Support glass substrate and laminated substrate using the same
A glass substrate with controlled thermal expansion and modulus addresses substrate warping and dimensional changes in semiconductor packaging, enabling high-density wiring and accurate solder bump formation.
Patent Information
- Application Number
- JP2024133742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-12-13
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2038-06-15
AI Technical Summary
Conventional semiconductor packaging methods face challenges in high-density wiring and solder bump formation due to dimensional changes and warping of substrates during heat treatment, which are exacerbated by the use of resin encapsulants and glass substrates with mismatched thermal expansion coefficients.
A supporting glass substrate with a regulated thermal expansion coefficient of 30×10^-7 to 55×10^-7 /℃ and a Young's modulus of 80 GPa or more is used to match the thermal expansion of processed substrates, reducing warping and enabling accurate solder bump formation and high-density wiring.
The solution effectively suppresses dimensional changes, allowing for precise wiring and solder bump formation, improving the rigidity and reusability of the glass substrate, and maintaining substrate integrity during high-temperature processing.
Smart Images

Figure 2024153929000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a supporting glass substrate and a laminated substrate using the same, and more specifically, to a supporting glass substrate used for supporting a processed substrate on which a semiconductor chip is molded in resin in a semiconductor package manufacturing process, and a laminated substrate using the same. [Background technology]
[0002] There is a demand for smaller and lighter portable electronic devices such as mobile phones, notebook personal computers, and PDAs (Personal Data Assistances). As a result, the mounting space for semiconductor chips used in these electronic devices is severely limited, making high-density mounting of semiconductor chips an issue. In recent years, therefore, high-density mounting of semiconductor packages has been attempted by using three-dimensional mounting technology, i.e., stacking semiconductor chips and connecting them with wiring.
[0003] In addition, conventional wafer-level packages (WLPs) are manufactured by forming bumps on a wafer and then dicing the wafer into individual pieces. However, conventional WLPs have the problem that it is difficult to increase the number of pins, and because the back surface of the semiconductor chip is exposed when it is mounted, the semiconductor chip is prone to chipping.
[0004] In response to this, a fan-out type WLP has been proposed as a new WLP, which allows for an increased number of pins and protects the edges of the semiconductor chip to prevent chipping and other problems.
[0005] There are two manufacturing methods for fan-out type WLP: chip-first type and chip-last type. The chip-first type, for example, includes a process of molding multiple semiconductor chips with a resin encapsulant to form a processed substrate, wiring one surface of the processed substrate, forming solder bumps, etc. The chip-last type, for example, includes a process of placing a wiring layer on a support substrate, arranging multiple semiconductor chips, molding the substrate with a resin encapsulant to form a processed substrate, and forming solder bumps, etc.
[0006] Recently, a semiconductor package called panel level packaging (PLP) has also been considered. In PLP, a rectangular support substrate is used instead of a wafer substrate in order to increase the number of semiconductor packages that can be produced from one support substrate while reducing manufacturing costs.
[0007] The manufacturing process for these semiconductor packages involves heat treatment at approximately 200°C, which can cause the encapsulant to deform and warp the processed substrate. If the processed substrate warps, it becomes difficult to form high-density wiring on one surface of the processed substrate, and it also becomes difficult to form solder bumps accurately.
[0008] Under these circumstances, in order to suppress warping of the processed substrate, the use of a glass substrate to support the processed substrate has been considered (see Patent Document 1).
[0009] The glass substrate has a surface that is easy to smooth and has rigidity. Therefore, when a glass substrate is used as a support substrate, it is possible to firmly and accurately support the processed substrate. Furthermore, the glass substrate is easily transparent to light such as ultraviolet light and infrared light. Therefore, when a glass substrate is used as a support substrate, the processed substrate can be easily fixed by providing an adhesive layer such as an ultraviolet curing adhesive. Furthermore, the processed substrate can be easily separated by providing a peeling layer that absorbs infrared light. As another method, the processed substrate can be easily fixed and separated by providing an adhesive layer using an ultraviolet curing tape or the like. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2015-78113 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0011] In fan-out type WLP and PLP, multiple semiconductor chips are molded in a resin encapsulant to form a processed substrate, and then the process includes wiring one surface of the processed substrate and forming solder bumps.
[0012] These processes involve heat treatment at approximately 200 to 300° C., which may cause the encapsulant to deform and the processed substrate to change dimensions. If the processed substrate changes dimensions, it becomes difficult to perform high-density wiring on one surface of the processed substrate, and it also becomes difficult to accurately form solder bumps.
[0013] In order to suppress the dimensional change of the processed substrate, it is effective to use a glass substrate as the support substrate, but even when a glass substrate is used, the dimensional change of the processed substrate may occur in some cases.
[0014] The present invention has been made in view of the above circumstances, and its technical object is to contribute to high-density mounting of semiconductor packages by inventing a supporting glass substrate that is less likely to cause dimensional changes in a processed substrate. [Means for solving the problem]
[0015] As a result of repeated various experiments, the present inventors have found that the above technical problems can be solved by strictly controlling the thermal expansion coefficient of the supporting glass substrate and increasing the Young's modulus of the supporting glass substrate, and propose this as the present invention. That is, the supporting glass substrate of the present invention has an average linear thermal expansion coefficient of 30×10 -7 / ℃ or more and 55×10 -7 / °C or less, and Young's modulus is 80 GPa or more. Here, "average linear thermal expansion coefficient in the temperature range of 30 to 380°C" can be measured by a dilatometer. "Young's modulus" can be measured by a well-known resonance method.
[0016] The supporting glass substrate of the present invention has an average linear thermal expansion coefficient of 30×10 -7 / ℃ or more and 55×10 -7 / °C or less. This makes it easier to match the thermal expansion coefficients of the processed substrate and the supporting glass substrate. When the thermal expansion coefficients of the two are matched, it becomes easier to suppress dimensional changes (particularly warpage) of the processed substrate during processing. As a result, it becomes possible to provide high density wiring on one surface of the processed substrate, and it also becomes possible to accurately form solder bumps.
[0017] Furthermore, in the supporting glass substrate of the present invention, the Young's modulus is restricted to 80 GPa or more, which improves the rigidity of the laminated substrate, making it easier to suppress dimensional changes (particularly warpage) of the processed substrate, and enabling the processed substrate to be supported firmly and accurately.
[0018] In addition, the supporting glass substrate of the present invention preferably has a total thickness deviation (TTV) of less than 2.0 μm. This makes it easier to improve the processing accuracy. In particular, wiring accuracy can be improved, enabling high-density wiring. Furthermore, the number of times the supporting glass substrate can be reused can be increased. Here, the "total thickness deviation (TTV)" is the difference between the maximum and minimum overall thicknesses, and can be measured, for example, by SBW-331ML / d manufactured by Kobelco Research Institute Co., Ltd.
[0019] The supporting glass substrate of the present invention preferably contains, in mass %, 50-66% SiO2, 7-34% Al2O3, 0-8% B2O3, 0-22% MgO, 1-15% CaO, and 0-20% Y2O3+La2O3+ZrO2, where "Y2O3+La2O3+ZrO2" refers to the total amount of Y2O3, La2O3, and ZrO2.
[0020] The supporting glass substrate of the present invention is preferably used to support a processed substrate having a semiconductor chip molded in a resin in a manufacturing process of a semiconductor package.
[0021] The laminated substrate of the present invention is a laminated substrate including at least a processed substrate and a supporting glass substrate for supporting the processed substrate, and the supporting glass substrate is preferably the above-mentioned supporting glass substrate.
[0022] In the laminated substrate of the present invention, the processed substrate is preferably a processed substrate in which a semiconductor chip is molded in a resin.
[0023] In addition, the manufacturing method for a semiconductor package of the present invention includes a step of preparing a laminated substrate having at least a processing substrate and a supporting glass substrate for supporting the processing substrate, and a step of performing a processing process on the processing substrate, and it is preferable that the supporting glass substrate is the above-mentioned supporting glass substrate.
[0024] In addition, in the method for manufacturing a semiconductor package of the present invention, the processing step preferably includes a step of forming wiring on one surface of the processing substrate.
[0025] In addition, in the method for manufacturing a semiconductor package of the present invention, the processing step preferably includes a step of forming solder bumps on one surface of the processing substrate. [Brief description of the drawings]
[0026] [Figure 1] 1 is a conceptual perspective view showing an example of a laminated substrate of the present invention. [Diagram 2] 1A to 1C are conceptual cross-sectional views showing the manufacturing process of a chip-first type of fan-out type WLP. [Diagram 3] 10A to 10C are conceptual cross-sectional views showing a process of thinning a processed substrate by using a supporting glass substrate as a back-grinding substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In the supporting glass substrate of the present invention, the average linear thermal expansion coefficient in the temperature range of 30 to 380° C. is 30×10 -7 / ℃ or more and 55×10 -7 / °C or less, preferably 32×10 -7 / ℃ or more and 52×10 -7 / ℃ or less, preferably 33×10 -7 / ℃ or more and 49×10 -7 / °C or less, and particularly preferably 34×10 -7 / ℃ or more and 44×10 -7 / °C or less. If the average linear thermal expansion coefficient in the temperature range of 30 to 380°C is outside the above range, it becomes difficult to match the thermal expansion coefficients of the processing substrate and the supporting glass substrate. If the thermal expansion coefficients of the two substrates do not match, the processing substrate is likely to undergo dimensional changes (especially warpage) during processing.
[0028] In the supporting glass substrate of the present invention, the Young's modulus is preferably 80 GPa or more, 85 GPa or more, 90 GPa or more, 95 GPa or more, particularly 96 to 130 GPa. If the Young's modulus is too low, it becomes difficult to maintain the rigidity of the laminate, and dimensional changes (particularly warpage deformation) of the processed substrate tend to occur.
[0029] In the supporting glass substrate of the present invention, the total thickness deviation (TTV) is preferably less than 2.0 μm, 1.5 μm or less, 1.0 μm or less, particularly 0.1 to less than 1.0 μm. If the total thickness deviation (TTV) is too large, the accuracy of processing tends to decrease. Furthermore, it becomes difficult to reuse the supporting glass substrate.
[0030] The entire surface of the supporting glass substrate of the present invention is preferably a polished surface. In this way, it is easy to regulate the total thickness deviation (TTV) to less than 2.0 μm, 1.5 μm or less, 1.0 μm or less, particularly less than 1.0 μm. As a method of polishing, various methods can be adopted, but a method of sandwiching both sides of the glass substrate between a pair of polishing pads and polishing the glass substrate while rotating both the glass substrate and the pair of polishing pads is preferred. Furthermore, it is preferable that the pair of polishing pads have different outer diameters, and it is preferable to perform the polishing process so that a part of the glass substrate intermittently protrudes from the polishing pad during polishing. This makes it easy to reduce the total thickness deviation (TTV) and the amount of warping. In the polishing process, the polishing depth is not particularly limited, but the polishing depth is preferably 50 μm or less, 30 μm or less, 20 μm or less, particularly 10 μm or less. The smaller the polishing depth, the higher the productivity of the supporting glass substrate.
[0031] The supporting glass substrate of the present invention more preferably contains, in mass %, SiO2 50-66%, Al2O3 7-34%, B2O3 0-8%, MgO 0-22%, CaO 1-15%, and Y2O3+La2O3+ZrO2 0-20% as a glass composition. The reasons for limiting the content of each component as described above are as follows. In the explanation of the content of each component, % indicates mass % unless otherwise specified.
[0032] SiO2 is a component that forms a glass network. The content of SiO2 is preferably 50 to 66%, 51 to 65%, 52 to 64%, 53 to 63%, 54 to 62.5%, 56 to 62%, and particularly 58 to 61%. If the content of SiO2 is too low, vitrification becomes difficult and weather resistance is easily reduced. Furthermore, the thermal expansion coefficient becomes too high. On the other hand, if the content of SiO2 is too high, meltability and moldability are easily reduced and the thermal expansion coefficient becomes too low.
[0033] Al2O3 is a component that enhances Young's modulus and weather resistance. The content of Al2O3 is preferably 7 to 34%, 8 to 26%, 9 to 24%, 11 to 23%, 12 to 22%, 14 to 21%, and particularly preferably 16 to 21%. If the content of Al2O3 is too low, Young's modulus and weather resistance are likely to decrease. On the other hand, if the content of Al2O3 is too high, meltability, formability, and devitrification resistance are likely to decrease.
[0034] B2O3 is a component that forms a glass network, but also reduces the Young's modulus and weather resistance. Therefore, the content of B2O3 is preferably 0 to 8%, 0.1 to 7%, 1 to 6%, and particularly preferably 3 to 5%.
[0035] MgO is a component that significantly increases the Young's modulus, and also reduces the high-temperature viscosity to improve meltability and moldability. The content of MgO is preferably 0 to 22%, 0.5 to 21%, 1 to 20.5%, 2 to 20%, 4 to 19.5%, 5 to 19%, 7 to 19%, 8 to 18%, 8.5 to 16%, 9 to 16%, 9 to 14%, and particularly 9 to 12%. If the content of MgO is too low, it is difficult to enjoy the above effects. On the other hand, if the content of MgO is too high, the devitrification resistance is easily reduced.
[0036] CaO is a component that reduces high-temperature viscosity and improves meltability and moldability. The CaO content is preferably 1 to 15%, 2 to 12%, 3 to 10%, and particularly 5 to 8%. If the CaO content is too low, it is difficult to obtain the above effects. On the other hand, if the CaO content is too high, devitrification resistance is easily reduced.
[0037] From the viewpoint of increasing the Young's modulus, the molar ratio MgO / (MgO+CaO+SrO+BaO) is preferably 0 or more, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, particularly 0.7 or more. Here, "MgO / (MgO+CaO+SrO+BaO)" is the value obtained by dividing the content of MgO by the total amount of MgO, CaO, SrO and BaO.
[0038] Y2O3, La2O3 and ZrO2 are components that increase the Young's modulus. The total amount of Y2O3, La2O3 and ZrO2 is preferably 0 to 20%, 0.1 to 18%, 0.5 to 16%, 1 to 15%, 1 to 14%, 1 to 12%, 1.2 to 10%, 1.3 to 8%, and particularly 1.5 to 5%. If the total amount of Y2O3, La2O3 and ZrO2 is too large, the devitrification resistance is likely to decrease. The content of Y2O3 is preferably 0 to 15%, 0.1 to 14%, 0.5 to 13%, 0.5 to 12%, 0.5 to 10%, 0.5 to 8%, 0.5 to 6%, and particularly 1 to 4%. The content of La2O3 is preferably 0 to 6%, 0 to 4%, and particularly 0 to 2%. The content of ZrO2 is preferably 0 to 10%, 0.1 to 6%, 0.5 to 4%, particularly 1 to 3%. If the content of Y2O3 is too high, the devitrification resistance is likely to decrease and the raw material cost is likely to increase. If the content of La2O3 is too high, the devitrification resistance is likely to decrease and the raw material cost is likely to increase. If the content of ZrO2 is too high, the devitrification resistance is likely to decrease.
[0039] In addition to the above components, the following components may be added:
[0040] SrO and BaO are components that reduce the high-temperature viscosity and improve the meltability and moldability. The contents of SrO and BaO are 0 to 15%, 0.1 to 12%, and particularly 0.5 to 10%, respectively.
[0041] ZnO is a component that reduces high-temperature viscosity and significantly increases melting property. The content of ZnO is preferably 0 to 7%, 0.1 to 5%, and particularly 0.5 to 3%. If the content of ZnO is too small, it becomes difficult to obtain the above effects. If the content of ZnO is too large, the glass becomes easily devitrified.
[0042] Li2O, Na2O and K2O are components that reduce the high-temperature viscosity and improve the meltability and moldability, but also increase the thermal expansion coefficient. In order to reduce the high-temperature viscosity and improve the meltability and moldability while increasing the thermal expansion coefficient, the total amount of Li2O, Na2O and K2O is preferably 0 to 15%, 0.01 to 10%, 0.05 to 8%, and particularly 0.1 to 5%. The respective contents of Li2O, Na2O and K2O are preferably 0 to 10%, 0.01 to 5%, 0.05 to 4%, and particularly less than 0.1 to 3%. In order to reduce the thermal expansion coefficient, the total amount of Li2O, Na2O and K2O is preferably 0 to 15%, 0 to 10%, 0 to 5%, 0 to 1%, 0 to 0.1%, 0 to 0.05%, and particularly less than 0 to 0.01%. The respective contents of Li2O, Na2O and K2O are preferably 0 to 15%, 0 to 10%, 0 to 5%, 0 to 1%, 0 to 0.1%, 0 to 0.05%, and particularly preferably 0 to less than 0.01%.
[0043] TiO2 is a component that enhances weather resistance, but also colors the glass, so the TiO2 content is preferably 0 to 0.5%, and particularly preferably 0 to less than 0.1%.
[0044] As a fining agent, one or more selected from the group consisting of SnO2, Cl, SO3 and CeO2 (preferably SnO2 and SO3) may be added in an amount of 0.05 to 0.5%.
[0045] Fe2O3 is a component that is inevitably mixed as an impurity in glass raw materials and is a coloring component. Therefore, the content of Fe2O3 is preferably 0.5% or less, 0.001 to 0.1%, 0.005 to 0.07%, 0.008 to 0.03%, particularly preferably 0.01 to 0.025%.
[0046] V2O5, Cr2O3, CoO3 and NiO are coloring components. Therefore, the content of each of V2O5, Cr2O3, CoO3 and NiO is preferably 0.1% or less, particularly preferably less than 0.01%.
[0047] From an environmental perspective, it is preferable that the glass composition does not substantially contain As2O3, Sb2O3, PbO, Bi2O3, and F. Here, "substantially does not contain ..." means that the specified components are not actively added as glass components, but are allowed to be mixed in as impurities, and specifically means that the content of the specified components is less than 0.05%.
[0048] The supporting glass substrate of the present invention preferably has the following characteristics.
[0049] The strain point is preferably 580°C or higher, 620°C or higher, 650°C or higher, or 680°C or higher, particularly 700 to 850°C. The higher the strain point, the easier it is to reduce the thermal shrinkage of the supporting glass substrate in the manufacturing process of the semiconductor package. As a result, it becomes easier to improve the accuracy of the processing. The "strain point" refers to a value measured based on the method of ASTM C336.
[0050] The liquidus temperature is preferably 1300°C or less, 1280°C or less, 1250°C or less, 1160°C or less, 1130°C or less, particularly 1100°C or less. In this way, it becomes easy to form into a plate shape, so that the total thickness deviation (TTV) can be reduced to less than 2.0 μm, particularly less than 1.0 μm, without polishing the surface or by polishing it only slightly, and as a result, the manufacturing cost of the supporting glass substrate can be reduced. Furthermore, it becomes easy to prevent the occurrence of devitrification crystals during forming. Here, the "liquidus temperature" can be calculated by putting the glass powder that passes through a standard sieve 30 mesh (500 μm) and remains on the 50 mesh (300 μm) into a platinum boat, and then holding it in a temperature gradient furnace for 24 hours to measure the temperature at which crystals precipitate.
[0051] The liquidus viscosity is preferably 10 3.8 dPa s or more, 10 4.0 dPa s or more, 10 4.2 dPa s or more, 10 4.4 dPa s or more, especially 10 4.6In this way, it becomes easy to form into a plate, and the total thickness deviation (TTV) can be reduced to less than 2.0 μm, particularly less than 1.0 μm, without polishing the surface or with only a small amount of polishing, resulting in a reduction in the manufacturing cost of the supporting glass substrate. Here, the "liquidus viscosity" can be measured by the platinum ball pulling method.
[0052] 10 2.5 The temperature at dPa·s is preferably 1550° C. or less, 1500° C. or less, 1480° C. or less, 1450° C. or less, particularly 1200 to 1400° C. or less. 2.5 When the temperature at 10 dPa·s increases, the melting property decreases, and the manufacturing cost of the supporting glass substrate increases. 2.5 The "temperature at dPa·s" can be measured using the platinum sphere pulling method.
[0053] The plate thickness is preferably 1.5 mm or less, 1.2 mm or less, 1.0 mm or less, particularly 0.9 mm or less. On the other hand, if the plate thickness is too thin, the strength of the supporting glass substrate itself decreases, making it difficult to function as a supporting substrate. Therefore, the plate thickness of the supporting glass substrate is preferably 0.5 mm or more, 0.6 mm or more, particularly more than 0.7 mm.
[0054] The amount of warpage is preferably 60 μm or less, 55 μm or less, 50 μm or less, 1 to 45 μm, and particularly 5 to 40 μm. The smaller the amount of warpage, the easier it is to improve the accuracy of processing. In particular, wiring accuracy can be improved, making it possible to achieve high-density wiring. In order to reduce the amount of warpage, it is preferable to laminate multiple glass substrates and perform heat treatment. The "amount of warpage" refers to the sum of the absolute value of the maximum distance between the highest point and the least squares focal plane in the entire supporting glass substrate, and the absolute value of the minimum point and the least squares focal plane, and can be measured, for example, by SBW-331ML / d manufactured by Kobelco Research Institute, Ltd.
[0055] The supporting glass substrate of the present invention is preferably in the form of a wafer (approximately circular), with a diameter of 100 mm to 500 mm, particularly preferably 150 mm to 450 mm, and a circularity (excluding the notch) of 1 mm or less, 0.1 mm or less, 0.05 mm or less, particularly preferably 0.03 mm or less. This makes it easier to apply to the manufacturing process of semiconductor packages. The "circularity" is the value obtained by subtracting the minimum value from the maximum value of the outer shape of the wafer.
[0056] The supporting glass substrate of the present invention preferably has a notch portion (notch-shaped alignment portion), and more preferably the deep portion of the notch portion is substantially circular or substantially V-groove-shaped in plan view. This makes it easier to fix the position of the supporting glass substrate by abutting a positioning member such as a positioning pin against the notch portion of the supporting glass substrate. As a result, alignment of the supporting glass substrate and the processing substrate becomes easier. In particular, if a notch portion is also formed in the processing substrate and a positioning member is abutted against it, alignment of the entire laminate becomes easier.
[0057] On the other hand, when the positioning member is brought into contact with the notch of the supporting glass substrate, stress is likely to be concentrated on the notch, and the supporting glass substrate is likely to be damaged starting from the notch. This tendency is particularly pronounced when the supporting glass substrate is curved by an external force. Therefore, it is preferable that all or part of the edge region where the surface of the notch intersects with the end face is chamfered. This makes it possible to effectively avoid damage starting from the notch.
[0058] It is more preferable that 50% or more of the edge area where the surface of the notch and the end face intersect is chamfered, it is particularly preferable that 90% or more of the edge area where the surface of the notch and the end face intersect is chamfered, and it is most preferable that the entire edge area where the surface of the notch and the end face intersect is chamfered. The larger the area that is chamfered in the notch, the more likely it is that breakage originating from the notch will be reduced.
[0059] The chamfer width of the notch in the front surface direction (similarly the chamfer width in the back surface direction) is preferably 50 to 900 μm, 200 to 800 μm, 300 to 700 μm, 400 to 650 μm, particularly 500 to 600 μm. If the chamfer width of the notch in the front surface direction is too small, the supporting glass substrate is likely to be damaged starting from the notch. On the other hand, if the chamfer width of the notch in the front surface direction is too large, the chamfer efficiency decreases, and the manufacturing cost of the supporting glass substrate is likely to increase.
[0060] The chamfer width of the notch in the plate thickness direction (total chamfer width of the front and back surfaces) is preferably 5 to 80%, 20 to 75%, 30 to 70%, 35 to 65%, particularly 40 to 60% of the plate thickness. If the chamfer width of the notch in the plate thickness direction is too small, the supporting glass substrate is likely to be damaged starting from the notch. On the other hand, if the chamfer width of the notch in the plate thickness direction is too large, external forces are likely to be concentrated on the end face of the notch, and the supporting glass substrate is likely to be damaged starting from the end face of the notch.
[0061] From the viewpoint of reducing the total thickness deviation (TTV), it is preferable that the supporting glass substrate of the present invention is not subjected to a chemical strengthening treatment, that is, it is preferable that the supporting glass substrate does not have a compressive stress layer on the surface.
[0062] As a method for forming the supporting glass substrate, various methods can be adopted, such as a slot-down method, a roll-out method, a redraw method, a float method, an ingot molding method, and the like.
[0063] The laminated substrate of the present invention is a laminated substrate including at least a processed substrate and a supporting glass substrate for supporting the processed substrate, and is characterized in that the supporting glass substrate is the above-mentioned supporting glass substrate. Here, the technical features (preferable configurations and effects) of the laminated substrate of the present invention overlap with the technical features of the supporting glass substrate of the present invention. Therefore, in this specification, detailed descriptions of the overlapping parts are omitted.
[0064] The laminated substrate of the present invention preferably has an adhesive layer between the processing substrate and the supporting glass substrate. The adhesive layer is preferably a resin, such as a thermosetting resin or a photocurable resin (particularly an ultraviolet-curable resin). It is also preferable that the adhesive layer has heat resistance that can withstand heat treatment in the manufacturing process of the semiconductor package. This makes it difficult for the adhesive layer to melt in the manufacturing process of the semiconductor package, and the accuracy of the processing can be improved.
[0065] The laminated substrate of the present invention preferably further has a release layer between the processed substrate and the supporting glass substrate, more specifically between the processed substrate and the adhesive layer, or between the supporting glass substrate and the adhesive layer. In this way, the processed substrate can be easily peeled off from the supporting glass substrate after a predetermined processing treatment is performed on the processed substrate. From the viewpoint of productivity, the peeling of the processed substrate is preferably performed by irradiating light such as laser light.
[0066] The peeling layer is made of a material that undergoes "intralayer peeling" or "interfacial peeling" when irradiated with light such as laser light. In other words, when irradiated with light of a certain intensity, the interatomic or intermolecular bonding force between atoms or molecules disappears or decreases, causing ablation or the like, resulting in peeling. In addition, when irradiated with light, the components contained in the peeling layer may turn into gas and be released, leading to separation, or the peeling layer may absorb light, turn into gas, and release the vapor, leading to separation.
[0067] In the laminated substrate of the present invention, the supporting glass substrate is preferably larger than the processing substrate, so that when the processing substrate and the supporting glass substrate are supported, even if their central positions are slightly separated from each other, the edge of the processing substrate is less likely to protrude from the supporting glass substrate.
[0068] The method for manufacturing a semiconductor package of the present invention includes a step of preparing a laminated substrate including at least a processing substrate and a supporting glass substrate for supporting the processing substrate, and a step of performing a processing process on the processing substrate, and is characterized in that the supporting glass substrate is the above-mentioned supporting glass substrate. Here, the technical features (preferable configurations and effects) of the method for manufacturing a semiconductor package of the present invention overlap with the technical features of the supporting glass substrate and the laminated substrate of the present invention. Therefore, in this specification, detailed description of the overlapping parts is omitted.
[0069] The method for manufacturing a semiconductor package of the present invention includes a step of preparing a laminated substrate including at least a processed substrate and a supporting glass substrate for supporting the processed substrate. The laminated substrate including at least a processed substrate and a supporting glass substrate for supporting the processed substrate has the above-mentioned material configuration. The above-mentioned molding method can be adopted as the molding method for the glass substrate.
[0070] The method for manufacturing a semiconductor package of the present invention preferably further includes a step of transporting the laminated substrate. This can improve the processing efficiency. Note that the "step of transporting the laminated substrate" and the "step of performing processing on the processed substrate" do not need to be performed separately, and may be performed simultaneously.
[0071] In the semiconductor package manufacturing method of the present invention, the processing is preferably a process for wiring one surface of the processed substrate, or a process for forming solder bumps on one surface of the processed substrate. In the semiconductor package manufacturing method of the present invention, the processed substrate is unlikely to change in size during these processes, so these steps can be carried out appropriately.
[0072] In addition to the above, the processing may be any of the following: mechanical polishing of one surface of the processing substrate (usually the surface opposite the supporting glass substrate), dry etching of one surface of the processing substrate (usually the surface opposite the supporting glass substrate), and wet etching of one surface of the processing substrate (usually the surface opposite the supporting glass substrate). In addition, in the manufacturing method of the semiconductor package of the present invention, warping is unlikely to occur in the processing substrate, and the rigidity of the laminated substrate can be maintained. As a result, the above processing can be performed appropriately.
[0073] The present invention will be further described with reference to the drawings.
[0074] Fig. 1 is a conceptual perspective view showing an example of a laminated substrate 1 of the present invention. In Fig. 1, the laminated substrate 1 includes a supporting glass substrate 10 and a processing substrate 11. The supporting glass substrate 10 is attached to the processing substrate 11 in order to prevent dimensional change of the processing substrate 11. The supporting glass substrate 10 has an average linear thermal expansion coefficient of 32 × 10 in a temperature range of 30 to 380°C. -7 / ℃ or more and 55×10 -7 / °C or less, and the Young's modulus is 80 GPa or more. In addition, a release layer 12 and an adhesive layer 13 are disposed between the supporting glass substrate 10 and the processing substrate 11. The release layer 12 is in contact with the supporting glass substrate 10, and the adhesive layer 13 is in contact with the processing substrate 11.
[0075] As can be seen from FIG. 1, the laminated substrate 1 is arranged by stacking a supporting glass substrate 10, a peeling layer 12, an adhesive layer 13, and a processed substrate 11 in this order. The shape of the supporting glass substrate 10 is determined according to the processed substrate 11, but in FIG. 1, the shapes of the supporting glass substrate 10 and the processed substrate 11 are both wafer shapes. In addition to amorphous silicon (a-Si), silicon oxide, silicate compounds, silicon nitride, aluminum nitride, titanium nitride, and the like are used for the peeling layer 12. The peeling layer 12 is formed by plasma CVD, spin coating by the sol-gel method, and the like. The adhesive layer 13 is made of a resin, and is formed by coating, for example, various printing methods, inkjet methods, spin coating methods, roll coating methods, and the like. After the supporting glass substrate 10 is peeled off from the processed substrate 11 by the peeling layer 12, the adhesive layer 13 is dissolved and removed by a solvent or the like.
[0076] FIG. 2 is a conceptual cross-sectional view showing the manufacturing process of the chip-first type of fan-out type WLP. FIG. 2(a) shows a state in which an adhesive layer 21 is formed on one surface of a support member 20. If necessary, a peeling layer may be formed between the support member 20 and the adhesive layer 21. Next, as shown in FIG. 2(b), a plurality of semiconductor chips 22 are attached on the adhesive layer 21. At that time, the active side surface of the semiconductor chip 22 is brought into contact with the adhesive layer 21. Next, as shown in FIG. 2(c), the semiconductor chip 22 is molded with a resin sealant 23. The sealant 23 is made of a material that has little dimensional change after compression molding and little dimensional change when forming wiring. Next, as shown in FIG. 2(d) and (e), after the processing substrate 24 on which the semiconductor chip 22 is molded is separated from the support member 20, it is bonded and fixed to the supporting glass substrate 26 via the adhesive layer 25. At that time, the surface of the processing substrate 24 opposite to the surface on which the semiconductor chip 22 is embedded is arranged on the supporting glass substrate 26 side. In this manner, a laminated substrate 27 can be obtained. If necessary, a release layer may be formed between the adhesive layer 25 and the supporting glass substrate 26. After the obtained laminated substrate 27 is transported, wiring 28 is formed on the surface of the processed substrate 24 on which the semiconductor chip 22 is embedded, and then a plurality of solder bumps 29 are formed, as shown in Fig. 2(f). Finally, after separating the processed substrate 24 from the supporting glass substrate 26, the processed substrate 24 is cut into individual semiconductor chips 22, and is subjected to a subsequent packaging process (Fig. 2(g)).
[0077] FIG. 3 is a conceptual cross-sectional view showing a process of thinning a processed substrate by using a supporting glass substrate as a back-grinding substrate. FIG. 3(a) shows a laminated substrate 30. The laminated substrate 30 is arranged by stacking a supporting glass substrate 31, a peeling layer 32, an adhesive layer 33, and a processed substrate (silicon wafer) 34 in this order. A plurality of semiconductor chips 35 are formed on the surface of the processed substrate that contacts the adhesive layer 33 by a photolithography method or the like. FIG. 3(b) shows a process of thinning the processed substrate 34 by a polishing device 36. In this process, the processed substrate 34 is mechanically polished and thinned to, for example, several tens of μm. FIG. 3(c) shows a process of irradiating the peeling layer 32 with ultraviolet light 37 through the supporting glass substrate 31. After this process, it becomes possible to separate the supporting glass substrate 31 as shown in FIG. 3(d). The separated supporting glass substrate 31 is reused as necessary. FIG. 3(e) shows a process of removing the adhesive layer 33 from the processed substrate 34. After this process, a thin processed substrate 34 can be obtained. EXAMPLES
[0078] The present invention will be described below based on examples. Note that the following examples are merely illustrative and the present invention is not limited to the following examples.
[0079] Tables 1 to 9 show examples of the present invention (samples No. 1 to 86) and a comparative example (sample No. 87).
[0080] [Table 1]
[0081] [Table 2]
[0082] [Table 3]
[0083] [Table 4]
[0084] [Table 5]
[0085] [Table 6]
[0086] [Table 7]
[0087] [Table 8]
[0088] [Table 9]
[0089] First, a glass batch prepared by mixing glass raw materials to obtain the glass composition shown in the table was placed in a platinum crucible, and then melted, clarified, and homogenized at 1500 to 1700°C for 24 hours. When melting the glass batch, a platinum stirrer was used for stirring and homogenization. Next, the molten glass was poured onto a carbon plate, formed into a plate shape, and then slowly cooled for 30 minutes at a temperature near the annealing point. The density, average linear thermal expansion coefficient CTE in the temperature range of 30 to 380°C, and the like were measured for each of the obtained glass substrates. 30~380℃ , Young's modulus, strain point Ps, annealing point Ta, softening point Ts, high temperature viscosity 10 4.0 Temperature in dPa·s, high temperature viscosity 10 3.0 Temperature in dPa·s, high temperature viscosity 10 2.5 The temperature was evaluated in dPa·s. In the table, "NA" means not measured.
[0090] The density is a value measured by Archimedes' method.
[0091] Average coefficient of linear thermal expansion (CTE) in the temperature range 30 to 380°C 30~380℃ is a value measured with a dilatometer.
[0092] The Young's modulus refers to a value measured by a resonance method.
[0093] The strain point Ps, annealing point Ta, and softening point Ts are values measured based on the methods of ASTM C336 and C338.
[0094] High temperature viscosity 10 4.0 dPa·s, 10 3.0 dPa·s, 10 2.5 The temperature in dPa·s was measured by the platinum sphere pulling method.
[0095] As is clear from Tables 1 to 9, Samples No. 1 to 86 have an average linear thermal expansion coefficient CTE in the temperature range of 30 to 380 ° C. 30~380℃ is 33.2 x 10 -7 / ℃~48.0×10 -7 / °C and Young's modulus of 80.0 to 101.2 GPa, it is considered to be suitable as a supporting glass substrate. On the other hand, sample No. 87 has an average linear thermal expansion coefficient CTE 30~380℃ 35×10 -7 / °C, but since the Young's modulus is 76 GPa, it is considered to be unsuitable as a supporting glass substrate.
[0096] Next, the glass substrates of Samples No. 1 to 86 were processed to φ300 mm×0.8 mm thickness, and then both surfaces were polished by a polishing device. Specifically, both surfaces of the glass substrate were sandwiched between a pair of polishing pads with different outer diameters, and both surfaces of the glass substrate were polished while rotating the glass substrate and the pair of polishing pads. During the polishing process, the glass substrate was controlled so that a part of the glass substrate occasionally protruded from the polishing pad. The polishing pads were made of urethane, the average particle size of the polishing slurry used during the polishing process was 2.5 μm, and the polishing speed was 15 m / min. The total thickness deviation (TTV) and the amount of warping of each of the obtained polished glass substrates were measured by SBW-331ML / d manufactured by Kobelco Research Institute Co., Ltd. As a result, the total thickness deviation (TTV) was 0.45 μm, and the amount of warping was 35 μm. [Explanation of symbols]
[0097] 1, 27, 30 Multilayer board 10, 26, 31 Support glass substrate 11, 24, 34 Processed board 12, 32 peeling layer 13, 21, 25, 33 Adhesive layer 20 Support member 22, 35 Semiconductor chips 23 Encapsulating materials 28 Wiring 29 Solder Bumps 36 Polishing equipment 37 Ultraviolet light
Claims
1. The average linear thermal expansion coefficient in the temperature range of 30 to 380°C is 30 x 10 -7 / °C or more and 55 x 10 -7 / ° C. or less and a Young's modulus of 80 GPa or more.
2. 2. The supporting glass substrate according to claim 1, wherein the total thickness variation (TTV) is less than 2.0 μm.
3. The glass composition is, in mass%, SiO 2 50-66%, Al 2 O 3 7-34%, B 2 O 3 0-8%, MgO 0-22%, CaO 1-15%, Y 2 O 3 +La 2 O 3 + ZrO 2 3. The supporting glass substrate according to claim 1, wherein the content is 0 to 20%.
4. 4. The supporting glass substrate according to claim 1, which is used to support a processed substrate having a semiconductor chip molded in a resin in a manufacturing process of a semiconductor package.
5. 5. A laminated substrate comprising at least a processed substrate and a supporting glass substrate for supporting the processed substrate, the supporting glass substrate being the supporting glass substrate according to any one of claims 1 to 4.
6. 6. The laminated substrate according to claim 5, wherein the processed substrate is a processed substrate in which a semiconductor chip is molded in a resin.
7. A step of preparing a laminated substrate including at least a processed substrate and a supporting glass substrate for supporting the processed substrate; A method for manufacturing a semiconductor package, comprising: a step of performing a processing treatment on a processing substrate; and wherein the supporting glass substrate is the supporting glass substrate according to any one of claims 1 to 4.
8. 8. The method for manufacturing a semiconductor package according to claim 7, wherein the processing step includes a step of wiring on one surface of the processing substrate.
9. 9. The method for manufacturing a semiconductor package according to claim 7, wherein the processing step includes a step of forming solder bumps on one surface of the processing substrate.
Citation Information
Patent Citations
Alkali metal-free aluminoborosilicates and uses
JP2004531443A
Rare earth-containing glass materials and substrates, and apparatus including these substrates
JP2011522767A
Alkali-free glass for magnetic recording medium, and glass substrate for magnetic recording medium using the same
JP2015028827A
Method for producing alkali-free glass
JP2015224150A
Support glass substrate and laminate comprising the same
JP2016117641A