atoms. is a substituent selected from the group consisting of: X is a direct bond or -COO-R'- (wherein R' is a divalent hydrocarbon group having 1 to 30 carbon atoms). H 2 C=CH-COOCHZ 1 Z 2 ・・・(3) [In general formula (3), Z 1 and Z 2 are each independently Hydrogen atoms, Hydroxyl group, a hydrocarbon group having 1 to 10 carbon atoms substituted with a hydroxyl group, Alkyl group having 1 to 30 carbon atoms a hydrocarbon group having 3 to 20 carbon atoms substituted with an alkoxycarbonyl group having 2 to 10 carbon atoms; a hydrocarbon group having 3 to 20 carbon atoms substituted by an acyloxy group having 2 to 10 carbon atoms, A hydrocarbon group having 2 to 20 carbon atoms substituted with a substituted amino group having 1 to 12 carbon atoms. A hydrocarbon group having 4 to 30 carbon atoms substituted with a substituted silyl group having 3 to 18 carbon atoms. Alkoxycarbonyl group having 2 to 20 carbon atoms Acyloxy group having 2 to 10 carbon atoms Amino group Substituted amino group having 1 to 12 carbon atoms Substituted silyl group having 3 to 18 carbon atoms and a halogen-substituted hydrocarbon group having 1 to 20 carbon atoms. is a substituent selected from the group consisting of 1 and Z 2 may be bonded to each other to form a ring.
3. Z in the general formula (3) 1 and Z 2 However, each independently, Hydrogen atoms, Alkyl group having 1 to 30 carbon atoms a hydrocarbon group having 3 to 20 carbon atoms substituted with an alkoxycarbonyl group having 2 to 10 carbon atoms; Alkoxycarbonyl group having 2 to 20 carbon atoms Acyloxy group having 2 to 10 carbon atoms and a halogen-substituted hydrocarbon group having 1 to 20 carbon atoms. The multi-component polar group-containing olefin copolymer according to claim 1 or 2, wherein the substituent is selected from the group consisting of:
4. T in the general formula (2) 2 but, t-butyl group, -CR a R b -O-R c (Here, R a , R b , R c is as defined in claim 1) The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 3, wherein the substituent is selected from the group consisting of:
5. T in the general formula (2) 2 The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 4, wherein is a t-butyl group.
6. The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 5, characterized in that the number of methyl branches contained in the multi-component polar group-containing olefin copolymer is 5 or less per 1,000 carbon atoms.
7. Absolute value of complex modulus G measured by a rotational rheometer * The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 6, wherein the phase angle δ at σ = 0.1 MPa is 50 degrees to 75 degrees.
8. The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 7, characterized in that it contains 0.1 to 20.0 mol % of the structural unit (B).
9. The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 8, characterized in that it contains 0.5 to 20.0 mol % of the structural unit (C) derived from the polar group-containing olefin monomer.
10. The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 9, characterized in that the weight average molecular weight / number average molecular weight (Mw / Mn) measured by gel permeation chromatography (GPC) is 1.5 or more and 4.0 or less.
11. The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 10, characterized in that the melting point (Tm, ° C.) observed by differential scanning calorimetry (DSC) and the total content [Y] (mol %) of the structural unit (B) and the structural unit (C) derived from the polar group-containing olefin monomer satisfy the following formula (I): 50<Tm<-3.74×[Y]+130...(I)
12. The multi-component polar group-containing olefin copolymer according to any one of claims 1 to 11, further comprising 20,000 μg / g or less of a transition metal element of Group 10 of the periodic table as measured by ICP-OES.
13. The multi-component polar group-containing olefin copolymer according to claim 12, wherein the transition metal of Group 10 of the periodic table is nickel or palladium.
14. The multi-component polar group-containing olefin copolymer according to any one of claims 2 to 13, characterized in that the structural unit (B) is at least one selected from the group consisting of structural units (b-2) derived from a polar group-containing olefin monomer represented by the general formula (2):
15. A method for producing the multi-component polar group-containing olefin copolymer according to claim 1, wherein the structural unit (B) is a structural unit having a carboxy group, the method comprising a step of thermally decomposing the multi-component polar group-containing olefin copolymer according to claim 14 at 80 to 350° C. or a step of hydrolyzing the copolymer with an acid catalyst.
Citation Information
Patent Citations
Ionically crosslinked ethylene copolymers
JP1977135392A
Process for producing ethyleneeethylacrylateeacrylic acid polymer
JP1978057295A
Preparation of alpha-olefin-(METH)acrylic acid ester copolymer, and alpha-olefin-(METH)acrylic acid ester copolymer
JP2009132898A
Olefin copolymer containing fluorine atom and polar group
JP2016222911A
JP1972023490U