Nitride phosphor and light-emitting device
The nitride phosphor with a tailored composition addresses the need for enhanced red light emission in plant growth lighting, achieving improved plant growth outcomes and efficiency by balancing red component ratios in the emission spectrum.
Patent Information
- Application Number
- JP2024129729
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Existing nitride phosphors for plant growth do not adequately adjust the emission intensity of red light based on the type of plant, necessitating a phosphor with a higher proportion of red components on the longer wavelength side for optimal plant growth.
A nitride phosphor with a specific composition (Ca s Sr. t EU u Si v Al w N x) is developed, where s, t, u, v, w, and x are within defined ranges, ensuring a high ratio of red components in the wavelength range of 700 nm to 780 nm, enhancing the emission spectrum with a balanced ratio of first and second red component values.
The nitride phosphor achieves a higher intensity of red components on the longer wavelength side, promoting stem elongation and flower bud formation in plants, while maintaining high luminous efficiency and reducing self-absorption, thus improving plant growth lighting.
Smart Images

Figure 2024153901000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to nitride phosphors and light emitting devices. [Background technology]
[0002] It has been proposed to use a light emitting device that combines a far-red phosphor having a peak wavelength in the range of 700 nm or more and 800 nm or less with a light emitting element that emits excitation light as a light source for growing plants (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2014 / 103671 Summary of the Invention [Problem to be solved by the invention]
[0004] Not only far-red phosphors, but also nitride phosphors that emit red light may be attracting attention as phosphors that constitute light sources for plant growth, as they are effective for plant growth. When using nitride phosphors as light sources for plant growth, depending on the type of plant to be grown and in order to promote the desired growth of the plant, it may be necessary to have an emission intensity of red light on the longer wavelength side of the emission spectrum of the nitride phosphor. Therefore, an object of one embodiment of the present disclosure is to provide a nitride phosphor having an emission spectrum that contains a large amount of red components on the longer wavelength side. [Means for solving the problem]
[0005] The first aspect is a nitride phosphor having a composition represented by the following formula (I), in which a ratio of a first red component value, which is the integral of the emission intensity in a wavelength range of 620 nm or more and less than 700 nm to a total component value, which is the integral of the emission intensity in a wavelength range of 500 nm or more and 830 nm or less, is 0.5 or more and 0.63 or less, and a ratio of a second red component value, which is the integral of the emission intensity in a wavelength range of 700 nm or more and 780 nm or less, to a total component value, is 0.27 or more and 0.37 or less.
[0006] Ca s Sr t EU u S v Al w N x (I)
[0007] In formula (I), s, t, u, v, w and x satisfy the following conditions: 0.82≦s≦0.905, 0≦t≦0.04, 0.017≦u≦0.042, 0.89≦s+t+u≦0.922, 0.8≦v≦1.2, 0.8≦w≦1.2, 1.8≦v+w≦2.2, and 2.5≦x≦3.2.
[0008] A second aspect is a light emitting device comprising: a fluorescent member containing the nitride phosphor having an emission peak wavelength in a wavelength range of 640 nm or more and 700 nm or less; and a light emitting element having an emission peak wavelength in a wavelength range of 365 nm or more and 500 nm or less. Effect of the Invention
[0009] According to one embodiment of the present disclosure, it is possible to provide a nitride phosphor having an emission spectrum that contains a large amount of red components on the longer wavelength side. [Brief description of the drawings]
[0010] [Figure 1] 2 is an example of an emission spectrum showing emission intensity versus wavelength of a nitride phosphor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In addition, the content of each component in a composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. In this specification, the relationship between the color name and the chromaticity coordinate, the relationship between the wavelength range of light and the color name of monochromatic light, etc. are in accordance with JIS Z8110. The half-width of a phosphor means the wavelength width of the emission spectrum where the emission intensity is 50% of the maximum emission intensity in the emission spectrum of the phosphor. The average particle size of a phosphor is the volume average particle size, and refers to the particle size corresponding to 50% of the volume cumulative from the small diameter side in the volume-based particle size distribution. The particle size distribution of a phosphor is measured using a particle size distribution measuring device by the pore electrical resistance method (electrical detection zone method) based on the Coulter principle. Hereinafter, an embodiment of the present invention will be described in detail. However, the embodiments described below are merely examples of nitride phosphors and light emitting devices for embodying the technical ideas of the present invention, and the present invention is not limited to the nitride phosphors and light emitting devices described below.
[0012] Nitride Phosphors The nitride phosphor according to this embodiment is a red-emitting phosphor having a composition represented by the following formula (I). In addition, in the emission spectrum of the nitride phosphor, when the integral value of the emission intensity in the wavelength range of 500 nm to 830 nm is the total component value, the integral value of the emission intensity in the wavelength range of 620 nm to less than 700 nm is the first red component value, and the integral value of the emission intensity in the wavelength range of 700 nm to 780 nm is the second red component value, the ratio of the first red component value to the total component value (first red component value / total component value; hereinafter, also referred to as the first red component ratio) is, for example, 0.5 to 0.63, and the ratio of the second red component value to the total component value (second red component value / total component value; hereinafter, also referred to as the second red component ratio) is, for example, 0.27 to 0.37.
[0013] Ca s Sr t EU u S v Al w Nx (I)
[0014] In formula (I), s, t, u, v, w and x satisfy the following conditions: 0.82≦s≦0.905, 0≦t≦0.04, 0.017≦u≦0.042, 0.89≦s+t+u≦0.922, 0.8≦v≦1.2, 0.8≦w≦1.2, 1.8≦v+w≦2.2, and 2.5≦x≦3.2.
[0015] The nitride phosphor has a specific composition and the first red component ratio and the second red component ratio are in specific ranges, so that the nitride phosphor can have an emission spectrum with a high intensity of the red component on the longer wavelength side (for example, 700 nm or more and 780 nm or less).
[0016] The total component value, the first red component value, and the second red component value of the nitride phosphor are calculated by integrating the emission intensity in a predetermined range in the emission spectrum obtained at an excitation wavelength of 450 nm. Here, the emission intensity in the emission spectrum may be an absolute value or a relative value. Specifically, the emission spectrum is measured at room temperature (25°C ± 5°C) using a quantum efficiency measuring device (e.g., QE-2000, manufactured by Otsuka Electronics Co., Ltd.).
[0017] In the nitride phosphor, the first red component ratio may be, for example, 0.5 or more and 0.63 or less, preferably 0.52 or more, 0.54 or more, or 0.55 or more, and preferably 0.62 or less, 0.61 or less, or 0.6 or less. The second red component ratio may be, for example, 0.27 or more and 0.37 or less, preferably 0.28 or more, 0.29 or more, or 0.30 or more, and preferably 0.36 or less, or 0.35 or less. Furthermore, the sum of the first red component ratio and the second red component ratio may be, for example, 0.85 or more and 0.95 or less, preferably 0.88 or more or 0.90 or more, and preferably 0.94 or less, or 0.92 or less. When the first red component ratio and the second red component ratio are in the above range, there is a tendency to obtain an emission spectrum with a higher intensity of the red component on the longer wavelength side.
[0018] In the emission spectrum of the nitride phosphor, the ratio of the first red component value to the second red component value (first red component value / second red component value) may be, for example, 0.7 or more and 2.5 or less, and is preferably 0.9 or more, 1 or more, or 1.1 or more, and preferably 2.2 or less, 2.1 or less, or 2 or less. If the ratio of the first red component value to the second red component value is within the above range, for example, when used as a light source for growing plants, stem elongation and flower bud formation tend to be promoted.
[0019] The nitride phosphor absorbs light in the range of 250 nm to 500 nm, which is the range from ultraviolet light to the short wavelength side of visible light. By using an excitation light source having an emission peak wavelength in this range, a light emitting device with high emission efficiency can be provided. In particular, it is preferable to use an excitation light source having a main emission peak wavelength in the range of 250 nm to 410 nm or 410 nm to 480 nm, and it is more preferable to use an excitation light source having a main emission peak wavelength in the range of 420 nm to 470 nm. The emission spectrum of the nitride phosphor has an emission peak wavelength in the range of, for example, 640 nm to 700 nm, and preferably in the range of 650 nm to 690 nm. The half width in the emission spectrum of the nitride phosphor is, for example, 70 nm to 130 nm, and preferably 80 nm to 100 nm.
[0020] The composition of the nitride phosphor includes calcium (Ca), europium (Eu), silicon (Si), aluminum (Al), and nitrogen (N), and may include strontium (Sr) as necessary. The composition of the nitride phosphor may include, when aluminum is 0.95 moles, a molar content ratio of calcium may be, for example, 0.82 to 0.905, preferably 0.85 to 0.9, or 0.86 to 0.895. The composition of the nitride phosphor may include, when aluminum is 0.95 moles, a molar content ratio of strontium may be, for example, 0 to 0.04, preferably 0.01 to 0.035, or 0.02 to 0.033. The composition of the nitride phosphor may be, for example, 0.017 to 0.042 in moles of europium, preferably 0.02 to 0.04, or 0.025 to 0.035, when aluminum is 0.95 moles. The composition of the nitride phosphor may be, for example, 0.8 to 1.2 in moles of silicon, preferably 0.9 to 1.1, or 0.95 to 1.05, when aluminum is 0.95 moles. The composition of the nitride phosphor may be, for example, 0.018 to 0.047 in moles of europium to the total moles of calcium, strontium, and europium, preferably 0.02 to 0.042, or 0.025 to 0.038, when aluminum is 0.95 moles.
[0021] In the composition of the nitride phosphor, a part of calcium and strontium may be replaced with at least one other element selected from the group consisting of magnesium (Mg), barium (Ba), lithium (Li), sodium (Na), potassium (K), and boron (B). When calcium and strontium are replaced with other elements in the composition of the nitride phosphor, the ratio of the total number of moles of other elements to the total number of moles of calcium and strontium may be, for example, 0.025 or more and 0.5 or less, preferably 0.4 or less, or 0.3 or less, and preferably 0.03 or more.
[0022] The nitride phosphor may have a composition represented by the above formula (I). In formula (I), preferably, s, t, u, v, w, and x may satisfy 0.82≦s≦0.905, 0≦t≦0.04, 0.017≦u≦0.042, 0.0.89≦s+t+u≦0.922, 0.8≦v≦1.2, 0.8≦w≦1.2, 1.8≦v+w≦2.2, and 2.8≦x≦3.2. In formula (I), s, t, and u may satisfy, for example, 0.018≦u / (s+t+u)≦0.047, and preferably 0.02≦u / (s+t+u)≦0.045, or 0.025≦u / (s+t+u)≦0.04.
[0023] In nitride phosphors, europium (Eu), a rare earth, is the luminescence center. However, the luminescence center in this embodiment is not limited to europium, and it is also possible to use a part of the luminescence center replaced with another rare earth metal or alkaline earth metal and co-activated with Eu. Eu, a divalent rare earth ion, 2+ If an appropriate host is selected, the compound will exist stably and emit light.
[0024] The volume average particle diameter of the nitride phosphor is 10 μm or more, and from the viewpoint of luminous efficiency, 13 μm or more is preferable, and 14 μm or more is more preferable. The volume average particle diameter is, for example, 30 μm or less, and preferably 28 μm or less. The larger the volume average particle diameter of the nitride phosphor particles, the higher the absorption rate of the excitation light and the luminous efficiency tend to be. In this way, by applying a nitride phosphor having excellent optical properties to a light emitting device described later, the luminous efficiency of the light emitting device is further improved. In addition, it is preferable that the nitride phosphor contains particles having the above volume average particle diameter value with a high frequency. In other words, it is preferable that the particle size distribution is distributed in a narrow range. By using a phosphor with a small variation in particle size distribution, color unevenness is further suppressed, and a light emitting device with a better color tone can be obtained.
[0025] Method for producing nitride phosphor The method for producing a nitride phosphor includes preparing a raw material mixture including a Eu source including Eu atoms, a Group 2 metal source including at least Ca atoms, an Al source including Al atoms, and a Si source including Si atoms, and heat-treating the raw material mixture. The raw material mixture may have a molar content ratio of each atom that satisfies the composition ratio represented by the formula (I), for example. The temperature of the heat treatment may be, for example, 1800°C or more and 2200°C or less.
[0026] By adjusting the content ratio of Eu atoms, Ca atoms, Sr atoms, Al atoms, and Si atoms in the raw material mixture to a predetermined ratio, it is possible to efficiently produce a nitride phosphor having an emission spectrum with a high intensity of the red component on the longer wavelength side.
[0027] Examples of the Eu source contained in the raw material mixture include europium compounds, europium metal alone, and europium alloys. Examples of europium compounds include oxides, hydroxides, nitrides, oxynitrides, fluorides, and chlorides containing europium. Specific examples of europium compounds include europium oxide (Eu2O3), europium nitride (EuN), and europium fluoride (EuF3), and it is preferable to use at least one selected from the group consisting of these. Europium nitride (EuN) is composed only of elements in the desired phosphor composition, so that it is possible to more effectively suppress the inclusion of impurities. In addition, europium oxide (Eu2O3) and europium fluoride (EuF3) may act as fluxes, and are preferably used. Europium compounds may be used alone or in combination of two or more.
[0028] The europium compound may be appropriately selected from commercially available products, or a desired europium compound may be manufactured and used. For example, europium nitride can be obtained by pulverizing the raw material europium in an inert gas atmosphere, and nitriding the obtained powder by heat treatment in a nitrogen atmosphere or an ammonia atmosphere. The average particle size of the pulverized europium is, for example, 0.1 μm or more and 10 μm or less. The heat treatment temperature is, for example, 600° C. or more and 1200° C. or less, and the heat treatment time is, for example, 1 hour or more and 20 hours or less. The obtained europium nitride can be subjected to a pulverization treatment, for example, in an inert gas atmosphere.
[0029] The raw material mixture may be a mixture in which at least a part of the Eu source is replaced with a metal compound, a simple metal, an alloy, or the like of a rare earth element such as scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), etc. Examples of the metal compound include oxides, hydroxides, nitrides, oxynitrides, fluorides, chlorides, etc.
[0030] The purity of the Eu source (e.g., europium compound) is, for example, 95% by weight or more, and preferably 99.5% by weight or more. By making the purity a predetermined value or more, the influence of impurities can be reduced and the luminous intensity of the phosphor can be further improved.
[0031] The Group 2 metal source contained in the raw material mixture contains at least Ca and is at least one selected from the group consisting of Mg, Sr and Ba, and preferably contains at least Ca and Sr.
[0032] Examples of the Group 2 metal source include alkaline earth metal compounds, alkaline earth metals alone, alloys containing alkaline earth metals, Mg compounds, Mg alone, and alloys containing Mg. Examples of the alkaline earth metal compounds and Mg compounds include hydrides, oxides, hydroxides, nitrides, oxynitrides, chlorides, amide compounds, and imide compounds containing alkaline earth metals or Mg, with hydrides and nitrides being preferred. The Group 2 metal source may also include Li, Na, K, B, Al, and the like.
[0033] The Group 2 metal compound may be appropriately selected from commercially available products, or a desired Group 2 metal compound may be manufactured and used. For example, calcium nitride can be obtained by pulverizing calcium as a raw material in an inert gas atmosphere, and nitriding the obtained powder by heat treatment in a nitrogen atmosphere. The heat treatment temperature is, for example, 600°C or higher and 900°C or lower, and the heat treatment time is, for example, 1 hour or higher and 20 hours or lower. The obtained calcium nitride can be subjected to a pulverization treatment, for example, in an inert gas atmosphere. Strontium nitride can be obtained in the same manner as calcium nitride, but unlike calcium nitride, the amount of nitrogen contained can be changed by the production conditions.
[0034] The purity of the Group 2 metal source is, for example, 95% by weight or more, and preferably 99.5% by weight or more. By making the purity a predetermined value or more, the influence of impurities can be reduced and the luminous intensity of the phosphor can be further improved.
[0035] Examples of the Al source contained in the raw material mixture include aluminum compounds, aluminum metal alone, and aluminum alloys. Examples of the aluminum compounds include oxides, hydroxides, nitrides, oxynitrides, fluorides, and chlorides containing aluminum. Specific examples of the aluminum compounds include aluminum nitride (AlN), aluminum oxide (Al2O3), and aluminum hydroxide (Al(OH)3). It is preferable to use at least one selected from the group consisting of these, and aluminum nitride is more preferable. Since aluminum nitride is composed only of elements of the desired phosphor composition, it is possible to more effectively suppress the inclusion of impurities. Compared to aluminum compounds containing, for example, oxygen and hydrogen, aluminum nitride can reduce the influence of these elements, and does not require a nitriding reaction compared to a simple metal. The aluminum compounds may be used alone or in combination of two or more.
[0036] The aluminum compound may be appropriately selected from commercially available products, or a desired aluminum compound may be produced and used. For example, aluminum nitride can be produced by a direct nitriding method of aluminum.
[0037] The raw material mixture may be a mixture in which at least a part of the Al source is replaced with a metal compound, a simple metal, an alloy, etc. of a Group III element such as gallium, indium, vanadium, chromium, cobalt, etc. Examples of the metal compound include oxides, hydroxides, nitrides, oxynitrides, fluorides, chlorides, etc.
[0038] The purity of the Al source (e.g., aluminum compound) is, for example, 95% by weight or more, and preferably 99% by weight or more. By making the purity a predetermined value or more, the influence of impurities can be reduced and the luminous intensity of the phosphor can be further improved.
[0039] Examples of the Si source contained in the raw material mixture include silicon compounds and silicon elemental substance. Examples of the silicon compounds include oxides, hydroxides, nitrides, oxynitrides, fluorides, chlorides, etc. containing silicon. Specific examples of the silicon compounds include silicon oxide, silicon nitride, silicon oxynitride, silicates, etc., and it is preferable to use at least one selected from the group consisting of these, and silicon nitride is more preferable. Since silicon nitride is composed only of elements of the desired phosphor composition, it is possible to more effectively suppress the inclusion of impurities. Compared to silicon compounds containing, for example, oxygen and hydrogen, silicon nitride can reduce the influence of these elements, and does not require a nitriding reaction compared to a metal elemental substance. The silicon compounds may be used alone or in combination of two or more.
[0040] The silicon compound may be appropriately selected from commercially available products, or a desired silicon compound may be manufactured and used. For example, silicon nitride can be obtained by pulverizing raw material silicon in an inert gas atmosphere and nitriding the obtained powder by heat treatment in a nitrogen atmosphere. The heat treatment temperature is, for example, 800°C or higher and 2000°C or lower, and the heat treatment time is, for example, 1 hour or higher and 20 hours or lower. The obtained silicon nitride can be subjected to, for example, a pulverization treatment in an inert gas atmosphere.
[0041] The raw material mixture may be a mixture in which a part of the Si source is replaced with a metal compound, a simple metal, an alloy, etc. of a Group IV element such as germanium, tin, titanium, zirconium, hafnium, etc. Examples of the metal compound include oxides, hydroxides, nitrides, oxynitrides, fluorides, chlorides, etc.
[0042] The purity of the Si source (e.g., silicon compound) is, for example, 95% by weight or more, and preferably 99% by weight or more. By making the purity a predetermined value or more, the influence of impurities can be reduced and the luminous intensity of the phosphor can be further improved.
[0043] The raw material mixture may further contain at least one metal fluoride. Examples of the metal fluoride include alkaline earth metal fluorides and alkali metal fluorides. The metal fluoride may contain at least an alkaline earth metal, and may further contain Li, Na, K, B, Al, etc. in addition to the alkaline earth metal. The alkaline earth metal contained in the alkaline earth metal fluoride is at least one selected from the group consisting of Mg, Ca, Sr, and Ba, and preferably contains at least Ca and at least one selected from the group consisting of Mg, Sr, and Ba, and more preferably contains at least one of Ca and Sr. In addition, the metal fluoride may also serve as at least one of the Eu source and the Group 2 metal source. The content of the metal fluoride in the raw material mixture may be, for example, an amount such that the molar content ratio of fluorine atoms to Al is 0.02 or more and 0.3 or less, and the molar content ratio is preferably 0.02 or more and less than 0.3, more preferably 0.02 or more and 0.27 or less, even more preferably 0.03 or more and 0.18 or less, and even more preferably 0.04 or more and 0.13 or less. By making the molar content ratio equal to or more than the lower limit, the effect of the flux can be sufficiently obtained. If a certain amount of flux is contained, the effect of the flux becomes saturated and no effect can be expected even if a larger amount is contained, so by making it equal to or less than the upper limit, the effect of the flux can be obtained without containing more than necessary.
[0044] The purity of the metal fluoride is, for example, 95% by weight or more, and preferably 99% by weight or more. By making the purity a predetermined value or more, the influence of impurities can be reduced and the luminous intensity of the phosphor can be further improved. The metal fluoride may be appropriately selected from commercially available products, or a desired metal fluoride may be manufactured and used.
[0045] The raw material mixture may further contain a flux such as a halide other than the metal fluoride. Examples of the halide include chlorides of rare earth elements, alkali metals, etc. When the raw material mixture contains a flux, the content of the flux is, for example, 20 mass % or less, preferably 10 mass % or less, and more preferably 1 mass % or less, based on the metal fluoride.
[0046] The raw material mixture may further contain silicon nitride particles prepared separately as necessary. When the raw material mixture contains silicon nitride particles, the content of the silicon nitride particles in the total amount of the raw material mixture may be, for example, 1 mass % or more and 50 mass % or less.
[0047] The raw material mixture can be prepared by mixing a Eu source, a Group 2 metal element source, an Al source, and a Si source in a predetermined ratio. The mixing ratio of each component in the raw material mixture may be selected so that i, j, k, l, m, and n in the following formula (Ia) satisfy the following requirements defined in formula (Ia). Ca i Sr j EU k S l Al m N n (Ia) In the formula, i, j, k, l, m, and n may satisfy 0.91≦i≦0.98, 0≦j≦0.06, 0.02≦k≦0.05, 0.8≦i+j+k≦1.1, 0.8≦l≦1.2, 0.8≦m≦1.2, 1.8≦l+m≦2.2, 2.5≦n≦3.2, and preferably satisfy 0.91≦i≦0.97, 0≦j≦0.05, 0.03≦k≦0.045, 0.9≦i+j+k≦1, 0.9≦l≦1.1, 0.9≦m≦1.1, 1.9≦l+m≦2.1, 2.7≦n≦3.1. In addition, i, j, and k may satisfy 0.02≦k / (i+j+k)≦0.05, and may satisfy 0.03≦k / (i+j+k)≦0.04.
[0048] In the method for producing a nitride phosphor, the molar content ratio of Eu contained in the nitride phosphor can be set to a predetermined range. If the molar content ratio of the Eu source to the total number of moles of the Eu source and the second metal element source in the raw material mixture or the nitride phosphor is the Eu ratio, the ratio of the Eu ratio in the nitride phosphor to the Eu ratio in the raw material mixture (nitride phosphor / raw material mixture) can be, for example, 0.8 or more and 0.9 or less, preferably 0.82 or more, or 0.84 or more, and preferably 0.86 or less, or less than 0.85.
[0049] The raw material mixture can be obtained by weighing out the components constituting the raw material mixture to a desired mixing ratio, and then mixing the components by a mixing method using a ball mill, a mixing method using a mixer such as a Henschel mixer or a V-type blender, a mixing method using a mortar and pestle, etc. Mixing can be performed by dry mixing, or by adding a solvent or the like and performing wet mixing.
[0050] By heat-treating the obtained raw material mixture, a nitride phosphor having desired luminescence characteristics can be obtained. The heat treatment temperature of the raw material mixture is, for example, 1200°C or higher, and may be preferably 1500°C or higher, 1800°C or higher, or 1900°C or higher. The heat treatment temperature is, for example, 2200°C or lower, and preferably 2150°C or lower, 2100°C or lower, or 2050°C or lower. By heat-treating at a temperature equal to or higher than the above lower limit, Eu is easily introduced into the crystal, and the desired nitride phosphor is efficiently formed. Furthermore, when the heat treatment temperature is equal to or lower than the above upper limit, decomposition of the formed nitride phosphor tends to be suppressed.
[0051] The atmosphere in the heat treatment of the raw material mixture is preferably an atmosphere containing nitrogen gas, and more preferably a substantially nitrogen gas atmosphere. By using an atmosphere containing nitrogen gas, silicon contained in the raw material can be nitrided. Also, decomposition of the raw material and phosphor, which are nitrides, can be suppressed. When the atmosphere in the heat treatment of the raw material mixture contains nitrogen gas, it may contain other gases such as rare gases such as hydrogen and argon, carbon dioxide, carbon monoxide, oxygen, and ammonia in addition to nitrogen gas. The content of nitrogen gas in the atmosphere in the heat treatment of the raw material mixture is, for example, 90% by volume or more, and preferably 95% by volume or more. By setting the content of gases containing elements other than nitrogen to a predetermined value or less, the decrease in the luminous intensity of the phosphor caused by the formation of impurities by those gas components is suppressed.
[0052] The pressure in the heat treatment of the raw material mixture can be, for example, normal pressure to 200 MPa. From the viewpoint of suppressing decomposition of the nitride phosphor produced, the higher the pressure, the more preferable, and the gauge pressure is preferably 0.1 MPa to 200 MPa, and more preferably 0.6 MPa to 1.2 MPa, which has fewer restrictions on industrial equipment.
[0053] The heat treatment of the raw material mixture may be performed at a single temperature, or may be performed in multiple stages including two or more heat treatment temperatures. When performing heat treatment in multiple stages, for example, a first stage of heat treatment may be performed at 800°C or more and 1400°C or less, and then the temperature may be gradually increased to perform a second stage of heat treatment at 1500°C or more and 2100°C or less.
[0054] In the heat treatment of the raw material mixture, for example, the temperature is raised from room temperature to a predetermined temperature. The temperature rise time is, for example, 1 hour or more and 48 hours or less, preferably 2 hours or more and 24 hours or less, and more preferably 3 hours or more and 20 hours or less. If the temperature rise time is equal to or more than the lower limit, the particle growth of the nitride phosphor tends to proceed sufficiently, and Eu tends to easily enter the crystals of the phosphor particles.
[0055] In the heat treatment of the raw material mixture, a holding time at a predetermined temperature may be set. The holding time is, for example, 0.5 hours or more and 48 hours or less, preferably 1 hour or more and 30 hours or less, and more preferably 2 hours or more and 20 hours or less. By setting the holding time to the above lower limit or more, uniform particle growth can be further promoted. Also, by setting the holding time to the above upper limit or less, decomposition of the phosphor can be further suppressed.
[0056] The time required for the temperature drop from a predetermined temperature to room temperature in the heat treatment of the raw material mixture is, for example, 0.1 hours or more and 20 hours or less, preferably 1 hour or more and 15 hours or less, and more preferably 3 hours or more and 12 hours or less. A holding time at an appropriately selected temperature may be provided during the temperature drop from the predetermined temperature to room temperature. This holding time is adjusted, for example, so as to further improve the emission intensity of the nitride phosphor. The holding time at the predetermined temperature during the temperature drop is, for example, 0.1 hours or more and 20 hours or less, and preferably 1 hour or more and 10 hours or less. The temperature during the holding time is, for example, 1000°C or more and less than 1800°C, and preferably 1200°C or more and 1700°C or less.
[0057] The heat treatment of the raw material mixture can be carried out, for example, using a gas pressure electric furnace. The heat treatment of the raw material mixture can be carried out, for example, by filling the raw material mixture into a crucible, boat, or the like made of a carbon material such as graphite or a boron nitride (BN) material. In addition to carbon materials and boron nitride materials, alumina (Al2O3), Mo materials, and the like can also be used. Among them, it is preferable to use a crucible or boat made of boron nitride material.
[0058] After the heat treatment of the raw material mixture, a sizing step may be included in which the nitride phosphor obtained by the heat treatment is subjected to a combination of processes such as crushing, pulverization, and classification. The sizing step can obtain a powder of a desired particle size. Specifically, after the nitride phosphor is coarsely pulverized, it can be pulverized to a predetermined particle size using a general pulverizer such as a ball mill, jet mill, or vibration mill. However, excessive pulverization may cause defects on the silicon nitride particle surface, resulting in a decrease in brightness. If particles of different particle sizes are present as a result of pulverization, classification can be performed to adjust the particle size.
[0059] Light-emitting device The light emitting device includes a fluorescent member containing the nitride phosphor, and a light emitting element having an emission peak wavelength in the wavelength range of 365 nm to 500 nm. The light emitting device includes a light emitting element of a gallium nitride compound semiconductor that emits light on the short wavelength side of visible light (for example, in the range of 380 nm to 485 nm) and has an emission peak wavelength in the range of 365 nm to 500 nm, and a molded body on which the light emitting element is placed. The molded body is formed by integrally molding a first lead, a second lead, and a resin part. The molded body forms a recess having a bottom surface and a side surface, and the light emitting element is placed on the bottom surface of the recess. The light emitting element has a pair of positive and negative electrodes, and the pair of positive and negative electrodes are electrically connected to the first lead and the second lead via wires, respectively. The light emitting element is covered with a fluorescent member. The fluorescent member contains, for example, a first phosphor, a second phosphor, and a resin as phosphors that convert the wavelength of light from the light emitting element.
[0060] The light emitting element has an emission peak wavelength in the wavelength range of 365 nm to 500 nm, preferably in the wavelength range of 380 nm to 470 nm, and more preferably in the wavelength range of 400 nm to 460 nm. By using a light emitting element having an emission peak wavelength within this wavelength range as an excitation light source, it is possible to configure a light emitting device that emits a mixed color light of the light from the light emitting element and the fluorescence from the phosphor. Furthermore, a part of the light emitted from the light emitting element can be effectively used as a part of the light emitted to the outside from the light emitting device, so that a light emitting device with high light emitting efficiency can be obtained.
[0061] The half-width of the emission spectrum of the light-emitting element can be, for example, 30 nm or less. As the light-emitting element, it is preferable to use, for example, a semiconductor light-emitting element using a nitride-based semiconductor. By using a semiconductor light-emitting element as the excitation light source, it is possible to obtain a stable light-emitting device that is highly efficient, has high linearity of output relative to input, and is resistant to mechanical shock.
[0062] The fluorescent member contains at least the first phosphor, and may contain other phosphors, resins, etc. as necessary. Details of the nitride phosphor contained in the first phosphor are as described above, and the preferred aspects are also the same.
[0063] The fluorescent member may contain a second phosphor in addition to the first phosphor. By including the second phosphor in the fluorescent member, it is possible to configure a light emitting device that emits a mixed color of light emitted by the light emitting element, the first phosphor, and the second phosphor.
[0064] The second phosphor may be, for example, a phosphor having a composition represented by any one of the following formulae (IIa) to (IIi), and preferably contains at least one phosphor having a composition represented by a formula selected from the group consisting of these, and more preferably contains at least one phosphor having a composition represented by formulae (IIa) to (IIf) in that a light emitting device having high color rendering properties and luminous efficiency can be obtained. The light emitting device may contain one type of the second phosphor alone, or may contain two or more types in combination.
[0065] (Y,Gd,Tb,Lu)3(Al,Ga)5O 12 :Ce (IIa) (Ba,Sr,Ca)2SiO4:Eu (IIb) (Ca,Sr)8MgSi4O 16 (Cl,F,Br)2:Eu (IIc) (Ba,Sr,Ca)Ga2S4:Eu (IId) (Ba,Sr,Ca)2Si5N8:Eu(IIe) K2(Si,Ge,Ti)F6:Mn (IIf) S 6-p Al p O p N 8-p :Eu(0 <p≦4.2) (IIg) (La,Y)3Si6N 11 :Ce (IIh) (Sr,Ca,Ba)LiAl3N4:Eu (IIi)
[0066] The average particle size of the second phosphor is, for example, 2 μm or more and 35 μm or less, and preferably 5 μm or more and 30 μm or less. When the average particle size of the second phosphor is equal to or more than the lower limit, the absorptance of the light from the excitation light source can be increased, and light emission having a desired chromaticity and high emission intensity can be obtained. When the average particle size of the second phosphor is equal to or less than the upper limit, the workability in the manufacturing process of the light emitting device can be improved when the second phosphor is contained in the fluorescent material of the light emitting device.
[0067] The fluorescent member may contain at least one type of resin in addition to the first phosphor, such as an epoxy resin or a silicone resin.
[0068] The fluorescent member may contain other components in addition to the first phosphor as necessary. Examples of the other components include fillers such as silica, barium titanate, titanium oxide, and aluminum oxide, light stabilizers, and colorants. When the fluorescent member contains other components, for example, when the fluorescent member contains a filler as the other component, the content of the filler can be 0.01 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the resin. EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0070] Example 1 Ca3N2, CaF2, AlN, Si3N4, and EuN were used as the raw materials, and they were weighed and mixed in an inert atmosphere glove box so that the molar ratio of the charged amounts was Ca(Ca3N2):Ca(CaF2):Eu:Al:Si:F = 0.951:0.029:0.02:0.95:1.05:0.059 to obtain a raw material mixture. The raw material mixture was filled into a crucible and heat-treated at 1800 to 2100°C in a nitrogen gas atmosphere with a gauge pressure of 0.92 MPa. After that, it was subjected to processes such as crushing, dispersion, and classification to obtain Ca s Sr t EU u Sv Al w N x As a phosphor having the composition represented by the above formula, a powder of the nitride phosphor of Example 1 was obtained.
[0071] Example 2 SrN x The nitride phosphor of Example 2 was obtained under the same conditions as in Example 1, except that the raw materials used were Ca(Ca3N2):Ca(CaF2):Sr:Eu:Al:Si:F=0.902:0.029:0.049:0.02:0.95:1.05:0.059 (equivalent to x=2 / 3), Ca3N2, CaF2, AlN, Si3N4, and EuN, and the molar ratio of the amounts charged was Ca(Ca3N2):Ca(CaF2):Sr:Eu:Al:Si:F=0.902:0.029:0.049:0.02:0.95:1.05:0.059.
[0072] Example 3 The nitride phosphor of Example 3 was obtained under the same conditions as in Example 1, except that Ca3N2, CaF2, AlN, Si3N4, and EuN were used as the raw materials and the molar ratio of each raw material was Ca(Ca3N2):Ca(CaF2):Eu:Al:Si:F=0.941:0.029:0.03:0.95:1.05:0.058.
[0073] Example 4 The nitride phosphor of Example 4 was obtained under the same conditions as Example 1, except that the molar ratio of each raw material was Ca(Ca3N2):Ca(CaF2):Eu:Al:Si:F=0.Ca3N2, CaF2, AlN, Si3N4, and EuN, and was 0.931:0.029:0.04:0.95:1.05:0.057.
[0074] Example 5 SrN x The nitride phosphor of Example 5 was obtained under the same conditions as in Example 1, except that the raw materials used were Ca(Ca3N2):Ca(CaF2):Sr:Eu:Al:Si:F=0.883:0.029:0.048:0.04:0.95:1.05:0.058, and the molar ratio of the raw materials was Ca(Ca3N2):Ca(CaF2):Sr:Eu:Al:Si:F=0.883:0.029:0.048:0.04:0.95:1.05:0.058.
[0075] Example 6 The nitride phosphor of Example 6 was obtained under the same conditions as in Example 1, except that Ca3N2, CaF2, AlN, Si3N4, and EuN were used as the raw materials and the molar ratio of each raw material was Ca(Ca3N2):Ca(CaF2):Eu:Al:Si:F=0.922:0.029:0.05:0.95:1.05:0.059.
[0076] Comparative Example 1 The nitride phosphor of Comparative Example 1 was obtained under the same conditions as in Example 1, except that Ca3N2, CaF2, AlN, Si3N4, and EuN were used as the raw materials and the molar ratio of each raw material was Ca(Ca3N2):Ca(CaF2):Eu:Al:Si:F=0.951:0.029:0.018:0.95:1.05:0.059.
[0077] The phosphors obtained in Comparative Example 1 and Examples 1 to 6 were analyzed for composition using an ICP-AES device (Perkin Elmer) and an ion chromatography system (Thermo Fisher Scientific / formerly Nippon Dionex Co., Ltd.). The results are shown in Table 1 as molar ratios based on Al=0.95. In addition, the emission spectrum of the phosphors obtained above was measured at an excitation wavelength of 450 nm and room temperature (25°C ± 5°C) using a quantum efficiency measurement device (QE-2000, Otsuka Electronics Co., Ltd.), and the chromaticity coordinates, emission peak wavelength, and emission brightness were also measured. The emission spectrum is shown in Figure 2.
[0078] Based on the obtained emission spectrum, the total component value, which is the integral value of the emission intensity in the wavelength range of 500 nm to 830 nm, the first red component value, which is the integral value of the emission intensity in the wavelength range of 620 nm to less than 700 nm, and the second red component value, which is the integral value of the emission intensity in the wavelength range of 700 nm to 780 nm, were calculated. Next, the ratio of the first red component value to the total component value (first red component ratio), the ratio of the second red component value to the total component value (second red component ratio), and the ratio of the first red component value to the second red component value (first red component value / second red component value) were calculated. In addition, the relative luminance (%), relative first red component value (%), and relative second red component value were calculated when Comparative Example 1 was taken as the reference (100%). The results are shown in Table 2.
[0079] [Table 1]
[0080] [Table 2]
[0081] As shown in Table 2, the phosphors of Examples 1 to 6 have a ratio of the first red component value to the second red component value of 2.5 or less, and the ratio of the first red component value to the second red component value is smaller and the ratio of the second red component value is larger than that of Comparative Example 1, in which the ratio of the first red component value to the second red component value is 2.6. This is considered to be because, as in Examples 1 to 6, the Eu molar ratio is made larger than that of Comparative Example 1, and the tendency of the emission of the phosphor to be absorbed by the phosphor itself (self-absorption) becomes stronger, and the emission intensity on the shorter wavelength side than the emission peak wavelength of the emission spectrum decreases. Therefore, the phosphors of Examples 1 to 6 have a ratio of the first red component value to the second red component value smaller than that of the phosphor of Comparative Example 1. In addition, as in Examples 2 and 5, the first red component value is also reduced by replacing Ca with Sr, and the ratio of the first red component value to the second red component value is smaller than that of the phosphors of Comparative Example 1 in Example 2 and Example 4 with the same Eu molar ratio in Example 5. It can be seen that the phosphors of Examples 1 to 6 are nitride phosphors having an emission spectrum containing more red components on the longer wavelength side. In particular, it can be seen that, by setting the molar ratio of Eu within a specific range in the phosphors of Examples 1 to 3, the self-absorption of the phosphor is suppressed to a certain extent, and the phosphor has an emission spectrum that contains a large amount of red components on the longer wavelength side.Furthermore, it can be seen that the emission brightness is maintained at a level almost equal to that of Comparative Example 1 and better than that of the other examples. [Industrial Applicability]
[0082] A light-emitting device using the nitride phosphor of the present disclosure can be suitably used as a light source for illumination having extremely excellent light-emitting characteristics using a light-emitting diode as an excitation light source, an LED display, a backlight source for liquid crystal displays, a traffic light, an illuminated switch, various sensors, various indicators, etc. In particular, it can be suitably used as a light source for lighting for plant cultivation, etc.
Claims
1. It has a composition represented by the following formula (I): A nitride phosphor having a ratio of a second red component value, which is an integral value of emission intensity in a wavelength range of 700 nm or more and 780 nm or less, to a total component value, which is an integral value of emission intensity in a wavelength range of 500 nm or more and 830 nm or less, of 0.27 or more and 0.37 or less. Ca s Sr t Eu u Yes v Al w N x (I) (In the formula (I), s, t, u, v, w and x satisfy 0.82≦s≦0.905, 0≦t≦0.04, 0.017≦u≦0.042, 0.89≦s+t+u≦0.922, 0.8≦v≦1.2, 0.8≦w≦1.2, 1.8≦v+w≦2.2, and 2.5≦x≦3.2.)
2. The nitride phosphor according to claim 1, wherein u in the formula (I) satisfies 0.02≦u≦0.
04.
3. 2. The nitride phosphor according to claim 1, wherein s, t, and u in formula (I) satisfy 0.018≦u / (s+t+u)≦0.
047.
4. 4. The nitride phosphor according to claim 1, wherein the volume average particle size of the nitride phosphor is 10 μm or more and 30 μm or less.
5. 5. A light emitting device comprising: a fluorescent member containing a nitride phosphor having an emission peak wavelength in a wavelength range of 640 nm or more and 700 nm or less according to claim 1; and a light emitting element having an emission peak wavelength in a wavelength range of 365 nm or more and 500 nm or less.
6. The light emitting device according to claim 5 , wherein the fluorescent member further comprises at least one kind selected from the group consisting of phosphors having a composition represented by any one of the following formulas (IIa) to (IIf): (Y,Gd,Tb,Lu) 3 (A-,1) 5 O 12 :Ce (--a) (Ba,Sr,Ca) 2 2019 4 :Eu (IIb) (Ca, Sr) 8 Yes 4 O 16 (Cl, F, Br) 2 :Eu (IIc) (Ba,Sr,Ca)Ga 2 S 4 :Eu (IId) (Ba,Sr,ャ) 2 Yes 5 N 8 :Eu (IIe) K 2 (Si,Ge,Ti)F 6 :Mn (-If)
Citation Information
Patent Citations
Light emitting diodes for plant growth
CN109192843A
Method for producing inorganic substance, phosphor, phosphor-including composition, emission device, illumination device, and image display device
JP2008285662A
Nitride-based red phosphor
JP2010018771A
Red phosphor and light-emitting device
JP2019019271A
Light emitting device, illumination device and plant cultivation method
JP2019102806A