Method for producing acrylic rubber
By adjusting the acrylic polymer concentration during coagulation and controlling the mass ratio of coagulating liquid to latex, the method addresses the compression set issue in acrylic rubber production, improving its flexibility and durability for automotive applications.
Patent Information
- Application Number
- JP2021135549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-08-23
- Publication Date
- 2024-10-30
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing acrylic rubber do not adequately address the reduction of compression set in crosslinked products, which is a critical property for applications requiring flexibility and durability.
Adjusting the concentration of the acrylic polymer during coagulation by controlling the mass ratio of the coagulating liquid to the latex and maintaining the acrylic polymer content within a specific range, along with a controlled emulsion polymerization process, to reduce the compression set of the crosslinked acrylic rubber.
The method effectively reduces the compression set of crosslinked acrylic rubber, enhancing its suitability for applications requiring flexibility and durability, such as hoses and seal parts in automobiles.
Smart Images

Figure 2024153957000005 
Figure 2024153957000001 
Figure 2024153957000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing acrylic rubber. [Background technology]
[0002] Acrylic rubber and its crosslinked products are excellent in physical properties such as heat resistance, oil resistance, and mechanical properties, and are therefore used as materials for hoses and seal parts in the engine compartment of automobiles. Acrylic rubber can be obtained, for example, by emulsion polymerization of monomers to obtain an acrylic polymer, and then solidifying the acrylic polymer. Since such a manufacturing method for acrylic rubber can affect various physical properties of the obtained acrylic rubber, a manufacturing method suitable for the desired physical properties is used.
[0003] For example, Patent Document 1 discloses a method for producing acrylic rubber that has excellent water resistance and compression set resistance when crosslinked, the method comprising an emulsion polymerization step of emulsion-polymerizing a monomer mainly composed of a (meth)acrylic acid ester using a polymerization catalyst in the presence of an emulsifier to obtain an emulsion polymerization liquid, a coagulation step of coagulating the emulsion polymerization liquid in the presence of polyethylene glycol to obtain water-containing crumbs, a washing step of washing the water-containing crumbs, and a drying step of drying the washed water-containing crumbs. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-189835 A Summary of the Invention [Problem to be solved by the invention]
[0005] According to the investigations of the present inventors, there is room for further improvement in the manufacturing method of acrylic rubber in order to reduce the compression set of the cross-linked acrylic rubber. An object of the present invention is to provide a manufacturing method of acrylic rubber capable of reducing the compression set of the cross-linked acrylic rubber. [Means for solving the problem]
[0006] The present inventors have found that in a method for producing acrylic rubber, changing the concentration of the acrylic polymer when the acrylic polymer obtained by emulsion polymerization is coagulated with a coagulant results in a difference in the compression set of the resulting cross-linked acrylic rubber, even if the composition of the monomers constituting the acrylic polymer is the same, and further, that when the concentration of the acrylic polymer is within a specified range, the compression set is small.
[0007] One aspect of the present invention is a method for producing acrylic rubber, comprising the steps of: emulsion polymerizing a monomer containing an alkyl acrylate in the presence of an emulsifier to obtain an acrylic polymer; mixing a latex containing the acrylic polymer and the emulsifier with a coagulating liquid containing a coagulating agent to coagulate the acrylic polymer; and washing the coagulated acrylic polymer to obtain an acrylic rubber, wherein the content of the acrylic polymer in the mixture of the latex and the coagulating liquid is 20 mass% or less based on the total amount of the mixture.
[0008] The content of the acrylic polymer in the latex may be 30% by mass or more based on the total amount of the latex, and the mass ratio of the content of the coagulation liquid to the content of the latex in the mixture may be 0.6 or more.
[0009] The content of the acrylic polymer in the latex may be less than 30% by mass based on the total amount of the latex.
[0010] The monomers may further include a crosslinking monomer. The crosslinking monomer may be a crosslinking monomer having a carboxyl group. Effect of the Invention
[0011] According to the present invention, there is provided a method for producing an acrylic rubber that can reduce the compression set of a cross-linked product of the acrylic rubber. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram showing an example of an extruder for carrying out a solidification step and subsequent steps in one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] One embodiment of the present invention is a method for producing acrylic rubber, comprising: a step (polymerization step) of emulsion-polymerizing a monomer containing an alkyl acrylate in the presence of an emulsifier to obtain an acrylic polymer; and a step (coagulation step) of mixing a latex containing the acrylic polymer and the emulsifier with a coagulation liquid containing a coagulant to coagulate the acrylic polymer.
[0014] In the polymerization step, the monomer is emulsion-polymerized in the presence of an emulsifier by a known emulsion polymerization method. Specifically, for example, a monomer (a monomer mixture when two or more types of monomers are used) and an aqueous solution of an emulsifier are mixed in a reaction vessel to prepare a suspension. Then, after replacing the atmosphere in the reaction vessel with nitrogen gas, a polymerization initiator is added to the suspension while stirring the suspension to start polymerization, and the polymerization is allowed to proceed, for example, at 40 to 100°C for 1 to 24 hours.
[0015] The alkyl acrylate contained in the monomer becomes the skeleton of the acrylic rubber. The alkyl acrylate contains, for example, one or more alkyl acrylates having an alkyl group having 1 to 8 carbon atoms. The alkyl group may be linear or branched.
[0016] The content of alkyl acrylate may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more, and may be 99% by mass or less, 98% by mass or less, or 97% by mass or less, based on the total amount of monomers.
[0017] The alkyl acrylate may include, for example, an alkyl acrylate having an alkyl group having 1 to 3 carbon atoms (hereinafter also referred to as "C1-C3 alkyl acrylate"), and may include an alkyl acrylate having an alkyl group having 4 to 8 carbon atoms (hereinafter also referred to as "C4-C8 alkyl acrylate").
[0018] Examples of C1-C3 alkyl acrylates include methyl acrylate, ethyl acrylate, and n-propyl acrylate. From the viewpoint of improving the tensile strength of the acrylic rubber, the C1-C3 alkyl acrylate preferably contains at least one selected from the group consisting of methyl acrylate and ethyl acrylate, more preferably ethyl acrylate.
[0019] The content of the C1-C3 alkyl acrylate may be 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, or 70% by mass or more, and may be 95% by mass or less, 90% by mass or less, or 80% by mass or less, based on the total amount of monomers.
[0020] Examples of C4-C8 alkyl acrylates include n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-methylpentyl acrylate, n-octyl acrylate, and 2-ethylhexyl acrylate. From the viewpoint of improving the cold resistance of the acrylic rubber, the alkyl acrylate preferably contains butyl acrylate, more preferably n-butyl acrylate.
[0021] The content of the C4-C8 alkyl acrylate may be 5% by mass or more, 10% by mass or more, or 20% by mass or more, and may be 80% by mass or less, 70% by mass or less, or 60% by mass or less, based on the total amount of monomers.
[0022] The alkyl acrylate preferably includes at least one selected from the group consisting of C1-C3 alkyl acrylates and at least one selected from the group consisting of C4-C8 alkyl acrylates, more preferably includes methyl acrylate or ethyl acrylate, and n-butyl acrylate, and even more preferably includes ethyl acrylate and n-butyl acrylate.
[0023] The monomer may further include other monomers copolymerizable with the alkyl acrylate. The other monomers may be, for example, alkyl methacrylate. The alkyl methacrylate includes, for example, one or more alkyl methacrylates having an alkyl group with 1 to 12 carbon atoms. The alkyl group may be linear or branched. The alkyl methacrylate includes an alkyl methacrylate having preferably an alkyl group with 1 to 8 carbon atoms, more preferably an alkyl group with 1 to 4 carbon atoms.
[0024] Examples of alkyl methacrylates include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, n-decyl methacrylate, and n-dodecyl methacrylate.
[0025] The alkyl methacrylate preferably includes at least one selected from the group consisting of methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, n-decyl methacrylate, and n-dodecyl methacrylate, more preferably includes at least one selected from the group consisting of methyl methacrylate, ethyl methacrylate, and n-butyl methacrylate, and even more preferably includes n-butyl methacrylate.
[0026] The content of alkyl methacrylate may be 5 mass % or more, 10 mass % or more, or 20 mass % or more, and may be 50 mass % or less, 40 mass % or less, or 30 mass % or less, based on the total amount of monomers.
[0027] The other monomer may be, for example, vinyl acetate. The content of vinyl acetate may be 5% by mass or more, 10% by mass or more, or 20% by mass or more, and may be 50% by mass or less, 40% by mass or less, or 30% by mass or less, based on the total amount of monomers.
[0028] The other monomer may be, for example, a crosslinking monomer. The crosslinking monomer is a monomer that is copolymerizable with the alkyl acrylate and has a functional group that forms a crosslinking site (also called a crosslinking point). The crosslinking monomer has a polymerizable carbon-carbon double bond, and has, for example, an acryloyl group, a methacryloyl group, an allyl group, a methallyl group, a vinyl group, or an alkenylene group.
[0029] Examples of the functional group include an epoxy group, a carboxyl group, and an active chlorine group. The crosslinking monomer may have one or more of these functional groups. The crosslinking monomer is preferably a crosslinking monomer having a carboxyl group, from the viewpoint of particularly suitably obtaining the effect of reducing the compression set of the crosslinked acrylic rubber (details will be described later) by setting the content of the acrylic polymer in the mixture in the solidification step within a predetermined range.
[0030] The crosslinking monomer having an epoxy group preferably has a glycidyl group, and examples of the crosslinking monomer having an epoxy group include glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, and methallyl glycidyl ether.
[0031] The number of carboxyl groups in the crosslinking monomer having a carboxyl group may be 1, 2, or 3 or more. Examples of the crosslinking monomer having a carboxyl group include acrylic acid, methacrylic acid, crotonic acid, 2-pentenoic acid, maleic acid, fumaric acid, itaconic acid, and maleic acid monoalkyl ester.
[0032] Examples of crosslinking monomers having an active chlorine group include 2-chloroethyl vinyl ether, 2-chloroethyl acrylate, vinylbenzyl chloride, vinyl chloroacetate, and allyl chloroacetate.
[0033] The content of the crosslinking monomer may be 0.5 parts by mass or more, 0.8 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more, and may be 10 parts by mass or less, 7 parts by mass or less, or 5 parts by mass or less, relative to 100 parts by mass of the total amount of monomers other than the crosslinking monomer.
[0034] The other monomer may be, for example, ethylene, alkoxyalkyl (meth)acrylate, fluorine-containing (meth)acrylate, hydroxyl group-containing (meth)acrylate, tertiary amino group-containing (meth)acrylate, alkyl vinyl ketone, vinyl ether, allyl ether, aromatic vinyl compound, vinyl nitrile, vinyl halide, vinylidene halide, etc. The content of these other monomers may be 1 mass % or more and 10 mass % or less based on the total amount of monomers.
[0035] The emulsifier may be a known emulsifier used in the emulsion polymerization. The emulsifier may be, for example, a nonionic emulsifier. The nonionic emulsifier may include at least one selected from the group consisting of ether-type nonionic emulsifiers, ester-type nonionic emulsifiers, ether-ester-type nonionic emulsifiers, nitrogen-containing nonionic emulsifiers, and polyvinyl alcohol-based emulsifiers.
[0036] Examples of ether-type nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene alkenyl ethers, polyoxyethylene alkylphenol ethers, polyoxyethylene polyoxypropylene copolymers, polyoxyethylene lauryl glycol, and polyoxypropylene glycol.
[0037] Examples of the ester-type nonionic emulsifier include sorbitan fatty acid esters and glycerin fatty acid esters. The sorbitan fatty acid esters may be, for example, monoesters. The glycerin fatty acid esters may be, for example, monoesters or diesters.
[0038] Examples of the ether ester type nonionic emulsifier include polyoxyethylene fatty acid esters and polyoxyethylene sorbitan fatty acid esters. The polyoxyethylene fatty acid esters may be, for example, monoesters or diesters. The polyoxyethylene sorbitan fatty acid esters may be, for example, monoesters.
[0039] Examples of nitrogen-containing nonionic emulsifiers include polyoxyethylene alkylamines, polyoxyethylene fatty acid monoethanolamides, and fatty acid diethanolamides.
[0040] The polyvinyl alcohol emulsifier may be a fully saponified polyvinyl alcohol or a partially saponified polyvinyl alcohol, and is preferably a partially saponified polyvinyl alcohol. The saponification degree of polyvinyl alcohol is preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and preferably 100 mol% or less, more preferably 99 mol% or less, even more preferably 90 mol% or less. The saponification degree of polyvinyl alcohol means a value measured according to JIS K6726 "3.5 Saponification degree".
[0041] The amount of the emulsifier added may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the total amount of monomers.
[0042] The polymerization initiator may be, for example, an azo compound such as azobisisobutyronitrile, an organic peroxide such as tert-butyl hydroperoxide, cumene hydroperoxide, or benzoyl peroxide, or an inorganic peroxide such as sodium persulfate or ammonium persulfate, and is preferably tert-butyl hydroperoxide. The amount of the polymerization initiator added may be, for example, 0.01 parts by mass or more and 2 parts by mass or less with respect to 100 parts by mass of the total amount of monomers.
[0043] A pH adjuster may be further added to the suspension. The pH adjuster may be, for example, an alkali metal salt such as sodium acetate, sodium hydroxide, potassium hydroxide, sodium phosphate, or sodium citrate, and is preferably sodium acetate. The amount of the pH adjuster added may be, for example, 0.1 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the total amount of monomers.
[0044] The coagulation step and subsequent steps following the polymerization step are carried out, for example, using an extruder. Fig. 1 is a schematic diagram showing an example of the extruder. In one embodiment, the extruder 1 includes a coagulation zone 2, a first drainage zone 3, a first washing zone 4, a second drainage zone 5, a second washing zone 6, a third drainage zone 7, and a drying zone 8, in this order.
[0045] In the coagulation step, a latex L containing an acrylic polymer and an emulsifier and a coagulation liquid C containing a coagulant are supplied to the coagulation zone 2, and the latex L and the coagulation liquid C are mixed to coagulate the acrylic polymer.
[0046] The coagulation liquid C may be, for example, an aqueous solution containing a coagulant, or may be an aqueous solution consisting of only a coagulant and water. The content of the coagulant in the coagulation liquid C is set so that an appropriate amount of coagulant is added depending on the amount of the acrylic polymer. For example, the amount of the coagulation liquid added may be 1 part by mass or more, 3 parts by mass or more, or 5 parts by mass or more, and 50 parts by mass or less, 40 parts by mass or less, or 30 parts by mass or less, relative to 100 parts by mass of the acrylic polymer. The content of the coagulation liquid C may be set so as to be such an amount added, and may be, for example, 1% by mass or more, 2% by mass or more, 3% by mass or more, 4% by mass or more, or 5% by mass or more, and 10% by mass or less, 9% by mass or less, 8% by mass or less, 7% by mass or less, 6% by mass or less, or 5% by mass or less, based on the total amount of the coagulation liquid C.
[0047] Examples of the coagulant include ammonium salts, monovalent to trivalent metal salts, inorganic acids, and organic acids. Examples of the ammonium salts include ammonium borate, ammonium sulfate, and ammonium chloride. Examples of the monovalent to trivalent metal salts include sodium salts, magnesium salts, calcium salts, aluminum salts, and zinc salts. Examples of the sodium salts include sodium borate, sodium sulfate, and sodium chloride. Examples of the magnesium salts include magnesium sulfate, magnesium chloride, and magnesium nitrate. Examples of the calcium salts include calcium sulfate, calcium chloride, and calcium nitrate. Examples of the aluminum salts include aluminum sulfate and aluminum chloride. Examples of the zinc salts include zinc chloride and zinc acetate. Examples of the inorganic acid include hydrochloric acid, sulfuric acid, and nitric acid. Examples of the organic acid include formic acid and acetic acid.
[0048] In the coagulation step, latex L and coagulation liquid C are supplied to the coagulation zone 2 so that the content of the acrylic polymer in the mixture of latex L and coagulation liquid C is 20% by mass or less based on the total amount of the mixture. This can reduce the compression set of the crosslinked acrylic rubber obtained. It is presumed that the reason for this effect is that the emulsifier coexisting with the acrylic polymer is easily removed in the washing step described below due to the low content of the acrylic polymer. The content of the acrylic polymer may be preferably 19% by mass or less, 17% by mass or less, 15% by mass or less, 14% by mass or less, 13% by mass or less, 12% by mass or less, 11% by mass or less, or 10% by mass or less based on the total amount of the mixture, from the viewpoint of further reducing the compression set of the crosslinked acrylic rubber.
[0049] The content of the acrylic polymer in the mixture can be adjusted to fall within the above range by adjusting the content of the acrylic polymer in the latex L and the mixing ratio of the latex L and the coagulation liquid C in the mixture (in other words, the supply amounts of the latex L and the coagulation liquid C).
[0050] As the latex L, the reaction product (containing an acrylic polymer and an emulsifier) obtained in the polymerization step may be used as it is, or the reaction product may be diluted with water, for example, to adjust the content of the acrylic polymer in the latex L before use.
[0051] In one embodiment, the content of the acrylic polymer in the latex L may be 30% by mass or more, 31% by mass or more, 32% by mass or more, 33% by mass or more, 34% by mass or more, or 35% by mass or more, and may be 50% by mass or less, based on the total amount of the latex L. In this case, in order to make the content of the acrylic polymer in the mixture within the above range, the mass ratio of the content of the coagulation liquid C to the content of the latex L in the mixture (supply amount of the coagulation liquid C / supply amount of the latex L) is preferably 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1 or more, 1.5 or more, 1.8 or more, 2 or more, or 2.2 or more, and may be, for example, 4 or less. In this case, in addition to being able to reduce the compression set of the crosslinked product of the acrylic rubber, the yield of the acrylic rubber can be increased.
[0052] In another embodiment, the content of the acrylic polymer in the latex L may be less than 30% by mass, 25% by mass or less, 20% by mass or less, 17% by mass or less, or 15% by mass or less, for example, 10% by mass or more, based on the total amount of the latex L. In this case, since the content of the acrylic polymer in the latex L is relatively small, it is easy to adjust the content of the acrylic polymer in the mixture to the above range. The mass ratio of the content of the coagulation liquid C to the content of the latex L in the mixture (the supply amount of the coagulation liquid C / the supply amount of the latex L) may be, for example, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, or 0.5 or more, and may be 1 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, or 0.5 or less. In this embodiment, the compression set of the crosslinked product of the acrylic rubber can be further reduced.
[0053] The method for producing acrylic rubber may further include a first drainage step, a first washing step, a second drainage step, a second washing step, a third drainage step, and a drying step, in this order, following the coagulation step. Each of these steps is carried out while extruding the acrylic polymer coagulated in the coagulation zone 2 by rotating the screw of the extruder 1. The rotation speed of the screw of the extruder 1 may be, for example, 40 rpm or more and 200 rpm or less.
[0054] In the first drainage step, in the first drainage zone 3, the acrylic polymer is dehydrated by the rotation of the screw of the extruder 1, and drainage D1 is performed through the drainage slit.
[0055] In the first washing step, the acrylic polymer is washed in the first washing zone 4 by rotating the screw of the extruder 1 while feeding a washing liquid W1, thereby removing impurities (emulsifier, coagulant, unreacted matter, etc.) in the acrylic polymer. The washing liquid W1 may be, for example, water.
[0056] In the second drainage step, in the second drainage zone 5, the acrylic polymer is dehydrated by the rotation of the screw of the extruder 1, and drainage D2 is performed through the drainage slit.
[0057] In the second washing step, the acrylic polymer is further washed in the second washing zone 6 by rotating the screw of the extruder 1 while feeding the washing liquid W2, and impurities in the acrylic polymer (emulsifier, coagulant, unreacted matter, etc.) are further removed. The washing liquid W2 may be, for example, water.
[0058] In the third drainage step, in the third drainage zone 7, the acrylic polymer is dehydrated by the rotation of the screw of the extruder 1, and drainage D3 is performed through the drainage slit.
[0059] The total amount of the cleaning liquids W1, W2 supplied in the first cleaning step and the second cleaning step may be, for example, 250 parts by mass or more and 800 parts by mass or less with respect to 100 parts by mass of the acrylic polymer.
[0060] In the drying step, the acrylic polymer is dried in the drying zone 8, for example, by heating under reduced pressure conditions. The pressure of the reduced pressure conditions may be, for example, 90 kPa or less, or 50 kPa or more. Heating is performed, for example, by increasing the temperature of the drying zone 8 and raising the head of the extruder 1. The temperature of the drying zone 8 may be, for example, 105°C or more, or 200°C or less. The temperature of the head of the extruder 1 may be, for example, 130°C or more, or 200°C or less.
[0061] Through the above steps, the acrylic rubber R is extruded from the extruder 1, and the acrylic rubber R is obtained. The acrylic rubber thus obtained may be mixed with additives as necessary and used as a rubber composition. Another embodiment of the present invention is a method for producing a rubber composition, comprising a step of obtaining an acrylic rubber by the above-mentioned method for producing an acrylic rubber, and a step of mixing the acrylic rubber with additives to obtain a rubber composition.
[0062] The content of the acrylic rubber may be, for example, 50 mass % or more, 55 mass % or more, or 60 mass % or more, and may be 90 mass % or less, based on the total amount of the rubber composition.
[0063] The additives include, for example, fillers, lubricants, antioxidants, surfactants, crosslinking agents, and crosslinking accelerators.
[0064] Examples of the filler include carbon black, silica, talc, and calcium carbonate. The content of the filler may be, for example, 30 parts by mass or more and 100 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.
[0065] Examples of the lubricant include liquid paraffin, stearic acid, stearylamine, fatty acid zinc, fatty acid ester, and organosilicone. The content of the lubricant may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.
[0066] Examples of the antioxidant include aromatic amine compounds and phenol compounds. The content of the antioxidant may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.
[0067] The surfactant may be, for example, an alkyl sulfate ester salt. The content of the surfactant may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.
[0068] Examples of the crosslinking agent include an imidazole compound and a diamine compound. The content of the crosslinking agent may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.
[0069] The crosslinking accelerator is preferably used when the rubber composition contains a crosslinking agent. Examples of the crosslinking accelerator include trimethylthiourea compounds, phenothiazine compounds, aliphatic monovalent secondary amine compounds, aliphatic monovalent tertiary amine compounds, quaternary onium salts, tertiary phosphine compounds, alkali metal salts of weak acids, diazabicycloalkene compounds, and guanidine compounds. The content of the crosslinking accelerator may be, for example, 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the acrylic rubber.
[0070] The rubber composition is preferably used in a crosslinked state (as a crosslinked product). Another embodiment of the present invention is a method for producing a crosslinked product of a rubber composition, comprising the steps of obtaining an acrylic rubber by the above-mentioned method for producing an acrylic rubber, mixing the acrylic rubber with an additive to obtain a rubber composition, and crosslinking the rubber composition to obtain a crosslinked product.
[0071] The method for crosslinking the rubber composition may be a known method, and may, for example, include a first crosslinking step of heating and pressurizing the rubber composition, and a second crosslinking step of further heating the rubber composition after the first crosslinking step.
[0072] In the first crosslinking step, the heating temperature may be, for example, 150° C. or higher and 220° C. or lower. The pressure during pressing may be, for example, 0.4 MPa or higher and 20 MPa or lower. The time for which heating and pressing are performed may be, for example, 5 minutes or longer and 2 hours or shorter.
[0073] In the second crosslinking step, the heating temperature may be, for example, 150° C. or more and 220° C. or less. The heating time may be, for example, 30 minutes or more and 24 hours or less.
[0074] When the monomers constituting the acrylic rubber contain a crosslinking group monomer, the crosslinking group (crosslinking point) of the crosslinking group monomer forms a crosslink between the acrylic rubbers. In this case, when the rubber composition contains a crosslinking agent, the crosslinking agent further forms a crosslink between the acrylic rubbers. Alternatively, when the monomers constituting the acrylic rubber do not contain a crosslinking group monomer and the rubber composition contains a crosslinking agent, the crosslinking agent forms a crosslink between the acrylic rubbers.
[0075] The crosslinked product of the rubber composition is particularly suitable for use as rubber hoses and sealing parts such as gaskets and packings. Examples of rubber hoses include transmission oil cooler hoses, engine oil cooler hoses, air duct hoses, turbo hoses, hot air hoses, radiator hoses, power steering hoses, fuel system hoses, and drain system hoses for automobiles, construction machinery, hydraulic equipment, etc. The crosslinked product of the rubber composition containing the acrylic rubber obtained by the above-mentioned production method is excellent in terms of compression set, and is therefore particularly suitable for turbo hoses and sealing parts.
[0076] Examples of sealing parts include engine head cover gaskets, oil pan gaskets, oil seals, lip seal packings, O-rings, transmission seal gaskets, crankshafts, camshaft seal gaskets, valve stems, power steering seal belt cover seals, constant velocity joint boot materials, and rack and pinion boot materials. EXAMPLES
[0077] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0078] <Examples 1-1 to 1-4 and Comparative Example 1-1> (Manufacture of acrylic rubber) Into a pressure-resistant reaction vessel with an internal volume of 40 liters, 11 kg of a monomer mixture consisting of 70 parts by mass of ethyl acrylate, 30 parts by mass of n-butyl acrylate, and 2.66 parts by mass of monobutyl maleate, 17 kg of a 4% by mass aqueous solution of partially saponified polyvinyl alcohol (saponification degree of polyvinyl alcohol: 88 mol%) as an emulsifier, and 22 g of sodium acetate were charged and mixed well in advance with a stirrer to prepare a uniform suspension. After replacing the air in the upper part of the vessel with nitrogen, stirring was continued and the vessel was kept at 55°C, and then 2 liters of an aqueous solution of t-butyl hydroperoxide (0.25% by mass) was added to start emulsion polymerization. The temperature in the vessel was kept at 55°C, and the reaction was terminated after 6 hours.
[0079] Water was added to the reaction liquid after the reaction was completed as necessary to obtain a latex containing the acrylic polymer (and further containing the above-mentioned emulsifier, etc.) in the amount (% by mass based on the total amount of the latex) shown in Table 1. In addition, a mixture of 1.25 parts by mass of sodium borate, 2.25 parts by mass of ammonium sulfate, and 3.75 parts by mass of ammonium borate was used as a coagulant, and the mixture (coagulant) was dissolved in water so that the content of the mixture (coagulant) became the amount shown in Table 1 (% by mass based on the total amount of the coagulation liquid), to obtain a coagulation liquid.
[0080] Next, in a twin-screw kneading extruder 1 (TEM-50, manufactured by Toshiba Machine Co., Ltd.) having a configuration as shown in FIG. 1 (details described above), the obtained latex L and the coagulation liquid C were fed to the coagulation zone 2 in the amounts shown in Table 1, respectively, and mixed to coagulate the acrylic polymer. Next, while the coagulated acrylic polymer was extruded at a screw rotation speed of 120 rpm of the extruder 1, drainage D1 was performed from the acrylic polymer in the first drainage zone 3. Thereafter, using water as the washing liquids W1 and W2, water washing in the first washing zone 4 and drainage D2 in the second drainage zone 5, and water washing in the second washing zone 6 and drainage D3 in the third drainage zone 7 were performed in sequence. The total amount of water used in the first washing zone 4 and the second washing zone 6 was 430 parts by mass relative to 100 parts by mass of the acrylic polymer. Finally, in the drying zone 8, the acrylic polymer was heated under reduced pressure (80 kPa) (temperature in the drying zone 8: 150° C., temperature of the extruder head: 155° C.) to obtain an acrylic rubber.
[0081] The content (mass%) of the acrylic polymer in the mixture of the latex and the coagulation liquid shown in Table 1 was calculated by the following formula. Content of acrylic polymer in the mixture = F A / (F L +F C ) x 100 During the ceremony, F A : Acrylic polymer supply rate (kg / h) F L :Latex supply rate (kg / h) F C : Supply amount of coagulation liquid (kg / h) and F A was calculated according to the following formula. F A =F L ×C A / 100 During the ceremony, C A : Acrylic polymer content in latex (mass%) It is.
[0082] (Preparation of Rubber Composition) Next, 100 parts by mass of each of the obtained acrylic rubbers and the following components were kneaded with an 8-inch open roll to obtain a rubber composition. Filler: Carbon black (Tokai Carbon Co., Ltd., SEAT SO) 50 parts by weight Lubricant: 1 part by weight of stearic acid (Kao Corporation, Lunac S-90) and 0.3 parts by weight of stearylamine (Kao Corporation, Farmin 80) Antioxidant: 1 part by weight of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Naugard #445, manufactured by Addivant) Crosslinking agent: 0.6 parts by mass of 6-aminohexylcarbamic acid (Diak#1, manufactured by DuPont) Crosslinking accelerator: 0.8 parts by mass of 1,8-diazabicyclo-5,4,0-undec-7-ene-containing material (RHENOGRAN XLA-60 manufactured by LANXESS)
[0083] (Evaluation of compression set) The obtained rubber composition was cut into a sheet having a thickness of 2.4 mm, and then, using a press vulcanizer, the sheets were stacked in six pieces and heated and pressed for 20 minutes under conditions of 170°C and 10 MPa to perform primary vulcanization (crosslinking). Then, using a gear oven, the sheets were heated at 170°C for 4 hours to perform secondary vulcanization (crosslinking), and a disk-shaped test piece having a diameter of 29.0±0.5 mm and a thickness of 12.5±0.5 mm was obtained. The compression set (%) of the test piece was measured at 150°C for 144 hours in accordance with JIS K6262. Table 1 shows the relative value of the compression set of each example when the compression set of Comparative Example 1-1 is taken as 100.
[0084] [Table 1]
[0085] <Examples 2-1 to 2-2 and Comparative Example 2-1> In the production of the acrylic rubber, the composition of the monomer mixture was changed to 80 parts by mass of ethyl acrylate, 20 parts by mass of n-butyl acrylate, and 4.00 parts by mass of monobutyl maleate, and the acrylic rubber was produced, the rubber composition was prepared, and the compression set was evaluated in the same manner as in Example 1-1, etc. The production conditions of the acrylic rubber and the evaluation results of the compression set (relative values of the compression set of each example when the compression set of Comparative Example 2-1 is taken as 100) are shown in Table 2.
[0086] [Table 2]
[0087] <Example 3-1 and Comparative Example 3-1> In the production of the acrylic rubber, the composition of the monomer mixture was changed to 46 parts by mass of ethyl acrylate, 26 parts by mass of n-butyl acrylate, 28 parts by mass of n-butyl methacrylate, and 4.00 parts by mass of monobutyl maleate, and the acrylic rubber was produced, the rubber composition was prepared, and the compression set was evaluated in the same manner as in Example 1-1, etc. The production conditions of the acrylic rubber and the evaluation results of the compression set (relative values of the compression set of the examples when the compression set of Comparative Example 3-1 is taken as 100) are shown in Table 3.
[0088] [Table 3]
[0089] <Examples 4-1 to 4-2 and Comparative Example 4-1> In the production of the acrylic rubber, the composition of the monomer mixture was changed to 20.9 parts by mass of vinyl acetate, 10.4 parts by mass of methyl acrylate, 68.7 parts by mass of n-butyl acrylate, and 1.55 parts by mass of glycidyl methacrylate, and the coagulant was changed to a mixture of 2.5 parts by mass of sodium borate and 1.5 parts by mass of ammonium sulfate, but the acrylic rubber was produced in the same manner as in Example 1-1, etc.
[0090] Next, 100 parts by mass of each of the obtained acrylic rubbers and the following components were kneaded with an 8-inch open roll to obtain a rubber composition. Filler: Carbon black (Tokai Carbon Co., Ltd., SEAT SO) 50 parts by weight Lubricant: 1 part by weight of stearic acid (Kao Corporation, Lunac S-90) and 0.3 parts by weight of stearylamine (Kao Corporation, Farmin 80) Antioxidant: 1 part by weight of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Naugard #445, manufactured by Addivant) Surfactant: Sodium lauryl sulfate (Kao Corporation, Emal 0) 1 part by weight Crosslinking agent: 1.4 parts by mass of 1-(2-cyanoethyl)-2-methylimidazole (CN-25, manufactured by Shikoku Chemical Industry Co., Ltd.) Crosslinking accelerator: 0.3 parts by weight of ammonium benzoate (Balnoc AB, manufactured by Ouchi Shinko Co., Ltd.)
[0091] The obtained rubber compositions were evaluated for compression set in the same manner as in Example 1-1, etc. The manufacturing conditions of the acrylic rubber and the evaluation results of compression set (relative values of compression set of each Example when the compression set of Comparative Example 4-1 is taken as 100) are shown in Table 4.
[0092] [Table 4] [Explanation of symbols]
[0093] 1...extruder, 2...coagulation zone, 3...first drainage zone, 4...first washing zone, 5...second drainage zone, 6...second washing zone, 7...third drainage zone, 8...drying zone.
Claims
1. A step of emulsion polymerizing an alkyl acrylate-containing monomer in the presence of an emulsifier to obtain an acrylic polymer; mixing a latex containing the acrylic polymer and the emulsifier with a coagulating liquid containing a coagulating agent to coagulate the acrylic polymer; a content of the acrylic polymer in the mixture of the latex and the coagulation liquid is 20 mass% or less based on the total amount of the mixture.
2. The content of the acrylic polymer in the latex is 30% by mass or more based on the total amount of the latex, 2. The method for producing an acrylic rubber according to claim 1, wherein a mass ratio of a content of the coagulation liquid to a content of the latex in the mixture is 0.6 or more.
3. 2. The method for producing an acrylic rubber according to claim 1, wherein a content of the acrylic polymer in the latex is less than 30% by mass based on a total amount of the latex.
4. The method for producing an acrylic rubber according to any one of claims 1 to 3, wherein the monomers further contain a crosslinking monomer.
5. The method for producing an acrylic rubber according to claim 4, wherein the crosslinking monomer is a crosslinking monomer having a carboxyl group.
Citation Information
Patent Citations
Process for producing acrylic rubber, and acrylic rubber obtained by said production process
JP2019189835A