Active energy ray-curable composition, cured product and laminate

The active energy ray-curable composition with a (meth)acrylate compound and fine particles addresses the challenge of balancing anti-glare and transparency in FPDs by providing a hard coat layer with controlled optical properties.

JP2024154092APending Publication Date: 2024-10-30DIC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023067713
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

Existing methods for controlling anti-glare properties in hard coat layers of flat panel displays (FPDs) face challenges in balancing anti-glare properties with haze and total light transmittance, as they often deteriorate mechanical properties or require complex adjustments in particle ratios and refractive indices.

Method used

An active energy ray-curable composition comprising a (meth)acrylate compound with a chain hydrocarbon group and a hydroxyl group, combined with fine particles, allows for precise control of anti-glare properties without affecting haze and total light transmittance.

Benefits of technology

The composition enables the formation of a hard coat layer with desired anti-glare properties while maintaining transparency and clarity, facilitating easy and precise control of optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154092000001
    Figure 2024154092000001
  • Figure 2024154092000002
    Figure 2024154092000002
  • Figure 2024154092000003
    Figure 2024154092000003
Patent Text Reader

Abstract

To provide an active energy ray-curable composition for forming a hard coat layer that facilitates strict control of antiglare performance without compromising other essential properties of the hard coat layer, such as haze and overall light transmission, a cured product thereof, and a laminate including a cured coating layer thereof.SOLUTION: An active energy ray-curable composition includes a compound (A) with one or two (meth)acryloyloxy groups, a hydroxy group (excluding a carboxy group), and an optionally substituted chain hydrocarbon group, an active energy ray-curable compound (B) that does not correspond to the compound (A), fine particles (C) and an organic solvent (D).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable composition and a cured product thereof, as well as a laminate having a cured coating film of the composition. [Background technology]

[0002] Flat panel displays (FPDs) such as liquid crystal displays (LCDs), organic light-emitting diode displays (OLEDs), and plasma displays (PDPs) are laminates of substrates with various functions, and in recent years, there has been an increasing demand for lower costs and higher definition. Various resin films are used for the surface (viewing side) of FPDs, but the surface of the resin film is soft and has low scratch resistance, so to compensate for this, it is common to provide a cured coating (hard coat layer) on the film surface. Specifically, the film is sent from a roll of raw film to a coater, and then a hard coat agent consisting of an active energy ray curable composition or the like is applied to the film surface and dried, and the hard coat agent is cured by irradiation with active energy rays such as ultraviolet rays to form a hard coat layer, and then the film is rolled up again to produce a film with a hard coat layer (hard coat film).

[0003] The hard coat layer that forms the outermost layer of an FPD is required to have a variety of functions in addition to protecting the resin film underneath. One of the desired functions is the effect of reducing reflections from fluorescent lights, etc. (anti-glare property) As a method for imparting anti-glare property to a hard coat layer, a method is known in which a hard coat agent containing organic or inorganic fine particles is used to provide a fine uneven structure on the surface of the hard coat layer to diffusely reflect light.

[0004] It is said that a combination of large and small irregularities is effective in suppressing glare and roughness caused by a fine uneven structure, suppressing the decrease in image clarity caused by haze, achieving high definition while maintaining an appropriate range of anti-glare properties, and controlling the suppression of white blur and decreased visibility. For example, Patent Document 1 discloses a photocurable resin composition that contains a photopolymerizable component including a photopolymerizable (meth)acrylic resin with a weight-average molecular weight of 10,000 or more, organic and / or inorganic fine particles with an average particle size of 1.0 to 2.8 μm, and a photopolymerization initiator, and has a viscosity of 1 mPa s or more and 1,000 mPa s or less at 23°C. Patent Document 2 discloses an antiglare film formed by laminating at least a transparent substrate film and an antiglare layer, in which the antiglare layer contains at least first light-transmitting fine particles and second light-transmitting fine particles having different refractive indices in a light-transmitting resin, the refractive index of the first light-transmitting fine particles being higher than the refractive index of the second light-transmitting fine particles, and the refractive index difference between the light-transmitting resin and the first light-transmitting fine particles being 0.04 to 0.20. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-45448 A [Patent Document 2] JP 2009-86677 A Summary of the Invention [Problem to be solved by the invention]

[0006] The invention described in the above Patent Document 1 is an invention that attempts to control the anti-glare property by the viscosity of the active energy ray-curable composition and the molecular weight of the photopolymerizable resin, while the invention described in Patent Document 2 is an invention that attempts to control the anti-glare property by using multiple particles with different refractive indices in combination. However, there is still room for improvement in the anti-glare property control methods described in Patent Documents 1 and 2. In addition, in the invention described in Patent Document 1, the antiglare properties are controlled by the viscosity of the composition and the weight-average molecular weight of the photopolymerizable (meth)acrylic resin, but there are concerns that increased viscosity may cause deterioration of leveling properties and reduced mechanical properties. In addition, in Patent Document 2, the anti-glare property is controlled by using a plurality of particles with different refractive indices. However, changing the particle amount also changes the refractive index. Therefore, changing the particle amount or particle ratio also significantly changes the haze, which is an important optical property, making it difficult to balance the anti-glare property and the haze.

[0007] Therefore, the problem to be solved by the present invention is to provide an active energy ray-curable composition for forming a hard coat layer, which is capable of easily and strictly controlling antiglare properties (transmission clarity) without deteriorating other properties required for the hard coat layer, such as haze and total light transmittance, and a laminate having a cured product thereof and a cured coating film thereof. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above problems, the inventors discovered that by using a (meth)acrylate compound having a chain hydrocarbon group and a hydroxyl group together with fine particles, it is possible to control the antiglare properties without impairing other properties, and thus completed the present invention.

[0009] That is, the present invention relates to the following inventions. (1) An active energy ray-curable composition comprising: a compound (A) having one or two (meth)acryloyloxy groups, a hydroxyl group (excluding a carboxyl group), and a chain hydrocarbon group which may have a substituent; an active energy ray-curable compound (B) which does not fall under the category of compound (A); fine particles (C); and an organic solvent (D). (2) The active energy ray-curable composition according to (1), wherein the compound (A) has a molecular weight of 1,000 or less. (3) The active energy ray-curable composition according to (1) or (2), wherein the active energy ray-curable compound (B) is an acrylic resin containing a (meth)acryloyl group in a side chain. (4) The active energy ray-curable composition according to any one of (1) to (3), wherein the active energy ray-curable compound (B) is a compound having a hydroxyl group. (5) The active energy ray-curable composition according to any one of (1) to (4), wherein the fine particles (C) are organic crosslinked fine particles. (6) The active energy ray-curable composition according to any one of (1) to (5), wherein the fine particles (C) are at least one selected from the group consisting of acrylic fine particles, acrylic-styrene copolymer fine particles, and polystyrene fine particles. (7) The active energy ray-curable composition according to any one of (1) to (6), wherein the fine particles (C) have an average particle size of 0.05 μm to 10 μm. (8) The active energy ray-curable composition according to any one of (1) to (7), wherein the fine particles (C) have a refractive index of 1.48 to 1.66. (9) A cured product of the active energy ray-curable composition according to any one of (1) to (8). (10) A laminate having a cured coating film of the active energy ray-curable composition according to any one of (1) to (8). Effect of the Invention

[0010] The active energy ray-curable composition of the present invention uses fine particles in combination with a (meth)acrylate compound having a hydroxyl group and a chain hydrocarbon group, and thereby can form a hard coat layer having desired antiglare properties without deteriorating other properties such as haze and total light transmittance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Active energy ray-curable composition> The active energy ray-curable composition of the present invention (hereinafter, may be simply referred to as the "composition") contains a compound (A) consisting of one or two (meth)acryloyloxy groups, a hydroxyl group (excluding a carboxy group), and a chain hydrocarbon group which may have a substituent, an active energy ray-curable compound (B) other than the compound (A), fine particles (C), and an organic solvent (D). In the present invention, "(meth)acrylate" refers to either or both of acrylate and methacrylate, "(meth)acryloyl" refers to either or both of acryloyl and methacryloyl, and "(meth)acrylic" refers to either or both of acrylic and methacrylic.

[0012] [Compound (A) Containing One or Two (Meth)acryloyloxy Groups, a Hydroxyl Group, and a Chain Hydrocarbon Group Which May Have a Substitute] In compound (A) consisting of one or two (meth)acryloyloxy groups, a hydroxyl group, and a chain hydrocarbon group which may have a substituent (hereinafter, sometimes referred to as "compound (A)" or "component (A)". The same applies to other compounds of component (A)), the (meth)acryloyloxy group refers to the group represented by "(CH2)=CR 1 -C(=O)-O-" (R 1 is H or CH3.) In addition, in this specification, the hydroxyl group (-OH) in the component (A) does not include the OH in the carboxy group (-COOH). Since component (A) is composed of a hydroxyl group, a chain hydrocarbon group which may have a substituent, and one or two (meth)acryloyloxy groups, it is a hydrophilic low molecular weight compound with relatively high polarity, and it is possible to control the antiglare property through the dispersibility and aggregation of fine particles (C) described later. Specifically, the control of antiglare property, which is one of the problems to be solved by the present application, is closely related to the dispersion state and aggregation state of the particles, and the use of compound (A) makes it possible to arbitrarily control the dispersion and aggregation state of the fine particles (C), thereby enabling the control of antiglare property.

[0013] The chain hydrocarbon group contained in the component (A) may be a straight-chain hydrocarbon group or a branched-chain hydrocarbon group. The straight-chain hydrocarbon group is preferably a straight-chain group in which one or two hydrogen atoms have been removed from an alkane, and examples of such a straight-chain alkyl group or straight-chain alkylene group include: Specific examples of the alkyl group include linear alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group; and linear alkylene groups such as a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, and a decamethylene group. The branched hydrocarbon group is preferably a branched group in which one or two hydrogen atoms have been removed from an alkane, and examples of the branched alkyl group and branched alkylene group include the branched alkyl group and the branched alkylene group. Specifically, branched alkyl groups such as an isopropyl group, an isobutyl group, a tert-butyl group, an isopentyl group, a neopentyl group, and groups in which the hydrogen atom of the above-mentioned linear alkyl group is substituted with an alkyl group having 1 to 10 carbon atoms; alkyl methylene groups such as -CH(CH3)-, -CH(CH2CH3)-, -C(CH3)2-, -C(CH3)(CH2CH3)-, -C(CH3)(CH2CH2CH3)-, and -C(CH2CH3)2-; alkylethylene groups such as -C(CH3)-, -C(CH3)2CH2-, -CH(CH2CH3)CH2-, -C(CH2CH3)2-CH2-, alkyltrimethylene groups such as -CH(CH3)CH2CH2-, -CH2CH(CH3)CH2-, and alkyltetramethylene groups such as -CH(CH3)CH2CH2CH2-, -CH2CH(CH3)CH2CH2-, and branched alkylene groups in which the hydrogen atoms of the above-mentioned linear alkylene groups are substituted with alkyl groups having 1 to 10 carbon atoms.

[0014] In this specification, the substituent that a hydrocarbon group has means both a monovalent substituent substituting a hydrogen atom (-H) in the hydrocarbon group, and a divalent substituent substituting a methylene group (-CH-) in the hydrocarbon group. Examples of the monovalent substituent include an alkoxy group, a halogen atom, a halogenated alkyl group, and a carboxy group. Divalent substituents include groups containing a heteroatom, such as -O-, -C(=O)-, -NH-, -P(=O)-, and the like, and these groups may be used in combination. The number of carbon atoms in the chain hydrocarbon group is preferably 1 to 20, more preferably 2 to 15, and particularly preferably 3 to 13. The chain hydrocarbon group preferably has one or more substituents selected from the group consisting of -O-, -C(=O)-, and -P(=O)-.

[0015] The number of (meth)acryloyloxy groups contained in the compound of component (A) may be 1 to 2. When the compound has two (meth)acryloyloxy groups, both of them may be acryloyloxy groups, both of them may be methacryloyl groups, or they may be a combination of an acryloyloxy group and a methacryloyl group. The hydroxyl group of the compound of component (A) exists in the compound as a substituent substituting a hydrogen atom of the chain hydrocarbon group which may have the above-mentioned substituent. The presence of the hydroxyl group makes component (A) a hydrophilic compound with relatively high polarity. As a result, when the fine particles (C) described later have hydrophobic properties such as acrylic, acrylic-styrene copolymer, polystyrene, etc., it is possible to promote aggregation of the fine particles (C), and the antiglare property can be strictly controlled according to the amount of component (A) added.

[0016] The component (A) is preferably a compound represented by the following formula (A-1) or the following formula (A-2).

[0017] [ka]

[0018] In the formula, R 1 is a hydrogen atom or -CH3, and 1 may be the same or different. R 2 ~R 3is a chain hydrocarbon group which may have a substituent and which has at least one hydroxyl group as a substituent. Examples of the chain hydrocarbon group which may have a substituent include those mentioned above.

[0019] Component (A) is preferably a low molecular weight compound, and the molecular weight is preferably not more than 1000, more preferably not more than 800. The low molecular weight compound enhances the mobility of the compound, and has the effect of controlling the aggregation of particles when the solvent in the composition evaporates.

[0020] The component (A) can be used alone or in combination of two or more types. In the composition of the present invention, the proportion of component (A) relative to the total amount of solid components is preferably 0.1 to 50 mass%, more preferably 0.3 to 40 mass%, even more preferably 0.5 to 30 mass%, particularly preferably 0.8 to 20 mass%, and most preferably 1 to 10 mass%.

[0021] [Active energy ray-curable compound (B)] The (B) component is not particularly limited as long as it does not fall under the category of the (A) component, and may be a low molecular weight monomer other than the (A) component, or a high molecular weight copolymer (resin) having a specific repeating unit. Examples of the monomer (B) that can be used include urethane (meth)acrylate (B1), epoxy (meth)acrylate (B2), other polyfunctional (meth)acrylates not corresponding to the (A) component (B3), polyester (meth)acrylate (B4), polyether (meth)acrylate, and styrene.

[0022] The urethane (meth)acrylate (B1) may be, for example, a reaction product of a polyisocyanate (b1-1) with a (meth)acrylate (b1-2) having a hydroxyl group; or a reaction product of a polyisocyanate (b1-1), a (meth)acrylate (b1-2) having a hydroxyl group, and a polyol (b1-3), which has one or more (preferably 2 to 6) (meth)acryloyl groups.

[0023] Examples of the polyisocyanate (b1-1) that can be used include aliphatic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate; alicyclic polyisocyanates such as norbornane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), 1,3-bis(isocyanatomethyl)cyclohexane, 2-methyl-1,3-diisocyanatocyclohexane, and 2-methyl-1,5-diisocyanatocyclohexane; and aromatic polyisocyanates such as toluene diisocyanate, xylene diisocyanate, and diphenylmethane diisocyanate. These polyisocyanates may be used alone or in combination of two or more.

[0024] As the polyisocyanate (b1-1), among the above-mentioned ones, it is preferable to use an aliphatic polyisocyanate and / or an alicyclic polyisocyanate, since it is possible to reduce coloration of the cured coating film of the active energy ray-curable composition, more preferably one or more polyisocyanates selected from the group consisting of hexamethylene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane diisocyanate, and even more preferably hexamethylene diisocyanate and / or isophorone diisocyanate.

[0025] The (meth)acrylate having a hydroxyl group (b1-2) has a hydroxyl group and a (meth)acryloyl group, and examples thereof include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,5-pentanediol mono(meth)acrylate, 1,6-hexanediol mono(meth)acrylate, neopentyl glycol mono(meth)acrylate, and neopentyl hydroxypivalate. mono(meth)acrylates of dihydric alcohols such as ethyl glycol mono(meth)acrylate; mono- or di(meth)acrylates of trihydric alcohols such as trimethylolpropane di(meth)acrylate, ethylene oxide (EO)-modified trimethylolpropane (meth)acrylate, propylene oxide (PO)-modified trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, and bis(2-(meth)acryloyloxyethyl)hydroxyethyl isocyanurate; Mono- and di(meth)acrylates having hydroxyl groups in which some of these alcoholic hydroxyl groups have been modified with ε-caprolactone; compounds having a monofunctional hydroxyl group and a trifunctional or higher (meth)acryloyl group, such as pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, or polyfunctional (meth)acrylates having hydroxyl groups in which the compounds have been further modified with ε-caprolactone; (meth)acrylates having an oxyalkylene chain, such as dipropylene glycol mono(meth)acrylate, diethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, etc.; (meth)acrylates having an oxyalkylene chain of a block structure, such as polyethylene glycol-polypropylene glycol mono(meth)acrylate, polyoxybutylene-polyoxypropylene mono(meth)acrylate, etc.;Examples of the methacrylate include poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate and poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate having a random structure of oxyalkylene chain.

[0026] These (meth)acrylates (b1-2) having a hydroxyl group may be used alone, or two or more of them may be used in combination. In particular, when the urethane (meth)acrylate (B1) is obtained without using the polyol (b1-3), it is preferable to use one or more compounds selected from the group consisting of pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and tripentaerythritol hepta(meth)acrylate as the compound (b1-2), since even better scratch resistance can be obtained. When the urethane (meth)acrylate (B1) is obtained using the polyol (b1-3), it is preferable to use 2-hydroxyethyl (meth)acrylate.

[0027] As the polyol (b1-3), for example, polyether polyols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyester polyols, polycarbonate polyols, etc. can be used. These polyols may be used alone or in combination of two or more. Among these, it is preferable to use polyether polyols, and polytetramethylene glycol is more preferable, since it provides even better flexibility.

[0028] The reaction between the polyisocyanate (a1-1) and the (meth)acrylate (b1-2) having a hydroxyl group, and the reaction between the polyisocyanate (b1-1), the (meth)acrylate (b1-2) having a hydroxyl group, and the polyol (b1-3) can be carried out using a conventional urethane reaction. In addition, when carrying out the urethanization reaction, a urethanization catalyst may be used as necessary.As the urethanization catalyst, for example, amine compounds such as pyridine, pyrrole, triethylamine, diethylamine, dibutylamine, etc.; phosphorus compounds such as triphenylphosphine, triethylphosphine, etc.; organic tin compounds such as dibutyltin dilaurate, octyltin trilaurate, octyltin diacetate, dibutyltin diacetate, tin octylate, etc.; organic zinc compounds such as zinc octylate, etc. can be used.

[0029] When the urethane (meth)acrylate (B1) is of the type that uses a polyol (b1-3), the number average molecular weight of the urethane (meth)acrylate is preferably in the range of 800 to 6,000, more preferably in the range of 1,000 to 4,000, in terms of obtaining even better flexibility and scratch resistance. The number average molecular weight of the urethane (meth)acrylate is a value measured by gel permeation column chromatography (GPC) (eluent: tetrahydrofuran, polystyrene equivalent).

[0030] The epoxy (meth)acrylate (B2) is not particularly limited as long as it does not fall under the category of the component (A), and specifically includes epoxy (meth)acrylates having a ring in the structure. As the epoxy (meth)acrylate (B2), for example, an addition reaction product of an unsaturated monocarboxylic acid and an epoxy compound can be used. As the unsaturated monocarboxylic acid, for example, (meth)acrylic acid, crotonic acid, cinnamic acid, etc. can be used. These compounds may be used alone or in combination of two or more. Among these, it is preferable to use (meth)acrylic acid from the viewpoint of scratch resistance.

[0031] As the epoxy compound, for example, epoxy compounds having a bisphenol A skeleton such as bisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, and brominated bisphenol A diglycidyl ether; epoxy compounds having a bisphenol F skeleton such as bisphenol F diglycidyl ether; epoxy compounds having a hydrogenated phthalic acid skeleton; compounds having an epoxy group and a (meth)acryloyl group such as glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate can be used. These compounds may be used alone or in combination of two or more kinds, or their polymers may be used. Among these, from the viewpoint of scratch resistance, it is preferable to use an epoxy group and a (meth)acrylic compound, and it is more preferable to use a polymer of glycidyl (meth)acrylate.

[0032] In the case where the epoxy compound polymer is used as the raw material of the epoxy (meth)acrylate (B2), the viscosity of the epoxy (meth)acrylate (B2) containing a solvent is preferably in the range of 100 to 3,000 mPa·s, more preferably in the range of 150 to 2,000 mPa·s, in order to further improve the coating stability when forming a hard coat layer. The viscosity is a value measured using a B-type viscometer.

[0033] The other polyfunctional (meth)acrylate (B3) refers to a monomer other than the components (A), (B1) and (B2) and having preferably 2 to 8, and more preferably 3 to 6, (meth)acryloyl groups in one molecule. Other polyfunctional (meth)acrylates (B3) include, for example, di(meth)acrylates of dihydric alcohols such as diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; di(meth)acrylates of polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate; di(meth)acrylates of diols obtained by adding 4 or more moles of ethylene oxide or propylene oxide to 1 mole of neopentyl glycol; di(meth)acrylates of diols obtained by adding 2 moles of ethylene oxide or propylene oxide to 1 mole of bisphenol A; trimethylolpropane tri(meth)acrylate, ethylene Oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, tris(2-(meth)acryloyloxyethyl)isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, etc. can be used. These compounds may be used alone or in combination of two or more.

[0034] As the compound (B3), among the above, it is more preferable to use one or more compounds selected from the group consisting of tripentaerythritol octa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, pentaerythritol tetra(meth)acrylate, and pentaerythritol tri(meth)acrylate, from the viewpoint of obtaining even better scratch resistance, and pentaerythritol tetra(meth)acrylate and / or pentaerythritol tri(meth)acrylate are more preferable.

[0035] The polyester (meth)acrylate (B4) may be, for example, a dehydration condensate of a polyester diol and (meth)acrylic acid. The polyester diol is preferably a reaction product of a diol and a dicarboxylic acid or an anhydride thereof. Examples of the diol that can be used include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, butylene glycol, polybutylene glycol, tetramethylene glycol, hexamethylene glycol, neopentyl glycol, cyclohexanedimethanol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol, as well as alkylene oxide adducts thereof. Examples of dicarboxylic acids or anhydrides thereof that can be used include orthophthalic acid, isophthalic acid, terephthalic acid, adipic acid, succinic acid, fumaric acid, maleic acid, hexahydrophthalic acid, tetrahydrophthalic acid, and trimellitic acid, as well as anhydrides thereof.

[0036] As the component (B) of the copolymer, for example, it is preferable to use an acrylic resin containing a (meth)acryloyl group in the side chain, and an example of such an acrylic resin is an acrylic acrylate resin (B11). The acrylic acrylate resin is a copolymer having a repeating unit derived from a (meth)acrylate monomer in the main chain, and has a (meth)acryloyl group in the side chain. The acrylic acrylate resin (B11) can be obtained, for example, by obtaining a homopolymer of a compound having a glycidyl group and a (meth)acryloyl group, or a copolymer of said compound and a (meth)acrylic acid ester (hereinafter, these are abbreviated as "precursor (1)"), and then reacting this with a compound having a carboxyl group and a (meth)acryloyl group.

[0037] Examples of the compound having a glycidyl group and a (meth)acryloyl group that is the raw material for precursor (1) include glycidyl (meth)acrylate, α-ethyl glycidyl (meth)acrylate, α-n-propyl glycidyl (meth)acrylate, α-n-butyl glycidyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 4,5-epoxypentyl (meth)acrylate, 6,7-epoxypentyl (meth)acrylate, α-ethyl-6,7-epoxypentyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, lactone-modified 3,4-epoxycyclohexyl (meth)acrylate, and vinylcyclohexene oxide. Among these, it is preferable to use glycidyl (meth)acrylate, α-ethyl glycidyl (meth)acrylate, and α-n-propyl glycidyl (meth)acrylate, since it is easy to adjust the (meth)acryloyl group equivalent of the resulting acrylic polymer (a) to a preferred range, and it is more preferable to use glycidyl (meth)acrylate.

[0038] As the (meth)acrylic acid ester that can be used in combination when producing the precursor (1), a (meth)acrylic acid ester having an alkyl group having 1 to 22 carbon atoms and a (meth)acrylic acid ester having an alicyclic alkyl group are preferred, and a (meth)acrylic acid ester having an alkyl group having 1 to 22 carbon atoms is more preferred. In particular, it is particularly preferred to use methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. The ratio of the copolymerization [a compound having a glycidyl group and a (meth)acryloyl group]:[a (meth)acrylic acid ester] is preferably 20 / 80 to 95 / 5 (mass ratio), more preferably 30 / 70 to 90 / 10 (mass ratio), further preferably 60 / 40 to 90 / 10 (mass ratio), and particularly preferably 80 / 20 to 90 / 10 (mass ratio).

[0039] The precursor (1) has an epoxy group derived from a compound having a glycidyl group and a (meth)acryloyl group, and the epoxy equivalent of the precursor (1) is preferably in the range of 150 to 500 g / eq, more preferably in the range of 150 to 250 g / eq, and even more preferably in the range of 150 to 180 g / eq, in that it becomes easy to adjust the acryloyl equivalent of the resulting acrylic polymer (a) to the range of 145 to 750 g / eq.

[0040] The precursor (1) can be produced, for example, by polymerizing the compound having a glycidyl group and a (meth)acryloyl group alone or in combination with the (meth)acrylic acid ester in the presence of a polymerization initiator in a temperature range of 60°C to 150°C. However, it is preferable to produce the precursor (1) by solution polymerization, since it is possible to continuously produce the precursor (1) and the subsequent reaction of the precursor (1) with the compound having a carboxyl group and a (meth)acryloyl group.

[0041] The solvent used in the production of the precursor (1) by solution polymerization desirably has a boiling point of 80° C. or higher, taking into consideration the reaction temperature. Examples of suitable solvents include ketone solvents such as methyl ethyl ketone, methyl-n-propyl ketone, methyl isopropyl ketone, methyl-n-butyl ketone, methyl isobutyl ketone, methyl-n-amyl ketone, methyl-n-hexyl ketone, diethyl ketone, ethyl-n-butyl ketone, di-n-propyl ketone, diisobutyl ketone, cyclohexanone, and phorone; ether solvents such as n-butyl ether, diisoamyl ether, and dioxane; n-propyl acetate, isopropyl acetate, and the like. Examples of suitable solvents include ester solvents such as propyl, n-butyl acetate, n-amyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and ethyl-3-ethoxypropionate; and hydrocarbon solvents such as toluene, xylene, Solvesso 100, Solvesso 150, Swazol 1800, Swazol 310, Isopar E, Isopar G, Exxon Naphtha No. 5, and Exxon Naphtha No. 6. These may be used alone or in combination of two or more. Among these, ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, and ester solvents such as isopropyl acetate and n-butyl acetate are preferred from the viewpoint of excellent solubility of the precursor (1) obtained.

[0042] Examples of the compound having a carboxyl group and a (meth)acryloyl group to be used next include unsaturated monocarboxylic acids such as (meth)acrylic acid, (acryloyloxy)acetic acid, 2-carboxyethyl acrylate, 3-carboxypropyl acrylate, 1-[2-(acryloyloxy)ethyl] succinate, 1-(2-acryloyloxyethyl) phthalate, 2-(acryloyloxy)ethyl hydrogen hexahydrophthalate, and lactone-modified products thereof; unsaturated dicarboxylic acids such as maleic acid; carboxyl group-containing polyfunctional (meth)acrylates obtained by reacting acid anhydrides such as succinic anhydride and maleic anhydride with hydroxyl group-containing polyfunctional (meth)acrylate monomers such as pentaerythritol triacrylate, etc. These may be used alone or in combination of two or more. Among these, (meth)acrylic acid, (acryloyloxy)acetic acid, 2-carboxyethyl acrylate, and 3-carboxypropyl acrylate are preferred, with (meth)acrylic acid being particularly preferred, since it is easy to adjust the (meth)acryloyl group equivalent of the resulting acrylic polymer (a) to the preferred range described above.

[0043] The acrylic acrylate resin (B11) has a higher double bond equivalent than general polyfunctional monomers, and by using the acrylic acrylate resin (B11), it is possible to suppress shrinkage of the cured product or the cured coating film when the composition of the present invention is cured with active energy rays.

[0044] When component (B) has a hydroxyl group in its structure, the presence of the hydroxyl group makes component (B) a hydrophilic compound with relatively high polarity, and as a result, component (B) having a hydroxyl group has the property of promoting aggregation when fine particles (C) described below are hydrophobic, such as acrylic, acrylic-styrene copolymer, polystyrene, etc. In addition, since component (A) also has a hydroxyl group, when component (B) has a hydroxyl group, the affinity and compatibility between component (A) and component (B) is improved. Therefore, it is also preferable to use a compound having a hydroxyl group as the component (B). As the component (B) having a hydroxyl group, a monomer such as pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, or tripentaerythritol hexa(meth)acrylate, or an acrylic acrylate resin (B11) having a hydroxyl group in its structure generated by the reaction of a glycidyl group with a carboxyl group is preferable.

[0045] The component (B) can be used alone or in combination of two or more types. In the composition of the present invention, the proportion of component (B) relative to the total amount of solid components is preferably 5 to 99 mass%, more preferably 10 to 98 mass%, further preferably 20 to 96 mass%, and particularly preferably 30 to 95 mass%.

[0046] [Fine particles (C)] The fine particles (C) (hereinafter sometimes referred to as "component (C)") may be organic fine particles (C1) or inorganic fine particles (C2), but it is preferable to use those having transparency. The refractive index of the component (C) is preferably from 1.48 to 1.66, more preferably from 1.50 to 1.63, and particularly preferably from 1.52 to 1.60, from the viewpoint of adjusting the difference in refractive index with the binder and achieving the desired coating film haze.

[0047] As the organic fine particles (C1), plastic polymer beads can be used, such as acrylic fine particles (refractive index 1.49 to 1.535), acrylic-styrene fine particles (refractive index 1.54 to 1.59), polystyrene fine particles (refractive index 1.60), melamine fine particles (refractive index 1.57), benzoguanamine-formaldehyde fine particles, polycarbonate fine particles, polyethylene fine particles, etc. Examples of the inorganic fine particles (C2) that can be used include silica particles such as spherical silica and amorphous silica, metal oxide particles such as titanium oxide, zinc oxide, zircon, zirconia and alumina, calcium carbonate particles, and barium sulfate particles. Among these, it is preferable to use organic fine particles, and it is preferable to use at least one selected from the group consisting of polystyrene fine particles, acrylic-styrene fine particles, and styrene fine particles, since they have excellent cohesive properties and form appropriate unevenness on the coating film surface, thereby obtaining even better antiglare properties, and acrylic-styrene fine particles are particularly preferable. The surfaces of the organic and inorganic fine particles may be untreated or may be subjected to a hydrophilic or hydrophobic treatment. The organic fine particles may be crosslinked organic fine particles (organic crosslinked fine particles). The method of crosslinking is not particularly limited, but a crosslinking agent generally used in this field may be added as necessary to adjust the degree of crosslinking to an appropriate range, thereby obtaining organic crosslinked fine particles.

[0048] The average particle size of the component (C) is preferably from 0.05 to 10 μm, more preferably from 0.1 to 5 μm, and particularly preferably from 0.5 to 3.0 μm, from the viewpoint of achieving high cohesive strength and even more excellent antiglare properties. The average particle size of component (C) refers to the particle size at which the integrated amount in the integrated particle amount curve of particle size distribution measurement accounts for 50%.

[0049] The component (C) can be used alone or in combination of two or more types. In the composition of the present invention, the proportion of component (C) relative to the total amount of solid components is preferably 0.1 to 50 mass%, more preferably 0.5 to 30 mass%, further preferably 1 to 20 mass%, and particularly preferably 1 to 10 mass%.

[0050] [Organic solvent (D)] The organic solvent (D) (hereinafter sometimes referred to as "component (D)") is not particularly limited, and ester-based solvents, glycol-based solvents, ketone-based solvents, hydrocarbon-based solvents, alcohol-based solvents, etc. can be used.

[0051] Among these, it is preferable to contain an organic solvent (D1) that disperses the component (C) and an organic solvent (D2) that aggregates the component (C). Hereinafter, these may be referred to as "component (D1)" and "component (D2)", respectively. In the composition of the present invention, by using at least two or more organic solvents which differ in the dispersibility and coagulation properties of component (C), the dispersibility of the particles in the coating film obtained by applying the composition can be controlled as desired, and the desired antiglare properties can be easily and precisely controlled. Furthermore, in the present invention, the antiglare properties are not controlled by the ratio of solid components, such as components (A) to (C), in the composition or the viscosity of the composition, so that it is possible to easily and simply control only the optical properties without affecting the coatability or coating hardness.

[0052] In the present invention, the "organic solvent for dispersing the component (C)" refers to an organic solvent in which the phase separation rate is 5.0% by volume or less of the total solid-liquid when 90 g of the organic solvent and 10 g of fine particles (acrylic-styrene copolymer crosslinked organic fine particles "ACRYBASE DLB-005" (product name, Fujikura Chemical Industries, refractive index 1.55, D50 average particle size 0.98 μm)) are mixed in a 140 mL transparent bottle (PS-NO. 10K, Isoya Glass Industry Co., Ltd.), uniformly mixed for 3 minutes using a vortex mixer (MIXER UZUSIO VTX-3000L, LMS CO., LTD.), allowed to stand for 10 minutes, and then observed visually. On the other hand, the "organic solvent that aggregates" component (C) refers to an organic solvent other than the above-mentioned "organic solvent that disperses" and which, when a test of mixing, leaving, and visual inspection is carried out in the same manner as described above, causes visual phase separation in an amount of more than 5.0 volume % of the total solid-liquid.

[0053] (Organic solvent (D1)) The (D1) component that disperses the (C) component may be, for example, an organic solvent that does not contain a primary hydroxyl group, and is preferably a non-alcoholic solvent. In this specification, when only one carbon atom is bonded to a carbon atom to which a hydroxyl group is directly bonded, the hydroxyl group is referred to as a "primary hydroxyl group". Specific examples of primary hydroxyl groups include hydroxyl groups in primary alcohols. As such component (D1), ester-based solvents, glycol-based solvents not having a primary hydroxyl group, ketone-based solvents, or hydrocarbon-based solvents are preferred. Examples of the ester solvent include methyl acetate, ethyl acetate, n-butyl acetate, n-propyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate. An example of a glycol solvent having no primary hydroxyl group is propylene glycol monomethyl ether. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl-n-pentyl ketone, methyl isopentyl ketone, 2-heptanone, and cyclohexanone. Examples of the hydrocarbon solvent include toluene and xylene.

[0054] Of these, the component (D1) is preferably ethyl acetate, n-butyl acetate, n-propyl acetate, methyl ethyl ketone, toluene, or propylene glycol monomethyl ether.

[0055] (Organic solvent (D2)) Examples of the component (D2) that aggregates the component (C) include organic solvents containing a hydroxyl group, and alcohol-based solvents or glycol-based solvents having a primary hydroxyl group are preferred. Examples of the alcohol solvent include methanol, ethanol, 1-propanol, isopropanol, 1-butanol, and t-butanol, with 1-propanol being preferred. Examples of glycol solvents having a primary hydroxyl group include ethylene glycol, diethylene glycol, propylene glycol (1,2-propanediol), and diethylene glycol monomethyl ether. The component (D2) may be used alone, or two or more types may be used in combination.

[0056] The blending ratio (mass %) of the (D1) component and the (D2) component is preferably (D1) component / (D2) component=5 / 95 to 100 / 0, more preferably 20 / 80 to 100 / 0, further preferably 30 / 70 to 100 / 0, and particularly preferably 40 / 60 to 100 / 0.

[0057] The amount of the organic solvent (D) in the composition of the present invention is not particularly limited as long as it is an amount that results in a viscosity suitable for the coating method described below. However, it is preferable to use about 1.0 to 5.0 times the total solid content of the component (D) by mass.

[0058] [Other ingredients] In the active energy ray-curable composition of the present invention, as other components other than the above components (A) to (D), additives such as leveling agents, polymerization initiators, coupling agents such as silane coupling agents, photosensitizers, polymerization inhibitors, defoamers, surface conditioners other than leveling agents, viscosity adjusters, light resistance stabilizers, weather resistance stabilizers, heat resistance stabilizers, ultraviolet absorbers, antioxidants, organic pigments, inorganic pigments, and pigment dispersants; inorganic fillers such as silicon oxide, aluminum oxide, titanium oxide, zirconia, and antimony pentoxide can be blended depending on the application and required properties. These other components can be used alone or in combination of two or more.

[0059] (Leveling agent) Leveling agents are used to adjust the surface tension of the coating film and smooth the surface of the coating film. The presence of a leveling agent reduces the surface tension (surface energy) of the coating film and increases the water contact angle, making it difficult for dirt to adhere, and imparting antifouling properties to the cured coating film.

[0060] Examples of the leveling agent include alkyl carboxylates, alkyl phosphates, alkyl sulfonates, fluoroalkyl carboxylates, fluoroalkyl phosphates, fluoroalkyl sulfonates, polyoxyethylene derivatives, fluoroalkylethylene oxide derivatives, polyethylene glycol derivatives, alkyl ammonium salts, and fluoroalkyl ammonium salts. Among these, fluorine compound-based leveling agents containing fluorine atoms, such as fluoroalkyl carboxylates, fluoroalkyl phosphates, fluoroalkyl sulfonates, fluoroalkyl ethylene oxide derivatives, and fluoroalkyl ammonium salts, are preferred.

[0061] Commercially available leveling agents may be used. Specific examples of commercially available leveling agents include "Megafac F-114", "Megafac F-251", "Megafac F-281", "Megafac F-410", "Megafac F-430", "Megafac F-444", "Megafac F-472SF", "Megafac F-477", "Megafac F-510", "Megafac F-511", "Megafac F-552", "Megafac F-553", "Megafac F-554", "Megafac F-555", "Megafac F-556", "Megafac F-557", and "Megafac F-558". "Megafac F-558", "Megafac F-559", "Megafac F-560", "Megafac F-561", "Megafac F-562", "Megafac F-563", "Megafac F-565", "Megafac F-567", "Megafac F-568", "Megafac F-569", "Megafac F-570", "Megafac F-571", "Megafac R-40", "Megafac R-41", "Megafac R-43", "Megafac R-94", "Megafac RS-72-K", "Megafac RS- 75", "Megafac RS-76-E", "Megafac RS-76-NS", "Megafac RS-90", "Megafac EXP.TF-1367", "Megafac EXP.TF1437", "Megafac EXP.TF1537", "Megafac EXP.TF-2066" (all manufactured by DIC Corporation); "Ftergent 100", "Ftergent 100C", "Ftergent 110", "Ftergent 150", "Ftergent 150CH", "Ftergent 100A-K", "Ftergent 300", "Ftergent "Ftergent 310", "Ftergent 320", "Ftergent 400SW", "Ftergent 251", "Ftergent 215M", "Ftergent 212M", "Ftergent 215M", "Ftergent 250", "Ftergent 222F", "Ftergent 212D", "FTX-218", "Ftergent 209F", "Ftergent 245F", "Ftergent 208G", "Ftergent 240G", "Ftergent 212P", "Ftergent 220P", "Ftergent 228P","DFX-18", "Ftergent 601AD", "Ftergent 602A", "Ftergent 650A", "Ftergent 750FM", "FTX-730FM", "Ftergent 730FL", "Ftergent 710FS", "Ftergent 710FM", "Ftergent 710FL", "Ftergent 750LL", "FTX-730LS", "Ftergent 730LM" (all manufactured by Neos Co., Ltd.); "BYK-300", "BYK-302", "BYK-306", "BYK-307", "BYK-310", "BYK-315", "BYK-320", "BYK-322", "BYK-3 23'', ``BYK-325'', ``BYK-330'', ``BYK-331'', ``BYK-333'', ``BYK-337'', ``BYK-340'', ``BYK-3'' 44", "BYK-350", "BYK-352", "BYK-354", "BYK-355", "BYK-356", "BYK-358N", "BYK-3 61N", "BYK-357", "BYK-370", "BYK-375", "BYK-377", "BYK-390", "BYK-392", "BYK- UV3500", "BYK-UV3510", "BYK-UV3570", "BYK-Silclean3700" (manufactured by BYK Corporation); "TEGO Rad2100'', ``TEGO Rad2011'', ``TEGO Rad2200N'', ``TEGO Rad2250'', ``TEGO Rad2300'', ``TEGO Rad2500'', ``TEGO Rad2600'', ``TEGO Rad2650'', ``TEGO Rad2700'', ``TEGO Flow300'', ``TEGO Flow370'', ``TEGO Flow425", "TEGO Flow ATF2", "TEGO Flow ZFS460", "TEGO Glide100", "TEGO Glide110", "TEGO Glide130", "TEGO Glide410", "TEGO Glide411", "TEGO Glide415", "TEGO Glide432", "TEGO Glide440", "TEGO Glide450”, “TEGO Glide482”, “TEGO Glide A115”, “TEGO Glide B1484”, “TEGO Glide ZG400”,"TEGO Twin4000", "TEGO Twin4100", "TEGO Twin4200", "TEGO Wet240", "TEGO Wet250", "TEGO Wet260", "TEGO Wet265", "TEGO Wet270", "TEGO Wet280", "TEGO Wet500", "TEGO Wet505", "TEGO Wet510", "TEGO Wet520", "TEGO Wet KL245" (all manufactured by Evonik Industries Ltd.), "FC-4430", "FC-4432" (all manufactured by 3M Japan Ltd.), "Unidyne NS" (all manufactured by Daikin Industries, Ltd.), "Surflon S-241", "Surflon S-242", "Surflon S-243", "Surflon S-420", "Surflon S-611", "Surflon S-651", "Surflon S-386" (all manufactured by AGC Seimi Chemical Co., Ltd.), "DISPARLON OX-880EF", "DISPARLON OX-881", "DISPARLON OX-883", "DISPARLON OX-77EF", "DISPARLON OX-710", "DISPARLON 1922", "DISPARLON 1927", "DISPARLON 1958", "DISPARLON DISPARLON LF-1983", "DISPARLON LF-1084", "DISPARLON LF-1985", "DISPARLON LHP-90", "DISPARLON LHP-91", "DISPARLON LHP-95", "DISPARLON LHP-96", "DISPARLON OX-715", "DISPARLON 1930N", "DISPARLON 1931", "DISPARLON 1933", "DISPARLON 1934", "DISPARLON 1711EF", "DISPARLON 1751N”, “DISPARLON 1761”, “DISPARLON LS-009”,"DISPARLON LS-001", "DISPARLON LS-050" (all manufactured by Kusumoto Chemicals Co., Ltd.), "PF-151N", "PF-636", "PF-6320", "PF-656", "PF-6520", "PF-652-NF", "PF-3320" (all manufactured by OMNOVA SOLUTIONS), "Polyflow No.7", "Polyflow No.50E", "Polyflow No.50EHF", "Polyflow No.54N", "Polyflow No.75", "Polyflow No.77", "Polyflow No.85", "Polyflow No.85HF", "Polyflow No.90", "Polyflow No.90D-50", "Polyflow No.95", "Polyflow No.99C", "Polyflow KL-400K", "Polyflow KL-400HF", "Polyflow KL-401", "Polyflow KL-402", "Polyflow KL-403", "Polyflow KL-404", "Polyflow KL-100", "Polyflow LE-604", "Polyflow KL-700", "Floren AC-300", "Floren Examples include "AC-303", "Floren AC-324", "Floren AC-326F", "Floren AC-530", "Floren AC-903", "Floren AC-903HF", "Floren AC-1160", "Floren AC-1190", "Floren AC-2000", "Floren AC-2300C", "Floren AO-82", "Floren AO-98", "Floren AO-108" (all manufactured by Kyoeisha Chemical Co., Ltd.), "L-7001", "L-7002", "8032ADDITIVE", "57ADDTIVE", "L-7064", "FZ-2110", "FZ-2105", "67ADDTIVE", "8616ADDTIVE" (all manufactured by Toray Dow Silicone Co., Ltd.).

[0062] The leveling agents can be used alone or in combination of two or more kinds. When a leveling agent is used, the ratio of the leveling agent to the total amount of solid components is preferably 0.0001 to 3 parts by mass, more preferably 0.0005 to 1 part by mass, and even more preferably 0.001 to 0.1 part by mass.

[0063] (Polymerization initiator) The active energy ray-curable composition of the present invention can be applied onto a substrate and then irradiated with active energy rays to form a cured coating film. The active energy rays include ionizing radiation such as ultraviolet rays, electron beams, α rays, β rays, and γ rays, and ultraviolet rays are widely used industrially. The polymerization initiator is contained in the composition of the present invention in order to initiate a polymerization reaction of compound (A) in response to irradiation with active energy rays, and any compound generally known as a photopolymerization initiator can be used. Specific examples of photopolymerization initiators include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methylpropanol, and the like. acetophenone compounds such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone; benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acylphosphine oxide compounds such as 2,4,6-trimethylbenzoindiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; benzyl(diphenylphosphine) benzyl compounds such as benzoyl), methylphenylglyoxyester, oxyphenylacetic acid 2-(2-hydroxyethoxy)ethyl ester, and oxyphenylacetic acid 2-(2-oxo-2-phenylacetoxyethoxy)ethyl ester; benzophenone, o-benzoylbenzoic acid methyl-4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4, Benzophenone compounds such as 4'-tetra(t-butylperoxycarbonyl)benzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2,4,6-trimethylbenzophenone, and 4-methylbenzophenone; thioxanthone compounds such as 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone; aminobenzophenone compounds such as Michler's ketone and 4,4'-diethylaminobenzophenone;10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, camphorquinone, 1-[4-(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylphenylsulfonyl)propan-1-one, etc.;

[0064] As the polymerization initiator, commercially available products can also be used. Specific examples of commercially available products include alkylphenone compounds: Omnirad 184, Omnirad 1173, Omnirad 1116, Omnirad 907, Omnirad 651, Omnirad 2959, Omnirad 127, Omnirad 369, and Omnirad 379 (all manufactured by IGM Resins BV); acylphosphine oxide compounds: Omnirad TPO and Omnirad 819 (all manufactured by IGM Resins BV); oxime ester compounds: Irgacure OXE01, Irgacure OXE02, Irgacure OXE03, and Irgacure OXE04 (all manufactured by IGM Resins BV); and hydrogen abstraction compounds: SB-PI 701, SB-PI 701, SB-PI 707, SB-PI 711, SB-PI 712, and SB-PI 716 (all manufactured by Sanyo Trading Co., Ltd.), Kayacure DETX-S, Kayacure EPA (all manufactured by Nippon Kayaku Co., Ltd.), and Cantacure-ITX (manufactured by Ward Prekinsop Co., Ltd.).

[0065] The polymerization initiators can be used alone or in combination of two or more. The amount of the polymerization initiator component added is preferably 0.05 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, and even more preferably 1 to 15 parts by mass, per 100 parts by mass of the total of the components (A) and (B).

[0066] (Coupling Agent) The active energy ray curable composition of the present invention may contain a coupling agent. The coupling agent is not particularly limited as long as it is a compound capable of bonding a plurality of materials, and any compound generally known as a coupling agent may be used, with silane coupling agents being preferred. Specifically, the silane coupling agent is Silane coupling agents having a vinyl group, such as vinyltrimethoxysilane and vinyltriethoxysilane; silane coupling agents having an epoxy group, such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane; Silane coupling agents having a styryl group, such as p-styryltrimethoxysilane; silane coupling agents having a (meth)acryloyl group, such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane; silane coupling agents having an amino group, such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride; Isocyanurate-based silane coupling agents such as tris-(trimethoxysilylpropyl)isocyanurate; Isocyanate-based silane coupling agents such as 3-isocyanatepropyltriethoxysilane; Silane coupling agents having a ureido group, such as 3-ureidopropyltrialkoxysilane; silane coupling agents having a mercapto group, such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; Sulfide-based silane coupling agents such as bis(triethoxysilylpropyl)tetrasulfide; 3-trimethoxysilylpropylsuccinic anhydride, and the like. The silane coupling agent or other coupling agents may be used alone or in combination of two or more kinds. When the active energy ray-curable composition of the present invention contains a coupling agent, the amount of the coupling agent to be blended may be 0.001 to 10 parts by mass per 100 parts by mass of the total of the components (A) and (B).

[0067] The active energy ray-curable composition of the present invention can be suitably used as a cured coating film (hard coat layer) that imparts hardness and scratch resistance to a substrate, for example, by applying it to at least one surface of various materials and then irradiating it with active energy rays. The cured coating film made from the composition of the present invention can impart hardness and scratch resistance to the film surface and can form a hard coat layer that has excellent anti-glare control, and therefore exerts particularly excellent effects when used as a hard coat for FPD materials that require reduced glare.

[0068] <Cured product / laminate> The cured product of the present invention is obtained by curing the above-mentioned active energy ray-curable composition of the present invention. The laminate of the present invention has a cured coating film of the active energy ray-curable composition of the present invention. The laminate can be obtained, for example, by applying the active energy ray-curable composition of the present invention onto a substrate and then curing the composition. The substrate is not particularly limited and may be appropriately selected depending on the application. Examples of the substrate include plastic, glass, wood, metal, metal oxide, paper, silicon, or modified silicon, and the substrate may be obtained by bonding different materials. The shape of the substrate is not particularly limited, and may be any shape according to the purpose, such as a flat plate, a sheet, or a three-dimensional shape having a curvature on the entire surface or part thereof, etc. Furthermore, there is no limitation on the hardness, thickness, etc. of the substrate.

[0069] The plastic substrate is not particularly limited as long as it is made of resin, and for example, the above-mentioned thermosetting resin or thermoplastic resin may be used. The substrate may be a substrate made of a single resin or a mixture of multiple resins, and may have a single layer or a laminate structure of two or more layers. In addition, these plastic substrates may be fiber reinforced plastic (FRP).

[0070] Furthermore, the base material may contain known additives such as known antistatic agents, antifogging agents, antiblocking agents, ultraviolet absorbers, antioxidants, pigments, organic fillers, inorganic fillers, light stabilizers, crystal nucleating agents, and lubricants, as long as the effects of the present invention are not impaired.

[0071] The laminate of the present invention may further have a second substrate on the substrate and the cured coating film. The material of the second substrate is not particularly limited, and examples thereof include glass, wood, metal, metal oxide, plastic, paper, silicon, or modified silicon, and may be a substrate obtained by bonding different materials. The shape of the substrate is not particularly limited, and may be any shape according to the purpose, such as a flat plate, a sheet, or a three-dimensional shape having a curvature on the entire surface or part. In addition, there is no limitation on the hardness, thickness, etc. of the substrate.

[0072] The cured coating film of the present invention has high adhesion to both plastics and inorganic materials, and can therefore be preferably used as an interlayer material between different materials. Particularly preferably, the substrate is plastic and the second substrate is an inorganic layer. Examples of inorganic layers include quartz, sapphire, glass, optical films, ceramic materials, inorganic oxides, vapor deposition films (CVD, PVD, sputtering), magnetic films, reflective films, metals such as Ni, Cu, Cr, Fe, and stainless steel, paper, plastic layers such as SOG (Spin On Glass), SOC (Spin On Carbon), polyester, polycarbonate, and polyimide, TFT array substrates, electrode plates for PDPs, conductive substrates such as ITO and metals, insulating substrates, silicon-based substrates such as silicon, silicon nitride, polysilicon, silicon oxide, and amorphous silicon.

[0073] The surface wet tension of the cured coating film of the present invention is preferably in the range of 35 to 60 mN / m, more preferably 40 to 55 mN / m, where the wet tension is a value measured in accordance with JIS test method K6768:1999.

[0074] (Manufacturing method) The laminate of the present invention can be obtained by applying the composition of the present invention to the surface of a substrate and then curing the composition. The composition can be applied to the substrate by directly applying the composition to the substrate or by directly molding the composition onto the substrate and then curing the composition. In the case of direct coating, the coating method is not particularly limited, and examples thereof include spraying, spin coating, dipping, roll coating, blade coating, doctor roll method, doctor blade method, curtain coating, slit coating, gravure coating, microgravure coating, die coating, screen printing, inkjet printing, offset printing, gravure printing, and flexographic printing. In the case of direct molding, examples of the method include in-mold molding, insert molding, vacuum molding, extrusion lamination molding, and press molding. The film of the present invention may also be obtained by laminating a cured product of the composition on a substrate. When laminating a cured product of the composition, a semi-cured cured product may be laminated on the substrate and then completely cured, or a completely cured cured product may be laminated on the substrate.

[0075] Since the composition of the present invention contains a compound having a polymerizable unsaturated group, it can be cured by irradiation with active energy rays. Examples of active energy rays include ultraviolet rays, electron beams, α rays, β rays, γ rays, and other ionizing radiation. Among these, ultraviolet rays (UV) are particularly preferred from the standpoint of curability and convenience. Here, when ultraviolet rays are used as the active energy rays, examples of the device for irradiating the ultraviolet rays include low pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, electrodeless lamps (fusion lamps), chemical lamps, black light lamps, mercury-xenon lamps, short arc lamps, helium-cadmium lasers, argon lasers, sunlight, LED lamps, etc. Using these, it is possible to obtain a cured coating film or a cured product by irradiating the coated or molded composition with ultraviolet rays having a wavelength of about 180 to 400 nm. The amount of ultraviolet irradiation is appropriately selected depending on the type and amount of the photopolymerization initiator used.

[0076] (Application) The cured coating film of the composition of the present application has high hardness and excellent hot water-resistant adhesion and light-resistant adhesion, and therefore can maintain high adhesion while protecting the object from external impact, moisture, and light, and can be suitably used for applications such as a film for preventing scratches on the surface of flat panel displays (FPDs) such as liquid crystal displays (LCDs), organic electroluminescent displays (OLEDs), and plasma displays (PDPs), and a protective film for electrodes made of conductive electrode materials for display elements inside displays and touch panels (touch sensors), etc. In addition, the composition can be suitably used for various applications such as decorative films (sheets) for the interior and exterior of automobiles, low-reflection films for windows, and heat-cutting films. EXAMPLES

[0077] The present invention will now be described in more detail with reference to examples. Unless otherwise specified, "%" means "% by mass".

[0078] Example 1 As the component (A), 5.0 parts by mass of 2-hydroxy-3-acryloyloxypropyl methacrylate "Light Ester G-201P" (trade name, manufactured by Kyoeisha Chemical Co., Ltd.), as the component (B), 26.59 parts by mass of a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate "Aronix M-450" (trade name, manufactured by Toagosei Co., Ltd.), 35.46 parts by mass of an acrylic acrylate resin "Luxidia EVS-301" (trade name, manufactured by DIC Corporation, solid content ratio 50%), 2.0 parts by mass of dimethylol-tricyclodecane diacrylate "Light Acrylate DCP-A" (trade name, manufactured by Kyoeisha Chemical Co., Ltd.) and polyester acrylate "Aronix M-9050" (trade name, manufactured by Toagosei Co., Ltd.), as the component (C), acrylic-styrene copolymer crosslinked organic fine particles "Acrybase An active energy ray-curable composition was obtained by uniformly mixing 2.89 parts by mass of “DLB-005” (trade name, manufactured by Fujikura Chemical Industries, Ltd., refractive index 1.55, D50 average particle size 0.98 μm), 81.77 parts by mass of butyl acetate as component (D), and 2.95 parts by mass of a photopolymerization initiator “Omnirad 184” (trade name, manufactured by IGM Resins).

[0079] (Examples 2 to 7, Comparative Examples 1 to 3) Except for changing the compositions shown in Tables 1 and 2, the same procedure as in Example 1 was carried out to obtain active energy ray-curable compositions of each example.

[0080] [Preparation of evaluation samples] The active energy ray-curable composition of each example was applied to a triacetyl cellulose film (TAC) substrate (manufactured by Fuji Film Corporation, product name "TAC-TD60U", thickness: 60 μm) to a film thickness of 4 μm, dried at 60° C. for 1 minute, and then exposed to 240 mW / cm 2 with a high-pressure mercury lamp. 2 , 150mJ / cm 2The resulting laminate consisting of the TAC substrate and the cured coating film was used as a test sample.

[0081] [Total light transmittance evaluation] The total light transmittance of the cured coating film of each example obtained above was measured using a haze meter ("NDH4000" manufactured by Nippon Denshoku Co., Ltd.) in accordance with JIS K7136. The results are shown in the table as "Transmittance".

[0082] [Haze value evaluation] The haze value of the cured coating film of each example obtained above was measured using a haze meter ("NDH4000" manufactured by Nippon Denshoku Co., Ltd.) in accordance with JIS K7136. The results are shown in the table as "haze".

[0083] [Transmission clarity evaluation] Using the test samples of each example obtained above, measurements were performed at five points with optical comb widths of 0.125, 0.25, 0.5, 1.0, and 2.0 mm using an image clarity measuring device ("ICM-IT" manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS K7374. The total value of the five measured points is recorded in the table as "image clarity."

[0084] [Table 1]

[0085] [Table 2]

[0086] In the above table, the abbreviations have the following meanings: A-1: 2-hydroxy-3-acryloxypropyl methacrylate "Light Ester G-201P" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-2: Phosphate (meth)acrylate "Light Ester P-1M" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-3: Phosphate (meth)acrylate "Light Ester P-2M" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-4: Aliphatic epoxy acrylate "Epoxy Ester 40EM" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-5: Aliphatic epoxy acrylate "Epoxy Ester 70PA" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-6: Aliphatic epoxy acrylate "Epoxy Ester 80MFA" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-7: Aliphatic epoxy acrylate "Laromer EA8765R" (product name, manufactured by BASF) A-C1: Polyethylene glycol diacrylate "Light Acrylate 9EG-A" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) A-C2: 2-Hydroxy-3-phenoxypropyl acrylate "Aronix M-5700" (product name, manufactured by Toagosei Co., Ltd.) B-1: A mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate "Aronix M-450" (product name, manufactured by Toagosei Co., Ltd.) B-2: Acrylic acrylate resin "Luxidia EVS-301" (product name, manufactured by DIC, solid content ratio 50%) B-3: Dimethylol-tricyclodecane diacrylate "Light Acrylate DCP-A" (product name, manufactured by Kyoeisha Chemical Co., Ltd.) B-4: Polyester acrylate "Aronix M-9050" (product name, manufactured by Toagosei Co., Ltd.) C-1: Acrylic-styrene copolymer crosslinked organic particles "Acrybase DLB-005" (product name, Fujikura Kasei Co., Ltd., refractive index 1.55, D50 average particle size 0.98 μm) D-1: n-Butyl acetate I-1: Photoinitiator "Omnirad 184" (trade name, manufactured by IGM Resins)

[0087] In the cured coating films of the active energy ray curable compositions according to the present invention in Examples 1 to 7, the component (A) was contained, and it was possible to arbitrarily reduce the transmission sharpness (image clarity) without changing the total light transmittance or significantly changing the haze. In the examples, it was confirmed that the transmission sharpness can be arbitrarily adjusted depending on the type of the component (A) used, and therefore the antiglare properties can be easily and strictly controlled. On the other hand, in Comparative Example 1, which did not contain component (A), and Comparative Examples 2 and 3, which used monomers other than component (A), the transmitted light clarity (image clarity) was high, and the antiglare properties could not be adjusted.

[0088] (Examples 8 to 16, Comparative Examples 4 to 5) Except for changing the composition shown in Tables 3 and 4, the active energy ray curable composition of each example was obtained in the same manner as in Example 1, and then an evaluation sample was prepared and evaluated for total light transmittance, haze value, and transmission clarity. The results are shown in Tables 3 and 4. In the table below, "D-2" means n-propyl alcohol.

[0089] [Table 3]

[0090] [Table 4]

[0091] In the cured coating films of the active energy ray-curable compositions according to the present invention in Examples 8 to 16, the transmission sharpness (image clarity) could be arbitrarily reduced by including the component (A) without significantly changing the total light transmittance and haze, compared to Comparative Examples 4 and 5. In the examples, it was confirmed that the transmission sharpness could be arbitrarily adjusted depending on the type and amount of the component (A) used, and therefore the antiglare properties could be easily and strictly controlled.

[0092] (Examples 17 to 18, Comparative Examples 6 to 10) The active energy ray-curable compositions of each example were obtained in the same manner as in Example 1, except that the compositions were changed to those shown in Table 5. Then, evaluation samples were prepared and evaluated for total light transmittance, haze value, and transmission clarity. The results are also shown in Table 5.

[0093] [Table 5]

[0094] In the above table, the abbreviations have the following meanings. A-C3: Acryloylmorpholine "ACMO" (product name, manufactured by KJ Chemicals) A-C4: ω-carboxy-polycaprolactone (n≒2) monoacrylate "Aronix M-5300" (product name, manufactured by Toagosei Co., Ltd.) A-C5: 1,9-nonanediol diacrylate "Light Acrylate 1,9ND-A" (product name, manufactured by Kyoeisha Chemical Co., Ltd.)

[0095] In the cured coating films of the active energy ray curable compositions according to the present invention in Examples 17 to 18, the transmission sharpness (image clarity) could be arbitrarily reduced without significantly changing the total light transmittance and haze by containing the component (A). In the examples, it was confirmed that the transmission sharpness could be arbitrarily adjusted depending on the type of the component (A) used, and therefore the antiglare properties could be easily and strictly controlled. On the other hand, in Comparative Examples 6 and 10, which did not contain the component (A), and Comparative Examples 7 to 9, which used a monomer other than the component (A), the transmitted light clarity (image clarity) was high, and the antiglare properties could not be adjusted.

[0096] (Example 19, Comparative Example 11) The active energy ray-curable compositions of each example were obtained in the same manner as in Example 1, except that the compositions were changed to those shown in Table 6. Then, evaluation samples were prepared and evaluated for total light transmittance, haze value, and transmission clarity. The results are also shown in Table 6. In the table below, "C-2" refers to acrylic-styrene copolymer crosslinked organic particles "ACRYBASE DLB-001" (product name, manufactured by Fujikura Chemical Industries, Ltd., refractive index 1.59, D50 average particle size 0.85 μm), and "D-3" refers to ethyl acetate.

[0097] [Table 6]

[0098] The cured coating film of the active energy ray-curable composition of Example 19 containing the component (A) was able to reduce image clarity without causing a significant change in total light transmittance and haze, as compared to Comparative Example 11 not containing the component (A).

Claims

1. An active energy ray-curable composition comprising: a compound (A) having one or two (meth)acryloyloxy groups, a hydroxyl group (excluding a carboxy group), and a chain hydrocarbon group which may have a substituent; an active energy ray-curable compound (B) which does not fall under the category of compound (A); fine particles (C); and an organic solvent (D).

2. The active energy ray-curable composition according to claim 1 , wherein the compound (A) has a molecular weight of 1,000 or less.

3. The active energy ray-curable composition according to claim 1 , wherein the active energy ray-curable compound (B) is an acrylic resin containing a (meth)acryloyl group in a side chain.

4. The active energy ray-curable composition according to claim 1 , wherein the active energy ray-curable compound (B) is a compound having a hydroxyl group.

5. The active energy ray-curable composition according to claim 1 , wherein the fine particles (C) are organic crosslinked fine particles.

6. 2. The active energy ray-curable composition according to claim 1, wherein the fine particles (C) are at least one selected from the group consisting of acrylic fine particles, acrylic-styrene copolymer fine particles, and polystyrene fine particles.

7. 2. The active energy ray-curable composition according to claim 1, wherein the fine particles (C) have an average particle size of 0.05 μm to 10 μm.

8. 2. The active energy ray-curable composition according to claim 1, wherein the refractive index of the fine particles (C) is 1.48 to 1.

66.

9. A cured product of the active energy ray-curable composition according to any one of claims 1 to 8.

10. A laminate having a cured coating film of the active energy ray-curable composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Antiglare film, sheet polarizer and transmission type display device

    JP2009086677A

  • Photocurable resin composition, cured coating and antidazzle film formed from the composition, image display device, and production method of cured coating and antidazzle film

    JP2016045448A